Process for producing agglomerated lignin and uses thereof
The lignin compaction, grinding, and sieving process addresses the risk of dust explosions by producing agglomerated lignin with controlled particle size, ensuring safe handling and storage.
Patent Information
- Application Number
- JP2021555190
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-14
- Filing Date
- 2020-03-11
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-03-11
Smart Images

Figure 0007572370000001 
Figure 0007572370000002 
Figure 0007572370000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for producing agglomerated lignin having a controlled particle size distribution, which is essentially dust-free, thereby greatly reducing the risk of dust explosions. [Background technology]
[0002] Lignin, an aromatic polymer, is the main component present in, for example, wood and is the second most abundant source of carbon on Earth after cellulose. In recent years, the development and commercialization of techniques to extract lignin in a highly refined, solid, powdered form from the pulp manufacturing process has attracted considerable attention as a potential renewable replacement for the major aromatic chemical precursors currently supplied by the petrochemical industry.
[0003] Lignin has been widely investigated as a suitable replacement for phenol during the manufacture of phenol-formaldehyde binders for the production of panel boards such as plywood, hardboard, medium density fiberboard, or particleboard.
[0004] It is preferable to utilize lignin products with minimal moisture content so as not to introduce unnecessary additional water into the process. However, handling lignin with a minimum moisture content of 0-5% (by weight) presents several significant problems. Among them is that lignin during handling of any kind will form dust clouds. These dust clouds can further cause dust explosions if a sufficiently high concentration of flammable material is airborne. Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, there is a need for a method of treating lignin in such a way that the risk of dust explosions can be significantly reduced.
[0006] Several attempts to apply roller compactor processing of lignin are known. RU2197389, RU2307033, US2010 / 0218420, and US2010 / 154296 disclose processes for producing briquettes in which lignin is a component of the final briquette composition. In the processes described therein, lignin is used as a liquid or solid binder that binds the various components together to produce the briquettes. The end use of these briquettes is in the field of energy generation. [Means for solving the problem]
[0007] Summary of the Invention The present invention provides a solution to one or more of the problems of the prior art. A particularly great advantage of the process according to the invention is that the fines forming the dust are reduced to such an extent that there is no risk of a dust explosion.
[0008] The present invention relates to the following: 1. A process for producing agglomerated lignin having a controlled particle size distribution, comprising: a) a lignin compression step, in which the lignin having a moisture content of 1% to 45% by weight is agglomerated by roll compression, the roll having cavities, and the depth of each cavity used in the roll compression being 0.1 mm to 10 mm; b) subjecting the compressed lignin obtained in step a) to grinding; followed by c) a sieving step in which the product of step b) is sieved to remove particles having a particle size less than 100 μm to produce a final agglomerated lignin with a controlled particle size distribution determined by the porosity of the sieving screen used in the sieving step, and less than 10% by weight of the particles retained after step c) have a particle size less than 100 μm. Agglomerated lignin production process.
[0009] The compaction according to the invention is preferably carried out without adding any additives to the material to be compacted. In the context of the present invention, additives are substances added to the process to improve the adhesion between the lignin particles. Additives therefore refer to substances which are added and which are not present in the lignin starting material of step a). Thus, in the context of the present invention, neither moisture such as water (moisture) nor other components already present in the lignin starting material of step a) are considered as additives.
[0010] The present invention also relates to the use of the agglomerated lignin with controlled particle size distribution obtained as product of step c), for example, the lignin may be utilized as an intermediate in chemical synthesis processes, such as the manufacture of binders. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Detailed Description Throughout the present specification, the expression "lignin" is intended to encompass any type of lignin, for example lignin derived from broadleaf (hardwood), coniferous (softwood) or annual plants. Preferably, the lignin is alkaline lignin, for example produced in the Kraft process. Preferably, the lignin is purified or isolated before being used in the process according to the invention. The lignin may be isolated from black liquor before being used in the process according to the invention and may optionally be further purified. The purification is typically carried out so that the purity of the lignin is at least 90%, preferably at least 95%. Thus, the lignin used according to the process of the invention preferably contains less than 10%, preferably less than 5% of impurities. The lignin may then be separated from the black liquor by using the process disclosed in WO2006 / 031175.
