Concrete composition and centrifugal concrete products
A concrete composition using Portland cement, blast furnace slag, and light calcium carbonate addresses the strength and environmental issues of cement replacement, enabling low-cost, high-strength centrifugal concrete products with reduced carbon emissions.
Patent Information
- Application Number
- JP2022031458
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-02
AI Technical Summary
Concrete compositions that replace a large amount of cement with blast furnace slag or do not use cement face delays in initial reaction and reduced initial strength, making it difficult to achieve high-strength concrete products, and the use of early strength agents increases cost and complicates compaction.
A concrete composition comprising Portland cement, pulverized blast furnace slag, light calcium carbonate, and aggregates, with a specific ratio of binder and filler materials, which fixes carbon dioxide and reduces environmental impact while maintaining initial strength without the need for costly early strength agents.
The composition allows for low-cost production of high-strength centrifugal concrete molded products with reduced carbon dioxide emissions, achieving compressive strengths of 55N/mm within 7 to 14 days without compromising on durability.
Smart Images

Figure 0007569816000009 
Figure 0007569816000010 
Figure 0007569816000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a concrete composition and a centrifugal concrete product comprising a binder containing Portland cement and ground granulated blast furnace slag. [Background technology]
[0002] Cement is generally produced by burning raw materials such as limestone and clay at high temperatures to produce a composition (intermediate) called cement clinker, which is then crushed and gypsum is added. During the cement clinker production stage, limestone, which is primarily composed of calcium carbonate (CaCO3), is burned to become cement clinker, which is primarily composed of calcium oxide (CaO), which releases carbon dioxide (CO2), so concrete, which uses cement, is said to be environmentally hazardous.
[0003] For this reason, in order to reduce the amount of carbon dioxide generated from cement production, concrete compositions with a low environmental impact have been proposed in which blast furnace slag or fly ash is used in place of cement to reduce the amount of cement used (see, for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-151517 A [Patent Document 2] JP 2010-285293 A [Patent Document 3] JP 2014-148434 A [Patent Document 4] JP 2009-269786 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the case of a concrete composition in which a large amount of cement is replaced with blast furnace slag, or in the case of a concrete composition that does not use cement, the amount of clinker is reduced, which delays the initial reaction and reduces the early strength, making it difficult to apply this to high-strength secondary concrete products that require early aging.
[0006] As a countermeasure, it is possible to accelerate the initial reaction by using early-strength agents such as silica fume, anhydrous gypsum, dihydrate gypsum, and CSH-based agents, but this has problems such as high product costs and vulnerability to carbonation.In addition, when used in centrifugal compaction concrete molding, there is a risk that compaction will become difficult.
[0007] The present invention has been made in consideration of the above-mentioned points, and an object of the present invention is to provide a concrete composition and a centrifugal concrete molded product that can be produced at low cost and reduce carbon dioxide emissions. [Means for solving the problem]
[0008] The concrete composition according to claim 1 includes water, a binder, a filler, and an aggregate, the binder includes Portland cement and ground granulated blast furnace slag, the water-binder ratio is 20% to 35%, and the binder is mixed with 370 kg / m 3 ~750 kg / m 3 The filler material comprises: Carbon dioxide was fixed in the waste Light calcium carbonate, 10 kg / m 3 ~100 kg / m 3 The substitution rate by mass of the ground granulated blast furnace slag to the Portland cement in the binder is 40% to 60%.
[0009] request request 2 The centrifugal concrete molded product described in the claims 1 The concrete structure comprises a concrete portion obtained by hardening the concrete composition described above, and a reinforcing material embedded in the concrete portion.
