Ultra-high molecular weight polyethylene powder and moldings

By controlling porosity, intrinsic viscosity, and particle size distribution, ultra-high molecular weight polyethylene powder achieves rapid gel formation and improved moldability, producing high-quality molded products like separators and fibers.

JP7573675B2Active Publication Date: 2024-10-25ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023055819
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-03-30
Publication Date
2024-10-25
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Ultra-high molecular weight polyethylene powder exhibits low fluidity during melting, making it difficult to mold uniformly due to changes in shape, surface condition, and pore condition during heating, leading to issues like air bubbles and distortion in molded products.

Method used

Control the porosity, intrinsic viscosity, particle size distribution, and titanium content of the polyethylene powder to achieve uniform gel formation and improved moldability, resulting in high-quality molded products.

Benefits of technology

The controlled ultra-high molecular weight polyethylene powder enables rapid gel formation with high polymer concentration, producing uniform molded products with excellent mechanical properties, such as separators for secondary batteries and fibers with improved yarn diameter uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573675000001
    Figure 0007573675000001
  • Figure 0007573675000002
    Figure 0007573675000002
  • Figure 0007573675000003
    Figure 0007573675000003
Patent Text Reader

Abstract

To provide an ultrahigh-molecular-weight polyethylene powder that is excellent in molding processability by having voids in the central part of the powder, and a high-quality molded article (e.g., a separator for secondary batteries and fibers) prepared by molding the same.SOLUTION: An ultrahigh-molecular-weight polyethylene powder has an intrinsic viscosity IV of 1.0 dL / g or more and 33.0 dL / g or less, wherein the proportion of predetermined voids inside the powder determined by a specific method is 5% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ultra-high molecular weight polyethylene powder and a molded article. [Background technology]

[0002] Polyethylene is used in a wide variety of applications, such as films, sheets, microporous membranes, fibers, foams, and pipes. Polyethylene is used because it is easy to melt process, and the molded products obtained have high mechanical strength and excellent chemical resistance, rigidity, etc. Among them, ultra-high molecular weight polyethylene has a large molecular weight, and therefore has high mechanical strength, excellent sliding properties and abrasion resistance, as well as excellent chemical stability and long-term reliability.

[0003] However, ultra-high molecular weight polyethylene has low fluidity even when melted at a temperature equal to or higher than its melting point. Therefore, various methods are used, such as a compression molding method in which polyethylene powder is compressed and molded under heating and then cut, or a molding method in which the polyethylene is dissolved in a solvent such as liquid paraffin, stretched, and then the solvent is removed to form the polyethylene into a sheet or thread shape.

[0004] Ultra-high molecular weight polyethylene is molded in powder form, but compared to pellets, the powder has a larger surface area and contains fine pores.

[0005] Regarding the pore state of the polyethylene powder, for example, Patent Document 1 discloses a polyethylene powder that can be quickly dissolved in a solvent and can give a molded product with little undissolved matter by adjusting the specific surface area determined by the BET method and the pore volume determined by mercury intrusion porosimetry to appropriate ranges.

[0006] Furthermore, for example, Patent Document 2 discloses a polyethylene powder that can obtain a molded product with little undissolved matter by adjusting the ratio of the median diameter and mode diameter of pores measured by mercury intrusion porosimetry to an appropriate range.

[0007] In recent years, polyethylene powders have been proposed which are excellent in moldability and allow high-quality molded articles to be obtained.

[0008] For example, Patent Document 3 discloses a polyethylene powder that has excellent solubility and can improve the productivity and product quality in processing (particularly wet extrusion) by simultaneously imparting a predetermined particle size distribution and a predetermined swelling ratio to the polyethylene powder.

[0009] Furthermore, for example, Patent Document 4 discloses a polyethylene polymer powder in which the intrinsic viscosity IV and the contents of Al, Mg and Si are controlled within specific ranges, thereby improving oxidation resistance and effectively improving the uniformity and smoothness of a thin film.

[0010] Furthermore, for example, Patent Document 5 discloses an ethylene-based polymer which, by containing a nonmagnetic substance satisfying specific conditions, reduces entanglement of the ethylene-based polymer when processed and stretched, and when made into a high-strength fiber, has excellent low-temperature tensile strength, and when made into a microporous film, has excellent film shrinkage rate and low-temperature puncture strength. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2017-088773 A [Patent Document 2] JP 2017-145306 A [Patent Document 3] JP 2019-019265 A [Patent Document 4] JP 2019-070117 A [Patent Document 5] JP 2019-123777 A Summary of the Invention [Problem to be solved by the invention]

[0012] As described above, ultra-high molecular weight polyethylene powder has a large surface area compared to pellets and has fine pores in the powder. Therefore, the shape, surface condition, crystal state, pore state, etc. of the powder change during heating, so when molding the ultra-high molecular weight polyethylene powder, it is required to adjust the temperature to an appropriate level and perform processing such as dissolution and compression. When compression molding the ultra-high molecular weight polyethylene powder, if the preheating temperature before compression is not appropriate, air bubbles tend to remain in the molded body, or distortion tends to remain in the molded body and cause deformation after cooling.

[0013] The polyethylene powder described in Patent Document 1 has only adjusted powder properties such as specific surface area and pore volume, and the powder properties change significantly at the temperature at which it actually melts or dissolves, leaving room for improvement in terms of moldability.

[0014] In addition, the polyethylene powder described in Patent Document 2 also only specifies the pore size of the powder, and the pore size changes significantly during the heating process, so there is room for improvement in moldability, and it may be difficult to obtain a uniform molded product.

[0015] On the other hand, while the polyethylene powders described in Patent Documents 3 to 5 have relatively excellent moldability, obtaining a uniform gel in a short period of time has not been considered, and there is room for improvement in moldability and quality of molded articles.

[0016] The present invention has been made in consideration of the above circumstances, and has an object to provide an ultra-high molecular weight polyethylene powder that can significantly shorten the kneading time when using ultra-high molecular weight polyethylene powder to produce a molded body, and can produce a uniform gel in a short time, and that has excellent moldability by producing a gel with a high polymer concentration, as well as a high-quality molded body obtained by molding the same (for example, a separator for secondary batteries that is excellent in terms of film thickness unevenness and puncture strength, and a fiber that is excellent in terms of yarn diameter unevenness and high-speed winding properties). [Means for solving the problem]

[0017] The inventors have conducted intensive research to solve the above problems, and as a result have discovered that the above problems can be solved by controlling the porosity (the proportion of the area occupied by voids in a given area of ​​powder) in ultra-high molecular weight polyethylene powder, thereby completing the present invention.

