Curable composition and cured product thereof
The use of an onium salt as an acid generator in curable compositions addresses the limitations of photoreactivity and thermal stability, resulting in improved curability and heat resistance for electronic and optical applications.
Patent Information
- Application Number
- JP2021034931
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-05
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-03-05
AI Technical Summary
Existing curable compositions used in cationic polymerization lack sufficient photoreactivity and thermal stability, leading to issues with curability, adhesiveness, transparency, and heat resistance, which are crucial for applications in electronic devices and optical elements.
Incorporation of an onium salt represented by a specific general formula as an acid generator in the curable composition, enhancing both photoreactivity and thermal stability, thereby improving curability, adhesiveness, transparency, and heat resistance.
The composition exhibits excellent curability, adhesiveness, transparency, and heat-resistant properties, making it suitable for optical elements and electronic devices, particularly in high-temperature conditions.
Smart Images

Figure 0007572267000001 
Figure 0007572267000002 
Figure 0007572267000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable composition which contains an acid generator having a specific structure and a cationic polymerizable compound and which has excellent curability and thermal stability, and to a cured product thereof. [Background technology]
[0002] As the curable composition, various compositions have been proposed so far, such as a cationically polymerizable resin composition, a radically polymerizable resin composition, and a resin composition using a cationically polymerizable composition and a radically polymerizable composition in combination.
[0003] In cationic polymerizable resin compositions, the cationic polymerization initiator present in the system generates cationic species (H + ) is generated, which in turn reacts with cationic polymerizable organic compounds such as epoxy compounds, causing the ring to open and the reaction to proceed. + A cationic polymerization initiator that generates is also called an acid generator. When a curable resin composition based on a cationic polymerizable organic compound is used, the shrinkage rate of the cured product obtained is generally smaller than that when a curable resin composition based on a radical polymerizable organic compound is used, and a molded object with good dimensional accuracy is obtained. For example, electronic devices such as portable electronic devices such as mobile phones and smartphones are equipped with small and thin imaging units, and the imaging units are generally composed of solid-state imaging devices (CCD type image sensors, CMOS type image sensors, etc.) and optical elements such as lenses. As materials for optical elements such as lenses, cationic curable compositions are preferably used compared to radical curable compositions because they are not inhibited by oxygen and shrink less during curing. They are also preferably used as adhesives between small components in displays and the above electronic devices, and in the field of fine processing such as fine three-dimensional objects. In these applications, processes using light irradiation suitable for fine processing are often applied.
[0004] In addition, the polymerization reaction of a cationic polymerizable organic compound is generally slower than that of a radically polymerizable organic compound, and therefore a cationic polymerizable resin composition with excellent curability is desired. When light irradiation is used, various photoacid generators have been proposed for the purpose of increasing photoreactivity (Patent Documents 1 to 4).
[0005] On the other hand, when mounting electronic components on a wiring board, there are many cases where light cannot be irradiated to the joint. For this reason, it has been disclosed that a specific sulfonium salt is applied and cured by applying heat (Patent Documents 5 to 8). In this case, it is desirable to develop a cationic polymerizable resin composition that is excellent in curability, such as curability at a lower temperature, in order to improve productivity, in addition to improving the corrosion resistance of the thermal cationic polymerizable adhesive by reducing the amount of fluorine ions generated during cationic polymerization, since the polymerization reaction of cationic polymerizable organic compounds is generally slower than the polymerization reaction of radically polymerizable organic compounds.
[0006] Furthermore, for the purpose of improving manufacturing efficiency, optical elements mounted on electronic devices are required to have heat resistance and heat yellowing resistance that allow mounting by soldering using the reflow method. Furthermore, in recent years, the use of lead has been restricted due to environmental considerations, and soldering has begun to be performed using lead-free solder, so even higher heat resistance (approximately 270°C) and heat yellowing resistance are now required.
[0007] The curing performance of cationic polymerizable compounds and the crosslinking reaction performance by acid catalysts differ depending on the type of anion. Generally, BF4 - <PF6 - <SbF6 - However, SbF6 has good polymerization and crosslinking properties. - Cationic polymerization initiators (acid generators) containing SbF6 are limited in their applications due to the toxicity of Sb. - There is a demand for a cationic polymerization initiator having such a high cationic polymerization initiation ability.
[0008] Contains no toxic metals, SbF6 -As a cationic polymerization initiator (acid generator) having high cationic polymerization performance and crosslinking reaction performance like a salt, an acid generator consisting of an anion having a specific structure with aluminum as the central element has been proposed (Patent Documents 9 and 10). However, although it has excellent curing properties, there is a problem that the transparency of the cured product decreases after heat resistance testing, and it has not been applied to components that require the above optical properties. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Special Publication No. 52-14277 [Patent Document 2] Special Publication No. 52-14278 [Patent Document 3] Japanese Patent Application Publication No. 10-287643 [Patent Document 4] Patent No. 5313873 [Patent Document 5] JP 2006-96742 A [Patent Document 6] JP 2006-282633 A [Patent Document 7] JP 2008-303167 A [Patent Document 8] JP 2010-132614 A [Patent Document 9] JP 2018-532866 A [Patent Document 10] JP 2019-85358 A Summary of the Invention [Problem to be solved by the invention]
[0010] In the above background, an object of the present invention is to provide a curable composition which contains an acid generator having excellent photoreactivity and thermal stability as a cationic polymerization initiator, thereby having excellent curability and thermal stability. A second object of the present invention is to provide a cured product that utilizes the above curable composition and that has excellent curability, adhesion, transparency, heat-resistant adhesion and heat-resistant transparency. A third object of the present invention is to provide a cured product for optical elements, which utilizes the above curable composition and has excellent curability, transparency and heat-resistant transparency. A fourth object of the present invention is to provide a three-dimensional object which is excellent in curability, dimensional stability, light resistance, and heat yellowing resistance, by utilizing the above curable composition. A fifth object of the present invention is to provide a cured product for an optical waveguide which utilizes the above curable composition and which has excellent pattern curability, heat-resistant coloration property and thermal stability. [Means for solving the problem]
[0011] As a result of extensive research aimed at achieving the above object, the present inventors have found that a curable composition having excellent curability and thermal stability can be obtained by using an onium salt represented by the following general formula (1) as an acid generator. That is, the present invention is a curable composition containing an acid generator containing an onium salt represented by the following general formula (1) and a cationically polymerizable compound.
[0012] [ka]
[0013] [In the formula, R 1 ~R 3 are each independently an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, or a phenyl group which may have a substituent; R 1 ~R 3 At least one of the hydrogen atoms bonded to the group R is partially or completely substituted with a fluorine atom, 1 ~R 3 30% to 70% of all hydrogen atoms bonded to the group are substituted with fluorine atoms; E represents an element having a valence n selected from S, I, N, or P, where n is an integer of 1 to 3; R 4 is an organic group bonded to E, and R 4The number of is n+1, and (n+1) R 4 may be the same or different, and two or more R 4 may form a ring structure containing the element E either directly or via -O-, -S-, -SO-, -SO2-, -NH-, -CO-, -COO-, -CONH-, an alkylene group, or a phenylene group.]
[0014] The present invention also provides an adhesive comprising the curable composition described above.
[0015] The present invention also provides a cured product obtained by curing the above-described curable composition.
[0016] The present invention also provides an optical element containing the above-described cured product as a constituent element.
[0017] The present invention also provides an optical device comprising the optical element described above.
[0018] The present invention also provides a resin composition for optical three-dimensional object fabrication, comprising the above-described curable composition, a radical polymerizable compound, and a radical polymerization initiator.
[0019] The present invention also provides a three-dimensional object optically produced using the resin composition for three-dimensional object optical production described above.
[0020] The present invention also provides a resin composition for an optical waveguide, comprising the above-described curable composition.
[0021] The present invention also provides a curable film for forming an optical waveguide core layer, which is obtained by forming the resin composition for an optical waveguide into a film shape.
[0022] The present invention also provides an optical waveguide comprising a substrate, a clad layer formed on the substrate, and a core layer for propagating an optical signal formed in a predetermined pattern in the clad layer, the core layer being formed by curing the resin composition for an optical waveguide or the curable film for forming an optical waveguide core layer described above.
[0023] The present invention also provides a hybrid flexible printed wiring board for optical and electrical transmission, characterized in that it includes an optical waveguide. Effect of the Invention
[0024] The composition of the present invention has excellent curability and thermal stability, and the cured product thereof has excellent adhesive properties, transparency, patterning properties, and electrical reliability such as migration resistance, and therefore can be suitably used for adhesive applications such as electronic components, three-dimensional objects, optical elements, optical waveguides, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Hereinafter, an embodiment of the present invention will be described in detail.
[0026] The acid generator of the present invention contains an onium salt represented by the following general formula (1).
[0027] [ka]
[0028] [In the formula, R 1 ~R 3 are each independently an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, or a phenyl group which may have a substituent; R 1 ~R 3 At least one of the hydrogen atoms bonded to the group R is partially or completely substituted with a fluorine atom, 1 ~R 330% to 70% of all hydrogen atoms bonded to the group are substituted with fluorine atoms; E represents an element having a valence n selected from S, I, N, or P, where n is an integer of 1 to 3; R 4 is an organic group bonded to E, and R 4 The number of is n+1, and (n+1) R 4 may be the same or different, and two or more R 4 may form a ring structure containing the element E either directly or via -O-, -S-, -SO-, -SO2-, -NH-, -CO-, -COO-, -CONH-, an alkylene group, or a phenylene group.]
[0029] In general formula (1), R 1 ~R 3 In the above formula, examples of the alkyl group having 1 to 8 carbon atoms include linear alkyl groups (methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-octyl, etc.), branched alkyl groups (isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl, 2-ethylhexyl, 1,1,3,3-tetramethylbutyl, etc.), and cycloalkyl groups (cyclopropyl, cyclobutyl, cyclopentyl, etc.).
[0030] In general formula (1), R 1 ~R 3 In the above formula, examples of the alkenyl group having 2 to 8 carbon atoms include linear or branched alkenyl groups (vinyl, allyl, 1-propenyl, 2-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, etc.), and cycloalkenyl groups (2-cyclohexenyl, 3-cyclohexenyl, etc.).
[0031] In general formula (1), R 1 ~R 3 In the above, the phenyl group which may have a substituent includes, in addition to the phenyl group, an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, a nitro group, -OR 5an alkoxy group represented by the formula -SR 6 embedded image which is substituted with an alkylthio group represented by the following formula:
[0032] In the above-mentioned substituents, the alkyl group having 1 to 8 carbon atoms and the alkenyl group having 2 to 8 carbon atoms are R 1 ~R 3 The same things as those explained in are included.
[0033] In the above substituents, -OR 5 an alkoxy group represented by the formula -SR 6 R of an alkylthio group represented by 5 ~R 6 Examples of the alkyl group include alkyl groups having 1 to 8 carbon atoms, and specific examples of the alkyl groups include those having 1 to 8 carbon atoms among the above alkyl groups.
[0034] -OR 5 Examples of the alkoxy group represented by the formula (I) include methoxy, ethoxy, n-propoxy, iso-propoxy, n-butoxy, sec-butoxy, tert-butoxy, n-pentoxy, iso-pentoxy, neo-pentoxy, and 2-methylbutoxy. -SR 6 Examples of the alkylthio group represented by the formula (I) include methylthio, ethylthio, butylthio, hexylthio, and cyclohexylthio.
[0035] Of these substituents, from the viewpoint of availability of raw materials, preferred are alkyl groups having 1 to 8 carbon atoms, alkenyl groups having 2 to 8 carbon atoms, -OR 5 embedded image embedded image or a chlorine atom or a bromine atom, and more preferably an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms or a chlorine atom.
[0036] R in formula (1) 1 ~R 3Among the groups in the above, from the viewpoint of availability of raw materials, preferred are an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, a phenyl group, and an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or a phenyl group substituted with a chlorine atom. 1 ~R 3 More preferably, the total number of carbon atoms in the formula is 4 to 9.
[0037] Furthermore, in formula (1), R 1 ~R 3 The groups in may be the same or different, and at least one of the hydrogen atoms bonded to the group is partially or completely substituted with a fluorine atom, and R 1 ~R 3 Of all the hydrogen atoms bonded to the group, 30% to 70% are substituted with fluorine atoms. This is called the fluorine substitution rate. From the viewpoint of heat resistance and heat yellowing resistance of the cured product, particularly heat yellowing resistance, the fluorine substitution rate must be 30% to 70%. If the fluorine substitution rate is less than 30%, the anion formed becomes unstable and it is difficult to use as an acid generator, which is unsuitable.
[0038] Preferred examples of the anion structure of the acid generator represented by general formula (1) include those represented by the following chemical formulas (A-1) to (A-14).
[0039] [ka]
[0040] R in formula (1) 4 R represents an organic group bonded to E and may be the same or different. 4 Examples of the aryl group include an alkyl group having 1 to 18 carbon atoms, an alkenyl group having 2 to 18 carbon atoms, and an aryl group having 6 to 14 carbon atoms. The aryl group can further include an alkyl group having 1 to 18 carbon atoms, an alkenyl group having 2 to 18 carbon atoms, an aryl group having 6 to 14 carbon atoms, a nitro group, a hydroxyl group, a cyano group, -OR 5 an alkoxy group or an aryloxy group represented by the formula: 6an alkylthio group or an arylthio group represented by the formula: 7 An acyl group represented by CO-, R 8 Acyloxy group represented by COO-, -NR 9 R 10 or a halogen atom.
[0041] Above R 4 Examples of the alkyl group having 1 to 18 carbon atoms in the formula (I) include linear alkyl groups (methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-octyl, n-decyl, n-dodecyl, n-tetradecyl, n-hexadecyl, n-octadecyl, and the like), branched alkyl groups (isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl, 2-ethylhexyl, 1,1,3,3-tetramethylbutyl, and the like), cycloalkyl groups (cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and the like), bridged cyclic alkyl groups (norbornyl, adamantyl, pinanyl, and the like), and arylalkyl groups (benzyl, naphthylmethyl, phenethyl, benzhydryl, phenacyl, and the like).
[0042] Above R 4 Examples of the alkenyl group having 2 to 18 carbon atoms in the formula (I) include linear or branched alkenyl groups (vinyl, allyl, 1-propenyl, 2-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, etc.), cycloalkenyl groups (2-cyclohexenyl, 3-cyclohexenyl, etc.), and arylalkenyl groups (styryl, cinnamyl, etc.).
[0043] Above R 4In the above, examples of the aryl group having 6 to 14 carbon atoms (not including the number of carbon atoms of the following substituents) include monocyclic aryl groups (phenyl, etc.), condensed polycyclic aryl groups (naphthyl, anthracenyl, phenanthrenyl, anthraquinolyl, fluorenyl, naphthoquinolyl, etc.), and aromatic heterocyclic hydrocarbon groups (monocyclic heterocycles such as thienyl, furanyl, pyranyl, pyrrolyl, oxazolyl, thiazolyl, pyridyl, pyrimidyl, pyrazinyl, etc.; and indolyl, benzoyl, zofuranyl, isobenzofuranyl, benzothienyl, isobenzothienyl, quinolyl, isoquinolyl, quinoxalinyl, quinazolinyl, carbazolyl, acridinyl, phenothiazinyl, phenazinyl, xanthenyl, thianthrenyl, phenoxazinyl, phenoxathiinyl, chromanyl, isochromanyl, coumarinyl, dibenzothienyl, xanthonyl, thioxanthonyl, dibenzofuranyl, and other condensed polycyclic heterocycles.
[0044] In addition to the above, the aryl group may be an aryl group in which some of the hydrogen atoms are substituted with an alkyl group having 1 to 18 carbon atoms, an alkenyl group having 2 to 18 carbon atoms, an aryl group having 6 to 14 carbon atoms, a nitro group, a hydroxyl group, a cyano group, -OR 5 an alkoxy group or an aryloxy group represented by the formula: 6 an alkylthio group or an arylthio group represented by the formula: 7 An acyl group represented by CO-, R 8 Acyloxy group represented by COO-, -NR 9 R 10 or a halogen atom.
[0045] In the above substituents, -OR 5 an alkoxy group represented by the formula -SR 6 an alkylthio group represented by R 7 An acyl group represented by CO-, R 8 Acyloxy group represented by COO-, -NR 9 R 10 R of the amino group represented by 5 ~R 10Examples of the alkyl group include alkyl groups having 1 to 8 carbon atoms, and specific examples of the alkyl groups include those having 1 to 8 carbon atoms among the above alkyl groups.
[0046] In the above substituents, -OR 5 an aryloxy group represented by -SR 6 an arylthio group represented by R 7 An acyl group represented by CO-, R 8 Acyloxy group represented by COO-, -NR 9 R 10 R of the amino group represented by 5 ~R 10 Examples of the aryl group include aryl groups having 6 to 14 carbon atoms, and specific examples thereof include the above-mentioned aryl groups having 6 to 14 carbon atoms.
