Soft magnetic metal powder, soft magnetic metal sintered body, and coil-type electronic component

A soft magnetic metal powder with controlled Fe-Ni-Si-M alloy composition and Si-containing oxide coating, combined with resin filling, addresses the challenges of high magnetic permeability and resistance, achieving enhanced inductance and Q values in coil-type electronic components.

JP7569795B2Active Publication Date: 2024-10-18TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021549051
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-26
Filing Date
2020-09-25
Publication Date
2024-10-18
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

Existing soft magnetic materials face challenges in achieving high magnetic permeability and specific resistance while maintaining high inductance and Q values, and are prone to plating elongation and short circuits.

Method used

The development of a soft magnetic metal powder composed of Fe-Ni-Si-M alloy with controlled compositions and particle sizes, coated with a Si-containing oxide film, and filled with resin to form a magnetic element, which enhances magnetic properties and resistance to plating elongation.

Benefits of technology

The solution results in a soft magnetic metal fired body with improved magnetic permeability, specific resistance, and high inductance and Q values, while reducing the likelihood of plating elongation and short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569795000015
    Figure 0007569795000015
  • Figure 0007569795000016
    Figure 0007569795000016
  • Figure 0007569795000017
    Figure 0007569795000017
Patent Text Reader

Abstract

[Problem] To provide a soft magnetic metal powder or the like from which a soft magnetic metal fired body can be provided which has a high magnetic permeability μ and a specific resistance ρ and is contained in a coil-type electronic component having sufficiently high inductance L and Q value and unlikely to be plating-extended and short-circuited. [Solution] Provided is a soft magnetic metal powder containing soft magnetic metal particles containing at least Fe and Ni. Said soft magnetic metal powder further contains P, Si, Cr and / or M. M is at least one selected from among B, Co, Mn, Ti, Zr, Hf, Nb, Ta, Mo, Mg, Ca, Sr, Ba, Zn, Al, and rare earth elements. The content of each element is within a predetermined range.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a soft magnetic metal powder, a sintered soft magnetic metal body, and a coil-type electronic component. [Background technology]

[0002] Patent Document 1 describes an invention relating to a laminated coil, which is characterized in that the gaps between Fe-Si-Cr alloy particles in the magnetic body are impregnated with resin.

[0003] Patent Document 2 describes an invention related to a soft magnetic alloy powder, which is characterized by containing Fe-Ni based particles in which the contents of Fe, Ni, Co and Si are each controlled within a specific range. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-238840 A [Patent Document 2] JP 2008-135674 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a soft magnetic metal powder etc. that can provide a soft magnetic metal sintered body having high magnetic permeability μ and resistivity ρ and that can be used in coil-type electronic components that have sufficiently high inductance L and Q value, are less susceptible to plating elongation and are less susceptible to short circuits. [Means for solving the problem]

[0006] The soft magnetic metal powder according to the first aspect of the present invention is A soft magnetic metal powder containing soft magnetic metal particles composed of an Fe-Ni-Si-M alloy, The Fe-Ni-Si-M alloy further contains P, M is one or more selected from B, Co, Mn, Ti, Zr, Hf, Nb, Ta, Mo, Mg, Ca, Sr, Ba, Zn, Al and rare earth elements; The Fe-Ni-Si-M alloy contains Ni in an amount of 15.0 mass% or more and 55.0 mass% or less, Si in an amount of 2.0 mass% or more and 6.0 mass% or less, M in an amount of 2.0 mass% or more and 40.0 mass% or less, and P in an amount of 100 ppm or more and 5000 ppm or less, where the total content of Fe, Ni, Si, and M is 100 mass%.

[0007] The soft magnetic metal powder according to the second aspect of the present invention is A soft magnetic metal powder containing soft magnetic metal particles composed of an Fe-Ni alloy, The Fe-Ni alloy further contains Cr, The Fe-Ni alloy further contains Si and / or M, M is one or more selected from B, Co, Mn, Ti, Zr, Hf, Nb, Ta, Mo, Mg, Ca, Sr, Ba, Zn, Al and rare earth elements; The Fe—Ni based alloy contains less than 2.0 mass % of Cr, with the total content of Fe, Ni, Si, M and Cr being 100 mass %.

[0008] The Fe-Ni alloy may further contain P, The Fe—Ni based alloy may contain P in an amount of 100 ppm or more and 5000 ppm or less, with the total content of Fe, Ni, Si, M and Cr being 100 mass %.

[0009] The following description is common to the soft magnetic alloy powder according to the first aspect and the soft magnetic metal powder according to the second aspect.

[0010] M may be Co.

[0011] The soft magnetic metal powder may have an average particle size (D50) of 1.5 μm or more and 15.0 μm or less.

[0012] The sintered soft magnetic metal body according to the first and second aspects of the present invention contains the soft magnetic metal powder according to the first and second aspects.

[0013] A sintered soft magnetic metal body containing the above-mentioned soft magnetic metal powder tends to have high magnetic permeability μ and resistivity ρ.

[0014] A coil-type electronic component according to a first and second aspect of the present invention is a coil-type electronic component having a magnetic base body and a coil conductor built into the magnetic base body, The magnetic body is made of the sintered soft magnetic metal body according to the first or second aspect.

[0015] A coil-type electronic component whose magnetic body is made of the above-mentioned sintered soft magnetic metal body has sufficiently high inductance L and Q value, and is less susceptible to plating extension and short circuits.

[0016] The soft magnetic metal particles may be covered with a coating film, The layer of the coating film that is in contact with the soft magnetic metal particles may contain Si or an oxide containing Si.

[0017] The layer of the coating film that is in contact with the soft magnetic metal particles may further contain P.

[0018] The coating film may have an average thickness of 5 nm or more and 60 nm or less.

[0019] A coil-type electronic component according to a third aspect of the present invention comprises: A coil-type electronic component having a magnetic body and a coil conductor built into the magnetic body, The magnetic body includes soft magnetic metal particles, The Cr content in the soft magnetic metal particles is less than 2.0% by mass (not including 0% by mass), The soft magnetic metal particles are covered with a coating film, the coating film comprises a first layer in contact with the soft magnetic metal particles and a second layer in contact with the first layer, the first layer includes Si or an oxide including Si; The second layer contains Cr.

[0020] The first layer may have an average thickness D1, the second layer may have an average thickness D2, and the relationship may be 0.5≦D2 / D1≦1.5.

[0021] D2 may be 2.5 nm or more and 30 nm or less.

[0022] The following description is common to all of the coil-type electronic components described above.

[0023] The magnetic body may include soft magnetic metal particles and a resin, The resin may fill interstitial spaces between the soft magnetic metal particles.

[0024] The resin may be a phenolic resin or an epoxy resin. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 shows a laminated coil according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of the magnetic body. [Diagram 3] FIG. 3 is an SEM image of the interlayer portion in Example 103. [Figure 4] FIG. 4 is an SEM image of the interlayer portion in Example 104. [Diagram 5] FIG. 5 is a BF image in Example 103. [Figure 6] FIG. 6 is a BF image in Example 103. [Figure 7] FIG. 7 is a C mapping image in Example 103. [Figure 8] FIG. 8 is a C mapping image in Example 103. [Figure 9] FIG. 9 is a Si mapping image in Example 103. [Figure 10] FIG. 10 is a Si mapping image in Example 103. [Figure 11] FIG. 11 is an O mapping image in Example 103. [Figure 12] FIG. 12 is an O mapping image in Example 103. [Figure 13] FIG. 13 is a schematic cross-sectional view of a soft magnetic metal particle in a magnetic body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Hereinafter, the present invention will be described based on the embodiments shown in the drawings.

