Crosslinkable adhesive composition and adhesive tape
A crosslinked adhesive composition using specific monomers forms an acrylic copolymer without a crosslinking agent, addressing adhesive deterioration and enhancing adhesion and puncture resistance in non-aqueous batteries, ensuring battery safety and performance.
Patent Information
- Application Number
- JP2022511589
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-02-02
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-02-02
AI Technical Summary
Existing adhesive tapes for non-aqueous batteries, such as lithium ion secondary batteries, face issues with adhesive deterioration and loss of strength when exposed to electrolytes due to the presence of crosslinking agents, leading to potential battery failures like short circuits and reduced adhesion, as well as vulnerability to foreign objects and burrs.
A crosslinked adhesive composition comprising specific monomer components (A1 to A4) forms an acrylic copolymer without a crosslinking agent, enhancing adhesion and puncture resistance by self-crosslinking, maintaining adhesive strength even when exposed to electrolytes.
The adhesive composition maintains excellent adhesion and puncture resistance, preventing tape tearing and ensuring battery safety by reducing crosslinking agent content, thus supporting insulation and fixing applications in non-aqueous batteries.
Smart Images

Figure 0007572427000001 
Figure 0007572427000002 
Figure 0007572427000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a crosslinkable pressure-sensitive adhesive composition and pressure-sensitive adhesive tape which can reduce the amount of crosslinking agent added and which can be suitably used for insulating and fixing applications in batteries, particularly non-aqueous batteries such as lithium ion secondary batteries. [Background technology]
[0002] 2. Description of the Related Art In recent years, non-aqueous batteries such as lithium ion secondary batteries (hereinafter also referred to as "nonaqueous batteries") have come to be widely used in personal computers, smartphones, and the like.
[0003] Various adhesive tapes are used in non-aqueous batteries for terminal fastening, electrode protection, etc. These adhesive tapes are used in an environment where they come into contact with electrolyte, and therefore the adhesive components of the adhesive tape may dissolve into the electrolyte, causing deterioration of the battery characteristics. In particular, additives such as crosslinking agents contained in the adhesive cause deterioration of the battery characteristics. Therefore, battery manufacturers are demanding adhesive tapes that use adhesives with reduced amounts of additives such as crosslinking agents.
[0004] In addition, when the adhesive tape comes into contact with the electrolyte inside the non-aqueous battery, the adhesive dissolves and the adhesive strength deteriorates, and it may not be possible to maintain the adhesive strength required for terminal fastening, electrode protection, etc. If the adhesive tape peels off inside the non-aqueous battery, it may cause problems such as a short circuit in the battery. Therefore, there is a demand for a performance that can maintain a certain adhesive strength even when it comes into contact with the electrolyte.
[0005] Furthermore, when adhesive tapes are used to fasten the terminals or protect the electrodes of non-aqueous batteries, foreign matter present in the separator or burrs on the electrodes may cause the adhesive tape to tear, which may lead to defects such as short-circuiting the battery. Higher safety is required for non-aqueous batteries, and therefore there is a demand for adhesive tapes that have high puncture strength and will not tear even if they come into contact with foreign matter or burrs inside the non-aqueous battery.
[0006] Patent Document 1 discloses an adhesive tape for application to a portion of a non-aqueous battery that may be immersed in or come into contact with an electrolyte, which can be easily applied to battery components at room temperature and can maintain excellent adhesion in the internal environment of the non-aqueous battery. However, the adhesive layer of the adhesive tape disclosed in Patent Document 1 contains an acrylic polymer and a polyisocyanate acting as a crosslinking agent as essential components, but the effect of the crosslinking agent component contained in the adhesive tape on the non-aqueous battery has not been examined. In contrast, in non-aqueous batteries such as lithium ion secondary batteries, high capacity, miniaturization, and further long-term use are issues, and the effect of trace components such as reaction residues of crosslinking agents, which have not been considered a problem in the past, becomes relatively large, so that an adhesive tape with a reduced content of crosslinking agent components is required.
[0007] Patent Document 2 also discloses a battery adhesive tape used inside a non-aqueous battery, which can prevent the separator from being penetrated by protrusions such as foreign matter or burrs, prevent the active material from peeling off, and improve the suitability of packing electrodes into a battery case without causing a decrease in battery characteristics. Patent Document 2 also discloses that a crosslinking agent may be added to the adhesive layer as necessary. However, although Patent Document 2 discloses that the adhesive layer in the examples verifying the effects of the invention contains a crosslinking agent as an essential component, Patent Document 2 does not mention the effect of the crosslinking agent component contained in the adhesive tape on the non-aqueous battery. Adding a crosslinking agent component to an adhesive is a common technique, and the purpose of including a crosslinking agent is to increase the crosslink density of the adhesive layer of the adhesive tape, promote curing, and improve and stabilize various physical properties. However, when a crosslinking agent component is included, the flexibility of the adhesive layer decreases compared to when the crosslinking agent component is not included, and the adhesiveness may deteriorate. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] WO2013 / 133167 issue [Patent Document 2] JP 2013-140765 A Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a crosslinkable pressure-sensitive adhesive composition capable of reducing the content of a crosslinking agent component, and a pressure-sensitive adhesive tape having an adhesive layer containing this crosslinkable pressure-sensitive adhesive composition and suitable for use in, for example, insulating and fixing batteries, particularly non-aqueous batteries such as lithium ion secondary batteries. [Means for solving the problem]
[0010] The crosslinkable pressure-sensitive adhesive composition of the present invention is a crosslinkable pressure-sensitive adhesive composition containing an acrylic copolymer including 3 parts by mass or more and less than 25 parts by mass of component (A1) consisting of a hydroxyl group-containing (meth)acrylate monomer represented by formula (1) and a hydroxyl group-containing (meth)acrylate monomer represented by formula (2), 5 parts by mass or more and less than 25 parts by mass of component (A2) consisting of a carboxylic acid group-containing (meth)acrylic monomer, 5 parts by mass or more and less than 30 parts by mass of component (A3) consisting of a (meth)acrylic acid alkyl ester monomer represented by formula (3), and 50 parts by mass or more and less than 90 parts by mass of component (A4) consisting of a (meth)acrylic acid alkyl ester monomer represented by formula (4) (the total of components (A1) to (A4) is 100 parts by mass).
