Silicon carbide substrate manufacturing method and silicon carbide substrate manufacturing apparatus

The method and apparatus efficiently convert BPDs in silicon carbide substrates to TED by detecting and manipulating SSFs using light irradiation, addressing inefficiencies in existing methods and enhancing substrate quality for power devices.

JP7570749B1Active Publication Date: 2024-10-22ITES CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024543924
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-22
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing silicon carbide substrates are inefficient in eliminating basal plane dislocations (BPD) and Shockley stacking faults (SSF) in the epitaxial layer, leading to increased manufacturing time and reduced quality, especially for large-diameter substrates, and are not optimized for high-quality substrates with minimal BPDs.

Method used

A method and apparatus that utilize inspection, expansion, and contraction steps using specific wavelengths and illuminance of light to detect and convert BPDs into threading edge dislocations (TED) by expanding and contracting SSFs, employing a galvano scanner for precise and simultaneous irradiation.

Benefits of technology

Efficiently reduces or eliminates BPDs in the epitaxial layer, enabling high-quality silicon carbide substrates with a wider usable area for power devices by converting BPDs to TED, thus improving manufacturing efficiency and substrate quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570749000001
    Figure 0007570749000001
  • Figure 0007570749000002
    Figure 0007570749000002
  • Figure 0007570749000003
    Figure 0007570749000003
Patent Text Reader

Abstract

A method for manufacturing a silicon carbide substrate, which is capable of efficiently manufacturing a silicon carbide substrate. A method for manufacturing a silicon carbide substrate 100 having a substrate layer 101 and an epitaxial layer 102, in which basal plane dislocations (BPDs) present in the epitaxial layer 102 are reduced or eliminated, the method comprising the steps of: irradiating the silicon carbide substrate 100 with an inspection light L1 to detect basal plane dislocations (BPDs) present in the epitaxial layer 102; and irradiating an area in which the basal plane dislocations (BPDs) detected in the detection step are present with an extension light L3 that extends Shockley stacking faults (SSFs) from the basal plane dislocations (BPDs). and a shrinking step of irradiating Shockley stacking faults (SSFs) expanded from basal plane dislocations (BPDs) in the expansion step with shrinking light L4 to shrink the Shockley stacking faults (SSFs). When there are multiple basal plane dislocations (BPDs) detected in the detection step, the expansion step irradiates one area where a basal plane dislocation (BPD) exists with expanding light, and then, simultaneously with the shrinking step, irradiates another area where a basal plane dislocation (BPD) exists with expanding light L3, and repeats this for all areas where a basal plane dislocation (BPD) exists.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a silicon carbide substrate having a substrate layer and an epitaxial layer, and an apparatus for manufacturing a silicon carbide substrate. [Background technology]

[0002] Silicon carbide is a wide-gap semiconductor and has been attracting attention in the field of power devices in recent years. Silicon carbide substrates used in power devices are usually manufactured by epitaxial growth, in which an epitaxial layer is grown on a substrate layer. However, since the difference in atomic radius between carbon and silicon atoms is large, silicon carbide is more likely to have crystal defects in the epitaxial layer than gallium nitride, which is also a wide-gap semiconductor. Crystal defects cause forward current degradation that affects device characteristics, and are therefore problematic in the manufacture of power devices.

[0003] The occurrence of forward current degradation in power devices is believed to be caused by carriers being trapped at basal plane dislocations (hereinafter referred to as "BPDs") in the epitaxial layer, and the recombination energy of the trapped carriers expanding Shockley stacking faults (hereinafter referred to as "SSFs"). Therefore, a technology has been developed to suppress the formation of BPDs in the epitaxial layer during the film formation process using the epitaxial growth method. For example, by setting the off-angle to 4°, more than 95% of the crystal defects inherited from the BPDs in the substrate layer to the epitaxial layer formed by the epitaxial growth method can be structurally converted to threading edge dislocations (hereinafter referred to as "TEDs").

[0004] However, in power devices for on-board applications, a large current exceeding the rated current may flow due to special circumstances, such as when the vehicle derails. In such cases, the SSF may expand from BPDs that penetrate the epitaxial layer (BPDs present in the epitaxial layer) without being converted to TEDs in the epitaxial layer. Even if the current density is small, the SSF may expand due to long-term use. Therefore, in order to further improve the stability of power devices for on-board applications, it is desirable to eliminate the BPDs present in the epitaxial layer in the manufacture of silicon carbide substrates.

[0005] Conventionally, a method for manufacturing a silicon carbide substrate that prevents the expansion of the SSF has been proposed (see, for example, Patent Document 1). The method for manufacturing a silicon carbide substrate described in Patent Document 1 prevents the expansion of the SSF by including a step of expanding the SSF in the epitaxial layer by irradiating ultraviolet light and a step of reducing the SSF by heating. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-140184 A Summary of the Invention [Problem to be solved by the invention]

[0007] The method for manufacturing a silicon carbide substrate in Patent Document 1 has a problem in that it is necessary to irradiate the entire surface of the silicon carbide substrate with ultraviolet light to expand the SSF, and it takes time to prevent the expansion of the SSF. In addition, the method for manufacturing a silicon carbide substrate in Patent Document 1 shrinks the SSF by heating the entire silicon carbide substrate, and therefore the step of expanding the SSF and the step of shrinking the SSF cannot be performed simultaneously in parallel. Therefore, when the manufacturing method in Patent Document 1 is applied to large-diameter silicon carbide substrates, which have been in high demand in recent years, it leads to an increase in manufacturing time.

[0008] On the other hand, silicon carbide substrates have made progress in terms of improving their quality. In particular, the BPDs present in the epitaxial layer are now 1 cm 2 It is now possible to suppress the occurrence of BPDs to approximately one or less per silicon carbide substrate (several in a 6-inch wafer). In this regard, the manufacturing method of Patent Document 1 assumes that many BPDs are present even in a high-quality silicon carbide substrate in which only a few BPDs are actually present in the epitaxial layer, and expands and contracts the SSF over the entire surface of the silicon carbide substrate. For this reason, ultraviolet light is irradiated to expand the SSF even in areas where no BPDs are present, which is inefficient.