[0027] <Soft magnetic metal powder> (First embodiment) The soft magnetic metal powder according to the first embodiment is an aggregate of a plurality of soft magnetic metal particles. The soft magnetic metal particles are composed of an Fe-Ni-Si-M alloy. The Fe-Ni-Si-M alloy further contains P. M is at least one selected from B, Co, Mn, Ti, Zr, Hf, Nb, Ta, Mo, Mg, Ca, Sr, Ba, Zn, Al, and rare earth elements. It is preferable that M is Co. In this embodiment, in the Fe-Ni-Si-M alloy, the total content of Fe, Ni, Si, and M is 100 mass%, and the contents of the other elements, except for P and O, may be 0.15 mass% or less. The content of O may be 0.5 mass% or less. The content of Cr may be less than 0.1 mass% or 0.03 mass% or less.

[0028] The Ni content is from 15.0 to 55.0 mass%, the Si content is from 2.0 to 6.0 mass%, and the M content is from 2.0 to 40.0 mass%. Furthermore, the P content is from 100 to 5000 ppm, that is, from 0.0100 to 0.5000 mass%.

[0029] The Ni content may be 22.0 mass% or more and 42.0 mass% or less. The Si content may be 2.5 mass% or more and 5.5 mass% or less, or 2.5 mass% or more and 4.0 mass% or less. The M content may be 5.0 mass% or more and 32.0 mass% or less. The P content may be 300 ppm or more and 2000 ppm or less.

[0030] By producing a soft magnetic metal sintered body using soft magnetic metal powder composed of soft magnetic metal particles having the above composition, it is possible to obtain a soft magnetic metal sintered body having a high magnetic permeability μ and resistivity ρ compared to a case in which a soft magnetic metal sintered body is produced using soft magnetic metal powder composed of soft magnetic metal particles that do not have the above composition.

[0031] In particular, if the Si content is too low, the resistivity tends to decrease because it becomes difficult to properly maintain the oxidation state of the soft magnetic metal particles after heat treatment.

[0032] The average particle diameter (D50) of the soft magnetic metal powder according to this embodiment may be 1.5 μm or more and 15.0 μm or less, 2.0 μm or more and 15.0 μm or less, or 5.0 μm or more and 10.0 μm or less. By setting the average particle diameter of the soft magnetic metal powder within the above range, it becomes easier to obtain a soft magnetic metal sintered body having high magnetic permeability μ and resistivity ρ. There is no particular limit to the method of measuring the average particle diameter (D50). For example, a laser diffraction scattering method may be used. The shape of the soft magnetic metal particles constituting the soft magnetic metal powder is not particularly limited.

[0033] <Soft magnetic metal sintered body> The sintered soft magnetic metal body according to the present embodiment has a configuration in which a plurality of soft magnetic metal particles are connected to each other by sintering. Specifically, elements contained in the soft magnetic metal particles that are in contact with each other react with other elements (e.g., O) by sintering, and a plurality of soft magnetic metal particles are connected to each other through bonds resulting from the reaction. In the sintered soft magnetic metal body according to the present embodiment, the soft magnetic metal particles derived from the soft magnetic metal powder are connected to each other by heat treatment, but the grain growth of each soft magnetic metal particle is almost not observed. In other words, the particle diameter of each soft magnetic metal particle is almost unchanged.

[0034] The particle diameter of the soft magnetic metal particles contained in the soft magnetic metal sintered body may be calculated by calculating the area of ​​the soft magnetic metal particles through image analysis of the cross section of the soft magnetic metal sintered body using SEM, STEM, etc., and calculating the diameter of a circle equivalent to that area (equivalent circle diameter).

[0035] The composition and particle size of the soft magnetic metal particles contained in the sintered soft magnetic metal are the same as the composition of the soft magnetic metal powder described above, except for the content of O. The content of O may be 0.5 mass % or less.

[0036] <Coil-type electronic components> The coil-type electronic component according to the present embodiment may be a laminated coil-type electronic component. The coil-type electronic component according to the present embodiment may be, for example, the laminated coil shown in FIG.

[0037] As shown in FIG. 1, the laminated coil 1 according to this embodiment has an element 2 and a terminal electrode 3. The element 2 has a configuration in which a coil conductor 5 is embedded three-dimensionally and spirally inside a magnetic base body 4. Terminal electrodes 3 are formed on both ends of the element 2, and the terminal electrodes 3 are connected to the coil conductor 5 via lead electrodes 5a, 5b. The element 2 also comprises a central portion 2b in which the coil conductor 5 is embedded, and surface portions 2a that are present above and below the central portion 2b in the stacking direction (z-axis direction) and in which the coil conductor 5 is not embedded. In this embodiment, the intermediate portions between the coil conductors 5 in the stacking direction of the magnetic base body 4 are referred to as interlayer portions 4a.

[0038] The element 2 may have any shape, but is usually rectangular. There are no particular limitations on its dimensions, and it may be of appropriate dimensions depending on the application. For example, it may be 0.2 to 2.5 mm×0.1 to 2.0 mm×0.1 to 1.2 mm.

[0039] The material of the terminal electrode 3 is not particularly limited as long as it is an electrical conductor. For example, Ag, Cu, Au, Al, Ag alloy, Cu alloy, etc. are used. In particular, Ag is preferably used because it is inexpensive and has low resistance. The terminal electrode 3 may contain glass frit. The terminal electrode 3 may have a two-layer structure of a metal layer formed on the element 2 and made of the above metal or the above metal and glass frit, and a resin layer formed on the metal layer and made of a conductive resin. There is no particular limit to the type of metal contained in the conductive resin. For example, Ag can be used. The terminal electrode 3 may have a surface plated. For example, Cu plating, Ni plating, and / or Sn plating may be appropriately applied.

[0040] The coil conductor 5 and the lead electrodes 5a and 5b can be made of any material that is an electrical conductor. For example, Ag, Cu, Au, Al, Ag alloys, Cu alloys, etc. are used. In particular, Ag is preferably used because it is inexpensive and has low resistance.

[0041] The magnetic element 4 may be made of soft magnetic metal particles 11 and resin 13 as shown in FIG. 2. The presence of resin 13 makes it easier to increase the inductance L and Q value. Furthermore, the laminated coil is less likely to short out. FIG. 2 is a schematic cross-sectional view of the magnetic element 4. The portions of the magnetic element 4 other than the soft magnetic metal particles 11 are defined as gap spaces 12. The gap spaces 12 are filled with resin 13, and the portions not filled with resin 13 are voids 14. Before filling with resin, all of the gap spaces 12 are voids 14.

[0042] The soft magnetic metal particles 11 may be covered with a coating film. Specifically, as shown in FIG. 13, the soft magnetic metal particles 11 may be composed of a soft magnetic metal particle body 11a and an oxide coating film 11b that coats the soft magnetic metal particle body 11a. Furthermore, the oxide coating film 11b that coats the soft magnetic metal particle body 11a according to this embodiment preferably includes a layer made of an oxide containing Si, and it is preferable that the soft magnetic metal particle body 11a and the layer made of an oxide containing Si are in contact with each other. When the oxide coating film 11b that coats the soft magnetic metal particle body 11a includes a layer made of an oxide containing Si, the insulation between the soft magnetic metal particles 11 is increased, thereby improving the Q value. Furthermore, when the oxide coating film 11b that coats the soft magnetic metal particle body 11a includes a layer made of a compound containing Si, it is also possible to prevent the formation of an oxide of Fe.