[0011] [ka]
[0012] (In formula (1), R 1 represents CH2=CH- or CH2=C(CH3)-, and R 2 is a hydrocarbon group of Represents x 1 is an integer between 1 and 3.)
[0013] [ka]
[0014] (In formula (2), R 3 represents CH2=CH- or CH2=C(CH3)-, and R 4 is a hydrocarbon group of Represents R 4 The number of carbon atoms in R in formula (1) 2 x is the number of carbon atoms in the 2 is an integer between 1 and 3.)
[0015] [ka] (In formula (3), R 5 represents CH2=CH- or CH2=C(CH3)-, and R 6 represents an alkyl group having 1 to 3 carbon atoms, a cyclohexyl group, or an isobornyl group.
[0016] [ka]
[0017] (In formula (4), R 7 represents CH2=CH- or CH2=C(CH3)-, and R 8 represents an alkyl group having 4 to 12 carbon atoms.
[0018] The crosslinkable pressure-sensitive adhesive composition according to the present invention is preferably a self-crosslinkable type that does not contain a crosslinking agent.
[0019] The crosslinkable pressure-sensitive adhesive composition according to the present invention may contain a crosslinking agent having a solid content of 0.5 parts by mass or less based on 100 parts by mass of the acrylic copolymer.
[0020] The pressure-sensitive adhesive tape according to the present invention has an adhesive layer containing the above-mentioned crosslinkable pressure-sensitive adhesive composition.
[0021] The pressure-sensitive adhesive tape according to the present invention may have a structure in which the pressure-sensitive adhesive layer is provided on a substrate, which is preferably at least one of a polyethylene terephthalate (PET) film, a biaxially oriented polypropylene (OPP) film, a polyimide (PI) film, and a polyphenylene sulfide (PPS) film.
[0022] The thickness of the adhesive layer of the adhesive tape according to the present invention is preferably 1 to 200 μm.
[0023] The adhesive tape according to the present invention preferably has an adhesive strength retention after immersion in an electrolyte solution of 45% or more, as calculated by the following formula. X = [(B) / (A)] × 100 [%] [X: Adhesion retention rate after immersion in electrolyte, (A): Adhesion before immersion in electrolyte measured according to the method described in JIS Z 0237:2000, (B): Adhesion after immersion in electrolyte measured according to the method described in JIS Z 0237:2000]
[0024] The pressure-sensitive adhesive tape according to the present invention is particularly useful when used in contact with the electrolyte of a non-aqueous battery. Effect of the Invention
[0025] The adhesive tape according to the present invention can suppress the amount of crosslinking agent added, and therefore, when used in a battery, particularly a non-aqueous battery such as a lithium ion secondary battery, the deterioration of battery characteristics can be suppressed. In addition, the adhesive tape according to the present invention has excellent adhesion to adherends such as separators and electrodes inside a non-aqueous battery, and has excellent adhesive force retention performance even when used in an environment in which it comes into contact with the electrolyte inside a non-aqueous battery. Furthermore, when the adhesive tape is used for terminal fastening or electrode protection of a non-aqueous battery, the adhesive tape according to the present invention can suppress the occurrence of tearing of the adhesive tape due to protrusions such as foreign matter present on the separator or burrs on the electrode. Therefore, the adhesive tape according to the present invention can be suitably used, for example, in insulation and fixing applications in batteries, particularly non-aqueous batteries such as lithium ion secondary batteries. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] <Acrylic copolymer> The resin component of the crosslinkable pressure-sensitive adhesive composition according to the present invention contains an acrylic copolymer containing the following components (A1) to (A4) as constituent components of the polymer chain. (A1) A component consisting of a hydroxyl group-containing (meth)acrylate monomer represented by the formula (1) [component (A1a)] and a hydroxyl group-containing (meth)acrylate monomer represented by the formula (2) [component (A1b)]: 3 parts by mass or more and less than 25 parts by mass. (A2) Component consisting of a carboxylic acid group-containing (meth)acrylic monomer: 5 parts by mass or more and less than 25 parts by mass. (A3) A component consisting of a (meth)acrylic acid alkyl ester monomer represented by the formula (3): 5 parts by mass or more and less than 30 parts by mass. (A4) A component consisting of a (meth)acrylic acid alkyl ester monomer represented by the formula (4): 50 parts by mass or more and less than 90 parts by mass. (The total of the above components (A1) to (A4) is 100 parts by mass). As the component (A1a), the hydroxyl group-containing (meth)acrylate monomers represented by the above formula (1) can be used alone or in combination of two or more. As the component (A1b), the hydroxyl group-containing (meth)acrylate monomers represented by the above formula (2) can be used alone or in combination of two or more. The monomer composition for forming the acrylic copolymer contained in the resin component of the crosslinkable pressure-sensitive adhesive composition according to the present invention preferably comprises components (A1) to (A4). It should be noted that the term "(meth)acrylic" is a general term that encompasses both "acrylic" and "methacrylic."
