Laminate for patch

The laminate for a patch with a central stretchable hot melt resin layer addresses the issue of widening by maintaining width, ensuring conformity to the affected area through a thermoplastic resin and plasticizer composition.

JP7573480B2Active Publication Date: 2024-10-25SEKISUI FULLER CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021074371
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-26
Publication Date
2024-10-25
Estimated Expiration
2041-04-26

AI Technical Summary

Technical Problem

Conventional medicinal patches experience widening near the center when stretched, leading to a reduction in width, which is not adequately addressed by existing support layers.

Method used

A laminate for a patch is designed with a stretchable hot melt resin layer on the support layer, specifically in the central area excluding 10% from both ends, providing a stress of 0.20 N/mm at 75% elongation, composed of a thermoplastic resin like styrene block copolymer and a plasticizer, to prevent narrowing.

Benefits of technology

The laminate effectively suppresses width reduction and ensures the patch conforms to the shape of the affected area by maintaining width even when stretched.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573480000002
    Figure 0007573480000002
  • Figure 0007573480000003
    Figure 0007573480000003
  • Figure 0007573480000004
    Figure 0007573480000004
Patent Text Reader

Abstract

To provide laminates for patches for manufacturing patches suppressed in width, in which the width is prevented from narrowing even if the center of the patch stretches when the patch is attached to an affected area.SOLUTION: There is provided a laminate for patches having an elastic hot-melt resin layer on at least a part of one side of a support layer, in which the elastic hot-melt resin layer is formed at least in the central portion of the support layer, which is an area other than the area of 10% from both ends in a TD direction of the support layer based on the area on which the elastic hot-melt resin layer is formed as 100%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate for a patch. [Background technology]

[0002] Conventionally, patches have been used as external medicines. By applying the patch to the affected skin surface, the patch gives a cooling or warming sensation to the skin surface while administering the active ingredient contained in the paste layer to the human body by transdermal absorption. The patch is formed by laminating a paste layer and a support layer that supports the paste layer.

[0003] A patch is required to conform to the shape of the affected area. As a support layer for such a patch that shows conformability to the shape of the affected area, a medicinal patch base sheet containing paraffin oil, styrene elastomer, and linear low-density polyethylene that exhibit specific properties has been proposed (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-102358 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when using the above-mentioned patch, there is a problem that the width narrows as the center of the patch stretches when the patch is applied to the affected area, which is called width narrowing. Patent Document 1 does not consider width narrowing, and the base sheet for medicinal patches described in Patent Document 1 has a problem that width narrowing cannot be suppressed.

[0006] In view of the above circumstances, the present invention has an object to provide a laminate for a patch, which is capable of suppressing narrowing in width even if the patch stretches near the center when the patch is applied to an affected area, and which is used to produce a patch in which width narrowing is suppressed. [Means for solving the problem]

[0007] As a result of extensive investigations into achieving the above-mentioned object, the present inventors have found that the above-mentioned object can be achieved by a laminate for a patch having an elastic hot-melt resin layer on at least a portion of one side of a backing layer, in which the elastic hot-melt resin layer is formed at least in the central portion, which is a region other than 10% of the area from each end of the backing layer in the TD direction, assuming that the area of ​​the surface of the backing layer on which the elastic hot-melt resin layer is formed is 100%, and have thus completed the present invention.

[0008] That is, the present invention relates to the following laminate for a patch: 1. A laminate for a patch having an elastic hot melt resin layer on at least a portion of one side of a backing layer, The elastic hot melt resin layer is formed at least in a central portion of the support layer, which is a region other than a region having an area of ​​10% from each end of the support layer in the TD direction, with the area of ​​the surface of the support layer on which the elastic hot melt resin layer is formed being 100%. 1. A laminate for a patch comprising: 2. The laminate for a patch according to item 1, wherein the support layer has a shape defined by points ABCD, and the central portion is defined by point abcd on a side parallel to the TD direction, the side being 1 / 10 the length of the side from the four points ABCD of the support layer. 3. The elastic hot melt resin composition forming the elastic hot melt resin layer has a stress of 0.20 N / mm at 75% elongation. 2 Item 3. The laminate for a patch according to item 1 or 2, which is as described above. 4. The elastic hot melt resin composition forming the elastic hot melt resin layer has a stress of 0.20 N / mm at 75% elongation. 2 More than 1.00N / mm 2 Item 4. The laminate for a patch according to any one of Items 1 to 3, which is as follows: 5. The laminate for a patch according to any one of items 1 to 4, wherein the stretchable hot melt resin layer contains a thermoplastic resin (A) and a plasticizer (B), and the thermoplastic resin (A) is a styrene-based block copolymer. 6. A patch comprising the laminate for a patch according to any one of items 1 to 5, and further comprising a paste layer formed on the laminate. 7. The patch according to item 6, wherein the ratio (Sh / Ss) of the measured value (Sh) of the stretchable hot-melt resin layer measured by the measurement method described below to the measured value (Ss) of the laminate comprising the support layer and the paste layer measured by the measurement method described below is 0.5 or less. [Method of measuring (Sh)] Using a tensile tester, the tensile strength of the elastic hot melt resin layer is measured under the measurement conditions of a tensile speed of 300 mm / min and 75% elongation, and this is taken as (Sh). [Method of measuring (Ss)] A 10% area region from each end of the laminate in the TD direction in which the support layer and the paste layer are laminated is fixed by a tensile tester, and the laminate is stretched by 75% at a tensile speed of 300 mm / min to measure the tensile force (Ss). Effect of the Invention

[0009] The laminate for a patch of the present invention is prevented from narrowing in width even if the central portion of the patch stretches when the patch is applied to an affected area, and thus width contraction is suppressed. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic plan view showing an example of a laminate for a patch of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of a laminate for a patch of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of a laminate for a patch of the present invention. [Figure 4] FIG. 1 is a schematic plan view showing an example of a laminate for a patch of the present invention. [Diagram 5] FIG. 1 is a schematic cross-sectional view showing an example of a laminate for a patch of the present invention. [Figure 6] FIG. 1 is a schematic plan view showing an example of a laminate for a patch of the present invention. [Figure 7] FIG. 1 is a schematic cross-sectional view showing an example of a laminate for a patch of the present invention. [Figure 8] FIG. 2 is a cross-sectional view showing an example of a patch formed using the laminate for a patch of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] 1.Laminate for patch The patch laminate of the present invention is a patch laminate having an elastic hot melt resin layer on at least a part of one side of a support layer, and the elastic hot melt resin layer is formed at least in the center, which is a region other than the region of 10% area from both ends of the support layer in the TD direction, assuming the area of ​​the surface of the support layer on which the elastic hot melt resin layer is formed as 100%. The patch laminate of the present invention has an elastic hot melt resin layer in the center, which is a region other than the region of 10% area from both ends of the support layer in the TD direction, assuming the area of ​​the surface of the support layer on which the elastic hot melt resin layer is formed as 100%, i.e., in a location of a certain area or more including the center of the support layer, so that the contraction in the width direction near the center of the support layer is suppressed by the elastic hot melt resin layer, and width insertion can be suppressed.