[0043] The soft magnetic metal particle body 11a is composed of the above-mentioned Fe-Ni-Si-M alloy. In particular, when the P content is within a predetermined range, it is considered that the oxidation state of the soft magnetic metal grains 11 constituting the magnetic element body 4 after the heat treatment, that is, the coverage and thickness of the oxide film 11b, etc., can be appropriately controlled. When the layer made of the oxide containing Si further contains P, the coverage and thickness of the oxide film 11b can be more appropriately controlled. As a result, the magnetic element body 4 after the heat treatment exhibits high resistivity and can exhibit predetermined magnetic properties. Therefore, the magnetic element body 4 according to this embodiment is suitable as a magnetic element body that comes into direct contact with the coil conductor 5.

[0044] The type of resin 13 is arbitrary. It may be a phenolic resin or an epoxy resin. When the resin 13 is a phenolic resin or an epoxy resin, the resin 13 is particularly likely to fill the gap space 12. In addition, it is preferable that the resin 13 is a phenolic resin because it is inexpensive and easy to handle.

[0045] Filling the gap spaces 12 with the resin 13 increases the strength (particularly the flexural strength) of the laminated coil 1. In addition, the insulation between the soft magnetic metal particles 11 is further improved, which makes it easier to improve the inductance L and the Q value. Furthermore, the reliability and heat resistance are improved.

[0046] Here, the interlayer portion 4a is the portion of the element 2 of the laminated coil 1 where the resin 13 is least likely to be filled in the gap space 12. Therefore, if the gap space 12 of the interlayer portion 4a is filled with the resin 13, it can be said that the entire element 2 of the laminated coil 1 is sufficiently filled with the resin 13.

[0047] There are no particular limitations on the method for confirming whether the oxide film 11b covering the soft magnetic metal particle body 11a includes a layer made of an oxide containing Si and whether the resin 13 is filled in the gap space 12. For example, SEM-EDS measurement and STEM-EDS measurement can be performed, and it can be visually confirmed whether the oxide film 11b covering the soft magnetic metal particle body 11a includes a layer made of an oxide containing Si and whether the resin 13 is filled in the gap space 12.

[0048] Here, Fig. 3 is an SEM image (magnification 10,000 times) of the interlayer portion of Example 103 described later, and Fig. 4 is an SEM image (magnification 10,000 times) of Example 104 described later. From Fig. 3 and Fig. 4, it can be seen that resin is present in addition to the soft magnetic metal particles, filling the gap spaces.

[0049] Furthermore, Figs. 5 to 12 are drawings showing the results of STEM-EDS measurement of the interlayer portion of Example 103 described later. Fig. 5 is a bright-field image (BF image) (magnification: 20,000 times) by STEM. Fig. 6 is a bright-field image (BF image) (magnification: 500,000 times) by STEM. Fig. 7 is a C mapping image (magnification: 20,000 times) by STEM-EDS. Fig. 8 is a C mapping image (magnification: 500,000 times) by STEM-EDS. Fig. 9 is a Si mapping image (magnification: 20,000 times) by STEM-EDS. Fig. 10 is a Si mapping image (magnification: 500,000 times) by STEM-EDS. Fig. 11 is an O mapping image (magnification: 20,000 times) by STEM-EDS. Fig. 12 is an O mapping image (magnification: 500,000 times) by STEM-EDS.

[0050] 5 to 12, it can be seen that the resin 13 is filled into the gap spaces 12 between the layers and hardened. Furthermore, it can be seen that Si is present substantially only in the soft magnetic metal particles 11, and C is present substantially only in the gap spaces 12.

[0051] In Example 103 described later, as shown in FIG. 13, there is an oxide film 11b covering the soft magnetic metal particle body 11a. The oxide film 11b includes a Si oxide layer. Si is substantially present only in the soft magnetic metal particle body 11a and the oxide film 11b. Furthermore, the oxide of Si is substantially present only in the oxide film 11b. The Si oxide layer 11b is a layer mainly composed of an oxide of Si.

[0052] There is no particular limit to the thickness of the oxide film 11b. The Si oxide layer may be in contact with the soft magnetic metal particle body 11a. For example, the oxide film 11b may be composed of only an Si oxide layer, or may have a multi-layer structure of an Si oxide layer and another oxide layer. The Si oxide layer in contact with the soft magnetic metal particle body 11a may be composed essentially of an oxide of Si. The thickness of the oxide film 11b and the thickness of each layer can be measured using a STEM-EDS measurement image. In this embodiment, the average thickness of the coating layer, that is, the average thickness of the entire oxide film 11b, may be 5 nm or more and 60 nm or less. The above average thickness is the average thickness when the thickness of the oxide film 11b is measured for at least 50 soft magnetic metal grains 11.

[0053] There is no particular limitation on the method for forming the oxide film 11b. For example, it can be formed by sintering the soft magnetic metal powder according to this embodiment. The thickness of the oxide film 11b and the thickness of each oxide layer can be controlled by sintering conditions such as sintering temperature and time, annealing conditions, etc. Note that the thicker the oxide film 11b, the smaller the gap space 12 becomes, and the less the amount of resin 13 filled. Note that it is preferable that the oxide of Si is substantially contained only in the oxide film 11b, and is hardly present in the portion (gap space 12) between the two soft magnetic metal particles 11 outside the oxide film 11b.

[0054] In the laminated coil 1 according to this embodiment, the soft magnetic material (soft magnetic metal particles 11) constituting the magnetic base body 4 has a high resistivity. This is because the soft magnetic metal particle main body 11a is covered with an oxide film 11b. Furthermore, when the gap space 12 is filled with the resin 13, the plating solution is less likely to enter the gap space 12. Therefore, when the resin 13 is filled, short circuits are less likely to occur even after plating, and the laminated coil 1 is more likely to have a high inductance L. Furthermore, the strength (particularly the flexural strength) of the laminated coil 1 is also improved.

[0055] In addition, the area ratio of the gap space 12 in the cross section of the interlayer portion 4a (central portion 2b) is preferably 5.0% or more and 35.0% or less of the entire SEM observation image. The area ratio of the gap space 12 can be controlled by the particle size distribution of the soft magnetic metal particles, and can also be controlled by controlling the amount of binder resin in the green chip, the molding pressure when forming the green chip, the firing conditions, the annealing conditions, etc. In addition, if the average particle size (D50) of the soft magnetic metal particles is about the same, the larger the gap space and the larger the amount of resin filled, the smaller the inductance L, but the Q value and flexural strength tend to be larger.

[0056] <Method of manufacturing soft magnetic metal powder> An example of a method for producing soft magnetic metal powder will be described. In this embodiment, the soft magnetic metal powder can be obtained using a method similar to a known method for producing soft magnetic metal powder. Specifically, the soft magnetic metal powder can be produced using a gas atomization method, a water atomization method, a rotating disk method, or the like. Among these, it is preferable to use the water atomization method from the viewpoint that a soft magnetic metal powder having the desired magnetic properties can be easily obtained.

