Method for treating alkali metal-containing material
By employing chloride roasting in a low oxygen atmosphere and subsequent water washing, the method effectively converts alkali metals in clay substitutes into soluble salts, reducing their content to enhance the suitability of these materials as cement raw materials.
Patent Information
- Application Number
- JP2021023342
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-02-17
AI Technical Summary
The challenge is to efficiently remove high concentrations of alkali metals from clay substitutes for coal ash, such as woody biomass ash, construction soil, and recycled fine powder from waste concrete, to make them suitable as cement raw materials, as alkali metals cause alkaline aggregate reactions in cement.
A method involving chloride roasting in an atmosphere with a low oxygen concentration (10% or less) is used to convert alkali metals into water-soluble salts, followed by water washing and solid-liquid separation to reduce alkali metal content, utilizing chlorine-containing materials like CaCl2 or MgCl2 to enhance the efficiency of alkali metal removal.
The method significantly reduces alkali metal content to 2.5% by mass or less, making the treated material suitable for use as a cement raw material, with improved efficiency and effectiveness compared to conventional methods.
Smart Images

Figure 0007570942000007 
Figure 0007570942000008 
Figure 0007570942000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for treating alkali metal-containing materials, and more particularly to a method for removing alkali metals from clay substitutes for coal ash. [Background technology]
[0002] In light of the impact on global warming, there has been a trend in recent years to reduce the utilization rate of coal-fired power plants, and a decrease in the amount of coal ash generated is expected. As a result, it is predicted that there will be a shortage of coal ash as a cement raw material, and there is a need to secure a substitute for clay to replace coal ash.
[0003] However, many clay substitutes other than coal ash contain high concentrations of alkali metals. If a large amount of alkali metals is contained in cement, it can cause alkali-aggregate reactions, and so alkali metals are generally considered to be repellent components for cement. For this reason, in order to use clay substitutes other than coal ash as a cement raw material in place of coal ash, it is necessary to remove the alkali metals, and the development of removal technologies is underway (see, for example, Patent Document 1 and Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-39038 A [Patent Document 2] JP 2004-59754 A Summary of the Invention [Problem to be solved by the invention]
[0005] Examples of clay substitutes other than coal ash include combustion ash generated from the combustion of woody biomass (hereinafter sometimes referred to as "woody biomass ash"), construction waste soil, recycled fine powder of waste concrete, etc. These clay substitutes contain a high content of alkali metals, especially potassium, compared to coal ash and waste incineration ash. Therefore, in order to use these clay substitutes as a cement raw material, it is necessary to efficiently remove the alkali metals.
[0006] In view of the above problems, an object of the present invention is to provide a method for treating an alkali metal-containing material, which makes it possible to remove alkali metals from the alkali metal-containing material more efficiently than ever before. [Means for solving the problem]
[0007] The method for treating an alkali metal-containing material according to the present invention is characterized by comprising a step (a) of heating a solid alkali metal-containing material together with a chlorine-containing material in an atmosphere with an oxygen concentration of 10% or less to obtain a heat-treated material.
[0008] As described in the above Patent Documents 1 and 2, a method for removing alkali metals from an alkali metal-containing material is known in the art, which involves heating the alkali metal-containing material together with a chlorine-containing material to convert the alkali metal contained in the alkali metal-containing material into a water-soluble salt (alkali metal chloride) (so-called "chlorination roasting"). As a result of intensive research by the present inventors, it has been newly discovered that alkali metals can be removed more efficiently than before by performing chlorination roasting in an atmosphere with a low oxygen concentration. The reason for this is believed to be that performing chlorination roasting in an atmosphere with a low oxygen concentration suppresses the volatilization of chlorine, making it easier to convert the alkali metal into an alkali metal salt. Details will be described later in the section "Mode for carrying out the invention" with reference to examples.
[0009] The oxygen concentration in the atmosphere during chlorination roasting is preferably 10% or less, more preferably 5% or less. The gas other than oxygen contained in the atmosphere is typically nitrogen, but other gases such as carbon dioxide may also be contained.
[0010] In the heat-treated product obtained by the above method, most of the alkali metals contained in the alkali metal-containing material are contained in a state converted to alkali metal salts. Therefore, for example, by performing a water-washing process to dissolve the alkali metals in water, a residue with a reduced alkali metal content can be obtained. In addition, the alkali metal salts may be removed (separated) from the heat-treated product by a method other than the water-washing process. The residue from which the alkali metal salts have been removed has a significantly reduced alkali metal content compared to the alkali metal-containing material before the process, and therefore can be effectively used as a cement raw material to replace coal ash.
[0011] The method for treating an alkali metal-containing material comprises the steps of: A step (b) of washing the heat-treated product obtained in the step (a) with water to obtain a slurry; The method may further include a step (c) of subjecting the slurry obtained in the step (b) to solid-liquid separation to obtain a cake having a lower alkali metal content than the alkali metal-containing material.
[0012] According to the above method, the alkali metal salt fixed as a solid phase in the heat-treated product through step (a) is dissolved into the liquid phase through step (b). Therefore, the residue (cake) obtained after the liquid containing the alkali metal is removed through the solid-liquid separation step in step (c) has a reduced alkali metal content. In particular, according to the above method, since the alkali metal-containing material is heat-treated together with the chlorine-containing material at a low oxygen concentration in step (a), after the end of step (a), most of the alkali metal contained in the alkali metal-containing material is converted into an alkali metal salt. As a result, the cake obtained in step (c) has a significantly reduced alkali metal content compared to the alkali metal-containing material before treatment.
[0013] The step (a) may include a step of heating to a temperature of 650°C to 1200°C.
