Polishing liquid composition for acidified siliceous film
The use of cerium oxide particles with specific size and density distributions in a polishing liquid composition addresses the reduced polishing rate issue in CMP processes, enhancing the efficiency and quality of silicon oxide film polishing in semiconductor manufacturing.
Patent Information
- Application Number
- JP2021037757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-03-09
AI Technical Summary
The challenge in CMP polishing for semiconductor devices is the reduction in polishing rate due to the use of smaller abrasive grains, which compromises the efficiency in polishing silicon oxide films, especially in highly integrated and complex wiring structures.
A polishing liquid composition containing cerium oxide particles with specific size and density ranges, mixed in a particular ratio, is used to enhance the polishing rate of silicon oxide films, utilizing the mechanical and chemical properties of cerium oxide to improve polishing speed and reduce scratches.
The composition significantly enhances the polishing rate of silicon oxide films, improving the productivity and quality of semiconductor substrates by maintaining a high polishing speed while reducing defects.
Smart Images

Figure 0007569717000001 
Figure 0007569717000002 
Figure 0007569717000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polishing composition for silicon oxide films that contains cerium oxide particles, a method for producing a semiconductor substrate, and a method for polishing a substrate using the same. [Background technology]
[0002] Chemical mechanical polishing (CMP) is a technique in which the surface of the substrate to be polished is brought into contact with a polishing pad, and a polishing liquid is supplied to the contact point while the substrate and polishing pad are moved relative to each other, thereby chemically reacting with and mechanically removing and planarizing the uneven surface of the substrate.
[0003] Currently, CMP technology is essential in the manufacturing process of semiconductor devices for flattening interlayer insulating films, forming shallow trench isolation structures, forming plugs and buried metal wiring, etc. In recent years, semiconductor devices have become increasingly multi-layered and highly precise, and there is a demand for further improvements in the yield and throughput of semiconductor devices. Accordingly, there is a demand for scratch-free and faster polishing in the CMP process.
[0004] For example, Patent Document 1 discloses that the use of ceria particles having primary and secondary particle sizes and density within specific ranges achieves both a good polishing rate and a good surface finish. Patent Document 2 discloses that the removal rate and the in-plane uniformity can be improved by mixing two types of abrasive particles in specific ranges and further containing functionalized pyridine, benzoic acid, or amino acid. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2011-545995 [Patent Document 2] Special Publication No. 2016-538359 Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, the semiconductor industry has become highly integrated, and there is a demand for more complex and finer wiring. For this reason, in CMP polishing, the grain size of the abrasive is reduced to reduce defects, but this causes a problem of a decrease in the polishing speed, and there is a demand for an improvement in the polishing speed of silicon oxide films.
[0007] Therefore, the present disclosure provides a polishing composition for silicon oxide films that can improve the polishing rate of silicon oxide films, a method for polishing substrates using the same, and a method for manufacturing semiconductor substrates. [Means for solving the problem]
[0008] In one aspect, the present disclosure provides a polishing composition for silicon oxide films, comprising cerium oxide particles and an aqueous medium, the cerium oxide particles having an average particle size of 15 nm or more and 50 nm or less and a density of 8 g / cm 3 The polishing liquid composition contains the above cerium oxide particles (component A) and cerium oxide particles (component B) having an average particle size of 60 nm or more and 1 μm or less, has a pH of 3 or more and 9 or less, and when D50 and D99 are the particle sizes at which the cumulative frequency from the small particle size side is 50% and 99%, respectively, in a particle size distribution on a weight basis obtained by centrifugal sedimentation of a mixture of components A and B, the D50 / D99 value is 0.32 or less.
[0009] In another aspect, the present disclosure relates to a polishing method comprising a step of polishing a film to be polished with the polishing liquid composition of the present disclosure, wherein the film to be polished is a silicon oxide film formed in the process of manufacturing a semiconductor substrate.
[0010] In another aspect, the present disclosure relates to a method for producing a semiconductor substrate, the method including a step of polishing a film to be polished with the polishing composition of the present disclosure. Effect of the Invention
[0011] According to one aspect of the present disclosure, a polishing composition for silicon oxide films, which can improve the polishing rate of silicon oxide films, can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In one aspect, the present disclosure is based on the finding that in a polishing composition containing cerium oxide (hereinafter also referred to as "ceria") particles as abrasive grains, small-diameter ceria having high density can contribute to improving the polishing rate when mixed with large-diameter ceria under specified conditions.
[0013] Although the details of the mechanism by which the effects of the present disclosure are manifested are not clear, it is presumed as follows. Ceria particles are generally used to polish silicon oxide films. Usually, the cerium in ceria particles is tetravalent, but occasionally an oxygen atom is lost to make it trivalent. It is believed that the trivalent cerium in ceria particles weakens the Si-O bond in the silicon oxide film, weakening it and facilitating polishing. Data suggest that the amount of trivalent cerium present on the surface of high-density, small-diameter ceria is high. It has also been found that the removal rate of high-density, small-diameter ceria is significantly maximized at relatively high temperatures. It is believed that the mixture of high-density small-diameter ceria with large-diameter ceria increases friction during polishing, resulting in high temperatures, allowing the small-diameter ceria to exert its functions and improve the polishing rate. In addition, in the present disclosure, it is believed that the polishing rate is improved by the action of both the function of small-diameter ceria and the physical cutting of large-diameter ceria, since D50 / D99 in the particle size distribution obtained by centrifugal sedimentation is 0.32 or less. It is known that particle size distribution can usually be measured by centrifugal sedimentation or dynamic light scattering, but in the present disclosure, the particle size distribution of ceria is measured by centrifugal sedimentation, which has a higher resolution than dynamic light scattering. However, the present disclosure need not be construed as being limited to these mechanisms.