[0009] The present invention has been made in consideration of the above problems, and has an object to provide a silicon carbide substrate manufacturing method and a silicon carbide substrate manufacturing apparatus that are capable of efficiently manufacturing silicon carbide substrates. [Means for solving the problem]

[0010] The method for manufacturing a silicon carbide substrate according to the present invention for solving the above problems comprises the steps of: A method for producing a silicon carbide substrate having a substrate layer and an epitaxial layer, the method comprising the steps of: reducing or eliminating basal plane dislocations (BPDs) present in the epitaxial layer; a detection step of detecting basal plane dislocations (BPDs) present in the epitaxial layer by irradiating the silicon carbide substrate with an inspection light; an expanding step of irradiating an area where the basal plane dislocations (BPDs) detected in the detection step are present with expanding light that expands Shockley stacking faults (SSFs) from the basal plane dislocations (BPDs); a shrinking step of irradiating the Shockley stacking faults (SSFs) expanded from the basal plane dislocations (BPDs) in the expansion step with shrinkage light for shrinking the Shockley stacking faults (SSFs); Inclusive of When multiple basal plane dislocations (BPDs) are detected in the detection process, the expansion process involves irradiating one region where a BPD is present with the expanding light, and then irradiating another region where a BPD is present with the expanding light simultaneously with the contraction process, and repeating this process for all regions where a BPD is present.

[0011] According to the method for manufacturing a silicon carbide substrate of this configuration, the detection step irradiates the silicon carbide substrate with inspection light to detect BPDs present in the epitaxial layer, and the expansion step irradiates the region where the BPDs detected in the detection step are present with expansion light that expands the SSF from the BPDs, so that the generated carriers are captured by the BPDs present in the epitaxial layer, and the SSF can be expanded from the BPDs in a short time. Next, the contraction step irradiates the SSF expanded from the BPDs in the expansion step with contraction light that contracts the SSF, so that the SSF expanded from the BPDs can be contracted and finally converted into a TED. In this way, by performing the expansion step and the contraction step, the BPDs present in the epitaxial layer are converted into TEDs, and the BPDs present in the epitaxial layer can be eliminated or reduced. Then, the silicon carbide substrate in which the BPDs present in the epitaxial layer are eliminated or reduced has a high yield, and a wider region of the substrate can be used for the manufacture of power devices. In the case where a plurality of BPDs are detected in the detection step, the expansion step irradiates one region where the BPDs are present with the expanding light, and then irradiates another region where the BPDs are present with the expanding light simultaneously with the contraction step, and repeats this process for all regions where the BPDs are present, thereby making it possible to sequentially eliminate or reduce the BPDs present in the epitaxial layer. Thus, according to the present invention, it is possible to efficiently manufacture a high-quality silicon carbide substrate in which the BPDs are reduced or eliminated.

[0012] In the method for manufacturing a silicon carbide substrate according to the present invention, The inspection light has a wavelength of 365 nm or less and an illuminance of 1 W / cm 2 It is preferable that:

[0013] According to the method for manufacturing a silicon carbide substrate having this configuration, the inspection light has a wavelength of 365 nm or less and an illuminance of 1 W / cm 2 By satisfying the condition below, the silicon carbide substrate can be excited and PL light can be emitted from the BPDs present in the epitaxial layer without further expanding the SSF from the BPDs, and therefore the BPDs present in the epitaxial layer can be appropriately detected.

[0014] In the method for manufacturing a silicon carbide substrate according to the present invention, The extended light preferably has a wavelength and illuminance that can reach at least the interface between the substrate layer and the epitaxial layer.

[0015] According to the method for manufacturing a silicon carbide substrate of this configuration, the expanded light has a wavelength and illuminance that reach at least the interface between the substrate layer and the epitaxial layer, so that when the SSF is expanded from the BPDs present in the epitaxial layer, the SSF can be expanded to the fullest extent until the epitaxial layer is filled. In addition, the SSF can be expanded from the BPDs converted to TEDs at the interface (near the interface) between the substrate layer and the epitaxial layer. In this way, by generating sufficient carriers in the epitaxial layer, the SSF is expanded from the BPDs present in the epitaxial layer, and then the expanded SSF can be contracted and efficiently converted to TEDs. Therefore, according to the present invention, it is possible to efficiently manufacture a high-quality silicon carbide substrate in which the BPDs are reduced or eliminated.

[0016] In the method for manufacturing a silicon carbide substrate according to the present invention, The expanded light has a wavelength of 325 to 365 nm and an illuminance of 10 W / cm 2 More preferably, it is equal to or greater than this.

[0017] According to the method for manufacturing a silicon carbide substrate having this configuration, the extended light has a wavelength of 325 to 365 nm and an illuminance of 10 W / cm 2As a result, sufficient carriers can be generated in the epitaxial layer, and the SSF can be sufficiently expanded from the BPDs present in the epitaxial layer. By sufficiently expanding the SSF and then contracting the expanded SSF, the BPDs present in the epitaxial layer are efficiently converted to TEDs, making it possible to efficiently manufacture high-quality silicon carbide substrates in which the BPDs are reduced or eliminated.

[0018] In the method for manufacturing a silicon carbide substrate according to the present invention, The shrinking light preferably has a wavelength of 975 to 1095 nm, or 487 to 548 nm.

[0019] According to the method for manufacturing a silicon carbide substrate having this configuration, the shrinking light has a wavelength of 975 to 1095 nm or 487 to 548 nm, so that the SSF can be shrinked without further expanding the SSF from the BPD. Therefore, the silicon carbide substrate in which the BPDs present in the epitaxial layer have disappeared or been reduced can be cut into any size and used as a product.

[0020] In the method for manufacturing a silicon carbide substrate according to the present invention, In the expanding step and the contracting step, the expanding light and the contracting light are preferably irradiated using a galvano scanner.

[0021] According to the method for manufacturing a silicon carbide substrate having this configuration, the expansion light and contraction light are irradiated using a galvanometer scanner, so that the silicon carbide substrate can be irradiated with the expansion light and contraction light with high accuracy. Moreover, by irradiating the expansion light and contraction light using a galvanometer scanner, the expansion process and the contraction process can be performed simultaneously in parallel. Therefore, it is possible to efficiently convert the BPDs present in the epitaxial layer into TEDs, and eliminate or reduce the BPDs.