[0014] If the heating temperature is less than 650°C, it may be difficult to convert the alkali metal into an alkali metal chloride due to the low temperature. If the heating temperature is more than 1200°C, the chlorine contained in the chlorine-containing material may volatilize easily, reducing the amount of contact with the alkali metal and decreasing the reactivity. Depending on the type of alkali metal-containing material, partial melting or enlargement may occur, slowing down the reaction rate of the chlorination roasting.
[0015] The alkali metal-containing material may include at least one selected from the group consisting of fly ash and bottom ash of woody biomass combustion ash.
[0016] The alkali metal-containing material may include at least one selected from the group consisting of construction waste soil and recycled fine powder of waste concrete. In this case, it is preferable that the step (a) includes a step of heating to a temperature of 1000°C to 1200°C.
[0017] Wood biomass combustion ash often contains potassium in the form of glass (K2O·4SiO2), while construction waste soil and recycled fine powder of waste concrete often contain potassium in the form of potassium feldspar (KAlSi3O8). As a result of intensive research by the inventors, we have newly discovered that alkali metal-containing materials, including potassium feldspar, can be easily converted into alkali metal salts by heating them at temperatures of 1000℃ to 1200℃ in an atmosphere with a low oxygen concentration.
[0018] On the other hand, in the case of an alkali metal-containing material that contains alkali metals in the form of glass, such as woody biomass combustion ash, it is possible to efficiently convert it into an alkali metal salt even if the heating temperature is less than 1000° C. As the heating temperature increases, the volatilization of chlorine contained in the chlorine-containing material progresses and the efficiency of chlorination roasting decreases. Therefore, when the alkali metal-containing material to be treated consists only of woody biomass combustion ash, the heating temperature is preferably 650° C. to 1000° C., and more preferably 800° C. to 1000° C.
[0019] When the alkali metal-containing material to be treated includes both alkali metals in the form of glass and alkali metals in the form of potassium feldspar, the heating temperature is preferably in the latter temperature range, that is, 1000° C. to 1200° C. However, from the viewpoint of more efficient chlorination roasting, it is more preferable to carry out the chlorination roasting of the woody biomass combustion ash and the chlorination roasting of the recycled fine powder of construction soil and waste concrete separately, each set at a suitable temperature range.
[0020] The method for treating an alkali metal-containing material comprises the steps of: The method includes a step (d) of pulverizing the alkali metal-containing material to a particle size of 5 mm or less, prior to the step (a); The step (a) may include a step of heating the alkali metal-containing material that has been subjected to the step (d) together with the chlorine-containing material.
[0021] It is assumed that the alkali metal-containing material contains the alkali metal evenly throughout. As in the above method, the exposed area of the alkali metal is increased by performing the crushing process (d) before the heating step (a), so that the reactivity with the chlorine contained in the chlorine-containing material in the heating step (a) is improved, and the alkali metal can be converted to an alkali metal salt more efficiently. In this specification, the "particle size" refers to the smallest sieve opening through which the target object can pass.
[0022] The step (a) may be a step of heating a mixture of the alkali metal-containing material and the chlorine-containing material, in which the ratio (M2 / M1) of the molar amount (M2) of the total chlorine in the chlorine-containing material to the molar amount (M1) of the total alkali metal components in the alkali metal-containing material is within a range of 1 to 5.
[0023] According to the above method, most of the alkali metals contained in the alkali metal-containing material can be efficiently converted into water-soluble salts. If the value of M2 / M1 exceeds 5, chlorine that does not contribute to the chlorination roasting remains, and some of the chlorine-containing material may be wasted. If the value of M2 / M1 is below 1, the heat-treated product obtained after the completion of step (a) may still contain a certain amount of poorly soluble alkali metals.
[0024] The chlorine-containing material may contain one or more selected from the group consisting of industrial raw materials, waste plastics, and waste polyvinyl chloride, containing at least one of CaCl2 and MgCl2.
[0025] According to the above method, chlorine-containing waste materials such as waste plastics and waste polyvinyl chloride can be effectively utilized. In addition, when industrial raw materials such as CaCl2 and MgCl2 are used as chlorine-containing materials, the conditions for forming alkali metal chlorides can be more easily optimized. Effect of the Invention
[0026] According to the present invention, regardless of the form of the alkali metal contained in the alkali metal-containing material, the alkali metal can be converted into an alkali metal chloride with high efficiency. [Brief description of the drawings]
[0027] [Figure 1] 1 is a flow chart illustrating a schematic procedure of a method for treating an alkali metal-containing material. [Diagram 2] FIG. 2 is a block diagram illustrating an example of an apparatus for carrying out the method shown in FIG. 1. [Diagram 3] These are TG curves when calcium chloride is heated in different heating atmospheres. [Figure 4] This is a graph showing the results of potassium removal rate when biomass ash was heated in different heating atmospheres and with different chlorine contents, and corresponds to the results in Table 4 described below. [Diagram 5]This is a graph showing the results of potassium removal rate when heating granite soil in different heating atmospheres and at different heating temperatures, and corresponds to the results in Table 5 described below. [Figure 6] 1 is a graph showing the relationship between the potassium removal rate and the oxygen concentration when biomass ash is heated with different oxygen concentrations in the heating atmosphere, and corresponds to the results in Table 6 described below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The alkali metal-containing material to be treated by the present invention is not particularly limited as long as it is a non-flammable alkali metal-containing material that contains a high concentration of alkali metal components. Examples of the alkali metal-containing material include fly ash and bottom ash of wood biomass ash, construction waste soil, and recycled fine powder of waste concrete.