[0014] [Cerium oxide (ceria) particles] The polishing liquid composition of the present disclosure contains, as polishing abrasive grains, cerium oxide particles of Component A and cerium oxide particles of Component B. Each of Component A and Component B may be one type or a combination of two or more types.
[0015] [Component A] Component A has an average particle size of 15 nm or more and 50 nm or less and a density of 8 g / cm 3 The above cerium oxide particles are preferably calcined cerium oxide particles. Here, the term "calcined cerium oxide particles" refers to cerium oxide particles (ceria particles) obtained by calcining a cerium compound. Examples of the calcined cerium oxide particles include calcined pulverized cerium oxide obtained by calcining and pulverizing a cerium compound. Examples of the cerium compound before calcination and oxidation include cerium carbonate and cerium nitrate. In one or more embodiments, the calcined cerium oxide particles may be referred to as calcined ceria. In one or more embodiments, the calcined pulverized cerium particles may be referred to as calcined pulverized ceria.
[0016] Examples of the shape of Component A include a substantially spherical shape, a polyhedral shape, and a raspberry shape.
[0017] From the viewpoint of improving the polishing rate, the average particle size of component A is 15 nm or more, preferably 20 nm or more, more preferably 22 nm or more, and from the same viewpoint, it is 50 nm or less, preferably 40 nm or less, more preferably 30 nm or less. From the same viewpoint, the average particle size of component A is 15 nm or more and 50 nm or less, preferably 20 nm or more and 50 nm or less, more preferably 20 nm or more and 40 nm or less, and even more preferably 22 nm or more and 30 nm or less.
[0018] In the present disclosure, the term "average particle size" refers to a particle size at which the cumulative frequency from the small diameter side is 50% in a particle size distribution calculated by weight obtained by centrifugal sedimentation. In the present disclosure, the centrifugal sedimentation method, in one or more embodiments, is a method of classifying and detecting particles by size based on the difference in sedimentation velocity (disk centrifugal sedimentation light transmission method). The particle size distribution by the centrifugal sedimentation method can be measured, for example, using a disk centrifugal particle size distribution measuring device (CPS Disc Centrifuge). In the following description, the particle size distribution by the centrifugal sedimentation method is sometimes referred to as "particle size distribution by CPS measurement". The average particle size can be calculated by the measurement method described in the examples.
[0019] The density of component A is set to 8 g / cm from the viewpoint of improving the polishing speed. 3 More than 8.5g / cm 3 More than 8.7 g / cm is preferable. 3 More preferably, from the same viewpoint, 10 g / cm 3 Less than 9.8 g / cm is preferred. 3 From the same viewpoint, the density of component A is preferably 8 g / cm or less. 3 More than 10g / cm 3 Less than 8.5 g / cm is preferred. 3 More than 10g / cm 3 Less than 8.7 g / cm is more preferable. 3 More than 9.8g / cm 3 The following is even more preferred: In the present disclosure, "density" refers to a value measured by a pycnometer. The density can be measured by the method described in the Examples.
[0020] In one or more embodiments, component A can be produced using tetravalent ceria. For example, nanocrystalline ceria is produced from a tetravalent ceria precursor, and then single-crystalline ceria (small-diameter ceria) is obtained by sintering the nanocrystalline ceria to grow the crystals. The single-crystalline ceria is then pulverized to produce small-diameter, high-density sintered ceria (component A). The average particle size and density of component A can be controlled by the size of the nanocrystalline ceria, the sintering conditions, and the pulverization conditions. For example, the density can be increased by increasing the sintering temperature.
[0021] The content of component A in the polishing liquid composition of the present disclosure is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.07 mass% or more, and even more preferably 0.1 mass% or more, from the viewpoint of improving the polishing rate, and from the same viewpoint, it is preferably 2 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, and even more preferably 0.4 mass% or less. From the same viewpoint, the content of component A in the polishing liquid composition of the present disclosure is preferably 0.01 mass% or more and 2 mass% or less, more preferably 0.05 mass% or more and 1 mass% or less, even more preferably 0.07 mass% or more and 0.5 mass% or less, and even more preferably 0.1 mass% or more and 0.4 mass% or less. When component A is a combination of two or more types of cerium oxide particles, the content of component A refers to the total content thereof.
[0022] [Component B] Component B is cerium oxide particles having an average particle size of 60 nm to 1 μm. Component B has a larger average particle size than Component A.
[0023] There may be no particular limitation on the manufacturing method, shape, and surface state of Component B. Examples of Component B include colloidal ceria, amorphous ceria, and ceria-coated silica. Colloidal ceria can be obtained by a build-up process, for example, by the method described in Examples 1 to 4 of JP-A No. 2010-505735. In one or more embodiments, colloidal ceria is an example of wet cerium oxide (hereinafter, also referred to as "wet ceria"). An example of the amorphous ceria is pulverized ceria. An example of the pulverized ceria is sintered pulverized cerium oxide obtained by sintering and pulverizing a cerium compound such as cerium carbonate or cerium nitrate. Another example of the pulverized ceria is single crystal pulverized ceria obtained by wet pulverizing ceria particles in the presence of an inorganic acid or an organic acid. An example of the inorganic acid used in the wet pulverization is nitric acid, and an example of the organic acid is an organic acid having a carboxyl group, specifically at least one selected from picolinic acid, glutamic acid, aspartic acid, aminobenzoic acid, and p-hydroxybenzoic acid. An example of the wet pulverization method is wet pulverization using a planetary bead mill or the like. Examples of ceria-coated silica include composite particles having a structure in which at least a portion of the surface of silica particles is coated with granular ceria, as described in, for example, Examples 1 to 14 of JP2015-63451A or Examples 1 to 4 of JP2013-119131A. The composite particles can be obtained, for example, by depositing ceria on silica particles.