[0022] In the method for manufacturing a silicon carbide substrate according to the present invention, The method further includes an additional detection step of irradiating the silicon carbide substrate with the inspection light again after performing the expansion step and the contraction step for all basal plane dislocations (BPDs) detected in the detection step, If a basal plane dislocation (BPD) is detected in the additional detection step, it is preferable to carry out the expansion step and the contraction step.

[0023] According to the method for manufacturing a silicon carbide substrate having this configuration, even if BPDs remain in the epitaxial layer, they can be detected by the additional detection step, and the expansion step and contraction step can be performed again to convert the BPDs present in the epitaxial layer to TEDs, thereby reliably eliminating the BPDs. Therefore, a high-quality silicon carbide substrate with no BPDs present in the epitaxial layer can be manufactured.

[0024] The present invention relates to a manufacturing apparatus for a silicon carbide substrate, and has a characteristic configuration thereof, which is characterized by the following: An apparatus for manufacturing a silicon carbide substrate having a substrate layer and an epitaxial layer, the apparatus comprising: a detection means for detecting basal plane dislocations (BPDs) present in the epitaxial layer by irradiating the silicon carbide substrate with an inspection light; an expanding means for irradiating an area where the basal plane dislocations (BPDs) detected by the detecting means are present with expanding light for expanding Shockley stacking faults (SSFs) from the basal plane dislocations (BPDs); a contraction means for irradiating the Shockley stacking faults (SSFs) expanded from the basal plane dislocations (BPDs) by the expansion means with contraction light for contracting the Shockley stacking faults (SSFs); Inclusive of When there are multiple basal plane dislocations (BPDs) detected by the detection means, the expansion means irradiates one region where a basal plane dislocation (BPD) exists with the expanded light, and then, simultaneously with the contraction of the Shockley stacking faults (SSFs) by the contraction means, irradiates another region where a basal plane dislocation (BPD) exists with the expanded light, and repeats this for all regions where a basal plane dislocation (BPD) exists.

[0025] According to the silicon carbide substrate manufacturing apparatus of this configuration, the detection means irradiates the silicon carbide substrate with inspection light to detect BPDs present in the epitaxial layer, and the expansion means irradiates the region where the BPDs detected by the detection means are present with expansion light that expands the SSF from the BPDs, so that the generated carriers are captured by the BPDs present in the epitaxial layer, and the SSF can be expanded from the BPDs in a short time. Next, the contraction means irradiates the SSF expanded from the BPDs by the expansion means with contraction light that contracts the SSF, so that the SSF expanded from the BPDs can be contracted and finally converted into TED. In this way, by irradiating the expansion light and contraction light, the BPDs present in the epitaxial layer are converted into TEDs, and the BPDs present in the epitaxial layer can be eliminated or reduced. Then, the silicon carbide substrate in which the BPDs present in the epitaxial layer are eliminated or reduced has a high yield, and a wider region of the substrate can be used for the manufacture of power devices. In the case where a plurality of BPDs are detected by the detection means, the expansion means irradiates one region where the BPDs are present with the expanded light, and then irradiates another region where the BPDs are present with the expanded light simultaneously with the contraction of the SSF by the contraction means, and by repeating this for all regions where the BPDs are present, the BPDs present in the epitaxial layer can be eliminated or reduced in sequence. Thus, according to the present invention, it is possible to efficiently manufacture a high-quality silicon carbide substrate in which the BPDs are reduced or eliminated. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic diagram of a silicon carbide substrate. [Diagram 2]Figure 2 is a schematic explanatory diagram showing the expansion of SSFs, where (a) is a perspective view showing the expansion of SSFs from BPDs present in the epitaxial layer, and (b) is a perspective view showing the expansion of SSFs from BPDs converted into TEDs at the interface between the substrate layer and the epitaxial layer. [Diagram 3] FIG. 3 is an explanatory diagram showing a schematic diagram of the process by which BPDs present in an epitaxial layer are converted into TEDs, in which (a) shows a silicon carbide substrate having BPDs present in the epitaxial layer, (b) shows the silicon carbide substrate of (a) after being irradiated with expanding light having a wavelength and illuminance that reaches the interface between the substrate layer and the epitaxial layer, and (c) shows the silicon carbide substrate of (b) after being irradiated with contracting light. [Figure 4] FIG. 4 is a schematic diagram of an apparatus for manufacturing a silicon carbide substrate according to the present invention. [Diagram 5] FIG. 5 is a flowchart showing the steps of a method for manufacturing a silicon carbide substrate according to the present invention. [Figure 6] FIG. 6 is a time chart showing a specific example of the expansion step and contraction step of S5 in the flowchart of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, embodiments of the method for manufacturing a silicon carbide substrate and the apparatus for manufacturing a silicon carbide substrate according to the present invention will be described in detail with reference to the drawings. However, the present invention is not intended to be limited to the configurations described below. Note that the thickness relationships of the layered structures of the silicon carbide substrate shown in Figures 1 to 3 are appropriately exaggerated or simplified for ease of explanation, and do not strictly reflect the magnitude relationships of the actual thicknesses of the layers.

[0028] [Silicon carbide substrate] Before describing a method and an apparatus for manufacturing a silicon carbide substrate according to the present invention, a silicon carbide substrate used in the manufacture of a power device will be described.

[0029] The silicon carbide substrate 100 has a structure in which a substrate layer 101 and an epitaxial layer 102 are stacked. The substrate layer 101 is a substrate of silicon carbide single crystal (4H-SiC) that serves as a base for manufacturing a thin film by an epitaxial growth method. The epitaxial layer 102 is a thin film made of silicon carbide single crystal (4H-SiC) deposited on the substrate layer 101 by an epitaxial growth method. An interface I exists between the substrate layer 101 and the epitaxial layer 102. If BPDs present in the substrate layer 101 pass beyond the interface I, they either penetrate the epitaxial layer 102 as they are or are converted to TEDs at the interface I or the epitaxial layer 102 near the interface I (hereinafter simply referred to as "interface I").