[0012] The laminate for a patch of the present invention will be described with reference to the drawings. FIG. 1 is a schematic plan view showing an example of the laminate for a patch of the present invention, and FIG. 2 is a schematic cross-sectional view showing an example of the laminate for a patch of the present invention. In FIG. 1 and FIG. 2, the laminate for a patch 1 of the present invention has an elastic hot melt resin layer 12 on a part of one side of a support layer 11. The elastic hot melt resin layer 12 is formed in the center, which is a region other than a region 11S having an area of ​​10% from two sides 111md parallel to the MD direction of the support layer 11, which are both ends in the TD direction, assuming that the area of ​​the surface on which the elastic hot melt resin layer 12 is formed is 100%. In FIG. 1 and FIG. 2, the support layer 11 has a shape specified by points ABCD, and the center is a quadrangular region specified by points abcd on a side 111td parallel to the TD direction, which is 1 / 10 the length of the side, from four points ABCD of the support layer. In Figs. 1 and 2, an elastic hot melt resin layer 12 is formed in the central portion.

[0013] The laminate for a patch of the present invention may have an elastic hot-melt resin layer on at least a part of one side of the support layer as shown in Figures 1 and 2, but may be provided on both sides of the support layer 11 as shown in Figure 3. Even in this case, the elastic hot-melt resin layer 12 is formed at least in the central portion of each side, which is a region other than the region 11s having an area of ​​10% from both ends 111md in the TD direction of the support layer 11, with the surface area (one side) of the support layer 11 being 100%.

[0014] In Figures 1 to 3, the elastic hot-melt resin layer is formed in the shape of three stripes in the central portion, but in the laminate for patch of the present invention, the elastic hot-melt resin layer may be formed in the shape of a single thick stripe as shown in Figures 4 and 5.

[0015] The patch laminate of the present invention only needs to have an elastic hot-melt resin layer on at least a portion of one side of the support layer, and may have an elastic hot-melt resin layer 12 on the entire surface of the support layer 11, as shown in Figures 6 and 7.

[0016] The layer structure of the patch laminate of the present invention may be such that at least one side of the support layer has an elastic hot-melt resin layer, and may be, for example, a two-layer structure of support layer / elastic hot-melt resin layer, or a three-layer structure of support layer / elastic hot-melt resin layer / support layer.

[0017] <Elastic hot melt resin layer> The stretchable hot melt resin layer is not particularly limited as long as it has stretchability and can suppress the width of the patch.

[0018] The stress at 75% elongation of the elastic hot melt resin composition forming the elastic hot melt resin layer is 0.20 N / mm 2 More than 0.30N / mm is preferable. 2 The stress at 75% elongation of the elastic hot melt resin composition is preferably 1.00 N / mm 2 Less than 0.90N / mm is preferable. 2 Less than 0.80N / mm is more preferable. 2 The following is even more preferable. By setting the lower limit of the stress at 75% elongation within the above range, the patch can be further prevented from becoming wider. Also, by setting the upper limit of the stress at 75% elongation within the above range, the patch can more easily conform to the shape of the affected area.

[0019] In this specification, the stress of the elastic hot melt resin layer at 75% elongation is measured by the following measurement method. That is, the elastic hot melt resin composition is applied to a release layer, and peeled off to prepare a test piece with a width of 25 mm, a length of 75 mm (measurement area 25 mm), and a thickness of 50 μm. Then, it is fixed in a tensile tester and elongated to 75% at a tensile speed of 300 mm / min to measure the stress. In addition, as the tensile tester, for example, AGS-X manufactured by Shimadzu Corporation can be used.

[0020] The measured value (Sh) of the elastic hot melt resin layer measured by the following measuring method is preferably 0.2 N or more, more preferably 0.4 N or more, and even more preferably 0.5 N or more. By having the lower limit of (Sh) within the above range, the patch can be further prevented from entering the width. Furthermore, the measured value (Sh) of the elastic hot melt resin layer is preferably 7.0 N or less, more preferably 5.0 N or less. By having the upper limit of the measured value (Sh) of the elastic hot melt resin layer within the above range, the patch can more easily conform to the shape of the affected area, and peeling from the affected area can be prevented.

[0021] [Method of measuring (Sh)] The tensile strength of the elastic hot melt resin layer is measured using a tensile tester under the measurement conditions of a tensile speed of 300 mm / min and 75% elongation, and is defined as (Sh). Note that, as the tensile tester, for example, AGS-X manufactured by Shimadzu Corporation can be used.

[0022] In the above-mentioned method for measuring (Sh), when the elastic hot melt resin layer is formed at multiple locations on the surface of the support layer, the (Sh) of the elastic hot melt resin layer at each location is measured and added together to obtain the (overall) (Sh) of the elastic hot melt resin layer. In addition, when it is difficult to peel the elastic hot melt resin layer from the support layer and the composition of the elastic hot melt resin composition for forming the elastic hot melt resin layer is known, the elastic hot melt resin composition may be applied to a release layer, peeled off, and a test piece having the same shape (width, length, thickness) as the elastic hot melt resin layer may be prepared, and (Sh) may be measured by the above-mentioned method.

[0023] The thickness of the elastic hot melt resin layer is preferably 25 μm or more, more preferably 35 μm or more, and even more preferably 50 μm or more. The thickness of the elastic hot melt resin layer is preferably 500 μm or less, more preferably 400 μm or less, and even more preferably 300 μm or less. By setting the lower limit of the thickness of the elastic hot melt resin layer within the above range, the width of the patch can be further suppressed. By setting the upper limit of the thickness of the support layer within the above range, the patch can more easily follow the shape of the affected area.

[0024] The elastic hot-melt resin composition forming the elastic hot-melt resin layer is not particularly limited as long as it has elasticity and can suppress the patch from entering the width direction.

[0025] The elastic hot melt resin layer contains a thermoplastic resin (A) and a plasticizer (B), and the thermoplastic resin (A) is preferably a styrene-based block copolymer. In the following description, the composition and content of the elastic hot melt resin layer are the same as the composition and content of the elastic hot melt resin composition that forms the elastic hot melt resin layer.