[0047] -OR 5 Examples of the alkoxy group represented by the formula (I) include methoxy, ethoxy, n-propoxy, iso-propoxy, n-butoxy, sec-butoxy, tert-butoxy, n-pentoxy, iso-pentoxy, neo-pentoxy, and 2-methylbutoxy. -OR 5 Examples of the aryloxy group represented by the formula (I) include phenoxy and naphthoxy. -SR 6 Examples of the alkylthio group represented by the formula (I) include methylthio, ethylthio, butylthio, hexylthio, and cyclohexylthio. -SR 6 Examples of the arylthio group represented by the formula (I) include phenylthio, naphthylthio, biphenylthio, and 2-thioxanthonylthio. R 7 Examples of the acyl group represented by CO- include acetyl, propanoyl, butanoyl, pivaloyl, and benzoyl. R 8 Examples of the acyloxy group represented by COO-- include acetoxy, butanoyloxy, and benzoyloxy. -NR 9 R 10Examples of the amino group represented by the formula (I) include methylamino, ethylamino, propylamino, dimethylamino, diethylamino, methylethylamino, dipropylamino, dipropylamino, and piperidino. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0048] Above R 4 Among these, preferred from the viewpoint of cationic polymerization initiation ability are an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 14 carbon atoms, a nitro group, a hydroxyl group, an alkyl group having 1 to 18 carbon atoms, -OR 5 an alkoxy group represented by the formula -SR 6 an arylthio group represented by R 7 An acyl group represented by CO-, R 8 It is an acyloxy group represented by COO- or an aryl group having 6 to 14 carbon atoms substituted with a chlorine atom. More preferred are alkyl groups having 1 to 18 carbon atoms, phenyl groups, hydroxyl groups, alkyl groups having 1 to 18 carbon atoms, -OR 5 an alkoxy group represented by the formula -SR 6 and phenyl groups substituted with an arylthio group, an acetyl group, a benzoyl group, or an acetoxy group, represented by the following formula:
[0049] Also, two or more R 4 may form a ring structure containing the element E directly or via -O-, -S-, -SO-, -SO2-, -NH-, -CO-, -COO-, -CONH-, an alkylene group or a phenylene group.
[0050] In formula (1), E represents an element having a valence of n selected from S (sulfur), I (iodine), N (nitrogen) or P (phosphorus), and an organic group R 4 and combines with the onium ion [E + n represents the valence of the element E and is an integer of 1 to 3. The corresponding onium ions are ammonium, phosphonium, sulfonium, and iodonium. Among them, ammonium, phosphonium, sulfonium, and iodonium, which are stable and easy to handle, are preferred, and sulfonium and iodonium, which are excellent in cationic polymerization performance and crosslinking reaction performance, are more preferred.
[0051] Specific examples of ammonium ions include tetraalkylammonium ions such as tetramethylammonium, ethyltrimethylammonium, diethyldimethylammonium, triethylmethylammonium, and tetraethylammonium; pyrrolidinium ions such as N,N-dimethylpyrrolidinium, N-ethyl-N-methylpyrrolidinium, and N,N-diethylpyrrolidinium; imidazolinium ions such as N,N'-dimethylimidazolinium, N,N'-diethylimidazolinium, N-ethyl-N'-methylimidazolinium, 1,3,4-trimethylimidazolinium, and 1,2,3,4-tetramethylimidazolinium; and N,N'-dimethyltetrahydropyrrolidinium. tetrahydropyrimidiniums such as midinium; morpholiniums such as N,N'-dimethylmorpholinium; piperidiniums such as N,N'-diethylpiperidinium; pyridiniums such as N-methylpyridinium, N-benzylpyridinium, and N-phenacylpyridinium; imidazoliums such as N,N'-dimethylimidazolium; quinoliums such as N-methylquinolium, N-benzylquinolium, and N-phenacylquinolium; isoquinoliums such as N-methylisoquinolium; thiazoniums such as benzylbenzothiazonium and phenacylbenzothiazonium; and acridiums such as benzylacridium and phenacylacridium.
[0052] Specific examples of phosphonium ions include tetraarylphosphonium ions such as tetraphenylphosphonium, tetra-p-tolylphosphonium, tetrakis(2-methoxyphenyl)phosphonium, tetrakis(3-methoxyphenyl)phosphonium, and tetrakis(4-methoxyphenyl)phosphonium; triarylphosphonium ions such as triphenylbenzylphosphonium, triphenylphenacylphosphonium, triphenylmethylphosphonium, and triphenylbutylphosphonium; and tetraalkylphosphonium ions such as triethylbenzylphosphonium, tributylbenzylphosphonium, tetraethylphosphonium, tetrabutylphosphonium, tetrahexylphosphonium, triethylphenacylphosphonium, and tributylphenacylphosphonium.
[0053] Specific examples of sulfonium ions include triphenylsulfonium, tri-p-tolylsulfonium, tri-o-tolylsulfonium, tris(4-methoxyphenyl)sulfonium, 1-naphthyldiphenylsulfonium, 2-naphthyldiphenylsulfonium, tris(4-fluorophenyl)sulfonium, tri-1-naphthylsulfonium, tri-2-naphthylsulfonium, tris(4-hydroxyphenyl)sulfonium, 4-(phenylthio)phenyldiphenylsulfonium, 4-(p-tolylthio)phenyldiphenylsulfonium, and the like. -p-tolylsulfonium, 4-(4-methoxyphenylthio)phenylbis(4-methoxyphenyl)sulfonium, 4-(phenylthio)phenylbis(4-fluorophenyl)sulfonium, 4-(phenylthio)phenylbis(4-methoxyphenyl)sulfonium, 4-(phenylthio)phenyldi-p-tolylsulfonium, [4-(4-biphenylylthio)phenyl]-4-biphenylylphenylsulfonium, [4-(9,9-diphenylfluorenyl-2-thio)phenyl]-2-(9,9-diphenyl)fluorenium fluorenylphenylsulfonium, [4-(9,9-dimethylfluorenyl-2-thio)phenyl]-2-(9,9-dimethyl)fluorenylphenylsulfonium, [4-(2-thioxanthonylthio)phenyl]diphenylsulfonium, bis[4-(diphenylsulfonio)phenyl]sulfide, bis[4-{bis[4-(2-hydroxyethoxy)phenyl]sulfonio}phenyl]sulfide, bis{4-[bis(4-fluorophenyl)sulfonio]phenyl}sulfide, bis{4-[bis(4-methylphenyl) sulfonio]phenyl}sulfide, bis{4-[bis(4-methoxyphenyl)sulfonio]phenyl}sulfide, 4-(4-benzoyl-2-chlorophenylthio)phenylbis(4-fluorophenyl)sulfonium, 4-(4-benzoyl-2-chlorophenylthio)phenyldiphenylsulfonium, 4-(4-benzoylphenylthio)phenylbis(4-fluorophenyl)sulfonium, 4-(4-benzoylphenylthio)phenyldiphenylsulfonium, 7-isopropyl-9-oxo-10-thia-9,10-Dihydroanthracen-2-yldi-p-tolylsulfonium, 7-isopropyl-9-oxo-10-thia-9,10-dihydroanthracen-2-yldiphenylsulfonium, 2-[(di-p-tolyl)sulfonio]thioxanthone, 2-[(diphenyl)sulfonio]thioxanthone, 4-(9-oxo-9H-thioxanthen-2-yl)thiophenyl-9-oxo-9H-thioxanthen-2-ylphenylsulfonium, 2-[(diphenyl)sulfonio]thioxanthone, [4-(9-oxo-9H-thioxanthen-2-yl)thio-2-tert-butyl-5-methylphenyl]-9 -oxo-9H-thioxanthen-2-yl-(3-butyl-5-methylphenyl)sulfonium, 4-[4-(4-tert-butylbenzoyl)phenylthio]phenyldi-p-tolylsulfonium, 4-[4-(4-tert-butylbenzoyl)phenylthio]phenyldiphenylsulfonium, 4-[4-(benzoylphenylthio)]phenyldi-p-tolylsulfonium, 4-[4-(benzoylphenylthio)]phenyldiphenylsulfonium, 5-(4-methoxyphenyl)thianthrenium, 5-phenylthianthrenium, 5-tolylthianthreneium, 5-(4-ethoxyphenyl)thianthrenium, 5-(2,4,6-trimethylphenyl)thianthrenium and other triarylsulfoniums;diphenylphenacylsulfonium, diphenyl4-nitrophenacylsulfonium, diphenylbenzylsulfonium, diphenylmethylsulfonium and other diarylsulfoniums;phenylmethylbenzylsulfonium, 4-hydroxyphenylmethylbenzylsulfonium, 4-methoxyphenylmethylbenzylsulfonium, 4-acetoxyphenylmethylbenzylsulfonium, 4-acetoxyphenyldimethylsulfonium, 4-hydroxyphenyl(1-naphthylmethyl)methylsulfonium, 2-naphthylmethylbenzylsulfonium, 4-hydroxyphenyl(4-nitrobenzyl ... Monoarylsulfonium such as (1-ethoxycarbonyl)ethylsulfonium, phenylmethylphenacylsulfonium, 4-hydroxyphenylmethylphenacylsulfonium, 4-methoxyphenylmethylphenacylsulfonium, 4-acetoxyphenylmethylphenacylsulfonium, 2-naphthylmethylphenacylsulfonium, 2-naphthyloctadecylphenacylsulfonium, and 9-anthracenylmethylphenacylsulfonium; and trialkylsulfonium such as dimethylphenacylsulfonium, phenacylstetrahydrothiophenium, dimethylbenzylsulfonium, benzyltetrahydrothiophenium, and octadecylmethylphenacylsulfonium.
[0054] Specific examples of iodonium ions include diphenyliodonium, di-p-tolyliodonium, di(4-tert-butylphenyl)iodonium, di(4-dodecylphenyl)iodonium, di(4-methoxyphenyl)iodonium, (4-octyloxyphenyl)phenyliodonium, di(4-decyloxyphenyl)iodonium, 4-(2-hydroxytetradecyloxy)phenylphenyliodonium, 4-isopropylphenyl(p-tolyl)iodonium, phenyl(2,4,6-trimethoxyphenyl)iodonium, and 4-isobutylphenyl(p-tolyl)iodonium.
[0055] The onium salt represented by formula (1) of the present invention can be produced by a metathesis method. The double decomposition method is described in, for example, Shin Jikken Kagaku Koza, Vol. 14-I (1978, Maruzen), p. 448; Advance in Polymer Science, 62, 1-48 (1984); Shin Jikken Kagaku Koza, Vol. 14-III (1978, Maruzen), pp. 1838-1846; Organic Sulfur Chemistry (Synthetic Reactions, 1982, Kagaku Dojin), Chapter 8, pp. 237-280; Nihon Kagaku Zasshi, 87, (5), 74 (1966); JP-A Nos. 64-45357, 61-212554, 61-100557, 5-4996, 7-82244, 7-82245, 58-210904, and 6-184170. First, the F of the onium cation is reacted with the cation of - , Cl - , Br - , I - Halogen ion salts such as;OH - Salt;ClO4 - Salt; FSO3 - , ClSO3 - , CH3SO3 - , C6H5SO3 - , CF3SO3 - Salts with sulfonic acid ions such as HSO4 - , SO4 2- Salts with sulfate ions such as HCO3 - , CO3 2- , and other carbonate ions;H2PO4 - , HPO4 2- , PO4 3-Salts with phosphate ions such as phosphate ions are prepared, and these are added to a solvent or aqueous solution containing a theoretical amount or more of an alkali metal salt, alkaline earth metal salt, or quaternary ammonium salt of the anion constituting the onium salt represented by formula (1) and, if necessary, other anion components such as KPF6, KBF4, LiB(C6F5)4 to cause metathesis. As the solvent, water or an organic solvent can be used. As the organic solvent, hydrocarbons (hexane, heptane, toluene, xylene, etc.), cyclic ethers (tetrahydrofuran and dioxane, etc.), chlorine-based solvents (chloroform and dichloromethane, etc.), alcohols (methanol, ethanol, isopropyl alcohol, etc.), ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), nitriles (acetonitrile, etc.) and polar organic solvents (dimethyl sulfoxide, dimethylformamide, N-methylpyrrolidone, etc.). These solvents may be used alone or in combination of two or more.
[0056] The target onium salt thus produced is separated as a crystal or oil. In the case of an oil, the precipitated oil is separated from the organic solvent solution, and the organic solvent contained in the oil is distilled off to obtain the product. In the case of a crystal, the precipitated solid is separated from the organic solvent solution, and the organic solvent contained in the solid is distilled off to obtain the product. The target onium salt thus obtained can be purified, if necessary, by a method such as recrystallization or washing with water or a solvent.
[0057] Purification by recrystallization can be performed by dissolving the target onium salt in a small amount of organic solvent, and separating the target onium salt from the organic solvent by adding a poor solvent directly (or after concentrating) to the organic solvent solution containing the target onium salt to precipitate the target onium salt. The poor solvent used here includes chain ethers (diethyl ether, dipropyl ether, etc.), esters (ethyl acetate, butyl acetate, etc.), aliphatic hydrocarbons (hexane, cyclohexane, etc.), and aromatic hydrocarbons (toluene, xylene, etc.). Purification can also be performed by utilizing the difference in solubility due to temperature. Purification can be performed by recrystallization (a method that utilizes the difference in solubility due to cooling, a method of precipitating by adding a poor solvent, and a combination of these). In addition, when the target product is an oily product (not crystallized), purification can be performed by washing the oily product with water or a poor solvent.
[0058] The structure of the onium salt thus obtained can be analyzed by a general analytical method, for example, 1 H, 13 C. 19 F, etc., infrared absorption spectrometry, mass spectrometry, elemental analysis, etc.
[0059] The curable composition of the present invention is characterized by containing an onium salt represented by general formula (1) as an acid generator, and the acid generator of the present invention may be used alone or in combination of two or more kinds. In addition, other conventionally known acid generators may be contained in the composition.
[0060] Other acid generators include conventionally known ones such as onium salts (sulfonium, iodonium, selenium, ammonium, phosphonium, etc.) and salts of transition metal complex ions and anions.
[0061] When another acid generator is contained, the content (mol %) of the other acid generator is preferably 0.1 to 100, and more preferably 0.5 to 50, based on the total number of moles of the onium salt represented by general formula (1) of the present invention.
[0062] The onium salt (acid generator) represented by formula (1) may be dissolved in advance in a solvent that does not inhibit the polymerization or crosslinking reaction, in order to facilitate dissolution in the cationically polymerizable compound.
[0063] Examples of the solvent include carbonates such as propylene carbonate, ethylene carbonate, 1,2-butylene carbonate, dimethyl carbonate, and diethyl carbonate; ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl isoamyl ketone, and 2-heptanone; polyhydric alcohols and derivatives thereof such as ethylene glycol, ethylene glycol monoacetate, diethylene glycol, diethylene glycol monoacetate, propylene glycol, propylene glycol monoacetate, dipropylene glycol, and the monomethyl ether, monoethyl ether, monopropyl ether, monobutyl ether, and monophenyl ether of dipropylene glycol monoacetate; and polyhydric alcohols and derivatives thereof such as dioxane. cyclic ethers such as ethyl formate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl pyruvate, ethyl ethoxyacetate, methyl methoxypropionate, ethyl ethoxypropionate, methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, β-propiolactone, β-butyrolactone, γ-butyrolactone, δ-valerolactone, and ε-caprolactone; and aromatic hydrocarbons such as toluene and xylene.
[0064] When a solvent is used, the proportion of the solvent used is preferably 15 to 1000 parts by weight, more preferably 30 to 500 parts by weight, based on 100 parts by weight of the onium salt (acid generator) represented by formula (1) of the present invention. The solvents used may be used alone or in combination of two or more kinds.
[0065] The curable composition of the present invention comprises the above-mentioned acid generator and a cationically polymerizable compound.
[0066] Examples of the cationically polymerizable compound that is a component of the curable composition include cyclic ethers (epoxides, oxetanes, etc.), ethylenically unsaturated compounds (vinyl ethers, styrenes, etc.), bicycloorthoesters, spiroorthocarbonates, and spiroorthoesters. (For example, examples of the cationically polymerizable compound component in the active energy ray curable composition include those described in JP-A-11-060996, JP-A-09-302269, JP-A-2003-026993, JP-A-2002-206017, JP-A-11-349895, JP-A-10-212343, JP-A-2000-119306, JP-A-10-67812, JP-A-2000-186071, JP-A-08-85775, JP-A-08-134405, JP-A-2008-208 38, JP 2008-20839, JP 2008-20841, JP 2008-26660, JP 2008-26644, JP 2007-277327, Photopolymer Handbook edited by Photopolymer Forum (1989, Kogyo Chosakai), UV / EB Curing Technology edited by General Technology Center (1982, General Technology Center), UV / EB Curing Materials edited by RadTech Research Group (1992, CMC), Causes of Curing Defects and Inhibitions in UV Curing and Countermeasures therefor edited by Technical Information Association (2003, Technical Information Association), Color Materials, 68, (5), 286-293 (1995), Fine Chemicals, 29, (19), 5-14 (2000), etc. These may be used as cationic polymerizable compound components in thermosetting compositions.}.
[0067] As the epoxide, known epoxides can be used, including aromatic epoxides, alicyclic epoxides and aliphatic epoxides.
[0068] Examples of aromatic epoxides include polyglycidyl ethers and polyglycidyl esters of polyhydric phenols or their alkylene oxide adducts. Specific examples include glycidyl ethers of bisphenol A, bisphenol E, bisphenol F, bisphenol AD, bisphenol S, bisphenol Z, or compounds obtained by further adding alkylene oxides such as ethylene oxide or propylene oxide to these, phenyl glycidyl ether, tert-butylphenyl glycidyl ether, resorcinol diglycidyl ether, tetraglycidyl ether of tetraphenolethane, triglycidyl ether of triphenolmethane, glycidyl products of condensates of phenols or naphthols with aldehydes (e.g., phenolic resins and novolac resins), glycidyl products of condensates of phenols and isopropenylacetophenone, glycidyl products of reaction products of phenols and dicyclopentadiene, diglycidyl esters of terephthalic acid, diglycidyl esters of isophthalic acid, and diglycidyl esters of o-phthalic acid.