[0030] FIG. 2 is an explanatory diagram showing the extension of SSFs, where (a) is a perspective view showing the extension of SSFs from BPDs present in the epitaxial layer 102, and (b) is a perspective view showing the extension of SSFs from BPDs converted to TEDs at the interface I between the substrate layer 101 and the epitaxial layer 102. In FIG. 2(a) and (b), a part of the silicon carbide substrate 100 is cut out to show a plane parallel to the basal plane. The basal plane is a plane perpendicular to the c-axis

[0001] used to specify a crystal structure. In FIG. 2(b), the TEDs present in the cut-out region are shown by dashed lines. The mechanism by which forward current degradation occurs in a power device manufactured using the silicon carbide substrate 100 is that carriers generated by current flow are captured by the BPDs and recombined, causing the SSFs to extend from the BPDs, resulting in a change in device characteristics. At this time, in the epitaxial layer 102, the SSFs expand from the BPDs formed parallel to the basal plane along a plane parallel to the basal plane to form a triangle shape, as shown in Fig. 2(a). Also, from the BPDs converted to TEDs at the interface I between the substrate layer 101 and the epitaxial layer 102, the SSFs become band-shaped, as shown in Fig. 2(b).

[0031] Here, as shown in FIG. 2(b), the conversion point from BPD to TED is located deep from the surface of the silicon carbide substrate 100 (at the interface I between the substrate layer 101 and the epitaxial layer 102), so the conversion point from BPD to TED does not move at room temperature. However, the conversion point from BPD to TED can be moved by raising the temperature. In this case, by expanding the SSF from the BPD present in the epitaxial layer and the BPD converted to TED at the interface I between the substrate layer 101 and the epitaxial layer 102, the BPD penetrating from the substrate layer 101 to the epitaxial layer 102 can be efficiently converted to TED at the interface I between the substrate layer 101 and the epitaxial layer 102.

[0032] 3 is an explanatory diagram showing a process in which BPDs present in the epitaxial layer 102 are converted into TEDs, in which (a) shows a silicon carbide substrate 100a having BPDs present in the epitaxial layer 102, (b) shows a silicon carbide substrate 100b after irradiating the silicon carbide substrate 100a of (a) with expanding light at a wavelength and illuminance that reaches the interface I between the substrate layer 101 and the epitaxial layer 102, and (c) shows a silicon carbide substrate 100c after irradiating the silicon carbide substrate 100b of (b) with contracting light. As shown in FIG. 3(a), most of the BPDs present in the substrate layer 101 are converted into TEDs at the interface I between the substrate layer 101 and the epitaxial layer 102, but some of the BPDs are inherited to the epitaxial layer 102. BPDs penetrating from the substrate layer 101 to the epitaxial layer 102 (BPDs present in the epitaxial layer 102) emit PL light with a wavelength of 710 nm due to recombination of carriers generated by irradiation of the silicon carbide substrate 100 with excitation light. Therefore, in a PL emission image of the silicon carbide substrate 100 captured through a filter that transmits light with a wavelength of 700 nm or more, if a BPD is present in the epitaxial layer 102, a linear defect image that is brighter than the surroundings can be confirmed. When an area in the PL emission image where a BPD is determined to exist is irradiated with extended light with a wavelength and illuminance that reaches the interface I between the substrate layer 101 and the epitaxial layer 102, as shown in FIG. 3(b), a triangular SSF (SSF shown in a light color) extends from the BPD present in the epitaxial layer 102, and a band-shaped SSF (SSF shown in a dark color) is generated from the BPD converted to TED at the interface I between the substrate layer 101 and the epitaxial layer 102 present in the same area. These SSFs are preferably expanded to their full extent until the epitaxial layer is filled. When the expanded SSFs are irradiated with contraction light at a wavelength that does not expand the SSFs further, the triangular and strip-shaped SSFs contract and the BPDs present in the epitaxial layer 102 are converted to TEDs at the interface I, as shown in Fig. 3(c). In this way, the BPDs present in the epitaxial layer 102 can be eliminated or reduced.

[0033] Based on this knowledge, the present inventor has come to create a silicon carbide substrate manufacturing method and a silicon carbide substrate manufacturing apparatus in which BPDs present in the epitaxial layer 102 are reduced or eliminated at the wafer stage prior to the manufacture of power devices.

[0034] [Silicon carbide substrate manufacturing apparatus] Fig. 4 is a schematic diagram of a silicon carbide substrate manufacturing apparatus 1 of the present invention. The silicon carbide substrate manufacturing apparatus 1 is an apparatus for reducing or eliminating BPDs present in an epitaxial layer 102 of a silicon carbide substrate 100 placed on a mounting table 10. As shown in Fig. 4, the silicon carbide substrate manufacturing apparatus 1 includes a detection means 2, an expansion means 3, and a contraction means 4. The operations of the detection means 2, the expansion means 3, and the contraction means 4 are controlled by a control means 5. Each component of the silicon carbide substrate manufacturing apparatus 1 will be described in detail below.

[0035] <Detection Method> The detection means 2 is a means for irradiating the silicon carbide substrate 100 with inspection light L1 to detect BPDs present in the epitaxial layer 102. The detection means 2 has an inspection light irradiating unit 21, an imaging unit 22, and a determination unit .

[0036] The inspection light irradiating unit 21 irradiates the entire silicon carbide substrate 100 with the inspection light L1. The inspection light L1 has a wavelength of 365 nm or less and an illuminance of 1 W / cm 2 It is preferable that the above-mentioned irradiation conditions are satisfied. Under the above-mentioned irradiation conditions, the inspection light L1 can excite the silicon carbide substrate 100 without further expanding the SSF from the BPDs. By irradiating the entire silicon carbide substrate 100 with the inspection light L1 by the inspection light irradiating unit 21, the BPDs present in the epitaxial layer 102 can emit PL light L2, and the BPDs present in the epitaxial layer 102 can be appropriately detected. As the light source of the inspection light irradiating unit 21, for example, an ultraviolet laser, a mercury xenon lamp, or the like can be used.