[0026] (Thermoplastic resin (A)) The thermoplastic resin (A) is not particularly limited as long as it can suppress the patch from being widened, and a thermoplastic elastomer is preferred in that the patch can more easily follow the shape of the affected area. In addition, a reactive thermoplastic resin can be used as the thermoplastic resin (A). An example of such a reactive thermoplastic resin is a thermoplastic resin containing a styrene-based block copolymer having a reactive polystyrene-based hard block in the molecule of the thermoplastic resin. By using such a thermoplastic resin and further containing a photopolymerization initiator, the elastic hot melt resin composition can be irradiated with light such as ultraviolet light to react the reactive polystyrene-based hard block, crosslinking the molecules, and adjusting the properties such as dynamic viscoelasticity of the elastic hot melt resin composition.

[0027] Examples of the thermoplastic elastomer include styrene-based block copolymers, olefin-based block copolymers, olefin-based random copolymers, urethane-based block copolymers, and polyester-based block copolymers. Among these, styrene-based block copolymers are preferred, and in particular, those containing a hydrogenated styrene-based block copolymer are more preferred. The hydrogenated styrene-based block copolymer refers to a block copolymer obtained by block copolymerizing a vinyl aromatic hydrocarbon with a conjugated diene compound, and hydrogenating all or a part of the blocks based on the conjugated diene compound in the resulting block copolymer.

[0028] Vinyl aromatic hydrocarbons are aromatic hydrocarbon compounds having vinyl groups.Specific examples of vinyl aromatic hydrocarbons include styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 1,3-dimethylstyrene, α-methylstyrene, vinylnaphthalene, vinylanthracene, etc., and among these, styrene is preferred.Vinyl aromatic hydrocarbons may be used alone or in combination of two or more.

[0029] The conjugated diene compound is a diolefin compound having at least one pair of conjugated double bonds.Specific examples of the conjugated diene compound include 1,3-butadiene, 2-methyl-1,3-butadiene (or isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene, and among these, 1,3-butadiene and 2-methyl-1,3-butadiene are preferred.The conjugated diene compound may be used alone or in combination of two or more.

[0030] In this specification, the hydrogenation ratio in a hydrogenated thermoplastic block copolymer, such as a hydrogenated product of a styrene-based block copolymer, is indicated by the "hydrogenation ratio". The "hydrogenation ratio" of a hydrogenated thermoplastic block copolymer refers to the ratio of ethylenically unsaturated double bonds that have been hydrogenated and converted to saturated hydrocarbon bonds, based on the total ethylenically unsaturated double bonds contained in the block based on a conjugated diene compound. The hydrogenation ratio can be measured by an infrared spectrophotometer, a nuclear magnetic resonance apparatus, or the like.

[0031] The hydrogenated styrene block copolymer may be a partially hydrogenated or fully hydrogenated product. Of these, a fully hydrogenated product is preferred. When the hydrogenated styrene block copolymer is fully hydrogenated, the heat stability of the hot melt composition is further improved. The hydrogenation rate of the hydrogenated styrene block copolymer is preferably about 100%.

[0032] The hydrogenated product of the styrene-based block copolymer is not particularly limited, and includes styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-butylene-butadiene-styrene copolymer (SBBS), styrene-ethylene-butylene / styrene-styrene copolymer (SEB / SS), styrene-ethylene-propylene-styrene copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS), styrene-ethylene-butylene-olefin crystal copolymer (SEBC), etc. By using the above-mentioned thermoplastic elastomer as the thermoplastic resin (A), the width of the patch can be further suppressed, and the patch can be more easily adapted to the shape of the affected area. Among these, styrene-ethylene-butylene-styrene copolymer and styrene-ethylene-butylene / styrene-styrene copolymer are preferred.

[0033] The hydrogenated styrene block copolymers may be used alone or in combination of two or more.

[0034] The styrene-ethylene-butylene-styrene copolymer (SEBS) is a copolymer in which the terminal styrene units form an end block phase and the ethylene-butylene units form a mid block phase. By using a copolymer in which the mid block phase is a hydrogenated ethylene-butylene unit, the polarity difference with the styrene units in the end block phase becomes more pronounced, and the styrene units in the end block phase become stronger than in a copolymer in which the mid block phase is not hydrogenated.

[0035] The styrene-ethylene-butylene-styrene copolymer may be a reactive styrene-ethylene-butylene-styrene copolymer containing a styrene-based block copolymer having a reactive polystyrene-based hard block in the molecule of the thermoplastic resin. By using a reactive styrene-ethylene-butylene-styrene copolymer and further containing a photopolymerization initiator, the elastic hot melt resin composition can be irradiated with light such as ultraviolet light to react the reactive polystyrene-based hard block and crosslink the molecules, thereby adjusting the properties such as dynamic viscoelasticity of the elastic hot melt resin composition. As such a reactive styrene-ethylene-butylene-styrene copolymer, a commercially available product can be used, and examples of the commercially available product include Septon V9827 manufactured by Kuraray Co., Ltd.

[0036] The styrene content of the styrene-ethylene-butylene-styrene copolymer is preferably 15% by mass or more, more preferably 20% by mass or more, based on 100% by mass of the styrene-ethylene-butylene-styrene copolymer. The styrene content of the styrene-ethylene-butylene-styrene copolymer is preferably 45% by mass or less, more preferably 40% by mass or less, based on 100% by mass of the styrene-ethylene-butylene-styrene copolymer. When the styrene content is within the above range, the patch can be further prevented from becoming wider, and the patch can more easily conform to the shape of the affected area.

[0037] In this specification, the "styrene content" of a styrene-based block copolymer refers to the content (mass %) of the styrene block in the styrene-based block copolymer.

[0038] In the present specification, the method for calculating the styrene content in the styrene-based block copolymer is not particularly limited, and examples thereof include a method using proton nuclear magnetic resonance spectroscopy or infrared spectroscopy in accordance with JIS K6239.

[0039] The styrene-ethylene-butylene-styrene copolymer may be a commercially available product, such as G1650 manufactured by Kraton Polymers, MD1648 manufactured by Kraton Polymers, or Tuftec H1041 manufactured by Asahi Kasei Corporation.

[0040] The styrene-ethylene-butylene-styrene copolymer may be used alone or in combination of two or more. For example, a styrene-ethylene-butylene-styrene copolymer having a high styrene content and a styrene-ethylene-butylene-styrene copolymer having a low styrene content may be used in combination. When two or more types are used in combination, the styrene content of the entire styrene-ethylene-butylene-styrene copolymer may be calculated as an average value based on weight.

