Surface coated cutting tools
A surface-coated cutting tool with a laminate structure of TiCN layers and a TiCN upper layer addresses adhesion issues, enhancing wear and chipping resistance for effective cutting of steel and cast iron.
Patent Information
- Application Number
- JP2021043130
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-03-17
AI Technical Summary
Existing surface-coated cutting tools exhibit insufficient adhesion resistance during cutting operations, particularly when machining steel and cast iron, despite having good wear resistance and chipping resistance.
A surface-coated cutting tool with a laminate layer composed of alternating TiCN layers with varying carbon content ratios, a TiCN upper layer, and optional additional layers like TiN, TiCNO, and Al2O3, designed to enhance adhesion, wear resistance, and chipping resistance.
The tool achieves improved adhesion, wear resistance, and chipping resistance, ensuring longevity and performance in cutting steel and cast iron applications.
Smart Images

Figure 0007570599000007 
Figure 0007570599000001 
Figure 0007570599000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-coated cutting tool (hereinafter sometimes referred to as a coated tool). [Background technology]
[0002] In order to improve the cutting performance of cutting tools, there have been coated tools in which a coating layer is formed by vapor deposition on the surface of a tool substrate such as a tungsten carbide (hereinafter referred to as WC)-based cemented carbide. These coated tools are known to exhibit excellent wear resistance. Although the coated tools having the above-mentioned conventional coating layers are excellent in wear resistance, various proposals have been made for further improving the coating layers.
[0003] For example, Patent Documents 1 and 2 disclose a coating layer having a plurality of columnar crystals, each of which is made of TiC x N z-x (0.45≦x<0.70, 0.80≦z≦1.20) and a first unit layer of TiC y N A-y A coated tool having a multilayer structure in which a first unit layer having a structure of (0.70≦y≦1, 0.80≦A≦1.20) and a second unit layer having a structure of (0.70≦y≦1, 0.80≦A≦1.20) are alternately laminated is described, and this coated tool is said to have excellent wear resistance and chipping resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-171546 A [Patent Document 2] JP 2019-171547 A Summary of the Invention [Problem to be solved by the invention]
[0005] According to the inventors' investigations, it has been found that while the coated tools described in Patent Documents 1 and 2 have excellent wear resistance and chipping resistance, they have insufficient adhesion resistance, particularly when cutting steel and cast iron.
[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a coated tool which has excellent wear resistance and chipping resistance while ensuring adhesion resistance particularly in cutting steel and cast iron. [Means for solving the problem]
[0007] The present inventors have conducted extensive research into means for ensuring adhesion resistance, particularly in cutting steel and cast iron, while also providing excellent wear resistance and chipping resistance. As a result, the inventors have discovered that the above-mentioned object can be achieved by a coated tool having a coating layer having a TiCN layer (upper layer) with a low C content of a predetermined average layer thickness on top of a laminate layer in which a predetermined number of TiCN layers (first layer) with a low C content and TiCN layers (second layer) with a high C content are alternately laminated. Here, the C content of the first layer and the upper layer is in the same range, and that of the second layer is higher than those.
[0008] The present invention is based on this finding and is as follows. "(1) A surface-coated cutting tool having a tool base and a coating layer provided on the surface of the tool base, the covering layer has a laminate layer in which seven or more laminate unit layers are laminated and an upper layer on the upper part of the laminate layer, the laminate unit layer has a first layer on the tool base side and a second layer on the opposite side, The first layer has a composition represented by the formula: TiC x N 1-x When expressed as, 0.50≦x≦0.60, The second layer has a composition represented by the formula: TiC y N 1-y When expressed as, 0.65≦y≦1.00, The composition of the upper layer is represented by the formula: TiC z N 1-zWhen expressed as, 0.50≦z≦0.60, The laminate layer has columnar crystals with an average width of 130 to 300 nm, The ratio of the average thickness of the first layer to the average thickness of the second layer, of Average layer thickness) / (2nd layer of The average layer thickness is 0.5 to 3.0. A surface-coated cutting tool comprising: (2) The surface-coated cutting tool according to (1) above, characterized in that the upper layer has one or more layers selected from the group consisting of a TiN layer, a TiCN layer, a TiCNO layer, an Al2O3 layer, and an AlTiN layer on the upper surface of the upper layer. Effect of the Invention
[0009] The surface-coated cutting tool of the present invention has excellent wear resistance and chipping resistance while ensuring adhesion resistance, particularly when cutting steel and cast iron. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic diagram showing an example of an embodiment of a vertical cross section of a coating layer of a surface-coated cutting tool of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In this specification and claims, when a numerical range is expressed as "M to N" (where M and N are both numerical values), the range includes an upper limit (N) and a lower limit (M), and the upper limit (N) and the lower limit (M) have the same units. Furthermore, the composition of a compound not expressed by a composition formula is not limited to a stoichiometric composition, and includes all compositions of conventionally known atomic ratios.