[0069] Examples of the alicyclic epoxide include polyglycidyl ethers of polyhydric alcohols having at least one alicyclic ring, and compounds containing a cyclohexene oxide structure or a cyclopentene oxide structure obtained by epoxidizing a compound containing a cyclohexene ring or a compound containing a cyclopentene ring with a suitable oxidizing agent such as hydrogen peroxide or a peracid. More specifically, examples of alicyclic epoxy compounds include alicyclic diglycidyl ether compounds such as hydrogenated bisphenol A diglycidyl ether, hydrogenated bisphenol F diglycidyl ether, hydrogenated bisphenol AD diglycidyl ether, hydrogenated bisphenol Z diglycidyl ether, cyclohexane dimethanol diglycidyl ether, and tricyclodecane dimethanol diglycidyl ether. Examples of the cyclohexene oxide structure-containing compound or the cyclopentene oxide structure-containing compound include 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, 3,4-epoxy-1-methylcyclohexyl-3,4-epoxy-1-methylcyclohexanecarboxylate, 6-methyl-3,4-epoxycyclohexylmethyl-6-methyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxy-3-methylcyclohexylmethyl-3,4-epoxy-3-methyl ... epoxy-5-methylcyclohexylmethyl-3,4-epoxy-5-methylcyclohexanecarboxylate, 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexane-metadioxane, bis(3,4-epoxycyclohexylmethyl)adipate, 3,4-epoxy-6-methylcyclohexylcarboxylate, dicyclopentadiene diepoxide, ethylene bis(3,4-epoxycyclohexanecarboxylate), dioctyl epoxyhexahydrophthalate, and di-2-ethylhexyl epoxyhexahydrophthalate. Further examples include ε-caprolactone-modified 3′,4′-epoxycyclohexylmethyl 3,4-epoxycyclohexane carboxylate and 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, both of which are available from Daicel Corporation. Further examples include bis(3,4-epoxycyclohexyl)methane, 2,2-bis(3,4-epoxycyclohexyl)propane, 1,1-bis(3,4-epoxycyclohexyl)ethane, alpha-pinene oxide, camphalenaldehyde, limonene monoxide, limonene dioxide, 4-vinylcyclohexene monoxide, and 4-vinylcyclohexene dioxide.
[0070] Examples of the aliphatic epoxide include polyglycidyl ethers of aliphatic polyhydric alcohols or their alkylene oxide adducts, polyglycidyl esters of aliphatic long-chain polybasic acids, homopolymers synthesized by vinyl polymerization of glycidyl acrylate or glycidyl methacrylate, and copolymers synthesized by vinyl polymerization of glycidyl acrylate and / or glycidyl methacrylate with other vinyl monomers. Representative compounds include glycidyl ethers of polyhydric alcohols such as butyl glycidyl ether, 2-ethylhexyl glycidyl ether, glycidyl ethers of higher alcohols, diglycidyl ethers of alkylene diols (e.g., diglycidyl ether of 1,4-butanediol, diglycidyl ether of 1,6-hexanediol, diglycidyl ether of neopentyl glycol, etc.), triglycidyl ether of glycerin, diglycidyl ether of trimethylolpropane, triglycidyl ether of trimethylolpropane, tetraglycidyl ether of sorbitol, hexaglycidyl ether of dipentaerythritol, diglycidyl ether of polyethylene glycol, diglycidyl ether of polypropylene glycol, and diglycidyl ether of polytetramethylene glycol. Further examples include polyglycidyl ethers of polyether polyols obtained by adding one or more alkylene oxides to an aliphatic polyhydric alcohol such as propylene, trimethylolpropane, or glycerin, and diglycidyl esters of aliphatic long-chain dibasic acids. Further examples include monoglycidyl ethers of higher aliphatic alcohols, monoglycidyl ethers of polyether alcohols obtained by adding phenol, cresol, butylphenol or alkylene oxides thereto, glycidyl esters of higher fatty acids, epoxidized soybean oil, epoxy butyl stearate, epoxidized polybutadiene, and glycidylated polybutadiene. Examples of the epoxyalkane include 1,2-epoxydecane, 1,2-epoxydodecane, 1,2-epoxytetradecane, 1,2-epoxycetane, 1,2-epoxyoctadecane, and 1,2-epoxyicosane.
[0071] Examples of oxetanes include 3-ethyl-3-hydroxymethyloxetane, 3-(meth)allyloxymethyl-3-ethyloxetane, (3-ethyl-3-oxetanylmethoxy)methylbenzene, 4-fluoro-[1-(3-ethyl-3-oxetanylmethoxy)methyl]benzene, 4-methoxy-[1-(3-ethyl-3-oxetanylmethoxy)methyl]benzene, [1-(3-ethyl-3-oxetanylmethoxy)ethyl]phenyl ether, isobutoxymethyl (3-ethyl-3-oxetanylmethyl) ether, isobornyloxyethyl (3-ethyl-3- oxetanylmethyl) ether, isobornyl (3-ethyl-3-oxetanylmethyl) ether, 2-ethylhexyl (3-ethyl-3-oxetanylmethyl) ether, ethyl diethylene glycol (3-ethyl-3-oxetanylmethyl) ether, dicyclopentadiene (3-ethyl-3-oxetanylmethyl) ether, dicyclopentenyloxyethyl (3-ethyl-3-oxetanylmethyl) ether, dicyclopentenyl (3-ethyl-3-oxetanylmethyl ether, tetrahydrofurfuryl (3-ethyl-3 -oxetanylmethyl) ether, tetrabromophenyl (3-ethyl-3-oxetanylmethyl) ether, 2-tetrabromophenoxyethyl (3-ethyl-3-oxetanylmethyl) ether, tribromophenyl (3-ethyl-3-oxetanylmethyl) ether, 2-tribromophenoxyethyl (3-ethyl-3-oxetanylmethyl) ether, 2-hydroxyethyl (3-ethyl-3-oxetanylmethyl) ether, 2-hydroxypropyl (3-ethyl-3-oxetanylmethyl) ether, butoxyethyl (3 -ethyl-3-oxetanylmethyl) ether, pentachlorophenyl (3-ethyl- monofunctional oxetane compounds such as pentabromophenyl (3-ethyl-3-oxetanylmethyl) ether, pentabromophenyl (3-ethyl-3-oxetanylmethyl) ether and bornyl (3-ethyl-3-oxetanylmethyl) ether, 3,7-bis(3-oxetanyl)-5-oxa-nonane, 3,3'-(1,3-(2-methyleneyl)propanediylbis(oxymethylene))bis-(3-ethyloxetane), 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, dicyclopentenyl bis(3-ethyl-3-oxetanylmethyl)ether, triethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, tetraethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, tricyclodecanediyldimethylene(3-ethyl-3-oxetanylmethyl)ether, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl)ether, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, pentaerythritol tris(3-ethyl-3-oxetanylmethyl) ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl)ether, polyethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol hexakis(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl)ether, caprolactone-modified dipentaerythritol hexakis(3-ethyl-3-oxetanylmethyl)ether, caprolactone-modified dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl)ether, ditrimethylolpropane tetrakis(3-ethyl-3-oxetanylmethyl)ether, EO-modified bisphenol A bis(3 Examples of polyfunctional oxetane compounds include polyfunctional oxetane compounds such as bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, PO-modified bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, EO-modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, PO-modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, and EO-modified bisphenol F(3-ethyl-3-oxetanylmethyl) ether.
[0072] Among these oxetanes, compounds having one or two oxetane rings are preferred from the viewpoint of curing speed. Specific examples thereof include 3,7-bis(3-oxetanyl)-5-oxa-nonane, 3,3'-(1,3-(2-methyleneyl)propanediylbis(oxymethylene))bis-(3-ethyloxetane), 1,4-bis[(3-ethyl- 3-oxetanylmethoxy)methyl]benzene, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, dicyclopentenyl bis(3-ethyl-3-oxetanylmethyl)ether, triethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, tetraethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, tricyclodecanediyldimethylene(3-ethyl-3-oxetanylmethyl)ether, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl)ether, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, and the like.
[0073] As the ethylenically unsaturated compound, known cationically polymerizable monomers and the like can be used, including aliphatic monovinyl ethers, aromatic monovinyl ethers, polyfunctional vinyl ethers, styrenes and cationically polymerizable nitrogen-containing monomers.
[0074] Examples of the aliphatic monovinyl ether include methyl vinyl ether, ethyl vinyl ether, butyl vinyl ether, and cyclohexyl vinyl ether.
[0075] Examples of the aromatic monovinyl ether include 2-phenoxyethyl vinyl ether, phenyl vinyl ether, and p-methoxyphenyl vinyl ether.
[0076] Examples of polyfunctional vinyl ethers include butanediol-1,4-divinyl ether and triethylene glycol divinyl ether.
[0077] Examples of styrenes include styrene, α-methylstyrene, p-methoxystyrene, and p-tert-butoxystyrene.
[0078] Examples of the cationically polymerizable nitrogen-containing monomer include N-vinylcarbazole and N-vinylpyrrolidone.
[0079] Bicyclo orthoesters include 1-phenyl-4-ethyl-2,6,7-trioxabicyclo[2.2.2]octane and 1-ethyl-4-hydroxymethyl-2,6,7-trioxabicyclo-[2.2.2]octane.
[0080] Examples of spiro orthocarbonates include 1,5,7,11-tetraoxaspiro[5.5]undecane and 3,9-dibenzyl-1,5,7,11-tetraoxaspiro[5.5]undecane.
[0081] Spiro orthoesters include 1,4,6-trioxaspiro[4.4]nonane, 2-methyl-1,4,6-trioxaspiro[4.4]nonane, and 1,4,6-trioxaspiro[4.5]decane.
[0082] Furthermore, polyorganosiloxanes having at least one cationically polymerizable group in one molecule can be used (described in JP-A 2001-348482, Journal of Polym. Sci., Part A, Polym. Chem., Vol. 28, 497 (1990), etc.). These polyorganosiloxanes may be linear, branched, or cyclic, or may be a mixture of these.
[0083] Among these cationic polymerizable compounds, epoxides, oxetanes and vinyl ethers are preferred, epoxides and oxetanes are more preferred, and alicyclic epoxides and oxetanes are particularly preferred. These cationic polymerizable compounds may be used alone or in combination of two or more.
[0084] The content of the onium salt (acid generator) represented by formula (1) of the present invention in the curable composition is preferably 0.05 to 20 parts by weight, more preferably 0.1 to 10 parts by weight, based on 100 parts by weight of the cationic polymerizable compound. In this range, the polymerization of the cationic polymerizable compound becomes more sufficient, and the physical properties of the cured product become more excellent. Note that this content is determined by considering various factors such as the properties of the cationic polymerizable compound, the type of light (light source, wavelength, etc.) and the amount of light irradiation when light is used, the heating temperature, the curing time, humidity, and the thickness of the coating film, and is not limited to the above range.
[0085] The curable composition of the present invention may contain, as necessary, known additives (such as sensitizers, pigments, fillers, antistatic agents, flame retardants, antifoaming agents, flow control agents, light stabilizers, antioxidants, adhesion imparting agents, ion scavengers, coloration inhibitors, solvents, non-reactive resins, and radically polymerizable compounds).
[0086] As the sensitizer, known sensitizers (such as those described in JP-A-11-279212 and JP-A-09-183960) can be used, and examples thereof include anthracene {anthracene, 9,10-dibutoxyanthracene, 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-dipropoxyanthracene, etc.}; pyrene; 1,2-benzanthracene; perylene; tetrafluoroethylene; Thracene;Coronene;Thioxanthone {thioxanthone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, 2,4-diethylthioxanthone, etc.};Phenothiazine {phenothiazine, N-methylphenothiazine, N-ethylphenothiazine, N-phenylphenothiazine, etc.};Xanthone;Naphthalene {1-naphthol, 2-naphthol, 1-methylthioxanthone, ketones {dimethoxyacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 4'-isopropyl-2-hydroxy-2-methylpropiophenone, 4-benzoyl-4'-methyldiphenyl sulfide, etc.}; carbazoles {N-phenylcarbazole, N-ethylcarbazole, poly-N-vinylcarbazole, N-glycidylcarbazole, etc.}; chrysene {1,4-dimethoxychrysene, 1,4-di-α-methylbenzyloxychrysene, etc.}; phenanthrene {9-hydroxyphenanthrene, 9-methoxyphenanthrene, 9-hydroxy-10-methoxyphenanthrene, 9-hydroxy-10-ethoxyphenanthrene, etc.}.
[0087] When a sensitizer is contained, the content of the sensitizer is preferably from 1 to 300 parts by weight, and more preferably from 5 to 200 parts by weight, based on 100 parts of the acid generator.
[0088] As the pigment, known pigments can be used, including inorganic pigments (titanium oxide, iron oxide, carbon black, etc.) and organic pigments (azo pigments, cyanine pigments, phthalocyanine pigments, quinacridone pigments, etc.).
[0089] When a pigment is contained, the content of the pigment is preferably 0.5 to 400,000 parts by weight, and more preferably 10 to 150,000 parts by weight, based on 100 parts of the acid generator.
[0090] As the filler, known fillers can be used, and examples thereof include fused silica, crystalline silica, calcium carbonate, aluminum oxide, aluminum hydroxide, zirconium oxide, magnesium carbonate, mica, talc, calcium silicate, and lithium aluminum silicate.
[0091] When a filler is contained, the content of the filler is preferably 50 to 600,000 parts by weight, and more preferably 300 to 200,000 parts by weight, based on 100 parts of the acid generator.
[0092] As the antistatic agent, known antistatic agents can be used, and examples of such agents include nonionic antistatic agents, anionic antistatic agents, cationic antistatic agents, amphoteric antistatic agents, and polymeric antistatic agents.
[0093] When an antistatic agent is contained, the content of the antistatic agent is preferably 0.1 to 20,000 parts by weight, and more preferably 0.6 to 5,000 parts by weight, based on 100 parts of the acid generator.
[0094] As the flame retardant, known flame retardants can be used, and examples thereof include inorganic flame retardants {antimony trioxide, antimony pentoxide, tin oxide, tin hydroxide, molybdenum oxide, zinc borate, barium metaborate, red phosphorus, aluminum hydroxide, magnesium hydroxide, calcium aluminate, and the like}; bromine flame retardants {tetrabromophthalic anhydride, hexabromobenzene, decabromobiphenyl ether, and the like}; and phosphate flame retardants {tris(tribromophenyl)phosphate, and the like}.
[0095] When a flame retardant is contained, the content of the flame retardant is preferably 0.5 to 40,000 parts by weight, and more preferably 5 to 10,000 parts by weight, based on 100 parts of the acid generator.
[0096] As the defoaming agent, known defoaming agents can be used, and examples thereof include alcohol defoaming agents, metal soap defoaming agents, phosphate ester defoaming agents, fatty acid ester defoaming agents, polyether defoaming agents, silicone defoaming agents, and mineral oil defoaming agents.
[0097] As the flow regulator, known flow regulators can be used, and examples thereof include hydrogenated castor oil, oxidized polyethylene, organic bentonite, colloidal silica, amide wax, metal soaps, and acrylic ester polymers. As the light stabilizer, known light stabilizers can be used, and examples thereof include ultraviolet absorbing stabilizers (benzotriazole, benzophenone, salicylate, cyanoacrylate, and derivatives thereof, etc.); radical scavenging stabilizers (hindered amines, etc.); and quenching stabilizers (nickel complexes, etc.). As the antioxidant, known antioxidants can be used, and examples of such antioxidants include phenol-based antioxidants (monophenol-based, bisphenol-based, and polymeric phenol-based, etc.), sulfur-based antioxidants, and phosphorus-based antioxidants. As the adhesion imparting agent, known adhesion imparting agents can be used, and examples thereof include coupling agents, silane coupling agents, and titanium coupling agents. As the ion scavengers, known ion scavengers can be used, and examples thereof include organic aluminum (alkoxy aluminum, phenoxy aluminum, etc.). As the coloring inhibitor, known coloring inhibitors can be used. Generally, antioxidants are effective, and examples of such antioxidants include phenol-based antioxidants (monophenol-based, bisphenol-based, polymeric phenol-based, etc.), sulfur-based antioxidants, and phosphorus-based antioxidants. However, these are almost ineffective in preventing coloring during heat resistance tests at high temperatures.
[0098] When a defoaming agent, a flow control agent, a light stabilizer, an antioxidant, an adhesion imparting agent, an ion scavenger, or a coloring inhibitor is contained, the content of each is preferably 0.1 to 20,000 parts by weight, and more preferably 0.5 to 5,000 parts by weight, relative to 100 parts of the acid generator.
[0099] There are no limitations on the solvent as long as it can be used to dissolve the cationic polymerizable compound and adjust the viscosity of the photo- and thermosetting composition, and those listed above as the solvent for the acid generator can be used.
[0100] When a solvent is contained, the content of the solvent is preferably 50 to 2,000,000 parts by weight, and more preferably 200 to 500,000 parts by weight, based on 100 parts of the acid generator.
[0101] Examples of non-reactive resins include polyester, polyvinyl acetate, polyvinyl chloride, polybutadiene, polycarbonate, polystyrene, polyvinyl ether, polyvinyl butyral, polybutene, hydrogenated styrene-butadiene block copolymer, copolymer of (meth)acrylic acid ester, polyurethane, etc. The number average molecular weight of these resins is preferably 1,000 to 500,000, more preferably 5,000 to 100,000 (the number average molecular weight is a value measured by a general method such as GPC).
[0102] When a non-reactive resin is contained, the content of the non-reactive resin is preferably from 5 to 400,000 parts by weight, and more preferably from 50 to 150,000 parts by weight, based on 100 parts of the acid generator.