[0018] That is, the present invention is as follows. [1] The intrinsic viscosity IV is 1.0 dL / g or more and 33.0 dL / g or less, The ultra-high molecular weight polyethylene powder has voids therein, In the cross-sectional structure of the powder, the ratio of an area occupied by the void portion to a cross-sectional area A is 5% or more, The cross-sectional structure is such that the particle diameter of the powder is an average particle diameter D 50 The cross-sectional structure of powder P, which is in the range of ±5 μm, The cross-sectional area A is a 20 μm × 20 μm square area centered on the intersection of the diagonals of a rectangle circumscribing the powder P, Ultra-high molecular weight polyethylene powder. [2] The proportion of ultra-high molecular weight polyethylene powder having a particle diameter of 300 μm or more is 10 mass% or less based on the total amount of the ultra-high molecular weight polyethylene powder, The proportion of ultra-high molecular weight polyethylene powder having a particle diameter of less than 53 μm is 20 mass% or less based on the total amount of the ultra-high molecular weight polyethylene powder. [1] The ultra-high molecular weight polyethylene powder according to the present invention. [3] The crystallinity is 70% or more and 85% or less. The ultra-high molecular weight polyethylene powder according to [1] or [2]. [4] Apparent density is 0.45g / cm 3 Below is the The ultra-high molecular weight polyethylene powder according to any one of [1] to [3]. [5] Titanium content is 10ppm or less. The ultra-high molecular weight polyethylene powder according to any one of [1] to [4]. [6] Titanium content is 3ppm or less. [1] to [5]. The ultra-high molecular weight polyethylene powder according to any one of [1] to [5]. [7] [1] to [6] are obtained by molding the ultra-high molecular weight polyethylene powder. Molded body. [8] The molded article is a separator for a secondary battery. The molded article according to [7]. [9] The molded body is a fiber. The molded article according to [7]. Effect of the Invention

[0019] According to the present invention, the ultra-high molecular weight polyethylene powder has a predetermined intrinsic viscosity IV and has a predetermined void inside the powder, and therefore has excellent moldability and can produce high-quality molded products (e.g., separators and fibers for secondary batteries). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment of the present invention (hereinafter, also referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the present embodiment, and can be modified in various ways without departing from the gist of the present invention.

[0021] [Ultra-high molecular weight polyethylene powder] The ultra-high molecular weight polyethylene powder of this embodiment (hereinafter simply referred to as "powder" or "polymer") has an intrinsic viscosity IV of 1.0 dL / g or more and 33.0 dL / g or less, preferably 1.5 dL / g or more and 31.0 dL / g or less, and more preferably 2.4 dL / g or more and 29.0 dL / g or less. The ultra-high molecular weight polyethylene powder of this embodiment has an intrinsic viscosity IV of not less than the above lower limit, thereby further improving the strength, and has an intrinsic viscosity IV of not more than the above upper limit, thereby further improving the molding processability.

[0022] Furthermore, the ultra-high molecular weight polyethylene powder of the present embodiment is not particularly limited, but for example, when used in a molded body for a separator for a secondary battery, the intrinsic viscosity IV is preferably 1.0 dL / g or more and 13.0 dL / g or less, more preferably 1.5 dL / g or more and 11.5 dL / g or less, and even more preferably 2.4 dL / g or more and 9.5 dL / g or less. A separator for a secondary battery obtained by molding an ultra-high molecular weight polyethylene powder having an intrinsic viscosity IV within the above range tends to be excellent in film strength, heat shrinkability, etc.

[0023] Furthermore, the ultra-high molecular weight polyethylene powder of the present embodiment is not particularly limited, but for example, when used for a fiber molding, the intrinsic viscosity IV is preferably 13.5 dL / g or more and 33.0 dL / g or less, more preferably 15.0 dL / g or more and 31.0 dL / g or less, and even more preferably 16.5 dL / g or more and 29.0 dL / g or less. Fibers obtained by molding (for example, ordinary molding or molding in the case of prior swelling at low temperature) ultra-high molecular weight polyethylene powder having an intrinsic viscosity IV within the above range tend to be excellent in thread strength, etc.

[0024] The method of controlling the intrinsic viscosity IV within the above range is not particularly limited, but for example, the polymerization temperature of the reactor when homopolymerizing ethylene or copolymerizing ethylene with olefins other than ethylene that can be copolymerized with ethylene can be changed. The intrinsic viscosity IV tends to be lower as the polymerization temperature is increased, and tends to be higher as the polymerization temperature is decreased. In addition, another method of controlling the intrinsic viscosity IV within the above range is not particularly limited, but for example, the type of organometallic compound used as a cocatalyst when homopolymerizing ethylene or copolymerizing ethylene with olefins other than ethylene that can be copolymerized with ethylene can be changed. In addition, another method of controlling the intrinsic viscosity IV within the above range is not particularly limited, but for example, the type of chain transfer agent added when homopolymerizing ethylene or copolymerizing ethylene with olefins other than ethylene that can be copolymerized with ethylene can be added. By adding a chain transfer agent, the intrinsic viscosity IV of the ultra-high molecular weight polyethylene produced at the same polymerization temperature tends to be lower. In the present embodiment, the intrinsic viscosity IV is not particularly limited, but can be determined, for example, by the method described in the Examples below.

[0025] The ultra-high molecular weight polyethylene powder of the present embodiment is preferably a powder made of an ethylene homopolymer and / or a copolymer of ethylene and an olefin other than ethylene that is copolymerizable with ethylene (hereinafter also referred to as a "comonomer") (hereinafter also referred to as an "ethylene-based polymer").

[0026] The comonomer copolymerizable with ethylene is not particularly limited, but specifically includes, for example, α-olefins having 3 to 15 carbon atoms, cyclic olefins having 3 to 15 carbon atoms, and copolymers represented by the formula CH2=CHR 1 (where R 1 is an aryl group having 6 to 12 carbon atoms.) and at least one comonomer selected from the group consisting of linear, branched or cyclic dienes having 3 to 15 carbon atoms. Among these, α-olefins having 3 to 15 carbon atoms are preferred.

[0027] The α-olefin is not particularly limited, but examples thereof include propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, and 1-tetradecene.

[0028] The ultra-high molecular weight polyethylene powder of the present embodiment is 13 The comonomer content measured by C-NMR is preferably 1.0 mol% or less, more preferably 0.1 mol% or less, and even more preferably 0 mol%. When the ultra-high molecular weight polyethylene powder of the present embodiment has a comonomer content within the above range, decomposition tends to be suppressed, and the strength of a molded product obtained by molding the ultra-high molecular weight polyethylene powder tends to be improved.

[0029] [Void ratio of ultra-high molecular weight polyethylene powder] The ultra-high molecular weight polyethylene powder of this embodiment has voids inside the powder that constitutes the ultra-high molecular weight polyethylene powder, and the proportion of the area occupied by the voids in the cross-sectional structure of the powder is 5% or more, preferably 10% or more, more preferably 15% or more, and most preferably 20% or more, of the cross-sectional area A described below.

[0030] Here, the cross-sectional structure is a cross-sectional structure in which the particle diameter of the powder is an average particle diameter D 50 The cross-sectional structure of powder P is within the range of ±5 μm, and the cross-sectional area A refers to the area of ​​a 20 μm × 20 μm square centered on the intersection of the diagonals of a rectangle circumscribing powder P.

[0031] In this embodiment, the quadrangle circumscribed by the powder P means only a quadrangle in which the proportion of the polymer occupied portion, which is the portion occupied by the polymer other than the void portion, in the cross section of the powder is 20% or more.

