Oxygen Evolution (OER) Electrocatalyst Materials and Their Applications

A Co oxide nanocluster with oxygen vacancies and Fe/Ni substitution, mimicking γ-CoOOH structure, addresses the limitations of existing OER catalysts by providing superior OER activity and stability for alkaline electrolysis and metal-air batteries.

JP7573271B2Active Publication Date: 2024-10-25HOKKAIDO UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020555609
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-08
Filing Date
2019-11-08
Publication Date
2024-10-25
Estimated Expiration
2039-11-08

AI Technical Summary

Technical Problem

Existing oxygen evolution reaction (OER) catalysts, including Brownmillerite-type transition metal oxides and amorphous Fe1-xCoxOy, exhibit limited activity and stability, necessitating the development of a catalyst with higher OER activity and long-term stability for applications in alkaline electrolytic hydrogen production and metal-air batteries.

Method used

A Co oxide nanocluster with an atomic arrangement similar to γ-CoOOH, containing oxygen vacancies and partially replaced with Fe and/or Ni, is synthesized through methods like anode polarization or alkaline solution immersion, forming a planar monolayer structure with coordinated protons, resulting in a catalyst with enhanced OER activity.

Benefits of technology

The new Co oxide catalyst demonstrates high and stable OER activity, outperforming conventional materials, suitable for air electrodes and water electrolysis anodes, and enabling efficient operation in metal-air secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573271000006
    Figure 0007573271000006
  • Figure 0007573271000007
    Figure 0007573271000007
  • Figure 0007573271000008
    Figure 0007573271000008
Patent Text Reader

Abstract

The present invention relates to a Co oxide material and a method for producing the same, which is a Co oxide nanocluster having an atomic arrangement structure identical or similar to a γ-CoOOH-type atomic arrangement structure and having oxygen vacancies, where a portion of the Co in the nanocluster may be substituted with Fe and / or Ni. The particle size of the Co oxide nanocluster is 10 nm or less. The Co oxide material of the present invention is a transition metal oxide catalyst with high OER activity, and the present invention also provides a catalyst for an air electrode, a catalyst for a water electrolysis anode, an air electrode, and an air secondary battery that use this catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to materials for oxygen evolution (OER) electrocatalysis and their uses. CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority from Japanese Patent Application No. 2018-210890, filed November 8, 2018, the entire disclosure of which is expressly incorporated herein by reference. [Background technology]

[0002] Oxygen evolution (OER) electrocatalysts are important as anodes for alkaline electrolytic clean hydrogen production and as air electrodes for metal-air batteries. To date, various crystalline Co-based oxides have been investigated as oxygen evolution electrocatalysts (Non-Patent Documents 1-3), and the identification of their surface active species has also progressed. Recently, Ba, which is known to be a highly active catalyst for oxidation, has been investigated. 0.5 Sr 0.5 Co 0.4 Fe 0.6 It has been reported that when O3 reaches or exceeds the oxygen evolution potential in an alkaline solution, it becomes amorphous and becomes an active species (Non-Patent Document 4). 1-x Co x O y It has been reported that the solid solution exhibits high oxygen evolution electrocatalytic activity (Non-Patent Document 5).

[0003] Furthermore, it has been reported that the use of the Brownmillerite-type transition metal oxide A2B2O5, which has not previously attracted attention as an oxygen generating catalyst, exhibits activity in the OER reaction comparable to that of a Pt catalyst, and that the use of a catalyst containing two types of transition metals in particular exhibits activity that exceeds that of precious metal catalysts (Patent Document 1).

[0004] As an example of an OER catalyst with a new structure, a material with a CoOOH nanosheet structure has been reported (Non-Patent Document 6). This material was prepared by exfoliating α-Co(OH)2 sheets by ultrasonic treatment in the presence of Cl anions and water, followed by oxidation treatment using NaClO. According to the TEM image in Fig. 1b and the AFMM image in Fig. 1c, the material has a particle size of 200-300 nm. Furthermore, according to the XRD result in Fig. 1d, the material has crystallinity.

[0005] Patent Document 1: WO2015 / 115592

[0006] Non-patent document 1: T. Maiyalagan, et al., Nature Commun., 5, 3949 (2014). Non-patent document 2: A. Grimoud et al, Nature Chem., 9, 457 (2017). Non-patent document 3: Y. Matsumoto et al, J. Electrochem. Soc., 127, 811 (1980). Non-patent document 4: KJ May et al, J. Phys. Chem. Lett., 3, 3264 (2012). Non-patent document 5: L. Wei et al., Adv. Mater., 10.1002 / adma.201701410 Non-Patent Document 6: J. Huang, et al., Angewandte_Chemie_International_Edition 2015, 54, 8722-8727 The entire disclosures of Patent Document 1 and Non-Patent Documents 1 to 6 are hereby expressly incorporated by reference. Summary of the Invention [Problem to be solved by the invention]

[0007] The Brownmillerite-type transition metal oxide A2B2O5 containing two types of transition metals described in Patent Document 1 exhibits OER activity superior to that of precious metal catalysts. However, in consideration of practical use, the development of a catalyst that has higher OER activity and exhibits stable activity for a long period of time is required. In addition, the material described in Non-Patent Document 3 has a complicated manufacturing method and does not have high OER activity, so there is room for further improvement.

[0008] Therefore, an object of the present invention is to develop a new transition metal oxide catalyst with higher OER activity, and further to provide an air electrode catalyst, a water electrolysis anode catalyst, an air electrode, and an air secondary battery that use this catalyst. [Means for solving the problem]

[0009] The present invention is as follows. [1] A Co oxide material, which is a Co oxide nanocluster having an atomic arrangement structure identical or similar to a γ-CoOOH type atomic arrangement structure and having oxygen defects, and in which a portion of Co in the nanocluster may be substituted with Fe and / or Ni. [2] The material according to [1], wherein the Co oxide nanoclusters have a particle size of 10 nm or less. [3] CoO6 octahedra are two-dimensionally connected by edge-sharing to form [CoO x ] Planar monolayer with protons for charge compensation [CoO x H y ] Planar monolayers are stacked in n layers [CoO x H y ] n A Co oxide material containing nanoclusters of a molecular layer sheet-like substance, in which x is in the range of 1.5 to 2.0, y is in the range of 0.01 to 1, n is the number of stacks of the planar monolayer in the direction perpendicular to the molecular layer plane (c-axis direction) and is in the range of 1 to 25, and [CoO x H y] The above material, in which a portion of the Co in the planar monolayer may be substituted with Fe and / or Ni, and a portion of the oxygen in the CoO6 octahedron may be missing. [4] [CoO x H y ]The material according to [3], wherein one side of the planar monolayer is 10 nm or less. [5] The material according to any one of [1] to [4], wherein the maximum outer diameter of the nanoclusters observed in a TEM image is in the range of 0.3 to 10 nm. [6] The material according to any one of [1] to [5], wherein a portion of Co in the nanoclusters is substituted with Fe and / or Ni. [7] The material according to [6], wherein the amount of substitution of Co with Fe and / or Ni is in the range of 100:0.1-10 as determined by the Co:Fe atomic ratio obtained by Auger spectroscopy analysis or the Co:Fe atomic ratio obtained by elemental analysis by ICP analysis. [8] The material according to any one of [1] to [7], which is for use as an OER catalyst. [9] A method for producing the material according to any one of [1] to [7], comprising placing a raw material containing Ca2CoFeO5 and / or Ca2CoNiO5 under anodic polarization or immersing it in an alkaline aqueous solution.

[10] The anodic polarization is performed at a current density resulting in a voltage in the range of 1.5 to 2.0 V vs. RHE, and the immersion in the alkaline aqueous solution is performed in an alkaline aqueous solution having a concentration of 1 M or more for one day or more.

[11] A method for producing the material according to any one of [1] to [7], comprising the steps of: adding an alkali to an aqueous solution containing an Fe salt and / or an Ni salt, and a Co salt, to precipitate a hydroxide containing Fe and / or Ni, and Co, and recovering the precipitate; and calcining the precipitate of the hydroxide containing Fe and / or Ni, and Co in an oxygen-containing atmosphere to obtain an oxyhydroxide containing Fe and / or Ni, and Co.

[12] The method according to

[11] , wherein the Fe salt, Ni salt and Co salt are each a nitrate, and the alkali is an alkali metal hydroxide.