[0029] Wood biomass ash contains alkali metals (Na, K) in the form of chlorides, carbonates, sulfates, and silicate glasses. When calculated as R2O (R2O=Na2O+0.658×K2O), fly ash from wood biomass ash contains approximately 3% to 50% by mass, and bottom ash from wood biomass ash contains approximately 3% to 20% by mass.
[0030] In addition, recycled fine powder from construction soil and waste concrete contains alkali metals (Na, K) in the form of feldspar (albite, potassium feldspar), and contains about 2% to 8% by mass in terms of RO.
[0031] According to the present invention, the concentration of the alkali metal component contained in the above-mentioned alkali metal-containing material can be reduced to 2.5 mass% or less, more typically 2.0 mass% or less, calculated as RO. This can then be effectively used, for example, as a cement raw material. The concentration of the alkali metal in the alkali metal-containing material can be measured by a well-known method, and a preferred example is a method conforming to JIS R 5204 "Method for fluorescent X-ray analysis of cement."
[0032] The present invention will be described in more detail below with reference to the drawings. However, the present invention is not limited to the embodiments described with these drawings.
[0033] Fig. 1 is a flow chart showing a typical procedure of a method for treating an alkali metal-containing material according to the present invention. Fig. 2 is a block diagram showing a typical example of an apparatus (hereinafter referred to as "treatment apparatus 1") for carrying out the method shown in Fig. 1. In Fig. 2, the flow of solids such as an alkali metal-containing material and liquids such as water are indicated by solid lines with arrows, and the flow of gas is indicated by dashed lines with arrows.
[0034] The method shown in Fig. 1 includes a pulverization step S1, a heating step S2, a water-washing step S3, and a solid-liquid separation step S4. As shown in Fig. 2, a processing device 1 for carrying out the method shown in Fig. 1 includes a pulverization device 3, a heating device 7, and a water-washing device 9. As will be described later, the pulverization step S1 can be omitted as appropriate depending on the properties of the alkali metal-containing material.
[0035] The processing contents in each step shown in FIG. 1 will be described in detail below with reference to FIG. 2 as needed.
[0036] (Crushing process S1) The pulverization process S1 is a process for pulverizing the supplied solid alkali metal-containing material A1 to a size that allows efficient processing in the subsequent steps S2 to S4. In the processing apparatus 1 shown in FIG. 2, the pulverization process S1 is performed by a pulverizer 3.
[0037] Specifically, the particle size of the pulverized alkali metal-containing material A2 obtained through the pulverization process S1 is preferably 5 mm or less, more preferably 4 mm or less, and particularly preferably 3 mm or less. There is no particular lower limit to the particle size of the pulverized alkali metal-containing material A2, but it is 1 μm or more from the viewpoint of preventing the pulverized alkali metal-containing material A2 from being discharged outside the heating furnace of the heating device 7 by the combustion exhaust gas in the subsequent heat treatment process S2. As described above, the "particle size" in this specification refers to the smallest sieve opening through which the target object (here, the pulverized alkali metal-containing material A2) can pass.
[0038] The crushing device 3 desirably crushes the lump alkali metal-containing material A1 to a particle size of 5 mm or less, and the equipment specifications may be appropriately set according to the properties of the lump alkali metal-containing material A1. The crushing device 3 may be a combination of multiple devices.
[0039] Specifically, as the pulverizer 3, a tube mill, a vertical roller mill, a jaw crusher, a gyratory crusher, a cone crusher, an impact crusher, a roll crusher, an aerofoil mill, and the like can be suitably used. When a plurality of these devices are combined to form the pulverizer 3, a classifier is provided between each pulverizer to construct a closed circuit pulverization system, thereby efficiently obtaining the alkali metal-containing pulverized material A2 having a uniform particle size. In this case, the classifier is not particularly limited as long as it can classify the alkali metal-containing pulverized material A2 at a predetermined classification point, and a sieve (in-plane motion sieve, vibrating sieve), a gravity type classifier, an inertia force type classifier, a centrifugal type classifier such as a cyclone, a centrifugal type classifier with a rotating blade such as a cyclone air separator, and the like can be suitably used. Among them, a centrifugal type classifier with a rotating blade such as a cyclone air separator is preferred from the viewpoint of the simplicity of the equipment and the ease of operation and adjustment. As the pulverizing device 3, a pulverizer having a built-in classifier or sieve can also be used.
[0040] In addition, if the supplied solid alkali metal-containing material A1 satisfies the above-mentioned preferred particle size in its actual form, this pulverization process S1 can be omitted. Figure 1 shows both a case where the alkali metal-containing material A1 is sent to the heat treatment process S2 via the pulverization process S1 and a case where the alkali metal-containing material A1 is sent directly to the heat treatment process S2 without passing through the pulverization process S1. Figure 2 also shows both a case where the supplied alkali metal-containing material A1 is pulverized in a pulverizer 3 to obtain an alkali metal-containing pulverized material A2 and a case where the supplied alkali metal-containing material A1 is sent directly to the alkali metal-containing material supplying device 4.
[0041] This pulverization step S1 corresponds to step (d).
[0042] (Heat treatment step S2) The heat treatment step S2 is a step of heating the alkali metal-containing material A1 or the ground alkali metal-containing material A2 having a particle size that meets the standard together with the chlorine-containing material CL. In the processing device 1 shown in FIG. 2, the heat treatment step S2 is performed by a heating device 7. In the following, in order to avoid complexity, the alkali metal-containing material A1 and the ground alkali metal-containing material A2 introduced into the heating device 7 are collectively referred to as "alkali metal-containing material A1 (A2)".
[0043] By this heat treatment step S2, the alkali metal contained in the alkali metal-containing material A1 (A2) is converted into an alkali metal chloride.
[0044] The processing apparatus 1 shown in FIG. 2 includes an alkali metal-containing material supplying device 4 for supplying an alkali metal-containing material A1 (A2) to a heating device .