[0057] In the water atomization method, molten raw material (molten metal) is supplied as a continuous linear fluid through a nozzle installed at the bottom of the crucible, and high-pressure water is sprayed onto the supplied molten metal to break it into droplets and rapidly cool it to obtain a fine powder.

[0058] In this embodiment, for example, the raw materials of Fe, Ni, Si, and Co are melted, and P is added to the melt, which is then pulverized by a water atomization method, thereby producing the soft magnetic metal powder according to this embodiment. In addition, when P is contained as an impurity in the raw materials, for example, in the raw material of Fe, the total content of P as an impurity and the amount of P to be added may be adjusted to produce a soft magnetic metal powder containing a desired amount of P. Alternatively, a plurality of raw materials of Fe with different P contents may be used, and the melt in which the P content has been adjusted may be pulverized by a water atomization method.

[0059] <Method of manufacturing sintered soft magnetic metal body and coil-type electronic component> First, an example of a method for producing a sintered soft magnetic metal body according to the present embodiment will be described. A binder is added to the soft magnetic metal powder obtained by the above method to produce a granulated powder. There is no particular limit to the type of binder. For example, an acrylic resin can be used. The obtained granulated powder is molded to obtain a molded body. There is no particular limit to the molding pressure. For example, a molding pressure of 3 ton / cm can be used. 2 More than 10ton / cm 2 Next, the binder is removed. There are no particular limitations on the holding temperature and holding time during binder removal. For example, the temperature may be 300°C or higher and 450°C or lower for 0.5 hours or longer and 2.0 hours or shorter. Next, the compact after binder removal is sintered to obtain a soft magnetic metal sintered body. There are no particular limitations on the type of reducing atmosphere. For example, N 2 Gas and H 2 and a mixed gas atmosphere with a gas. There are no particular limitations on the sintering temperature and time. For example, the sintering may be performed at 550°C or higher and 850°C or lower for 0.5 hours or longer and 3.0 hours or shorter. The thickness of the coating film (oxide film 11b) covering the soft magnetic metal powder increases as the sintering time increases and the hydrogen concentration in the reducing atmosphere decreases.

[0060] When using Fe-Si-Cr-based soft magnetic metal powder that mainly contains Fe, Si, and Cr and has a small content of other elements such as Ni and M, the resistivity is improved by sintering at 400 to 900 ° C in an atmosphere containing oxygen. This is because a highly insulating oxide film made of Si and / or Cr is formed. However, when using the soft magnetic metal powder according to this embodiment, iron oxide is likely to be preferentially generated when sintered in an atmosphere containing oxygen. As a result, the resistivity of the soft magnetic metal powder is rather reduced, and the inductance L of the finally obtained coil-type electronic component is reduced.

[0061] Furthermore, the obtained sintered soft magnetic metal body may be annealed (heat treated). There are no particular limitations on the conditions of the annealing treatment. For example, the annealing treatment may be performed at a temperature of 500°C or higher and 800°C or lower for 0.5 hours or longer and 2.0 hours or shorter. There are also no particular limitations on the atmosphere during the heat treatment. For example, the atmosphere may have an oxygen concentration of 0.05% or higher and 21.0% or lower.

[0062] The binder removal and firing may be performed in an oxidizing atmosphere such as air. However, it is preferable to perform the debinding and firing in an atmosphere with a weaker oxidizing power than air, such as a nitrogen atmosphere or a mixed atmosphere of nitrogen and hydrogen. In this way, the density of the magnetic body can be improved while maintaining a high resistivity of the soft magnetic metal particles, and the magnetic permeability can be improved. In addition, it becomes easier to form a Si oxide film on the surface of the soft magnetic metal particles, and it becomes more difficult to form Fe oxide. As a result, it is possible to prevent a decrease in inductance L due to oxidation of Fe.

[0063] The amount of P contained in the soft magnetic metal particles after the heat treatment is the same as the amount of P contained in the soft magnetic metal particles before the heat treatment.

[0064] Furthermore, a coil-type electronic component can be obtained by winding a coil around the obtained soft magnetic metal sintered body. There are no particular limitations on the method for producing the coil-type electronic component, and any method used in this technical field can be used.

[0065] <Manufacturing method for stacked coil type electronic components> As an example of a method for manufacturing a laminated coil type electronic component, a method for manufacturing a laminated coil type electronic component shown in FIG. 1 will be described. First, the obtained soft magnetic metal powder is slurried together with additives such as a solvent and a binder to prepare a paste. Then, using this paste, a green sheet is formed that will become a magnetic body (sintered soft magnetic metal body) after sintering. Next, silver (Ag) or the like that will become a coil conductor is formed in a predetermined pattern on the formed green sheet. Next, a plurality of green sheets on which coil conductor patterns are formed are stacked, and then each coil conductor pattern is joined via a through hole, thereby obtaining a green laminate in which a coil conductor is formed three-dimensionally and spirally.

[0066] The obtained laminate is subjected to heat treatment (binder removal step and sintering step) to remove the binder, and a sintered body (element) is obtained in which the soft magnetic metal particles contained in the soft magnetic metal powder are connected and fixed (integrated) to each other. The holding temperature in the binder removal step (binder removal temperature) is not particularly limited as long as it is a temperature at which the binder can be decomposed and removed as a gas. For example, it may be 300°C or higher and 450°C or lower. Furthermore, the holding time in the binder removal step (binder removal time) is also not particularly limited. For example, it may be 0.5 hours or higher and 2.0 hours or lower.

[0067] The holding temperature (sintering temperature) in the sintering step is not particularly limited as long as it is a temperature at which the soft magnetic metal particles constituting the soft magnetic metal powder are connected to each other. It may be 550°C or higher and 850°C or lower. In addition, the holding time (sintering time) in the sintering step is also not particularly limited. It may be 0.5 hours or higher and 3.0 hours or lower.

[0068] The amount of phosphorus (P) contained in the soft magnetic metal particles after the heat treatment is the same as the amount of phosphorus (P) contained in the soft magnetic metal particles before the heat treatment.

[0069] In this embodiment, it is preferable to adjust the atmosphere during binder removal and firing.

[0070] After the firing, an annealing treatment (heat treatment) may be performed. There are no particular limitations on the conditions for the annealing treatment. For example, the annealing treatment may be performed at 500 to 800° C. for 0.5 to 2.0 hours. There are also no particular limitations on the atmosphere after the annealing.

[0071] The composition of the soft magnetic metal particles after the above heat treatment is substantially the same as the composition of the soft magnetic metal powder before the above heat treatment.

[0072] Next, terminal electrodes are formed on the element. There are no particular limitations on the method for forming the terminal electrodes, and they are usually prepared by forming a slurry of the metal (such as Ag) that will become the terminal electrodes together with additives such as a solvent and a binder.

[0073] Next, when the magnetic element contains a resin, the element is impregnated with the resin to fill the gap space with the resin. There are no particular limitations on the method of impregnating the resin. For example, a method using vacuum impregnation can be used.

[0074] Vacuum impregnation is performed by immersing the elements of the laminated coil in resin and controlling the air pressure. The resin penetrates into the magnetic body contained in the element by lowering the air pressure. Then, since there is a gap space from the surface of the magnetic body to the inside, the resin penetrates into the magnetic body through the gap space by the principle of capillary action, especially into the interlayer area where it is most difficult for resin to penetrate, and the resin fills the gap space. The resin is then hardened by heating. The heating conditions vary depending on the type of resin.