[0010] Claim 3 The centrifugal concrete molded product described in the claims 2 In the centrifugal concrete molded product described above, the concrete part has a compressive strength of 55N / mm at 7 to 14 days of age. 2 That is all. Effect of the Invention
[0011] According to the present invention, it is possible to produce a concrete composition which can be produced at low cost and which can reduce carbon dioxide emissions. [Brief description of the drawings]
[0012] [Figure 1] 1 is a graph showing compressive strength versus replacement rate of ground granulated blast furnace slag for each test specimen in a first example of an embodiment of the present invention. [Diagram 2] FIG. 1A is a perspective view showing a test specimen in the second embodiment, and FIG. [Diagram 3] 13 is a graph showing an example of bending performance of a test specimen in the third example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] An embodiment of the present invention will now be described.
[0014] A concrete composition according to one embodiment of the present invention includes water, a binder, a filler material, and an aggregate.
[0015] The binder contains Portland cement and ground granulated blast furnace slag.
[0016] The Portland cement is as specified in JIS R 5210, and preferably, ordinary Portland cement or high-early-strength Portland cement is used.
[0017] The ground granulated blast furnace slag is ground granulated blast furnace slag for concrete as specified in JIS A 6206, and preferably any one of Ground Granulated Blast Furnace Slag 3000, Ground Granulated Blast Furnace Slag 4000, and Ground Granulated Blast Furnace Slag 6000 is used.
[0018] As the filler material, light calcium carbonate powder is used. Light calcium carbonate powder is usually produced from limestone. It is produced by crushing and calcining limestone, reacting it with water to make milk of lime, and passing carbon dioxide discharged from calcination through the milk of lime to produce crystals of light calcium carbonate. On the other hand, the light calcium carbonate used in the present embodiment is derived from waste. For example, the light calcium carbonate of the present embodiment is obtained by fixing carbon dioxide contained in the boiler exhaust gas from a factory or the like to a liquid obtained by solid-liquid separation of concrete sludge or washing water derived from a concrete product factory or a ready-mixed concrete plant. Alternatively, light calcium carbonate is obtained by fixing carbon dioxide to waste seawater. For example, light calcium carbonate produced by adding an alkali agent as a pH adjuster to waste seawater after producing magnesium hydroxide from seawater, and reacting carbon dioxide contained in the exhaust gas from a factory or a power plant with the calcium component is used. Preferably, the light calcium carbonate has a specific surface area of 2000 cm 2 / g~4000cm 2 / g is used.
[0019] Preferably, in the concrete composition of the present embodiment, an admixture is used depending on the state of the concrete composition. As the admixture, a high-strength admixture, an expansive agent, or a shrinkage reducing agent is used. As the admixture, a chemical admixture for concrete specified in JIS A 6204, for example, a polycarboxylic acid-based high-performance water reducing agent or a naphthalene sulfonate-based high-performance water reducing agent is used. The admixture is contained, for example, at 0.5% to 3.5% of the total content of the binder. Also, the admixture is contained, for example, at 3% to 10% by mass of the total content of the binder.
[0020] The concrete composition of this embodiment has a water-binder ratio of 20% to 35%. If the water-binder ratio is below 20%, the plastic viscosity increases and handling properties decrease, and if the water-binder ratio is above 35%, the plastic viscosity decreases and formability by centrifugal molding decreases. In short, the upper and lower limits of the water-binder ratio are set based on the plastic viscosity (handling properties and formability).
[0021] The mass replacement rate of the ground granulated blast furnace slag to the Portland cement in the binder is 40% to 60%. In other words, the ratio of the content of the ground granulated blast furnace slag to the total content of the Portland cement and the ground granulated blast furnace slag is 40% to 60% of the total mass.
[0022] The replacement rate of this ground granulated blast furnace slag increases the strength development from the same as that of Portland cement alone to 10N / mm 2 The amount is set so that the strength reduction is limited to about 100% and the water-cement ratio can be easily adjusted when the compressive strength is lower than that of Portland cement alone. In other words, the higher the replacement rate of ground granulated blast furnace slag, the greater the strength reduction, so the upper limit of the replacement rate of ground granulated blast furnace slag is set based on the compressive strength at a specified material age. The lower limit of the replacement rate of ground granulated blast furnace slag is set based on the amount of carbon dioxide emissions, as described below.