[0024] Examples of the shape of component B include an approximately spherical shape, a polyhedral shape, and a raspberry shape.
[0025] From the viewpoint of improving the polishing rate, the average particle size of component B is 60 nm or more, preferably 70 nm or more, more preferably 80 nm or more, and even more preferably 90 nm or more. From the viewpoint of reducing polishing scratches, it is 1 μm or less, preferably 500 nm or less, more preferably 250 nm or less, and even more preferably 125 nm or less. From the same viewpoint, the average particle size of component B is 60 nm or more and 1 μm or less, preferably 70 nm or more and 500 nm or less, more preferably 80 nm or more and 250 nm or less, and even more preferably 90 nm or more and 125 nm or less.
[0026] The density of component B is set to 8 g / cm from the viewpoint of improving the polishing speed. 3 Less than 7.8 g / cm is preferred. 3 Less than 7.5 g / cm is more preferable. 3From the viewpoint of reducing polishing scratches, 6 g / cm or less is more preferable. 3 More than 6.3 g / cm is preferable. 3 More preferably, 6.6 g / cm 3 From the same viewpoint, the density of component B is preferably 6 g / cm 3 More than 8g / cm 3 Less than 6.3 g / cm is preferred. 3 More than 7.8g / cm 3 Less than 6.6 g / cm is more preferable. 3 More than 7.5g / cm 3 The density of component B obtained by the above method is usually 8 g / cm3 or less. 3 is less than.
[0027] The content of component B in the polishing liquid composition of the present disclosure is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 0.07% by mass or more, and even more preferably 0.1% by mass or more, from the viewpoint of improving the polishing rate, and is preferably 4% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and even more preferably 1.5% by mass or less, from the viewpoint of reducing polishing scratches. The content of component B in the polishing liquid composition of the present disclosure is preferably 0.01% by mass or more and 4% by mass or less, more preferably 0.05% by mass or more and 3% by mass or less, even more preferably 0.07% by mass or more and 2% by mass or less, and even more preferably 0.1% by mass or more and 1.5% by mass or less, from the same viewpoint. When component B is a combination of two or more types of cerium oxide particles, the content of component B refers to the total content thereof.
[0028] In the particle size distribution of the mixture of component A and component B in the polishing liquid composition of the present disclosure, the particle size at which the cumulative frequency from the small particle size side is 50% and 99% in weight conversion obtained by centrifugal sedimentation is D50 and D99, respectively. From the viewpoint of improving the polishing rate, the value of D50 / D99 is 0.32 or less, preferably 0.3 or less, more preferably less than 0.3, and even more preferably 0.25 or less. From the viewpoint of reducing polishing scratches, the value of D50 / D99 is preferably 0.01 or more, more preferably 0.05 or more, more preferably 0.08 or more, and even more preferably 0.1 or more. From the same viewpoint, the value of D50 / D99 in the polishing liquid composition of the present disclosure is preferably 0.01 or more and 0.32 or less, more preferably 0.05 or more and 0.3 or less, more preferably 0.08 or more and less than 0.3, and even more preferably 0.1 or more and 0.25 or less.
[0029] The weight ratio (A / B) of the content of component A to the content of component B in the polishing liquid composition of the present disclosure is preferably 1 / 6 or more, more preferably 1 / 4 or more, and even more preferably 1 / 3 or more, from the viewpoint of reducing polishing scratches. From the viewpoint of improving the polishing rate, it is preferably 4 / 1 or less, more preferably 3 / 1 or less, and even more preferably 2 / 1 or less. From the viewpoint of improving the polishing rate, the weight ratio (A / B) in the polishing liquid composition of the present disclosure is preferably 1 / 6 or more and 4 / 1 or less, more preferably 1 / 4 or more and 3 / 1 or less, and even more preferably 1 / 3 or more and 2 / 1 or less.
[0030] The total content of component A and component B in the polishing liquid composition of the present disclosure is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.2% by mass or more, and even more preferably 0.3% by mass or more, from the viewpoint of improving the polishing rate. From the viewpoint of reducing polishing scratches, it is preferably 6% by mass or less, more preferably 5% by mass or less, even more preferably 3% by mass or less, and even more preferably 2% by mass or less. From the same viewpoint, the total content of component A and component B in the polishing liquid composition of the present disclosure is preferably 0.05% by mass or more and 6% by mass or less, more preferably 0.1% by mass or more and 5% by mass or less, even more preferably 0.2% by mass or more and 3% by mass or less, and even more preferably 0.3% by mass or more and 2% by mass or less.
[0031] [Aqueous medium] Examples of the aqueous medium contained in the polishing liquid composition of the present disclosure include water such as distilled water, ion-exchanged water, pure water, and ultrapure water, or a mixed solvent of water and a solvent. Examples of the solvent include a solvent miscible with water (for example, an alcohol such as ethanol). When the aqueous medium is a mixed solvent of water and a solvent, the ratio of water to the entire mixed medium may not be particularly limited as long as the effects of the present disclosure are not hindered. From the viewpoint of economy, for example, 95% by mass or more is preferable, 98% by mass or more is more preferable, and substantially 100% by mass is even more preferable. From the viewpoint of the surface cleanliness of the substrate to be polished, water is preferable as the aqueous medium, ion-exchanged water and ultrapure water are more preferable, and ultrapure water is even more preferable. The content of the aqueous medium in the polishing liquid composition of the present disclosure can be the remainder excluding component A, component B, and component C and optional components to be described later that are blended as necessary.