[0032] In this embodiment, the void portion includes a polymer-poor portion where the polymer is so thin that it can be regarded as the same as a void portion when observing a cross-sectional image of the powder with an optical microscope.

[0033] The average particle size of the above powder D 50 is not particularly limited, but can be calculated, for example, by the following method.

[0034] 100 g of the ultra-high molecular weight polyethylene powder of this embodiment is classified using 10 types of sieves (mesh openings: 710 μm, 500 μm, 425 μm, 355 μm, 300 μm, 212 μm, 150 μm, 106 μm, 75 μm, 53 μm) specified in JIS Z8801, and the weight of the particles remaining on each sieve is integrated from the side with the smaller openings, and the particle diameter at which the weight is 50% on the integral curve is defined as the average particle diameter (D 50 ) can be used.

[0035] The cross-sectional structure of the powder is not particularly limited, but specifically, for example, it can be observed by the following method.

[0036] Average particle diameter D 50 A fraction containing the particle diameter of 100 μm is collected, and the collected powder is embedded in the high-performance adhesive Araldite Standard (Nichiban Co., Ltd.) and dried at 30°C for 24 hours to prepare an embedded resin sample. The epoxy resin, which is the base agent, and the modified polyamine, which is the hardener, are mixed in a 1:1 ratio. The embedded resin sample is then cut into 10 μm-thick sections using a microtome manufactured by Japan Microtome Laboratory Co., Ltd., and the cut sample is placed on a slide glass, and a small amount (0.05 mL) of liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Co., Ltd. is added, and a cover glass is placed on top of it. The cross-section of the powder can be observed by performing transmission differential interference observation (the light intensity of the microscope is fixed at memory 9) using an optical microscope BX51 manufactured by Olympus Co., Ltd.

[0037] The area that the voids occupy in the cross-sectional structure of the powder relative to the cross-sectional area A is not particularly limited, but can be calculated, for example, by the following method.

[0038] D 50 ±5μm particles are observed at, but not limited to, 10 arbitrary points, and the powder cross-sectional image is taken. Then, using image analysis software (Asahi Kasei Corporation, A-zo-kun ver.2.50), the powder cross-sectional image taken by microscope observation is binarized (white: polymer-occupied portion, black: void portion). An arbitrary rectangle circumscribing the polymer-occupied portion (white) is drawn, and the intersection of the diagonal lines of the rectangle is taken as the center of the powder (hereinafter, also referred to as the powder center). Here, the rectangle circumscribing the powder P in this embodiment is only a rectangle in which the proportion of the polymer-occupied portion (white) is 20% or more. Next, a square of 20μm×20μm is drawn with the powder center as the axis so as to be parallel to the rectangle, and the proportion of the void portion (black) and the polymer-occupied portion (white) in the square is obtained. A similar image analysis is performed on all 10 points taken by optical microscope observation, and the average value can be taken as the proportion of the area of ​​the void portion (black).

[0039] The ultra-high molecular weight polyethylene powder of the present embodiment has a ratio of voids within the above range, and therefore, for example, when fibers (e.g., high-strength fibers) or secondary battery separators (e.g., microporous membranes) are wet extruded, the energy required for wet extrusion can be reduced, thereby reducing the environmental load and significantly improving the production efficiency of molded bodies. Generally, wet extrusion refers to a process in which a slurry in which a powder is impregnated with liquid paraffin is kneaded while being heated in an extruder to form a gel, which is then processed into each molded body. Here, the amount of entanglement of molecular chains in the gel determines the processability of the molded body. In the ultra-high molecular weight polyethylene powder, the molecular chains in the amorphous part are very strongly entangled, and it is difficult to obtain a uniform gel in which the entanglements are released. However, since the ultra-high molecular weight polyethylene powder of the present embodiment has voids in the center of the powder, it is considered that the amount of entanglement of molecular chains per gram of powder is less than that of a normal powder that does not have voids. In addition, when liquid paraffin penetrates from the powder surface to the center through the pores in the powder, a certain amount or more of liquid paraffin can be stored in the voids. In other words, liquid paraffin penetrates the amorphous part from both the powder surface and the center, and the entanglement of molecular chains can be disentangled, so that the powder has excellent moldability and a uniform gel can be obtained in a short time compared to normal powders that do not have voids. As a result, when wet extrusion processing is performed, a high-quality molded product, for example, a separator for a secondary battery with reduced thickness variation and high breaking strength, or a fiber with reduced yarn diameter variation and capable of being stretched at high speed can be obtained.

[0040] The method for controlling the proportion of voids in the ultra-high molecular weight polyethylene powder within the above range is not particularly limited, but examples include a method in which a polymer obtained by prepolymerization is used as a prepolymerization catalyst under high pressure conditions (hereinafter also referred to as control method 1), a method in which polymerization is performed using a precipitation-type catalyst in which the catalyst particle size is fine and has little variation in particle size, and then drying at high temperature while rotating at high speed (hereinafter also referred to as control method 2), and a method in which only the fine powder polymer is collected by classification, and then dried again while rotating at high temperature while rotating at high speed (hereinafter also referred to as control method 3).

[0041] The mechanism by which the proportion of dilute or void portions in the ultra-high molecular weight polyethylene powder can be controlled within the above range by the above-mentioned method is not clear and is not limited to the following, but the inventors presume it as follows.

[0042] Regarding the method of control method 1, the reason is unclear and is not limited to the following, but it is possible to carry out polymerization under high pressure conditions using a prepolymerization catalyst, so that the polymerization can be carried out in a state where the initial polymerization activity is high. Therefore, it is considered that a large amount of polymerization heat energy is generated in the polymerization process, and in the process in which the heat energy escapes from the center of the powder to the outside, voids are formed in the center of the powder.

[0043] The reason for the above control method 2 is unclear and is not limited to the following, but by carrying out polymerization using a precipitation-type catalyst with a fine catalyst particle size and little variation in particle size, primary polymer particles with small and uniform particle sizes are produced. The primary polymer particles are dried at high temperature while rotating at high speed, controlling the number of contacts between the primary polymer particles, and the contact points are partially fused to form a powder in which the primary polymer particles are aggregated. It is believed that the powder has a structure with voids between the primary polymer particles, and a structure with voids in the center of the powder is formed.

[0044] The reason for the above-mentioned control method 3 is unclear and is not limited to the following, but the powder polymerized using a precipitation catalyst is classified and only the fine powder component is collected. The fine powder component is dried at high temperature while rotating at high speed, thereby controlling the number of contacts between the fine powders, and the contact points are partially fused to form a powder in which the fine powders are aggregated together. It is believed that the powder has a structure with voids between the fine powders, and a structure with voids in the center of the powder is formed.

[0045] [Ratio of fine and coarse powder components in ultra-high molecular weight polyethylene powder] In the ultra-high molecular weight polyethylene powder of this embodiment, the proportion of ultra-high molecular weight polyethylene powder having a particle size of 300 μm or more is 10 mass% or less, preferably 8 mass% or less, more preferably 6 mass% or less, and most preferably 4 mass% or less, based on the total amount of the ultra-high molecular weight polyethylene powder. Also, the proportion of ultra-high molecular weight polyethylene powder having a particle size of less than 53 μm is 20 mass% or less, preferably 15 mass% or less, more preferably 10 mass% or less, and most preferably 6 mass% or less, based on the total amount of the ultra-high molecular weight polyethylene powder.