[13] A catalyst for an air electrode comprising the material according to any one of [1] to [7] or the material produced by the method according to any one of [9] to

[12] .

[14] A catalyst for a water electrolysis anode, comprising the material according to any one of [1] to [7] or a material produced by the method according to any one of [9] to

[12] .

[15] An air electrode for a metal-air secondary battery, comprising the catalyst according to

[13] or

[14] .

[16] The air electrode according to

[15] , wherein the material is contained as an oxygen evolution catalyst and further contains an oxygen reduction catalyst.

[17]

[15] or

[16] . A metal-air secondary battery comprising: an air electrode according to

[15] or

[16] ; a negative electrode containing a negative electrode active material; and an electrolyte interposed between the air electrode and the negative electrode.

[18] The metal-air secondary battery according to

[17] , further comprising an oxygen reduction air electrode containing an oxygen reduction catalyst. Effect of the Invention

[0010] According to the present invention, a new material useful as an OER catalyst, which has high and stable OER activity for a long period of time, can be provided. Furthermore, this material can be used to provide an air electrode catalyst or a water electrolysis anode catalyst that exhibits excellent OER activity for a long period of time, and thus an air electrode and an air secondary battery that are superior to conventional products can be provided. [Brief description of the drawings]

[0011] [Figure 1]High-resolution TEM images of (a) Brown-mirror Ca2FeCoO5+δ (before OER polarization) and (b) Ca2FeCoO5+δ after OER polarization at 1.6 V vs RHE for 1 h. The lattice fringes in (a) correspond to the 110 spacing of the Brown-mirror phase. In (b), several nanoclusters with periodic structures are enclosed by yellow dashed lines. The inset shows the electron diffraction pattern measured near the center of the TEM image. [Diagram 2] This is a current-time curve of Ca2FeCoO5 (sometimes abbreviated as CFC) supported on a carbon sheet, which was subjected to an OER polarization cycle of 2 h at a constant current of 40 mA cm-2 and then held at an open circuit potential for 15 min, repeated for one month. [Diagram 3] shows the XRD patterns of the CFC-loaded carbon electrode immediately after preparation (as-prepared), after 1 hour (1h), and after 1 month (1 month). The XRD pattern of the CFC powder is also shown for reference. ▼ and ◯ indicate peaks derived from the carbon sheet and Nafion, respectively. [Figure 4] shows the Auger spectra of CFC particles before and after one month of OER polarization. [Diagram 5] (a) Co K-edge and (b) Fe K-edge XANES spectra of Ca2FeCoO5 immediately after preparation (As prepared) and after anodic polarization at 20 mA cm-2 constant current for 1 hour (1h) and 1 month. Radial distributions around Co atoms ((c), (e)) and Fe atoms ((d), (f)) determined by extended X-ray absorption fine structure (EXAFS). (c) and (d) show a comparison between the As prepared and 1h samples, and (e) and (f) show a comparison between the As prepared and 1 month samples. (c) and (d) also show the fitting results (dotted lines) using the γ-CoOOH structural model (Figure 6). [Figure 6]shows a model of the crystal structure of γ-CoOOH (hexagonal). The small red spheres, large blue spheres, and small white spheres (isolated between layers) represent oxygen, cobalt, and hydrogen atoms, respectively. [Figure 7] The isopotential polarization curves of the CFCs before and after one month of OER polarization are shown. The results of γ-CoOOH prepared by pyrolysis are also shown. [Figure 8] 1 shows the XRD patterns of Fe0.05Co0.95OxHy, Fe0.1Co0.9OxHy, and Ni0.1Co0.95OxHy prepared in Example 2. The XRD pattern of γ-CoOOH is also shown. [Figure 9] 1 shows the OER polarization curves of Fe0.05Co0.95OxHy, Fe0.1Co0.9OxHy and Ni0.1Co0.95OxHy prepared in Example 2. The OER polarization curves of CFCs are also shown. [Figure 10] 1 shows XRD of the sample (CFC) before KOH treatment and the KOH-treated sample prepared in Example 3. [Figure 11] 1 shows the OER polarization curves of the sample (CFC) before KOH treatment and the KOH-treated sample prepared in Example 3. [Figure 12] 1 shows an example of the configuration of the metal-air secondary battery of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <The Co oxide material of the present invention> The Co oxide material of the present invention is a Co oxide nanocluster having an atomic arrangement structure that is the same as or similar to a γ-CoOOH type atomic arrangement structure and has oxygen defects, and a part of the Co in the nanocluster may be substituted with Fe and / or Ni.

[0013] The Co oxide material of the present invention is a Co oxide nanocluster, and the Co oxide nanocluster is characterized by the following (1) to (3). (1) Having an atomic arrangement structure identical or similar to that of γ-CoOOH type and having oxygen vacancies: The atomic arrangement structure of the γ-CoOOH type is the atomic arrangement structure of the crystal structure model of γ-CoOOH (hexagonal crystal), and FIG. 6 shows the crystal structure model of γ-CoOOH (hexagonal crystal). The red ball (small), blue ball (large), and white ball (small, isolated between layers) in the figure represent oxygen atoms, cobalt atoms, and hydrogen atoms, respectively. γ-CoOOH has a layered structure in which [CoO2] planar molecular layers formed by edge sharing of CoO6 octahedra are stacked on the c-axis by hydrogen bonds via protons. The Co oxide material of the present invention has an atomic arrangement structure that is the same as or similar to the crystal structure model of γ-CoOOH (hexagonal crystal) shown in FIG. 6. In the case of a single planar molecular layer of [CoO2], the Co oxide material of the present invention has an atomic arrangement structure that is the same as the crystal structure model of γ-CoOOH (hexagonal crystal), and in other cases, it has an atomic arrangement structure similar to the crystal structure model of γ-CoOOH (hexagonal crystal). As described later in the manufacturing method, it is presumed that such an atomic structure is formed by rearrangement of atoms due to OER polarization, forming a Co-rich oxide portion in the oxide matrix, which forms an arrangement structure very similar to that of γ-CoOOH. Figure 1 shows a nanocluster in the Co oxide of the present invention observed by high-resolution TEM, and this nanocluster has an atomic arrangement structure identical or similar to that of the γ-CoOOH type. Since the nanocluster of the present invention has oxygen vacancies, the part with oxygen vacancies is defined as having an atomic arrangement structure similar to that of the γ-CoOOH type, not identical to that of the γ-CoOOH type.

[0014] The Co oxide material of the present invention has oxygen deficiencies. There is no particular limit to the degree of oxygen deficiency (less than the stoichiometric ratio), but it can be, for example, more than 0 and 25% or less of the total amount of valences of elements other than oxygen. However, more oxygen deficiencies than this are also acceptable.

[0015] (2) Co oxide nanoclusters: The diameter of the Co oxide nanoclusters varies depending on the manufacturing method and conditions. For example, in the manufacturing methods in the test examples and embodiments described below, the diameter can be 20 nm or less, and the diameter of the Co oxide nanoclusters can be 10 nm or less. FIG. 1 shows a nanocluster in the Co oxide of the present invention prepared from a raw material containing Ca2CoFeO5(CFC) observed by high-resolution TEM in Test Example 1. As described above, this nanocluster is a nanocluster having an atomic arrangement structure identical or similar to the atomic arrangement structure of the γ-CoOOH type arrangement structure. This nanocluster is confirmed to have a diameter of 10 nm or less by the high-resolution TEM image shown in FIG. 1, and specifically, is a nanocluster of about 0.5-2 nm. In addition, the fact that no peak derived from the molecular structure that should be observed is confirmed in the XRD pattern of the Co oxide of the present invention supports the fact that the cluster diameter is 10 nm or less.

[0016] FIG. 8 shows the Fe 0.05 Co 0.95 O x H y , Fe 0.1 Co 0.9 O x H y and Ni 0.1 Co 0.95 O x H y The XRD pattern of is very broad, and the crystallite size is estimated to be about 8-15 nm from the half-width of the 002 peak at around 20°. The nanoclusters in the Co oxide of the present invention prepared from the raw material prepared by the coprecipitation method can be clusters with a diameter of 20 nm or less, preferably 5 nm or more and 15 nm or less.

[0017] The Co oxide of the present invention is clearly different from the material described in Non-Patent Document 6 in which a clear X-ray peak appears, at least because of the particle size and the fact that no diffraction peak due to crystals is observed by XRD, or even if observed, the peak is very broad.