[0027] R in the formula (1) and the formula (2) 2 and R 4 are each independently a hydrocarbon group inAny of the above groups may be used, and the type is not particularly limited. These groups may be either saturated or unsaturated, but are preferably saturated hydrocarbon groups and oxygen atom-containing saturated hydrocarbon groups. These groups may be either aliphatic groups or aromatic groups, but are preferably aliphatic hydrocarbon groups and oxygen atom-containing saturated aliphatic hydrocarbon groups. Furthermore, in the case of an aliphatic group, it may be either linear, branched, or alicyclic, but is preferably a linear or branched aliphatic hydrocarbon group, and an oxygen atom-containing linear or branched aliphatic hydrocarbon group, and more preferably a linear aliphatic hydrocarbon group and an oxygen atom-containing linear aliphatic hydrocarbon group. By being a linear aliphatic hydrocarbon group and an oxygen atom-containing linear aliphatic hydrocarbon group, the crosslink density of the acrylic copolymer is improved, and the dissolution of the adhesive by the electrolyte can be further suppressed.
[0028] R in the above formula (1) 2 is a hydrocarbon group; 2 -(OH) x1 and R in the formula (2) 4 is a hydrocarbon group; 4 -(OH) x2 Specific examples of each of the groups (i.e., hydrocarbon groups having a hydroxyl group) are preferably alkyl groups having a hydroxyl group, and more preferably alkyl groups having a hydroxyl group having 1 to 4 carbon atoms. Specific examples thereof include a hydroxyethyl group, a hydroxypropyl group, and a hydroxybutyl group.
[0029] component R of the hydroxyl group-containing (meth)acrylate monomers represented by the formula (1) and the formula (2) contained in (A1) 2 and R 4 At least one of these is preferably a hydrocarbon group.
[0030] R in the above formula (2) 4 The number of carbon atoms in 2 More than the number of carbon atoms in R 2 The number of carbon atoms and R 4The difference in the number of carbon atoms between R and R in formula (2) is 1 or more, preferably 2 or more, and more preferably 2 or more and 8 or less. In particular, when the difference is 2 or more, a more significant effect is obtained in terms of suppressing dissolution of the adhesive by the electrolyte. This is presumably because the molecular chains are more fully entangled. Therefore, R in formula (2) 4 It is preferable that the number of carbon atoms in R is moderately large. However, if the number is too large, 4 In some cases, this is undesirable because the ratio of the amount of hydroxyl groups to the amount of R in the formula (2) is relatively decreased. 4 The number of carbon atoms in R in the formula (1) is 2 or more, preferably 3 or more, and more preferably 4 or more and 12 or less. 2 The number of carbon atoms in R in the formula (1) and the formula (2) is 1 or more, preferably 1 or more and 4 or less, and more preferably 2 or 3. 2 and R 4 When the number of carbon atoms is within the above range, the crosslink density of the acrylic copolymer is improved, and dissolution of the pressure-sensitive adhesive by the electrolyte can be further suppressed.
[0031] R in the formula (1) and the formula (2) 1 and R 3 are each independently CH2=CH- or CH2=C(CH3)-. 1 and R in the above formula (2) 3 may be the same as or different from each other.
[0032] In the formula (1) and the formula (2), x 1 and x 2 is R 2 and R 4 x represents the number of hydroxyl groups (-OH) bonded to each 1 and x 2 are each independently an integer of 1 to 3, preferably 1 or 2, and most preferably 1. 1 and x 2When x is within these ranges, the polymerization reaction can be stabilized, and a pressure-sensitive adhesive having the required adhesive strength can be obtained. 1 and x 2 may be the same as or different from each other.
[0033] R in the formula (1) and the formula (2) 2 and R 4 The bonding position of -(OH) to R in the formula (2) is not particularly limited. 4 Regarding the bonding position of -(OH) to R 4 The molecular end side (R 3 The end farther from the target is preferred. 4 By providing the bonding position of -(OH) to the above, the crosslinking density of the acrylic copolymer is improved, and dissolution of the pressure-sensitive adhesive by the electrolyte can be further suppressed.