[0037] The photographing unit 22 photographs the silicon carbide substrate 100 emitting PL light. The photographing unit 22 may be a digital camera having an image sensor in which solid-state imaging elements such as CCD (Charged-coupled devices) and CMOS (Complementary metal-oxide-semiconductor) are arranged in a two-dimensional array, and the image sensor detects the light incident on the photographing unit 22. The photographing unit 22 is preferably configured to be movable so that an arbitrary position on the silicon carbide substrate 100 can be photographed from the normal direction of the substrate surface. The photographing unit 22 has a filter 22a that transmits light with a wavelength of 700 nm or more. The filter 22a that transmits light with a wavelength of 700 nm or more selectively transmits PL light with a wavelength of 710 nm emitted from the BPD, and may be, for example, a high-pass filter with a transmission band of 700 nm or more. After the inspection light L1 is irradiated from the inspection light irradiating unit 21, the photographing unit 22 transmits the PL light L2 emitted from the silicon carbide substrate 100 through the filter 22a to photograph a PL emission image. In the PL emission image photographed in this manner, a bright linear defect image appears at a position where a BPD exists in the epitaxial layer 102. The photographing unit 22 records the photographed image in a storage (not shown) such as a hard disk.

[0038] The determination unit 23 determines whether or not a BPD exists by referring to the PL light emission image captured by the imaging unit 22. The determination unit 23 is a computer having a CPU, memory, storage, etc., and the CPU reads and executes a program recorded in the memory, thereby realizing a determination function. Specifically, the determination unit 23 extracts a defect image of a BPD, which is a bright linear defect image, by image analysis of the PL light emission image, and determines that a BPD exists. The extraction of the defect image can be performed, for example, by edge detection processing. When the determination unit 23 determines that a BPD exists, the detection means 2 detects the area in which the defect image extracted by the determination unit 23 occurs as an area in which a BPD exists.

[0039] <Extension methods> The extension means 3 is a means for irradiating an area where the BPD detected by the detection means 2 exists with the extended light L3 that extends the SSF from the BPD. By irradiating an area where the BPD detected by the detection means 2 exists with the extended light L3 that extends the SSF from the BPD, carriers generated by the irradiation of the extended light L3 are captured by the BPD present in the epitaxial layer 102, and the SSF is extended from the BPD. Therefore, since the extended light L3 is not irradiated to an area where the BPD does not exist, the SSF can be extended from the BPD in a short time without taking extra time. It is preferable that the extended light L3 has a wavelength and illuminance that reach at least the interface I between the substrate layer 101 and the epitaxial layer 102. Since the expanded light L3 has a wavelength and illuminance that reach at least the interface between the substrate layer 101 and the epitaxial layer 102, when the SSF is expanded from the BPDs present in the epitaxial layer 102, the SSF can also be expanded from the BPDs converted to TEDs at the interface I between the substrate layer 101 and the epitaxial layer 102. In this way, by generating sufficient carriers in the epitaxial layer 102, the SSF can be expanded to the fullest extent to fill the epitaxial layer 102, and the BPDs present in the epitaxial layer 102 can be efficiently converted to TEDs when the SSF is contracted.

[0040] The extended light L3 has a wavelength of 325 to 365 nm and an illuminance of 10 W / cm 2 It is preferable that the wavelength is 355 nm and the illuminance is 100 W / cm or more. 2 It is more preferable that the wavelength of the extended light L3 is 325 to 365 nm and the illuminance is 10 W / cm 2 By satisfying the above, it is possible to generate sufficient carriers in the epitaxial layer 102 and to sufficiently extend the SSF from the BPDs present in the epitaxial layer 102. Note that when the illuminance of the extended light L3 is 10 W / cm 2If it is smaller, the SSF expansion speed becomes slow, and there is a risk that rapid inspection desired in the manufacturing process of power devices cannot be performed. The type of the expansion means 3 is not limited as long as it can irradiate expansion light L3 having a wavelength and illuminance that can reach at least the interface I between the substrate layer 101 and the epitaxial layer 102, and examples of the expansion means include a YAG laser, a He-Cd laser, and an InGaN laser. Among these, it is preferable to use the third harmonic (355 nm) of a YAG laser.

[0041] <Contraction Method> The contraction means 4 is a means for irradiating the SSF expanded from the BPD by the expansion means 3 with contraction light L4 for contracting the SSF. By irradiating the SSF expanded from the BPD by the expansion means 3 with contraction light L4 for contracting the SSF, the SSF expanded from the BPD can be contracted and finally converted into a TED. As a result, the BPD present in the epitaxial layer 102 is converted into a TED, so that the BPD present in the epitaxial layer 102 can be eliminated or reduced, and a wider area of ​​the silicon carbide substrate 100 can be used for manufacturing power devices.

[0042] The wavelength of the contraction light L4 is preferably 975 to 1095 nm or 487 to 548 nm, and more preferably 1064 nm or 532 nm. By using the wavelength of the contraction light L4 of 975 to 1095 nm or 487 to 548 nm, the SSF can be contracted without further expanding the SSF from the BPD. The type of the contraction means 4 is not limited as long as it can irradiate the contraction light L4 with a wavelength equal to or greater than the absorption edge wavelength at which the SSF does not expand, or equal to or less than the absorption edge wavelength, and examples of the contraction means include a YAG laser, a He-Cd laser, and an InGaN laser. Among these, it is preferable to use the fundamental wavelength (1064 nm) or the second harmonic (532 nm) of the YAG laser.

[0043] <Control Means> The control means 5 is a computer having a CPU, memory, storage, etc., and the function of controlling the operations of the detection means 2, expansion means 3, and contraction means 4 is realized by the CPU reading and executing a program recorded in the memory.