[0032] [Additive (Component C)] In one or more embodiments, the polishing liquid composition of the present disclosure may contain a compound (component C) having a reduction potential of 0.45 V or more and 0.95 V or less when measured by cyclic voltammetry (Ag / AgCl electrode standard) for a 10 ppm aqueous solution from the viewpoint of improving the polishing rate.
[0033] From the viewpoint of improving the polishing rate, the reduction potential is preferably 0.45 V or more, more preferably 0.5 V or more, and even more preferably 0.55 V or more. From the same viewpoint, it is preferably 0.95 V or less, more preferably 0.92 V or less, and even more preferably 0.89 V or less. The reduction potential can be measured by the method described in the examples.
[0034] In one or more embodiments, component C is preferably a reducing compound containing a heteroaromatic ring skeleton from the viewpoint of improving the polishing rate. Examples of component C include an N-oxide compound or a salt thereof containing a nitrogen-containing heteroaromatic ring skeleton in which at least one hydrogen atom is substituted with a hydroxyl group. Component C may be of one type or a combination of two or more types.
[0035] <N-oxide compound> In one embodiment, component C contained in the polishing liquid composition of the present disclosure is an N-oxide compound or a salt thereof, which includes a nitrogen-containing heteroaromatic ring skeleton in which at least one hydrogen atom of the nitrogen-containing heteroaromatic ring is substituted with a hydroxyl group. Examples of the salt include alkali metal salts, alkaline earth metal salts, organic amine salts, and ammonium salts. Component C may be used alone or in combination of two or more kinds. Thus, in one aspect, the present disclosure relates to a polishing liquid composition for silicon oxide films, which contains cerium oxide particles (components A and B), an N-oxide compound (component C), and an aqueous medium, wherein component C is an N-oxide compound or a salt thereof that contains a nitrogen-containing heteroaromatic ring skeleton in which at least one hydrogen atom is substituted with a hydroxyl group.
[0036] In this aspect, in one or more embodiments, the N-oxide compound refers to a compound having an N-oxide group (N→O group). The N-oxide compound may have one or more N→O groups, and from the viewpoint of availability, the number of N→O groups is preferably one. In this embodiment, the term "nitrogen-containing heteroaromatic ring skeleton in which at least one hydrogen atom is substituted with a hydroxyl group" refers to a structure in which at least one hydrogen atom of a nitrogen-containing heteroaromatic ring is substituted with a hydroxyl group.
[0037] In this embodiment, at least one nitrogen atom contained in the nitrogen-containing heteroaromatic ring skeleton of Component C forms an N-oxide. In one or more embodiments, the nitrogen-containing heteroaromatic ring contained in Component C may be a monocyclic or bicyclic condensed ring. In one or more embodiments, the number of nitrogen atoms in the nitrogen-containing heteroaromatic ring contained in Component C may be 1 to 3, and from the viewpoint of improving the polishing rate, 1 or 2 is preferable, and 1 is more preferable. In one or more embodiments, the nitrogen-containing heteroaromatic ring skeleton contained in component C may be at least one selected from a pyridine N-oxide skeleton, a quinoline N-oxide skeleton, and the like. In the present disclosure, the pyridine N-oxide skeleton refers to a structure in which a nitrogen atom contained in a pyridine ring forms an N-oxide. The quinoline N-oxide skeleton refers to a structure in which a nitrogen atom contained in a quinoline ring forms an N-oxide.
[0038] In one or more embodiments, Component C may be at least one selected from an N-oxide compound having a pyridine ring in which at least one hydrogen atom is substituted with a hydroxyl group, an N-oxide compound having a quinoline ring in which at least one hydrogen atom is substituted with a hydroxyl group, and salts thereof. Among these, from the viewpoint of improving the polishing rate, Component C is preferably an N-oxide compound having a pyridine ring in which at least one hydrogen atom of the pyridine ring is substituted with a hydroxyl group, or a salt thereof. In one or more embodiments, component C includes 2-hydroxypyridine N-oxide.
[0039] The content of component C in the polishing liquid composition of the present disclosure is preferably 0.0001 mass% or more, more preferably 0.001 mass% or more, more preferably 0.006 mass% or more, and even more preferably 0.01 mass% or more, from the viewpoint of improving the polishing rate, and from the same viewpoint, it is preferably 1 mass% or less, more preferably 0.5 mass% or less, more preferably 0.1 mass% or less, and even more preferably 0.06 mass% or less. The content of component C in the polishing liquid composition of the present disclosure is preferably 0.0001 mass% or more and 1 mass% or less, more preferably 0.001 mass% or more and 0.5 mass% or less, more preferably 0.006 mass% or more and 0.1 mass% or less, and even more preferably 0.01 mass% or more and 0.06 mass% or less. When component C is a combination of two or more kinds, the content of component C refers to the total content thereof.
