Ready-mixed concrete shipping type rapid hardening concrete material, ready-mixed concrete shipping type rapid hardening concrete composition
A two-material system using cement, a rapidly hardening material, and an aluminum sulfate accelerator achieves balanced pot life and initial strength development, addressing the limitations of existing ready-mixed concrete technologies.
Patent Information
- Application Number
- JP2022550469
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-18
- Filing Date
- 2021-09-03
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-09-03
AI Technical Summary
Existing ready-mixed concrete technologies face challenges in achieving both sufficient pot life and rapid initial strength development, particularly when transporting and using rapid-hardening concrete, leading to increased costs and limitations in supply volume.
A two-material system comprising a ready-mixed concrete shipping type rapid hardening concrete material, consisting of cement, a rapidly hardening material, and a sleeping agent, combined with an aluminum sulfate hardening accelerator, is used to ensure a stoichiometric ratio that balances pot life and initial strength development.
The system provides a practical ready-mixed concrete composition with excellent initial strength development while ensuring a minimum pot life of 120 minutes, suitable for large-scale construction applications.
Smart Images

Figure 0007573634000001 
Figure 0007573634000002 
Figure 0007573634000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a ready-mixed concrete material for rapid hardening concrete and a ready-mixed concrete composition for rapid hardening concrete. [Background technology]
[0002] Globally, cement production is increasing, and infrastructure development is progressing at a rapid pace. In particular, a construction boom is continuing in China and Southeast Asia. Road construction is an important part of infrastructure development. When building new roads or repairing existing ones, it is desirable to open them to traffic as quickly as possible, so there is a demand for materials that allow for quick return to service. One example is rapid hardening concrete.
[0003] Pot life is also an important performance requirement for rapid hardening concrete. Considering the time required to produce ready-mix concrete at a ready-mix concrete plant, transport it to the construction site, and carry it through construction, as well as the time required to clean the agitator truck that transports the ready-mix concrete, it is desirable to ensure a pot life of at least 120 minutes, and ideally 180 minutes or more. However, ensuring a long pot life means delaying the hardening time, which means that the required strength cannot be met at a short material age. For this reason, with conventional technology, it was difficult to ensure sufficient pot life while also achieving the required strength development at early material ages.
[0004] Currently, rapid hardening concrete is prepared at the construction site. For small-volume construction, 0.1 to 0.2 m 3In this method, the quick-hardening concrete is mixed in a mixer of about 100 mm, and the quick-hardening concrete is prepared and poured by human wave tactics. This method requires a lot of manpower, which increases the number of steps and costs, and there is a limit to the volume of quick-hardening concrete that can be supplied. In addition, in construction projects that require a large amount of concrete to be poured, quick-hardening concrete is continuously supplied using a concrete mobile truck. However, this method has the problem that the cost of quick-hardening concrete is significantly high because it requires the arrangement of a concrete mobile truck, and because it requires the amount of steps to pack fine aggregate and coarse aggregate with a constant moisture content in advance into flexi-con packs and transport them to the site, and to pack quick-hardening cement into flexi-con packs and transport them to the site in preparation. In addition, there is a limit to the arrangement of concrete mobile trucks.
[0005] Today, there is a strong demand for the development of rapid-hardening concrete that can be shipped from ready-mix concrete plants. If rapid-hardening concrete could be shipped from ready-mix concrete plants, it would be possible to supply large quantities of rapid-hardening concrete to construction sites using existing mixing equipment and transportation systems.
[0006] For example, Patent Document 1 discloses a rapid-hardening concrete material for shipment with ready-mixed concrete that uses a hardening agent for rapid-hardening concrete for shipment with ready-mixed concrete, which contains at least one selected from the group consisting of calcium hydroxide, calcium carbonate, calcium aluminate compounds, calcium silicate compounds, colloidal silica, Portland cement, calcium sulfoaluminate cement, and blast furnace slag. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2018 / 154890 Summary of the Invention [Problem to be solved by the invention]
[0008] According to the ready-mixed concrete shipping type rapid-hardening concrete material of Patent Document 1, it is possible to produce a ready-mixed concrete shipping type rapid-hardening concrete composition that is excellent in initial strength development while ensuring a sufficient pot life.
[0009] Incidentally, Patent Document 1 indicates that when aluminum sulfate is used as a quick-setting agent, it sets instantly and the pot life cannot be secured. Aluminum sulfate is an excellent quick-setting agent like sodium aluminate and alkali metal hydroxides, but unlike them, it is easy to handle and can be said to be a highly practical material. In addition, aluminum sulfate can be used in either liquid or solid form, so it is highly practical in that the form can be selected depending on the construction site and situation.