[0045] The alkali metal-containing material supplying device 4 may include a hopper that stores the alkali metal-containing material A1 (A2), and may be capable of adjusting the supply amount of the alkali metal-containing material A1 (A2) discharged from the hopper toward the heating device 7 by an attached discharge amount adjustment valve. Such a hopper is not particularly limited as long as it can discharge a quantitative amount by adjusting the valve, and a loss-in-weight type hopper or a hopper equipped with a quantitative feeder or rotary feeder can be suitably used.
[0046] The treatment device 1 shown in Fig. 2 is equipped with a chlorine-containing material supplying device 5 for supplying the received chlorine-containing material CL to the heating device 7. The chlorine-containing material CL is not particularly limited as long as it contains chlorine and does not contain a large amount of alkali metal, but suitable materials include waste plastics such as waste polyvinyl chloride that contain at least one organic chlorine in a monomer, and combustible waste that is contaminated with inorganic chlorine compounds such as calcium chloride. The chlorine-containing material supplying device 5 may be provided with a storage tank for the received chlorine-containing material CL.
[0047] The chlorine-containing material CL preferably contains 0.8% by mass or more of chlorine, more preferably 1.2% by mass or more, and particularly preferably 2% by mass or more. The chlorine concentration in the chlorine-containing material CL can be measured by a known method, for example, a method conforming to JIS R 5204 "Fluorescent X-ray analysis method for cement".
[0048] From the viewpoint of efficiently carrying out the reaction between the alkali metal in the alkali metal-containing material A1 (A2) and the chlorine in the chlorine-containing material CL in the heat treatment step S2, it is preferable that the chlorine-containing material CL is small in size and exists adjacent to the alkali metal-containing material A1 (A2). Specifically, the size of the chlorine-containing material CL may be approximately the same as that of the alkali metal-containing material A1 (A2), and the particle size is preferably 5 mm or less, more preferably 4 mm or less, and particularly preferably 3 mm or less.
[0049] From the above viewpoint, a classification device for removing coarse materials from the received chlorine-containing material CL and a crushing and classifying device for reducing the coarse materials to a predetermined particle size may be provided upstream of the storage tank provided in the chlorine-containing material supplying device 5. These classification devices and crushing and classifying devices may be used appropriately depending on the state of the received chlorine-containing material CL.
[0050] The chlorine-containing material supplying device 5 is preferably configured to be equipped with an emission amount adjusting device such as an emission amount adjusting valve, so that the amount of the chlorine-containing material CL supplied to the heating device 7 can be adjusted. In this case, the amount of chlorine supplied to the heating device 7 can be appropriately managed by appropriately controlling the emission amount adjusting device.
[0051] Specifically, the ratio of the alkali metal-containing material A1 (A2) and the chlorine-containing material CL to be treated in the heat treatment step S2 is preferably set so that the ratio (M2 / M1) of the molar amount (M1) of the total chlorine in the chlorine-containing material CL to be subjected to the heat treatment step S2 in a unit time to the molar amount (M2) of the total alkali metal components in the alkali metal-containing material A1 (A2) to be subjected to the heat treatment step S2 in a unit time is 1 to 5. The value of the ratio (M2 / M1) is more preferably 2 to 5. If the value of the ratio (M2 / M1) is less than 1, the amount of chlorine is small, so that a large amount of alkali metal components that cannot react with chlorine may remain among the alkali metal components in the alkali metal-containing material A1 (A2). On the other hand, if the value of the ratio (M2 / M1) is more than 5, the amount of chlorine that volatilizes and dissipates may increase, accelerating the progress of corrosion of the equipment.
[0052] As described above, the heating device 7 heats the alkali metal-containing material A1 (A2) and the chlorine-containing material CL together. Specifically, the chlorine-containing material CL is supplied from the chlorine-containing material supplying device 5, and the alkali metal-containing material A1 (A2) is supplied from the alkali metal-containing material supplying device 4 to the heating device 7, and the chlorine-containing material CL and the alkali metal-containing material A1 (A2) are heated together in the heating device 7. As a result, the alkali metal in the alkali metal-containing material A1 (A2) reacts with the chlorine in the chlorine-containing material CL to produce a chloride of the alkali metal.
[0053] The heating temperature in the heat treatment step S2 is preferably 650°C to 1200°C from the viewpoint of efficiently causing chlorination roasting by the alkali metal in the alkali metal-containing material A1 (A2) and the chlorine in the chlorine-containing material CL while not melting the alkali metal-containing material A1 (A2).
[0054] As described later, the more preferable temperature conditions vary depending on the form of the alkali metal contained in the alkali metal-containing material A1 (A2). Specifically, when the alkali metal-containing material A1 contains the alkali metal in the form of glass, such as wood biomass combustion ash, efficient chlorination roasting occurs even at 1000°C or less, so 650°C to 1000°C is more preferable, and 800°C to 1000°C is particularly preferable. When the alkali metal-containing material A1 contains the alkali metal in the form of feldspar (especially potassium feldspar), such as construction waste soil or recycled fine powder of waste concrete, the effect of chlorination roasting may not be sufficiently obtained at a temperature condition of about 800°C, so 1000°C to 1200°C is more preferable.
[0055] In particular, when the heating temperature in the heat treatment step S2 is high, chlorine is likely to volatilize from the chlorine-containing material CL. If a large amount of chlorine volatilizes, the probability of contact between the alkali metal contained in the alkali metal-containing material A1 (A2) and chlorine decreases, and it is assumed that the rate at which the alkali metal is converted to an alkali metal chloride decreases. And, the higher the heating temperature, the more significant this problem becomes.