[0023] Light calcium carbonate suppresses the decrease in early strength caused by the use of ground granulated blast furnace slag. In other words, there are cases where it has been reported that limestone fine powder promotes the hydration of alite (tricalcium silicate) in concrete that uses limestone fine powder, and since the main component of limestone fine powder is considered to be calcium carbonate, a similar effect can be obtained by using the light calcium carbonate mentioned above.
[0024] The formula for the proportion of precipitated calcium carbonate is considered as aggregate replacement. The more precipitated calcium carbonate is used, the more carbon dioxide emissions from the concrete composition can be reduced, so the more it is used, the more preferable it is.
[0025] The carbon dioxide emissions of the materials used in the concrete composition of this embodiment are shown in Table 1. The values are taken from JIS Q 13315-4, Appendix C. The data for the precipitated calcium carbonate was calculated based on the chemical formula and the amount of electricity used during the reaction.
[0026] [Table 1]
[0027] Table 2 shows an example of the composition of each material based on the reduction rate of carbon dioxide emissions.
[0028] [Table 2]
[0029] Based on the above data, the lower limit of the replacement rate of ground granulated blast furnace slag and the lower limit of the blending ratio of light calcium carbonate are set so that the reduction rate of carbon dioxide emissions is within a predetermined range, for example, 30% to 60%, based on the case where the binder is only Portland cement (for example, No. 1 in Table 2). For example, as shown in No. 2 in Table 2, when the blending ratio of light calcium carbonate is 10 kg / m 3 In this case, the replacement rate of ground granulated blast furnace slag is 40% and the reduction rate of carbon dioxide emissions is about 35%, so if the replacement rate of ground granulated blast furnace slag falls below 40%, it is predicted that the reduction rate of carbon dioxide emissions will fall below 30% regardless of the blend of light calcium carbonate, and therefore the lower limit of the replacement rate of ground granulated blast furnace slag is set at 40%. Therefore, from the above range of the water-binder ratio, the total content of the binder in the concrete composition of this embodiment, that is, Portland cement and ground granulated blast furnace slag, is 、3 70kg / m 3 ~750kg / m 3 in be.
[0030] On the other hand, when used as an aggregate replacement, light calcium carbonate has a large specific surface area and high water absorption rate compared to aggregate, so the more light calcium carbonate is used, the more stiff the finished product becomes. Therefore, the amount of light calcium carbonate used should be within the range that can be adjusted with a water reducing agent. In short, the lower limit of the light calcium carbonate blend is set based on the amount of carbon dioxide emissions, and the upper limit is set according to the state of the finished product.
[0031] For example, in the present embodiment, light calcium carbonate is 、 10kg / m 3 ~100kg / m 3 Contains Can be enjoyed.
[0032] The aggregate includes a coarse aggregate and a fine aggregate. The coarse aggregate is preferably a crushed stone. The fine aggregate is preferably a crushed sand.
[0033] Then, a centrifugal concrete molded product is manufactured using the concrete composition of this embodiment. Examples of centrifugal concrete molded products include concrete piles, concrete columns, walls, and other centrifugally molded products. The centrifugal concrete molded product has a concrete part formed by hardening the concrete composition, and a reinforcing material embedded in the concrete part. The concrete part has a compressive strength of 55 N / mm at a short-term age (age of 7 to 14 days). 2 The above is a high-strength concrete section. The reinforcing material is steel bars, etc.
[0034] Next, a method for producing the above centrifugal concrete molded product will be described.
[0035] The manufacturing method of this embodiment includes a manufacturing process (step S1) for manufacturing a concrete composition, a centrifugal molding process (step S2) using the concrete composition manufactured in the manufacturing process, and a curing process (step S3) after the centrifugal molding process.