[0034] Particularly preferred specific examples of the hydroxyl group-containing (meth)acrylate monomers represented by the formula (1) and the formula (2) include hydroxyalkyl (meth)acrylate esters such as 2-hydroxyethyl (meth)acrylate [e.g., 2-hydroxyethyl acrylate (2-HEA)], 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate [e.g., 4-hydroxybutyl acrylate (4-HBA)]. ; Among these, at least two kinds of monomers which become the components (A1a) and (A1b) are used in combination to form the component (A1). By using at least two kinds of monomers in this way in combination, the crosslink density of the acrylic copolymer is improved, and the dissolution of the pressure-sensitive adhesive by the electrolyte can be further suppressed.
[0035] The content of component (A1) with respect to a total of 100 parts by mass of all monomers of components (A1) to (A4) is 3 parts by mass or more and less than 25 parts by mass. If this content is less than 3 parts by mass, the crosslinking points of the adhesive decrease, and the adhesive is dissolved by the electrolytic solution, so the adhesive force after immersion in the electrolytic solution cannot be maintained. Also, if this content is 25 parts by mass or more, the normal adhesive force decreases, so the adhesive force required for insulation and fixing applications in non-aqueous batteries cannot be satisfied. The content of this component (A1) is more preferably 3 parts by mass or more and 23 parts by mass or less.
[0036] The ratio (by mass) of the amount (Ma) of component (A1a) forming component (A1) to the amount (Mb) of component (A1b) may be set so as to obtain the effects intended in the present invention. From the viewpoint of resistance to the electrolytic solution in combination with component (A2) at a predetermined blending ratio, for example, maintaining the adhesive force after immersion in the electrolytic solution, it is preferable that Ma be the same as Mb or that Ma be less than Mb (Ma = Mb or Ma < Mb). Further, it is more preferable that Ma be less than Mb within the range up to twice the amount of Ma (Ma < Mb ≦ [2 × Ma]), and it is particularly preferable to select Ma:Mb from the range of 1:1.2 to 1:2.
[0037] The carboxylic acid group-containing (meth)acrylic monomer as component (A2) is a monomer having a (meth)acrylic group and a carboxyl group. Examples thereof include, for example, (meth)acrylic acid [for example, acrylic acid (AA)], β-carboxyethyl (meth)acrylate, itaconic acid, crotonic acid, maleic acid, fumaric acid, citraconic acid, glutaconic acid, 2-acryloyloxyethyl succinic acid, 2-acryloyloxyethyl phthalic acid, etc. Among these, considering the crosslinking density of the obtained adhesive and the ease of availability, it is preferable to use (meth)acrylic acid. The carboxylic acid group-containing (meth)acrylic monomer as component (A2) can be used alone or in combination of two or more.
[0038] The content of component (A2) is 5 parts by mass or more and less than 25 parts by mass relative to 100 parts by mass of the total of all monomers of components (A1) to (A4). If the content of component (A2) is less than 5 parts by mass, the crosslinking points of the adhesive are reduced and the adhesive is dissolved by the electrolyte, so that the adhesive strength after immersion in the electrolyte cannot be maintained. If the content of component (A2) is 25 parts by mass or more, the normal adhesive strength is reduced, so that the adhesive strength required for insulation and fixing applications in non-aqueous batteries cannot be satisfied. The content of component (A2) is more preferably 10 parts by mass or more and 23 parts by mass or less.
[0039] As the (meth)acrylic acid alkyl ester monomer represented by the formula (3) as component (A3), for example, methyl acrylate (MA), ethyl acrylate, propyl acrylate, isopropyl acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, etc. can be used. Considering the crosslink density of the resulting adhesive, it is preferable to use methyl acrylate. As the (meth)acrylic acid alkyl ester monomer as component (A3), one type can be used or two or more types can be used in combination.
[0040] The content of component (A3) relative to 100 parts by mass of the total of all monomers of components (A1) to (A4) is 5 parts by mass or more and less than 30 parts by mass. If the content of component (A3) is less than 5 parts by mass, the repulsion resistance of the adhesive decreases and the adhesive strength required for applications such as fixing components inside electronic devices cannot be satisfied. If the content of component (A3) is 30 parts by mass or more, the adhesive strength decreases and the adhesive strength required for insulation and fixing applications in non-aqueous batteries cannot be satisfied. The content of component (A3) is more preferably 5 parts by mass or more and 25 parts by mass or less.
[0041] Examples of the (meth)acrylic acid alkyl ester monomer represented by the formula (4) as component (A4) include butyl (meth)acrylate [e.g., butyl acrylate (BA)], isobutyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, isohexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate [e.g., 2-ethylhexyl acrylate (2-EHA)], nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, dodecyl (meth)acrylate, and isododecyl (meth)acrylate. In order to maintain the tack of the adhesive containing an acrylic copolymer, it is preferable to use 2-ethylhexyl (meth)acrylate, etc., which has a low Tg (glass transition temperature). The (meth)acrylic acid alkyl ester monomer as component (A4) can be used alone or in combination of two or more.