[0040] The mass ratio (A+B) / C of the total of components A and B to component C (the total content of components A and B / the content of component C) in the polishing liquid composition of the present disclosure is, from the viewpoint of improving the polishing rate, preferably 0.1 or more, more preferably 10 or more, even more preferably 25 or more, and even more preferably 50 or more, and from the same viewpoint, preferably 6000 or less, more preferably 600 or less, even more preferably 300 or less, and even more preferably 200 or less. The mass ratio A / B in the polishing liquid composition of the present disclosure is preferably 0.1 or more and 6000 or less, more preferably 10 or more and 600 or less, even more preferably 25 or more and 300 or less, and even more preferably 50 or more and 200 or less.
[0041] [Optional ingredients] The polishing liquid composition of the present disclosure may further contain optional components such as pH adjusters, surfactants, thickeners, dispersants, rust inhibitors, preservatives, basic substances, polishing rate enhancers, silicon nitride film polishing inhibitors, polysilicon film polishing inhibitors, and counter ions. When the polishing liquid composition of the present disclosure further contains optional components, the content of the optional components in the polishing liquid composition of the present disclosure is preferably 0.001 mass% or more, more preferably 0.0025 mass% or more, even more preferably 0.01 mass% or more, and preferably 1 mass% or less, more preferably 0.5 mass% or less, and even more preferably 0.1 mass% or less, from the viewpoint of improving the polishing rate. The content of the optional components in the polishing liquid composition of the present disclosure is preferably 0.001 mass% or more and 1 mass% or less, more preferably 0.0025 mass% or more and 0.5 mass% or less, and even more preferably 0.01 mass% or more and 0.1 mass% or less.
[0042] The polishing fluid composition of the present disclosure, in one or more embodiments, may be free of functionalized pyridine, benzoic acid, amino acid, or combinations thereof.
[0043] [Polishing liquid composition] The polishing liquid composition of the present disclosure can be produced, for example, by a production method including a step of blending component A, component B, and an aqueous medium, and, if desired, the above-mentioned component C and any optional components, by a known method. For example, the polishing liquid composition of the present disclosure can be produced by blending at least component A, component B, and an aqueous medium. When component A and / or component B are a combination of multiple types of cerium oxide particles, component A and / or component B can be obtained by blending multiple types of cerium oxide particles, respectively. When component C is a combination of multiple types of N-oxide compounds, component C can be obtained by blending multiple types of N-oxide compounds, respectively. In the present disclosure, "blending" includes mixing component A, component B, and the aqueous medium, and, if necessary, the above-mentioned component C and any optional components simultaneously or in sequence. The order of mixing is not particularly limited. The blending can be performed using a mixer such as a homomixer, a homogenizer, an ultrasonic disperser, or a wet ball mill. The blending amount of each component in the method for producing the polishing liquid composition of the present disclosure can be the same as the content of each component in the above-mentioned polishing liquid composition of the present disclosure.
[0044] The embodiment of the polishing liquid composition of the present disclosure may be a so-called one-liquid type in which all components are supplied to the market in a pre-mixed state, or a so-called two-liquid type in which the components are mixed at the time of use. One embodiment of the two-liquid type polishing liquid composition is composed of a first liquid containing component A and a second liquid containing component B, and the first liquid and the second liquid are mixed at the time of use. The first liquid and the second liquid may be mixed before being supplied to the surface of the object to be polished, or they may be supplied separately and mixed on the surface of the substrate to be polished. The first liquid and the second liquid may each contain the above-mentioned component C and optional components as necessary.
[0045] From the viewpoint of improving the polishing rate, the pH of the polishing liquid composition of the present disclosure is 3 or more, preferably 3.5 or more, more preferably 4 or more, even more preferably 4.5 or more, and 9 or less, preferably 8.5 or less, more preferably 8 or less, even more preferably less than 8, even more preferably 7 or less, and even more preferably 6 or less. The pH of the polishing liquid composition of the present disclosure is 3 or more and 9 or less, preferably 3.5 or more and 9 or less, more preferably 4 or more and 8.5 or less, even more preferably 4.5 or more and 8 or less, even more preferably 4.5 or more and 7 or less, and even more preferably 4.5 or more and 6 or less. In the present disclosure, the pH of the polishing liquid composition is a value at 25°C, and can be measured using a pH meter, and can be measured by the method described in the Examples.
[0046] In the present disclosure, "the content of each component in the polishing liquid composition" refers to the content of each component at the time of polishing, that is, at the time when the polishing liquid composition is started to be used for polishing. The polishing liquid composition of the present disclosure may be stored and supplied in a concentrated state within a range in which its stability is not impaired. In this case, it is preferable in that the manufacturing and transportation costs can be reduced. And, this concentrated liquid can be appropriately diluted with water as necessary and used in the polishing process. The dilution ratio is preferably 5 to 100 times.
[0047] [Polished film] Examples of films to be polished using the polishing composition of the present disclosure include silicon oxide films. Therefore, the polishing composition of the present disclosure can be used in a process that requires the polishing of a silicon oxide film. That is, in one or more embodiments, the polishing composition of the present disclosure is a polishing composition used for polishing a silicon oxide film (polishing composition for silicon oxide films). In one or more embodiments, the polishing composition of the present disclosure can be suitably used for polishing a silicon oxide film performed in a process for forming an element isolation structure of a semiconductor substrate, polishing a silicon oxide film performed in a process for forming an interlayer insulating film, polishing a silicon oxide film performed in a process for forming embedded metal wiring, or polishing a silicon oxide film performed in a process for forming an embedded capacitor. In one or more other embodiments, the polishing composition of the present disclosure can be suitably used for manufacturing a three-dimensional semiconductor device such as a three-dimensional NAND flash memory.