[0046] When wet extrusion processing ultra-high molecular weight polyethylene powder, there is a step of impregnating the ultra-high molecular weight polyethylene powder with liquid paraffin as a preliminary step. This step is carried out while stirring at a temperature below the melting point of the ultra-high molecular weight polyethylene powder, so that the liquid paraffin penetrates into the amorphous part through the pores in the powder, and the powder swells and expands in the process of disentangling the molecular chains. At this time, the time until the swelling is completed (swelling time; the time until the powder is impregnated with liquid paraffin and the equivalent circle diameter of the powder becomes maximum) differs depending on the particle diameter of the powder, and the swelling time is long for particles with a large particle diameter (hereinafter also referred to as coarse powder component) and short for particles with a small particle diameter (hereinafter also referred to as fine powder component). In other words, if the swelling time is not sufficient to match the coarse powder component, it is not possible to obtain a uniform gel in which the molecular chains are disentangled. If the swelling time is shortened in accordance with the fine powder component, the coarse powder component is fed into the extruder in an insufficiently swollen state, so that the fine powder component starts to melt first and fuses to the surface of the coarse powder component, further inhibiting the swelling of the coarse powder component. For this reason, all the powder melts without fully disentangling the molecular chains of the coarse powder component, so that a uniform gel cannot be obtained. However, taking a long swelling time in accordance with the coarse powder component is poor in production efficiency. Therefore, it is important to reduce the time difference until the swelling between the powders is completed by controlling the fine powder component and the coarse powder component within the above range, and by doing so, a higher quality molded body can be obtained when wet extrusion processing is performed. In this embodiment, the particle size distribution is not particularly limited, but can be determined, for example, by the method described in the examples described later.

[0047] The method for controlling the particle size of the ultra-high molecular weight polyethylene powder of this embodiment within the above range is not particularly limited, but for example, it can be controlled by adjusting the particle size and / or amount of the catalyst used in polymerization. By adjusting the particle size of the catalyst, the particle size of the ultra-high molecular weight polyethylene powder produced can be controlled. Furthermore, by polymerizing using a catalyst in which catalysts with various particle sizes are mixed, the content of each particle size in the ultra-high molecular weight polyethylene powder produced can also be controlled.

[0048] [Crystallization of ultra-high molecular weight polyethylene powder] Moreover, the ultra-high molecular weight polyethylene powder of this embodiment has a crystallinity of 70% or more and 85% or less, preferably 70% or more and 83% or less, more preferably 72% or more and 83% or less, and most preferably 74% or more and 83% or less. The ultra-high molecular weight polyethylene powder of this embodiment has a crystallinity of 70% or more, which allows a molded product with high strength to be obtained. This is presumably because the proportion of amorphous parts is small, which makes it easy to form a uniform gel in which the entanglement of molecular chains is released. Furthermore, the ultra-high molecular weight polyethylene powder of this embodiment has a crystallinity of 85% or less, which makes it easy to mold, i.e., tends to have excellent moldability.

[0049] In this embodiment, the method for controlling the crystallinity of the ultra-high molecular weight polyethylene powder to the above range is not particularly limited, but for example, it is considered that polymerization is performed using a hexane solvent containing 0.05 to 0.5 g of a low molecular weight polyethylene component (molecular weight 1,000 to 3,000) per 1 L of hexane solvent, whereby the low molecular weight polyethylene component acts as a crystal nucleating agent to promote crystallization. Note that in this embodiment, the crystallinity is not particularly limited, but can be determined, for example, by the method described in the Examples below.

[0050] [Apparent density of ultra-high molecular weight polyethylene powder] In addition, the ultra-high molecular weight polyethylene powder of the present embodiment has an apparent density of 0.45 g / cm 3 or less, preferably 0.43 g / cm 3 More preferably, it is 0.41 g / cm or less. 3 or less, most preferably 0.39 g / cm 3 The ultra-high molecular weight polyethylene powder of the present embodiment has an apparent density of 0.45 g / cm 3 By satisfying the above condition, the composition can be smoothly sent from the extruder hopper into the extruder without clogging in the hopper, and excellent moldability can be achieved.

[0051] Here, in the present embodiment, the apparent density means the density of the powder when the powder is filled to the brim in a container of a certain volume and the internal volume is taken as the volume. That is, the apparent density of the ultra-high molecular weight polyethylene powder means the mass of the ultra-high molecular weight polyethylene powder per unit volume in the above-mentioned container of a certain volume. A specific method for calculating the apparent density in the present embodiment is not particularly limited, but it can be determined, for example, by the method described in the Examples below.

[0052] In this embodiment, the method for controlling the apparent density of the ultra-high molecular weight polyethylene powder to be within the above range is not particularly limited, but for example, as described above, it can be adjusted by controlling the proportion of voids in the ultra-high molecular weight polyethylene powder.

[0053] [Titanium (Ti) content in ultra-high molecular weight polyethylene powder] The ultra-high molecular weight polyethylene powder of this embodiment has a titanium (Ti) content of 10 ppm or less, preferably 8 ppm or less, more preferably 6 ppm or less, and even more preferably 4 ppm or less. Generally, a large amount of metal derived from catalyst residue remaining in the ultra-high molecular weight polyethylene powder tends to cause uneven thickness of the molded product, but the ultra-high molecular weight polyethylene powder of this embodiment tends to have excellent quality by adjusting the titanium content to such a range. In addition, safety tends to be improved when used for batteries.

[0054] The Ti content in the ultra-high molecular weight polyethylene powder can be controlled by the productivity of the ethylene homopolymer or ethylene-based polymer per unit catalyst. The productivity of the ethylene homopolymer or ethylene-based polymer can be controlled by the polymerization temperature, polymerization pressure, and slurry concentration of the reactor during production. That is, the productivity of the ethylene homopolymer or ethylene-based polymer used in this embodiment can be increased, but is not particularly limited, by, for example, increasing the polymerization temperature, increasing the polymerization pressure, and / or increasing the slurry concentration. As other methods, the titanium content can be controlled by selecting the type of promoter component, decreasing the concentration of the promoter component, or washing the ethylene homopolymer or ethylene-based polymer with an acid or alkali when polymerizing the ethylene homopolymer or ethylene-based polymer.

[0055] The method for measuring the Ti content is not particularly limited, but can be carried out, for example, by the method described in the Examples below.

[0056] [Method of manufacturing ultra-high molecular weight polyethylene powder] The method for producing the ultra-high molecular weight polyethylene powder of this embodiment will be described in detail below.