[0041] The styrene-ethylene-butylene / styrene-styrene copolymer (SEB / SS) is a styrene-ethylene-butylene-styrene copolymer in which the terminal styrene units form an end block phase and the ethylene-butylene units form a midblock phase, and in which styrene is also dispersed in the midblock phase. By using a copolymer in which styrene is dispersed in the midblock phase, even if the total styrene content of the styrene block copolymer is increased, the styrene block copolymer does not become too hard and exhibits good extensibility, so that the elastic hot melt resin composition containing the styrene-ethylene-butylene / styrene-styrene copolymer can achieve both good extensibility and improved stress during elongation. Furthermore, by using a styrene-ethylene-butylene / styrene-styrene copolymer in which styrene is dispersed in the midblock phase for the elastic hot melt resin composition, the increase in melt viscosity at low temperatures is suppressed, and the coatability of the elastic hot melt resin composition can be further improved.

[0042] The method for preparing the styrene-ethylene-butylene / styrene-styrene copolymer is not particularly limited, and examples thereof include the method described in US Pat. No. 7,169,848.

[0043] The styrene content of the styrene-ethylene-butylene / styrene-styrene copolymer is preferably 20% by mass or more, more preferably 25% by mass or more, based on 100% by mass of the styrene-ethylene-butylene / styrene-styrene copolymer. The styrene content of the styrene-ethylene-butylene / styrene-styrene copolymer is preferably 60% by mass or less, more preferably 55% by mass or less, based on 100% by mass of the styrene-ethylene-butylene / styrene-styrene copolymer. When the styrene content is within the above range, the patch can be further prevented from becoming wider, and the patch can more easily follow the shape of the affected area.

[0044] As the styrene-ethylene-butylene / styrene-styrene copolymer, commercially available products can be used, such as MD6951 and A1536 manufactured by Kraton Polymers.

[0045] The styrene-ethylene-butylene / styrene-styrene copolymer may be used alone or in combination of two or more. For example, a styrene-ethylene-butylene / styrene-styrene copolymer having a high styrene content and a styrene-ethylene-butylene / styrene-styrene copolymer having a low styrene content may be used in combination. When two or more types are used in combination, the styrene content of the entire styrene-ethylene-butylene / styrene-styrene copolymer may be calculated by the average value based on weight.

[0046] The styrene-ethylene-butylene-olefin crystalline copolymer (SEBC) is a block polymer of styrene-ethylene-butylene-olefin crystal. By using the styrene-ethylene-butylene-olefin crystalline copolymer, the hot melt composition has better elasticity recovery after heating and holding, and the coatability is improved, and the tensile strength and transparency are improved.

[0047] The method for producing the styrene-ethylene-butylene-olefin crystal copolymer is not particularly limited, and it can be produced by the following production method. That is, first, 1,3-butadiene is polymerized using an organolithium initiator, and then 1,3-butadiene is polymerized so that the 1,2-vinyl bond content is 30 to 70%, to produce block-shaped polybutadiene with different 1,2-vinyl bond contents. Next, a vinyl aromatic compound containing 90 mass% or more of styrene is added to the polybutadiene and polymerized to produce a block copolymer before hydrogenation. Next, the block copolymer before hydrogenation is hydrogenated by a known method to produce a styrene-ethylene-butylene-olefin crystal copolymer.

[0048] Examples of vinyl aromatic compounds include styrene, t-butylstyrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylstyrene, N,N-diethyl-p-aminoethylstyrene, and vinylpyridine. Among these, styrene and α-methylstyrene are preferred.

[0049] Examples of organolithium compounds used as organolithium initiators include n-butyllithium, sec-butyllithium, tert-butyllithium, propyllithium, amyllithium, and butyllithium / barium nonylphenoxide / trialkylaluminum / dialkylaminoethanol.

[0050] The styrene content of the styrene-ethylene-butylene-olefin crystal copolymer is preferably 10% by mass or more, more preferably 15% by mass or more, based on 100% by mass of the styrene-ethylene-butylene-olefin crystal copolymer. The styrene content of the styrene-ethylene-butylene-olefin crystal copolymer is preferably 30% by mass or less, more preferably 25% by mass or less, based on 100% by mass of the styrene-ethylene-butylene-olefin crystal copolymer. When the styrene content is within the above range, the patch can be further prevented from becoming wider, and the patch can more easily follow the shape of the affected area.

[0051] As the styrene-ethylene-butylene-olefin crystalline copolymer, a commercially available product can be used, such as DYNARON 4600P manufactured by JSR Corporation.

[0052] The styrene-ethylene-butylene-olefin crystal copolymer may be used alone or in combination of two or more. For example, a styrene-ethylene-butylene-olefin crystal copolymer having a high styrene content and a styrene-ethylene-butylene-olefin crystal copolymer having a low styrene content may be used in combination. When two or more types are used in combination, the styrene content of the styrene-ethylene-butylene-olefin crystal copolymer may be calculated as an average value based on weight.

[0053] The content of the thermoplastic resin (A) in the elastic hot melt resin layer is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 65% ​​by mass or more, based on 100% by mass of the elastic hot melt resin layer. The content of the thermoplastic resin (A) in the elastic hot melt resin layer is preferably 75% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less, based on 100% by mass of the elastic hot melt resin layer. By having the content of the thermoplastic resin (A) in the above range, the width of the patch can be further suppressed, and the patch can more easily follow the shape of the affected area.

[0054] The styrene content of the thermoplastic resin (A) contained in the stretchable hot melt resin layer is preferably 10% by mass or more, more preferably 12% by mass or more, based on 100% by mass of the thermoplastic resin (A). The styrene content of the thermoplastic resin (A) contained in the stretchable hot melt resin layer is preferably 35% by mass or less, more preferably 25% by mass or less, based on 100% by mass of the thermoplastic resin (A). When the styrene content of the thermoplastic resin (A) is within the above range, the width of the patch can be further suppressed, and the patch can more easily follow the shape of the affected area.

[0055] The weight average molecular weight (Mw) of the thermoplastic resin (A) is preferably 30,000 or more, more preferably 40,000 or more, and even more preferably 45,000 or more. The weight average molecular weight (Mw) of the thermoplastic resin (A) is preferably 200,000 or less, more preferably 150,000 or less, and even more preferably 125,000 or less. By having the weight average molecular weight within the above range, the width of the patch can be further suppressed, and the patch can more easily follow the shape of the affected area.

[0056] The weight average molecular weight (Mw) of the thermoplastic resin (A) is a measured value obtained by using a gel permeation chromatography measuring device and converting it into standard polystyrene.