[0048] [Polishing liquid kit] In another aspect, the present disclosure relates to a kit for producing the polishing liquid composition of the present disclosure (hereinafter also referred to as the "polishing liquid kit of the present disclosure"). The polishing liquid kit of the present disclosure may be, for example, a polishing liquid kit (two-liquid type polishing liquid composition) that contains a polishing abrasive dispersion containing component A, component B, and an aqueous medium, and an aqueous solution containing other components (component C or optional components) in a mutually unmixed state. The polishing abrasive dispersion and the additive aqueous solution are mixed at the time of use, and diluted with an aqueous medium as necessary. The aqueous medium contained in the polishing abrasive dispersion may be the entire amount of the aqueous medium used to prepare the polishing liquid composition, or may be a part of the aqueous medium. The additive aqueous solution may contain a part of the aqueous medium used to prepare the polishing liquid composition. The polishing abrasive dispersion and the additive aqueous solution may each contain the above-mentioned optional components as necessary. According to the polishing liquid kit of the present disclosure, a polishing liquid composition can be obtained that can improve polishing selectivity while ensuring the polishing rate.
[0049] [Polishing method] In one aspect, the present disclosure relates to a polishing method (hereinafter also referred to as the "polishing method of the present disclosure") that includes a step of polishing a film to be polished using the polishing liquid composition of the present disclosure, the film to be polished being a silicon oxide film formed in the manufacturing process of a semiconductor substrate. By using the polishing method of the present disclosure, it is possible to improve the polishing speed of the silicon oxide film, and therefore it is possible to achieve an effect of improving the productivity of semiconductor substrates with improved quality. The polishing method and conditions in the polishing method of the present disclosure can be the same as those in the manufacturing method of a semiconductor substrate of the present disclosure described below.
[0050] [Method of manufacturing semiconductor substrate] In one aspect, the present disclosure relates to a method for producing a semiconductor substrate, comprising a step of polishing a silicon oxide film with the polishing composition of the present disclosure (polishing step). In one aspect, the present disclosure relates to a method for producing a semiconductor substrate, comprising a step of polishing a silicon oxide film using the polishing method of the present disclosure (polishing step). In the present disclosure, the term "the method for manufacturing a semiconductor substrate according to the present disclosure" can refer to the above two aspects. According to the method for manufacturing a semiconductor substrate of the present disclosure, it is possible to improve the polishing speed of a silicon oxide film, and therefore it is possible to achieve the effect of efficiently manufacturing semiconductor substrates with improved quality.
[0051] In one or more embodiments of the method for manufacturing a semiconductor substrate of the present disclosure, a silicon substrate is first exposed to oxygen in an oxidation furnace to grow a silicon dioxide layer on the surface of the substrate, and then a silicon nitride (Si 3 N 4 A polishing stopper film such as a silicon dioxide film or a polysilicon film is formed by, for example, a CVD method (chemical vapor deposition method). Next, a trench is formed by photolithography in a substrate including a silicon substrate and a polishing stopper film disposed on one main surface side of the silicon substrate, for example, a substrate in which a polishing stopper film is formed on a silicon dioxide layer of a silicon substrate. Next, a silicon dioxide (SiO 2) film is formed, and a substrate to be polished in which the polishing stopper film is covered with the polishing film (silicon oxide film) is obtained. By forming the silicon oxide film, the trench is filled with silicon oxide of the silicon oxide film, and the surface of the polishing stopper film opposite to the surface on the silicon substrate side is covered with the silicon oxide film. The surface opposite to the surface on the silicon substrate side of the silicon oxide film thus formed has a step formed corresponding to the unevenness of the lower layer. Next, the silicon oxide film is polished by the CMP method until at least the surface opposite to the surface on the silicon substrate side of the polishing stopper film is exposed, and more preferably, the silicon oxide film is polished until the surface of the silicon oxide film and the surface of the polishing stopper film are flush with each other. The polishing liquid composition of the present disclosure can be used in the step of performing polishing by this CMP method. The width of the convex portion formed corresponding to the unevenness of the lower layer of the silicon oxide film is, for example, 0.5 μm to 5000 μm, and the width of the concave portion is, for example, 0.5 μm to 5000 μm.
[0052] In polishing by the CMP method, the surface of the substrate to be polished is brought into contact with a polishing pad, and the substrate to be polished and the polishing pad are moved relative to each other while the polishing liquid composition of the present disclosure is supplied to the contact site, thereby flattening the uneven portions of the surface of the substrate to be polished. In the semiconductor substrate manufacturing method of the present disclosure, another insulating film may be formed between the silicon dioxide layer of the silicon substrate and the polishing stopper film, or another insulating film may be formed between the film to be polished (e.g., a silicon oxide film) and the polishing stopper film (e.g., a silicon nitride film).
[0053] In the polishing step, the rotation speed of the polishing pad is, for example, 30 to 200 r / min, the rotation speed of the substrate to be polished is, for example, 30 to 200 r / min, and the polishing load set in the polishing apparatus equipped with the polishing pad is, for example, 20 to 500 gf / cm. 2 The supply rate of the polishing composition can be set to, for example, 10 to 500 mL / min or less. When the polishing composition is a two-liquid type polishing composition, the polishing rates of the polishing target film and the polishing stopper film, and the polishing rate ratio (polishing selectivity) between the polishing target film and the polishing stopper film can be adjusted by adjusting the supply rates (or supply amounts) of the first liquid and the second liquid.