[0012] 1 is a schematic diagram showing an example of an embodiment of a longitudinal section of a coating layer of a surface-coated cutting tool of the present invention (a section perpendicular to the surface of a tool substrate when the surface is treated as a flat surface, ignoring minute irregularities on the surface), and the coating layer on the surface of a tool substrate (1) has a base layer (2), a laminate layer formed by laminating laminate unit layers including a first layer (3) and a second layer (4), an upper layer (5), and an outermost surface layer (6). This embodiment will be described in detail below.
[0013] 1.Coating layer (1) Lamination unit layer and laminate layer The laminate unit layer has a first layer on the tool base side and a second layer on the opposite side. The composition of the first layer is expressed as the formula: TiC x N 1-x When expressed as above, 0.50≦x≦0.60 is preferable, The second layer has a composition represented by the formula: TiC y N 1-y When expressed as: 0.65≦y≦1.00 is preferable. The reason why it is preferable to set x and y within the above ranges is that the difference in thermal expansion coefficient due to the difference in composition becomes appropriate, and the laminate layer formed by laminating a plurality of laminate unit layers can reliably exhibit the function as a stress relaxation layer.
[0014] The average thickness of the laminate layer is preferably 4.0 to 16.0 μm. When it is in this range, the laminate layer can more reliably suppress the propagation of cracks. In the laminate unit layer, the ratio of the average layer thickness of the first layer to the average layer thickness of the second layer, (first layer of Average layer thickness) / (2nd layer of The average layer thickness is preferably 0.5 to 3.0 mm. If it is in this range, the function as a stress relaxation layer is reliably exhibited.
[0015] The number of laminated unit layers is preferably 7 or more. There is no upper limit on the number of laminated layers, but in an example of the manufacturing method described later, the upper limit is about 50 layers due to the constraints of the manufacturing method.
[0016] Both the first and second layers of the laminate unit layer are preferably fine columnar crystals, and the average width is preferably 130 to 300 nm. When the average width is in this range, the TiCN layer having a low C content, which is the upper layer described later, can also be made fine columnar, improving the wear resistance and chipping resistance.
[0017] Here, the average grain width is measured as follows. The cross section is observed with a scanning electron microscope (SEM), a line segment of at least 1 μm in length parallel to the substrate surface is drawn 4 μm from the surface of the tool substrate in the thickness direction of the coating layer, the number of grain boundaries intersecting with the line segment is counted, and the average grain width is calculated by dividing the line segment length by the number measured. The reason for choosing the 4 μm position is that the grain size of the crystal grains increases as they approach the tool surface, so the measurement was made at 4 μm.
[0018] Here, the composition of each layer is measured by cross-sectional measurement using a Transmission Electron Microscope (TEM) and Energy Dispersive X-ray Spectroscopy (EDS), and the measured values are averaged.
[0019] The surface of the tool base, which is the starting point of the length in the layer thickness direction, is the reference line of the interface roughness between the tool base and the coating layer (if there is a base layer, it is the base layer, as described later) in the observation image of the vertical section (almost in the layer thickness direction) almost perpendicular to the tool base. That is, when the tool base has a flat surface like an insert, element mapping is performed using EDS on the vertical section, and the interface between the coating layer and the tool base is determined by performing known image processing on the obtained element map, and the average line is arithmetically obtained for the roughness curve of the interface between the coating layer and the tool base thus obtained, and this is the surface of the tool base. The direction perpendicular to this average line is the direction perpendicular to the tool base (layer thickness direction).
[0020] Even if the tool base has a curved surface like a drill, if the tool diameter is sufficiently large compared to the thickness of the coating layer, the interface between the coating layer and the tool base in the measurement area will be approximately flat, so the surface of the tool base can be determined by a similar method. That is, for example, in the case of a drill, element mapping is performed using EDS on the longitudinal section of the coating layer in a section perpendicular to the axial direction, and the interface between the coating layer and the tool base is determined by performing known image processing on the obtained element map, and the average line is arithmetically obtained for the roughness curve of the interface between the coating layer and the tool base thus obtained, and this is taken as the surface of the tool base. Then, the direction perpendicular to this average line is taken as the direction perpendicular to the tool base (layer thickness direction).