[0057] The weight average molecular weight (Mw) in this specification can be measured, for example, using the following measuring device and under the following measuring conditions. Measurement device: Waters product name "ACQUITY APC" Measurement conditions: Column ·ACQUITY APCXT45 1.7μm×1 piece ·ACQUITY APCXT125 2.5μm×1 piece ·ACQUITY APCXT450 2.5μm×1 piece Mobile phase: Tetrahydrofuran 0.8mL / min Sample concentration: 0.2% by mass Detector: Refractive index (RI) detector Standard material: polystyrene (Waters, molecular weight: 266-1,800,000) Column temperature: 40°C RI detector temperature: 40℃

[0058] (Plasticizer (B)) The stretchable hot melt resin layer may contain a plasticizer (B). The plasticizer (B) is preferably liquid at 23°C. In this specification, "liquid" refers to a state exhibiting fluidity. The pour point of such a plasticizer (B) is preferably 23°C or lower, more preferably 10°C or lower.

[0059] In this specification, the pour point is a value measured by a measurement method in accordance with JIS K2269.

[0060] The plasticizer (B) is not particularly limited, and examples thereof include paraffinic process oil, naphthenic process oil, aromatic process oil, liquid paraffin oil, hydrocarbon synthetic oil, etc. Among them, from the viewpoint of excellent heat stability, paraffinic process oil, naphthenic process oil, liquid paraffin oil, and hydrocarbon synthetic oil are preferred, and from the viewpoint of further suppressing the width of the patch, hydrocarbon synthetic oil is more preferred.

[0061] As the paraffin-based process oil, commercially available products can be used, such as PW-32 and PS-32 manufactured by Idemitsu Kosan Co., Ltd.

[0062] As the naphthenic process oil, commercially available products can be used, such as Diana Fresia N28 manufactured by Idemitsu Kosan Co., Ltd., Diana Fresia U46 manufactured by Idemitsu Kosan Co., Ltd., and Nyflex 222B manufactured by Nynas Corporation.

[0063] As the liquid paraffin oil, commercially available products can be used, such as P-100 manufactured by MORESCO and Kaydol manufactured by Sonneborn.

[0064] As the synthetic hydrocarbon oil, commercially available products can be used, such as LUCANT HC-10 and LUCANT HC-20 manufactured by Mitsui Chemicals.

[0065] The above plasticizers may be used alone or in combination of two or more.

[0066] The content of the plasticizer (B) in the elastic hot melt resin layer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 12% by mass or more, based on 100% by mass of the elastic hot melt resin layer. The content of the plasticizer (B) in the elastic hot melt resin layer is preferably 50% by mass or less, more preferably 45% by mass or less, based on 100% by mass of the elastic hot melt resin layer. By having the content of the plasticizer (B) in the above range, the width of the patch can be further suppressed, and the patch can more easily follow the shape of the affected area.

[0067] (Wax (C)) The stretchable hot melt resin layer may further contain a wax (C). The wax (C) is preferably a wax having at least one group selected from the group consisting of a carbonyl group, a carboxyl group, and a carboxylic anhydride group in the molecule.

[0068] The wax (C) is preferably solid at 23° C. In this specification, the term "solid" refers to a state in which the wax does not exhibit fluidity. The softening point of the wax (C) is preferably 23° C. or higher, more preferably 30° C. or higher, and even more preferably 40° C. or higher.

[0069] In this specification, the softening point is a value measured by a measurement method in accordance with ASTM D-3954.

[0070] Waxes having at least one group selected from the group consisting of carbonyl groups, carboxyl groups, and carboxylic anhydride groups in the molecule have high polarity, and therefore have good compatibility with styrene-based block copolymers and good dispersion in the composition. Therefore, compared with waxes not having carbonyl groups, carboxyl groups, and carboxylic anhydride groups in the molecule, the heat stability of the stretchable hot melt resin composition can be further improved. Waxes (C) having at least one group selected from the group consisting of carbonyl groups, carboxyl groups, and carboxylic anhydride groups in the molecule are not particularly limited, and examples thereof include vinyl acetate wax, acrylic acid wax, and maleic anhydride modified wax. Among these, vinyl acetate wax is preferred from the viewpoint of better heat stability.

[0071] As the vinyl acetate wax, commercially available products can be used, such as AC-400 manufactured by Honeywell and AC-430 manufactured by Honeywell.

[0072] As the acrylic acid wax, commercially available products can be used, such as AC-540 and AC-580 manufactured by Honeywell.

[0073] As the maleic anhydride modified wax, commercially available products can be used, such as AC-573P and AC-577P manufactured by Honeywell, and MAW-0300 manufactured by Nippon Seiro Co., Ltd.

[0074] The wax having at least one group selected from the group consisting of a carbonyl group, a carboxyl group, and a carboxylic anhydride group in the molecule may be used alone or in combination of two or more kinds.

[0075] The content of the wax (C) in the elastic hot melt resin layer is preferably 5% by mass or more, more preferably 10% by mass or more, based on 100% by mass of the elastic hot melt resin layer. The content of the wax (C) in the elastic hot melt resin layer is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less, based on 100% by mass of the elastic hot melt resin layer. When the content of the wax (C) is within the above range, the width of the patch can be further suppressed, and the patch can more easily follow the shape of the affected area.

[0076] (Other additives) The stretchable hot melt resin layer may contain other additives, such as antioxidants, ultraviolet absorbers, tackifier resins, photopolymerization initiators, liquid rubbers, and particulate fillers, as long as the additives do not substantially impede the object of the present invention.

[0077] Antioxidants include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenyl)propionate, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,4-bis(octylthiomethyl)-o-cresol, 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2,4-di-t-amyl-6-[1-(3,5-di-t-amyl-2-hydroxyphenyl)ethyl ester, and 2,2'-methylenebis(4-ethyl-6-t-butylphenol). hindered phenol-based antioxidants such as 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)] acrylate, tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl) propionate] methane; sulfur-based antioxidants such as dilauryl thiodipropionate, lauryl stearyl thiodipropionate, pentaerythritol tetrakis(3-lauryl thiopropionate); phosphorus-based antioxidants such as tris(nonylphenyl) phosphite, tris(2,4-di-t-butylphenyl) phosphite, etc. The antioxidants may be used alone or in combination of two or more.

[0078] The content of the antioxidant in the stretchable hot melt resin layer is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on 100% by mass of the stretchable hot melt resin layer. The content of the antioxidant in the stretchable hot melt resin layer is preferably 2% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1% by mass or less, based on 100% by mass of the stretchable hot melt resin layer. When the lower limit of the antioxidant content is in the above range, the thermal stability of the stretchable hot melt resin layer is further improved. When the upper limit of the antioxidant content is in the above range, the odor of the stretchable hot melt resin layer is reduced.