[0103] When a non-reactive resin is contained, it is desirable to dissolve the non-reactive resin in a solvent in advance so that the non-reactive resin can be easily dissolved in the cationic polymerizable compound and the like.
[0104] As the radical polymerizable compound, known radical polymerizable compounds (such as those described in "Photopolymer Handbook" edited by the Photopolymer Forum (1989, Industrial Research Institute), "UV / EB Curing Technology" edited by the General Technology Center (1982, General Technology Center), and "UV / EB Curing Materials" edited by the RadTech Research Group (1992, CMC)) can be used, and these include monofunctional monomers, bifunctional monomers, polyfunctional monomers, epoxy (meth)acrylates, polyester (meth)acrylates, and urethane (meth)acrylates.
[0105] When a radically polymerizable compound is contained, the content of the radically polymerizable compound is preferably from 5 to 400,000 parts by weight, and more preferably from 50 to 150,000 parts by weight, based on 100 parts of the acid generator of the present invention.
[0106] When a radically polymerizable compound is contained, it is preferable to use a radical polymerization initiator that initiates polymerization by light and heat in order to increase the molecular weight of the compound by radical polymerization.
[0107] As the radical polymerization initiator, known radical polymerization initiators can be used, including thermal radical polymerization initiators (organic peroxides, azo compounds, etc.) and photoradical polymerization initiators (acetophenone-based initiators, benzophenone-based initiators, Michler's ketone-based initiators, benzoin-based initiators, thioxanthone-based initiators, acylphosphine-based initiators, etc.).
[0108] When a radical polymerization initiator is contained, the content of the radical polymerization initiator is preferably 0.01 to 20 parts by weight, and more preferably 0.1 to 10 parts by weight, based on 100 parts of the radical polymerizable compound.
[0109] The curable composition of the present invention can be prepared by uniformly mixing and dissolving a cationically polymerizable compound, an acid generator, and, if necessary, an additive at room temperature (about 20 to 30° C.) or, if necessary, under heating (about 40 to 90° C.), or further by kneading with a three-roll mill or the like.
[0110] The curable composition of the present invention can be cured by irradiation with light to give a cured product. The light to be irradiated may be any light as long as it has energy that induces decomposition of the acid generator, but is preferably an energy ray in the ultraviolet to visible light region (wavelength: about 100 to about 800 nm) obtained from a low-, medium-, high-, or ultra-high-pressure mercury lamp, a metal halide lamp, an LED lamp, a xenon lamp, a carbon arc lamp, a fluorescent lamp, a semiconductor solid-state laser, an argon laser, a He-Cd laser, a KrF excimer laser, an ArF excimer laser, or an F2 laser, etc. Incidentally, the energy ray may also be a high-energy radiation such as an electron beam or an X-ray.
[0111] The light irradiation time is affected by the light intensity and the light transmittance to the curable composition, but about 0.1 to 10 seconds at room temperature (about 20 to 30°C) is sufficient. However, when the light transmittance is low or the film thickness of the curable composition is thick, it may be preferable to apply a longer time. Most curable compositions are cured by cationic polymerization 0.1 seconds to several minutes after light irradiation, but if necessary, after light irradiation, it is possible to aftercure by heating at room temperature (about 20 to 30°C) to 200°C for several seconds to several hours.
[0112] The curable composition of the present invention can be cured by heating to give a cured product.
[0113] As a heating method for hardening, a conventionally known method such as heat circulation heating, infrared heating, high frequency heating, etc. can be used.
[0114] The heating temperature required for curing is not particularly limited as long as it is within a range in which the curing proceeds sufficiently and does not deteriorate the base material, but is preferably in the range of 50 to 250°C, more preferably 80 to 200°C. The heating time depends on the heating temperature, but is preferably from a few minutes to a few hours from the viewpoint of productivity.
[0115] Specific applications of the curable composition of the present invention include paints, coating agents, various coating materials (hard coats, stain-resistant coatings, anti-fogging coatings, contact-resistant coatings, optical fibers, etc.), back treatment agents for adhesive tapes, release coating materials for release sheets for adhesive labels (release paper, release plastic films, release metal foils, etc.), printing plates, dental materials (dental compounds, dental composites) inks, inkjet inks, positive resists (connection terminals and wiring pattern formation in the manufacture of electronic parts such as circuit boards, CSPs, and MEMS elements), resist films, liquid resists, resists for MEMS, positive photosensitive materials, negative resists, etc. Examples of such materials include photosensitive materials, various adhesives (temporary fixing agents for various electronic components, adhesives for HDDs, adhesives for pickup lenses, adhesives for functional films for FPDs (deflectors, anti-reflection films, etc.)), holographic resins, FPD materials (color filters, black matrices, partition materials, photospacers, ribs, alignment films for liquid crystals, sealants for FPDs, etc.), optical components, molding materials (for building materials, optical components, lenses), casting materials, putty, glass fiber impregnation agents, filling materials, sealing materials, encapsulants, optical semiconductor (LED) encapsulants, optical waveguide materials, nanoimprint materials, materials for photolithography, and materials for microphotolithography.
[0116] <Adhesive> More specifically, the curable composition of the present invention can be applied to the surface of a substrate and used as a coating agent or adhesive. Usable substrates include polymer substrates such as polycarbonates and polycarbonate blends, acrylic resins such as poly(methyl methacrylate), polyesters such as poly(ethylene terephthalate) and poly(butylene terephthalate), polyamides, polyimides, acrylonitrile-styrene copolymers, styrene-acrylonitrile-butadiene copolymers, polyvinyl chloride, polystyrene, blends of polystyrene and polyphenylene ether, cellulose acetate butyrate, and polyethylene, as well as metal substrates, painted surfaces, glass, ceramics, concrete, slate boards, and fabrics.
[0117] The method of applying the adhesive made of the curable composition of the present invention to a substrate is not particularly limited, and conventionally known methods such as bar coating, spray coating, curtain coating, roll coating, screen printing, offset printing, gravure printing, etc. may be used. In addition, the adhesive may be diluted with various solvents to obtain an appropriate viscosity, and applied using a spin coater, die coater, etc., and then the solvent may be removed by heating. The thickness of the composition layer of the present invention provided on the substrate is not particularly limited, and may be, for example, 1 to 500 μm, and preferably 10 to 200 μm. After irradiating the adhesive made of the composition of the present invention provided on a substrate with energy light, the substrate is placed on the composition layer and then heated to obtain an adhesive body between the substrates. When bonding the substrates together, appropriate pressure may be applied or the substrates may be bonded while being heated. The heating temperature and heating time are not particularly limited as long as the composition is thermally cured and the substrates are bonded to each other, but are preferably 80°C or higher for 30 minutes or longer. The heating temperature and heating time are preferably selected taking into consideration the heat resistance of the substrate.
[0118] <Optical element materials> Furthermore, the cured product obtained by curing the curable composition of the present invention has excellent heat resistance, and the 5% weight loss temperature is, for example, 260° C. or higher, preferably 280° C. or higher, and particularly preferably 300° C. or higher. The 5% weight loss temperature is determined by simultaneous differential thermal analysis-thermogravimetry (TG-DTA). Therefore, the shape can be maintained even under high temperature conditions such as soldering by a reflow method. Furthermore, the cured product has excellent transparency, and the yellowness index (YI) of the cured product before a heat resistance test is, for example, 1.5 or less. The cured product obtained by curing the curable composition of the present invention can suppress yellowing and maintain transparency even under high temperature conditions such as soldering by a reflow method, and the yellowness index (YI) of the cured product after a heat resistance test is, for example, 1.5 or less.
[0119] An optical element containing the cured product obtained by curing the curable composition of the present invention as a component has excellent heat resistance and heat yellowing resistance, and is suitable for use as an optical element for, for example, lenses, prisms, LEDs, organic EL elements, semiconductor lasers, transistors, solar cells, CCD image sensors, optical waveguides, optical fibers, and alternative glass (for example, display substrates, hard disk substrates, and polarizing films).
[0120] In addition, an optical element containing the cured product obtained by curing the curable composition of the present invention as a component has excellent heat resistance, so that it can be mounted together with other components by reflow treatment when mounting on a substrate. It can also be used in in-vehicle electronic devices that require heat resistance. Examples of optical devices equipped with the above-mentioned optical element include portable electronic devices such as mobile phones, smartphones, and tablet PCs; and in-vehicle electronic devices such as near-infrared sensors, millimeter-wave radars, LED spot lighting devices, near-infrared LED lighting devices, mirror monitors, meter panels, combiners for head-mounted displays (projection type), and combiners for head-up displays.
[0121] <Resin composition for optical three-dimensional modeling> The curable composition of the present invention can also be used as a resin composition for optical three-dimensional modeling, which further contains a radical polymerizable compound and a radical polymerization initiator.
[0122] In the resin composition for optical three-dimensional modeling of the present invention, one or more of the above-mentioned epoxy compounds can be used as the cationic polymerizable compound, and it is preferable that the cationic polymerizable compound contains a polyepoxy compound having two or more epoxy groups in one molecule in a proportion of 30% by weight or more based on the total weight of the cationic polymerizable compound.
[0123] When the resin composition for optical three-dimensional modeling of the present invention contains the above-mentioned alicyclic diglycidyl ether compound as a part of the cationic polymerizable compound, the three-dimensional object obtained by optical modeling generally has further improved transparency, further reduced yellowness, and excellent dimensional stability over time, water resistance, moisture resistance, heat resistance, etc. Furthermore, when an aromatic compound having three or more glycidyl etherified phenol groups is contained as part of the cationic polymerizable compound in the resin composition for optical 3D modeling of the present invention, it is possible to obtain a resin composition for optical 3D modeling that gives a 3D object having a high heat distortion temperature and excellent heat resistance. When an aromatic compound having three or more glycidyl etherified phenol groups is contained as a part of a cationic polymerizable compound in order to improve the heat resistance of a three-dimensional object obtained by stereolithography, the content thereof is preferably 5 to 80 wt %, more preferably 10 to 50 wt %, and further preferably 20 to 40 wt %, based on the total weight of the cationic polymerizable compound.
[0124] As the aromatic compound having three or more glycidyl etherified phenol groups, any compound can be used as long as it can maintain the viscosity of the resin composition for optical 3D modeling at a level suitable for optical 3D modeling even when it contains the aromatic compound. Examples of the compound include polyglycidyl ethers of phenolic resins such as novolac resins and resol resins, tetraglycidyl ethers of tetraphenolethane, triglycidyl ethers of triphenolmethane and triphenolethane, and 2-[4-(2,3-epoxypropoxy)phenyl]-2-[4-[1,1-bis[4-(2,3-epoxypropoxy)phenyl]ethyl]phenyl]propane (manufactured by Printec Co., Ltd., product name: VG3101L).
[0125] When the above-mentioned VG3101L is contained as a part of the cationic polymerizable compound in the resin composition for optical 3D modeling, the heat distortion temperature of the 3D object obtained by stereolithography is increased and the heat resistance is improved. When VG3101L is contained as a part of the cationic polymerizable compound in order to improve the heat resistance of the 3D object obtained by stereolithography, the content of VG3101L is preferably 1.5 to 80 wt%, more preferably 5 to 50 wt%, and more preferably 20 to 40 wt%, based on the total weight of the cationic polymerizable compound.
[0126] From the standpoint of photocuring performance and improved modeling properties due to reduced viscosity, the resin composition for optical 3D modeling of the present invention preferably contains an oxetane compound in an amount of 1 to 35% by weight, and more preferably 5 to 20% by weight, based on the total weight of the cationically polymerizable compound contained in the resin composition for optical 3D modeling.
[0127] Preferred examples of the oxetane compound include monooxetane monoalcohols such as 3-hydroxymethyl-3-methyloxetane, 3-hydroxymethyl-3-ethyloxetane, 3-hydroxymethyl-3-propyloxetane, 3-hydroxymethyl-3-normal butyloxetane, and 3-hydroxymethyl-3-propyloxetane, and dioxetane compounds such as bis(3-methyl-3-oxetanylmethyl)ether, bis(3-ethyl-3-oxetanylmethyl)ether, bis(3-propyl-3-oxetanylmethyl)ether, and bis(3-butyl-3-oxetanylmethyl)ether. Among these, from the viewpoints of availability, reactivity, and the like, 3-hydroxymethyl-3-methyloxetane, 3-hydroxymethyl-3-ethyloxetane, bis(3-methyl-3-oxetanylmethyl)ether, and bis(3-ethyl-3-oxetanylmethyl)ether are more preferred.
[0128] In addition, when the diglycidyl ether of an alkylene diol is contained in the resin composition for optical three-dimensional modeling of the present invention, the toughness of the three-dimensional model obtained by optical modeling is improved. As the diglycidyl ether of an alkylene diol, diglycidyl ethers of alkylene diols having 2 to 10 carbon atoms such as ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, butanediol diglycidyl ether, pentanediol diglycidyl ether, hexanediol diglycidyl ether, heptanediol diglycidyl ether, octanediol diglycidyl ether, nonanediol diglycidyl ether, and decanediol diglycidyl ether are preferred, and one or more of these can be used. Among them, 1,6-hexanediol diglycidyl ether is more preferably used from the viewpoint of curing performance. When a diglycidyl ether of an alkylene diol is contained in the resin composition for optical 3D modeling of the present invention in order to improve the toughness of a 3D object obtained by optical modeling, the content of the diglycidyl ether of an alkylene diol is preferably 0.1 to 20% by weight, more preferably 0.5 to 10% by weight, and even more preferably 1 to 5% by weight, based on the total weight of the cationically polymerizable compound contained in the resin composition for optical 3D modeling.
[0129] By incorporating an aromatic thiol compound into the resin composition for optical three-dimensional modeling of the present invention, a three-dimensional model having low yellowness and excellent color tone and appearance, which is colorless and transparent or nearly so, can be obtained. There is no particular limitation on the aromatic thiol compound, and one type of aromatic thiol compound may be used, or two or more types may be used. From the viewpoints of availability, odor, solubility, little effect on the curing reaction, and effect of reducing the yellowness of the three-dimensional modeled product obtained by photolithography, naphthalene thiol, dimercapto naphthalene, and dimercapto diphenyl sulfide are preferred. When an aromatic thiol compound is contained in the resin composition for optical 3D modeling of the present invention, the content of the aromatic thiol compound is preferably 0.1 to 5 wt %, more preferably 0.2 to 2 wt %, based on the weight of the photoacid generator in the resin composition for optical 3D modeling.
[0130] Representative examples of radical polymerizable compounds include compounds having a (meth)acrylate group, unsaturated polyester compounds, allyl urethane compounds, polythiol compounds, etc., and one or more of the above radical polymerizable compounds can be used. Among them, compounds having at least one (meth)acryloyloxy group in one molecule are preferably used, and specific examples include reaction products of epoxy compounds and (meth)acrylic acid, (meth)acrylic acid esters of alcohols, urethane (meth)acrylates, polyester (meth)acrylates, polyether (meth)acrylates, etc.
[0131] Examples of the reaction product of the epoxy compound and (meth)acrylic acid include (meth)acrylate-based reaction products obtained by reacting an aromatic epoxy compound, an alicyclic epoxy compound, and / or an aliphatic epoxy compound with (meth)acrylic acid. Specific examples include (meth)acrylates obtained by reacting glycidyl ether obtained by reacting a bisphenol compound such as bisphenol A or bisphenol S, or a bisphenol compound such as bisphenol A or bisphenol S in which the benzene ring is substituted with an alkoxy group or the like, or an alkylene oxide adduct of the bisphenol compound or the substituted bisphenol compound with an epoxidizing agent such as epichlorohydrin, with (meth)acrylic acid, and (meth)acrylate-based reaction products obtained by reacting an epoxy novolac resin with (meth)acrylic acid.
[0132] In addition, examples of the (meth)acrylic acid esters of the above-mentioned alcohols include (meth)acrylates obtained by reacting aromatic alcohols, aliphatic alcohols, alicyclic alcohols, and / or alkylene oxide adducts thereof, each of which has at least one hydroxyl group in the molecule, with (meth)acrylic acid. More specifically, for example, di(meth)acrylates of bisphenol compounds such as bisphenol A and bisphenol S, or bisphenol compounds such as bisphenol A and bisphenol S in which the benzene ring is substituted with an alkoxy group or the like, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isooctyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, Examples of the polyhydric alcohol having three or more hydroxyl groups include glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyalkylene glycol di(meth)acrylate [e.g., polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, etc.], poly(meth)acrylates of polyhydric alcohols having three or more hydroxyl groups such as trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and (meth)acrylates of alkylene oxide adducts of polyhydric alcohols such as the above-mentioned diols, triols, tetraols, and hexaols.
[0133] In addition, the above-mentioned urethane (meth)acrylate may be, for example, a (meth)acrylate obtained by reacting a hydroxyl group-containing (meth)acrylic acid ester with an isocyanate compound. The hydroxyl group-containing (meth)acrylic acid ester is preferably a hydroxyl group-containing (meth)acrylic acid ester obtained by esterification reaction of an aliphatic dihydric alcohol with (meth)acrylic acid, and a specific example thereof may be 2-hydroxyethyl (meth)acrylate. In addition, the isocyanate compound is preferably a polyisocyanate compound having two or more isocyanate groups in one molecule, such as tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, etc.
[0134] Furthermore, the above-mentioned polyester (meth)acrylate may be a polyester (meth)acrylate obtained by reacting a hydroxyl group-containing polyester with (meth)acrylic acid, and the above-mentioned polyether (meth)acrylate may be a polyether acrylate obtained by reacting a hydroxyl group-containing polyether with acrylic acid.