[0010] In view of the above, an object of the present invention is to provide a highly practical rapid-hardening concrete composition for shipping with ready-mixed concrete, which has excellent initial strength development while ensuring sufficient pot life, and to provide a rapid-hardening concrete material for shipping with ready-mixed concrete that is suitable for producing the rapid-hardening concrete composition for shipping with ready-mixed concrete. [Means for solving the problem]
[0011] Therefore, the inventors of the present invention have made various efforts to solve the above problems, and as a result, have found that by preparing concrete by mixing cement, a hardening agent, and material A containing a sleep aid in a ready-mix concrete plant, transporting the concrete to the site, and then adding and mixing material B containing an aluminum sulfate-based hardening accelerator including aluminum sulfate, it is possible to prepare a practical quick-hardening concrete composition that is excellent in initial strength development while ensuring sufficient pot life, and have completed the present invention. That is, the present invention is as follows.
[0012] [1] A two-component ready-mix rapid-hardening concrete material comprising material A containing cement, a hardening agent, and a sleeper, and material B containing an aluminum sulfate-based hardening accelerator containing aluminum sulfate, wherein the stoichiometric ratio of the sleeper to the aluminum sulfate, as represented by the following formula (1), is 0.5 to 5. Formula (1): Stoichiometric ratio = amount of aluminum sulfate (mol) x number of aluminum x valence of aluminum ion / (amount of retardant in sleeping pill (mol) x valence of retardant ion in sleeping pill) [2] Furthermore, the aluminum sulfate-based hardening accelerator contains magnesium and calcium, and the content of these is 0.007 to 4 parts by mass, calculated as oxide, per 100 parts by mass of the aluminum sulfate. [3] A ready-mixed concrete composition for rapid hardening, which is obtained by mixing material A containing cement, a hardening agent, and a sleeper with material B containing an aluminum sulfate-based hardening accelerator containing aluminum sulfate, wherein the stoichiometric ratio of the sleeper to the aluminum sulfate, as represented by the following formula (1), is 0.5 to 5. Formula (1): Stoichiometric ratio = amount of aluminum sulfate (mol) x number of aluminum x valence of aluminum ion / (amount of retardant in sleeping pill (mol) x valence of retardant ion in sleeping pill) Effect of the Invention
[0013] According to the present invention, it is possible to provide a highly practical rapid-hardening concrete composition for shipping with ready-mixed concrete, which has excellent initial strength development while ensuring sufficient pot life, and a rapid-hardening concrete material for shipping with ready-mixed concrete suitable for producing the rapid-hardening concrete composition for shipping with ready-mixed concrete. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to these embodiments. In this specification, "parts" and "%" are based on mass unless otherwise specified. In addition, the composition in this specification collectively refers to a cement composition, a mortar composition, and a concrete composition.
[0015] [1] Ready-mixed rapid hardening concrete material The two-component ready-mix concrete material of this embodiment is composed of at least two materials, including material A containing cement, a hardening agent, and a sleeping agent, and material B containing an aluminum sulfate-based hardening accelerator including aluminum sulfate.
[0016] In this embodiment, "ready-mixed concrete shipped quickly" refers to concrete that is mixed in a ready-mixed concrete factory or plant, transported by an agitator truck or the like, shipped to a construction site such as a civil engineering or construction site, and hardens relatively quickly after pouring. In the case of ready-mixed concrete shipped quickly, due to transportation time, a pot life of at least 120 minutes is required from shipping to the completion of work, and if the transportation distance is long, it is desirable to ensure a pot life of 180 minutes or more. This embodiment is specialized for use in such applications. The above-mentioned "agitator truck" is a freight vehicle equipped with a mixing drum (container for mixing) in the loading area, which allows it to transport ready-mixed concrete while stirring it. There is no significant difference in their functions, but there are models with maximum load capacities ranging from 2 to 26 tons, and they are used according to the application.
[0017] In this embodiment, the sleeping agent in material A puts the ready-mix rapid-hardening concrete into a sleep-like state, i.e., the hydration hardening is almost stopped. This makes it possible to ensure pot life. Furthermore, the addition of the aluminum sulfate-based hardening accelerator in material B reawakens the hydration hardening of the rapid-hardening concrete that was put to sleep by adding a large amount of sleeping agent at the construction site. Furthermore, the other components such as the rapid-hardening agent provide excellent early strength development. Adding the B material accelerates the setting and hardening, but even after adding the B material, it is necessary to ensure working time, and it is necessary to ensure a pot life of at least 15 minutes. However, aluminum sulfate exhibits instant setting when added in normal amounts, and sufficient pot life cannot be ensured. In this embodiment, the stoichiometric ratio of the sleeping agent and aluminum sulfate is considered and set to a range of 0.5 to 5, thereby ensuring sufficient pot life and realizing excellent early strength development. As described above, aluminum sulfate is easy to handle and can be used in either liquid or solid form (preferably powder), so that the form can be selected depending on the application location and situation, making it highly practical. Materials B and A will be explained in detail below.