[0056] Therefore, in the present invention, even when the heat treatment step S2 is performed at a high temperature exceeding 800° C., in order to efficiently convert the alkali metal into an alkali metal chloride, the heat treatment step S2 is performed in an atmosphere with a low oxygen concentration. Specifically, the oxygen concentration in the atmosphere is preferably 10% or less, and more preferably 5% or less. The lower limit of the oxygen concentration in the atmosphere is 0%, and is typically a nitrogen atmosphere.
[0057] The inventors believe that the reason for this is that when the atmosphere contains a lot of oxygen (e.g., air atmosphere), the reaction of the following formula (1) becomes dominant, and when the atmosphere contains little oxygen (e.g., nitrogen atmosphere), the reaction of the following formula (2) becomes dominant. Note that in the following formulas (1) and (2), CaCl2 (calcium chloride) is given as an example of a chlorine-containing substance CL. As will be described later with reference to the examples, it has been confirmed that the volatilization rate of CaCl2 is slower than that of Cl2 (chlorine). CaCl2(s) + 1 / 2O2(g) → CaO(s) + Cl2(g) …(1) CaCl2(s) → CaCl2(g) …(2)
[0058] The heating time in the heat treatment step S2 may be appropriately set within a range of 10 minutes to 2 hours depending on the heating temperature. In order to sufficiently react the alkali metal in the alkali metal-containing material A1 (A2) with the chlorine in the chlorine-containing material CL, the heating time needs to be short when the heating temperature is high and long when the heating temperature is low. Specifically, when the alkali metal-containing material A1 (A2) is wood biomass ash, it is preferable to set the heating time to 30 minutes to 2 hours when the heating temperature is 650°C, and 10 minutes to 60 minutes when the heating temperature is 1000°C. In addition, when the alkali metal-containing material A1 (A2) is construction generated soil or recycled fine powder of waste concrete, it is preferable to set the heating time to 30 minutes to 2 hours when the heating temperature is 1000°C, and 10 minutes to 60 minutes when the heating temperature is 1200°C.
[0059] In the heating device 7, in order to efficiently generate the reaction to produce the alkali metal salt, it is desirable to heat the alkali metal-containing material A1 (A2) and the chlorine-containing material CL in a state of being sufficiently mixed. From this viewpoint, the heating device 7 can be configured as an internal combustion rotary kiln. If the firing furnace is a rotary kiln in which rotational motion occurs, it is possible to perform the heat treatment while physically and continuously mixing and stirring the alkali metal-containing material A1 (A2) and the chlorine-containing material CL, which are the objects to be heat-treated.
[0060] As described above, the atmosphere in the heating device 7 preferably has an oxygen concentration of 10% or less, and in the example of Fig. 2, the combustion gas G1 is fed into the heating device 7 from the gas source 34 through the intake fan 33. Note that the gas source 34 here may be an air separation device that separates oxygen from air, or may be a gas exhaust passage through which exhaust gas from another combustion furnace is discharged.
[0061] Also, air may be introduced into the heating device 7 through an intake fan 33. In this case, the amount of intake air and the amount of fuel burned may be appropriately adjusted to reduce the oxygen concentration in the atmosphere within the heating device 7.
[0062] In a rotary kiln, gas G1 used as combustion gas for the internal combustion burner 31 by the intake fan 33 flows inside the kiln in a direction countercurrent to the flow of the alkali metal-containing material A1 (A2) and the chlorine-containing material CL, and is then discharged outside the kiln as combustion exhaust gas G2.
[0063] In addition, since both alkali metals and chlorine are components that tend to volatilize during heat treatment, the combustion exhaust gas G2 may contain alkali metals and chlorine. Therefore, for example, in the flue of the exhaust system of the heating device 7, at a location where the temperature is below the freezing point of the chloride of the alkali metal, precipitation of the chloride may occur. Such chloride may be recovered and used as fertilizer, etc.
[0064] The heating device 7 is not particularly limited as long as it can heat the mixture of the alkali metal-containing material A1 (A2) and the chlorine-containing material CL in a temperature range of 650°C to 1200°C (preferably 800°C to 1200°C), and a heating furnace such as a fixed furnace, a stoker furnace, a rotary kiln, a fluidized bed furnace, a vertical furnace, a multi-stage furnace, etc. Among them, the above-mentioned rotary kiln is preferable from the viewpoint of physical stirring.
[0065] A storage tank for the supplied alkali metal-containing material A1 (A2) may be attached to the heating device 7. Furthermore, a supply device for quantitatively supplying the alkali metal-containing material A1 (A2) from the storage tank to the heating device 7 may be attached. In this case, the alkali metal-containing material supply device 4 may be integrated with the heating device 7.
[0066] A heat-treated product P1, which is a mixture of an alkali metal-containing material A1 (A2) containing an alkali metal in a state where the alkali metal has been converted into an alkali metal chloride and an incineration residue of a chlorine-containing material CL, is discharged from the heating device 7. The discharged heat-treated product P1 is sent to a water washing device 9.
[0067] This heat treatment step S2 corresponds to step (a).
[0068] (Water washing process S3) The water-washing process S3 is a process for washing the heat-treated product P1 obtained in the heat treatment process S2. The water-washing process S3 dissolves and removes water-soluble alkali metal chlorides contained in the heat-treated product P1. In the processing device 1 shown in FIG. 2, the water-washing process S3 is performed by a water-washing device 9.
[0069] The solvent used in the water washing step S3 is preferably industrial water (fresh water). Potassium chloride (KCl) and sodium chloride (NaCl) both have very high solubility in water, and the solubility does not change significantly even if the water temperature is changed. Therefore, the water used as the solvent in the elution tank may be room temperature water in an amount of at least three times, preferably at least four times, more preferably at least five times the mass of the heat-treated product P1 supplied from the heat treatment step S2.