[0075] There is no particular limit to the type of resin. It is preferable that the resin is finally filled into the gap spaces. For example, particularly when phenolic resin or epoxy resin is used, the resin penetrates sufficiently into the gap spaces inside the magnetic body (particularly in the interlayer portions), and is easily filled into the gap spaces even after hardening. Furthermore, it is not easily decomposed even when heated, so it has high heat resistance. In contrast, when silicone resin is used, the resin is present in a film form on the surface of the soft magnetic metal particles, particularly in the surface portion, and it is difficult for the resin to penetrate sufficiently into the gap spaces inside the magnetic body (particularly in the interlayer portions). Furthermore, the resin decomposes when heated at 300°C or higher, so its heat resistance is also low.

[0076] The resin content in the magnetic body of the finally obtained laminated coil type electronic component is preferably 0.5% by weight or more and 3.0% by weight or less. The resin content can be controlled by changing, for example, the resin solution concentration during impregnation, the immersion time, the number of immersions, etc.

[0077] In this embodiment, electrolytic plating can be performed on the terminal electrodes after filling with resin. Since the resin fills the gap spaces, even if the magnetic body is immersed in a plating solution, the plating solution does not easily penetrate into the magnetic body. Therefore, even after plating, no short circuit occurs inside the laminated coil type electronic component, and the inductance L is kept high.

[0078] Second embodiment The second embodiment will be described below, but unless otherwise specified, it is the same as the first embodiment.

[0079] The soft magnetic metal powder according to the second embodiment is an aggregate of a plurality of soft magnetic metal particles. The soft magnetic metal particles are composed of an Fe-Ni alloy. The Fe-Ni alloy further contains Cr. The Fe-Ni alloy further contains Si and / or M. When M is contained, it is preferable that M is Co. In the present embodiment, the Fe-Ni alloy contains less than 2.0% by mass of the total content of Fe, Ni, Si, M and Cr as 100% by mass. The Cr content may be 0.1% by mass or more and 1.8% by mass or less, or 0.5% by mass or more and 1.5% by mass or less.

[0080] In particular, by having the Cr content within the above range, the magnetic permeability μ and the resistivity ρ become high.

[0081] Furthermore, the soft magnetic metal powder according to the second embodiment may further contain P. With the total content of Fe, Ni, Si, M and Cr being 100 mass %, P may be contained in an amount of 100 ppm or more and 5000 ppm or less, or may be contained in an amount of 200 ppm or more and 2000 ppm or less.

[0082] The Ni content may be 15.0 mass% or more and 80.0 mass% or less, or 15.0 mass% or more and 55.0 mass% or less. When Si is contained, the Si content may be 1.0 mass% or more and 6.0 mass% or less, or 2.0 mass% or more and 6.0 mass% or less, or 2.0 mass% or more and 4.0 mass% or less. When M is contained, the M content may be 1.0 mass% or more and 50.0 mass% or less, or 2.0 mass% or more and 40.0 mass% or less.

[0083] Furthermore, the Ni content may be 22.0 mass% or more and 42.0 mass% or less. The Si content may be 2.5 mass% or more and 5.5 mass% or less, or 2.5 mass% or more and 4.0 mass% or less. The M content may be 5.0 mass% or more and 32.0 mass% or less. The P content may be 300 ppm or more and 2000 ppm or less.

[0084] Third embodiment The third embodiment will be described below, but unless otherwise specified, it is similar to the first and second embodiments.

[0085] In the third embodiment, the composition of the soft magnetic metal particles is not particularly limited except that the Cr content is less than 2.0 mass % (not including 0 mass %). The soft magnetic metal particles may be the same as those in the second embodiment.

[0086] A coil-type electronic component manufactured using a soft magnetic metal powder containing the soft magnetic metal particles is a coil-type electronic component having a magnetic body and a coil conductor built into the magnetic body, The magnetic body includes soft magnetic metal particles, The soft magnetic metal particles are covered with a coating film, the coating film comprises a first layer in contact with the soft magnetic metal particles and a second layer in contact with the first layer, the first layer includes Si or an oxide including Si, The coil-type electronic component in which the second layer contains Cr is the coil-type electronic component according to the third embodiment.

[0087] The coating film (oxide film 11b) covering the soft magnetic metal particles is made up of a first layer and a second layer, each of which has the above composition, thereby improving the magnetic permeability μ and resistivity ρ of the sintered soft magnetic metal body made of soft magnetic metal particles, and improving the Q value and inductance L of a coil-type electronic component having a magnetic body containing the soft magnetic metal particles.

[0088] However, when the Cr content in the soft magnetic metal particles is 2.0 mass % or more, the magnetic permeability μ is significantly reduced, and the Q value and inductance L of the coil-type electronic component are also reduced.

[0089] The first layer may have a higher Si content and a lower Fe content than the soft magnetic metal particles, and the second layer may have higher Si, Cr, and Ni contents and a lower Fe content than the soft magnetic metal particles.

[0090] The average thickness of the first layer is D1, and the average thickness of the second layer is D2, and the relationship may be satisfied: 0.5≦D2 / D1≦1.5. When D2 / D1 is within the above range, an oxide film of appropriate thickness is easily formed, and the magnetic permeability μ and resistivity ρ of the sintered soft magnetic metal body are easily improved.

[0091] D2 may be 2.5 nm or more and 30 nm or less, or 5 nm or more and 20 nm or less. When D2 is 30 nm or less, the magnetic permeability μ of the soft magnetic metal particles is easily improved, and the Q value and inductance L of the coil-type electronic component are also easily improved. In addition, when D2 is 2.5 nm or more, the resistivity ρ of the soft magnetic metal particles is easily improved, and the plating elongation of the coil-type electronic component is also easily suppressed.

[0092] There is no particular limit to the method for covering the soft magnetic metal particles contained in the magnetic body with the coating film. For example, in addition to the method of forming the first and second layers at the stage of soft magnetic metal powder, there is a method of forming the first and second layers on the surface of the soft magnetic metal particles by firing. The first and second layers are formed on the surface of the soft magnetic metal particles by firing soft magnetic metal particles containing Si and Cr in a reducing atmosphere. Note that, if the firing temperature is the same, the longer the firing time and the lower the hydrogen concentration in the firing atmosphere, the thicker both the first and second layers become. If the firing time is the same, the higher the firing temperature and the lower the hydrogen concentration in the firing atmosphere, the thicker the second layer becomes. Furthermore, the higher the Cr content in the soft magnetic metal particles, the thicker the second layer becomes.

[0093] The soft magnetic metal particles contained in the coil-type electronic component of the second embodiment may be covered with a coating film similar to that of the soft magnetic metal particles contained in the coil-type electronic component of the third embodiment.

[0094] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention.

[0095] Known coil-type electronic components include transformers, choke coils, coils, etc. The coil-type electronic component according to the present embodiment is suitable for use as an inductor or impedance in the power supply circuits of various electronic devices such as portable devices. EXAMPLES

[0096] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0097] (Experimental Example 1) First, Fe-Ni alloy, Fe alone, Ni alone, Si alone, and M alone were prepared as raw materials. The shape of each alloy and / or element was ingot, chunk, or shot. Next, these raw materials were mixed to obtain the composition shown in Tables 1 to 3, and placed in a crucible placed in a water atomizer. Examples 2b to 2p in Table 3 were carried out under the same conditions as in Example 2, except that the type of M was changed.