[0018] (3) Co oxide materials, in which a portion of the Co in the nanoclusters may be substituted with Fe and / or Ni: The Co oxide material of the present invention prepared in Example 1 is found to have a portion of Co in the nanoclusters substituted with Fe from the results of composition analysis by Auger spectroscopy. The amount of Fe substituted for Co is, for example, in the upper limit of the substitution range of the Co:Fe atomic ratio obtained by Auger spectroscopy spectrum analysis, 100:10 or less, preferably 100:5 or less. The lower limit is 100:0.1 or more, preferably 100:1 or more. The range of 100:0.1 to 10 is preferred, and the range of 100:1 to 5 is more preferred.

[0019] The Co oxide material of the present invention prepared in Example 2 was found to have a part of Co in the nanoclusters substituted with Fe and / or Ni as a result of elemental analysis by ICP. The amount of substitution of Co with Fe and / or Ni is, for example, in the upper substitution range of Co:Fe and / or Ni atomic ratio by ICP of 100:10 or less, preferably 100:5 or less. The lower substitution range is 100:0.1 or more, preferably 100:1 or more. The range of 100:0.1 to 10 is preferred, and the range of 100:1 to 5 is more preferred.

[0020] More specifically, the Co oxide material of the present invention is [CoO x ] Planar monolayer with protons for charge compensation [CoO x H y ] Planar monolayers are stacked perpendicular to the plane via hydrogen bonds to form n-layers [CoO x H y ] n A Co oxide material containing nanoclusters of a molecular layer sheet-like substance, in which x is in the range of 1.5 to 2.0, y is in the range of 0.01 to 1, n is the number of stacks of the planar monolayer in the direction perpendicular to the molecular layer plane (c-axis direction) and is in the range of 1 to 25, and [CoO x H y ] The material may have a portion of Co in the planar monolayer substituted with Fe and / or Ni.

[0021] The nanoclusters of the Co oxide material of the present invention are [CoO x ] Planar monolayer with protons for charge compensation [CoO x H y ] Planar monolayers are stacked in the direction perpendicular to the plane to form [CoO x H y ] n This is a nanocluster of a molecular layer sheet material. According to the EXAFS fitting results shown in Example 1, the oxygen coordination number around Co is 5.1 in the case of 1 hour polarization, and about 5.3 in the case of 1 month polarization (Table 2). On the other hand, [CoO2] has no oxygen deficiency at all. n The Co coordination number in the molecular layer sheet is 6. Therefore, the nanoclusters of the Co oxide material of the present invention shown in the experimental examples have oxygen vacancies [CoO x H y ] n It is considered that this material has a molecular layer sheet as a basic skeleton. On the other hand, from the XRD results shown in Figure 3, since the XRD peak of γ-CoOOH does not appear in the Co oxide material of the present invention, it is considered that the stacking in the c-axis direction is present but not developed in this nanocluster. Therefore, the stacking in the direction perpendicular to the plane is present in the nanocluster of the Co oxide material of the present invention but is not developed, and [CoO X H y ] n It was identified as a molecular layer sheet material. X H y ] n It can be said that the atomic arrangement structure of the molecular layer sheet material is not identical to the atomic arrangement structure of the γ-CoOOH type, but has an atomic arrangement structure similar to the atomic arrangement structure of the γ-CoOOH type.

[0022] [CoO X H y ] nIn the molecular layer sheet, x is in the range of 1.5 to 2.0, preferably in the range of 1.6 to 1.9, y is in the range of 0.01 to 1, preferably in the range of 0.05 to 0.5, and n is in the range of 1 to 25. The nanoclusters of the Co oxide material of the present invention have a maximum outer diameter of 0.3 to 10 nm, preferably in the range of 0.6 to 7 nm, more preferably in the range of 0.9 to 5 nm, as observed in a TEM image. The diameter of the CoO6 octahedron is about 0.29 nm (approximately 0.3 nm), and the diameter of the [CoO X H y ] The interlayer distance of the monolayer is about 0.4 nm. Assuming a cluster with a maximum diameter of 10 nm, the [CoO X H y ]CoO in the monolayer X H y The number of octahedral molecules is 10 / 0.29 x 10 / 0.29 (approximately 1200), 7 / 0.29 x 7 / 0.29 (approximately 580) for the maximum diameter range of 7 nm, and 5 / 0.29 x 5 / 0.29 (approximately 300) for the maximum diameter range of 5 nm.

[0023] As described above, the nanoclusters of the Co oxide material of the present invention have stacking in the direction perpendicular to the plane, but they are not well developed [CoO X H y ] n It is a molecular layer sheet material, where n is the number of layers in the direction perpendicular to the molecular layer plane of the planar monolayer (c-axis direction). Assuming a cluster with a maximum diameter of 0.3 to 10 nm, n is 1 to 10 / 0.4 (about 25). Therefore, the above n is in the range of 1 to 25. Furthermore, in the case of a diameter range of 0.6 to 7 nm, n is 2 to 7 / 0.4 (about 18), and in the case of a diameter range of 0.9 to 5 nm, n is 2 or 3 to 5 / 0.4 (about 12).

[0024] The Co oxide material of the present invention is extremely useful as an OER catalyst, which will be described later.

[0025] <Method of manufacturing the Co oxide material of the present invention> The Co oxide material of the present invention can be produced, for example, by a method comprising: (a) placing a raw material containing Ca2CoFeO5 and / or Ca2CoNiO5 under anodic polarization or immersing it in an alkaline aqueous solution; or (b) adding an alkali to an aqueous solution containing an Fe salt and / or a Ni salt, and a Co salt to precipitate a hydroxide containing Fe and / or Ni, and Co, recovering the precipitate, and calcining the precipitate of hydroxide containing Fe and / or Ni, and Co in an oxygen-containing atmosphere to obtain an oxyhydroxide containing Fe and / or Ni, and Co.

[0026] Manufacturing method (a) Ca2CoFeO5 and Ca2CoNiO5 are types of Brownmillerite transition metal oxides, and can be prepared by a solid-phase reaction method using each metal oxide as a raw material with reference to the method described in Patent Document 1. In addition to the solid-phase reaction method, they can also be synthesized using a liquid-phase reaction method. In the liquid-phase reaction method, salts of each metal, such as nitrates, acetates, citrates, etc., are used as raw materials for each metal oxide. For example, Ca salts (e.g., Ca(NO3)2), Fe salts (e.g., Fe(NO3)3)·9H2O), Ni salts (e.g., Ni(NO3)3)·9H2O), Co salts (e.g., Co(NO3)2)·6H2O) are used, and a mixture to which citric acid is added as a gelling agent is mixed using, for example, water (distilled water or ion-exchanged water) as a solvent. The ratio of each metal salt is appropriately determined in consideration of the composition of the target metal oxide. The amount of citric acid used as a gelling agent can be, for example, in the range of 10 to 1000 parts by mass per 100 parts by mass of the metal salt. As a gelling agent, other than citric acid, for example, EDTA (ethylenediaminetetraacetic acid) or glycine can be used. The mixture is gelled by heating, for example, to 50 to 90°C to remove the solvent. The gelled product is pre-calcined, for example, in air at 300 to 500°C (for example, 450°C) for 10 minutes to 6 hours (for example, 1 hour) to synthesize a precursor. Next, the precursor is calcined, for example, in air at 600 to 800°C for 1 to 24 hours to synthesize Brownmillerite type Ca2FeCoO5 or Ca2CoNiO5. The calcination conditions can be, for example, calcined at 600°C for a predetermined time (1 to 12 hours), and then the temperature is raised and calcined, for example, at 800°C for a predetermined time (6 to 12 hours).

[0027] (1) Anodic polarization method Anode polarization is suitably carried out by passing a predetermined amount of electricity or more at a current density that results in a voltage in the range of, for example, 1.5 to 2.0 V relative to the RHE using a raw material containing Ca2CoFeO5 (CFC) and / or Ca2CoNiO5 (CNC) as an electrode. The predetermined amount of electricity or more can be appropriately selected from the amount of electricity that generates the desired nanoclusters depending on the composition and concentration of the alkaline aqueous solution, the temperature, the structure of the electrode using the raw material as the electrode, and the like. In the examples, the amount of CFC applied to the anode electrode is 10 mg cm -2 A three-electrode system was used, using a carbon sheet electrode as the electrode substrate, a platinum plate as the counter electrode (cathode), and a reference electrode for the anode electrode, and the current was measured at 40 mA cm in an aqueous KOH solution under an inert argon atmosphere. -2 The anodic polarization was repeated for 2 hours under a constant oxidation current condition with a period of zero current in between. The amount of electricity used for the anodic polarization in this case was 1 cm 2 When applying CFC to an anode electrode and carrying out polarization treatment, the polarization conditions can be selected based on this quantity of electricity.