[0044] When there are a plurality of BPDs detected by the detection means 2, the control means 5 controls the expansion means 3 and the contraction means 4 so that the expansion means 3 irradiates the expanded light L3 on one area where the BPDs are present, and then irradiates the expanded light L3 on another area where the BPDs are present, simultaneously with the contraction of the SSF by the contraction means 4, and repeats this for all areas where the BPDs are present. For example, when there are three BPDs (A, B, C) detected by the detection means 2, the expansion means 3 first irradiates the expanded light L3 on A to expand the SSF. Next, the contraction means 4 irradiates the contraction light L4 on the SSF generated from A to contract the SSF, and simultaneously, the expansion means 3 irradiates the expanded light L3 on B to expand the SSF. Next, the contraction means 4 irradiates the contraction light L4 on the SSF generated from B to contract the SSF, and simultaneously, the expansion means 3 irradiates the expanded light L3 on C to expand the SSF. Finally, the contraction means 4 irradiates the contraction light L4 onto the SSF generated from C to contract the SSF. In this way, when there are multiple BPDs detected by the detection means 2, the expansion means 3 irradiates one region where the BPDs exist with the expanding light L3, and then irradiates another region where the BPDs exist with the expanding light L3 simultaneously with the contraction of the SSF by the contraction means 4. By repeating this process for all regions where the BPDs exist, it is possible to efficiently eliminate or reduce the BPDs present in the epitaxial layer 102.

[0045] The expanded light L3 and the contracted light L4 are preferably irradiated using a galvanometer scanner. In this embodiment, as shown in FIG. 4, the expansion means 3 includes a light source 31, a light collecting unit 32, and a galvanometer scanner 33. The galvanometer scanner 33 has an X-axis galvanometer mirror 33x, a Y-axis galvanometer mirror 33y, and an actuator (not shown) that rotates the X-axis galvanometer mirror 33x and the Y-axis galvanometer mirror 33y. The light source 31 generates the expanded light L3. The light collecting unit 32 collects the expanded light L3 output from the light source 31 and adjusts it to a desired spot diameter. The galvanometer scanner 33 irradiates the expanded light L3 to the silicon carbide substrate 100 while changing the irradiation direction of the expanded light L3 output from the light collecting unit 32. Similarly, the contraction means 4 includes a light source 41, a light collecting unit 42, and a galvanometer scanner 43. The galvanometer scanner 43 has an X-axis galvanometer mirror 43x, a Y-axis galvanometer mirror 43y, and an actuator (not shown) for rotating the X-axis galvanometer mirror 43x and the Y-axis galvanometer mirror 43y. The light source 41 generates the contraction light L4. The light collecting unit 42 collects the contraction light L4 output from the light source 41 and adjusts it to a desired spot diameter. The galvanometer scanner 43 irradiates the contraction light L4 onto the silicon carbide substrate 100 while changing the irradiation direction of the contraction light L4 output from the light collecting unit 42. In this way, the expansion means 3 and the contraction means 4 irradiate the expansion light L3 and the contraction light L4 using the galvanometer scanners 33 and 43, so that the expansion light L3 and the contraction light L4 can be irradiated onto the silicon carbide substrate 100 with high accuracy, and the expansion and contraction of the SSF can be performed simultaneously in parallel. Therefore, it is possible to efficiently convert the BPDs present in the epitaxial layer 102 into TEDs, and eliminate or reduce the BPDs. In this embodiment, one galvanometer scanner is used for each of the expansion means 3 and the contraction means 4, but for example, if expansion takes longer than contraction of the SSF, the expansion light L3 may be irradiated using multiple galvanometer scanners, and multiple BPDs can be irradiated simultaneously in parallel with the expansion light L3. By irradiating the contraction light L4 from the SSF that has been fully expanded, the BPDs present in the epitaxial layer 102 can be eliminated or reduced more efficiently in a shorter time.

[0046] <Placement table> The mounting table 10 has a built-in heater and heats the silicon carbide substrate 100 mounted on the upper surface. When the expansion means 3 and contraction means 4 irradiate the silicon carbide substrate 100 with the expansion light L3 and contraction light L4, the mounting table 10 is preferably heated so that the temperature of the silicon carbide substrate 100 is 100 to 200° C., and more preferably heated to 100 to 150° C. By heating the silicon carbide substrate 100 to 100 to 200° C., the carrier generation efficiency is improved, and by irradiating the expansion light L3 and contraction light L4, the SSF can be expanded and contracted in a short time, thereby shortening the manufacturing time.

[0047] [Method for manufacturing silicon carbide substrate] Fig. 5 is a flow chart showing the procedure of the method for manufacturing a silicon carbide substrate of the present invention. In the method for manufacturing a silicon carbide substrate of the present invention, a detection step, an expansion step, and a contraction step are performed in order using the silicon carbide substrate manufacturing apparatus 1 of Fig. 4, and an additional detection step is further performed as an optional step. In the flow chart of Fig. 5, the symbol "S" in the figure represents a step.

[0048] <Detection steps: S1 to S4> In the detection step, the detection means 1 irradiates the silicon carbide substrate 100 with the inspection light L1 to detect BPDs present in the epitaxial layer 102.

[0049] In S1, the inspection light irradiating unit 21 irradiates the entire silicon carbide substrate 100 with inspection light L1, thereby exciting the silicon carbide substrate 100 to emit PL light L2. In the detection step, the inspection light L1 has a wavelength of 365 nm or less and an illuminance of 1 W / cm 2 By irradiating the inspection light L1 under the above irradiation conditions, the silicon carbide substrate 100 can be excited and the BPDs present in the epitaxial layer 102 can emit PL light L2 without further expanding the SSF from the BPDs. Therefore, the BPDs present in the epitaxial layer 102 can be appropriately detected.

[0050] In S2, while the silicon carbide substrate 100 is emitting the PL light L2, the photographing unit 22 photographs a PL emission image by transmitting the PL light L2 through a filter 22a that transmits light having a wavelength of 700 nm or more. In general, in a power device such as a SiC-MOSFET, the epitaxial layer 102 is formed to a thickness of about 0.5 to 20 μm and the off angle is set to 4°, so that the length of the BPD in the epitaxial layer 102 photographed from the normal direction of the substrate surface is about 7 to 286 μm. Therefore, the PL emission image photographs BPDs having a length of about 7 to 286 μm at a size corresponding to a plurality of pixels. In the photographing process, the entire silicon carbide substrate 100 may be photographed at once, or the silicon carbide substrate 100 may be divided into a plurality of regions and photographed.