[0098] Next, in an inert atmosphere, the crucible was heated to 1600°C or higher by high-frequency induction using a work coil installed outside the crucible, and the ingots, chunks, or shots in the crucible were melted and mixed to obtain a molten metal. The phosphorus content was adjusted by adjusting the amount of phosphorus contained in the Fe simple substance raw material when the raw material for the soft magnetic metal powder was melted and mixed.

[0099] Next, a high-pressure (50 MPa) water flow was collided with the molten metal supplied from a nozzle provided in the crucible so as to form a linear continuous fluid, and the molten metal was turned into droplets, and was then rapidly cooled, dehydrated, dried, and classified to produce soft magnetic metal powders made of Fe-Ni-Si-M alloy particles. The soft magnetic metal powders were adjusted to have the average particle diameters (D50) shown in Tables 1 to 3.

[0100] The obtained soft magnetic metal powder was subjected to composition analysis by ICP analysis, and as a result, it was confirmed that the soft magnetic metal powder used in each of the examples and comparative examples had the composition shown in Tables 1 to 3. Furthermore, it was confirmed that elements other than Fe, Ni, Si, M, and P, such as Cr, were not substantially contained.

[0101] Acrylic resin was added as a binder to the obtained soft magnetic metal powder to prepare granulated powder. The granulated powder was then molded under a molding pressure of 6 ton / cm to obtain a toroidal shape with an outer diameter of 13 mm, an inner diameter of 6 mm, and a height of 2.7 to 3.3 mm. 2 Next, the compact was held at 400°C in an inert atmosphere to remove the binder, and then heated in a reducing atmosphere (N 2 Gas and H 2 The compact after debindering was fired at 750°C for 1 h in an inert gas atmosphere (mixed gas atmosphere with N 2 The reducing atmosphere is N 2 Gas and H 2 The atmosphere was a mixture of hydrogen and nitrogen gas. The hydrogen concentration in the mixed gas atmosphere was 1.0%. The sintered body was then heat-treated at 700°C for 1 hour in an atmosphere with an oxygen partial pressure of 1%, to obtain a sintered body for evaluation.

[0102] For the obtained fired bodies for evaluation, the magnetic permeability (μ) and resistivity (ρ) were measured by the following method.

[0103] The magnetic permeability was measured at f=2 MHz by the coaxial method using an RF impedance material analyzer (Agilent Technologies: 4991A).

[0104] In Table 1, the increase rate (Δμ / μ) of μ in samples with the same conditions other than the P content was calculated relative to μ in each comparative example (Comparative Example 8, Comparative Example 1, Comparative Example 10, Comparative Example 12) with a P content of 50 ppm. Samples with Δμ / μ of 20.0% or more were considered good.

[0105] In Comparative Examples 3 and 4, and Examples 2, 5 to 6, 5a, and 6a in Table 2, Δμ / μ was calculated for samples in which the Si content was changed relative to μ in Comparative Example 3, which had a Si content of 1.5 mass %. Samples with Δμ / μ of 20.0% or more were deemed good.

[0106] In Comparative Examples 5, 6a, and 6, and Examples 7 to 10, 7a, and 9a in Table 2, Δμ / μ was calculated for samples in which the Co content was changed relative to μ in Comparative Example 5, which had a Co content of 1.0 mass %. Samples with Δμ / μ of 20.0% or more were deemed good.

[0107] In Comparative Examples 7 and 7a and Examples 11 and 12 in Table 2, Δμ / μ was calculated for samples in which the Ni content was changed relative to μ for Comparative Example 7, in which the Ni content was 56.0 mass%. Samples with Δμ / μ of 20.0% or more were deemed good.

[0108] In Table 3, the increase rate (Δμ / μ) of μ in samples with the same conditions other than the P content and the type of M was calculated relative to μ in Comparative Example 1, in which the P content was 50 ppm. Samples with Δμ / μ of 20.0% or more were deemed good.

[0109] The ρ was calculated by applying In-Ga electrodes to both sides of the obtained sintered body, measuring the DC resistance with an ultra-high resistance meter (Advantest: R8340), and calculating ρ from the volume and DC resistance of the sintered body. A ρ of 1.0E06 Ω m or more was considered good.

[0110] [Table 1]

[0111] [Table 2]

[0112] [Table 3]

[0113] From Tables 1 and 3, the examples in which the P content was 100 ppm or more and 5000 ppm or less had better μ and ρ than the comparative examples in which the P content was 50 ppm and other conditions were the same. In contrast, the comparative examples in which the P content was 50 ppm had lower ρ. Moreover, the comparative examples in which the P content was 6000 ppm had lower μ and tended to have lower ρ than the examples in which the P content was 100 to 5000 ppm and other conditions were the same.

[0114] As can be seen from Table 2, the examples in which the content of each component was within the specified range tended to have better μ and ρ than the comparative examples in which the content of Ni, Si and / or Co was outside the specified range.

[0115] (Experimental Example 2) Experimental Example 2 was carried out in the same manner as Experimental Example 1, except that elemental Cr was further prepared as a raw material, and it was confirmed that the soft magnetic metal powder contained substantially no elements other than Fe, Ni, Si, M, Cr and P.

[0116] In Tables 4 to 6, the increase rate (Δμ / μ) of μ in samples with a Cr content of less than 2.0 mass% was calculated relative to μ in Comparative Example 537 with a Cr content of 2.0 mass%. Samples with Δμ / μ of 20.0% or more were rated as good.

[0117] Examples 538 to 542 in Table 4 are examples in which the Cr content was changed mainly from Comparative Example 537. Examples 543 to 546 and 544a in Table 4 are examples in which the Si content was changed mainly from Example 540. Examples 547 to 550 in Table 5 are examples in which the P content was changed from Example 540. Examples 540b to 540p in Table 6 are examples carried out under the same conditions as Example 540 except that the type of M was changed.

[0118] [Table 4]

[0119] [Table 5]

[0120] [Table 6]

[0121] From Tables 4 to 6, each of the Examples in which the Cr content was less than 2.0 mass % had better μ and ρ than Comparative Example 537 in which the Cr content was 2.0 mass %.

[0122] (Experimental Example 3) The soft magnetic metal powder produced in Experimental Example 1 was slurried together with additives such as a solvent and a binder to produce a paste. The types of soft magnetic metal powder are shown in Tables 7 to 10. This paste was then used to form green sheets that would become magnetic bodies after firing. A predetermined pattern of Ag conductors (coil conductors) was formed on the green sheets, and the sheets were laminated to produce a green laminate with a thickness of 0.8 mm.

[0123] Next, the obtained green laminate was cut into a shape of 2.0 mm × 1.2 mm to obtain a green laminate coil. The obtained green laminate coil was placed in an inert atmosphere (N 2 The samples shown in Tables 7 to 9 were then subjected to a binder removal treatment at 400°C in a reducing atmosphere (N 2 Gas and H 2 A sintered body was obtained by sintering at 750°C for 1 hour in a mixed gas atmosphere with nitrogen gas (hydrogen concentration 1.0%). For the samples shown in Table 10, a sintered body was obtained by sintering at the sintering temperature, sintering time, and sintering atmosphere shown in Table 10. A terminal electrode paste was applied to both end faces of the obtained sintered body, dried, and baked at 700°C for 1 hour in an atmosphere with an oxygen partial pressure of 1%, forming terminal electrodes, and a laminated coil (baked product) was obtained.