[0070] In the water washing device 9, the heat-treated material P1 supplied from the heating device 7 is mixed with water W1 to generate a slurry Lr1, and then the slurry Lr1 is continuously stirred to dissolve the water-soluble alkali metal salt in the heat-treated material P1 in the water.
[0071] As an example, the water washing device 9 shown in Fig. 2 is provided with a supply hopper 11 for the heat-treated material P1 and a supply device 13 for water W1. The water washing device 9 is also provided with a slurry agitator 35 for mixing the heat-treated material P1 and the water W1 and agitating the slurry Lr1 generated by the mixing. As the slurry agitator 35, for example, a general paddle type or screw type may be used, and in the embodiment shown in Fig. 2, an agitator blade is provided.
[0072] A crushing device for crushing large-diameter objects in the received heat-treated object P1 to an appropriate size may be provided upstream of the supply hopper 11. This crushing device may be used appropriately depending on the state of the heat-treated object P1 supplied from the heat treatment step S2.
[0073] The stirring time of the slurry Lr1 in the water washing treatment step S3 is preferably 10 minutes or more, more preferably 15 minutes or more, and particularly preferably 20 minutes or more. Since water-soluble alkali metal salts are usually very soluble in water, no special conditions are required for stirring the slurry Lr1.
[0074] This water washing treatment step S3 corresponds to step (b).
[0075] (Solid-liquid separation process S4) The slurry Lr1 in which the alkali metal is dissolved in water by the water washing treatment step S3 is separated into a solid (cake C1) whose moisture content has been effectively reduced and which can be used as a cement raw material, etc., and wastewater W3 by a solid-liquid separator 17 installed in the downstream stage.
[0076] When transporting the slurry Lr1 to the solid-liquid separator 17, a general-purpose slurry liquid transport device (not shown) such as a slurry centrifugal pump, a piston pump, a mono pump, or a hose pump may be used.
[0077] As the solid-liquid separator 17, a general-purpose filter such as a filter press, a pressurized leaf filter, a screw press, a belt press, a belt filter, etc. may be used. In the embodiment shown in Fig. 2, the solid-liquid separator 17 is illustrated as being composed of a filter press.
[0078] The solid-liquid separator 17 is provided with a supply device 15 for washing water W2, and separates the transported slurry Lr1 into a cake C1 (solid phase) of the washed product and wastewater W3 (liquid phase) containing alkali metals. At this time, the cake C1 is separated while being washed with the washing water W2. As the washing water W2, room temperature water may be used in an amount of at least three times, preferably at least four times, and more preferably at least five times the mass of the washed product.
[0079] The cake C1 separated by the solid-liquid separator 17 has an alkali metal component concentration reduced to 2.5 mass % or less, more typically 2.0 mass % or less, and can be effectively used as a cement raw material, etc. The alkali metal concentration here refers to an analytical value obtained by a well-known method, for example, an analytical value obtained by a method conforming to JIS R 5204 "Method for fluorescent X-ray analysis of cement" or an analytical value obtained by ICP atomic emission spectrometry on an acid-digested sample.
[0080] This solid-liquid separation treatment step S4 corresponds to step (c). EXAMPLES
[0081] Specific test examples are presented below to explain the present invention in more detail, but the present invention is not limited to the embodiments of these test examples.
[0082] (Verification 1) Calcium chloride, an example of a chlorine-containing substance CL, was placed in a thermogravimetric differential thermal analyzer (TG-DTA) and the change in weight was measured while changing the temperature in two atmospheres, air and nitrogen. The results are shown as a TG curve in Figure 3. In Figure 3, the horizontal axis indicates temperature [°C] and the vertical axis indicates the ratio of the weight loss (weight after treatment - weight before treatment) to the weight of the sample before treatment.
[0083] According to FIG. 3, when heated to around 800°C, there is almost no weight loss due to temperature increase. However, when the temperature exceeds 850°C, the weight loss rate due to temperature increase is higher in the air atmosphere than in the nitrogen atmosphere. In particular, when calcium chloride is heated in a nitrogen atmosphere within the range of 800°C to 1300°C, the weight loss is smaller than that in the air atmosphere. It is confirmed that even in the nitrogen atmosphere, the weight loss rate increases with temperature increase under temperature conditions exceeding 1200°C.
[0084] When calcium chloride is heated in an atmosphere that contains a lot of oxygen, such as air, the reaction shown in formula (1) above becomes dominant, and it is believed that the weight is reduced by the evaporation of chlorine. CaCl2(s) + 1 / 2O2(g) → CaO(s) + Cl2(g) …(1)
[0085] On the other hand, when calcium chloride is heated in an atmosphere with low oxygen concentration or no oxygen (here, a nitrogen atmosphere), the reaction of the above formula (2) becomes dominant, and it is considered that the weight is reduced by the evaporation of calcium chloride itself, which is the object to be heated. CaCl2(s) → CaCl2(g) …(2)
[0086] The results of FIG. 3 suggest that the volatilization rate of chlorine is faster than that of calcium chloride. In other words, assuming that the mixture of the chlorine-containing material CL and the alkali metal-containing material A1 (A2) is heated at about 1000° C. in the heat treatment step S2, when the heating furnace of the heating device 7 is in an air atmosphere, chlorine is easily volatilized from the chlorine-containing material CL, and the reaction efficiency with the alkali metal-containing material A1 (A2) is reduced. On the other hand, when the heating furnace of the heating device 7 is in a nitrogen atmosphere, the volatilization of chlorine is suppressed, and the contact probability between the chlorine contained in the chlorine-containing material CL and the alkali metal contained in the alkali metal-containing material A1 (A2) can be maintained high, and the alkali metal chloride can be produced with high efficiency. In this verification, the case where CaCl2 (calcium chloride) is used as the chlorine-containing material CL is taken up, but similar results can be obtained even when MgCl2 (magnesium chloride) or BaCl2 (barium chloride) is used.