[0012] Preferably, the lignin is dried before compression, i.e. before step a) of the process according to the invention. Drying of the lignin is carried out by methods and devices known in the art. The lignin used in step a) has a moisture content of 1% to 45% by weight. Preferably, the moisture content of the lignin before compression according to the invention is less than 25% by weight, preferably less than 10% by weight, more preferably less than 8% by weight. The temperature during drying is preferably in the range of 80°C to 160°C, more preferably in the range of 100°C to 120°C.
[0013] The lignin powder obtained after drying has a wide particle size distribution ranging from 1 μm to 2 mm, with a strong inclination towards the micrometer range, meaning that the majority of the particles have a particle size ranging from 1 to 200 μm. It is known in the art that there is a strong correlation between explosion properties and particle size distribution, i.e. the smaller the particles, the more significant the explosion risk (see BIA-Report 13 / 97 Combustion and Explosion Properties of Dusts). Here, particles with a size below 100 μm are considered as fines.
[0014] Roll compaction of lignin can be accomplished by a roller compactor, which agglomerates the lignin particles. The present invention is a process that includes three steps: compaction, crushing, and sieving.
[0015] In the compression step a), a first intermediate product is produced. Here, fine lignin powder is usually fed through a hopper and conveyed by a horizontal or vertical feed screw to the compression zone, where the material is compressed into flake shape by compression rollers with a predetermined gap. By controlling the feed screw speed, the pressure generation in the compression zone, a uniform density of flakes can be obtained. The pressure generation in the compression zone can preferably be monitored and controlled by the rotation speed of the compression rolls. As the powder is dragged between the rollers, it enters what is called the nip zone, where the density of the material increases and the powder is converted into a flake or ribbon shape. The rolls used have cavities. The depth of each cavity used for roll compression is 0.1 mm to 10 mm, preferably 1 mm to 8 mm, more preferably 1 mm to 5 mm, or 1 mm to 3 mm. The specific pressing force applied during compression can vary depending on the equipment used for compression, but may range from 1 kN / cm to 100 kN / cm. Suitable devices for performing the compression are known in the art.
[0016] Preferably, the lignin used in step a) is provided in the form of a powder having a particle size distribution such that at least 25% by weight of the lignin has a particle size between 1 μm and 100 μm.
[0017] In the grinding step b) of the process, the first intermediate product obtained in the compaction step is subjected to milling or grinding, such as by means of a rotary granulator, a cage mill, a beater mill, a hammer mill or a crusher mill, and / or combinations thereof. During this step, a second intermediate product is obtained.
[0018] In the sieving step c) of the process, the second intermediate product obtained in the grinding step b) is screened by physical separation, such as sieving (also called screening), to obtain a final product, which is an agglomerated lignin with a well-defined particle size distribution set by the porosity of the sieve or screen. The sieve or screen is selected such that most particles with a size smaller than 100 μm pass through it and are rejected, preferably returned to the compression step, while most particles with a size larger than 100 μm are retained and become the product of the sieving step (product of the process according to the invention). The sieving can be carried out in several stages, i.e. the sieving can be carried out such that the ground material obtained in step b) passes through several screens or sieves in succession. By using two or more screening stages with different screen porosities, several fractions with a better defined particle size distribution are obtained.
[0019] In one embodiment, the rolls are configured such that the first roll has an annular rim and the powder in the nip region is sealed axially along the roller surface.
[0020] In one embodiment, the rolls are configured such that the nip region is sealed axially along the roller surface with a stationary plate, ensuring a sealed nip region minimizes powder loss at the axial ends of the rollers compared to generally cylindrical nip rollers.
[0021] It is particularly advantageous to carry out the compaction according to the invention with a material that is essentially lignin, i.e., in the absence of additives, since it facilitates use of the compacted product due to the absence of binders or other components that might otherwise adversely affect the application for which the compacted, crushed and sieved lignin is intended to be used.
[0022] A particular advantage of the process according to the invention is that the dust-forming fines are reduced to such an extent that there is no risk of dust explosion.