[0018] [B material] The aluminum sulfate-based hardening accelerator in Material B refers to an accelerator whose main component is aluminum sulfate (preferably 70% or more, and more preferably 80% or more). In addition, the presence of substances (other components) other than the hardening accelerator in material B can increase the dispersibility of the aluminum sulfate-based hardening accelerator or promote the effect of the aluminum sulfate-based hardening accelerator, and can be contained in the range of 30% or less as long as they do not impair the effects of the present invention.
[0019] The aluminum sulfate according to this embodiment is represented by the general formula Al2(SO4)3·nH2O (n = 0 to 18), where n is in the range of 0 to 18. There are aluminum sulfates such as anhydrous aluminum sulfate and aluminum sulfates with various numbers of water of crystallization, and either of them can be used in the present invention.
[0020] Aluminum sulfate is available in powder form or in liquid form dissolved in water, either of which can be used. If aluminum sulfate is liquid, material B will also be liquid, and if it is powder, material B will also be powder.
[0021] Of these, when good mixing with cement concrete and prevention of dust generation are particularly required, it is preferable to use it in liquid form such as an aqueous solution. In this case, the concentration of aluminum sulfate is preferably 10 to 40% in terms of solid content (anhydride), more preferably 20 to 30. By making it 10 to 40%, storage stability is improved and it is possible to prevent the setting and hardening of cement concrete from being excessively accelerated. In addition, "liquid" includes a slurry or suspension state.
[0022] When very early strength development is particularly required, the aluminum sulfate is preferably in the form of a powder. Aluminum sulfate may not be able to be ground if it is 14-hydrate or more, so 12-hydrate or less is preferable. Anhydrous salts may have poor coagulation properties, so 4-hydrate or more is preferable. More preferably, it is 4-12-hydrate, that is, aluminum sulfate is a hydrate with 4-12 waters of hydration. The number of water molecules of hydration can be adjusted, for example, by dehydrating aluminum sulfate 18-hydrate by heating or the like until the desired number of water molecules of hydration is obtained.
[0023] When the aluminum sulfate is in the form of a powder, there is no limitation as to the particle size, but since it is difficult to dissolve if it is in a lump form, it is usually preferable that the aluminum sulfate pass through a 1.2 mm sieve, and more preferably a 0.6 m sieve.
[0024] The aluminum sulfate-based hardening accelerator contains magnesium and calcium, and the content of these is preferably 0.007 to 4 parts by mass, more preferably 0.01 to 2 parts by mass, calculated as oxide, relative to 100 parts by mass of aluminum sulfate. By using 0.007 to 4 parts, sufficient adhesion can be imparted even at room temperature to low temperature environments, and it is also possible to prevent a significant decrease in long-term strength in high temperature environments. In addition, the initial strength development can be well maintained. In addition, "low temperature" in the above "low temperature environment" refers to 5°C or below, and "high temperature" in the above "high temperature environment" refers to 25°C or above.
[0025] Here, when material B is liquid, an embodiment in which the aluminum sulfate-based hardening accelerator contains magnesium and calcium may be one in which compounds containing magnesium and calcium are dissolved in the liquid material B, so that the magnesium and calcium contents are 0.007 to 4 parts in terms of oxide per 100 parts of aluminum sulfate.
[0026] In order to adjust the magnesium and calcium contents to the above ranges, it is sufficient to dissolve a prescribed amount of a magnesium compound and a calcium compound.
[0027] When material B is in powder form, an embodiment in which the aluminum sulfate-based hardening accelerator contains magnesium and calcium includes an embodiment in which aluminum sulfate contains magnesium and calcium, and the content of these is 0.007 to 4 parts in terms of oxide per 100 parts of aluminum sulfate.
[0028] To make aluminum sulfate contain magnesium and calcium, compounds such as CaO and / or MgO contained in sulfuric acid may be adjusted to a desired range when aluminum hydroxide and sulfuric acid are mixed to produce aluminum sulfate, or compounds such as CaO and MgO may be intentionally mixed with aluminum hydroxide and sulfuric acid to a desired range and then heated to cause a reaction. In this case, aluminum sulfate is identified as having CaO and MgO in addition to aluminum sulfate by X-ray fluorescence analysis, but X-ray diffraction (XRD) analysis only identifies a broad peak of aluminum sulfate, and does not identify peaks for CaO and MgO. In other words, although the aluminum sulfate contains calcium and magnesium, it can be considered to be essentially the same as aluminum sulfate.
[0029] Whether the material B is in liquid or powder form, magnesium and calcium are preferably contained as oxides (MgO, CaO), and the CaO content is preferably 0.005-2% and the MgO content is preferably 0.002-2% in the material B. The CaO content is more preferably 0.01-1.5%, and the MgO content is more preferably 0.008-1.5%.