[0087] (Verification 2) Two types of materials were used as the alkali metal-containing material A1. The first material was fly ash from woody biomass ash collected in an exhaust gas dust collector (bag filter) of a biomass power plant (circulating fluidized bed boiler), and the second material was decomposed granite. Table 1 shows the chemical composition of each of the alkali metals, which was obtained by analyzing an acid-digested sample using ICP emission spectroscopy, and the other chemical components, which were obtained by analyzing a pellet sample using X-ray fluorescence analysis. Note that, as described above, R2O in Table 1 indicates the value calculated as the total amount of alkali metal components in this composition using "R2O = Na2O + 0.658 × K2O".
[0088] [Table 1]
[0089] Table 2 shows the results of XRD analysis of wood biomass ash as the first material of alkali metal-containing material A1, and Table 3 shows the results of XRD analysis of granite soil as the second material of alkali metal-containing material A1. In Tables 2 and 3, the results of XRD analysis indicate that a large amount of a metal was present, that a presence was confirmed, and that a trace amount was present, with "◎", "○", and "△", respectively.
[0090] [Table 2]
[0091] [Table 3]
[0092] Table 2 shows that in wood biomass ash, potassium as an alkali metal exists mainly in the form of glass, whereas in granite soil, potassium exists mainly in the form of feldspar (potassium feldspar).
[0093] The alkali metal-containing material A1 was mixed with a chlorine-containing material (CaCl2 reagent powder) having a molar number that is a predetermined ratio to the content (mol) of potassium as an alkali metal component in the alkali metal-containing material A1, and then the mixture was left to stand in a thermostatic electric furnace for 60 minutes with the temperature and atmosphere set to the conditions shown in Tables 4 to 6 to obtain a heat-treated material P1. The mixture was then stirred for 30 minutes at room temperature with four times the amount of water as the heat-treated material P1, and the resulting slurry Lr1 was suction-filtered, washed with the same amount of water as used for preparing the slurry Lr1, and filtered to obtain a cake C1. The particle size of the alkali metal-containing material A1 used for heating was 35 μm (median diameter) in the case of woody biomass ash and 155 μm (median diameter) in the case of granite.
[0094] The content of alkali metal components in the resulting cake C1 was determined by analyzing an acid-decomposed sample by ICP atomic emission spectrometry. The results are shown in Tables 4 to 6 and in Figs. 4 to 6.
[0095] [Table 4]
[0096] [Table 5]
[0097] [Table 6]
[0098] In Tables 4 to 6, #A11, #B11, etc. are used as level codes to identify the test conditions, and the alphabet (A, B) following the # in this code indicates the type of sample used as the alkali metal-containing material A1, with "A" corresponding to biomass ash and "B" corresponding to granite soil. The numbers (1, 2) displayed following the alphabet indicate the atmosphere during heating, with "1" corresponding to an oxygen concentration of 15% or more, including air, and "2" corresponding to an oxygen concentration of 10% or less, including nitrogen. The numbers at the very end of the list correspond to identifiers to distinguish them from one another.
[0099] In addition, the K removal rate was calculated using the following formula (3). K removal rate=[d1-{(1-d2)-d3}×d4] / d1 …(3) Here, the symbols in equation (3) have the following values: d1: The content (concentration) of K (potassium) contained in the alkali metal-containing material A1 before heat treatment d2: Weight loss rate of the alkali metal-containing material A1 due to the heat treatment step S2 d3: Weight loss rate of the alkali metal-containing material A1 due to the water washing treatment step S3 and the solid-liquid separation treatment step S4 d4: K content (concentration) in the cake C1 obtained after the solid-liquid separation process S4
[0100] The K content of the biomass ash used in the experiment before treatment was d1 = 3.4%, and the K content of the granite soil before treatment was d1 = 3.6%.
[0101] Table 4 shows the comparative results of the amount of potassium removed when the amount of chlorine-containing material CL mixed is changed, when biomass ash is used as the alkali metal-containing material A1, the heating temperature is common at 800°C, the heating atmosphere is air (levels #A11 to #A13), and the heating atmosphere is nitrogen (levels #A21 to #A23). Figure 4 is a graph of the results of Table 4.
[0102] Comparing level #A11 and level #A21, it can be seen that the potassium removal rate is higher in the nitrogen atmosphere than in the air atmosphere, even if the amount of chlorine-containing material CL is the same. This tendency can also be understood by comparing level #A12 and level #A22, and level #A13 and level #A23.
[0103] In addition, when comparing levels #A11 to #A13 in which the heating atmosphere is air, the K removal rate from the alkali metal-containing material A1 clearly decreases when Cl / K is decreased, i.e., when the amount of the chlorine-containing material CL mixed is decreased. In contrast, when comparing levels #A21 to #A23 in which the heating atmosphere is nitrogen, the degree of decrease in the K removal rate is mitigated compared to when the heating atmosphere is air, even when Cl / K is decreased. In other words, even in the case of level #A21 where Cl / K=1, a K removal rate is achieved that is almost the same as that in the case of the heating atmosphere being air and Cl / K=2 (level #A13). From this, it can be seen that by changing the heating atmosphere from air to nitrogen, the amount of the chlorine-containing material CL used in the heat treatment step S2 can be reduced while still achieving an equal or higher potassium removal rate.