[0021] (2) Upper layer The upper layer is a TiCN layer, and its composition is: TiCN z N 1-z When z is in this range, the affinity with the work material is reduced while the columnar crystals of the lower laminate layer are retained, and adhesion can be suppressed. The upper layer preferably has an average thickness of 3.0 to 16.0 μm, because when the sum of the average thicknesses of the laminate layer and the upper layer is 7.0 to 20.0 μm, abrasion resistance can be maintained for a long period of time.
[0022] (3) Other layers Although the coating layer of the present invention can achieve the above-mentioned object of the invention with only the laminate layer and the top layer, it can also include layers other than these layers. Such layers include an outermost layer, an intermediate layer, and an undercoat layer.
[0023] (3-1) Uppermost surface layer When a compound layer having a total average thickness of 0.1 to 20.0 μm is provided on the upper layer as a top surface layer with a total average thickness of 1.0 to 25.0 μm, the top surface layer can exhibit even better wear resistance and chipping resistance in combination with the effects of these layers. Here, if the total average thickness of the top surface layer is less than 1.0 μm, the effect of the top surface layer is not sufficiently exhibited, while if it exceeds 25.0 μm, the crystal grains of the top surface layer are easily coarsened, and chipping is easily generated.
[0024] (3-2) Middle class The intermediate layer is provided between the laminate layer and the upper layer in order to improve the adhesion between the two layers. The intermediate layer is preferably a TiCNO layer, and the average layer thickness is preferably 0.3 to 3.0 μm. When the average layer thickness is in this range, the adhesion between the two layers is further improved.
[0025] (3-3) Base layer The underlayer is provided between the tool base and the laminate layer to improve the adhesion between the two layers. The underlayer is a Ti compound layer such as a TiC layer, a TiN layer, a TiCN layer, or a TiCNO layer, and the average layer thickness is preferably 0.1 to 20.0 μm. When the average layer thickness is within this range, the adhesion between the two layers is further improved.
[0026] (4) Measurement of average layer thickness The average thickness of each layer constituting the coating layer can be obtained, for example, by cutting the coating layer at a vertical cross section at any position using a focused ion beam system (FIB), a cross section polisher (CP), or the like to prepare a sample for observation, and observing the vertical cross section at multiple locations (e.g., five locations) using an SEM or a transmission electron microscope (TEM), a scanning transmission electron microscope (STEM), or an energy dispersive X-ray spectrometry (EDX) device attached to the SEM or TEM to identify each layer, and measuring and averaging the layer thicknesses.
[0027] 2. Tool base Any known substrate for this type of tool substrate may be used as the tool substrate, provided that it does not impede the achievement of the object of the present invention. Examples include cemented carbide (WC-based cemented carbide, WC, and those containing Co and further containing carbonitrides of Ti, Ta, Nb, etc.), cermets (those mainly composed of TiC, TiN, TiCN, etc.), ceramics (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide, etc.), and cBN sintered body, and any of these is preferable.
[0028] 3. Manufacturing method The coating layer of the present invention can be produced, for example, by the following method.
[0029] (1) Stacking unit layer The following percentages are by volume (volume%). (1-1) 1st layer TiCl4:1.0~3.0%, CH3CN:0.5~2.0%, N2:2.0~30.0%, H2:Remaining Temperature: 850~950℃ Pressure: 5.0~10.0kPa
[0030] (1-2)Second layer TiCl4: 1.0-3.0%, CH3CN: 0.10-0.70%, C2H4: 1.1-3.0%, N2: 0.0-40.0%, H2: balance Temperature: 850~950℃ Pressure: 5.0~10.0kPa
[0031] (2) Upper layer TiCl4:1.0~3.0%, CH3CN:0.5~2.0%, N2:2.0~30.0%, H2:Remaining Temperature: 850~950℃ Pressure: 5.0~10.0kPa EXAMPLES
[0032] Next, an embodiment will be described. Here, as a specific example of the coated tool of the present invention, we will describe its application to an insert cutting tool using a WC-based cemented carbide as the tool base. However, as mentioned above, the tool base is not limited to a WC-based cemented carbide, and the same applies when the coated tool is applied to a drill, end mill, etc.