[0042] The content of component (A4) is 50 parts by mass or more and less than 90 parts by mass relative to 100 parts by mass of the total of all monomers of components (A1) to (A4). If the content of component (A4) is less than 50 parts by mass, the normal adhesive strength decreases, and the adhesive strength required for insulation and fixing applications in non-aqueous batteries cannot be satisfied. If the content of component (A4) is 90 parts by mass or more, the content of hydroxyl group-containing (meth)acrylate monomer and carboxylic acid group-containing (meth)acrylate monomer decreases, and the crosslinking points of the adhesive decrease, so that the adhesive dissolves in the electrolyte and the adhesive strength cannot be maintained after immersion in the electrolyte. The content of component (A4) is more preferably 50 parts by mass or more and 80 parts by mass or less.
[0043] The acrylic copolymer used in the preparation of the crosslinked pressure-sensitive adhesive composition of the present invention can be produced by polymerizing these monomers by various polymerization methods such as solution polymerization, bulk polymerization, suspension polymerization, emulsion polymerization, etc. For example, the acrylic copolymer can be obtained by dissolving these monomers and a polymerization initiator in a solvent such as ethyl acetate in a reaction vessel and stirring the mixture at a constant temperature for a certain period of time.
[0044] The weight average molecular weight of the acrylic copolymer is not particularly limited. The weight average molecular weight can be adjusted so that the adhesive strength and swelling degree of the crosslinked pressure-sensitive adhesive composition are suitable for the use environment of the pressure-sensitive adhesive tape according to the present invention. The weight average molecular weight is preferably 200,000 or more and 1,200,000 or less, more preferably 250,000 or more and 1,000,000 or less.
[0045] By configuring the monomer composition as described above, crosslinking occurs between the carboxylic acid group and the hydroxyl group contained in the monomer, and a crosslinkable pressure-sensitive adhesive composition that allows the amount of crosslinking component to be reduced can be provided. As a result, the adhesive layer containing such a pressure-sensitive adhesive can maintain a sufficient level of adhesive strength retention after immersion in an electrolyte solution.
[0046] In addition, the crosslinkable adhesive composition of the present invention can improve the normal adhesive strength by suppressing the addition of a crosslinking agent component. The improved normal adhesive strength provides excellent adhesion to adherends such as separators and electrodes inside non-aqueous batteries. The reason for the improved normal adhesive strength is believed to be that the adhesive has a self-crosslinking portion that crosslinks functional groups in the acrylic copolymer without the use of a crosslinking agent, which makes the adhesive relatively flexible and improves its wettability to the adherend. The normal adhesive strength of the adhesive obtained by crosslinking the crosslinkable adhesive composition of the present invention can be set according to the intended use of the adhesive, and is preferably set to at least 1.0 N / 10 mm.
[0047] Furthermore, the crosslinked adhesive composition of the present invention has improved puncture strength by suppressing the addition of a crosslinking agent component. When the tape is used for terminal fastening or electrode protection of a non-aqueous battery, the improved puncture strength can suppress the occurrence of tape tearing due to protrusions such as foreign matter present in the separator or electrode burrs. The reason for the improved puncture strength is believed to be that the adhesive has a self-crosslinking portion that crosslinks between functional groups in the acrylic copolymer without the aid of a crosslinking agent, which makes the adhesive relatively flexible and disperses the force applied to the adhesive layer when punctured with a needle.
[0048] The crosslinkable pressure-sensitive adhesive composition of the present invention only needs to have a self-crosslinking portion to such an extent that the desired effect of the present invention can be obtained when the above-mentioned crosslinking agent is not added, and the crosslinkable pressure-sensitive adhesive composition of the present invention may contain a crosslinking agent within a range that does not impair the desired effect of the present invention. In applications in which the addition of a crosslinking agent is undesirable, the crosslinkable pressure-sensitive adhesive composition of the present invention is preferably a self-crosslinking type that does not contain a crosslinking agent. In order to ensure good electrolyte resistance without reducing the normal adhesive strength, the solid content ratio of the crosslinking agent relative to 100 parts by mass of the acrylic copolymer constituting the crosslinkable adhesive composition can be selected from the range of 0 to 0.5 parts by mass. When the crosslinkable pressure-sensitive adhesive composition of the present invention contains a crosslinking agent, the crosslinking agent is preferably added in a proportion of 0.5 parts by mass or less, in terms of solid content, relative to 100 parts by mass of the acrylic copolymer constituting the crosslinkable pressure-sensitive adhesive composition, i.e., more than 0 parts by mass and 0.5 parts by mass or less, and more preferably added in a proportion selected from the range of 0.001 to 0.5 parts by mass. Examples of the crosslinking agent include glycidyl group-containing compounds (e.g., 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, N,N,N',N'-tetraglycidylaminophenylmethane, triglycidyl isocyanurate, mN,N-diglycidylaminophenyl glycidyl ether, N,N-diglycidyl toluidine, N,N-diglycidylaniline, pentaerythritol polyglycidyl ether, 1,6-hexanediol diglycidyl ether, etc.), and isocyanate group-containing compounds (e.g., tolylene diisocyanate, xylylene diisocyanate, chlorophenylene diisocyanate, hexamethylene diisocyanate, tetramethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, etc.).