[0023] A further advantage of the process according to the invention is that the final agglomerated lignin can be easily handled, transported and stored.A further advantage of the process according to the invention is that it can be highly automated in a closed loop configuration, whereby rejects from the compaction step, the subsequent grinding step and the final screening step are returned to the roller compaction stage, maintaining a stable process flow and a uniform particle size distribution of the final product. EXAMPLES
[0024] Example 1 – Production and characterization of lignin feedstock Lignin powder dried in a ring dryer to a final dry content of 96% Wet lignin obtained from the final filter of a production plant operating according to the LignoBoost process was processed in a VetterTec ring dryer until a final dry content of 96% was reached. The dry content of the final material was obtained as described in ISO-638. The particle size distribution (PSD) was analyzed by sieving as described in the ASTM D1921-06 standard method. The bulk density of the product was obtained as described in ISO697. The explosive properties of the final material were obtained by measuring the minimum ignition energy (MIE) according to EN 13821.
[0025] The dry content and explosion properties obtained for the described products are shown in Table 1.
[0026] Example 2 (comparison) – Agglomeration of dry lignin by briquetting The lignin obtained in Example 1 was subjected to briquetting to produce briquettes. Briquetting was carried out using a roller press type 52 / 6.5 (Maschinenfabrik Koppern GmbH) equipped with compression rolls of 130 mm working width. The compression rolls were equipped with briquetting dies of dimensions approximately 30 x 20 x 20 mm (length x width x depth) uniformly distributed around the circumference of the compression roll. No sealing was used in the nip area between the compression rolls.
[0027] It was found that the fine powder would simply flow through the static gap between the two rollers and therefore no agglomeration of the lignin material could be achieved.
[0028] Example 3 (comparative) - Agglomeration of wet lignin by briquetting The lignin obtained in Example 1 was premixed with water prior to agglomeration. The moisture content was 11% on a dry weight basis. Premixing was performed prior to agglomeration using an Eirich R08 batch mixer. The resulting intermediate was used to produce briquettes as described in Example 2. It was observed that excessive clogging of the dies on the compression roll surface occurred to such an extent that briquettes could not be produced.
[0029] Example 4 (comparative) - Agglomeration of wet lignin by briquetting The lignin obtained in Example 1 was premixed with water prior to agglomeration. The moisture content was 30% on a dry weight basis. Premixing was performed prior to agglomeration using an Eirich R08 batch mixer. The resulting intermediate was used to produce briquettes as described in Example 2. It was observed that excessive clogging of the dies on the compression roll surface occurred to such an extent that briquettes could not be produced.
[0030] Example 5 (comparative) - Lignin agglomeration by briquetting with additive 1 The lignin obtained in Example 1 was used in combination with recycled fluff pulp to produce briquettes as described in Example 2. The fluff pulp was used to slow the rapid flow of material and ensure uniform material feed. It was observed that excessive clogging of the dies on the compression roll surface occurred to the extent that briquettes could not be produced.
[0031] Example 6 (Comparative) - Lignin flocculation with additive 2 The lignin obtained in Example 1 was used in combination with recycled fluff pulp to produce flakes by roller press type 52 / 10 (Maschinenfabrik Koppern GmbH). In the roller press type 52 / 10, the compression roll was equipped with a flaking die having elliptical cavities with dimensions of 30 x 20 x 5 mm evenly distributed around the circumference of the compression roll. The fluff pulp was used to slow down the rapid flow of material and ensure a uniform material supply. It was observed that excessive clogging of the die on the compression roll surface occurred to such an extent that flakes could not be produced.
[0032] Example 7 - Wet lignin agglomeration The lignin obtained in Example 1 was premixed with water prior to agglomeration. The moisture content was 13% on a dry weight basis. Premixing was performed prior to agglomeration using an Eirich R08 batch mixer. Premixing was performed prior to agglomeration using an Eirich R08 batch mixer. The obtained intermediate was used to produce flakes on a roller press type 52 / 10, in which the compression roll was equipped with a flaking die with elliptical cavities of dimensions 30 x 20 x 5 mm evenly distributed around the circumference of the compression roll. It was observed that flakes could be produced. Subsequent grinding with a beater mill (Gebr. Jehmlich GmbH) and manual sieving produced agglomerated lignin with a target particle size distribution of 0.25-1.0 mm. The results are shown in Table 2.