[0030] If the CaO content is 0.005% or more, it is easier to obtain long-term strength under high temperature conditions, and if it is 2% or less, it is easier to suppress the deterioration of setting properties. Also, if the MgO content is 0.002% or more, it is easier to obtain long-term strength under high temperature conditions, and if it is 2% or less, it is easier to suppress abnormal expansion under high temperature conditions.
[0031] In this embodiment, as described above, the stoichiometric ratio of aluminum sulfate to the sleep aid described below was examined, and the range was set to 0.5 to 5, thereby ensuring sufficient pot life and achieving excellent initial strength development. The stoichiometric ratio is expressed by the following formula (1). Equation (1) represents the ratio of aluminum sulfate, a hardening accelerator, to the sleeper in concrete that contains a hardening agent and a sleeper. This ratio is in the range of 0.5 to 5, meaning that if the ratio is too low, there will be too much sleeper and rapid hardening will not be achieved, and if the ratio is too high, there will be too much hardening accelerator and the concrete will set instantly.
[0032] Formula (1): Stoichiometric ratio = amount of aluminum sulfate (mol) x number of aluminum x valence of aluminum ion / (amount of retardant in sleeping pill (mol) x valence of retardant ion in sleeping pill)
[0033] In the following, the stoichiometric ratio will be explained using an example in which aluminum sulfate (material B) and potassium carbonate and citric acid (potassium carbonate:citric acid = 75:25 (mass ratio)) are used as the sleeping agent (material A).
[0034] First, the molar masses of aluminum sulfate and citric acid are as follows. Aluminum sulfate (Al2(SO4)3) MW=342.2 Citric acid (C6H8O7) MW=192.1
[0035] If 500 kg of binder in concrete contains 1% aluminum sulfate and 1.5% sleep aid, the respective components per concrete will be as follows. The hardening accelerator acts on citric acid, which is a retarder for sleep aid. Aluminum sulfate: Binder 500,000g x 0.01 (=1%) ÷ 342.2 = 14.6mol Citric acid: Binder 500,000g x 0.015(=1.5%) x 0.25(=25%) ÷ 192.1 = 9.7mol
[0036] Since aluminum ions act as trivalent acids, aluminum sulfate contains two Al atoms, and citrate ions are trivalent bases (valence of retarder ions = 3), the above formula (1) is calculated as follows: Formula (1): Stoichiometric ratio = (14.6×2×3) / (9.7×3)=3.0
[0037] [Material A] Materials A include cement, hardening agents, and sleepers. (Sleeping pills) The sleeping agent used in this embodiment has the function of putting the rapid hardening concrete shipped from the ready-mix concrete to sleep (almost stopping hydration hardening), and prevents rapid hardening problems at ready-mix concrete plants and when transporting with an agitator truck. Examples of sleeping agents include oxycarboxylic acid or its salt, or a combination of these with alkali metal carbonate, sugar, boric acid, etc. Of these, the retarder corresponds to oxycarboxylic acid or its salt, sugar, and boric acid. Among the above, the combined use of oxycarboxylic acid and alkali metal carbonate is preferable because it has a large effect of putting the rapid hardening concrete to sleep and because it provides good strength development after adding material B. However, it is preferable to select an alkali metal carbonate other than lithium. It is necessary to ensure sufficient pot life of the base concrete, a certain pot life even after adding material B, and good strength development, and from this perspective, the use of lithium carbonate is not preferable. Also, when an alkali metal carbonate is used alone without being combined with oxycarboxylic acid, it does not act as a sleeping aid. In this specification, the base concrete refers to concrete obtained by mixing at least cement, a hardening agent, a sleep aid, aggregate, and mixing water.
[0038] The sleeping agent preferably contains a mixture of an oxycarboxylic acid, an alkali metal carbonate other than lithium, and an oxycarboxylic acid, and more preferably contains a mixture of an alkali metal carbonate other than lithium and an oxycarboxylic acid. The mixing ratio of the alkali metal carbonate other than lithium and the oxycarboxylic acid, alkali metal carbonate / oxycarboxylic acid, is preferably 10 / 90 to 90 / 10, and more preferably 20 / 80 to 80 / 20.
[0039] The oxycarboxylic acid includes an oxycarboxylic acid or a salt thereof, and examples of the oxycarboxylic acid include citric acid, gluconic acid, tartaric acid, malic acid, etc., and examples of the salts thereof include sodium salts, potassium salts, calcium salts, magnesium salts, etc. One or more of these may be used in combination.