[0028] The alkaline aqueous solution used as the electrolyte for polarization in the alkaline aqueous solution can be, for example, an alkaline aqueous solution in the range of 0.1M to 10M, and is preferably an alkaline aqueous solution in the range of 1M to 6M.

[0029] After the polarization treatment, the nanocluster material of the present invention can be recovered from the anode electrode, but the anode electrode on which the nanocluster material of the present invention is formed can also be used as a product as it is.

[0030] (2) Alkaline solution immersion method The alkaline aqueous solution immersion can be carried out by immersing the raw material containing Ca2CoFeO5 (CFC) and / or Ca2CoNiO5 (CNC) in an aqueous solution of an alkali metal hydroxide or an alkaline earth metal hydroxide at a temperature range of, for example, 0 to 100°C. The temperature is preferably in the range of 60 to 90°C. The concentration of the alkaline aqueous solution is not particularly limited, but can be, for example, in the range of 0.1M to 10M, preferably in the range of 1M to 6M. The immersion time can be appropriately determined in consideration of the type of raw material, the immersion temperature, the concentration of the alkaline aqueous solution, etc., until the desired nanoclusters are generated. When the temperature is 80°C, the immersion in the alkaline aqueous solution is preferably carried out for one day or more in an alkaline aqueous solution with a concentration of 1M or more from the viewpoint of generating the desired nanoclusters.

[0031] After immersion in the alkaline aqueous solution, the immersed product is recovered and washed with water to obtain the nanocluster material of the present invention.

[0032] Manufacturing method (b) In this manufacturing method, a raw material is prepared by a coprecipitation method in which an alkali is added to an aqueous solution containing an Fe salt and / or Ni salt and a Co salt to precipitate a hydroxide containing Fe and / or Ni and Co, and the precipitate is collected. The obtained precipitate of hydroxide containing Fe and / or Ni and Co is fired in an oxygen-containing atmosphere to obtain an oxyhydroxide containing Fe and / or Ni and Co.

[0033] The Fe salt, Ni salt and Co salt are not particularly limited as long as each salt is water-soluble, and can be, for example, a nitrate, and chlorides can be used in addition to nitrates. The alkali is not particularly limited as long as it is water-soluble, and can be, for example, an alkali metal hydroxide, and can be lithium hydroxide, sodium hydroxide, potassium hydroxide, etc. The coprecipitation method can be carried out at room temperature, but can also be carried out under cooling or heating. It is appropriate to use an aqueous alkali solution for adding an alkali to an aqueous solution containing an Fe salt and / or Ni salt and a Co salt. The salt concentration of the aqueous solution containing an Fe salt and / or Ni salt and a Co salt, and the alkali concentration of the aqueous alkali solution can be appropriately determined.

[0034] The precipitate of hydroxide containing Fe and / or Ni and Co prepared by the coprecipitation method is calcined in an oxygen-containing atmosphere. The oxygen-containing atmosphere may contain oxygen, and may be pure oxygen or air, but is preferably an oxygen atmosphere from the viewpoint of easily obtaining oxyhydroxide. The calcination temperature may be any temperature at which oxyhydroxide can be obtained, and may be, for example, in the range of 50 to 200°C, preferably in the range of 80 to 150°C. The heating time can be appropriately determined in consideration of the heating temperature and the degree of oxyhydroxide production. By this calcination, oxyhydroxide containing Fe and / or Ni and Co is obtained, and the Co oxide material of the present invention can be obtained by using the raw material obtained by the coprecipitation method.

[0035] <Catalyst for electrode> The present invention includes a cathode catalyst comprising the material of the present invention. The present invention further includes a water electrolysis anode catalyst comprising the material of the present invention. The air electrode catalyst and water electrolysis anode catalyst of the present invention may contain the above-mentioned CFC as a raw material in addition to the material of the present invention.

[0036] The air electrode catalyst and the water electrolysis anode catalyst containing the material of the present invention have a surface area of, for example, 1 to 100 m 2 / g, preferably 10 to 100 m2 / g, but is not intended to be limited to this range.

[0037] The material of the present invention is extremely useful for air electrodes, and is extremely promising for hydrogen production by photochemical water splitting, and for use as air electrodes in metal-air secondary batteries, which are expected to be the next-generation high-capacity secondary batteries.

[0038] The reaction at the anode during water electrolysis is represented by the following reaction formula: H2O→O2+4H + +4e - (neutral to acidic) 4OH - →O2+2H2O+4e - (Basic) Both reactions are oxygen evolution reactions (OER). The material of the present invention has excellent OER activity and is extremely useful as a catalyst for water electrolysis anodes.

[0039] <Air electrode> The air electrode usually has a porous structure and contains an oxygen reaction catalyst and a conductive material. The air electrode may also contain an oxygen reduction (ORR) catalyst, a binder, etc., as necessary. The air electrode in a secondary battery is required to have OER catalytic activity as a function during charging and ORR catalytic activity as a function during discharging. Since the catalyst of the present invention is an OER catalyst, the air electrode can also contain an ORR catalyst in addition to this catalyst. The chemical formulas at the air electrode during charging and discharging are shown below. [ka]

[0040] The content of the catalyst of the present invention (OER catalyst) in the air electrode is not particularly limited, but from the viewpoint of improving the oxygen reaction performance of the air electrode, it is preferably, for example, 1 to 90 mass %, particularly preferably 10 to 60 mass %, and more preferably 30 to 50 mass %.

[0041] Examples of the ORR catalyst include, but are not limited to, Pt or Pt-based materials (e.g., PtCo, PtCoCr, Pt-W2C, Pt-RuOx, etc.), Pd-based materials (e.g., PdTi, PdCr, PdCo, ​​PdCoAu, etc.), metal oxides (e.g., ZrO 2-x , TiO x ,TaN x O y , IrMO x etc.), complexes (Co-porphyrin complexes), others (PtMoRuSeO x , RuSe, etc. Other examples include LaNiO3 (Nat. Chem. 3, 546 (2011)), which has been reported by Suntivich et al. as being highly active, and CoO / N-doped CNT (Nat. Commun. 4, 1805 (2013)), reported by Li et al. However, it is not intended to be limited to these. Also, multiple catalysts can be used in combination, taking into consideration the performance and properties of each catalyst. Furthermore, the above catalysts can be used in combination with a promoter (for example, TiO x , RuO2, SnO2, etc.) can also be used in combination. When an ORR catalyst is used in combination, the content can be appropriately determined taking into consideration the type and catalytic activity of the ORR catalyst, and can be, for example, 1 to 90 mass %. However, it is not intended to be limited to this numerical range.

[0042] The conductive material is not particularly limited and may be any material that can be generally used as a conductive assistant, with conductive carbon being preferred. Specific examples include mesoporous carbon, graphite, acetylene black, carbon nanotubes, and carbon fibers. Conductive carbon with a large specific surface area is preferred because it provides many reaction sites at the air electrode. Specifically, conductive carbon with a specific surface area of ​​1 to 3,000 m2 is preferred. 2 / g, especially 500~1500m 2 The catalyst for the air electrode may be supported on a conductive material.

[0043] The content of the conductive material in the air electrode is not particularly limited, but from the viewpoint of increasing the discharge capacity, it is preferably, for example, 10 to 99 mass %, particularly preferably 20 to 80 mass %, and more preferably 20 to 50 mass %.

[0044] By incorporating a binder in the air electrode, the catalyst and conductive material can be immobilized, and the cycle characteristics of the battery can be improved. The binder is not particularly limited, and examples thereof include polyvinylidene fluoride (PVDF) and its copolymers, polytetrafluoroethylene (PTFE) and its copolymers, and styrene butadiene rubber (SBR). The content of the binder in the air electrode is not particularly limited, but from the viewpoint of the binding strength between the carbon (conductive material) and the catalyst, it is preferably, for example, 1 to 40 mass%, particularly preferably 5 to 35 mass%, and more preferably 10 to 35 mass%.