[0051] In S3, the determination unit 23 extracts a BPD defect image, which is a bright linear defect image, in the PL light emission image captured by the imaging unit 22, and determines whether or not a BPD exists. The extraction of the defect image can be performed, for example, by edge detection processing or the like. The PL light emission image is subjected to image analysis to extract a BPD defect image, which is a bright linear defect image, and it is determined that a BPD exists. If it is determined that a BPD exists (S3: YES), the region in which the BPD defect image, which is a bright linear defect image extracted by the determination unit 23, occurs is detected as a region in which a BPD exists (S4). If it is determined that a BPD does not exist (S3: NO), the manufacture of the silicon carbide substrate 100 is terminated.

[0052] <Expansion process / contraction process: S5> In S5, in the expansion step, the expansion means 3 irradiates the region where the BPD detected in the detection step exists with the expansion light L3 that expands the SSF from the BPD, and in the contraction step, the contraction means 4 irradiates the SSF expanded from the BPD in the expansion step with the contraction light L4 that contracts the SSF. By irradiating the region where the BPD detected in the detection step exists with the expansion light L3 that expands the SSF from the BPD, carriers generated by the irradiation of the expansion light L3 are captured by the BPD present in the epitaxial layer 102, and the SSF can be expanded from the BPD in a short time. Next, in the contraction step, the SSF expanded from the BPD in the expansion step is irradiated with the contraction light L4 that contracts the SSF, thereby contracting the SSF expanded from the BPD, and finally converting it to a TED. In this way, by performing the expansion step and the contraction step, the BPD present in the epitaxial layer 102 is converted to a TED, and the BPD present in the epitaxial layer 102 can be eliminated or reduced. Furthermore, the silicon carbide substrate 100 in which the BPDs present in the epitaxial layer 102 have been eliminated or reduced can have a high yield, and a larger area of ​​the silicon carbide substrate 100 can be used for manufacturing power devices.

[0053] The expansion light L3 in the expansion step preferably has a wavelength and illuminance that reach at least the interface I between the substrate layer 101 and the epitaxial layer 102. By having the wavelength and illuminance that reach at least the interface I between the substrate layer 101 and the epitaxial layer 102, when the SSF is expanded from the BPDs present in the epitaxial layer 102, the SSF can be expanded to the fullest extent until the epitaxial layer 102 is filled. In addition, the SSF can be expanded from the BPDs converted to TEDs at the interface I between the substrate layer 101 and the epitaxial layer 102. In this way, by generating sufficient carriers in the epitaxial layer 102, the SSF is expanded from the BPDs present in the epitaxial layer 102, and then the expanded SSF can be contracted and efficiently converted to TEDs. Therefore, it is possible to efficiently manufacture a high-quality silicon carbide substrate 100 in which the BPDs are reduced or eliminated.

[0054] The expansion light L3 in the expansion step has a wavelength of 325 to 365 nm and an illuminance of 10 W / cm 2 or more. By irradiating the extended light L3 under the above irradiation conditions, sufficient carriers can be generated in the epitaxial layer 102, and the SSF can be sufficiently expanded from the BPDs present in the epitaxial layer 102. By sufficiently expanding the SSF and then contracting the expanded SSF, the BPDs present in the epitaxial layer 102 are efficiently converted to TEDs, making it possible to efficiently manufacture a high-quality silicon carbide substrate 100 in which the BPDs are reduced or eliminated.

[0055] The wavelength of the shrinking light L4 in the shrinking step is preferably 975 to 1095 nm, or 487 to 548 nm. By irradiating the shrinking light L4 under the above irradiation conditions, the SSF can be shrunk without further expanding the SSF from the BPD. Therefore, the silicon carbide substrate 100 in which the BPDs present in the epitaxial layer 102 have disappeared or been reduced can be cut into any size and used as a product.

[0056] If multiple BPDs are detected in the detection process, the expansion process involves irradiating one area where the BPDs are present with expansion light L3, and then, simultaneously with the contraction process, irradiating another area where the BPDs are present with expansion light L3. By repeating this process for all areas where the BPDs are present, the BPDs present in the epitaxial layer 102 can be sequentially eliminated or reduced.

[0057] FIG. 6 is a time chart showing a specific example of the expansion step and contraction step of S5 in the flowchart of FIG. 5. FIG. 6 shows a case where the number of regions in which BPDs are present detected in the detection step is n. First, at time t0, the expansion step is started for the first BPD (region in which BPDs are present), and the expansion means 3 irradiates the first BPD with expansion light L3. Next, after the SSF is sufficiently expanded from the first BPD by the expansion step, the contraction step is started at time t1, and the contraction means 4 irradiates the SSF expanded from the first BPD with contraction light L4, which contracts the SSF. At time t1, the expansion step is started for the second BPD in parallel at the same time, and the expansion means 3 irradiates the second BPD with expansion light L3. The expansion step and contraction step are repeated in the same manner, and finally, at time t n In the contraction process, the SSF expanded from the nth BPD is irradiated with contraction light L4, which contracts the SSF. In this embodiment, the contraction process of the nth BPD and the expansion process of the n+1th BPD are started simultaneously, but for example, if the contraction process takes time, the expansion process of the n+1th BPD and the expansion process of the n+2th BPD may be performed during the contraction process of the nth BPD, and the start timing of the expansion process and contraction process can be set appropriately.

[0058] In the expansion step and the contraction step, it is preferable to irradiate the expansion light L3 and the contraction light L4 using the galvano scanner 33. By irradiating using the galvano scanner 33, the expansion light L3 and the contraction light L4 can be irradiated to the silicon carbide substrate 100 with high accuracy. In addition, by irradiating the expansion light L3 and the contraction light L4 using separate galvano scanners, the expansion step and the contraction step can be performed simultaneously. Therefore, it is possible to efficiently convert the BPDs present in the epitaxial layer 102 into TEDs, and to eliminate or reduce the BPDs. In addition, in each of the expansion step and the contraction step, the expansion light L3 and the contraction light L4 can be irradiated using a plurality of galvano scanners. For example, when the expansion light L3 is irradiated using two galvano scanners, the expansion steps of the n-th BPD and the n+1-th BPD can be performed simultaneously in parallel, and the SSF can be expanded from the BPDs in a shorter time. In S5, the control means 5 controls, for example, a galvano scanner to irradiate an arbitrary region with the expanding light L3 and the contracting light L4 at an arbitrary timing.