[0040] The content of the sleeper is preferably 0.3 to 5 parts, more preferably 0.3 to 4.5 parts, per 100 parts of cement and hardening agent combined. By using 0.3 to 5 parts, it becomes easier to secure sufficient work time in addition to the transportation time to the site. Also, it becomes easier to reactivate hydration hardening when material B is added.
[0041] (Sudden hardwood) The hardening agent of the present embodiment is preferably composed of a calcium aluminate compound and gypsum. Here, the calcium aluminate compound is a general term for compounds mainly composed of CaO and Al2O3, and is not particularly limited. Specific examples include CaO·Al2O3, 12CaO·7Al2O3, 11CaO·7Al2O3·CaF2, 3CaO·Al2O3, 3CaO·3Al2O3·CaSO4, and amorphous substances mainly composed of CaO and Al2O3 (for example, CaO-Al2O3-SiO2 compounds). Among them, it is preferable to select an amorphous substance from the viewpoint of strength development.
[0042] Here, the degree of amorphousness in this embodiment is defined as follows. After annealing the target material at 1000°C for 2 hours, it is slowly cooled at a cooling rate of 5°C / min to crystallize it. Then, the crystallized material is measured by powder X-ray diffraction method to obtain the area S0 of the main peak of the crystalline mineral. Next, the degree of amorphousness X is calculated from the main peak area S of the crystal of the material before annealing by the following formula. X(%)=100×(1-S / S0)
[0043] In addition, general industrial raw materials contain impurities such as SiO2, MgO, Fe2O3, TiO2, K2O, Na2O, etc., but these impurities also promote the amorphization of calcium aluminate compounds, so there is no problem if the total amount of these impurities is within the range of 20% or less. Among them, the presence of SiO2 is preferable, and it can be contained within the range of 1 to 18% in order to obtain amorphous calcium aluminate.
[0044] Therefore, the hardening agent contains a CaO-Al2O3-SiO2 compound and gypsum, and the CaO-Al2O3-SiO2 compound has an amorphous degree of 70% or more and SiO2 is in the range of 1 to 18 mass%. More preferably, the CaO-Al2O3-SiO2 compound has an amorphous degree of 80% or more and SiO2 is in the range of 2 to 13 mass%.
[0045] Calcium aluminate compounds are crushed to a Blaine specific surface area of 3000 to 9000 cm. 2 / g, and the range is preferably 4000 to 8000 cm 2 It is more preferable to adjust the fineness (Blaine specific surface area) of the calcium aluminate compound to 4000 to 9000 cm 2 / g, sufficient rapid hardening is easily obtained, and strength development at low temperatures is also easily obtained.
[0046] In addition, the rapid hardening material of the present embodiment has a Blaine specific surface area of 3000 to 9000 cm by pulverization. 2 / g, and the range is preferably 4000 to 8000 cm2 It is more preferable to adjust the fineness of the hardening agent to 3000 to 9000 cm / g. 2 / g, sufficient ultra-fast hardening properties are easily obtained, and strength development at low temperatures is also easily obtained.
[0047] The content of the hardening agent is preferably 10 to 35 parts, more preferably 15 to 30 parts, and even more preferably 20 to 25 parts, per 100 parts of the total of the cement and the hardening agent. When the content is 10 to 35 parts, good early strength development is easily obtained, and a decrease in long-term strength is less likely to occur.
[0048] For the hardening agent and cement, ultra-fast hardening cement can be used. Ultra-fast hardening cement is calcium fluoroaluminate (C 11 Some are known to contain compounds such as calcium sulfoaluminate (3CaO·3Al2O3·CaSO4) as their main components.
[0049] The gypsum used in this embodiment may be any of anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum. Furthermore, natural gypsum, chemical gypsum such as gypsum produced by by-product of phosphoric acid, gypsum dehydrated, and gypsum produced by by-product of hydrofluoric acid, or gypsum obtained by heat treatment of these may also be used. Among these, anhydrous gypsum and / or hemihydrate gypsum are preferred from the viewpoint of strength development, but it is desirable to select anhydrous gypsum from the viewpoint of cost, and type II anhydrous gypsum and / or natural anhydrous gypsum are preferred. The particle size of gypsum is 3000 cm in Blaine value. 2 / g or more is preferable, and 4000 to 7000 cm 2 / g is more preferable. 2 / g or more, good early strength development can be achieved.
[0050] The amount of gypsum used is preferably 10 to 200 parts, more preferably 15 to 150 parts, and even more preferably 20 to 130 parts, per 100 parts of the calcium aluminate compound. Within these ranges, strength development can be satisfactorily achieved.