[0135] When the resin composition for optical 3D modeling contains, as a part of the radical polymerizable compound, 1 to 40% by weight, particularly 5 to 20% by weight of polyalkylene glycol di(meth)acrylate such as polytetramethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, or polyethylene glycol di(meth)acrylate, based on the weight of the radical polymerizable compound, the toughness of the 3D object obtained from the resin composition for optical 3D modeling is improved. However, if the content of polyalkylene glycol di(meth)acrylate is too high, the heat distortion temperature of the obtained 3D object is lowered, and the heat resistance is reduced.
[0136] As the radical polymerization initiator, any polymerization initiator that can initiate radical polymerization of a radically polymerizable compound when irradiated with active energy rays such as light can be used. Examples of the radical polymerization initiator include benzyl or its dialkyl acetal compound, phenyl ketone compound, acetophenone compound, benzoin or its alkyl ether compound, benzophenone compound, and thioxanthone compound.
[0137] Specifically, examples of benzyl or its dialkyl acetal compounds include benzyl dimethyl ketal and benzyl-β-methoxyethyl acetal. An example of the phenyl ketone compound is 1-hydroxy-cyclohexyl phenyl ketone. Examples of acetophenone compounds include diethoxyacetophenone, 2-hydroxymethyl-1-phenylpropan-1-one, 4'-isopropyl-2-hydroxy-2-methyl-propiophenone, 2-hydroxy-2-methyl-propiophenone, p-dimethylaminoacetophenone, p-tert-butyldichloroacetophenone, p-tert-butyltrichloroacetophenone, and p-azidobenzalacetophenone.
[0138] Examples of the benzoin compounds include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin normal butyl ether, and benzoin isobutyl ether. Examples of the benzophenone compounds include benzophenone, methyl o-benzoylbenzoate, Michler's ketone, 4,4'-bisdiethylaminobenzophenone, and 4,4'-dichlorobenzophenone. Examples of thioxanthone compounds include thioxanthone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, and 2-isopropylthioxanthone.
[0139] The resin composition for optical three-dimensional object formation of the present invention may contain one or more suitable amounts of an antifoaming agent, a leveling agent, a thickening agent, a flame retardant, an antioxidant, a modifying resin, etc., as necessary, so long as the effects of the present invention are not impaired.
[0140] When optically forming a three-dimensional object using the resin composition for optical three-dimensional modeling of the present invention, any of the conventionally known optical three-dimensional modeling methods and devices can be used.A representative example of the optical three-dimensional modeling method that can be preferably adopted is a method in which the liquid resin composition for optical three-dimensional modeling of the present invention is selectively irradiated with active energy rays to form a cured layer having a desired pattern, and then an uncured liquid resin composition for optical three-dimensional modeling is supplied to this cured layer, and similarly irradiated with active energy rays to form a new cured layer continuous with the cured layer, and the lamination operation is repeated to finally obtain a three-dimensional object as desired. As described above, examples of the active energy rays used in this case include ultraviolet rays, electron beams, X-rays, radiation, high frequency waves, etc. Among these, ultraviolet rays having a wavelength of 300 to 400 nm are preferably used from an economical viewpoint, and examples of the light source that can be used in this case include ultraviolet lasers (e.g., semiconductor pumped solid-state lasers, Ar lasers, He-Cd lasers, etc.), high pressure mercury lamps, ultra-high pressure mercury lamps, low pressure mercury lamps, xenon lamps, halogen lamps, metal halide lamps, ultraviolet LEDs (light emitting diodes), and ultraviolet fluorescent lamps.
[0141] When forming each cured resin layer having a predetermined shape pattern by irradiating active energy rays onto a modeling surface made of a resin composition for optical three-dimensional modeling, the cured resin layer may be formed by a pointillist or line drawing method using active energy rays focused into a point shape such as laser light, or a modeling method may be adopted in which the cured resin layer is formed by irradiating active energy rays in a planar manner onto the modeling surface through a planar drawing mask formed by arranging a plurality of micro-optical shutters such as liquid crystal shutters or digital micromirror shutters (DMDs).
[0142] The resin composition for optical 3D modeling of the present invention can be widely used in the field of optical 3D modeling, and can be effectively used in applications such as, but not limited to, shape confirmation models for verifying appearance designs during the design process, function test models for checking the functionality of parts, master models for producing casting molds, master models for producing metal molds, direct molds for prototype molds, automobile and motorcycle lenses, art restorations, replicas, modern art, art and crafts such as design presentation models for glass-covered buildings, models, master molds, and processing of precision parts, electric and electronic parts, furniture, architectural structures, automobile parts, various containers, and castings.
[0143] <Resin composition for optical waveguide> The curable composition of the present invention can also be used as a resin composition for optical waveguides, which contains a resin having a cationically polymerizable substituent and an acid generator.
[0144] The resin component includes various epoxy resins used as core forming materials, such as side chain polyfunctional aliphatic epoxy resins. The side chain polyfunctional aliphatic epoxy resins are aliphatic resins having two or more functional groups in the side chain, such as polyfunctional aliphatic epoxy resins such as 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol. These are used alone or in combination of two or more. From the viewpoint of availability and ease of handling, a preferred specific example is EHPE3150 (manufactured by Daicel Corporation).
[0145] In the epoxy resin such as the side-chain polyfunctional aliphatic epoxy resin, a polymerizable substituent is present in the epoxy resin, and the polymerizable substituent is preferably a cationically polymerizable substituent. Examples of the cationically polymerizable substituent include an epoxy group and an epoxy group having an alicyclic skeleton.
[0146] Furthermore, an example of the aliphatic epoxy resin having the polymerizable substituent is, for example, a bifunctional long-chain aliphatic epoxy resin. The bifunctional long-chain aliphatic epoxy resin is, for example, a long-chain aliphatic epoxy resin having epoxy groups, which are polymerizable functional groups, at both ends. In this way, by using the long-chain aliphatic epoxy resin, it is possible to reduce the crosslink density in cationic polymerization, and the flexibility of the cured product can be imparted. Examples of such bifunctional long-chain aliphatic epoxy resins include hydrogenated bisphenol A type epoxy resins and hydrogenated bisphenol F type epoxy resins. These are used alone or in combination of two or more kinds. Specific examples include YX-8040 (manufactured by Mitsubishi Chemical Corporation) and ST-4000D (manufactured by Nippon Steel Chemical Co., Ltd.).
[0147] For example, when the side chain polyfunctional aliphatic epoxy resin (A) and the bifunctional long chain aliphatic epoxy resin (B) are used in combination, the mixing weight ratio [(A):(B)] is preferably (A):(B)=4:1 to 1:1, and particularly preferably (A):(B)=3:1 to 1:1. If the mixing weight ratio is outside the above range, for example, if the side chain polyfunctional aliphatic epoxy resin (A) is too little, patterning properties tend to deteriorate in photo- and thermo-curing.
[0148] The content of the acid generator is preferably set to 0.1 to 3 parts by weight, more preferably 0.5 to 3 parts by weight, and particularly preferably 0.5 to 1 part by weight, based on 100 parts by weight of the resin component of the resin composition for optical waveguide of the present invention. That is, if the content of the acid generator is too low, it is difficult to obtain satisfactory curability, for example, when curing by light irradiation (ultraviolet irradiation), while if the content is too high, the photosensitivity increases, and there is a tendency for shape abnormalities to occur during patterning, and for the required physical property of initial loss to deteriorate.
[0149] In addition to the above-mentioned resin components and specific acid generators, the resin composition for optical waveguide of the present invention may contain, as necessary, for example, silane-based or titanium-based coupling agents for enhancing adhesion, cycloolefin-based oligomers and polymers such as olefin-based oligomers and norbornene-based polymers, synthetic rubbers, adhesion promoters such as silicone compounds, various antioxidants such as hindered phenol-based antioxidants and phosphorus-based antioxidants, leveling agents, defoamers, etc. These additives are appropriately blended within a range that does not impair the effects of the present invention. These can be used alone or in combination of two or more types.
[0150] The resin composition for optical waveguide of the present invention can be prepared by mixing the above resin components and a specific acid generator, and if necessary, other additives, at a predetermined mixing ratio. Furthermore, in order to prepare the photosensitive resin composition of the present invention as a coating varnish, it may be stirred and dissolved in an organic solvent under heating (for example, at about 60 to 90°C). The amount of the organic solvent used is appropriately adjusted, but is preferably set to 20 to 80 parts by weight, and particularly preferably 30 to 40 parts by weight, per 100 parts by weight of the resin components of the curable resin composition. That is, if the amount of organic solvent used is too small, the viscosity becomes high when prepared as a coating varnish, and the coatability tends to decrease, and if the amount of organic solvent used is too large, it tends to be difficult to form a thick coating using the coating varnish.
[0151] Examples of organic solvents used in preparing the coating varnish include ethyl lactate, methyl ethyl ketone, cyclohexanone, ethyl lactate, 2-butanone, N,N-dimethylacetamide, diglyme, diethylene glycol methyl ethyl ether, propylene glycol methyl acetate, propylene glycol monomethyl ether, tetramethylfuran, dimethoxyethane, etc. These organic solvents may be used alone or in combination of two or more, and may be used in a predetermined amount within the above range so as to provide a viscosity suitable for coating.
[0152] The optical waveguide obtained by the present invention is composed of, for example, a substrate, a cladding layer (undercladding layer) formed on the substrate in a predetermined pattern, a core layer formed on the cladding layer in a predetermined pattern for propagating an optical signal, and a cladding layer (overcladding layer) formed on the core layer. The optical waveguide obtained by the present invention is characterized in that the core layer is formed from the above-mentioned curable resin composition. As for the undercladding layer forming material and the overcladding layer forming material, a resin composition for forming a cladding layer having the same component composition may be used, or a resin composition having a different component composition may be used. In the optical waveguide obtained by the present invention, the cladding layer needs to be formed so as to have a smaller refractive index than the core layer.
[0153] In the present invention, the optical waveguide can be manufactured, for example, through the following steps. That is, a substrate is prepared, and a varnish made of a curable resin composition, which is a cladding layer forming material, is applied onto the substrate. The varnish-coated surface is irradiated with light such as ultraviolet light, and further heated as necessary to cure the varnish. In this way, an undercladding layer (the lower portion of the cladding layer) is formed.
[0154] Next, a core layer forming material (curable varnish) made by dissolving the curable resin composition of the present invention in an organic solvent is applied onto the undercladding layer to form an uncured layer for core formation. At this time, after the core layer forming material (curable varnish) is applied, the organic solvent is heated and dried to remove it, so that it is formed into a film shape that becomes an uncured optical waveguide core layer forming curable film. Then, a photomask for exposing a predetermined pattern (optical waveguide pattern) is arranged on the surface of the core forming uncured layer, and light irradiation such as ultraviolet light is performed through the photomask, and further heat treatment is performed as necessary. Thereafter, the unexposed portion of the core forming uncured layer is dissolved and removed using a developer to form a core layer of a predetermined pattern.
[0155] Next, a varnish made of a curable resin composition, which is the cladding layer forming material, is applied onto the core layer, and then the varnish is irradiated with light such as ultraviolet light, and further heated as necessary to form an overcladding layer (the upper part of the cladding layer). Through these steps, the desired optical waveguide can be manufactured.
[0156] Examples of the substrate material include silicon wafers, metal substrates, polymer films, glass substrates, etc. Examples of the metal substrate include stainless steel plates such as SUS. Specific examples of the polymer film include polyethylene terephthalate (PET) films, polyethylene naphthalate films, polyimide films, etc. The thickness of the film is usually set within the range of 10 μm to 3 mm.
[0157] Specifically, the light irradiation is performed by ultraviolet irradiation. Examples of the ultraviolet light source for the ultraviolet irradiation include a low pressure mercury lamp, a high pressure mercury lamp, and an ultra-high pressure mercury lamp. The irradiation dose of ultraviolet light is usually 10 to 20,000 mJ / cm. 2 , preferably 100 to 15,000 mJ / cm 2 , more preferably 500 to 10,000 mJ / cm 2 The degree can be given.
[0158] After the exposure to ultraviolet light, a heat treatment may be further carried out to complete the curing by the photoreaction. The heat treatment is usually carried out at 80 to 250° C., preferably 100 to 150° C., for 10 seconds to 2 hours, preferably 5 minutes to 1 hour.
[0159] Examples of the cladding layer-forming material include various liquid epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, fluorinated epoxy resin, and epoxy-modified silicone resin, solid epoxy resin, and resin compositions containing the above-mentioned various acid generators as appropriate, and are formulated to have a lower refractive index as appropriate compared with the core layer-forming material. Furthermore, since the cladding layer-forming material is prepared as a varnish and applied as necessary, various conventionally known organic solvents may be used to obtain a viscosity suitable for application, and various additives (antioxidants, adhesion promoters, leveling agents, ultraviolet (UV) absorbers) may be used in appropriate amounts to the extent that they do not reduce the function of the optical waveguide using the core layer-forming material.
[0160] As described above, examples of the organic solvent used in preparing the varnish include ethyl lactate, methyl ethyl ketone, cyclohexanone, ethyl lactate, 2-butanone, N,N-dimethylacetamide, diglyme, diethylene glycol methyl ethyl ether, propylene glycol methyl acetate, propylene glycol monomethyl ether, tetramethylfuran, dimethoxyethane, etc. These organic solvents are used alone or in combination of two or more kinds in an appropriate amount so as to obtain a viscosity suitable for application.
[0161] Examples of the method for applying the materials for forming each layer onto the substrate include a coating method using a spin coater, a coater, a circular coater, a bar coater, etc., a screen printing method, a method in which a gap is formed using a spacer and the material is injected into the gap by capillary action, a method in which the material is continuously applied in a roll-to-roll (R-to-R) manner using a coating machine such as a multi-coater, etc. The optical waveguide can also be made into a film-like optical waveguide by peeling off the substrate.
[0162] The optical waveguide thus obtained can be used, for example, as an optical waveguide for a hybrid flexible printed wiring board for optical and electrical transmission. EXAMPLES
[0163] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following, unless otherwise specified, parts means parts by weight and % means % by weight.
[0164] <Synthesis of anion part> (Synthesis Example 1) Synthesis of lithium tetrakis(2-trifluoromethyl-2-propoxy)aluminate (A-1) 0.95g of lithium aluminum hydride and 5.0g of dimethoxyethane were charged into a 200mL four-neck flask equipped with a reflux condenser that had been thoroughly dried under a nitrogen atmosphere, and 150mL of toluene was added thereto and stirred. This was cooled to 10°C in an ice bath. 16.0g of 2-trifluoromethyl-2-propanol was added dropwise, and then stirred at room temperature for 1 hour. This was further heated and refluxed for 5 hours. The reaction solution was returned to room temperature, the precipitated solid was filtered, and the reaction solution was transferred to an evaporator, and the solvent was distilled off to obtain a white solid (11.6g). 1 H, 19 F-NMR confirmed that this white solid was (A-1) (yield 86%, fluorine substitution rate 33%).
[0165] (Synthesis Example 2) Synthesis of lithium tetrakis(2-pentafluoroethyl-2-propoxy)aluminate (A-2) A white solid (15.6 g) was obtained in the same manner as in Synthesis Example 1, except that 16.0 g of 2-trifluoromethyl-2-propanol was changed to 22.3 g of 2-pentafluoroethyl-2-propanol. 1 H, 19 F-NMR confirmed that this white solid was (A-2) (yield 84%, fluorine substitution rate 45%).
[0166] (Synthesis Example 3) Synthesis of lithium tetrakis(hexafluoro-tert-butoxy)aluminate (A-4) A white solid (16.0 g) was obtained in the same manner as in Synthesis Example 1, except that 16.0 g of 2-trifluoromethyl-2-propanol was changed to 22.8 g of hexafluoro-tert-butanol. 1 H, 19 F-NMR confirmed that this white solid was (A-4) (yield 84%, fluorine substitution rate 67%).
[0167] (Synthesis Example 4) Synthesis of lithium tetrakis(2-phenyl-hexafluoro-2-propoxy)aluminate (A-7) A white solid was obtained (17.5 g) in the same manner as in Synthesis Example 1, except that 16.0 g of 2-trifluoromethyl-2-propanol was changed to 30.5 g of 2-phenyl-hexafluoro-2-propanol. 1 H, 19 F-NMR confirmed that this white solid was (A-7) (yield 70%, fluorine substitution rate 55%).
[0168] (Synthesis Example 5) Synthesis of lithium tetrakis(2-p-chlorophenyl-hexafluoro-2-propoxy)aluminate (A-10) A pale yellow solid (12.8 g) was obtained in the same manner as in Synthesis Example 1, except that 16.0 g of 2-trifluoromethyl-2-propanol was changed to 34.8 g of 2-p-chlorophenyl-hexafluoro-2-propanol. 1 H, 19 F-NMR confirmed that this pale yellow solid was (A-10) (yield 45%, fluorine substitution rate 60%).
[0169] (Synthesis Example 6) Synthesis of lithium tris(2-trifluoromethyl-2-propoxy)(nonafluoro-tert-butoxy)aluminate (A-13) 0.95g of lithium aluminum hydride and 5.0g of dimethoxyethane were charged into a 200mL four-neck flask equipped with a reflux condenser that had been thoroughly dried under a nitrogen atmosphere, and 150mL of toluene was added thereto and stirred. This was cooled to 10°C in an ice bath. 9.6g of 2-trifluoromethyl-2-propanol was added dropwise, and then stirred at room temperature for 1 hour. 11.8g of nonafluoro-tert-butanol was added thereto, and this was further heated and refluxed for 6 hours. The reaction solution was returned to room temperature, the precipitated solid was filtered, and the reaction solution was transferred to an evaporator, and the solvent was distilled off to obtain a white solid (7.1g). 1 H, 19 F-NMR confirmed that this white solid was (A-13) (yield 44%, fluorine substitution rate 50%).