[0057] (Catalyst Component) The catalyst component used in the production of the ultra-high molecular weight polyethylene powder according to the present embodiment is not particularly limited, but examples thereof include general Ziegler-Natta catalysts and metallocene catalysts. <Ziegler-Natta catalyst> The Ziegler-Natta catalyst is preferably a catalyst comprising a solid catalyst component [A] and an organometallic compound component [B], in which the solid catalyst component [A] is an olefin polymerization catalyst produced by reacting an organomagnesium compound (A-1) represented by the following formula 1, which is soluble in an inert hydrocarbon solvent, with a titanium compound (A-2) represented by the following formula 2. (A-1):(M 1 )α(Mg)β(R 2 ) a (R 3 )b (Y 1 ) c ...Formula 1 (In formula 1, M 1 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 is alkoxy, siloxy, aryloxy, amino, amido, -N=CR 4 , R 5 , -SR 6 (where R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other.) or a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0≦c, 0 <a+b、0≦c / (α+β)≦2、nα+2β=a+b+c(ここで、nはM 1 Represents the valence of .

[0058] (A-2): Ti(OR 7 ) d X 1 (4-d) ...Formula 2 (In formula 2, d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)

[0059] The inert hydrocarbon solvent used in the reaction of (A-1) and (A-2) is not particularly limited, but specific examples include aliphatic hydrocarbons such as pentane, hexane, and heptane; aromatic hydrocarbons such as benzene and toluene; and alicyclic hydrocarbons such as cyclohexane and methylcyclohexane.

[0060] First, (A-1) will be described. (A-1) is shown in the form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, and includes all dihydrocarbylmagnesium compounds and complexes of these compounds with other metal compounds. The relational formula nα+2β=a+b+c of the symbols α, β, a, b, and c indicates the stoichiometry of the valence of the metal atom and the substituent.

[0061] In formula 1, R 2 and R 3 The hydrocarbon group having 2 to 20 carbon atoms represented by the formula (1) is not particularly limited, but specific examples thereof include an alkyl group, a cycloalkyl group, and an aryl group, such as ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, cyclohexyl, and phenyl groups. Among these, an alkyl group is preferable. When α>0, the metal atom M 1 As the metal atom, a metal atom belonging to the group consisting of Groups 12, 13, and 14 of the periodic table can be used, and although there is no particular limitation, examples thereof include zinc, boron, aluminum, etc. Among these, aluminum and zinc are preferred.

[0062] metal atom M 1 The ratio β / α of magnesium to R is not particularly limited, but is preferably 0.1 to 30, and more preferably 0.5 to 10. When a certain organomagnesium compound with α=0 is used, it is not particularly limited, but for example, 2 In the case where R is 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also gives a preferable result in this embodiment. 2 , R 3 It is recommended that patients meet one of the following three groups: (1), (2), or (3).

[0063] Group(1):R 2 , R 3 At least one of R is a secondary or tertiary alkyl group having 4 to 6 carbon atoms. 2 , R 3are both alkyl groups having 4 to 6 carbon atoms, and at least one of them is a secondary or tertiary alkyl group. Group(2):R 2 and R 3 and R are alkyl groups having different numbers of carbon atoms. 2 is an alkyl group having 2 or 3 carbon atoms, and R 3 is an alkyl group having 4 or more carbon atoms. Group(3):R 2 , R 3 At least one of R is a hydrocarbon group having 6 or more carbon atoms. 2 , R 3 The alkyl group must have 12 or more carbon atoms when added together.

[0064] Specific examples of these groups are shown below. In group (1), the secondary or tertiary alkyl group having 4 to 6 carbon atoms is not particularly limited, but specific examples include 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, 2-methylbutyl, 2-ethylpropyl, 2,2-dimethylpropyl, 2-methylpentyl, 2-ethylbutyl, 2,2-dimethylbutyl, and 2-methyl-2-ethylpropyl groups. Among these, the 1-methylpropyl group is particularly preferred.

[0065] In addition, the alkyl group having 2 or 3 carbon atoms in group (2) is not particularly limited, but specific examples thereof include ethyl, 1-methylethyl, and propyl groups. Among these, the ethyl group is particularly preferred. In addition, the alkyl group having 4 or more carbon atoms is not particularly limited, but specific examples thereof include butyl, pentyl, hexyl, heptyl, and octyl groups. Among these, the butyl and hexyl groups are particularly preferred.

[0066] Furthermore, in group (3), the hydrocarbon group having 6 or more carbon atoms is not particularly limited, but specific examples include hexyl, heptyl, octyl, nonyl, decyl, phenyl, 2-naphthyl groups, etc. Among the hydrocarbon groups, alkyl groups are preferred, and among the alkyl groups, hexyl and octyl groups are particularly preferred.

[0067] Generally, the more carbon atoms contained in the alkyl group, the more easily the compound dissolves in an inert hydrocarbon solvent, and the more the viscosity of the solution tends to increase. Therefore, it is preferable to use an alkyl group with a moderately long chain in terms of handling. The above-mentioned organomagnesium compound can be used after diluting with an inert hydrocarbon solvent, but it can be used without any problem even if a small amount of Lewis basic compound such as ether, ester, or amine is contained or remains in the solution.

[0068] Next, Y 1 In formula 1, Y 1 is alkoxy, siloxy, aryloxy, amino, amido, -N=CR 4 ,R 5 , -SR 6 (where R 4 , R 5 and R 6 each independently represents a hydrocarbon group having 2 to 20 carbon atoms, or a β-keto acid residue.

[0069] In formula 1, R 4 , R 5 and R 6The hydrocarbon group represented by the formula (I) is preferably an alkyl group or aryl group having 1 to 12 carbon atoms, particularly preferably an alkyl group or aryl group having 3 to 10 carbon atoms. Although not particularly limited, examples thereof include methyl, ethyl, propyl, 1-methylethyl, butyl, 1-methylpropyl, 1,1-dimethylethyl, pentyl, hexyl, 2-methylpentyl, 2-ethylbutyl, 2-ethylpentyl, 2-ethylhexyl, 2-ethyl-4-methylpentyl, 2-propylheptyl, 2-ethyl-5-methyloctyl, octyl, nonyl, decyl, phenyl, naphthyl groups, etc. Among these, butyl, 1-methylpropyl, 2-methylpentyl, and 2-ethylhexyl groups are particularly preferred.

[0070] In addition, in formula 1, Y 1 is preferably an alkoxy group or a siloxy group. The alkoxy group is not particularly limited, but specifically, for example, methoxy, ethoxy, propoxy, 1-methylethoxy, butoxy, 1-methylpropoxy, 1,1-dimethylethoxy, pentoxy, hexoxy, 2-methylpentoxy, 2-ethylbutoxy, 2-ethylpentoxy, 2-ethylhexoxy, 2-ethyl-4-methylpentoxy, 2-propylheptoxy, 2-ethyl-5-methyloctoxy, octoxy, phenoxy, and naphthoxy groups are preferred. Among these, butoxy, 1-methylpropoxy, 2-methylpentoxy, and 2-ethylhexoxy groups are more preferred. The siloxy group is not particularly limited, but specifically, for example, hydrodimethylsiloxy, ethylhydromethylsiloxy, diethylhydrosiloxy, trimethylsiloxy, ethyldimethylsiloxy, diethylmethylsiloxy, and triethylsiloxy groups are preferred. Of these, hydrodimethylsiloxy, ethylhydromethylsiloxy, diethylhydrosiloxy and trimethylsiloxy groups are more preferred.