[0049] <Adhesive tape> The adhesive tape according to the present invention is an adhesive tape using as an adhesive the crosslinked adhesive composition containing the acrylic copolymer (and optional components as required) described above. The "adhesive tape using as an adhesive the crosslinked adhesive composition" refers to, for example, an adhesive tape consisting of an adhesive layer formed from this crosslinked adhesive composition in a sheet shape (so-called baseless type adhesive tape), or an adhesive tape in which an adhesive layer is formed on one or both sides of a substrate using this crosslinked adhesive composition.
[0050] The baseless type adhesive tape can be formed, for example, by coating an acrylic copolymer on a support such as release paper and then drying. On the other hand, the adhesive tape having a substrate can be produced by coating the crosslinked adhesive composition according to the present invention on a substrate and then drying to form an adhesive layer. Alternatively, the crosslinked adhesive composition according to the present invention may be coated on a support such as release paper to form an adhesive layer, and then this adhesive layer may be transferred to one or both sides of the substrate and laminated. The adhesive layer of the baseless type adhesive tape and the adhesive tape having a substrate may be a single layer or may be a laminate of a plurality of layers.
[0051] The thickness of the adhesive layer in an adhesive tape having a substrate is preferably 1 to 200 μm, more preferably 5 to 100 μm. The thickness of a baseless type adhesive tape is preferably 1 to 200 μm, more preferably 5 to 100 μm.
[0052] The method for applying the crosslinkable pressure-sensitive adhesive composition onto a support such as a substrate or release paper is not particularly limited, and any known method may be used, such as a method using a roll coater, a die coater, a lip coater, a dip roll coater, a bar coater, a knife coater, a spray roll coater, etc.
[0053] The adhesive strength retention rate after immersion in electrolyte (a 1:1 volumetric mixture of ethylene carbonate and diethyl carbonate), calculated using the following formula, can be used as an index for evaluating the adhesive strength of an adhesive tape suitable for use in areas that come into contact with the electrolyte of a non-aqueous battery. X = [(B) / (A)] × 100 [%] (X: Adhesion retention rate after immersion in electrolyte, (A): Adhesion before immersion in electrolyte measured according to the method described in JIS Z 0237:2000, (B): Adhesion after immersion in electrolyte measured according to the method described in JIS Z 0237:2000) The normal adhesive strength can be used as the adhesive strength (A) before immersion in the electrolyte. A detailed calculation method for the adhesive strength retention rate after immersion in the electrolyte will be described later. The adhesive strength retention rate of an adhesive tape for use in a non-aqueous battery after immersion in an electrolyte solution is preferably 45% or more, that is, at least 45%.
[0054] When the adhesive tape has a substrate, specific examples of the substrate include fiber substrates such as paper, cloth, nonwoven fabric, and net, resin substrates (resin films or resin sheets) such as olefin resins, polyester resins, polyvinyl chloride resins, vinyl acetate resins, polyamide resins, polyimide resins, polyether ether ketone (PEEK), and polyphenylene sulfide (PPS), rubber sheets, foam sheets (foam substrates), metal foils, and metal plates. Of these, it is preferable to use at least one of polyethylene terephthalate (PET) film, biaxially oriented polypropylene (OPP) film, polyimide (PI) film, and polyphenylene sulfide (PPS) film as the material of the substrate, taking into consideration versatility and chemical resistance to the electrolyte of non-aqueous batteries. Furthermore, the substrate may be a laminate of these, for example, a laminate of a resin substrate and a substrate other than resin, or a laminate of resin substrates. The substrate may be either a single layer or a multilayer. The surface of the substrate on which the pressure-sensitive adhesive layer is provided may be subjected to various treatments, such as backside treatment, antistatic treatment, undercoat treatment, corona treatment, plasma treatment, etc. The thickness of the substrate is preferably 5 to 500 μm, more preferably 10 to 200 μm.
[0055] The adhesive tape may be protected by a release paper or other film. The release paper or other film is not particularly limited, and known ones can be used as necessary. EXAMPLES
[0056] The present invention will be described in further detail below with reference to examples and comparative examples.
[0057] [Normal adhesive strength (A)] A 10 mm wide single-sided adhesive tape sample was applied to a stainless steel (SUS304) plate that had been polished with #280 waterproof abrasive paper by pressing it with a 2.0 kg roller back and forth once, and the 180° peel adhesive strength (N / 10 mm width) 20 minutes after application was measured according to the method described in JIS Z 0237:2000.
[0058] [Adhesive strength after immersion in electrolyte (B)] A 10 mm wide single-sided adhesive tape sample was applied to a SUS304 plate polished with No. 280 waterproof abrasive paper by pressing it with a 2.0 kg roller back and forth. 20 minutes after pressing, the sample was immersed in an electrolyte solution in which ethylene carbonate and diethyl carbonate were mixed at a volume ratio of 1:1, and left for 24 hours in an atmosphere at a temperature of 40 ± 5 ° C. Then, the sample was taken out of the container, the electrolyte solution was wiped off with pure water, and after wiping off water droplets, the sample was left for 2 hours in an atmosphere at a temperature of 23 ± 5 ° C. and a humidity of 50 ± 5%. The 180 ° peel adhesion strength (N / 10 mm width) of the sample was measured according to the method described in JIS Z 0237:2000, and the measured value was taken as "adhesive strength after immersion in electrolyte solution".