[0170] (Comparative Synthesis Example 1) Synthesis of lithium tetrakis(perfluoro-tert-pentoxy)aluminate (A-21) A white solid was obtained (21.2 g) in the same manner as in Synthesis Example 1, except that 16.0 g of 2-trifluoromethyl-2-propanol was changed to 35.8 g of perfluoro-tert-amyl alcohol. 1 H, 19 F-NMR confirmed that this white solid was (A-21) (yield 74%, fluorine substitution rate 100%).
[0171] (Comparative Synthesis Example 2) Synthesis of lithium tetrakis(octafluoro-tert-pentoxy)aluminate (A-24) A white solid (11.2 g) was obtained in the same manner as in Synthesis Example 1, except that 16.0 g of 2-trifluoromethyl-2-propanol was changed to 29.0 g of octafluoro-tert-amyl alcohol. 1 H, 19 F-NMR confirmed that this white solid was (A-21) (yield 47%, fluorine substitution rate 73%).
[0172] <Synthesis of photoacid generator>
[0173] (Synthesis Example 7) Synthesis of [4-(4-biphenylthio)phenyl]-4-biphenylphenylsulfonium tetrakis(2-trifluoromethyl-2-propoxy)aluminate (AG-1) 11g of 4-[(phenyl)sulfinyl]biphenyl, 12g of 4-(phenylthio)biphenyl, 22g of acetic anhydride, and 16g of methanesulfonic acid were mixed uniformly and reacted at 65°C for 3 hours. The reaction solution was cooled to room temperature, poured into 100mL of ion-exchanged water, extracted with 100g of dichloromethane, and washed with water until the pH of the aqueous layer became neutral. The solvent was removed from the dichloromethane layer using a rotary evaporator to obtain a brown solid. This was washed with ethyl acetate / hexane, and the organic solvent was concentrated to obtain 20g of [4-(4-biphenylthio)phenyl]-4-biphenylphenylsulfonium methanesulfonate (intermediate-1). 6.2 g of (Intermediate-1) was dissolved in 60 mL of dichloromethane, and 70 g of an equimolar aqueous solution of lithium salt (A-1) was mixed at room temperature and stirred for 3 hours. The dichloromethane layer was washed five times with water by a separation operation, and then transferred to a rotary evaporator to distill off the solvent, yielding acid generator (AG-1) in 75% yield. The product was 1 H, 19 Identification was performed using F-NMR.
[0174] (Synthesis Example 8) Synthesis of [4-(4-biphenylthio)phenyl]-4-biphenylphenylsulfonium tetrakis(hexafluoro-tert-butoxy)aluminate (AG-2) An acid generator (AG-2) was obtained in a yield of 78% in the same manner as in Synthesis Example 7, except that the aqueous solution of lithium salt (A-1) in Synthesis Example 7 was changed to an aqueous solution of lithium salt (A-4). 1 H, 19 Identification was performed using F-NMR.
[0175] (Synthesis Example 9) Synthesis of [4-(phenylthio)phenyl]sulfonium tetrakis(2-p-chlorophenyl-hexafluoro-2-propoxy)aluminate (AG-3) 15g of diphenyl sulfoxide, 16g of diphenyl sulfide, 25g of acetic anhydride, 15g of trifluoromethanesulfonic acid and 130g of acetonitrile were mixed uniformly and reacted at 40°C for 6 hours. The reaction solution was cooled to room temperature, poured into 500g of ion-exchanged water, extracted with 500g of dichloromethane, and washed with ion-exchanged water until the pH of the aqueous layer became neutral. The dichloromethane layer was transferred to a rotary evaporator, the solvent was distilled off, and a brown liquid product was obtained. 200g of ethyl acetate was added to this, and the mixture was dissolved in a water bath at 60°C. After that, 600g of hexane was added and stirred, and the mixture was cooled to 5°C and left to stand for 30 minutes, and the supernatant was removed twice to wash the product. This was transferred to a rotary evaporator and the solvent was distilled off to obtain 30g of [4-(phenylthio)phenyl]sulfonium trifluoromethanesulfonate (intermediate-2). 5.2 g of (Intermediate-2) was dissolved in 50 mL of dichloromethane, and 70 g of an equimolar aqueous solution of lithium salt (A-10) was mixed at room temperature and stirred for 3 hours. The dichloromethane layer was washed five times with water by a separation operation, and then transferred to a rotary evaporator to distill off the solvent, obtaining an acid generator (AG-3) with a yield of 83%. The product was 1 H, 19 Identification was performed using F-NMR.
[0176] (Synthesis Example 10) Synthesis of [4-(phenylthio)phenyl]sulfonium tetrakis(2-phenyl-hexafluoro-2-propoxy)aluminate (AG-4) An acid generator (AG-4) was obtained in a yield of 80% in the same manner as in Synthesis Example 9, except that the aqueous solution of lithium salt (A-10) in Synthesis Example 9 was changed to an aqueous solution of lithium salt (A-7). 1 H, 19 Identification was performed using F-NMR.
[0177] (Synthesis Example 11) Synthesis of [4-(9,9-dimethylfluorenyl-2-thio)phenyl]-2-(9,9-dimethyl)fluorenylphenylsulfonium tetrakis(2-pentafluoroethyl-2-propoxy)aluminate (AG-5) 13g of 2-(phenylsulfinyl)-9,9-dimethylfluorene, 14g of 2-(phenylthio)-9,9-dimethylfluorene, 22g of acetic anhydride, and 16g of methanesulfonic acid were mixed uniformly and reacted at 65°C for 3 hours. The reaction solution was cooled to room temperature, poured into 100mL of ion-exchanged water, extracted with 100g of dichloromethane, and washed with water until the pH of the aqueous layer became neutral. The dichloromethane layer was transferred to a rotary evaporator to distill off the solvent, thereby obtaining a brown solid. This was washed with ethyl acetate / hexane, and the organic solvent was concentrated to obtain 25g of [4-(9,9-dimethylfluorenyl-2-thio)phenyl]-2-(9,9-dimethyl)fluorenylphenylsulfonium methanesulfonate (intermediate-3). 7.0 g of (Intermediate-3) was dissolved in 60 mL of dichloromethane, and 70 g of an equimolar aqueous solution of lithium salt (A-2) was mixed at room temperature and stirred for 3 hours. The dichloromethane layer was washed five times with water by a separation operation, and then transferred to a rotary evaporator to distill off the solvent, yielding acid generator (AG-5) in 69% yield. The product was 1 H, 19 Identification was performed using F-NMR.
[0178] (Synthesis Example 12) Synthesis of [4-(9,9-dimethylfluorenyl-2-thio)phenyl]-2-(9,9-dimethyl)fluorenylphenylsulfonium tris(2-trifluoromethyl-2-propoxy)(nonafluoro-tert-butoxy)aluminate (AG-6) An acid generator (AG-6) was obtained in a yield of 72% in the same manner as in Synthesis Example 11, except that the aqueous solution of lithium salt (A-2) in Synthesis Example 11 was changed to an aqueous solution of lithium salt (A-13). 1 H, 19 Identification was performed using F-NMR.
[0179] (Synthesis Example 13) Synthesis of di(4-tert-butylphenyl)iodonium tetrakis(2-phenyl-hexafluoro-2-propoxy)aluminate (AG-7) A reaction vessel was charged with 5.4 g of di(4-tert-butylphenyl)iodonium hexafluorophosphate and 50 g of dichloromethane. 50 parts of an aqueous solution containing an equimolar amount of lithium salt (A-7) was added with stirring and stirred at room temperature for 8 hours. After standing, the aqueous layer was removed by separation, and the organic layer was washed five times with 50 parts of water. The organic solvent was distilled off under reduced pressure to obtain an acid generator (AG-7) in a yield of 88%. The product was 1 H, 19 Identification was performed using F-NMR.
[0180] (Synthesis Example 14) Synthesis of di(4-tert-butylphenyl)iodonium tetrakis(2-p-chlorophenyl-hexafluoro-2-propoxy)aluminate (AG-8) An acid generator (AG-8) was obtained in a yield of 81% in the same manner as in Synthesis Example 13, except that the aqueous solution of lithium salt (A-7) in Synthesis Example 13 was changed to an aqueous solution of lithium salt (A-10). 1 H, 19 Identification was performed using F-NMR.
[0181] (Synthesis Example 15) Synthesis of (4-isopropylphenyl)tolyliodonium tetrakis(2-trifluoromethyl-2-propoxy)aluminate (AG-9) 20 g of 4-methyliodobenzene was added to a reaction vessel, and 50 g of acetic acid and 10 g of sulfuric acid were added and dissolved. While cooling in an ice-water bath, 10 g of potassium persulfate was gradually added at 15°C or less. The reaction was allowed to proceed at 20°C for 4 hours, and 24.4 g of cumene (isopropylbenzene) was added dropwise thereto so as not to exceed 20°C. The reaction was then allowed to proceed at room temperature for 20 hours. The reaction liquid was poured into 500 parts of an aqueous solution containing an equimolar amount of lithium salt (A-1), and the mixture was stirred for another 3 hours. 500 parts of dichloromethane was added thereto. After leaving the mixture to stand, the aqueous layer was removed by separation, and the organic layer was washed five times with 100 parts of water. The dichloromethane was concentrated and recrystallized with cyclohexane to obtain an acid generator (AG-9) with a yield of 84%. The product was 1 H, 19 Identification was performed using F-NMR.
[0182] (Synthesis Example 16) Synthesis of (4-isopropylphenyl)tolyliodonium tris(2-trifluoromethyl-2-propoxy)(nonafluoro-tert-butoxy)aluminate (AG-10) An acid generator (AG-10) was obtained in a yield of 76% in the same manner as in Synthesis Example 15, except that the aqueous solution of lithium salt (A-1) in Synthesis Example 15 was changed to an aqueous solution of lithium salt (A-13). 1 H, 19 Identification was performed using F-NMR.
[0183] (Synthesis Example 17) Synthesis of phenyl(2,4,6-trimethoxyphenyl)iodonium tetrakis(hexafluoro-tert-butoxy)aluminate (AG-11) A reaction vessel was charged with 5.4 g of phenyl(2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate and 50 g of dichloromethane. 50 parts of an aqueous solution containing an equimolar amount of lithium salt (A-4) was added while stirring, and the mixture was stirred at room temperature for 8 hours. After standing, the aqueous layer was removed by separation, and the organic layer was washed five times with 50 parts of water. The organic solvent was distilled off under reduced pressure to obtain an acid generator (AG-11) in a yield of 83%. The product was 1 H, 19 Identification was performed using F-NMR.
[0184] (Synthesis Example 18) Synthesis of phenyl(2,4,6-trimethoxyphenyl)iodonium tetrakis(2-pentafluoroethyl-2-propoxy)aluminate (AG-12) An acid generator (AG-12) was obtained in a yield of 87% in the same manner as in Synthesis Example 17, except that the aqueous solution of lithium salt (A-4) in Synthesis Example 17 was changed to an aqueous solution of lithium salt (A-2). 1 H, 19 Identification was performed using F-NMR.
[0185] (Comparative Synthesis Example 3) Synthesis of [4-(phenylthio)phenyl]sulfonium tetrakis(perfluoro-tert-pentoxy)aluminate (AG-H1) An acid generator (AG-H1) was obtained in a yield of 85% in the same manner as in Synthesis Example 9, except that the aqueous solution of lithium salt (A-10) in Synthesis Example 9 was changed to an aqueous solution of lithium salt (A-21). 1 H, 19 Identification was performed using F-NMR.
[0186] (Comparative Synthesis Example 4) Synthesis of [4-(phenylthio)phenyl]sulfonium tetrakis(octafluoro-tert-pentoxy)aluminate (AG-H2) An acid generator (AG-H2) was obtained in a yield of 82% in the same manner as in Synthesis Example 9, except that the aqueous solution of lithium salt (A-10) in Synthesis Example 9 was changed to an aqueous solution of lithium salt (A-24). 1 H, 19 Identification was performed using F-NMR.
[0187] (Comparative Synthesis Example 5) Synthesis of di(4-tert-butylphenyl)iodonium tetrakis(perfluoro-tert-pentoxy)aluminate (AG-H3) An acid generator (AG-H3) was obtained in a yield of 78% in the same manner as in Synthesis Example 13, except that the aqueous solution of lithium salt (A-7) in Synthesis Example 13 was changed to an aqueous solution of lithium salt (A-21). 1 H, 19 Identification was performed using F-NMR.
[0188] Comparative Synthesis Example 6: Synthesis of di(4-tert-butylphenyl)iodonium tetrakis(octafluoro-tert-pentoxy)aluminate (AG-H4) An acid generator (AG-H4) was obtained in a yield of 82% in the same manner as in Synthesis Example 13, except that the aqueous solution of lithium salt (A-7) in Synthesis Example 13 was changed to an aqueous solution of lithium salt (A-24). 1 H, 19 Identification was performed using F-NMR.
[0189] <Synthesis of thermal acid generator> (Synthesis Example 19) Synthesis of 4-hydroxyphenyl-methyl-benzylsulfonium tetrakis(2-trifluoromethyl-2-propoxy)aluminate (AG-13) 3.0 g of 4-hydroxyphenyl-methyl-benzylsulfonium chloride was dispersed in 50 g of dichloromethane, and 30 g of an aqueous solution containing an equimolar amount of lithium salt (A-1) was mixed at room temperature and stirred for 3 hours. The dichloromethane layer was washed five times with water by a separation operation, and then transferred to a rotary evaporator to distill off the solvent, yielding an acid generator (AG-13) in 89% yield. The product was 1 H, 19 Identification was performed using F-NMR.
[0190] (Synthesis Example 20) Synthesis of 4-hydroxyphenyl-methyl-benzylsulfonium tetrakis(hexafluoro-tert-butoxy)aluminate (AG-14) An acid generator (AG-14) was obtained in a yield of 81% in the same manner as in Synthesis Example 19, except that the aqueous solution of lithium salt (A-1) in Synthesis Example 19 was changed to an aqueous solution of lithium salt (A-4). 1 H, 19 Identification was performed using F-NMR.
[0191] (Synthesis Example 21) Synthesis of 4-hydroxyphenyl-methyl-benzylsulfonium tris(2-trifluoromethyl-2-propoxy)(nonafluoro-tert-butoxy)aluminate (AG-15) An acid generator (AG-15) was obtained in a yield of 71% in the same manner as in Synthesis Example 19, except that the aqueous solution of lithium salt (A-1) in Synthesis Example 19 was changed to an aqueous solution of lithium salt (A-13). 1 H, 19 Identification was performed using F-NMR.
[0192] (Synthesis Example 22) Synthesis of 4-hydroxyphenyl-methyl-1-naphthylmethylsulfonium tetrakis(2-pentafluoroethyl-2-propoxy)aluminate (AG-16) 3.2 g of 4-hydroxyphenyl-methyl-1-naphthylmethylsulfonium chloride was dispersed in 50 g of dichloromethane, and 30 g of an aqueous solution containing an equimolar amount of lithium salt (A-2) was mixed at room temperature and stirred for 3 hours. The dichloromethane layer was washed five times with water by a separation operation, and then transferred to a rotary evaporator to distill off the solvent, yielding an acid generator (AG-16) in 87% yield. The product was 1 H, 19 Identification was performed using F-NMR.
[0193] (Synthesis Example 23) Synthesis of 4-hydroxyphenyl-methyl-benzylsulfonium tetrakis(2-phenyl-hexafluoro-2-propoxy)aluminate (AG-17) An acid generator (AG-17) was obtained in a yield of 77% in the same manner as in Synthesis Example 23, except that in Synthesis Example 22, the aqueous solution of lithium salt (A-2) was changed to an aqueous solution of lithium salt (A-7). 1 H, 19 Identification was performed using F-NMR.
[0194] (Synthesis Example 24) Synthesis of 4-hydroxyphenyl-methyl-benzylsulfonium tetrakis(2-p-chlorophenyl-hexafluoro-2-propoxy)aluminate (AG-18) An acid generator (AG-18) was obtained in a yield of 75% in the same manner as in Synthesis Example 23, except that in Synthesis Example 22, the aqueous solution of lithium salt (A-2) was changed to an aqueous solution of lithium salt (A-10). 1 H, 19 Identification was performed using F-NMR.
[0195] (Comparative Synthesis Example 7) Synthesis of 4-hydroxyphenyl-methyl-benzylsulfonium tetrakis(perfluoro-tert-pentoxy)aluminate (AG-H5) An acid generator (AG-H5) was obtained in a yield of 83% in the same manner as in Synthesis Example 19, except that the aqueous solution of lithium salt (A-1) in Synthesis Example 19 was changed to an aqueous solution of lithium salt (A-21). 1 H, 19 Identification was performed using F-NMR.
[0196] (Comparative Synthesis Example 8) Synthesis of 4-hydroxyphenyl-methyl-benzylsulfonium tetrakis(octafluoro-tert-pentoxy)aluminate (AG-H6) An acid generator (AG-H6) was obtained in a yield of 80% in the same manner as in Synthesis Example 19, except that the aqueous solution of lithium salt (A-1) in Synthesis Example 19 was changed to an aqueous solution of lithium salt (A-24). 1 H, 19 Identification was performed using F-NMR.
[0197] <Evaluation of photocurable compositions for adhesives> The components shown in Table 1 below were mixed according to the composition (unit: parts by weight) and stirred and mixed at room temperature using a planetary centrifugal mixer to obtain uniform and transparent photocurable compositions for adhesives (hereinafter referred to as adhesives) (Examples 1 to 20, Comparative Examples 1 to 8). The obtained adhesives were evaluated according to the following evaluation methods.