[0045] The air electrode can be formed, for example, by dispersing the air electrode constituent material in a suitable solvent to prepare a slurry, which is then applied to a substrate and dried. The solvent is not particularly limited, and examples thereof include acetone, N,N-dimethylformamide, and N-methyl-2-pyrrolidone (NMP). The air electrode constituent material and the solvent are usually mixed for 3 hours or more, preferably 4 hours. The mixing method is not particularly limited, and a general method can be used.

[0046] The substrate to which the slurry is applied is not particularly limited, and examples thereof include a glass plate, a Teflon (registered trademark) plate, and the like. These substrates are peeled off from the obtained air electrode after the slurry is dried. Alternatively, the current collector of the air electrode or the solid electrolyte layer can be treated as the substrate. In this case, the substrate is not peeled off and is used as it is as a component of the metal-air secondary battery.

[0047] The method for applying and drying the slurry is not particularly limited, and a common method can be used. For example, a spray method, a doctor blade method, a gravure printing method, or the like can be used as the application method, and a drying method such as a heat drying method or a reduced pressure drying method can be used.

[0048] The thickness of the air electrode is not particularly limited and may be appropriately set depending on the application of the metal-air secondary battery, but is usually preferably 5 to 100 μm, 10 to 60 μm, and particularly preferably 20 to 50 μm.

[0049] An air electrode current collector that collects current from the air electrode is usually connected to the air electrode. The material and shape of the air electrode current collector are not particularly limited. Examples of materials for the air electrode current collector include stainless steel, aluminum, iron, nickel, titanium, and carbon. Examples of the shape of the air electrode current collector include foil, plate, mesh (grid), and fiber, and among these, a porous shape such as a mesh is preferable. This is because a porous current collector has excellent oxygen supply efficiency to the air electrode.

[0050] <Metal-air secondary battery> The metal-air secondary battery of the present invention has an air electrode containing a catalyst including the material of the present invention, a negative electrode containing a negative electrode active material, and an electrolyte interposed between the air electrode and the negative electrode. The air electrode of the metal-air secondary battery of the present invention contains a catalyst including the material of the present invention, and this catalyst exhibits excellent OER catalytic properties. Therefore, by using an air electrode using this catalyst, the metal-air secondary battery of the present invention has excellent charging speed and charging voltage.

[0051] In addition, the air electrode can also be made to coexist with a catalyst having ORR catalytic activity as described above. Alternatively, an air electrode for oxygen reduction (ORR) containing a catalyst having ORR catalytic activity can be provided separately from an air electrode for oxygen evolution (OER) containing a catalyst including the material of the present invention. In this case, the metal-air secondary battery has an air electrode for oxygen reduction and an air electrode for oxygen evolution (three-electrode system). The air electrode for oxygen reduction is used during discharge, and the air electrode for oxygen evolution is used during charge. The catalyst having ORR catalytic activity is as described above, and an air electrode for oxygen evolution can be obtained by using this catalyst and the conductive material, binder, etc. described in the description of the air electrode above.

[0052] An example of the configuration of the metal-air secondary battery of the present invention will be described below. The metal-air secondary battery of the present invention is not limited to the following configuration. FIG. 12 is a cross-sectional view showing an example of the metal-air secondary battery of the present invention. The metal-air secondary battery 1 comprises an air electrode 2 using oxygen as an active material, an anode 3 containing an anode active material, an electrolyte 4 for ion conduction between the air electrode 2 and the anode 3, an air electrode current collector 5 for collecting the air electrode 2, and an anode current collector 6 for collecting the anode 3, and these are housed in a battery case (not shown). The air electrode 2 is electrically connected to the air electrode current collector 5 for collecting the air electrode 2, and the air electrode current collector 5 has a porous structure capable of supplying oxygen to the air electrode 2. The anode 3 is electrically connected to the anode current collector 6 for collecting the anode 3, and one of the ends of the air electrode current collector 5 and the anode current collector 6 protrudes from the battery case. They function as a positive electrode terminal (not shown) and a negative electrode terminal (not shown), respectively.

[0053] (Negative electrode) The negative electrode contains a negative electrode active material. The negative electrode active material may be a general air battery negative electrode active material, and is not particularly limited. The negative electrode active material is usually capable of absorbing and releasing metal ions. Specific examples of the negative electrode active material include metals such as Li, Na, K, Mg, Ca, Zn, Al, and Fe, alloys, oxides, and nitrides of these metals, and carbon materials.

[0054] Among them, zinc-air secondary batteries are expected to be the next generation secondary batteries because of their superior safety. From the viewpoint of high voltage and high output, lithium-air secondary batteries and magnesium-air secondary batteries are promising. An example of a zinc-air secondary battery is described below. The reaction formula is as follows: TIFF0007573271000002.tif30153

[0055] In the zinc-air secondary battery of the present invention, a material capable of absorbing and releasing zinc ions is used as the negative electrode. In addition to metallic zinc, a zinc alloy can also be used as such a negative electrode. Examples of the zinc alloy include zinc alloys containing one or more elements selected from aluminum, indium, magnesium, tin, titanium, and copper.

[0056] Examples of the negative electrode active material for the lithium-air secondary battery include metallic lithium; lithium alloys such as lithium aluminum alloys, lithium tin alloys, lithium lead alloys, and lithium silicon alloys; metal oxides such as tin oxide, silicon oxide, lithium titanium oxide, niobium oxide, and tungsten oxide; metal sulfides such as tin sulfide and titanium sulfide; metal nitrides such as lithium cobalt nitride, lithium iron nitride, and lithium manganese nitride; and carbon materials such as graphite. Of these, metallic lithium is preferred.

[0057] Furthermore, a material capable of absorbing and releasing magnesium ions is used as the negative electrode active material of the magnesium-air secondary battery. In addition to metallic magnesium, magnesium alloys such as magnesium aluminum, magnesium silicon, and magnesium gallium can be used as the negative electrode.

[0058] When a foil- or plate-shaped metal, alloy, or the like is used as the negative electrode active material, the foil- or plate-shaped negative electrode active material can be used as the negative electrode itself.

[0059] The negative electrode may contain at least a negative electrode active material, and may contain a binder to fix the negative electrode active material as necessary. The type and amount of the binder are the same as those of the air electrode described above, and therefore will not be described here.

[0060] A negative electrode current collector that collects current from the negative electrode is usually connected to the negative electrode. The material and shape of the negative electrode current collector are not particularly limited. Examples of the material of the negative electrode current collector include stainless steel, copper, nickel, etc. In addition, examples of the shape of the negative electrode current collector include foil, plate, mesh (grid), etc.

[0061] (electrolyte) The electrolyte is disposed between the air electrode and the negative electrode. Metal ion conduction between the negative electrode and the air electrode occurs via the electrolyte. The form of the electrolyte is not particularly limited, and examples thereof include a liquid electrolyte, a gel electrolyte, and a solid electrolyte.

[0062] For example, when the negative electrode is zinc or an alloy thereof, the electrolyte may be an alkaline aqueous solution such as an aqueous potassium hydroxide solution or an aqueous sodium hydroxide solution containing zinc oxide, an aqueous solution containing zinc chloride or zinc perchlorate, or a non-aqueous solvent containing zinc perchlorate or a non-aqueous solvent containing zinc bis(trifluoromethylsulfonyl)imide. For example, when the negative electrode is magnesium or an alloy thereof, a non-aqueous solvent containing magnesium perchlorate or magnesium bis(trifluoromethylsulfonyl)imide may be used. Here, examples of the non-aqueous solvent include organic solvents used in conventional secondary batteries and capacitors, such as ethylene carbonate (EC), propylene carbonate (PC), γ-butyrolactone (γ-BL), diethyl carbonate (DEC), and dimethyl carbonate (DMC). These may be used alone or in combination. Alternatively, an ionic liquid such as N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethylsulfonyl)imide (am) can be used.

[0063] In the secondary battery of the present invention, the electrolyte preferably contains a dendrite formation inhibitor. It is believed that the dendrite formation inhibitor is adsorbed to the negative electrode surface during charging to reduce the energy difference between crystal planes and prevent preferred orientation, thereby suppressing the generation of dendrites. The dendrite formation inhibitor is not particularly limited, and may be, for example, at least one selected from the group consisting of polyalkyleneimines, polyallylamines, and asymmetric dialkylsulfones (see, for example, JP 2009-93983 A). The amount of the dendrite formation inhibitor used is not particularly limited, and may be, for example, an amount sufficient to saturate the electrolyte at room temperature and normal pressure, or may be used as a solvent.