[0036] In the manufacturing process, commercially available Portland cement, ground granulated blast furnace slag, light calcium carbonate, and aggregate are mixed, and then mixing water and admixtures are added and mixed to produce a concrete composition.
[0037] At this time, because the specific gravity of light calcium carbonate is lighter than that of cement, if sludge is generated by centrifugal compaction in the next centrifugal molding process, some of it will be discharged. This is not a problem when molding without sludge when the finished mixture has a hard mix (slump 0cm to 5cm), but when molding with sludge, it is necessary to assume that 10% to 25% of the mixed amount of light calcium carbonate will be discharged, so molding with a slump of 0 to 5cm is desirable.
[0038] Light calcium carbonate is used in a powder or slurry state, and the powder state contains 1% to 4% water. For example, light calcium carbonate is used at 50 kg / m 3 When used, 0.5kg / m 3 ~2.0kg / m 3 Therefore, the amount of water to be mixed must be adjusted taking into account the amount of water contained in the light calcium carbonate powder. When light calcium carbonate is used in a slurry state, the water content must be understood. For example, when the water content is 50%, light calcium carbonate must be mixed at 50 kg / m 3 To use it, the slurry containing light calcium carbonate must be added at 100 kg / m 3 It is necessary to use 50kg / m 3 Therefore, the amount of water to be mixed must be adjusted taking into account the amount of water contained in the slurry containing precipitated calcium carbonate.
[0039] In the centrifugal molding process, the concrete composition produced in the manufacturing process is poured into a predetermined formwork in which reinforcing materials are arranged, and centrifugal molding is performed using a known centrifuge. In the centrifugal molding, the centrifugal acceleration caused by the rotation of the formwork is gradually increased, for example, from initial speed (1G to 2G), low speed (3G to 5G), medium speed (10G to 15G), and high speed (20G to 35G). The time for each speed is appropriately determined according to the diameter and thickness of the centrifugal concrete product.
[0040] In the curing process, the intermediate product produced by centrifugal molding in the centrifugal molding process is subjected to normal pressure steam curing in a steam curing tank. The steam curing is performed by pre-setting at room temperature for 3 to 5 hours, increasing the temperature by 20°C / hour, and then curing at a maximum temperature of 60°C to 70°C for 3 to 5 hours, followed by natural cooling.
[0041] The centrifugal concrete molded product produced in this way has a compressive strength of 55N / mm2 at a short period of time (7 to 14 days). 2 It exhibits higher strength than that of the conventional steel.
[0042] In this way, the concrete composition of the present embodiment is a concrete composition in which the binder is 370 kg / m 3 ~750 kg / m 3 The mass replacement rate of the blast furnace slag powder in the binder to the Portland cement is 40% to 60%, and the filler material is light calcium carbonate. kg / m 3 ~100 kg / m 3 This feature suppresses delays in the initial reaction during hardening without the need for early-strengthening agents, making it possible to produce the product at low cost, while reducing carbon dioxide emissions by 30% to 60% compared to concrete products made using only Portland cement as a binder.
[0043] Furthermore, centrifugal concrete molded products produced using this concrete composition exhibit early aging and are suitable as high-strength concrete secondary products.
[0044] In particular, the concrete part of the centrifugal concrete molded product of this embodiment has a compressive strength of 55 N / mm2 at a short-term material age (7 to 14 days) after steam curing, as described above. 2 It is possible to achieve the above-mentioned high strength and at the same time, the steel is not weakened by carbonation. EXAMPLES
[0045] <First Example> In this example, the relationship between the amount of ground granulated blast furnace slag used and the compressive strength was evaluated by comparing the compressive strength at a specified age, for example, 7 days, of centrifugal concrete products obtained by centrifugally molding a concrete composition using only Portland cement and centrifugal concrete products obtained by centrifugally molding a concrete composition in which part of the Portland cement was replaced with ground granulated blast furnace slag.
[0046] The concrete compositions were manufactured using the same common materials by mixing them in a diagonal mixer or a twin-shaft mixer.