[0071] In this embodiment, the synthesis method of (A-1) is not particularly limited. For example, 2 MgX 1 , and formula R 2 Mg(R 2has the meaning mentioned above, and X 1 is a halogen.) and an organomagnesium compound of the formula M 1 R 3 n and M 1 R 3 (n-1) H(M 1 , and R 3 has the meaning as above, and n is M 1 ) in an inert hydrocarbon solvent at 25° C. to 150° C., and then, if necessary, reacting the compound with an organometallic compound of the formula Y 1 -H(Y 1 has the above-mentioned meaning.) or Y 1 Among these, the compound can be synthesized by reacting an organomagnesium compound and / or an organoaluminum compound having a functional group represented by the formula Y 1 When reacting a compound represented by formula Y with an organomagnesium compound, the order of addition to the reaction system is not particularly limited. 1 -H, a method of adding a compound represented by the formula Y 1 Either a method of adding the organomagnesium compound to the compound represented by --H or a method of adding both simultaneously can be used.

[0072] In this embodiment, Y relative to all metal atoms in (A-1) 1 The molar composition ratio c / (α+β) of is 0≦c / (α+β)≦2, and preferably 0≦c / (α+β)<1. 1 When the molar composition ratio of is 2 or less, the reactivity of (A-1) with respect to (A-2) tends to be improved.

[0073] Next, (A-2) will be described. (A-2) is a titanium compound represented by formula 2. (A-2): Ti(OR 7 ) d X 1 (4-d) ...Formula 2 (In formula 2, d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)

[0074] In the above formula 2, d is preferably 0 or more and 1 or less, and more preferably 0. 7 The hydrocarbon group represented by the formula (I) is not particularly limited, but specific examples thereof include aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, 2-ethylhexyl, heptyl, octyl, decyl, and allyl groups; alicyclic hydrocarbon groups such as cyclohexyl, 2-methylcyclohexyl, and cyclopentyl groups; and aromatic hydrocarbon groups such as phenyl and naphthyl groups. Among these, aliphatic hydrocarbon groups are preferred. X 1 The halogen represented by the formula (I) may be, for example, chlorine, bromine, or iodine. Among these, chlorine is preferred. In this embodiment, (A-2) is particularly preferably titanium tetrachloride. In this embodiment, it is possible to use a mixture of two or more of the compounds selected from the above.

[0075] Next, the reaction between (A-1) and (A-2) will be described. The reaction is preferably carried out in an inert hydrocarbon solvent, more preferably in an aliphatic hydrocarbon solvent such as hexane or heptane. The molar ratio of (A-1) to (A-2) in the reaction is not particularly limited, but the molar ratio (Ti / Mg) of Ti atoms contained in (A-2) to Mg atoms contained in (A-1) is preferably 0.1 to 10, more preferably 0.3 to 3. The reaction temperature is not particularly limited, but is preferably carried out in the range of -80°C to 150°C, more preferably -40°C to 100°C. The order of addition of (A-1) and (A-2) is not particularly limited, and any of the following methods is possible: adding (A-2) after (A-1), adding (A-2) after (A-1), or adding (A-1) and (A-2) simultaneously, but the method of adding (A-1) and (A-2) simultaneously is preferred. In this embodiment, the solid catalyst component [A] obtained by the above reaction is used as a slurry solution using an inert hydrocarbon solvent.

[0076] Another example of the Ziegler-Natta catalyst component used in this embodiment is preferably an olefin polymerization catalyst comprising a solid catalyst component [C] and an organometallic compound component [B], the solid catalyst component [C] being produced by supporting an organomagnesium compound (C-4) represented by formula 5 and a titanium compound (C-5) represented by formula 6, which are soluble in an inert hydrocarbon solvent, on a support (C-3) prepared by reacting an organomagnesium compound (C-1) represented by formula 3 and soluble in an inert hydrocarbon solvent with a chlorinating agent (C-2) represented by formula 4.

[0077] (C-1):(M 2 )γ(Mg)δ(R 8 ) e (R 9 ) f (OR 10 ) g ...Formula 3 (In formula 3, M 2 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 8 , R9 and R 10 are hydrocarbon groups having 1 to 20 carbon atoms, and γ, δ, e, f, and g are real numbers that satisfy the following relationships: 0≦γ, 0<δ, 0≦e, 0≦f, 0≦g, 0 <e+f、0≦g / (γ+δ)≦2、kγ+2δ=e+f+g(ここで、kはM 2 Represents the valence of .

[0078] (C-2):H h SiCl i R 11 (4-(h+i)) ...Formula 4 (In formula 4, R 11 is a hydrocarbon group having 1 to 12 carbon atoms, and h and i are real numbers that satisfy the following relationship: 0 <h、0<i、0<h+i≦4)

[0079] (C-4):(M 1 )α(Mg)β(R 2 ) a (R 3 ) b Y 1 c ...Formula 5 (In formula 5, M 1 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 is alkoxy, siloxy, aryloxy, amino, amido, -N=CR 4 ,R 5 , -SR 6 (where R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other.) or a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0≦c, 0 <a+b、0≦c / (α+β)≦2、nα+2β=a+b+c(ここで、nはM 1 Represents the valence of .

[0080] (C-5): Ti(OR 7 ) d X 1 (4-d) ...Formula 6 (In formula 6, d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)

[0081] First, (C-1) will be explained. (C-1) is shown as a form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, but it includes all dihydrocarbylmagnesium compounds and complexes of this compound with other metal compounds. The relational formula kγ+2δ=e+f+g of the symbols γ, δ, e, f, and g in formula 3 indicates the stoichiometry of the valence of the metal atom and the substituent.

[0082] In the above formula 3, R 8 Or R 9 The hydrocarbon group represented by is not particularly limited, but specifically, it is an alkyl group, a cycloalkyl group, or an aryl group, and examples thereof include methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, cyclohexyl, and phenyl groups. Among these, R 8 and R 9 are alkyl groups. When γ>0, the metal atom M 2 As the metal atom, a metal atom belonging to the group consisting of Groups 12, 13, and 14 of the periodic table can be used, and although there is no particular limitation, examples thereof include zinc, boron, aluminum, etc. Among these, aluminum and zinc are particularly preferred.

[0083] metal atom M 2 The ratio δ / γ of magnesium to R is not particularly limited, but is preferably 0.1 to 30, more preferably 0.5 to 10. When a certain organomagnesium compound with γ=0 is used, for example, R 8 In the case where R is 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also gives a preferable result in this embodiment.8 , R 9 It is recommended that patients be in one of the following three groups: (1), (2), or (3).

[0084] Group(1):R 8 , R 9 At least one of R is a secondary or tertiary alkyl group having 4 to 6 carbon atoms. 8 , R 9 Both have 4 to 6 carbon atoms, and at least one of them is a secondary or tertiary alkyl group. Group(2):R 8 and R 9 and R are alkyl groups having different carbon numbers. 8 is an alkyl group having 2 or 3 carbon atoms, and R 9 is an alkyl group having 4 or more carbon atoms. Group(3):R 8 , R 9 At least one of R is a hydrocarbon group having 6 or more carbon atoms. 8 , R 9 The sum of the carbon atoms contained in the alkyl group is 12 or more.