[0198] [Curability] A 0.04 mm spacer was placed on both ends of a glass slide, and the adhesive was dropped in the center. The adhesive was spread using a squeegee to a thickness of 0.04 mm, and light irradiation was performed using a high-pressure mercury lamp under the following conditions. After light irradiation, the sample was left at room temperature for 60 minutes to obtain a cured product. The tackiness of the surface of the obtained cured product was judged by touch, and the curability was evaluated according to the following criteria. Evaluation criteria ○: The surface was not tacky, and the surface shape of the cured product did not change when palpated. △: No tackiness on the surface, but the surface shape of the cured product changed when palpated. ×: The surface had tackiness. <High pressure mercury lamp> Irradiation device: Belt conveyor type UV irradiation device (manufactured by iGraphics Co., Ltd.) Lamp: 1.0kW high pressure mercury lamp Filter: L-34 (Kenko Optical Co., Ltd.) Irradiation intensity (measured with a 365 nm illuminometer): 100 mW / cm 2 Accumulative irradiation dose: 1000mJ / cm 2
[0199] [Adhesiveness] A 0.04 mm spacer was placed on both ends of the slide glass, and the adhesive was dropped in the center. A squeegee was used to spread the adhesive to a thickness of 0.03 mm, and an epoxy resin cube (outer diameter: 4 mm x 4 mm x 1 mm, inner diameter: 3.7 mm x 3.7 mm x 0.8 mm, adhesive area: 2.3 mm) was placed on top of it. 2 ) was set and light irradiation was carried out in the same manner as above. After the light irradiation, the samples were left at room temperature for 60 minutes or more, and the adhesiveness was evaluated from the load (kgf) at which the epoxy resin cube peeled off using a die shear tester (product name "4000PXY", manufactured by DAGE) under the following conditions. Five samples were prepared, and the average value was used for evaluation. The higher the load, the better the adhesiveness. Adhesion measurement conditions Shear height: 0.65mm Shear speed: 500μm / s
[0200] [Heat-resistant adhesion] The same samples as those used in the [Adhesion] evaluation above were subjected to a heat resistance test three times in a row using a tabletop reflow oven (manufactured by Synapec) based on the reflow temperature profile (maximum temperature: 270°C) specified in the JEDEC standard, and then the adhesion was evaluated using the same method as above (number of samples: 5). The smaller the change before and after the heat resistance test, the better the thermal stability.
[0201] [Transparency] A Teflon (registered trademark) spacer measuring 20 mm in length, 20 mm in width, and 0.1 mm in thickness was prepared and sandwiched between slide glasses (product name "S2111", manufactured by Matsunami Glass Co., Ltd.). The curable composition was poured into the gap, irradiated with light in the same manner as above, and left at room temperature for 60 minutes after irradiation to obtain a cured product. The transparency (YI) of the obtained cured product was evaluated by measuring it using a spectrophotometer (product name "U-3900", manufactured by Hitachi High-Technologies Corporation). The yellowness index (YI) was read as a value in a 2-degree visual field under a D65 light source.
[0202] [Heat-resistant transparency] The cured product obtained in the same manner as in the above [Transparency] evaluation was subjected to a heat resistance test three times in succession using a tabletop reflow oven (manufactured by Synapec) based on the reflow temperature profile (maximum temperature: 270°C) specified in the JEDEC standard, and the transparency (YI) was then measured in the same manner as above to evaluate the heat resistance and transparency.
[0203] The above evaluation results are shown in Table 1. As can be seen from Table 1, the photocurable composition for adhesives of the present invention is excellent in curability, adhesiveness, heat-resistant adhesiveness, and transparency of the cured product, particularly heat-resistant transparency.
[0204] [Table 1]
[0205] The compound names of the components in Table 1 are as follows. <Cationic polymerizable compound> CELLOXIDE 2021P: 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, manufactured by Daicel Corporation THI-DE: Diepoxidized tetrahydroindene, manufactured by JXTG Nippon Oil & Energy Corporation jER 828: Bisphenol A diglycidyl ether, manufactured by Mitsubishi Chemical Corporation jER YX8000: Hydrogenated bisphenol A diglycidyl ether, manufactured by Mitsubishi Chemical Corporation TECHMORE VG3101L: 2-[4-(2,3-epoxypropoxy)phenyl]-2-[4-[1,1-bis[4-(2,3-epoxypropoxy)phenyl]ethyl]phenyl]propane, manufactured by Printec Co., Ltd. SR-NPG: Neopentyl glycol diglycidyl ether, manufactured by Sakamoto Pharmaceutical Co., Ltd. OXT-121: Xylylene bisoxetane, manufactured by Toagosei Co., Ltd. OXT-221: 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, manufactured by Toagosei Co., Ltd. X-22-169: Epoxy-modified silicone oligomer with alicyclic ends, manufactured by Shin-Etsu Chemical Co., Ltd. Denacol EX-146: p-tert-butylphenyl glycidyl ether, manufactured by Nagase ChemteX Corporation <Photoacid generator> AG-1 to AG-12 and AG-H1 to H4: Compounds obtained in Synthesis Examples 7 to 18 and Comparative Synthesis Examples 3 to 6 <Coupling Agent> KBM-403: 3-glycidoxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. <Antifoaming agent> BYK-1790: BYK Japan <Leveling agent> LS-460: Polyether modified silicone, manufactured by Kusumoto Chemicals Co., Ltd.
[0206] <Evaluation of thermosetting compositions for adhesives> The components shown in Table 2 below were mixed according to the composition (unit: parts by weight) and stirred and mixed at room temperature using a planetary centrifugal mixer to obtain uniform and transparent thermosetting compositions for adhesives (hereinafter referred to as adhesives) (Examples 21 to 40, Comparative Examples 9 to 16). The obtained adhesives were evaluated according to the following evaluation methods.
[0207] [Thermosetting] A 0.03 mm spacer was placed on both ends of a slide glass (product name "S9112", manufactured by Matsunami Glass Industrial Co., Ltd.), and the curable composition was dropped in the center. The curable composition was spread using a squeegee to a thickness of 0.03 mm, and heated on a hot plate at 130°C for 10 minutes to obtain a cured product.
[0208] The curability of the resulting cured product was confirmed based on the presence or absence of tackiness on the surface, which was judged by palpation. Evaluation criteria ○: The surface was not tacky and the surface shape of the cured product did not change. △: There is no tackiness on the surface, but the surface shape of the cured product has changed. ×: The surface had tackiness.
[0209] [Adhesiveness] A 0.04 mm spacer was placed on both ends of the slide glass, and the adhesive was dropped in the center. A squeegee was used to spread the adhesive to a thickness of 0.03 mm, and an epoxy resin cube (outer diameter: 4 mm x 4 mm x 1 mm, inner diameter: 3.7 mm x 3.7 mm x 0.8 mm, adhesive area: 2.3 mm) was placed on top of it. 2 ) was set and heating was carried out in the same manner as above. After heating, the samples were left at room temperature for 60 minutes or more, and the adhesiveness was evaluated from the load (kgf) at which the epoxy resin cube peeled off using a die shear tester (product name "4000PXY", manufactured by DAGE) under the following conditions. Five samples were prepared, and the average value was used for evaluation. The higher the load, the better the adhesiveness. Adhesion measurement conditions Shear height: 0.65mm Shear speed: 500μm / s
[0210] [Heat-resistant adhesion] The same samples as those used in the [Adhesion] evaluation above were subjected to a heat resistance test three times in a row using a tabletop reflow oven (manufactured by Synapec) based on the reflow temperature profile (maximum temperature: 270°C) specified in the JEDEC standard, and then the adhesion was evaluated using the same method as above (number of samples: 5). The smaller the change before and after the heat resistance test, the better the thermal stability.
[0211] [Transparency] A Teflon (registered trademark) spacer measuring 20 mm in length, 20 mm in width, and 0.1 mm in thickness was prepared and sandwiched between slide glasses (product name "S2111", manufactured by Matsunami Glass Co., Ltd.). The curable composition was poured into the gap and heated in the same manner as above to obtain a cured product. The transparency (YI) of the obtained cured product was evaluated by measuring it using a spectrophotometer (product name "U-3900", manufactured by Hitachi High-Technologies Corporation). The yellowness index (YI) was read as a value in a 2-degree visual field under a D65 light source.
[0212] [Heat-resistant transparency] The cured product obtained in the same manner as in the above [Transparency] evaluation was subjected to a heat resistance test three times in succession using a tabletop reflow oven (manufactured by Synapec) based on the reflow temperature profile (maximum temperature: 270°C) specified in the JEDEC standard, and the transparency (YI) was then measured in the same manner as above to evaluate the heat resistance and transparency.
[0213] The evaluation results are shown in Table 2. As can be seen from Table 2, the thermosetting adhesive composition of the present invention is excellent in curability, adhesiveness, heat-resistant adhesiveness, and transparency of the cured product, particularly heat-resistant transparency.
[0214] [Table 2]
[0215] The compound names of the components in Table 2 are as follows. <Cationic polymerizable compound> CELLOXIDE 2021P: 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, manufactured by Daicel Corporation THI-DE: Diepoxidized tetrahydroindene, manufactured by JXTG Nippon Oil & Energy Corporation jER 828: Bisphenol A diglycidyl ether, manufactured by Mitsubishi Chemical Corporation jER YX8000: Hydrogenated bisphenol A diglycidyl ether, manufactured by Mitsubishi Chemical Corporation TECHMORE VG3101L: 2-[4-(2,3-epoxypropoxy)phenyl]-2-[4-[1,1-bis[4-(2,3-epoxypropoxy)phenyl]ethyl]phenyl]propane, manufactured by Printec Co., Ltd. SR-NPG: Neopentyl glycol diglycidyl ether, manufactured by Sakamoto Pharmaceutical Co., Ltd. OXT-121: Xylylene bisoxetane, manufactured by Toagosei Co., Ltd. OXT-221: 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, manufactured by Toagosei Co., Ltd. X-22-169: Epoxy-modified silicone oligomer with alicyclic ends, manufactured by Shin-Etsu Chemical Co., Ltd. Denacol EX-146: p-tert-butylphenyl glycidyl ether, manufactured by Nagase ChemteX Corporation <Thermal acid generator> AG-13 to AG-18 and AG-H5 to H6: Compounds obtained in Synthesis Examples 19 to 24 and Comparative Synthesis Examples 7 to 8 <Coupling Agent> KBM-403: 3-glycidoxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. <Antifoaming agent> BYK-1790: BYK Japan <Leveling agent> LS-460: Polyether modified silicone, manufactured by Kusumoto Chemicals Co., Ltd.
[0216] <Evaluation of photocurable compositions for optical materials> The components shown in Table 3 below were mixed according to the composition (unit: parts by weight) and stirred and mixed at room temperature using a planetary centrifugal mixer to obtain uniform and transparent photocurable compositions for optical materials (Examples 41 to 63, Comparative Examples 17 to 24). The obtained curable compositions were evaluated according to the following evaluation methods.
[0217] [Curability] A 0.03 mm spacer was placed on both ends of a slide glass, and the photocurable composition for optical materials was dropped in the center. The curable composition was spread using a squeegee to a thickness of 0.03 mm, and light irradiation was performed using a high-pressure mercury lamp under the following conditions. After light irradiation, the material was left at room temperature for 60 minutes to obtain a cured product. The tackiness of the surface of the obtained cured product was judged by touch, and the curability was evaluated according to the following criteria. Evaluation criteria ○: The surface was not tacky, and the surface shape of the cured product did not change when palpated. △: No tackiness on the surface, but the surface shape of the cured product changed when palpated. ×: The surface had tackiness. <High pressure mercury lamp> Irradiation device: Belt conveyor type UV irradiation device (manufactured by iGraphics Co., Ltd.) Lamp: 1.0kW high pressure mercury lamp Filter: L-34 (Kenko Optical Co., Ltd.) Irradiation intensity (measured with a 365 nm illuminometer): 100 mW / cm 2 Accumulative irradiation dose: 1000mJ / cm 2
[0218] [Transparency] A Teflon (registered trademark) spacer measuring 20 mm long x 20 mm wide x 0.3 mm thick was prepared and sandwiched between glass slides. The curable composition was poured into the gap, irradiated with light in the same manner as above, and left at room temperature for 60 minutes after irradiation to obtain a cured product. The yellowness index (YI) of the obtained cured product was measured using a spectrophotometer (product name "U-3900", manufactured by Hitachi High-Technologies Corporation) to evaluate transparency. The yellowness index (YI) was read as a value in a 2-degree visual field under a D65 light source. The smaller the value, the higher and better the transparency.
[0219] [Heat-resistant transparency] The cured product obtained in the same manner as in the above [Transparency] evaluation was subjected to a heat resistance test three times in succession using a tabletop reflow oven (manufactured by Synapec) based on the reflow temperature profile (maximum temperature: 270°C) specified in the JEDEC standard, and the transparency (YI) was then measured in the same manner as above to evaluate the heat resistance and transparency.
[0220] The evaluation results are shown in Table 3. As can be seen from Table 3, the photocurable composition for optical materials of the present invention is excellent in curability and transparency, in particular in heat-resistant transparency.
[0221] [Table 3]
[0222] The compound names of the components in Table 3 are as follows. <Cationic polymerizable compound> CELLOXIDE 2021P: 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, manufactured by Daicel Corporation EHPE3150: 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, manufactured by Daicel Corporation EP-4088S: Dicyclopentadiene type epoxy resin, manufactured by ADEKA Corporation jER 828: Bisphenol A diglycidyl ether, manufactured by Mitsubishi Chemical Corporation OGSOL EG-200: bifunctional epoxy resin containing fluorene structure, manufactured by Osaka Gas Chemicals Co., Ltd. TEPIC-VL: Triglycidyl isocyanurate, manufactured by Nissan Chemical Industries, Ltd. X-40-2670: Alicyclic epoxy modified silicone oligomer, manufactured by Shin-Etsu Chemical Co., Ltd. OXT-101: 3-ethyl-3-hydroxymethyloxetane, manufactured by Toagosei Co., Ltd. OXT-221: 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, manufactured by Toagosei Co., Ltd. <Photoacid generator> AG-1 to AG-12 and AG-H1 to H4: Compounds obtained in Synthesis Examples 7 to 18 and Comparative Synthesis Examples 3 to 6 <Leveling agent> BYK-UV3510: BYK Japan <Antioxidants> Irganox 1010: (Pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], manufactured by BASF
[0223] <Evaluation of thermosetting compositions for optical materials> The components shown in Table 4 below were mixed according to the composition (unit: parts by weight) and stirred and mixed at room temperature using a planetary centrifugal mixer to obtain uniform and transparent thermosetting compositions for optical materials (Examples 64 to 86, Comparative Examples 25 to 28). The obtained curable compositions were evaluated according to the following evaluation methods.
[0224] [Curability] A 0.03 mm spacer was placed on both ends of a slide glass (product name "S9112", manufactured by Matsunami Glass Industrial Co., Ltd.), and the thermosetting composition for optical materials was dropped in the center. The curable composition was spread using a squeegee to a thickness of 0.03 mm, and heated on a hot plate at 130°C for 10 minutes to obtain a cured product. The curability of the resulting cured product was confirmed based on the presence or absence of tackiness on the surface, which was judged by palpation. Evaluation criteria ○: The surface was not tacky and the surface shape of the cured product did not change. △: There is no tackiness on the surface, but the surface shape of the cured product has changed. ×: The surface had tackiness.
[0225] [Transparency] A Teflon (registered trademark) spacer measuring 20 mm long x 20 mm wide x 0.3 mm thick was prepared and sandwiched between glass slides. The curable composition was poured into the gap and heated in the same manner as above to obtain a cured product. The transparency (YI) of the obtained cured product was measured using a spectrophotometer (product name "U-3900", manufactured by Hitachi High-Technologies Corporation) to evaluate the transparency. The yellowness index (YI) was read as a value in a 2-degree visual field under a D65 light source. The smaller the value, the higher and better the transparency.
[0226] [Heat-resistant transparency] The cured product obtained in the same manner as in the above [Transparency] evaluation was subjected to a heat resistance test three times in succession using a tabletop reflow oven (manufactured by Synapec) based on the reflow temperature profile (maximum temperature: 270°C) specified in the JEDEC standard, and the transparency (YI) was then measured in the same manner as above to evaluate the heat resistance and transparency.
[0227] The evaluation results are shown in Table 4. As can be seen from Table 4, the thermosetting composition for optical materials of the present invention is excellent in curability and transparency, in particular in heat-resistant transparency.
[0228] [Table 4]
[0229] The compound names of the components in Table 4 are as follows. <Cationic polymerizable compound> CELLOXIDE 2021P: 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, manufactured by Daicel Corporation EHPE3150: 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, manufactured by Daicel Corporation EP-4088S: Dicyclopentadiene type epoxy resin, manufactured by ADEKA Corporation jER 828: Bisphenol A diglycidyl ether, manufactured by Mitsubishi Chemical Corporation OGSOL EG-200: bifunctional epoxy resin containing fluorene structure, manufactured by Osaka Gas Chemicals Co., Ltd. TEPIC-VL: Triglycidyl isocyanurate, manufactured by Nissan Chemical Industries, Ltd. X-40-2670: Alicyclic epoxy modified silicone oligomer, manufactured by Shin-Etsu Chemical Co., Ltd. OXT-101: 3-ethyl-3-hydroxymethyloxetane, manufactured by Toagosei Co., Ltd. OXT-221: 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, manufactured by Toagosei Co., Ltd. <Thermal acid generator> AG-13 to AG-18 and AG-H5 to H6: Compounds obtained in Synthesis Examples 19 to 24 and Comparative Synthesis Examples 7 to 8 <Leveling agent> BYK-UV3510: BYK Japan <Antioxidants> Irganox 1010: (Pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], manufactured by BASF
[0230] <Evaluation of curable compositions for photolithography> The components shown in Table 5 below were mixed according to the composition (unit: parts by weight) to obtain curable compositions for optical 3D modeling (Examples 87 to 110, Comparative Examples 29 to 36). The obtained curable compositions were evaluated according to the following evaluation methods.