[0051] (cement) The term "cement" in this embodiment is not particularly limited, but may be, for example, any of various Portland cements of normal, early strength, medium heat, and low heat as defined by the Japanese Industrial Standards (JIS), various mixed cements mixed with blast furnace slag, fly ash, and silica, filler cements mixed with limestone powder and pulverized slowly cooled blast furnace slag, and environmentally friendly cements (ecocement) manufactured using municipal waste incineration ash and sewage sludge incineration ash as raw materials. In addition, any of the cements defined by the overseas EN197-2000 and the Chinese GB standard may be used, and one or more of these may be used.
[0052] Portland cement is composed of alite (3CaO·SiO2), belite (2CaO·SiO2), aluminate (3CaO·Al2O3), ferrite (4CaO·Al2O3·Fe2O3), and further gypsum dihydrate (some of which may change to hemihydrate). In this embodiment, it is desirable to select a cement that does not contain admixtures such as blast furnace slag, fly ash, silica, and limestone fine powder from the viewpoint of strength development, and it is preferable to select a cement that has a high alite content and a high degree of fineness (fine grain size). Examples of cement that fall into this category include high-early-strength cement and normal cement, for example, in the case of Japanese cement. Examples of Chinese cement include P·II52.5 and P·II42.5.
[0053] In this embodiment, in addition to the aforementioned hardening accelerators, sleep aids, and aluminum sulfate-based hardening accelerators, one or more of the following may be used in material A and / or material B to the extent that the object of the present invention is not substantially hindered: expansion agents, water reducing agents, AE water reducing agents, high-performance water reducing agents, slag such as slowly cooled blast furnace slag powder and slowly cooled blast furnace slag powder, admixtures such as limestone fine powder, fly ash, and silica fume, defoamers, thickeners, rust inhibitors, antifreeze agents, shrinkage reducing agents, polymers, clay minerals such as bentonite, and anion exchangers such as hydrotalcite.
[0054] [2] Ready-mixed rapid hardening concrete composition The ready-mixed concrete shipping type rapid hardening concrete composition according to this embodiment is made by mixing material A containing cement, an accelerating agent, and a sleeper, and material B containing an aluminum sulfate-based hardening accelerator containing aluminum sulfate. The stoichiometric ratio of the sleeper and aluminum sulfate represented by the above-mentioned formula (1) is 0.5 to 5. The preferred ranges are the same as those mentioned in the "ready-mixed concrete shipping type rapid hardening concrete material".
[0055] At ready-mix concrete plants, it is necessary to prepare various types of base concrete mixed with material A, and material B must be added and mixed into the various types of base concrete after it is transported to the site. If material B is mixed into the various types of base concrete in advance at the ready-mix concrete plant rather than at the construction site, the pot life cannot be secured. Also, if both the quick-hardening material and material B are added at the ready-mix concrete plant, the pot life becomes extremely short, and concrete must be discarded during transportation. If material B is added at the ready-mix concrete plant and the rapid hardening agent is added at the construction site, the pot life after the rapid hardening agent is added is extremely short, at less than 10 minutes, making construction impossible. If the rapid hardening agent and material B are added at the construction site, not only is the pot life shortened and the compressive strength low, but only about 30% of the agitator drum volume can be transported. Thus, the timing of adding materials A and B is extremely important.
[0056] Therefore, in this embodiment, a two-material type consisting of material A and material B is used. Specifically, base concrete mixed with material A at a ready-mix concrete plant is transported to a construction site, and material B is mixed at the construction site, thereby making it possible to produce the ready-mix concrete shipping type rapid-hardening concrete composition of this embodiment.
[0057] [Preparation method for ready-mixed shipping rapid hardening concrete] An embodiment of the method for preparing ready-mixed rapid-hardening concrete of the present invention sequentially includes a step of mixing at least material A together with mixing water in a mixing vessel to prepare base concrete (mixing step), and further a step of mixing material B, for example, at a construction site. The mixing water is supplied, for example, from a ready-mixed concrete factory or a ready-mixed concrete plant, etc. In the mixing process, transportation is often performed together with mixing.
[0058] In the mixing step, the volume of the base concrete containing material A and mixing water is preferably 40% (volume %) or more of the internal volume of the mixing (and transportation) container, and more preferably 50% or more by volume. Here, the mixing (and transport) vessel refers to a vessel that is attached to a ready-mixed concrete transport vehicle, such as the drum of an agitator vehicle, and can hold ready-mixed concrete while stirring it.
[0059] It is preferable to determine the type of B material and the above-mentioned stoichiometric ratio within an appropriate range so that the pot life after mixing of B material can be ensured to be 10 minutes or more, preferably 15 minutes or more.
[0060] As described above, the two-component type quick-hardening concrete material according to this embodiment is suitable for use as a material added after mixing ready mixed concrete (ready mixed concrete), transporting the mixture to a construction site, and placing the mixture in the construction site. The pot life can be set to, for example, 120 minutes or more, preferably 180 minutes or more. EXAMPLES
[0061] The present invention will be described in more detail below based on experimental examples, but the present invention is not limited to these.