[0059] [Adhesive strength retention rate after immersion in electrolyte (X)] The adhesive strength retention (X) after immersion in the electrolyte was calculated using the following formula. X = [(B) / (A)] × 100 [%]
[0060] [Weight average molecular weight] The weight average molecular weight (Mw) of the acrylic copolymer is a value obtained by measuring the molecular weight of the acrylic copolymer in terms of standard polystyrene by a GPC method using the following measuring device and conditions. Equipment: LC-2000 series (JASCO Corporation) Columns: Shodex KF-806M x 2, Shodex KF-802 x 1 Eluent: Tetrahydrofuran (THF) ·Flow rate: 1.0mL / min Column temperature: 40℃ ·Injection volume: 100μL Detector: Refractometer (RI)
[0061] [Puncture strength] In an atmosphere of 23±5°C, a single-sided adhesive tape was applied to a metal plate with a circular hole of 5 mm in diameter so as to cover the hole, and the adhesive tape was clamped and fixed with a jig with an O-ring. A semicircular needle with a diameter of 1 mm and a tip radius of 0.5 mm was pierced from the adhesive layer side of the adhesive tape at a speed of 50 mm per minute, and the maximum stress until the needle penetrated the adhesive tape was measured, which was taken as the piercing strength.
[0062] [Examples 1 to 8, Comparative Examples 1 to 13] (Preparation of Acrylic Copolymer) In a reaction apparatus equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet tube, the following monomers, toluene, ethyl acetate, chain transfer agent, and radical polymerization initiator for preparing the acrylic copolymer in the parts by mass shown in Table 1 were charged, and after sealing in nitrogen gas, the mixture was reacted at 65°C for 3 hours under a nitrogen gas stream while stirring. Then, the radical polymerization initiator was charged, and the mixture was reacted at 75°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, and 2-propanol was added. As a result, an acrylic copolymer with a solid content concentration of 30% was obtained. (i) Acrylic monomers: Ingredient (A1) 2-HEA: 2-hydroxyethyl acrylate (A1a) 4-HBA: 4-hydroxybutyl acrylate (A1b) ·Ingredients (A2) AA: Acrylic acid ·Ingredients (A3) MA: Methyl acrylate ·Ingredients (A4): BA: Butyl acrylate 2-EHA: 2-ethylhexyl acrylate (ii) Radical polymerization initiator Initiator species A: 2,2'-azobis-2-methylbutyronitrile (AMBN) Initiator type B: Dilauroyl peroxide (product name: Perloyl L, manufactured by NOF Corporation) (iii) Chain transfer agent n-Dodecanethiol
[0063] (Preparation of Crosslinkable Pressure-Sensitive Adhesive Composition) Pressure sensitive adhesives for Examples 1 to 4 and Comparative Examples 1 to 6 were prepared using the acrylic polymer prepared by the above method without adding a crosslinking agent. A crosslinking agent (E-5XM manufactured by Soken Chemical Industries, Ltd., solid content concentration 5%) was added to 100 parts by mass of the acrylic polymer prepared by the above method in the solid content amounts (parts by mass) shown in Tables 1 and 3 to prepare adhesives for Examples 5 to 8 and Comparative Examples 7 to 13.
[0064] (Manufacturing single-sided adhesive tape) Each of the adhesives prepared by the above method was applied evenly to one side of a 25 μm-thick polyimide film that had been corona discharge-treated on both sides, and then heated and dried at 120° C. to form an adhesive layer with a thickness of 5 μm. A long-chain alkyl release paper was then attached to the adhesive layer, and the layer was aged at 40° C. for 3 days to obtain a single-sided adhesive tape with a total thickness of 30 μm.
[0065] (Adhesive tape evaluation) Tables 1 to 3 show the evaluation results of the pressure-sensitive adhesive tapes obtained in each of the Examples and Comparative Examples.
[0066] [Table 1]
[0067] [Table 2]
[0068] [Table 3]
[0069] In Examples 1 to 4 in Table 1, by appropriately selecting the monomer composition (type and blending ratio of monomer) and using a self-crosslinking acrylic polymer not containing a crosslinking agent as the resin component of the adhesive, good results were obtained in each evaluation item even without the addition of a crosslinking agent. In particular, an adhesive tape having a good balance of sufficient normal adhesive strength, adhesive strength retention rate after immersion in an electrolyte solution, and puncture strength was obtained. Although the weight average molecular weight of Example 1 could not be measured, the adhesive tape could be manufactured without any problems, and good results were obtained in each evaluation item. This is considered to be because the weight average molecular weight is larger than the measurable range, but does not become a factor that deteriorates the intramolecular crosslinking of the acrylic copolymer. In contrast, in Comparative Examples 1 to 6, which do not contain a crosslinking agent and whose monomer composition does not satisfy the provisions of the present invention, an adhesive tape having a good balance of both adhesive strength retention rate after immersion in an electrolyte solution and puncture strength could not be obtained. In Examples 5 to 8 in Table 1, even by adjusting the amount of crosslinking agent added to be small, adhesive tapes were obtained that had a good balance of properties related to each evaluation item, in particular, sufficient normal adhesive strength, adhesive strength retention after immersion in an electrolyte, and puncture strength.