[0033] First, Co powder, TiC powder, TaC powder, NbC powder, Cr3C2 powder, and WC powder were prepared as raw material powders. These raw material powders were mixed according to the composition shown in Table 1, and wax was added and wet mixed in a ball mill for 72 hours. The mixture was dried under reduced pressure and then pressed at a pressure of 100 MPa. These powder compacts were sintered and processed to the specified dimensions to produce tool substrates A to C made of WC-based cemented carbide having the insert shape of ISO standard CNMA120412.
[0034] Next, coated tools 1 to 10 of the present invention shown in Table 4 were obtained on the tool substrates A to C under the conditions shown in Table 2. The undercoat layer, intermediate layer, and outermost layer were formed under the conditions shown in Table 3. When two types of layers are listed in the layer type column for the outermost layer, the layer on the left is the upper layer, and the corresponding average layer thickness is also listed.
[0035] For comparison, coating layers were formed on the surfaces of these tool substrates A to C under the deposition conditions shown in Table 2 to obtain comparative coated tools 1 to 10 shown in Table 4. The outermost layers were deposited under the conditions shown in Table 3.
[0036] [Table 1]
[0037] [Table 2]
[0038] [Table 3]
[0039] [Table 4]
[0040] Next, the coated tools 1 to 10 of the present invention and the comparative coated tools 1' to 10' were subjected to wet cutting tests 1 and 2 described below while being clamped to the tip of a tool steel bit with a fixing jig, and the flank wear of the cutting edge was measured. The results of each cutting test are shown in Tables 5 and 6.
[0041] Cutting test 1: Wet continuous external cutting Work material: FCD700, round bar with outer diameter of φ300mm Cutting speed: 300m / min Cutout: 2.5 mm Feed rate: 0.25 mm / rev Cutting time: 10 minutes
[0042] Cutting test 2: Wet intermittent cutting Workpiece: FCD700, 4-slit end face of round bar with outer diameter of φ300mm Cutting speed: 250m / min Cutting depth: 2.0 mm Feed rate: 0.2 mm / rev Cutting time: 10 minutes
[0043] [Table 5]
[0044] [Table 6]
[0045] From the results shown in Tables 5 and 6, the coated tools 1 to 10 of the present invention all have excellent wear resistance and chipping resistance while ensuring the adhesion resistance of the coating layer, and therefore do not suffer from chipping even when used to cut steel or cast iron, and exhibit excellent wear resistance over a long period of time. In contrast, the comparative coated tools 1 to 10, which do not satisfy even one of the requirements for the coated tools of the present invention, suffer from chipping when used to cut steel or cast iron, and reach the end of their useful life in a short period of time. [Industrial Applicability]
[0046] As described above, the coated tool of the present invention exhibits excellent wear resistance and anti-abrasion properties while ensuring long-term weldability, and therefore can satisfactorily meet the needs for improving the performance of cutting equipment, reducing labor and energy required for cutting, and reducing costs. [Explanation of symbols]
[0047] 1 Tool base 2 Base layer 3 1st layer 4 2nd layer 5 Upper layer 6 Top layer
Claims
1. A surface-coated cutting tool having a tool base and a coating layer provided on a surface of the tool base, the covering layer has a laminate layer in which seven or more laminate unit layers are laminated and an upper layer on the upper part of the laminate layer, the laminate unit layer has a first layer on the tool base side and a second layer on the opposite side, The first layer has a composition represented by the formula: TiC x N 1-x When expressed as: 0.50≦x≦0.60, The second layer has a composition represented by the formula: TiC y N 1-y When expressed as: 0.65≦y≦1.00, The composition of the upper layer is represented by the formula: TiC z N 1-z where z is a number between 0.50 and 0.60; the laminate layer has columnar crystals, the average width of which is 130 to 300 nm; The ratio of the average thickness of the first layer to the average thickness of the second layer, (average thickness of the first layer) / (average thickness of the second layer), is 0.5 to 3.
0. A surface-coated cutting tool comprising:
2. A TiN layer, a TiCN layer, a TiCNO layer, an Al layer, 2 O 3 2. The surface-coated cutting tool according to claim 1, further comprising one or more of a TiN layer, an AlTiN layer and an AlTiN layer.
Citation Information
Patent Citations
Cutting tool made of surface coating tungsten carbide group super hard alloy excellent in chipping resistance property
JP1994008009A
Surface coated cutting tool
JP1998109206A
Surface coated cutting tool
JP2005186221A
Surface coated member and surface coated cutting tool
JP2006281361A
Surface-coated cutting tool with hard coating layer exhibiting superior chipping resistance
JP2013078837A