[0085] Specific examples of these groups are shown below. In group (1), specific examples of the secondary or tertiary alkyl group having 4 to 6 carbon atoms include 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, 2-methylbutyl, 2-ethylpropyl, 2,2-dimethylpropyl, 2-methylpentyl, 2-ethylbutyl, 2,2-dimethylbutyl, and 2-methyl-2-ethylpropyl groups. Among these, the 1-methylpropyl group is particularly preferred.

[0086] In addition, in group (2), the alkyl group having 2 or 3 carbon atoms is not particularly limited, but examples thereof include ethyl, 1-methylethyl, and propyl groups. Among these, the ethyl group is particularly preferred. In addition, the alkyl group having 4 or more carbon atoms is not particularly limited, but specific examples thereof include butyl, pentyl, hexyl, heptyl, and octyl groups. Among these, the butyl and hexyl groups are particularly preferred.

[0087] Furthermore, in group (3), the hydrocarbon group having 6 or more carbon atoms is not particularly limited, but specific examples include hexyl, heptyl, octyl, nonyl, decyl, phenyl, 2-naphthyl groups, etc. Among the hydrocarbon groups, alkyl groups are preferred, and among the alkyl groups, hexyl and octyl groups are particularly preferred.

[0088] Generally, the more carbon atoms contained in the alkyl group, the more easily the compound dissolves in an inert hydrocarbon solvent, and the more the viscosity of the solution tends to increase. Therefore, it is preferable to use an alkyl group with a moderate chain length in terms of handling. The above-mentioned organomagnesium compound is used as an inert hydrocarbon solution, but it can be used without any problem even if a small amount of Lewis basic compound such as ether, ester, or amine is contained or remains in the solution.

[0089] Next, the alkoxy group (OR 10 ) will be explained. 10 The hydrocarbon group represented by the formula (I) is preferably an alkyl group or aryl group having 1 to 12 carbon atoms, particularly preferably an alkyl group or aryl group having 3 to 10 carbon atoms. 10is not particularly limited, specific examples thereof include methyl, ethyl, propyl, 1-methylethyl, butyl, 1-methylpropyl, 1,1-dimethylethyl, pentyl, hexyl, 2-methylpentyl, 2-ethylbutyl, 2-ethylpentyl, 2-ethylhexyl, 2-ethyl-4-methylpentyl, 2-propylheptyl, 2-ethyl-5-methyloctyl, octyl, nonyl, decyl, phenyl, naphthyl groups, etc. Among these, butyl, 1-methylpropyl, 2-methylpentyl and 2-ethylhexyl groups are particularly preferred.

[0090] In this embodiment, the synthesis method of (C-1) is not particularly limited, but it is preferable to use a compound represented by the formula R 8 MgX 1 and formula R 8 Mg(R 8 has the meaning mentioned above, and X 1 is a halogen atom.) and an organomagnesium compound of the formula M 2 R 9 k and formula M 2 R 9 (k-1) H(M 2 , R 9 and k has the same meaning as above) in an inert hydrocarbon solvent at a temperature of 25° C. to 150° C., and if necessary, subsequently reacting with R 9 (R 9 has the above meaning.) R soluble in alcohol or inert hydrocarbon solvent having a hydrocarbon group represented by 9 In another preferred method, the compound is reacted with an alkoxy magnesium compound having a hydrocarbon group represented by the following formula: and / or an alkoxy aluminum compound.

[0091] Among these, when an organomagnesium compound soluble in an inert hydrocarbon solvent is reacted with an alcohol, there is no particular restriction on the order of addition to the reaction system, and any of the following methods can be used: adding the alcohol to the organomagnesium compound, adding the organomagnesium compound to the alcohol, or adding both at the same time. In this embodiment, the reaction ratio of the organomagnesium compound soluble in an inert hydrocarbon solvent and the alcohol is not particularly limited, but the molar composition ratio g / (γ+δ) of the alkoxy group to the total metal atom in the alkoxy group-containing organomagnesium compound obtained as a result of the reaction is 0≦g / (γ+δ)≦2, and preferably 0≦g / (γ+δ)<1.

[0092] Next, (C-2) will be described. (C-2) is a silicon chloride compound represented by formula 4 and having at least one Si—H bond.

[0093] (C-2):H h SiCl i R 11 (4-(h+i)) ...Formula 4 (In formula 4, R 11 is a hydrocarbon group having 1 to 12 carbon atoms, and h and i are real numbers that satisfy the following relationship: 0 <h、0<i、0<h+i≦4)

[0094] In Equation 4, R 11 The hydrocarbon group represented by is not particularly limited, but specifically includes an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group, such as methyl, ethyl, propyl, 1-methylethyl, butyl, pentyl, hexyl, octyl, decyl, cyclohexyl, and phenyl groups. Among these, alkyl groups having 1 to 10 carbon atoms are preferred, and alkyl groups having 1 to 3 carbon atoms, such as methyl, ethyl, propyl, and 1-methylethyl groups, are more preferred. Furthermore, h and i are numbers greater than 0 that satisfy the relationship h+i≦4, and it is preferred that i is 2 to 3.

[0095] These compounds are not particularly limited, but specific examples include HSiCl3, HSiCl2CH3, HSiCl2C2H5, HSiCl2(C3H7), HSiCl2(2-C3H7), HSiCl2(C4H9), HSiCl2(C6H5), HSiCl2(4-Cl-C6H4), HSiCl2(CH=CH2), HSiCl2(CH2C6H5), HSiCl2(1-C 10 H7), HSiCl2(CH2CH=CH2), H2SiCl(CH3), H2SiCl(C2H5), HSiCl(CH3)2, HSiCl(C2H5)2, HSiCl(CH3)(2-C3H7), HSiCl(CH3)(C6H5), HSiCl(C6H5)2, etc. Silicon chloride compounds consisting of these compounds or mixtures of two or more selected from these compounds are used. Among these, HSiCl3, HSiCl2CH3, HSiCl(CH3)2, and HSiCl2(C3H7) are preferred, and HSiCl3 and HSiCl2CH3 are more preferred.

[0096] Next, the reaction between (C-1) and (C-2) will be described. In the reaction, it is preferable to dilute (C-2) in advance with an inert hydrocarbon solvent, chlorinated hydrocarbon such as 1,2-dichloroethane, o-dichlorobenzene, dichloromethane, etc.; ether medium such as diethyl ether, tetrahydrofuran, etc.; or a mixture of these. Among these, inert hydrocarbon solvents are more preferable in terms of catalyst performance. The reaction ratio between (C-1) and (C-2) is not particularly limited, but the silicon atom contained in (C-2) is preferably 0.01 mol or more and 100 mol or less, more preferably 0.1 mol or more and 10 mol or less, per 1 mol of magnesium atom contained in (C-1).