[0033] Example 8 - Wet lignin agglomeration The lignin obtained in Example 1 was premixed with water prior to agglomeration. The moisture content was 30% on a dry weight basis. Premixing was performed prior to agglomeration using an Eirich R08 batch mixer. The resulting intermediate was used to produce flakes on a roller press type 52 / 10, in which the compression roll was equipped with a flaking die having elliptical cavities with dimensions of 30 x 20 x 5 mm evenly distributed around the circumference of the compression roll. It was observed that flakes could be produced. Subsequent grinding in a cage mill (Stedman Machine Company) and manual sieving produced agglomerated lignin with a target particle size distribution of 1-2.0 mm. The results are shown in Table 2.
[0034] Example 9 - Dry lignin agglomeration The lignin obtained in Example 1 was agglomerated using a Hosokawa Pharmapaktor L 200 / 50P equipped with compression rolls with a working diameter of 50 mm. The compression rolls had grooves with dimensions of 50 x 1 x 1 mm spaced apart in the axial direction of the compression roll. Static plates were attached to the radial sides of the two compression rolls to seal the nip area.
[0035] It was observed that flakes with dimensions of about 80×50×2 mm (length×width×depth) could be produced as the first intermediate product, and the approximate yield of this first intermediate product on a weight basis was at least 80%.
[0036] The flakes were then crushed in a FC200 flake crusher (Hosokawa Bepex) equipped with a 2 mm screen to produce a second intermediate product. This second intermediate product was screened using a vibrating screener equipped with a screen having a mesh size determined to match the target fraction of agglomerated lignin. In this example, a screen with a mesh size of 200 μm was used.
[0037] Example 10 - Dry lignin agglomeration The lignin obtained in Example 1 was agglomerated using a Hosokawa Pharmapaktor L 200 / 50P equipped with compression rolls with a working diameter of 50 mm. The compression rolls were equipped with an annular rim with a height of 10 mm on the first roll. The second roll had a complementary annular recess to the rim of the first roll. The rolls were further equipped with grooves with dimensions of 50 x 1 x 1 mm (length x width x depth) spaced apart in the axial direction of the compression roll. It was observed that flakes with dimensions of about 80 x 50 x 2 mm (length x width x depth) could be produced as a first intermediate product. An approximate yield of this first intermediate product on a weight basis was obtained of at least 85%.
[0038] The first intermediate product was processed through an FC200 flake crusher equipped with a 5 mm screen, and the second intermediate was screened using a vibrating screener equipped with a 500 μm mesh size screen. The product yields are shown in Table 2.
[0039] Example 11 - Dry lignin agglomeration The lignin obtained in Example 1 was agglomerated using an Alexanderwerk WP200 Pharma (Alexanderwerk Aktiengesellschaft). The unit was equipped with knurled and grooved rollers with a working width of 75 mm. Static side plates were used. The unit was further equipped with a two-stage granulator, the first stage equipped with a 2.5 mm screen and the second stage equipped with a 1.25 mm screen. Immediately after the two-stage granulator was a screening deck with a single screen with a mesh size determined to match the target fraction of the final agglomerated lignin. In this example, a mesh size of 600 μm was used.
[0040] Two fractions of the aggregated lignin were collected: fraction 1 was collected before the screening deck and fraction 2 was collected after the screening deck. The particle size distribution of fractions 1 and 2 was determined by sieve analysis (Table 3).
[0041] Example 12 - Dry lignin agglomeration The lignin obtained in Example 1 was agglomerated as described in Example 11 using a 5.0 mm screen in the first stage of a two-stage granulator and a 2.0 mm screen in the second stage of the two-stage granulator. A screening deck with four screens with mesh sizes of 1.6 mm, 1.25 mm, 1.00 mm and 0.80 mm was used. Two fractions of the agglomerated lignin were collected: fraction 1 was collected before the screening deck and fraction 2 was collected after the screening deck. The particle size distribution of fractions 1 and 2 was determined by sieve analysis (Table 3).