[0064] The liquid electrolyte having lithium ion conductivity is usually a non-aqueous electrolyte solution containing a lithium salt and a non-aqueous solvent. Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6; and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, and LiC(CF3SO2)3.

[0065] Examples of the non-aqueous solvent include ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), butylene carbonate, γ-butyrolactone, sulfolane, acetonitrile, 1,2-dimethoxymethane, 1,3-dimethoxypropane, diethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, and mixtures thereof. Ionic liquids can also be used as the non-aqueous solvent.

[0066] The concentration of the lithium salt in the non-aqueous electrolyte is not particularly limited, but is preferably within the range of, for example, 0.1 mol / L to 3 mol / L, and is preferably 1 mol / L. In the present invention, a low-volatility liquid such as an ionic liquid may be used as the non-aqueous electrolyte.

[0067] A gel electrolyte having lithium ion conductivity can be obtained, for example, by adding a polymer to the non-aqueous electrolyte solution and gelling it. Specifically, the gelling can be achieved by adding a polymer such as polyethylene oxide (PEO), polyvinylidene fluoride (PVDF, Kynar, manufactured by Arkema, etc.), polyacrylonitrile (PAN), or polymethyl methacrylate (PMMA) to the non-aqueous electrolyte solution.

[0068] The solid electrolyte having lithium ion conductivity is not particularly limited, and a general solid electrolyte that can be used in a lithium metal air secondary battery can be used. For example, Li 1.5 Al 0.5 Ge 1.5 Examples of the solid electrolyte include oxide solid electrolytes such as (PO4)3, and sulfide solid electrolytes such as Li2S-P2S5 compounds, Li2S-SiS2 compounds, and Li2S-GeS2 compounds.

[0069] The thickness of the electrolyte varies greatly depending on the configuration of the battery, but is preferably within the range of 10 μm to 5000 μm, for example.

[0070] (Included configuration) In the metal-air secondary battery of the present invention, a separator is preferably disposed between the air electrode and the negative electrode in order to ensure electrical insulation between these electrodes. The separator is not particularly limited as long as it has a structure that can ensure electrical insulation between the air electrode and the negative electrode and allows an electrolyte to be interposed between the air electrode and the negative electrode.

[0071] Examples of the separator include porous membranes such as polyethylene, polypropylene, cellulose, polyvinylidene fluoride, and glass ceramics; and nonwoven fabrics such as resin nonwoven fabrics and glass fiber nonwoven fabrics. Among these, separators made of glass ceramics are preferred.

[0072] In addition, a battery case for a general metal-air secondary battery can be used as the battery case for housing the metal-air secondary battery. The shape of the battery case is not particularly limited as long as it can hold the air electrode, the negative electrode, and the electrolyte described above, but specific examples include a coin type, a flat type, a cylindrical type, a laminate type, and the like.

[0073] The metal-air secondary battery of the present invention can discharge by supplying oxygen, which is an active material, to the air electrode. Examples of the oxygen supply source include air and oxygen gas, and oxygen gas is preferred. The pressure of the air or oxygen gas to be supplied is not particularly limited and may be set appropriately.

[0074] The air electrode catalyst containing the material of the present invention is useful not only for metal-air secondary batteries, but also in other fields where OER electrode catalysts are used. OER electrode catalysts have long been studied and used as counter electrode reactions for various electrochemical reactions, and can be used in alkali metal plating, electrolytic degreasing, and cathodic protection technology. Recently, it is expected that they will be applied to highly efficient and clean hydrogen production technology by combining them with solar cells and photocatalysts. EXAMPLES

[0075] The present invention will be described in more detail below with reference to examples. However, the examples are merely illustrative of the present invention and are not intended to limit the present invention.

[0076] Example 1 Experimental Method Ca2CoFeO 5+δ (CFC) was prepared as follows. Ca(NO3) dihydrate, Co(NO3) dihydrate and Fe(NO3) dihydrate were dissolved in pure water so that the molar ratio of Ca:Co:Fe was 2:1:1, and then an appropriate amount of citric acid was added. The mixture was evaporated to dryness at 120°C and then calcined at 500°C. Finally, the calcined powder was calcined in oxygen at 800°C for 8 hours to produce CFC. The prepared CFC, acetylene black (AB), and Nafion solution were dispersed in ethanol at a weight ratio of CFC:AB:Nafion = 5:1:1 to prepare a catalyst ink, which was then applied to a GC disk (5 mmφ) or a carbon sheet (15 mm x 5 mm, film thickness 0.2 mm) to prepare an electrode. The amount of ink applied was 10 mg cm of CFC catalyst. -2 The carbon sheet used was a water-resistant carbon sheet made by Tokai Carbon.

[0077] Preparation of Co oxide materials The preparation of Co oxide materials by OER polarization for 1 hour and 1 month was carried out using a carbon sheet electrode with Hg / HgO / 4 mol dm -3 In a three-electrode system with KOH as the reference electrode and a platinum plate as the counter electrode, 4 mol dm -3 The experiment was carried out in an aqueous KOH solution under an inert argon atmosphere. -2 The OER polarization was performed for 2 hours under a constant oxidation current condition of 1000 Ω, followed by leaving it for 15 minutes under a zero current condition. The above two steps were alternately repeated for one month, and the polarized material was then collected to obtain a Co oxide material by one-month OER polarization. The 1-hour OER polarization was performed for 1 hour under the same constant oxidation current condition as above, and the polarized material was collected to obtain a Co oxide material.

[0078] In addition, the OER current-voltage curves of the CFC electrodes were measured before and after one month of OER polarization to evaluate the OER activity. -3 In a three-electrode system with KOH as the reference electrode and a platinum plate as the counter electrode, 4 mol dm -3 The ORR and OER measurements were performed in an oxygen-saturated atmosphere and an argon-saturated atmosphere, respectively.

[0079] Comparative Example 1 For comparison, γ-CoOOH was used as a catalyst. γ-CoOOH was prepared by baking commercially available Co(OH)2 at 125°C for 6 hours. γ-CoOOH, AB, and Nafion solutions were dispersed in ethanol at a weight ratio of γ-CoOOH : AB : Nafion = 5: 1 : 1 to prepare a catalyst ink, which was then applied to a GC disk (5 mmφ) to prepare an electrode. The amount of ink applied was 10 mg cm of γ-CoOOH catalyst. -2 The electrode was adjusted to be 0.01 to 0.01. The OER and ORR polarization curves were measured using this electrode, and the activity was evaluated. The polarization measurement was performed with Hg / HgO / 4 mol dm -3 A three-electrode system was used, with KOH as the reference electrode and a platinum plate as the counter electrode. -3 The ORR and OER measurements were performed in an oxygen-saturated atmosphere and an argon-saturated atmosphere, respectively.

[0080] Test Example 1 The composition of the CFC particles on the CFC electrode before and after one month of OER polarization was analyzed by Auger spectroscopy. Spectroscopic measurements were performed using a JEOL-2000A, and the electron beam probe system was narrowed to about 10 nm to evaluate a single CFC particle exposed on the electrode surface. The obtained spectrum was fitted based on the X-ray emission efficiency and emission energy of each element to determine the surface composition.

[0081] In addition, the CFC electrodes before and after one month of OER polarization were subjected to EXAFS measurements at the BL28XU line of Spring 8. The measurements were performed by the transmission method.

[0082] (1) High-resolution TEM image (formation and particle size of Co oxide nanoclusters) Figure 1 shows high-resolution TEM images of the CFC catalyst before and after polarization when the CFC was applied to a GC electrode and polarized for 1 hour at 1.6 V vs RHE. The sample before polarization had clear lattice fringes corresponding to the 110 spacing of the Brownmiller phase, and the electron diffraction also showed spots corresponding to the Brownmiller structure, indicating that a highly crystalline sample had been obtained. On the other hand, the bulk crystal structure of the sample polarized for 1 hour was clearly broken, and it was found to have transitioned to an amorphous phase. Combined with the results of potentiostatic polarization, it was confirmed that the OER activity of CFC was expressed not by the Brownmiller phase of the starting material, but by the amorphous phase formed during anodic polarization. The TEM image shows that this amorphous phase has a clearly heterogeneous structure, with nanoclusters of about 0.5-2 nm dispersed in the amorphous matrix. Furthermore, the nanoclusters showed the characteristics of an ordered structure, and in the selected-area electron diffraction, in addition to the halo derived from the amorphous phase, clear rings were observed.