[0054] In the polishing step, the polishing rate of the film to be polished (silicon oxide film) is preferably 50 nm / min or more, more preferably 80 nm / min or more, and even more preferably 90 nm / min or more, from the viewpoint of improving productivity. EXAMPLES
[0055] The present disclosure will be described in more detail below with reference to examples, but these are merely illustrative and the present disclosure is not limited to these examples.
[0056] 1.Measuring methods for each parameter (1) pH of the polishing composition The pH value of the polishing composition at 25°C was measured using a pH meter (manufactured by Toa Denpa Kogyo Co., Ltd., "HM-30G"), and was the value measured one minute after the pH meter electrode was immersed in the polishing composition.
[0057] (2) Measurement method for D50 and D99 of cerium oxide particles by centrifugal sedimentation method (CPS measurement) Cerium oxide particles were diluted with ion-exchanged water to prepare a dispersion containing 0.4% by mass of cerium oxide particles, and the particle size distribution was measured by centrifugal sedimentation using the following measuring device. The particle sizes at which the cumulative frequency from the small diameter side in the particle size distribution in weight conversion obtained by centrifugal sedimentation was 50% and 99%, respectively, were defined as D50 and D99. The D50 of component A and component B were defined as their average particle sizes. <Measurement conditions> Measurement device: CPS DC24000 UHR manufactured by CPS Instruments Measurement range: 0.02 to 3 μm Particle extinction coefficient: 0.1 Particle shape factor: 1.2 or 1.0 Revolution speed: 17,000 rpm Calibration standard particle size: 0.476μm Standard particle density: 1.0465 (13%, 34℃) Density gradient solution: Sucrose aqueous solution (8%, 24%) Solvent viscosity: 1.16cp (13%, 34℃) Refractive index of solvent: 1.3592 (18%, 34°C) Measurement temperature: 15~45℃ Measurement time: 3 to 420 minutes
[0058] (3) Density of cerium oxide particles The cerium oxide particles were dried for 2 hours at 400°C using a hot stirrer (As One, CERAMIC HOT PLATE CHP-170DF), and then fired for 1 hour at 650°C using an electric furnace (Furutech, FT-101).Then, the density of the sample was measured using a fully automatic pycnometer (Quantachrome, ULTRAPYC 1200e).
[0059] (4) Reduction potential and oxidation potential 1) Prepare an aqueous solution of sodium sulfate to be used as a supporting electrolyte at 0.1 mol / L using ultrapure water, and replace with nitrogen for at least 3 hours. 2) Weigh out 9.9 mL of sodium sulfate solution into a glass vial (20 mL). 3) The surface of the glassy carbon working electrode is polished thoroughly using a 1 μm polishing diamond and diamond polishing pad (both manufactured by BAS) by pressing the electrode vertically and drawing a figure 8. Next, using a 0.05 μm alumina and alumina polishing pad (both manufactured by BAS), the electrode surface is polished thoroughly by drawing a figure 8 until it becomes a mirror surface. After that, the electrode surface is washed with ultrapure water and dried. 4) Connect the glassy carbon electrode, the silver / silver-silver chloride reference electrode, and the platinum counter electrode to an ALS electrochemical analyzer (Model 611D) and immerse it in the sodium sulfate aqueous solution to assemble a three-electrode electrochemical cell. 5) Set the cyclic voltammetry variables as follows: high potential 1 V, low potential 1 V, scan rate 0.1 V / s, sweep segment 5 w, and display the potential-current data points on the monitor. 6) After thoroughly replacing the nitrogen gas in the glass vial by inserting a Teflon tube into the vial, the measurement is performed using only the supporting electrolyte. If the nitrogen replacement is insufficient, a peak due to dissolved oxygen will be detected. 7) A measurement sample (additive: 1000 ppm) was prepared in ultrapure water and thoroughly substituted with nitrogen. After that, 0.1 mL of the measurement sample was added to 9.9 mL of an aqueous sodium sulfate solution in a glass vial to obtain a 10 ppm aqueous solution of the additive. 8) Measure the open circuit potential, set it as the initial potential of the cyclic voltammetry variable, and perform the measurement. At this time, confirm that no peaks due to dissolved oxygen are detected, and confirm the redox potential from the cyclic voltammogram derived from the measurement sample.
[0060] 2. Preparation of Polishing Composition (Examples 1 to 7 and Comparative Examples 1 to 13) Cerium oxide particles (component A, component B), an additive (component C), and water were mixed to obtain polishing liquid compositions of Examples 1 to 7 and Comparative Examples 1 to 13. The content of each component in the polishing liquid composition is as shown in Tables 1 to 3. The content of water is the remainder excluding components A, B, and C. The pH of the polishing liquid compositions of Examples 1 to 7 and Comparative Examples 1 to 13 was 5. The pH was adjusted using ammonia or nitric acid.
[0061] Component A, component B, and component C used in preparing the polishing compositions of Examples 1 to 7 and Comparative Examples 1 to 13 are shown below. [Component A] Cerium oxide particles A1: particle size 26nm, density 9g / cm 3 , calcined cerium oxide Cerium oxide particles A2: particle size 53nm, density 7.6g / cm 3 , wet cerium oxide (colloidal ceria), "HC-30" manufactured by Solvay SpecialChem Japan Cerium oxide particles A3: particle size 76nm, density 7.9g / cm 3 , calcined cerium oxide [Component B] Cerium oxide particles b1: particle size 97nm, density 7.4g / cm 3 , calcined cerium oxide Cerium oxide particles b2: particle size 111nm, density 6.9g / cm 3, wet cerium oxide (colloidal ceria), "HC-60" manufactured by Solvay SpecialChem Japan [Component C] 2-Hydroxypyridine N-oxide (Tokyo Chemical Industry Co., Ltd., reduction potential: 0.87 V)
[0062] Method for producing calcined cerium oxide The calcined cerium oxide particles a1, a3, and b1 were produced by calcining a cerium compound. In addition, the shapes of the calcined cerium oxide particles a1, a3, and b1 were observed with a scanning electron microscope (SEM), and as a result, the particles a1 and a3 were polyhedral, and the particle b1 was irregular.