[0104] Table 5 shows the comparative results of the amount of potassium removed when the heating temperature was changed from 800°C to 1200°C for the cases where decomposed granite soil was used as the alkali metal-containing material A1, the amount of chlorine-containing material CL mixed was the same, the heating atmosphere was air (levels #B11 to #B14) and the heating atmosphere was nitrogen (levels #B21 to #B24). Figure 5 is a graph of the results of Table 5.
[0105] Comparing levels #B12 and #B22, #B13 and #B23, and #B14 and #B24, it can be seen that when the heating temperature is 1000°C or higher, the potassium removal rate is higher in a nitrogen atmosphere than in an air atmosphere, even if the heating temperature and the mixed amount of chlorine-containing material CL are the same.
[0106] In contrast, when the heating temperature is 800°C, comparing standard #B11 and standard #B21, no substantial difference in the potassium removal rate is found between air and nitrogen atmospheres. This result is presumably due to the fact that in the case of granite, potassium exists in the form of potassium feldspar, so the reaction rate with chlorine is slow at 800°C, and there is no difference in the amount of reaction due to the atmosphere.
[0107] In other words, from the results of Table 5 and Figure 5, it can be seen that when using granite as the alkali metal-containing material A1, in other words when using a material containing potassium in the form of potassium feldspar, it is preferable to set the heating temperature to 1000°C or higher and to have the heating atmosphere have a low oxygen concentration.
[0108] Table 6 shows the comparative results of the amount of potassium removed when biomass ash is used as the alkali metal-containing material A1, the heating temperature and the mixed amount of the chlorine-containing material CL are kept the same (heating temperature 800°C, Cl / K=1), and the oxygen concentration in the heating atmosphere is changed within the range of 0% to 21%. Figure 6 is a graph of the results of Table 6.
[0109] In Table 6, the case where the oxygen concentration in the atmosphere is 0% corresponds to a nitrogen atmosphere, and is the same as level #A21 in Table 4. In Table 6, the case where the oxygen concentration in the atmosphere is 21% corresponds to an air atmosphere, and is the same as level #A11 in Table 4.
[0110] According to Fig. 6, when the oxygen concentration in the atmosphere is changed within the range of 0% to 10%, the K removal rate decreases almost linearly as the oxygen concentration increases. In contrast, when the oxygen concentration exceeds 10%, the degree of decrease in the K removal rate is mitigated. In particular, when the oxygen concentration is 15% or more, the K removal rate does not differ significantly from that in the air atmosphere.
[0111] 6 and Table 6 show that by performing heat treatment with an oxygen concentration of 10% or less, the potassium removal rate can be increased even if the amount of chlorine-containing material CL used in heat treatment step S2 is the same. This result suggests that by lowering the oxygen concentration in the atmosphere, the reaction of formula (2) becomes more dominant than the reaction of formula (1) above, suppressing the progress of chlorine volatilization and maintaining a high probability of contact between chlorine and the alkali metal contained in the alkali metal-containing material A1, thereby enabling the efficient production of alkali metal chlorides. [Explanation of symbols]
[0112] 1: Processing equipment 3: Crushing device 4: Alkali metal-containing material supply device 5: Chlorine-containing material supply device 7: Heating device 9:Water washing device 11: Supply hopper 13:Water supply device 15: Cleaning water supply device 17:Solid-liquid separator 31: Internal combustion burner 33: Intake fan 34: Gas source 35: Slurry mixing device A1: Alkali metal-containing material A2: Ground material containing alkali metals C1: Cake CL: Chlorine content G1: Atmospheric gas G2: Combustion exhaust gas Lr1: Slurry P1: Heat-treated material W1:Water W2: Cleaning water W3: Drainage
Claims
1. The method includes a step (a) of heating a solid alkali metal-containing material together with a chlorine-containing material in an atmosphere with an oxygen concentration of 10% or less to obtain a heat-treated product, The alkali metal-containing material contains at least one selected from the group consisting of construction waste soil and recycled fine powder of waste concrete, The method for treating an alkali metal-containing material, wherein the step (a) includes a step of heating to a temperature of 1000°C to 1200°C.
2. A step (b) of washing the heat-treated product obtained in the step (a) with water to obtain a slurry; 2. The method for treating an alkali metal-containing material according to claim 1, further comprising a step (c) of subjecting the slurry obtained in the step (b) to solid-liquid separation to obtain a cake having a lower alkali metal content than the alkali metal-containing material.
3. The method includes a step (d) of pulverizing the alkali metal-containing material to a particle size of 5 mm or less, prior to the step (a); 3. The method for treating an alkali metal-containing material according to claim 1, wherein the step (a) includes a step of heating the alkali metal-containing material that has been subjected to the step (d) together with the chlorine-containing material.
4. The method for treating an alkali metal-containing material according to any one of claims 1 to 3, characterized in that the step (a) is a step of heating a mixture of the alkali metal-containing material and the chlorine-containing material, in which a ratio (M2 / M1) of the molar amount (M2) of total chlorine in the chlorine-containing material to the molar amount (M1) of all alkali metal components in the alkali metal-containing material is within a range of 1 to 5.
5. The chlorine-containing substance is CaCl 2 or MgCl 2 The method for treating an alkali metal-containing material according to any one of claims 1 to 4, characterized in that the material contains one or more selected from the group consisting of industrial raw materials, waste plastics, and waste polyvinyl chloride, and at least one of the above.
Citation Information
Patent Citations
Method for treating waste
JP2003039038A
Method for treating waste material and method for manufacturing raw material of cement
JP2004059754A
Method for treating alkali metal-containing waste
JP2013013843A
Combustible material treatment apparatus, and combustible material treatment method
JP2020099885A
Method of removing alkali metal and device for removing alkali metal
JP2020157230A