[0083] (2) Voltage-time curve (stability of Co oxide nanoclusters) Figure 2 shows the voltage-time curves obtained when the electrode was repeatedly polarized at a constant current for one month. The potential gradually increased from 1.6 to 1.8 V vs RHE for 20 hours after the start of the current flow, but then remained constant for one month. This initial increase in potential was confirmed to be an overpotential increase caused by poor conduction to the CFC due to the oxidative consumption of the AB particles. Therefore, it was confirmed that the OER activity of the nanoclustered CFC did not deteriorate even after the OER reaction was carried out continuously for one month, demonstrating its excellent durability.

[0084] (3) XRD pattern Figure 3 shows the XRD patterns after polarization for one hour and one month. The peaks of the Brown-mirror structure that appeared in the sample before polarization (As prepared) completely disappeared after polarization for one hour and one month, and no peaks other than those of the carbon sheet appeared. Therefore, it was confirmed that the nanoclustered CFC after anodic polarization for one hour and one month was basically in an amorphous phase and did not contain crystal particles larger than 10 nm, which would be expected to show XRD peaks.

[0085] (4) Auger spectroscopy (chemical composition and structure of Co oxide nanoclusters) Table 1 shows the results of the composition analysis of the sample particles by Auger spectroscopy before and after one month of OER polarization. In both cases, a C signal derived from Nafion is seen at around 240 eV. After one month of electrolysis, the Ca signal at around 300 eV has clearly disappeared, and the Fe signal at around 600 eV has also become very weak. On the other hand, a mixed signal of F, Co, and Fe appears between 640 and 800 eV, but its intensity seems to have hardly changed. Here, the F signal is thought to be derived from Nafion. Furthermore, an increase in the K signal is observed after one month of testing, which is considered to have been introduced when the Nafion protons were exchanged. The composition of the material particles before and after OER polarization was determined by fitting to each spectrum. The results are summarized in Table 1.

[0086] [Table 1]

[0087] The CFC particles before one month of OER polarization showed a composition close to the Ca / Fe / Co ratio of the Brownmiller-type phase starting material, i.e., 2 / 1 / 1. On the other hand, it can be seen that the Co oxide material of the present invention prepared by one month of OER polarization has almost completely lost Ca and Fe. In other words, it was shown that Ca and Fe were dissolved during polarization in the CFC, and it was almost converted into an oxide or hydrated oxide mainly composed of Co.

[0088] This chemical composition is obtained when the amorphous matrix disappears and the nanoclusters remain, and the influence of the amorphous matrix being mixed in is eliminated. The chemical composition of the Co oxide nanoclusters immediately after generation (1 hour after polarization) is also considered to be similar to this composition based on the voltage-time curve results, EXAFS fitting results, and OER current-voltage curves.

[0089] (5) EXAFS measurements To investigate the structure of the amorphous phase of the Co oxide material prepared by OER polarization for 1 hour and for 1 month, we measured the EXAFS of the samples before and after OER polarization at BL28XU in Spring8 to investigate the local structure around Fe and Co. The results are shown in Figure 5. The radial distribution function around Fe and Co changed significantly after polarization for 1 month, and it can be seen that the bulk structure changes as in TEM. The periodicity of the Fe local structure was decreased by polarization, and only the coordination sphere (1.6 Å) corresponding to the nearest oxygen was observed. On the other hand, the symmetry of the Co local structure was rather improved after polarization, and a new peak appeared around 2.4 Å, indicating the formation of a second coordination sphere. This suggests that the amorphization during the OER reaction leads to the formation of Co oxide clusters with a periodic structure.

[0090] Therefore, we performed fitting to EXAFS based on the crystal data of various Co oxides, hydroxides and oxyhydroxides, and found that the EXAFS vibration of the polarized sample could be well fitted with the crystal model of γ-CoOOH. The fitting results are shown in Figure 5(d) and Table 2. γ-CoOOH has a layered structure in which [CoO2] planar monolayers formed by edge-sharing of CoO6 octahedra are stacked on the c-axis by hydrogen bonds mediated by protons (Figure 6). Therefore, it was shown that the Co oxide material of the present invention causes atomic rearrangement by OER, forming Co-rich oxide parts in the oxide matrix, which form an array structure very similar to that of γ-CoOOH. In other words, it was determined that the nanocluster observed by high-resolution TEM in Figure 1 is a nanocluster having this γ-CoOOH type array structure or an array structure similar to it.

[0091] Furthermore, the EXAFS fitting results show that the oxygen coordination number around Co is 5.1 in the case of one-hour polarization and about 5.3 in the case of one-month polarization (Table 2). On the other hand, the Co coordination number in a [CoO2] planar monolayer with no oxygen vacancies is 6. Therefore, the nanoclusters formed in the Co oxide material of the present invention are [CoO 1.8 ] is considered to be a material having a basic skeleton of a planar monolayer. On the other hand, since no XRD peak of γ-CoOOH appears in the results of Figure 3, it is considered that this nanocluster has a certain degree of stacking in the c-axis direction, as inferred from the particle diameter observed in the TEM image, but is not developed. Therefore, the nanocluster formed in the Co oxide material of the present invention has some stacking in the direction perpendicular to the plane, but this stacking is not very developed. 1.8 ] planar monolayer and [CoO 1.8 H y ] n It was identified as a molecular layer sheet material.

[0092] Based on the γ-CoOOH structure, there are six Co atoms at a distance of approximately 2.8 Å in the second coordination sphere of the Co atom. On the other hand, according to the EXAFS fitting results (Table 2), the coordination number of the second coordination sphere of Co is approximately four, and therefore, a nanocluster is formed by stacking γ-CoOOH planar molecular layers in which some of the Co atoms are replaced by heteroelements or are missing, via hydrogen bonds. Combined with the above results, this [CoO 1.8 H y ] n It was suggested that some of the Co in the molecular layer sheets was replaced by Fe.

[0093] [Table 2]

[0094] (6) OER current-voltage curve (characteristics of Co oxide nanoclusters) Figure 7 shows the OER current-voltage curves of the CFC sample and γ-CoOOH powder before and after one month of OER reaction. The curves are almost the same before and after one month of polarization, confirming that the OER activity has not changed at all. Furthermore, at 5 mA cm -2 If the onset potential of OER is defined as the time when the current flows, the onset potentials of the nanoclustered CFC and γ-CoOOH powders after one month of polarization are 1.47 V vs RHE and 1.58 V vs RHE, respectively, and the OER current value at 1.6 V vs RHE is 100 mA cm. -2 and 12 mA cm -2 Therefore, the nanoclustered CFC showed much higher activity than γ-CoOOH. From the above, it is suggested that high activity cannot be obtained simply by having a γ-CoOOH type structure, and that the size of the structure must be on the order of several nm in order to show high activity. Furthermore, it is suggested that the substitution of part of Co with Fe is also effective.

[0095] Example 2 (1) Preparation of Fe- or Ni-doped CoOOH The preparation of Fe-doped CoOOH and Ni-doped CoOOH was carried out by the coprecipitation method. Co(NO3)3·6H2O and Fe(NO3)3·6H2O or Ni(NO3)3·6H2O were mixed and dissolved in pure water at a specified molar ratio to give a solution with a metal ion concentration of 0.2 M (Co+Fe or Co+Ni) of 50 cm 3 The mixture was then stirred at 200 rpm while 50 cm of 2M KOH solution was added. 3 The hydroxide precipitate was obtained by filtration. 3 After washing twice with 1000 ml of pure water, the mixture was dried under reduced pressure at room temperature overnight. Finally, it was calcined at 120 °C for 6 h in an O2 stream to obtain oxyhydroxide Fe, which is γCoOOH in which Co is replaced by Fe. 0.05 Co 0.95 O x H y , Fe 0.1 Co 0.9 O x H y and Ni 0.1 Co 0.95 O x H y (Hereafter, these will be referred to as Fe-dope CoOOH or Ni-dope CoOOH.)