[0063] Wet Cerium Oxide The wet cerium oxide particles a2 and b2 were found to have a polyhedral shape as a result of observation with a scanning electron microscope (SEM).
[0064] 3. Evaluation of polishing composition [Measurement of polishing speed] The workpiece was an 8-inch silicon wafer with SiO 2 A plain film substrate was prepared, on whose entire surface a film was formed to a thickness of 2000 nm. A polishing device (Ebara Corporation, F-REX200) and polishing pads (Nitta Haas, upper layer: IC1000, lower layer: SUBA400) were used. The polishing conditions were: processing pressure: 3 psi (288 gf / cm 2 ), polishing composition flow rate: 200 ml / min, polishing head rotation speed: 107 rpm, platen rotation speed: 100 rpm, polishing time: 60 seconds. Next, the polishing rate (polishing speed) per minute was calculated from the amount of reduction in the thickness of the workpiece before and after polishing using an optical interference film thickness measuring device (Nanospec 6100 manufactured by Nano Metrics).
[0065] Tables 1 and 2 show the results of polishing using a polishing composition in which the total concentration of cerium oxide particles (component A and component B) in the polishing composition was 0.5 mass %.
[0066] [Table 1]
[0067] [Table 2]
[0068] Table 3 shows the results of polishing using a polishing composition in which the total concentration of cerium oxide particles (component A and component B) in the polishing composition was 1.5 mass %.
[0069] [Table 3]
[0070] As shown in Table 1, the polishing compositions of Examples 1 and 2 had improved removal rates compared to the polishing compositions of Comparative Examples 1-6. As shown in Table 2, the polishing compositions of Examples 3 and 4 had improved removal rates compared to the polishing compositions of Comparative Examples 7 to 9. As shown in Table 3, the polishing compositions of Examples 5 to 7 had improved polishing rates compared to the polishing compositions of Comparative Examples 10 to 13. Furthermore, the polishing compositions of Examples 6 and 7, which contained the additive (component C), had improved polishing rates compared to the polishing composition of Example 5, which did not contain the additive (component C). [Industrial Applicability]
[0071] The polishing composition of the present disclosure is useful in a method for producing semiconductor substrates for high density or high integration.
Claims
1. A polishing composition for silicon oxide films, comprising cerium oxide particles and an aqueous medium, As cerium oxide particles, The average particle size is 15 nm or more and 50 nm or less, and the density is 8 g / cm 3 The above cerium oxide particles (component A), and Contains cerium oxide particles (component B) having an average particle size of 60 nm or more and 1 μm or less, The pH is 3 or more and 9 or less, A polishing composition, in which the value of D50 / D99 is 0.32 or less, when D50 and D99 are the particle sizes at which the cumulative frequency from the small particle size side is 50% and 99%, respectively, in a particle size distribution calculated on a weight basis obtained by centrifugal sedimentation of a mixture of components A and B.
2. Component A has an average particle size of 20 nm or more and 50 nm or less and a density of 8.5 g / cm 3 10g / cm or more 3 2. The polishing composition according to claim 1, wherein the cerium oxide particles are:
3. 3. The polishing composition according to claim 1, wherein component A is calcined cerium oxide particles.
4. 4. The polishing composition according to claim 1, wherein a weight ratio (A / B) of the content of component A to the content of component B in the polishing composition is 1 / 6 or more and 4 / 1 or less.
5. The density of component B is 6 g / cm 3 8g / cm or more 3 The polishing composition according to claim 1 , wherein the abrasive grain size is less than 100 nm.
6. 6. The polishing composition according to claim 1, wherein the total content of Component A and Component B in the polishing composition is 0.3 mass % or more and 2 mass % or less.
7. 7. The polishing composition according to claim 1, wherein the value of D50 / D99 is 0.1 or more and 0.25 or less.
8. The polishing composition according to any one of claims 1 to 7, further comprising a compound (component C) having a reduction potential of 0.45 V or more and 0.95 V or less when a 10 ppm aqueous solution is measured by cyclic voltammetry (Ag / AgCl electrode standard).
9. 9. The polishing composition according to claim 8, wherein component C is at least one selected from the group consisting of an N-oxide compound having a pyridine ring in which at least one hydrogen atom is substituted with a hydroxyl group, an N-oxide compound having a quinoline ring in which at least one hydrogen atom is substituted with a hydroxyl group, and salts thereof.
10. 10. A polishing method comprising the step of polishing a film to be polished with the polishing composition according to claim 1, wherein the film to be polished is a silicon oxide film formed in the course of manufacturing a semiconductor substrate.
11. A method for producing a semiconductor substrate, comprising a step of polishing a film to be polished with the polishing composition according to claim 1 .
Citation Information
Patent Citations
Abrasive slurry for glass
JP2010059310A
JP2011-545995A
Cerium oxide abrasive and polishing method of substrate using the same
JP2011224751A
Mixed abrasive polishing composition
JP2016538359A
Selective nitride slurry with improved stability and improved polishing properties
JP2018534379A