[0047] The compressive strength test was carried out using specimens with a diameter of 20 cm, a length of 30 cm and a wall thickness of 4 cm. The specimens were manufactured using each concrete composition by the same manufacturing method.
[0048] Figure 1 and Table 3 show examples of test results.
[0049] [Table 3]
[0050] As can be seen from FIG. 1 and Table 3, the higher the substitution rate of ground granulated blast furnace slag in the concrete composition, the lower the compressive strength. For example, a centrifugal concrete product made using a concrete composition with a substitution rate of 75% ground granulated blast furnace slag has a compressive strength of about 25 N / mm 2 It showed a decrease in strength.
[0051] Therefore, to bring out the hydraulic properties of ground granulated blast furnace slag, an alkaline stimulant such as cement or gypsum is required, but Portland cement alone is insufficient as a stimulant. Therefore, by keeping the replacement rate of ground granulated blast furnace slag to 60% or less, the decrease in compressive strength of centrifugal concrete products can be reduced to 10N / mm without using a stimulant. 2 It was shown that it is possible to keep
[0052] <Second Example> In this example, the fresh properties and compressive strength were evaluated depending on the amount of light calcium carbonate used. Specifically, the fresh properties and compressive strength were evaluated when 45 to 50% of Portland cement was replaced with ground granulated blast furnace slag and the amount of light calcium carbonate substituted for aggregate was increased.
[0053] Precipitated calcium carbonate is treated as a filler material, and when used, its blending is considered as aggregate replacement. The test specimens were manufactured using the same manufacturing method as in Example 1. The test results are shown in Table 4. The carbon dioxide reduction rate is based on Test Example 2-1.
[0054] [Table 4]
[0055] The more light calcium carbonate used, the more carbon dioxide emissions from the concrete composition can be reduced, so it is preferable to use a larger amount, but the results showed that the more the amount used, the more stiff the finished product became. In Test Example 2-5, mixing became difficult despite adjustments using a water-reducing agent, so the amount of light calcium carbonate used was 100 kg / m 3 It was also shown that the early strength tended to improve slightly as the amount of precipitated calcium carbonate increased.
[0056] <Third Example> In this example, a centrifugal concrete product using ground granulated blast furnace slag and light calcium carbonate, which have similar compressive strength, was compared with a centrifugal concrete product not using these materials to determine whether there was any effect on the amount of drying shrinkage, creep coefficient, and neutralization.
[0057] The formulations of these concrete compositions are shown in Table 5.
[0058] [Table 5]
[0059] As in the above-mentioned respective examples, the same materials were used except for the ground granulated blast furnace slag and light calcium carbonate, and the test specimens were manufactured by the same manufacturing method.
[0060] First, the drying shrinkage test method was based on "Part 3: Dial Gauge Method" of JIS A 1129-3 "Methods for Measuring Changes in Length of Mortar and Concrete," and a 10x10x40cm specimen was manufactured, gauge plugs were embedded in both ends of the specimen, and the length change was measured at each age (1 week, 2 weeks, 4 weeks, 2 months, 3 months, 6 months) using a dial gauge measuring device to calculate the amount of shrinkage. During measurement, the specimens were stored in a constant temperature and humidity room at a temperature of 20±1°C and a humidity of 60±5%.
[0061] For the creep test method, a hollow cylindrical centrifugal specimen with a diameter of 20 cm x 30 cm was manufactured in accordance with JIS A 1136, wire strain gauges were attached to the surface of the specimen at two opposing longitudinal locations on the outer circumference, the surface was sealed with sealing tape, and the maximum prestress force of 10 N / mm was applied to the centrifugal concrete molded product. 2 The load was applied to the test specimens and the strain was measured at each age. Unloaded test specimens were also prepared at the same time and the strain was measured at each age (1 week, 2 weeks, 4 weeks, 2 months, 3 months, 6 months). The creep strain is calculated by subtracting the strain of the unloaded test specimen from the strain of the loaded test specimen. During the measurements, the test specimens were stored in a constant temperature and humidity room at a temperature of 20±1°C and a humidity of 60±5%.