[0062] (Experimental Example 1) Cement 375kg / m 3 , Rapid hardwood A125kg / m 3 A quick-hardening concrete was prepared with a water / binder ratio of 32%, s / a=42%, and air content of 2.0±1.5% by volume. At this time, 1.5 parts of sleeper 1 were added to 100 parts of binder consisting of cement and quick-hardening agent to prevent hydration hardening for more than 24 hours (material A). Assuming that there was a transportation time to the site and a waiting time after arriving at the construction site, material B containing a hardening accelerator was added after 120 minutes in the stoichiometric ratio shown in Table 1 below. The pot life after adding material B was measured, and the compressive strength was measured 6 hours after adding material B (8 hours after mixing). Note that s / a is the fine aggregate ratio, which is the absolute volume ratio of the fine aggregate to the total aggregate in the concrete expressed as a percentage. The environmental temperature was set to 20°C. The stoichiometric ratio was calculated from the above-mentioned formula (1).
[0063] <Materials used> (1) Hardening accelerators A and B Hardening accelerator B: Liquid aluminum sulfate with an aluminum sulfate content of 27% (used in Experiments 1-2 to 1-6), solvent is water Hardening accelerator B: Powdered aluminum sulfate (14-hydrate) that passed through a 0.6 mm sieve was used (used in Experiments 1-7).
[0064] (2) Rapidly hardened wood Rapid hardening material A: A mixture of equal amounts of CaO-Al2O3-SiO2 amorphous material and anhydrous gypsum. The CaO-Al2O3-SiO2 amorphous material is 43% CaO, 44% Al2O3, 10% SiO2, and 3% others. Density 2.85g / cm 3 , Blaine specific surface area 5000cm 2 / g, amorphous content 90%
[0065] (3) Sleeping pills Sleeping agent 1: A mixture of 75 parts of reagent grade potassium carbonate and 25 parts of reagent grade citric acid.
[0066] (4)Other Cement: Commercially available ordinary Portland cement (Denka Co., Ltd., density 3.15 g / cm 3 ) Anhydrous gypsum: Type II anhydrous gypsum, pH 3.0, Blaine specific surface area 5000 cm 2 / g Water: Tap water Fine aggregate: Natural river sand Coarse aggregate: crushed stone
[0067] <Measurement method> Pot life: The time until the initial setting of the mixture was measured according to JIS A 1147 and used as the pot life. Compressive strength: Measured according to JIS A 1108.
[0068] [Table 1]
[0069] (Experimental Example 2) CaO and MgO (both reagents) were dissolved in hardening accelerator A so that the contents would be as shown in Table 2 below per 100 parts of aluminum sulfate to prepare hardening accelerators A-1 to A-4, and the same procedure as in Experimental Example 1 was repeated except for using these instead of hardening accelerator A. The results are shown in Table 2.
[0070] [Table 2]
[0071] (Experimental Example 3) The same experiment as in Experiment 1 was carried out, except that the B material used in Experiments No. 1-4 was used and the type and stoichiometric ratio of the sleeping agent were changed as shown in Table 3. The results are shown in Table 3. When non-sleeping agent 2 was used, the amount of non-sleeping agent 2 was adjusted to 112 parts per 100 parts of aluminum sulfate.
[0072] <Materials used> Sleeping agent 1: A mixture of 75 parts of reagent grade potassium carbonate and 25 parts of reagent grade citric acid. Non-sleeping agent 2: Reagent grade potassium carbonate Sleeping aid 3: Reagent grade citric acid Sleeping agent 4: Reagent grade tartaric acid (C4H6O6, MW=150.09, divalent base)
[0073] [Table 3]
[0074] From Table 3, it can be seen that the effects of the present invention are particularly excellent when an oxycarboxylic acid or a mixture of an oxycarboxylic acid and an alkali metal carbonate other than lithium is used as the sleeping aid.
[0075] (Experimental Example 4) In the A material used in Experiment No. 1-4, the same procedure as in Experiment Example 1 was carried out except that the type of cement and the amount of Sleeping Agent 1 used were changed as shown in Table 4 below. The results are shown in Table 4 below.
[0076] [Table 4]
[0077] Table 4 shows that for any cement, by properly controlling the amount of sleeper used, it is possible to obtain a certain pot life and good 6-hour strength and 1-day strength.