[0070] As shown in Tables 1 and 3, in the monomer configuration of the present invention, high normal adhesive strength can be maintained by suppressing the amount of crosslinking agent component added.
[0071] The results in Tables 1 to 3 reveal that by adjusting the monomer composition according to the present invention, it is possible to obtain an adhesive tape that reduces the amount of crosslinking agent added while maintaining sufficient properties in each evaluation item in a well-balanced manner, and even does not contain a crosslinking agent. [Industrial Applicability]
[0072] According to the present invention, it is possible to provide a crosslinked adhesive composition containing an acrylic copolymer with a reduced amount of crosslinking agent added, preferably with no crosslinking agent added, and an adhesive tape using the same. This adhesive tape is particularly suitable for use in applications in which it comes into contact with the electrolyte of a non-aqueous battery, for example, for insulation and fixing applications in batteries, particularly non-aqueous batteries such as lithium ion secondary batteries.
Claims
1. A crosslinkable pressure-sensitive adhesive composition containing an acrylic copolymer including 3 parts by mass or more and less than 25 parts by mass of at least one monomer (A1) selected from the group consisting of a hydroxyl group-containing (meth)acrylate monomer represented by formula (1) and a (meth)acrylic acid hydroxyalkyl ester, which is a hydroxyl group-containing (meth)acrylate monomer represented by formula (2), 5 parts by mass or more and less than 25 parts by mass of a carboxylic acid group-containing (meth)acrylic monomer (A2), 5 parts by mass or more and less than 30 parts by mass of a (meth)acrylic acid alkyl ester monomer (A3) represented by formula (3), and 50 parts by mass or more and less than 90 parts by mass of a (meth)acrylic acid alkyl ester monomer (A4) represented by formula (4) (the total of the above monomers being 100 parts by mass), wherein the crosslinkable pressure-sensitive adhesive composition self-crosslinks via a carboxylic acid and a hydroxyl group of the acrylic copolymer without the intervention of a crosslinking agent. 【Chemistry 1】 (In formula (1), R 1 is CH 2 =CH- or CH 2 =C(CH 3 )-, R 2 represents a hydrocarbon group; x 1 is 1 to 3.) 【Chemistry 2】 (In formula (2), R 3 is CH 2 =CH- or CH 2 =C(CH 3 )-, R 4 represents a hydrocarbon group, R 4 The number of carbon atoms in R 2 x is a number of carbon atoms greater than or equal to 2 is 1 to 3.) 【Chemistry 3】 (In formula (3), R 5 is CH 2 =CH- or CH 2 =C(CH 3 )-, R 6 represents an alkyl group having 1 to 3 carbon atoms, a cyclohexyl group, or an isobornyl group. 【Chemistry 4】 (In formula (4), R 7 is CH 2 =CH- or CH 2 =C(CH 3 )-, R 8 represents an alkyl group having 4 to 12 carbon atoms.
2. A crosslinked adhesive composition as described in claim 1, which does not contain a crosslinking agent.
3. The crosslinked pressure-sensitive adhesive composition according to claim 1, comprising a crosslinking agent having a solid content of 0.5 parts by mass or less per 100 parts by mass of the acrylic copolymer.
4. A pressure-sensitive adhesive tape having an adhesive layer comprising the crosslinkable pressure-sensitive adhesive composition according to any one of claims 1 to 3.
5. The adhesive tape according to claim 4 , wherein the adhesive layer is provided on a substrate.
6. The pressure-sensitive adhesive tape according to claim 5 , wherein the substrate comprises at least one selected from the group consisting of a polyethylene terephthalate (PET) film, a biaxially oriented polypropylene (OPP) film, a polyimide (PI) film, and a polyphenylene sulfide (PPS) film.
7. The adhesive tape according to claim 4, wherein the adhesive layer has a thickness of 1 to 200 μm.
8. The pressure-sensitive adhesive tape according to claim 4 , which has an adhesive strength retention (X) after immersion in an electrolyte solution, calculated by the following formula, of 45% or more. X=[(B) / (A)]×100[%] (X: adhesion retention rate after immersion in electrolyte solution, (A): adhesion before immersion in electrolyte solution measured according to the method described in JIS Z 0237:2000, (B): adhesion after immersion in electrolyte solution measured according to the method described in JIS Z 0237:2000)
9. 5. The adhesive tape according to claim 4, which is for use in contact with an electrolyte of a non-aqueous battery.
Citation Information
Patent Citations
Composition for self-adhesive
JP1991220280A
Synthetic resin emulsion, easily water-swelling pressure- sensitive adhesive composition containing the same, and method for producing synthetic resin emulsion
JP2003201306A
Medical adhesive composition
JP2007000338A
Active energy ray-curable resin composition, adhesive agent, adhesive sheet and production method of adhesive sheet
JP2008308670A
Pressure-sensitive adhesive tape for battery and battery using the pressure-sensitive adhesive tape
JP2013140765A
Cited By
Method for determining adhesability of a film
US20240118185A1