[0079] Examples of the ultraviolet absorbent include benzotriazole-based ultraviolet absorbents such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-t-butylphenyl)benzotriazole, and 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole; benzophenone-based ultraviolet absorbents such as 2-hydroxy-4-methoxybenzophenone; salicylic acid ester-based ultraviolet absorbents; cyanoacrylate-based ultraviolet absorbents; and hindered amine-based light stabilizers. The ultraviolet absorbent may be used alone or in combination of two or more.

[0080] The content of the ultraviolet absorbing agent in the stretchable hot melt resin layer is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on 100% by mass of the stretchable hot melt resin layer. The content of the ultraviolet absorbing agent in the stretchable hot melt resin layer is preferably 2% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1% by mass or less, based on 100% by mass of the stretchable hot melt resin layer. When the lower limit of the content of the ultraviolet absorbing agent is in the above range, the weather resistance of the stretchable hot melt resin layer is further improved. When the upper limit of the content of the ultraviolet absorbing agent is in the above range, the odor of the stretchable hot melt resin layer is reduced.

[0081] Examples of the tackifier resin include natural rosin, modified rosin, glycerol ester of natural rosin, glycerol ester of modified rosin, pentaerythritol ester of natural rosin, pentaerythritol ester of modified rosin, copolymer of natural terpene, three-dimensional polymer of natural terpene, hydrogenated derivative of copolymer of natural terpene, terpene resin, hydrogenated derivative of phenol-based modified terpene resin; petroleum resin such as C5-based petroleum resin, C9-based petroleum resin, C5C9-based petroleum resin, dicyclopentadiene-based petroleum resin, and partially hydrogenated petroleum resin and fully hydrogenated petroleum resin obtained by adding hydrogen to these petroleum resins. As the tackifier resin, petroleum resin, partially hydrogenated petroleum resin, and fully hydrogenated petroleum resin are preferred, and partially hydrogenated petroleum resin and fully hydrogenated petroleum resin are more preferred, in that the elastic hot melt resin layer has excellent odor and thermal stability. These tackifier resins may be used alone or in combination of two or more.

[0082] The Ring and Ball softening point temperature of the tackifier resin is preferably 80° C. or higher, more preferably 90° C. or higher, in order to provide the stretchable hot-melt resin layer with even better stretchability and thermal stability. The Ring and Ball softening point temperature of the tackifier resin is preferably 125° C. or lower, more preferably 120° C. or lower, in order to provide the stretchable hot-melt resin layer with even greater flexibility and to further prevent it from becoming brittle. In this specification, the Ring and Ball softening point temperature of the tackifier resin is a value measured in accordance with JIS K2207.

[0083] The content of the tackifier resin in the elastic hot melt resin layer is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on 100% by mass of the elastic hot melt resin layer. When the upper limit of the tackifier resin content is within the above range, the width of the patch can be further suppressed, and the patch can more easily conform to the shape of the affected area.

[0084] Examples of the photopolymerization initiator include an ultraviolet polymerization initiator. When the stretchable hot melt resin layer contains a styrene-based block copolymer having a reactive polystyrene-based hard block in the molecule as the thermoplastic resin (A), the layer further contains a photopolymerization initiator, so that the stretchable hot melt resin composition can be irradiated with light such as ultraviolet light to react the reactive polystyrene-based hard block and crosslink the molecules, thereby adjusting the properties of the stretchable hot melt resin composition such as dynamic viscoelasticity. When the stretchable hot melt resin composition is irradiated with ultraviolet light, the irradiation intensity of the ultraviolet light is 50 mW / cm. 2 More than 1,000mW / cm 2 The preferred dose is 1,000 mJ / cm or less. 2 More than 15,000mJ / cm 2 The following are preferred, and may be appropriately adjusted to obtain the desired properties. The photopolymerization initiator may be used alone or in combination of two or more kinds.

[0085] Examples of the liquid rubber include liquid polybutene, liquid polybutadiene, liquid polyisoprene, and hydrogenated resins thereof. The liquid rubber may be used alone or in combination of two or more kinds.

[0086] The content of the liquid rubber in the elastic hot melt resin layer is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on 100% by mass of the elastic hot melt resin layer. The content of the liquid rubber in the elastic hot melt resin layer is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the elastic hot melt resin layer. When the lower limit of the content of the liquid rubber is within the above range, the melt viscosity of the elastic hot melt resin composition is reduced, and the applicability is further improved. When the upper limit of the content of the liquid rubber is within the above range, the width of the patch can be further suppressed, and the patch can more easily follow the shape of the affected area.

[0087] The particulate filler is not particularly limited, and examples thereof include calcium carbonate, kaolin, talc, titanium oxide, mica, styrene beads, etc. The particulate filler may be used alone or in combination of two or more kinds.

[0088] The stretchable hot melt resin composition has a melt viscosity at 180°C of preferably 45,000 mPa·s or less, more preferably 28,000 mPa·s or less, and even more preferably 22,000 mPa·s or less. When the upper limit of the melt viscosity is within the above range, the coatability of the stretchable hot melt resin composition is further improved. In addition, the lower limit of the melt viscosity at 180°C of the stretchable hot melt resin composition is not particularly limited, and may be about 5,000 mPa·s.

[0089] In this specification, the "melt viscosity" refers to the viscosity of a stretchable hot melt resin composition in a molten state at a certain temperature. For example, a method for measuring the melt viscosity at 180°C includes a method for measuring the viscosity of the stretchable hot melt resin composition in a molten state at 180°C using a Brookfield RVT viscometer (spindle No. 29).

[0090] The elastic hot melt resin composition forming the elastic hot melt resin layer is produced by a known method, for example, by feeding a thermoplastic resin (A), a plasticizer (B), and optionally wax and various additives, etc., into a twin-arm kneader heated to 150°C and melt-kneading them while heating.

[0091] <Support layer> The support layer is not particularly limited as long as it can support the paste layer to form a patch and has elasticity to such an extent that the patch can conform to the affected area when applied to the affected area. Examples of such support layers include nonwoven fabrics and cloths.

[0092] Examples of fibers forming the nonwoven fabric include fibers containing polyester resin, polyethylene resin, polypropylene resin, polyamide resin, acrylic resin, etc. Among these, fibers containing a polyester resin such as polyethylene terephthalate resin are preferred from the viewpoint of less interaction with the drug contained in the paste layer.