[0231] [Curing evaluation] The curable composition for optical 3D modeling was applied to a glass plate to a film thickness of 20 μm, and irradiated with light using a high pressure mercury lamp under the following conditions. After irradiation, the material was left at room temperature for 60 minutes to obtain a cured product. The tackiness of the surface of the obtained cured product was judged by touch, and the curability was evaluated according to the following criteria. Evaluation criteria ○: The surface was not tacky, and the surface shape of the cured product did not change when palpated. △: No tackiness on the surface, but the surface shape of the cured product changed when palpated. ×: The surface had tackiness. <High pressure mercury lamp> Irradiation device: Belt conveyor type UV irradiation device (manufactured by iGraphics Co., Ltd.) Lamp: 1.0kW high pressure mercury lamp Filter: L-34 (Kenko Optical Co., Ltd.) Irradiation intensity (measured with a 365 nm illuminometer): 100 mW / cm 2 Accumulative irradiation dose: 600mJ / cm 2
[0232] [Dimensional stability evaluation] The curable compositions for optical 3D modeling obtained in the Examples and Comparative Examples were applied to a 100 μm thick PET film, and cured products were obtained by irradiating the films with ultraviolet light using a high-pressure mercury lamp as a light source in an air atmosphere. A test piece (length x width = 2 cm x 10 cm) was prepared from the obtained cured product, one side of the test piece (one of the 2 cm sides) was fixed to the surface of the substrate with tape, and the dimensional stability was evaluated based on the degree of warping of the other side (the other of the 2 cm sides) according to the following criteria. The smaller the warping, the better the dimensional stability. Evaluation criteria ◎: Warpage is less than 4mm ○: Warpage is 4mm or more and less than 7mm △: Warpage is 7mm or more and less than 10mm ×: Warpage is 10mm or more
[0233] [Light resistance] The stereolithography model created in the above [Dimensional stability evaluation] was used to measure the amount of ultraviolet light equivalent to one year (308 MJ / m 2 The color (yellowing) was evaluated visually. The evaluation criteria were as follows: (Evaluation Criteria) ◎: Colorless (no yellowing) ○:Pale yellow to yellow ×: Brown
[0234] [Heat yellowing resistance] The stereolithography produced in the above [Evaluation of dimensional stability] was heated for 2 hours on a hot plate controlled at 200°C, and the hue (yellowing) was visually evaluated. The evaluation criteria were as follows: (Evaluation Criteria) ◎: Colorless (no yellowing) ○:Pale yellow to yellow ×: Brown
[0235] The evaluation results are shown in Table 5. As can be seen from Table 5, the curable composition for optical 3D modeling of the present invention has excellent photocurability, and by performing optical modeling using the resin composition for optical 3D modeling of the present invention, it is possible to obtain a 3D object that has a small shrinkage rate during curing, excellent dimensional accuracy, excellent light resistance, excellent heat resistance, and further has low yellowness and excellent color tone and transparency.
[0236] [Table 5]
[0237] The compound names of each component in Table 5 are as follows. <Cationic polymerizable compound> CELLOXIDE 2021P: 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, manufactured by Daicel Corporation EHPE3150: 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, manufactured by Daicel Corporation jER 828: Bisphenol A diglycidyl ether, manufactured by Mitsubishi Chemical Corporation Rikaresin HBE-100: Hydrogenated bisphenol A type epoxy resin, manufactured by New Japan Chemical Co., Ltd. jER 157S70: Novolac type solid epoxy resin, manufactured by Mitsubishi Chemical Corporation OGSOL PG-100: Fluorene skeleton-containing epoxy resin, manufactured by Osaka Gas Chemicals Co., Ltd. TECHMORE VG3101L: 2-[4-(2,3-epoxypropoxy)phenyl]-2-[4-[1,1-bis[4-(2,3-epoxypropoxy)phenyl]ethyl]phenyl]propane, manufactured by Printec Co., Ltd. Epogosey PT: Polytetramethylene glycol diglycidyl ether, manufactured by Yokkaichi Chemical Co., Ltd. X-22-163: Side-chain epoxy-modified silicone, manufactured by Shin-Etsu Chemical Co., Ltd. 4CH-DVE: Cyclohexanediol divinyl ether, manufactured by Daicel Corporation OXT-101: 3-ethyl-3-hydroxymethyloxetane, manufactured by Toagosei Co., Ltd. OXT-221: 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, manufactured by Toagosei Co., Ltd. <Radical curing compound> A-9950W: Dipentaerythritol polyacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd. AP-150: Polypropylene glycol monoacrylate, manufactured by Nippon Oil & Fats Co., Ltd. <Photoacid generator> AG-1 to AG-12 and AG-H1 to H4: Compounds obtained in Synthesis Examples 7 to 18 and Comparative Synthesis Examples 3 to 6 <Radical generator> Irgacure 184: 1-hydroxycyclohexyl phenyl ketone, manufactured by BASF <Aromatic thiol compounds> 2-Naphthalenethiol, manufactured by Tokyo Chemical Industry Co., Ltd.
[0238] <Evaluation of Resin Composition for Optical Waveguide> First, prior to the production of the optical waveguides of the Examples and Comparative Examples, photosensitive varnishes (resin compositions for optical waveguides; Examples 111 to 135, Comparative Examples 37 to 44) serving as materials for forming the cladding layer and the core layer were prepared. [Preparation of materials for forming clad layer and core layer] Under light-shielded conditions, the components shown in Table 6 below were mixed in the proportions shown in the same table, and completely dissolved at 110°C. After that, it was cooled to room temperature (25°C) and filtered under heat and pressure using a membrane filter with a diameter of 1.0 μm to produce a photosensitive varnish. In this way, an undercladding layer of a specific pattern was formed on the back surface of the FPC substrate [a laminate of SUS (stainless steel) and polyimide], a core layer of a specific pattern was formed on this undercladding layer, and an overcladding layer was further formed on this core layer to produce an optical waveguide (total optical waveguide thickness 75 μm).
[0239] [Preparation of resin layer for evaluation] A photosensitive varnish was applied onto a silicon wafer using a spin coater, and then the organic solvent was dried on a hot plate (130°C x 10 minutes) to form an uncured layer in an uncured film state. The uncured layer was irradiated with 200 mJ / cm2 UV light using a UV irradiator (ultra-high pressure mercury lamp, full beam (without bandpass filter)). 2 The film was exposed to a glass mask pattern (pattern width / pattern spacing (L / S) = 50 μm / 200 μm) with a wavelength of 365 nm (integrated), and then post-baked (140°C x 10 minutes).Then, the film was developed in γ-butyrolactone (room temperature 25°C, 3 minutes), washed with water, and dried on a hot plate (120°C x 5 minutes) to produce a resin layer (thickness 50 μm) with a specified pattern. Using each of the resin layers thus obtained, the pattern curing property, heat coloring resistance, and heat stability of each layer were measured and evaluated according to the methods described below. The results are shown in Table 6 below.
[0240] [Pattern hardening] The appearance of the pattern obtained under the above-mentioned conditions for producing each layer was observed under a microscope, and the results were evaluated based on the following criteria. ○: A rectangular pattern was created. △: Some areas where the pattern was not formed were observed. ×: No pattern was formed, and a functional problem occurred.
[0241] [Heat-resistant coloration] After drying by heating (130°C x 10 minutes) using a spin coater, a photosensitive varnish was applied so that a coating film with a thickness of 50 μm was formed, forming an uncured layer. The uncured layer thus formed was irradiated with 1000 mJ / cm2 using a UV irradiator [ultra-high pressure mercury lamp, total light (no bandpass filter)]. 2 The film was exposed to light (integrated wavelength 365 nm) and then post-baked (140°C x 10 minutes). The formed cured resin film was placed in a 125°C oven for 500 hours, and the change in transmittance at a wavelength of 400 nm before and after placing in the oven was measured using a spectrophotometer. The results were evaluated according to the following criteria. ○: The 400 nm transmittance after being placed in a 125℃ oven is 90% or more of the transmittance before being placed in the oven △: The 400 nm transmittance after being placed in a 125°C oven is 70% or more but less than 90% of the transmittance before being placed in the oven. ×: The 400 nm transmittance after being placed in a 125°C oven is less than 70% of the transmittance before being placed in the oven.
[0242] [Loss evaluation (material loss)] The above example was applied to a silicon substrate (thickness 500 μm) with an oxide film by spin coating. The photosensitive varnish obtained in the comparative example was applied to a thickness of about 5 to 10 μm. Then, after pre-baking on a hot plate (130°C x 5 minutes), it was irradiated with 5000mJ / cm using a UV irradiator [ultra-high pressure mercury lamp, full beam (no bandpass filter)]. 2A thin film was formed by exposure to light (integrated wavelength 365 nm) and post-heating (step heating at 80°C, 120°C, and 140°C for 5 minutes each). Next, light with a wavelength of 850 nm was incident on the thin film by prism coupling and propagated through the thin film. Then, the propagation length was changed and the light intensity at that length was measured using an optical measurement system (optical multi-power meter Q8221, manufactured by Advantest Corporation). The optical loss versus propagation length was plotted and linear approximation was performed. The material loss (dB) of each photosensitive varnish was calculated from the slope of the straight line and evaluated based on the following criteria (prism coupler method). ○: Material loss was less than 0.02 dB / cm. ×: The material loss was 0.02 dB / cm or more.
[0243] The evaluation results are shown in Table 6. As can be seen from Table 6, the resin composition for optical waveguide of the present invention is excellent in pattern curing property and heat resistant coloring stability, and is therefore useful in forming a component part of an optical waveguide.
[0244] [Table 6]
[0245] The compound names of each component in Table 6 are as follows. <Cationic polymerizable compound> EHPE3150: 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, manufactured by Daicel Corporation jER 157S70: Novolac type solid epoxy resin, manufactured by Mitsubishi Chemical Corporation TECHMORE VG3101L: 2-[4-(2,3-epoxypropoxy)phenyl]-2-[4-[1,1-bis[4-(2,3-epoxypropoxy)phenyl]ethyl]phenyl]propane, manufactured by Printec Co., Ltd. CELLOXIDE 2021P: 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, manufactured by Daicel Corporation jER 828: Bisphenol A diglycidyl ether, manufactured by Mitsubishi Chemical Corporation OGSOL PG-100: Fluorene skeleton-containing epoxy resin, manufactured by Osaka Gas Chemicals Co., Ltd. Epogosey PT: Polytetramethylene glycol diglycidyl ether, manufactured by Yokkaichi Chemical Co., Ltd. OXT-221: 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, manufactured by Toagosei Co., Ltd. <Photoacid generator> AG-1 to AG-12 and AG-H1 to H4: Compounds obtained in Synthesis Examples 7 to 18 and Comparative Synthesis Examples 3 to 6 <Antioxidants> Irganox 1010: (Pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], manufactured by BASF HCA: 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide [Industrial Applicability]
[0246] The curable composition of the present invention can be used in a wide variety of applications, including paints, coating agents, various coating materials (hard coats, stain-resistant coating materials, anti-fogging coating materials, contact-resistant coating materials, optical fibers, etc.), back-treatment agents for adhesive tapes, release coating materials for release sheets for adhesive labels (release paper, release plastic film, release metal foil, etc.), printing plates, dental materials (dental compounds, dental composites) inks, inkjet inks, positive resists (for forming connection terminals and wiring patterns in the manufacture of electronic parts such as circuit boards, CSPs, and MEMS elements), resist films, liquid resists, resists for MEMS, positive photosensitive materials, negative photosensitive materials, various adhesives ( It is preferably used as a photoacid generator in temporary fixing agents for various electronic components, adhesives for HDDs, adhesives for pickup lenses, adhesives for functional films for FPDs (deflectors, anti-reflection films, etc.), resins for holographs, FPD materials (color filters, black matrices, partition materials, photospacers, ribs, alignment films for liquid crystals, sealants for FPDs, etc.), optical members, molding materials (for building materials, optical parts, lenses), casting materials, putties, glass fiber impregnating agents, filling materials, sealing materials, encapsulants, optical semiconductor (LED) encapsulants, optical waveguide materials, nanoimprint materials, materials for photolithography, and materials for microphotolithography.
Claims
1. An adhesive comprising a curable composition containing an acid generator containing an onium salt represented by the following general formula (1) and a cationic polymerizable compound: [Formula 1] [In the formula, R 1 ~R 3 are each independently an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, or a phenyl group which may have a substituent; R 1 ~R 3 A part or all of the hydrogen atoms bonded to at least one of the groups R 1 ~R 3 30% to 70% of all hydrogen atoms bonded to the group are substituted with fluorine atoms; E represents an element having a valence n selected from S, I, N, or P, n being an integer of 1 to 3; R 4 is an organic group bonded to E, R 4 The number of R is n+1, and (n+1) R 4 may be the same or different, and two or more R 4 are each directly or -O-, -S-, -SO-, -SO 2 A ring structure containing the element E may be formed via -, -NH-, -CO-, -COO-, -CONH-, an alkylene group or a phenylene group.
2. 2. The adhesive according to claim 1, wherein E in the onium salt represented by the general formula (1) is S or I.
3. An optical element comprising, as a component, a cured product obtained by curing a curable composition containing an acid generator containing an onium salt represented by the following general formula (1) and a cationic polymerizable compound: [chemical 2] [In the formula, R 1 to R 3 are each independently an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, or a phenyl group which may have a substituent, some or all of the hydrogen atoms bonded to at least one of the groups R 1 to R 3 are substituted with fluorine atoms, and 30% to 70% of all the hydrogen atoms bonded to the groups R 1 to R 3 are substituted with fluorine atoms; E represents an element having a valence n selected from S, I, N, or P, n is an integer of 1 to 3, R 4 is an organic group bonded to E, the number of R 4 is n+1, the (n+1) R 4 s may be the same or different, and two or more R 4 s may form a ring structure containing the element E directly or via -O-, -S-, -SO-, -SO 2 -, -NH-, -CO-, -COO-, -CONH-, an alkylene group, or a phenylene group.]
4. An optical device comprising the optical element according to claim 3 .
5. A resin composition for optical three-dimensional modeling, comprising a curable composition containing an acid generator containing an onium salt represented by the following general formula (1) and a cationic polymerizable compound, and further containing a radical polymerizable compound and a radical polymerization initiator. [C3] [In the formula, R 1 to R 3 are each independently an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, or a phenyl group which may have a substituent, some or all of the hydrogen atoms bonded to at least one of the groups R 1 to R 3 are substituted with fluorine atoms, and 30% to 70% of all the hydrogen atoms bonded to the groups R 1 to R 3 are substituted with fluorine atoms; E represents an element having a valence n selected from S, I, N, or P, n is an integer of 1 to 3, R 4 is an organic group bonded to E, the number of R 4 is n+1, the (n+1) R 4 s may be the same or different, and two or more R 4 s may form a ring structure containing the element E directly or via -O-, -S-, -SO-, -SO 2 -, -NH-, -CO-, -COO-, -CONH-, an alkylene group, or a phenylene group.]
6. A three-dimensional object optically produced using the resin composition for three-dimensional modeling according to claim 5.
7. A resin composition for optical waveguides, comprising a curable composition containing an acid generator containing an onium salt represented by the following general formula (1) and a cationic polymerizable compound: [C4] [In the formula, R 1 to R 3 are each independently an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, or a phenyl group which may have a substituent, some or all of the hydrogen atoms bonded to at least one of the groups R 1 to R 3 are substituted with fluorine atoms, and 30% to 70% of all the hydrogen atoms bonded to the groups R 1 to R 3 are substituted with fluorine atoms; E represents an element having a valence n selected from S, I, N, or P, n is an integer of 1 to 3, R 4 is an organic group bonded to E, the number of R 4 is n+1, the (n+1) R 4 s may be the same or different, and two or more R 4 s may form a ring structure containing the element E directly or via -O-, -S-, -SO-, -SO 2 -, -NH-, -CO-, -COO-, -CONH-, an alkylene group, or a phenylene group.]
8. 8. The resin composition for optical waveguide according to claim 7, which is a material for forming a core layer in an optical waveguide comprising a substrate, a clad layer formed on the substrate, and a core layer for propagating an optical signal formed in a predetermined pattern in the clad layer.
9. A curable film for forming an optical waveguide core layer, which is obtained by forming the resin composition for an optical waveguide according to claim 7 into a film shape.
10. 8. An optical waveguide comprising a substrate, a clad layer formed on the substrate, and a core layer for propagating an optical signal formed in a predetermined pattern in the clad layer, wherein the core layer is formed by curing the resin composition for optical waveguides according to claim 7.
11. 10. An optical waveguide comprising a substrate, a clad layer formed on the substrate, and a core layer for propagating an optical signal formed in a predetermined pattern in the clad layer, wherein the core layer is formed by curing the curable film for forming an optical waveguide core layer according to claim 9.
12. 12. A flexible printed wiring board for optical and electrical transmission comprising the optical waveguide according to claim 10.
Citation Information
Patent Citations
Panel positioning apparatus
JP1977014277A
Panel assemly process
JP1977014278A
Tape carrier
JP1978013873A
New onium salt, photopolymerization initiator, energy ray-curable composition containing the same, and cured product of the composition
JP1998287643A
Sulfonium compound
JP2006096742A