[0078] (Experimental Example 5) In the material A used in Experiment No. 1-4, the type and amount of the hardening agent used were changed as shown in Table 5 below, but the same procedure was followed as in Experiment Example 1. The results are shown in Table 5 below. The hardening agents B to D are as follows:
[0079] <Materials used> - Hardening agent B: A mixture of equal parts of CaO-Al2O3-SiO2 amorphous material and anhydrous gypsum. The CaO-Al2O3-SiO2 amorphous material is 47% CaO, 47% Al2O3, 3% SiO2, and 3% others. Density 2.85g / cm 3, Blaine specific surface area 5000cm 2 / g, amorphous content 90% Accelerator C: A mixture of equal parts of alumina cement No. 1, whose main component is CaO·Al2O3, and anhydrous gypsum. Density 3.00g / cm 3 , Blaine specific surface area 5000cm 2 / g - Rapid hardening material D: Ultra rapid hardening cement containing 3CaO·3Al2O3·CaSO4 compounds as the main component (40%). Density 2.80g / cm 3 , Blaine specific surface area 5000cm 2 / g
[0080] [Table 5]
[0081] From Table 5, it can be seen that when no hardening agent is added, the material does not harden for 24 hours or more, and does not exhibit 6-hour or 1-day strength, but when a hardening agent is added, it achieves a certain pot life and exhibits good 6-hour or 1-day strength. In addition, it can be seen that the abrasion resistance is also excellent. It can also be seen that the effects of the present invention are exhibited even when the type of hardening agent is changed.
[0082] (Experimental Example 6) Experiments No. 1-4 were conducted in the same manner as in Experimental Example 1, except that the timing (location) of addition of Materials A and B was changed as shown in Table 6 below. The results are shown in Table 6 below.
[0083] [Table 6]
[0084] From Table 6, it can be seen that the effects of the present invention cannot be obtained unless material A is added at the ready-mix concrete plant and material B is added at the construction site. When both materials A and B are added at the ready-mix concrete plant, the pot life is extremely short at 60 minutes, and it was necessary to discard it during transportation. Furthermore, when material B is added at the ready-mix concrete plant and material A is added at the construction site, the pot life after its addition is extremely short at 10 minutes, and construction is not possible. It can be seen that when materials A and B are added at the construction site, not only is the pot life shortened and the compressive strength reduced, but only about 30% of the drum volume of the agitator, which serves as the mixing and transporting container, can be transported. [Industrial Applicability]
[0085] The ready-mixed concrete shipping type rapid-hardening concrete composition of the present invention has excellent initial strength development while ensuring sufficient pot life, and is therefore particularly suitable for use in the civil engineering and construction fields.
Claims
1. The present invention comprises a material A including a cement, a hardening agent, and a sleeping agent, and a material B including an aluminum sulfate-based hardening accelerator including aluminum sulfate, wherein the stoichiometric ratio of the sleeping agent to the aluminum sulfate represented by the following formula (1) is 0.5 to 5, The hardening agent is composed of a calcium aluminate compound and a gypsum, The sleep aid is an oxycarboxylic acid or a salt thereof, or a combination of these with an alkali metal carbonate, a sugar, or boric acid; A two-component type rapid-hardening concrete material for ready-mix shipping, in which the retarder in the following formula (1) is any one of an oxycarboxylic acid or a salt thereof, a sugar, and boric acid. Formula (1): Stoichiometric ratio = amount of aluminum sulfate (mol) x number of aluminum molecules x valence of aluminum ion / (amount of retardant in sleeping pill (mol) x valence of retardant ion in sleeping pill)
2. Furthermore, the aluminum sulfate-based hardening accelerator contains magnesium and calcium, and the content of these is 0.007 to 4 parts by mass in terms of oxide per 100 parts by mass of the aluminum sulfate. The two-material type ready-mixed concrete shipping type rapid hardening concrete material according to claim 1.
3. A ready-mixed concrete composition for rapid hardening, which is obtained by mixing material A containing cement, a hardening agent, and a sleeper, and material B containing an aluminum sulfate-based hardening accelerator containing aluminum sulfate, wherein the stoichiometric ratio of the sleeper to the aluminum sulfate represented by the following formula (1) is 0.5 to 5, The hardening agent is composed of a calcium aluminate compound and a gypsum, The sleep aid is an oxycarboxylic acid or a salt thereof, or a combination of these with an alkali metal carbonate, a sugar, or boric acid; A ready-mixed concrete composition for rapid hardening, in which the retarder in the following formula (1) is any one of an oxycarboxylic acid or a salt thereof, a sugar, and boric acid. Formula (1): Stoichiometric ratio = amount of aluminum sulfate (mol) x number of aluminum molecules x valence of aluminum ion / (amount of retardant in sleeping pill (mol) x valence of retardant ion in sleeping pill)
Citation Information
Patent Citations
Method of rapidly hardening cement
JP1977110724A
Quick hardening cement concrete and casting-in-place lining construction method
JP2001253753A
Quick hardening agent for cement asphalt mortar and cement asphalt mortar using the same
JP2007119317A
Method of producing concrete and concrete
JP2014148446A
Cement mortar spraying method
JP2017110354A