[0096] (2) Elemental analysis To investigate the Fe / Co or Ni / Co ratio of the obtained powder, the powder was dissolved in 0.1M KCl solution and analyzed by ICP. The metal composition ratios were consistent with the values ​​of the starting materials.

[0097] (3) BET specific surface area The BET specific surface area of ​​the obtained powder was measured and found to be Fe 0.05 Co 0.95 O x H y , Fe 0.1 Co 0.9 O x H y and Ni 0.1 Co 0.95 O x H y are 86, 75, and 61 m, respectively.2 g -1 These BET specific surface areas were an order of magnitude higher than those of ordinary ceramics with micrometer-sized particles, suggesting that the powder obtained was a nanoparticulate material.

[0098] (4) OER activity of Fe-doped CoOOH and Ni-doped CoOOH electrodes A carbon mixed electrode was prepared in the same manner as in Example 1, and measured in 4M KOH. That is, acetylene black (AB) and Nafion solution were dispersed in ethanol in a weight ratio of Fe-dope CoOOH or Ni-dope CoOOH:AB:Nafion = 5:1:1 to prepare a catalyst ink, which was then applied to a GC disk (5 mmφ) or a carbon sheet (15 mm x 5 mm, film thickness 0.2 mm) to prepare an electrode. The amount of ink applied was 10 mg cm of Fe-dope CoOOH or Ni-dope CoOOH. -2 It was adjusted so that (5) XRD Fe prepared in (1) above 0.05 Co 0.95 O x H y , Fe 0.1 Co 0.9 O x H y and Ni 0.1 Co 0.95 O x H y The XRD pattern of γ-CoOOH is also shown in Fig. 8. 0.05 Co 0.95 O x H y , Fe 0.1 Co 0.9 O x H y and Ni 0.1 Co 0.95 O x H yAll of the oxyhydroxides showed the same XRD patterns as γ-CoOOH, confirming that they had a γ-CoOOH type layered structure. The XRD patterns of the three oxyhydroxides were very broad, and the crystallite sizes were therefore estimated to be about 8-15 nm based on the half-width of the 002 peak at around 20°. (5)OER Fe prepared in (1) above 0.05 Co 0.95 O x H y , Fe 0.1 Co 0.9 O x H y and Ni 0.1 Co 0.95 O x H y The OER polarization curves of the two are shown in Fig. 9. In all cases, the current rises from 1.45 V vs. RHE and reaches 5 mA cm at 1.47, 1.46, and 1.49 V vs. RHE, respectively. -2 The current value reached 120 mA cm at 1.6 V vs RHE. -2 The above current was shown. (6) As described above, the Fe- or Ni-dope γ-CoOOH type nanocrystalline materials prepared by the coprecipitation method in this embodiment exhibited structures and activities equivalent to those of the CFC shown in Example 1.

[0099] Example 3 As in Example 1, Ca2CoFeO 5+δ (CFC) was prepared, immersed in 4M KOH and subjected to airtight Ar bubbling at 50°C for 3 days. It was then thoroughly washed with Milli-Q water. The sample was filtered to obtain the Ca / Fe / Co (ICP emission analysis) of the KOH-treated sample was 0.03 / 0.21 / 0.76. The BET value measured before the KOH treatment was 2.92 m. 2 g -1 After the KOH treatment, the value increased by about 80 times to 230. The XRD of the sample (CFC) before the KOH treatment and the KOH-treated sample are shown in Figure 10, and the OER polarization curve is shown in Figure 11. The EXAFS of the KOH-treated sample was similar to that of the 1-hour OER polarization sample in Figure 5 of Example 1.

[0100] The results of the EXAFS fitting are shown in Table 3 below. From the results in this table, it can be seen that the KOH-treated sample is also a nanocluster with a γ-CoOOH type structure or a similar arrangement structure.

[0101] [Table 3] [Industrial Applicability]

[0102] INDUSTRIAL APPLICABILITY The present invention is useful in the fields of secondary batteries, metal-air secondary batteries which are expected to be the next-generation high-capacity secondary batteries, water electrolysis, and hydrogen production by photochemical water decomposition.

Claims

1. A Co oxide material, which is a Co oxide nanocluster having an atomic arrangement structure identical or similar to a γ-CoOOH type atomic arrangement structure and having oxygen defects, and in which a part of Co in the nanocluster may be substituted with Fe and / or Ni. (However, it is an amorphous oxygen-non-deficient or oxygen-deficient transition metal oxide containing one or more elements selected from the following Group A, one or more elements selected from Group B, and cobalt, However, group A consists of Ca, Sr, Ba and rare earth elements (RE), Group B consists of the 3d transition elements other than Co. and in which a cluster structure having a particle size in the range of 0.1 to 10 nm is observed under high-resolution transmission electron microscope observation, the cluster structure portion having a γ-CoOOH type element arrangement structure or an element arrangement structure similar thereto is excluded.

2. The material of claim 1 , wherein the Co oxide nanoclusters have a particle size of 10 nm or less.

3. Chief of Staff 6 Octahedrons are connected two-dimensionally by edge-sharing to form [CoO x ] Planar monolayer with protons for charge compensation [CoO x H y ] Planar monolayers are stacked in n layers [CoO x H y ] n A Co oxide material containing nanoclusters of molecular layer sheet-like substances, where x is in the range of 1.5 to 2.0, y is in the range of 0.01 to 1, n is the number of stacks of the planar monolayer in the direction perpendicular to the molecular layer plane (c-axis direction) and is in the range of 1 to 25, and [CoO x H y ] A part of Co in the planar monolayer may be replaced by Fe and / or Ni, and CoO 6The material may have some oxygen vacancies in the octahedrons (provided that the material is an amorphous oxygen-non-vacant or oxygen-deficient transition metal oxide containing one or more elements selected from the following Group A, one or more elements selected from Group B, and cobalt, However, group A consists of Ca, Sr, Ba and rare earth elements (RE), Group B consists of the 3d transition elements other than Co. and in which a cluster structure having a particle size in the range of 0.1 to 10 nm is observed under high-resolution transmission electron microscope observation, the cluster structure portion having a γ-CoOOH type element arrangement structure or an element arrangement structure similar thereto is excluded.

4. [CoO x H y ] The material of claim 3, wherein one side of the planar monolayer is 10 nm or less.

5. The material according to any one of claims 1 to 4, wherein the maximum outer diameter of the nanoclusters observed in the TEM images is in the range of 0.3 to 10 nm.

6. The material according to any one of claims 1 to 5, wherein a portion of Co in the nanoclusters is substituted with Fe and / or Ni.

7. The material according to claim 6, wherein the substitution amount of Co with Fe and / or Ni is in the range of 100:0.1 to 10, as determined by Auger spectroscopy analysis or by elemental analysis using ICP analysis.

8. The material according to any one of claims 1 to 7 for use as an OER catalyst.

9. 8. A method for producing the material according to any one of claims 1 to 7, comprising the steps of: adding an alkali to an aqueous solution containing an Fe salt and / or Ni salt, and a Co salt to precipitate a hydroxide containing Fe and / or Ni, and Co, and recovering the precipitate; and calcining the precipitate of the hydroxide containing Fe and / or Ni, and Co in an oxygen-containing atmosphere to obtain an oxyhydroxide containing Fe and / or Ni, and Co.

10. 10. The method according to claim 9, wherein the Fe salt, Ni salt and Co salt are each a nitrate, and the alkali is an alkali metal hydroxide.

11. A catalyst for an air electrode comprising the material according to any one of claims 1 to 7.

12. A catalyst for a water electrolysis anode comprising the material according to any one of claims 1 to 7.

13. An air electrode for a metal-air secondary battery comprising the catalyst according to claim 11 or 12.

14. The cathode of claim 13 , wherein the material is included as an oxygen evolution catalyst and further includes an oxygen reduction catalyst.

15. 15. A metal-air secondary battery comprising: the air electrode according to claim 13; a negative electrode containing a negative electrode active material; and an electrolyte interposed between the air electrode and the negative electrode.

16. The metal-air secondary battery according to claim 15, further comprising an oxygen reduction air electrode containing an oxygen reduction catalyst.

Citation Information

Patent Citations

  • Hydrogen gas generation device, and hydrogen gas suction apparatus including the same

    JP2018165396A

  • Catalyst for air electrode for metal / air secondary battery, and air electrode

    WO2015115592A1

  • Amorphous transition metal oxide and use thereof

    WO2019093441A1