[0042] [Table 1]
[0043] [Table 2]
[0044] [Table 3]
[0045] Thus, the particle size distribution of the final agglomerated and granulated lignin can be controlled by the configuration of the sieving stage. For example, by employing a sieving stage with one particular screen porosity, two fractions are generated: one targeted fraction and one reject fraction. The targeted fraction can be further used, but the reject fraction can be returned to the compaction stage, minimizing losses during the process. Depending on the end use, the targeted fraction can be further screened or used as the final product. By employing sieving stages with more than one screen porosity, several fractions with more defined particle size distributions are obtained.
[0046] In view of the above detailed description of the invention, other modifications and variations will be apparent to those skilled in the art. It should be apparent, however, that such other modifications and variations can be made without departing from the spirit and scope of the invention. Various aspects or embodiments that can be included in the present invention are summarized as follows. [1]. 1. A process for producing agglomerated lignin having a controlled particle size distribution, comprising: a) a lignin compression step, in which the lignin having a moisture content of 1% to 45% by weight is agglomerated by roll compression, the roll having cavities, and the depth of each cavity used in the roll compression being 0.1 mm to 10 mm; b) subjecting the compressed lignin obtained in step a) to grinding; followed by c) a sieving step, in which the product of step b) is sieved to remove particles having a particle size less than 100 μm to produce a final agglomerated lignin with a controlled particle size distribution determined by the porosity of the sieving screen used in the sieving step, and in which less than 10% by weight of the particles retained after step c) have a particle size less than 100 μm. [2]. The process according to item 1, characterized in that the lignin is agglomerated without the addition of additives. [3]. The process according to any one of the preceding claims, wherein the lignin used in step a) has a moisture content of 5% by weight to 25% by weight. [4]. The process according to item 3, wherein the lignin used in step a) has a moisture content of 5% by weight to 10% by weight. [5]. The process according to any one of the above items 1 to 4, wherein the depth of each cavity used in the roll compaction in step a) is between 1 mm and 5 mm. [6]. 6. The process according to any one of the above items 1 to 5, wherein the sieving is carried out in two or more stages using at least two sieving screens having different porosities.
Claims
1. 1. A process for producing agglomerated lignin having a controlled particle size distribution, comprising: a) a step of compressing the lignin, in which the lignin having a moisture content of 1% to 45% by weight is agglomerated by roll compression, the rolls having cavities, the depth of each cavity used for roll compression being between 0.1 mm and 10 mm; b) subjecting the compressed lignin obtained in step a) to grinding; followed by c) a sieving step, in which the product of step b) is sieved to remove particles having a particle size less than 100 μm to produce a final agglomerated lignin with a controlled particle size distribution determined by the porosity of the sieving screen used in the sieving step, and in which less than 10% by weight of the particles retained after step c) have a particle size less than 100 μm.
2. 2. The process of claim 1, wherein the lignin is agglomerated without the addition of additives.
3. 3. The process according to claim 1 or 2, wherein the lignin used in step a) has a moisture content of from 5% to 25% by weight.
4. 4. The process of claim 3, wherein the lignin used in step a) has a moisture content of from 5% to 10% by weight.
5. The process according to any one of claims 1 to 4, wherein the depth of each cavity used in the roll compaction in step a) is between 1 mm and 5 mm.
6. A process according to any one of claims 1 to 5, wherein the sieving is carried out in two or more stages using at least two sieving screens having different porosities.
Citation Information
Patent Citations
Granular hydrophobic dye composition, its production and dyeing using the same
JP1997272813A
Method for manufacturing pellets or briquettes
JP2012512270A
Carbonaceous adsorbent and methode of manufacturing the same
KR1020120117246A
Coal particles briquette where the binder is lignin and methods and systems of preparing the same
US20100154296A1
Method and Installation for the Production of Pellets from Biomass in a Pelletizing Press for Use as Fuel in Furnaces
US20100263268A1