[0124] Next, in the examples and comparative examples shown in Tables 7 to 10 below, the obtained baked products were impregnated with resin. Specifically, the raw material mixture of phenolic resin or epoxy resin was vacuum impregnated, and then heated to harden the resin at 150°C for 2 hours to fill the resin. Note that the solvent contained in the raw material mixture evaporated when the resin was hardened. Then, electrolytic plating was performed to form a Ni plating layer and a Sn plating layer on the terminal electrodes.

[0125] The raw material mixture for phenolic resin contains approximately 50% by weight of phenols (C 7 H 8 O.C.H. 2 O.C. 4 H 10 O) x The epoxy resin raw material mixture is a mixture of naphthalene-type epoxy resin, a hardener, a solvent (toluene), etc. ...

[0126] Then, for each of the laminated coils of the examples and comparative examples, an LCR meter (4285A manufactured by Hewlett Packard) was used to measure the inductance L and Q value at f=2 MHz and I=0.1 A. The L and Q values ​​shown in Tables 7 to 10 are the average values ​​of the L and Q values ​​of 30 laminated coils, respectively.

[0127] For Table 7, the increase rate (ΔL / L) of L in a laminate coil with the same conditions except for the P content was calculated relative to L in the comparative examples (Comparative Examples 102 and 103) with a P content of 50 ppm. A ΔL / L of 20.0% or more was evaluated as good.

[0128] In Table 8, for Comparative Examples 111 and 112, and Examples 111 to 113, 111a, and 112a, ΔL / L was calculated for samples in which the Si content was changed relative to L in Comparative Example 111, which had a Si content of 1.5 mass %. Samples with ΔL / L of 20.0% or more were deemed good.

[0129] In Comparative Examples 113 to 115 and Examples 114 to 117, 114a, and 116a, ΔL / L was calculated for samples in which the Co content was changed relative to L in Comparative Example 113, which had a Co content of 1.0 mass %. Samples with ΔL / L of 20.0% or more were deemed good.

[0130] In Comparative Examples 116 and 117 and Examples 118 and 119, ΔL / L was calculated for samples in which the Ni content was changed relative to L in Comparative Example 116, in which the Ni content was 56.0 mass%. Samples with ΔL / L of 20.0% or more were deemed good.

[0131] For Table 9, ΔL / L was calculated for samples with the same conditions other than the P content and the type of M as L of Comparative Example 102, which had a P content of 50 ppm. Samples with ΔL / L of 20.0% or more were deemed good.

[0132] Regarding Table 10, for Examples 121 to 126 in which the firing conditions of Example 116 also shown in Table 8 were changed, ΔL / L was calculated relative to Comparative Example 113 also shown in Table 8. Samples with ΔL / L of 20.0% or more were deemed good.

[0133] The Q value of the laminate coil was rated as good when it was 40.0 or more.

[0134] The plating elongation was evaluated for the laminated coils of each of the examples and comparative examples. The evaluation of the plating elongation was performed by observing the appearance of the laminated coil. The results are shown in Tables 7 to 10, with A being the case where no plating elongation was observed, B being the case where plating elongation was observed but was 50 μm or less, C being the case where plating elongation was more than 50 μm and less than 400 μm, and D being the case where plating elongation was 400 μm or more. In Experimental Example 3 and Experimental Example 4 described later, plating elongation rated as A or B was considered good, and A was considered particularly good.

[0135] The short circuit rate was measured for the laminated coils of each of the examples and comparative examples. Thirty laminated coils were produced for each sample, and the number of short-circuited laminated coils was measured using an LCR meter to calculate the short circuit rate. A short circuit rate of 3% or less, i.e., 0 / 30, was deemed good.

[0136] The average thickness of the coating film was measured for the laminated coils listed in Table 10. The average thickness of the coating film was measured by appropriately combining observation of the cross section of the interlayer portion at a magnification of 20,000 times using STEM-EDS with a size of 7 μm×7 μm and observation of the cross section of the interlayer portion at a magnification of 500,000 times using STEM-EDS with a size of 0.3 μm×0.3 μm. Specifically, the thicknesses of the coating films of at least 50 soft magnetic metal particles 11 in the cross section of the interlayer portion were measured using STEM-EDS and averaged.

[0137] [Table 7]

[0138] [Table 8]

[0139] [Table 9]

[0140] [Table 10]

[0141] As can be seen from Tables 7 and 9, the laminated coils made from the soft magnetic metal powders of Comparative Examples 1 and 2 did not have favorable L and Q values. Furthermore, the plating elongation was also inferior to the examples in Tables 7 and 9.

[0142] From Table 8, Examples 111 to 119, Examples 111a, 112a, 114a, 116a, and Comparative Examples 111 to 117, when a laminated coil was produced using the soft magnetic metal powder of Comparative Examples 3 to 7, 6a, and 7a, the L and / or Q values ​​were lower than when a laminated coil was produced using the soft magnetic metal powder of Examples 2 to 12, 5a, 6a, 7a, and 9a. Furthermore, when the soft magnetic metal powder of Comparative Example 3, in which the Si content was too small, was used, the plating elongation and short circuit rate were also poor.

[0143] From Table 10 and Examples 116 and 121 to 126, it was found that the shorter the firing time and the higher the hydrogen concentration in the firing atmosphere, the higher the μ of the fired body and the lower the ρ. Furthermore, the L of the laminate coil tended to be higher and the coating film thinner.

[0144] It was confirmed that the average thickness of the coating film in the examples shown in Tables 7 to 9 was about 40 nm.

[0145] (Experimental Example 4) For the laminated coils of Examples 103 and 104, the presence or absence of resin filling in the gap space between the layers was confirmed. Specifically, a cross-sectional photograph of the interlayer was taken with a size of 13 μm×10 μm at a magnification of 10,000 times using an SEM, and observed. FIG. 3 is an SEM image of the interlayer in the laminated coil of Example 103, and FIG. 4 is an SEM image of the interlayer in the laminated coil of Example 104. It was found that the resin was filled in the gap space between the layers in both Examples 103 and 104.

[0146] Furthermore, the laminated coil of Example 103 was observed at a magnification of 20,000 times, which is higher than the above measurement, at a size of 7 μm × 7 μm using STEM-EDS. Furthermore, it was observed at a magnification of 500,000 times at a size of 0.3 μm × 0.3 μm. The results are shown in Figures 5 to 12. Figure 5 is a BF image at a magnification of 20,000 times, Figure 6 is a BF image at a magnification of 500,000 times, Figure 7 is a C mapping image at a magnification of 20,000 times, Figure 8 is a C mapping image at a magnification of 500,000 times, Figure 9 is a Si mapping image at a magnification of 20,000 times, Figure 10 is a Si mapping image at a magnification of 500,000 times, Figure 11 is an O mapping image at a magnification of 20,000 times, and Figure 12 is an O mapping image at a magnification of 500,000 times.

[0147] From these images, it was found that the soft magnetic metal particle body was covered with an oxide film, which is a type of coating film, and that the layer of the oxide film in contact with the soft magnetic metal particle body was made of Si or an oxide containing Si. Furthermore, it was found that Si was substantially contained only in the soft magnetic metal particle body and the coating film, and C was substantially contained only in the resin filled in the gap space. In addition, it was confirmed that the average thickness of the coating film was 5 nm or more and 60 nm or less in all examples listed in Tables 7 to 9.