[0062] Furthermore, for the carbonation test method, a hollow cylindrical centrifugal specimen of 20cm diameter x 30cm was manufactured in accordance with JIS A 1136, and this specimen was cut in the axial direction to form an arch-shaped specimen 1 as shown in Figure 2(a) and Figure 2(b), and the cut surface 2 was coated 3 with epoxy resin. Three specimens 1 were manufactured for each test example, and an accelerated carbonation test was carried out on each of them. This accelerated carbonation test was carried out in accordance with JIS A 1153, and the arch-shaped specimen 1 was split or cut when it reached the designated accelerated period (1 week, 4 weeks, 8 weeks, 13 weeks, and 26 weeks), and was measured in accordance with JIS A 1152.
[0063] The results of the drying shrinkage test, creep test, and carbonation test are shown in Tables 6 to 8, respectively.
[0064] [Table 6]
[0065] [Table 7]
[0066] [Table 8]
[0067] Compared to Test Example No. 3-1, Test Example No. 3-2 showed a roughly equivalent rate of length change in terms of drying shrinkage up to an age of six months. Also, although the creep coefficient was somewhat large, it showed a tendency to converge after an age of four weeks, so no particular problems were found as a prestressing concrete. Furthermore, with regard to carbonation, while no change was seen on the outer periphery, carbonation progressed on the inner surface. However, since the durability guideline in the High Durability Guidelines (draft) specifies that the carbonation depth at an age of 26 weeks is 25 mm or less, there are no problems as a concrete.
[0068] Therefore, it was shown that the centrifugal concrete molded product made of the concrete composition of this embodiment has sufficient performance against drying shrinkage, creep, and carbonation.
[0069] <Fourth Example> Under the conditions of Test Example No. 3-2 of the third embodiment, a PHC pile (Type B) with a diameter of 60 cm was manufactured as a test specimen, and its bending performance was evaluated. An example of the test result is shown in Figure 3.
[0070] No concrete sludge was generated during centrifugal molding, and the molded product was able to be manufactured without cracks on the inside surface. In accordance with JIS A 5373 Appendix E "(Regulations) Pile", the bending performance test results showed that the initial crack generation moment was 1.0 times the design value M cf The breaking moment is 1.29 times the design value M u This indicated that the test specimen had the performance required for a PHC pile (Type B).
[0071] Therefore, the above first to fourth examples have demonstrated that the various conditions of the concrete composition of this embodiment are suitable for providing centrifugal concrete molded products with the required performance.
Claims
1. Water, a binder, a filler, and an aggregate; The binder contains Portland cement and ground granulated blast furnace slag, The water-binder ratio is 20% to 35%; The binder is 370 kg / m3 to 750 kg / m3, The filler material is a precipitated calcium carbonate in which carbon dioxide is fixed in waste, and has a density of 10 kg / m3 to 100 kg / m3; The mass replacement rate of the ground granulated blast furnace slag to the Portland cement in the binder is 40% to 60%.
1. A concrete composition comprising:
2. A concrete part obtained by hardening the concrete composition according to claim 1; A reinforcement material embedded in the concrete portion, A centrifugal concrete molded product comprising:
3. The concrete part has a compressive strength of 55N / mm at 7 to 14 days old. 2 That's all.
3. The centrifugal concrete molded product according to claim 2.
Citation Information
Patent Citations
Cement composition for centrifugal forming and centrifugal formed body using the same
JP1999060311A
Hydraulic composition for cement concrete product
JP1999157889A
Hydraulic composition and concrete using the hydraulic composition
JP2009269786A
Concrete composition using blast-furnace slag composition
JP2010285293A
Hydraulic composition
JP2014148434A