[0093] The weight of the nonwoven fabric is 30g / m 2 More than 50 g / m is preferable. 2 More preferably, 80 g / m 2 More preferably, the weight of the nonwoven fabric is 300 g / m 2 Less than 200 g / m is preferable. 2 Less than 150 g / m is more preferable. 2 The following is even more preferable. By setting the lower limit of the basis weight of the backing layer within the above range, the paste layer can be sufficiently supported, and the strength of the patch is further improved. By setting the upper limit of the basis weight of the backing layer within the above range, the patch can more easily conform to the shape of the affected area.

[0094] The thickness of the support layer is preferably 30 μm or more, more preferably 50 μm or more, and even more preferably 80 μm or more. The thickness of the support layer is preferably 500 μm or less, more preferably 400 μm or less, and even more preferably 300 μm or less. By setting the lower limit of the thickness of the support layer within the above range, the paste layer can be sufficiently supported, and the strength of the patch is further improved. By setting the upper limit of the thickness of the support layer within the above range, the patch can more easily follow the shape of the affected area.

[0095] The shape of the backing layer is not particularly limited and may be a typical patch shape such as a rectangle or a square, with a rectangle being preferred.

[0096] The length of the backing layer in the MD direction is preferably 50 mm or more, more preferably 60 mm or more, and even more preferably 100 mm or more. The length of the backing layer in the MD direction is preferably 300 mm or less, more preferably 250 mm or less, and even more preferably 200 mm or less. When the laminate for a patch is rectangular, the MD direction is usually parallel to the short side.

[0097] The length of the backing layer in the TD direction is preferably 50 mm or more, more preferably 75 mm or more, and even more preferably 100 mm or more. The length of the backing layer in the TD direction is preferably 350 mm or less, more preferably 300 mm or less, and even more preferably 250 mm or less. When the laminate for a patch is rectangular, the direction parallel to the long side is usually the MD direction.

[0098] 2. Patches The patch of the present invention is a patch in which a paste layer is further formed on the above-mentioned laminate for a patch.

[0099] In the patch of the present invention, the measured value (Ss) of the laminate in which the backing layer and the paste layer are laminated, measured by the following measuring method, is preferably 3N or more, more preferably 4N or more, and even more preferably 5N or more. Moreover, (Ss) is preferably 30N or less, more preferably 20N or less, and even more preferably 15N or less. By setting the lower limit of (Ss) within the above range, the patch can be further prevented from becoming wider. Furthermore, by setting the upper limit of (Ss) within the above range, the patch can be more easily adapted to the shape of the affected area.

[0100] [Method of measuring (Ss)] A laminate in which the support layer and the paste layer are laminated is fixed in a tensile tester at 10% of the area from each end in the TD direction, and the laminate is stretched by 75% at a tensile speed of 300 mm / min to measure the tensile force (Ss). The tensile tester may be, for example, AGS-X manufactured by Shimadzu Corporation.

[0101] In the laminate for patch of the present invention, the ratio (Sh / Ss) of the above (Sh) to the above (Ss) is preferably 0.5 or less, more preferably 0.4 or less, and even more preferably 0.3 or less. Moreover, Sh / Ss is preferably 0.01 or more, more preferably 0.02 or more, and even more preferably 0.03 or more. By keeping Sh / Ss within the above range, the width of the patch can be further suppressed.

[0102] The layer structure of the patch is not particularly limited as long as it has a paste layer on the above-mentioned laminate for patch, and may be, for example, a layer structure of paste layer / support layer / elastic hot-melt resin layer, a layer structure of paste layer / elastic hot-melt resin layer / support layer, or a layer structure of paste layer / support layer / elastic hot-melt resin layer / support layer.

[0103] Fig. 8 is a cross-sectional schematic diagram showing an example of a patch formed using the above-mentioned laminate for a patch. As shown in Fig. 8, when the elastic hot-melt resin layer 12 is formed on one side of the resin layer 11 in the laminate for a patch, it is preferable that the paste layer 13 is formed on the side of the support layer 11 of the laminate for a patch opposite to the side on which the elastic hot-melt resin layer 12 is formed.

[0104] In the patch of the present invention, the laminate for a patch of the present invention described above can be used as the laminate for a patch.

[0105] <Paste layer> The paste layer is not particularly limited as long as it is a typical paste layer used in patches. Examples of such paste layers include paste layers containing adhesives such as acrylic adhesives, rubber adhesives, and silicone adhesives; anti-inflammatory drugs such as non-steroidal anti-inflammatory analgesics, etc.

[0106] The thickness of the paste layer is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thickness of the support layer is preferably 500 μm or less, more preferably 450 μm or less, and even more preferably 400 μm or less. By setting the lower limit of the thickness of the support layer within the above range, the paste layer can be sufficiently supported, and the strength of the patch is further improved. By setting the upper limit of the thickness of the support layer within the above range, the patch can more easily follow the shape of the affected area. EXAMPLES

[0107] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0108] The following three types of commercially available products were prepared as Comparative Examples 1 to 3. (Laminate 1) Hisamitsu Pharmaceutical Co., Ltd. Salonship, rectangular (100mm x 140mm), containing glycol salicylate, analgesic, anti-inflammatory, cooling patch, layer structure: support layer / plaster layer (Laminate 2) Cool Crest manufactured by Tsuruha Group Merchandising Co., Ltd., rectangular (100mm x 140mm), containing methyl salicylate, analgesic, anti-inflammatory, cooling patch, layer structure: support layer / plaster layer (Laminate 3) Daiichi Sankyo Healthcare Patex, rectangular (100mm x 140mm), containing glycol salicylate, analgesic, anti-inflammatory, cooling patch, layer structure: support layer / plaster layer

[0109] A stretchable hot-melt resin composition was applied to the surface of the support layer of each of the laminates 1 to 3 opposite to the surface on which the paste layer was formed under the conditions shown in Table 1, and cured to form a stretchable hot-melt resin layer. In Examples 1 to 4 and 6, the stretchable hot-melt resin layer was formed in a three-line pattern as shown in Fig. 1, with the width of each line being 10 mm and the distance between each line being 10 mm.

[0110] The composition of the stretchable hot melt resin composition, stretchable hot melt-1, is as follows: (Elastic hot melt-1) Thermoplastic resin (A): 30 parts by mass of styrene-based thermoplastic elastomer (SEBS), 30 parts by mass of styrene-based thermoplastic elastomer (SEBSS), 14.5% by mass of paraffin-based plasticizer, 25% by mass of wax, 0.5% by mass of antioxidant

[0111] The stretchable hot melt resin composition was prepared by putting the above-mentioned raw materials in the above-mentioned amounts into a stirring kneader equipped with a heating device and kneading them while heating at 150° C. for 90 minutes.