[0148] (Experimental Example 5) The soft magnetic metal powder produced in Experimental Example 2 was slurried together with additives such as a solvent and a binder to produce a paste. Thereafter, a laminated coil was produced in the same manner as in Experimental Example 3. As for the firing conditions, the samples shown in Tables 11 to 13 were fired in a reducing atmosphere (N 2 Gas and H 2 The samples were fired at 750°C for 1 hour in a mixed gas atmosphere (hydrogen concentration 1.0%) to obtain fired bodies. The samples shown in Table 14 were fired at the firing temperature, firing time, and firing atmosphere shown in Table 14 to obtain fired bodies. The Q value of the laminated coil was rated as good when it was 40.0 or more.

[0149] In addition, for the laminated coils shown in Tables 11 to 14, the coating films were observed in the same manner as for the laminated coils shown in Table 10. Then, D1 and D2 were measured to calculate D2 / D1. It was confirmed in all of the examples shown in Tables 11 to 14 (except for Examples 116 and 116c) that the first layer had a higher Si content and a lower Fe content than the soft magnetic metal particles, and that the second layer had higher Si, Cr, and Ni contents and a lower Fe content than the soft magnetic metal particles.

[0150] In Experimental Example 5, the increase rate (ΔL / L) of L in a laminate coil in which the Cr content is less than 2.0 mass% and the type of resin is the same as that in the comparative example (Comparative Examples 601 and 602) in which the Cr content is 2.0 mass% was calculated relative to L. A ΔL / L of 20.0% or more was evaluated as good.

[0151] [Table 11]

[0152] [Table 12]

[0153] [Table 13]

[0154] [Table 14]

[0155] From Tables 11 to 13, the laminated coils made from the soft magnetic metal powder of Comparative Example 537 did not have suitable L and Q values. Also, the laminated coils of Examples 116 and 116c made from the soft magnetic metal powder of Example 9, which does not contain Cr, had a structure in which the coating film was composed only of the first layer. And, compared to other Examples under the same conditions except for the Fe content and Cr content, the Q value was lower.

[0156] As can be seen from Table 12, when the Cr content was the same, the higher the Si content, the larger D1 tended to be and the smaller D2 tended to be.

[0157] From Table 14 and Examples 608, 631 to 636, the shorter the firing time and the higher the hydrogen concentration of the firing atmosphere, the higher the μ of the fired body and the lower the ρ. Furthermore, the L of the laminated coil tended to be higher and the coating film thinner. Moreover, from Examples 608, 637 to 640, the higher the firing temperature and the lower the hydrogen concentration of the firing atmosphere, the lower the μ of the fired body and the higher the ρ. Furthermore, the lower the L of the laminated coil, the thicker the coating film, and the higher the D2 / D1. [Explanation of symbols]

[0158] 1... Multilayer coil 2... Element 2a…Surface part 2b…Central part 3…Terminal electrode 4…Magnetic element 4a… Interlayer 5... Coil conductor 5a,5b...Extraction electrode 11...Soft magnetic metal particles 11a...Soft magnetic metal particle body 11b...Oxide film 12…Gap space 13...Resin 14...Void

Claims

1. A soft magnetic metal powder containing soft magnetic metal particles composed of an Fe-Ni-Si-M alloy, The Fe-Ni-Si-M alloy further contains P, M is one or more selected from B, Co, Mn, Ti, Zr, Hf, Nb, Ta, Mo, Mg, Ca, Sr, Ba, Zn, Al, and rare earth elements; The Fe-Ni-Si-M based alloy contains, with the total content of Fe, Ni, Si and M being 100 mass%, Ni in an amount of 15.0 mass% or more and 55.0 mass% or less, Si in an amount of 2.0 mass% or more and 6.0 mass% or less, M in an amount of 2.0 mass% or more and 40.0 mass% or less, and P in an amount of 100 ppm or more and 5000 ppm or less.

2. A soft magnetic metal powder containing soft magnetic metal particles composed of an Fe—Ni based alloy, The Fe—Ni-based alloy further contains Cr, The Fe—Ni-based alloy further contains Si and / or M, M is one or more selected from B, Co, Mn, Ti, Zr, Hf, Nb, Ta, Mo, Mg, Ca, Sr, Ba, Zn, Al, and rare earth elements; The Fe-Ni alloy contains soft magnetic metal powder containing 0.1% by mass or more and 1.8% by mass or less of Cr, with the total content of Fe, Ni, Si, M and Cr being 100% by mass.

3. The Fe—Ni-based alloy further contains P, 3. The soft magnetic metal powder according to claim 2, wherein the Fe-Ni alloy contains P in an amount of 100 ppm to 5000 ppm, with the total content of Fe, Ni, Si, M and Cr being 100 mass %.

4. The soft magnetic metal powder according to any one of claims 1 to 3, wherein M is Co.

5. A soft magnetic metal powder described in any one of claims 1 to 3, wherein the Co content is 2.0 mass % or more and 40.0 mass % or less.

6. The soft magnetic metal powder according to any one of claims 1 to 5, wherein the average particle diameter (D50) of the soft magnetic metal powder is 1.5 μm or more and 15.0 μm or less.

7. A sintered soft magnetic metal body comprising the soft magnetic metal powder according to any one of claims 1 to 6.

8. A coil-type electronic component having a magnetic body and a coil conductor built into the magnetic body, 8. A coil-type electronic component, wherein the magnetic body is made of the sintered soft magnetic metal body according to claim 7.

9. The soft magnetic metal particles are covered with a coating film, 9. The coil-type electronic component according to claim 8, wherein a layer of the coating film in contact with the soft magnetic metal particles contains Si or an oxide containing Si.

10. 10. The coil-type electronic component according to claim 9, wherein the layer of the coating film which is in contact with the soft magnetic metal particles further contains P.

11. 11. The coil-type electronic component according to claim 9, wherein the coating film has an average thickness of 5 nm or more and 60 nm or less.

12. A coil-type electronic component having a magnetic body and a coil conductor built into the magnetic body, The magnetic body includes soft magnetic metal particles, The Cr content in the soft magnetic metal particles is 0.1% by mass or more and 1.8% by mass or less, The soft magnetic metal particles are covered with a coating film, the coating film comprises a first layer in contact with the soft magnetic metal particles and a second layer in contact with the first layer, the first layer includes Si or an oxide including Si; A coil-type electronic component, wherein the second layer contains Cr.

13. A coil-type electronic component as described in claim 12, wherein the soft magnetic metal particles contain Co in an amount of 2.0 mass % or more and 40.0 mass % or less.

14. 14. The coil-type electronic component according to claim 12, wherein the average thickness of the first layer is D1, the average thickness of the second layer is D2, and 0.5≦D2 / D1≦1.

5.

15. The coil-type electronic component according to any one of claims 12 to 14, wherein D2 is 2.5 nm or more and 30 nm or less.

16. the magnetic body includes soft magnetic metal particles and a resin, The coil-type electronic component according to any one of claims 8 to 15, wherein the resin is filled into gap spaces between the soft magnetic metal particles.

17. 17. The coil-type electronic component according to claim 16, wherein the resin is a phenol resin or an epoxy resin.

Citation Information

Patent Citations

  • Method and apparatus for controlling opening and closing of automatic door

    JP1983054185A

  • Soft magnetic alloy powder, compact, and inductance element

    JP2008135674A

  • Multilayer inductor

    JP2012238840A

  • Manufacturing method of oriented electromagnetic steel sheet

    JP2017101311A

  • Coil component

    JP2019117921A