[0059] <Additional detection process: S6> The additional detection step is a step of confirming whether BPDs remain in the epitaxial layer. If the additional detection step is to be performed (S6: YES), the process returns to S1 and the additional detection step of irradiating the silicon carbide substrate 100 with the inspection light L1 again is performed. The additional detection step is similar to the detection step, and S1 to S4 are performed in order. If a BPD is detected in the additional detection step, the expansion step and contraction step (S5) are performed. If the additional detection step is not to be performed (S6: NO), the manufacture of the silicon carbide substrate 100 is terminated. By performing the additional detection step, even if a BPD remains in the epitaxial layer 102, it can be detected by the additional inspection step. Therefore, the expansion step and contraction step are performed again, and the BPDs present in the epitaxial layer 102 can be converted into TEDs, and the BPDs can be reliably eliminated. Therefore, a high-quality silicon carbide substrate 100 in which no BPDs exist in the epitaxial layer 102 can be manufactured.

[0060] As described above, in the silicon carbide substrate manufacturing method and silicon carbide substrate manufacturing apparatus of the present invention, when multiple BPDs are detected in the detection process, the expansion process irradiates expanded light onto one area where the BPDs are present, and then, simultaneously with the contraction process, irradiates expanded light onto another area where the BPDs are present, and this is repeated for all areas where the BPDs are present, making it possible to efficiently manufacture high-quality silicon carbide substrates in which BPDs are reduced or eliminated. [Industrial Applicability]

[0061] INDUSTRIAL APPLICABILITY The silicon carbide substrate manufacturing method and silicon carbide substrate manufacturing apparatus of the present invention can be used in the manufacturing process of power device elements such as SiC-MOSFETs. [Explanation of symbols]

[0062] 1. Silicon carbide substrate manufacturing equipment 2. Detection Methods 3. Expansion methods 4. Contraction Method 33, 43 Galvanometer Scanner 100 Silicon carbide substrate 101 Substrate layer 102 Epitaxial layer L1 Inspection light L3 Extended Light L4 Contraction Light I interface

Claims

1. A method for manufacturing a silicon carbide substrate having a substrate layer and an epitaxial layer, the method comprising the steps of: reducing or eliminating basal plane dislocations (BPDs) present in the epitaxial layer; a detection step of detecting basal plane dislocations (BPDs) present in the epitaxial layer by irradiating the silicon carbide substrate with an inspection light; an expanding step of irradiating an area where the basal plane dislocations (BPDs) detected in the detection step are present with expanding light that expands Shockley stacking faults (SSFs) from the basal plane dislocations (BPDs); a shrinking step of irradiating the Shockley stacking faults (SSFs) expanded from the basal plane dislocations (BPDs) in the expansion step with shrinkage light for shrinking the Shockley stacking faults (SSFs); Inclusive of When multiple basal plane dislocations (BPDs) are detected in the detection process, the expansion process involves irradiating the expanding light onto one region where basal plane dislocations (BPDs) exist, and then irradiating the expanding light onto another region where basal plane dislocations (BPDs) exist, simultaneously with the contraction process, and repeating this process for all regions where basal plane dislocations (BPDs) exist.

2. The inspection light has a wavelength of 365 nm or less and an illuminance of 1 W / cm 2 The method for manufacturing a silicon carbide substrate according to claim 1 , wherein:

3. The method for manufacturing a silicon carbide substrate according to claim 1 , wherein the extended light has a wavelength and illuminance that reach at least an interface between the substrate layer and the epitaxial layer.

4. The expanded light has a wavelength of 325 to 365 nm and an illuminance of 10 W / cm 2 The method for manufacturing a silicon carbide substrate according to claim 3 .

5. 2. The method for manufacturing a silicon carbide substrate according to claim 1, wherein the shrinking light has a wavelength of 975 to 1095 nm or 487 to 548 nm.

6. The method for manufacturing a silicon carbide substrate according to claim 1 , wherein in the expanding step and the contracting step, the expanding light and the contracting light are irradiated using a galvano scanner.

7. Further comprising an additional detection step of irradiating the silicon carbide substrate with the inspection light again after performing the expansion step and the contraction step for all basal plane dislocations (BPDs) detected in the detection step; 7. The method for manufacturing a silicon carbide substrate according to claim 1, wherein the expansion step and the contraction step are performed when a basal plane dislocation (BPD) is detected in the additional detection step.

8. An apparatus for manufacturing a silicon carbide substrate having a substrate layer and an epitaxial layer, the apparatus comprising: a detection means for detecting basal plane dislocations (BPDs) present in the epitaxial layer by irradiating the silicon carbide substrate with an inspection light; an expanding means for irradiating an area where the basal plane dislocations (BPDs) detected by the detecting means are present with expanding light for expanding Shockley stacking faults (SSFs) from the basal plane dislocations (BPDs); a contraction means for irradiating the Shockley stacking faults (SSFs) expanded from the basal plane dislocations (BPDs) by the expansion means with contraction light for contracting the Shockley stacking faults (SSFs); Inclusive of When there are multiple basal plane dislocations (BPDs) detected by the detection means, the expansion means irradiates one region where the basal plane dislocations (BPDs) exist with the expanded light, and then irradiates another region where the basal plane dislocations (BPDs) exist with the expanded light simultaneously with the contraction of Shockley stacking faults (SSFs) by the contraction means, and repeats this process for all regions where the basal plane dislocations (BPDs) exist.

Citation Information

Patent Citations

  • Multilayer structure, method for manufacturing the same and method for manufacturing semiconductor device

    JP2021014378A

  • Method of manufacturing silicon carbide epitaxial substrate, and method of manufacturing semiconductor device

    JP2024010363A

  • Defect inspection method, defect inspection device, and silicon carbide chip manufacturing method

    JP7368041B1

  • Manufacturing method of silicon carbide epitaxial substrate and manufacturing method of semiconductor device

    JP2019140184A

  • JPP7368041B