[0112] The characteristics of the examples and comparative examples were evaluated under the following measurement conditions.

[0113] (Stress at 75% elongation of elastic hot melt resin layer) The elastic hot melt resin layer was measured for stress at 75% elongation by the following measurement method. That is, the elastic hot melt resin composition was applied to the release layer, and peeled off to prepare a test piece with a width of 25 mm, a length of 75 mm (measurement area 25 mm), and a thickness of 50 μm. Then, it was fixed in a tensile tester (Shimadzu Corporation AGS-X) and elongated to 75% at a tensile speed of 300 mm / min, and the stress was measured.

[0114] (Elastic hot melt resin layer (Sh)) The (Sh) of the elastic hot melt resin layer was measured by the following measurement method. That is, the elastic hot melt resin composition was applied to the release layer and peeled off to form an elastic hot melt resin layer having the shape described in Table 1. Next, using a tensile tester (Shimadzu Corporation AGS-X), the tensile force of the elastic hot melt resin layer was measured under the measurement conditions of 75% elongation at a tensile speed of 300 mm / min, and was taken as (Sh). In Examples 1 to 4 and Example 6, the elastic hot melt resin layer was arranged in three places, so the elastic hot melt resin layer was formed in each place, (Sh) was measured, and the total was used to determine the elastic hot melt resin layer (overall) (Sh).

[0115] ((Ss) of the laminate in which the support layer and the paste layer are laminated) The (Ss) of the laminate in which the support layer and the paste layer were laminated was measured by the following measurement method: A 10% area region from each end in the TD direction of the laminate in which the support layer and the paste layer were laminated was fixed by a tensile tester (Shimadzu Corporation, AGS-X), and the tensile force was measured by elongating it by 75% at a tensile speed of 300 mm / min, and this was taken as (Ss).

[0116] (with width) In the Examples and Comparative Examples, each patch or laminate was stretched by 75% in the TD direction. The width in the MD direction was measured at three points: the center in the TD direction and 20 mm from the center on both sides in the TD direction. The measurement was performed three times, and the average was taken as the measured value.

[0117] Furthermore, for Laminates 1 to 3 of Comparative Examples 1 to 3, the width at 75% elongation was measured in the same manner as above.

[0118] Next, the difference in width at 75% elongation between the Examples and Comparative Examples using the same laminate was calculated. That is, the difference in width at 75% elongation between Examples 1 and 6 and Comparative Example 1, the difference in width at 75% elongation between Example 2 and Comparative Example 2, and the difference in width at 75% elongation between Examples 3 to 5 and Comparative Example 3 were calculated. Next, the width at 75% elongation of each of Comparative Examples 1 to 3 was set as 100%, and the ratio of the difference in width at 75% elongation of the corresponding Examples was calculated, and the width was evaluated according to the following evaluation criteria. It should be noted that if the overall average evaluation is C or higher, it can be evaluated as being suitable for practical use. A: 6% or more B: 3% or more but less than 6% C: 2% or more but less than 3% D: Less than 2%

[0119] The results are shown in Table 1.

[0120] [Table 1]

Claims

1. A laminate for a patch having an elastic hot melt resin layer on at least a portion of one surface of a support layer, The elastic hot melt resin layer is formed at least in a central portion of the support layer, which is a region other than a region having an area of ​​10% from each end of the support layer in the TD direction, with the area of ​​the surface of the support layer on which the elastic hot melt resin layer is formed being 100%, The elastic hot melt resin layer is formed in stripes in the MD direction of the support layer, The area ratio of the stretchable hot melt resin layer is 26.8% or more, with the area of ​​the central portion being 100%, The support layer is a nonwoven fabric or a fabric, The stretchable hot melt resin layer contains a thermoplastic resin (A), a plasticizer (B) and a wax (C), and the thermoplastic resin (A) contains a styrene-based block copolymer having a styrene content of 25% by mass or more and 60% by mass or less.

1. A laminate for a patch comprising:

2. 2. The laminate for a patch according to claim 1, wherein the support layer has a shape defined by points ABCD, and the central portion is defined by point abcd, which is on a side parallel to the TD direction and is 1 / 10 the length of the side from the four points ABCD of the support layer.

3. The elastic hot melt resin composition forming the elastic hot melt resin layer has a stress of 0.20 N / mm at 75% elongation. 2 The laminate for a patch according to claim 1 or 2, wherein

4. The elastic hot melt resin composition forming the elastic hot melt resin layer has a stress of 0.20 N / mm at 75% elongation. 2 More than 1.00N / mm 2 The laminate for a patch according to any one of claims 1 to 3, wherein:

5. A patch comprising the laminate for a patch according to any one of claims 1 to 4, further comprising a paste layer formed on the laminate.

6. A patch comprising a paste layer formed on a laminate for a patch, The laminate for a patch has an elastic hot melt resin layer on at least a part of one surface of a support layer, The elastic hot melt resin layer is formed at least in a central portion of the support layer, which is a region other than a region having an area of ​​10% from each end of the support layer in the TD direction, with the area of ​​the surface of the support layer on which the elastic hot melt resin layer is formed being 100%, The elastic hot melt resin layer is formed in stripes in the MD direction of the support layer, The area ratio of the stretchable hot melt resin layer is 26.8% or more, with the area of ​​the central portion being 100%, The support layer is a nonwoven fabric or a fabric, The paste layer is formed on the surface of the support layer opposite to the surface on which the stretchable hot-melt resin layer is formed. Patch.

7. 7. The patch according to claim 5 or 6, wherein the ratio (Sh / Ss) of a measured value (Sh) of the elastic hot melt resin layer measured by the measurement method described below to a measured value (Ss) of a laminate obtained by laminating the support layer and the paste layer by the measurement method described below is 0.5 or less. [Method for measuring (Sh)] Using a tensile tester, the tensile strength of the elastic hot melt resin layer is measured under measurement conditions of a tensile speed of 300 mm / min and 75% elongation, and this is taken as (Sh). [Method of measuring (Ss)] A 10% area region from each end of the laminate in the TD direction in which the support layer and the paste layer are laminated is fixed by a tensile tester, and the laminate is stretched by 75% at a tensile speed of 300 mm / min to measure the tensile force (Ss).

Citation Information

Patent Citations

  • Laminated material for application medicine and application agent using the same

    JP1996217667A

  • Transdermal patch

    JP1997124463A

  • Tacky tape

    JP2006087488A

  • Base material sheet for adhesive preparation and adhesive preparation

    JP2006102358A

  • Viscoelastic medical article

    JP2017500133A