[0097] There is no particular restriction on the reaction method between (C-1) and (C-2), and any of the following methods can be used: simultaneous addition method in which (C-1) and (C-2) are simultaneously introduced into a reactor and reacted; method in which (C-2) is charged in advance into a reactor and then (C-1) is introduced into the reactor; or method in which (C-1) is charged in advance into a reactor and then (C-2) is introduced into the reactor. Among these, the method in which (C-2) is charged in advance into a reactor and then (C-1) is introduced into the reactor is preferred. The support (C-3) obtained by the above reaction is preferably separated by filtration or decantation, and then thoroughly washed with an inert hydrocarbon solvent to remove unreacted materials or by-products.

[0098] The reaction temperature between (C-1) and (C-2) is not particularly limited, but is preferably 25°C to 150°C, more preferably 30°C to 120°C, and even more preferably 40°C to 100°C. In the simultaneous addition method in which (C-1) and (C-2) are simultaneously introduced into a reactor and reacted, it is preferable to adjust the temperature of the reactor to a predetermined temperature in advance, and adjust the temperature in the reactor to a predetermined temperature while performing the simultaneous addition, thereby adjusting the reaction temperature to a predetermined temperature. In the method in which (C-2) is charged in a reactor in advance and then (C-1) is introduced into the reactor, it is preferable to adjust the temperature of the reactor charged with (C-2) to a predetermined temperature, and adjust the temperature in the reactor to a predetermined temperature while introducing (C-1) into the reactor, thereby adjusting the reaction temperature to a predetermined temperature. In the method of charging (C-1) into a reactor in advance and then introducing (C-2) into the reactor, it is preferable to adjust the temperature of the reactor into which (C-1) has been charged to a predetermined temperature, and then adjust the temperature inside the reactor to a predetermined temperature while introducing (C-2) into the reactor, thereby adjusting the reaction temperature to a predetermined temperature.

[0099] Next, the organomagnesium compound (C-4) will be described. As (C-4), the compound represented by the above formula 5 is preferable. (C-4):(M 1 )α(Mg)β(R 2 ) a (R 3 )b Y 1 c ...Formula 5 (In formula 5, M 1 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 is alkoxy, siloxy, aryloxy, amino, amido, -N=CR 4 ,R 5 , -SR 6 (where R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other.) or a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0 <a+b、0≦c / (α+β)≦2、nα+2β=a+b+c(ここで、nはM 1 Represents the valence of .

[0100] The amount of (C-4) used is preferably 0.1 or more and 10 or less, more preferably 0.5 or more and 5 or less, in terms of the molar ratio of magnesium atoms contained in (C-4) to titanium atoms contained in (C-5).

[0101] The temperature for the reaction of (C-4) and (C-5) is not particularly limited, but is preferably in the range of -80°C or higher and 150°C or lower, and more preferably in the range of -40°C or higher and 100°C or lower.

[0102] The concentration of (C-4) when used is not particularly limited, but is preferably 0.1 mol / L or more and 2 mol / L or less, and more preferably 0.5 mol / L or more and 1.5 mol / L or less, based on the titanium atoms contained in (C-4). It is preferable to use an inert hydrocarbon solvent to dilute (C-4).

[0103] There is no particular restriction on the order of addition of (C-4) and (C-5) to (C-3), and any of the following methods is possible: adding (C-4) followed by (C-5), adding (C-4) followed by (C-5), or adding (C-4) and (C-5) simultaneously. Among these, the method of adding (C-4) and (C-5) simultaneously is preferred. The reaction between (C-4) and (C-5) is carried out in an inert hydrocarbon solvent, and it is preferable to use an aliphatic hydrocarbon solvent such as hexane or heptane. The catalyst thus obtained is used as a slurry solution using an inert hydrocarbon solvent.

[0104] Next, (C-5) will be described. In this embodiment, (C-5) is a titanium compound represented by the above formula 6.

[0105] (C-5): Ti(OR 7 ) d X 1 (4-d) ...Formula 6 (In formula 6, d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)

[0106] In Equation 6, R 7 The hydrocarbon group represented by the formula (I) is not particularly limited, but specific examples thereof include aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, 2-ethylhexyl, heptyl, octyl, decyl, and allyl groups; alicyclic hydrocarbon groups such as cyclohexyl, 2-methylcyclohexyl, and cyclopentyl groups; and aromatic hydrocarbon groups such as phenyl and naphthyl groups. Among these, aliphatic hydrocarbon groups are preferred. X 1 The halogen represented by is not particularly limited, but specifically includes, for example, chlorine, bromine, and iodine. Among these, chlorine is preferable. The (C-5) selected from the above may be used alone or in combination of two or more.

[0107] The amount of (C-5) used is not particularly limited, but the molar ratio of titanium atoms contained in the titanium compound (C-5) to magnesium atoms contained in the carrier (C-3) is preferably 0.01 or more and 20 or less, and particularly preferably 0.05 or more and 10 or less.

[0108] The reaction temperature of (C-5) is not particularly limited, but is preferably in the range of -80°C or higher and 150°C or lower, and more preferably in the range of -40°C or higher and 100°C or lower. In this embodiment, the method for supporting (C-5) on (C-3) is not particularly limited. A method of reacting an excess of (C-5) with (C-3) or a method of efficiently supporting (C-5) by using a third component may be used, but a method of supporting (C-5) by reacting (C-5) with an organomagnesium compound (C-4) is preferred.

[0109] Next, the organometallic compound component [B] used in this embodiment will be described. The solid catalyst component used in this embodiment becomes a highly active polymerization catalyst by combining with the organometallic compound component [B]. The organometallic compound component [B] is sometimes called a "co-catalyst." The organometallic compound component [B] is preferably a compound containing a metal belonging to the group consisting of Groups 1, 2, 12, and 13 of the periodic table, and is particularly preferably an organoaluminum compound and / or an organomagnesium compound.

[0110] As the organoaluminum compound, it is preferable to use a compound represented by the following formula 7 alone or in combination.

[0111] AlR 12 j Z 1 (3-j) ...Formula 7 (In formula 7, R 12 is a hydrocarbon group having 1 to 20 carbon atoms, Z 1 is a radical belonging to the group consisting of hydrogen, halogen, alkoxy, aryloxy, and siloxy groups, and j is a number between 2 and 3.

[0112] In the above formula 7, R 12 The hydrocarbon group having 1 to 20 carbon atoms represented by the formula (1) is not particularly limited, but specifically includes an aliphatic hydrocarbon group, an aromatic hydrocarbon group, and an alicyclic hydrocarbon group, and is preferably, for example, trialkylaluminum such as trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, tri(2-methylpropyl)aluminum (or triisobutylaluminum), tripentylaluminum, tri(3-methylbutyl)aluminum, trihexylaluminum, trioctylaluminum, or tridecylaluminum, halogenated aluminum compounds such as diethylaluminum chloride, ethylaluminum dichloride, bis(2-methylpropyl)aluminum chloride, ethylaluminum sesquichloride, or diethylaluminum bromide, alkoxyaluminum compounds such as diethylaluminum ethoxide or bis(2-methylpropyl)aluminum butoxide, siloxyaluminum compounds such as dimethylhydrosiloxyaluminum dimethyl, ethylmethylhydrosiloxyaluminum diethyl, or ethyldimethylsiloxyaluminum diethyl, or mixtures thereof. Among these, trialkylaluminum compounds are particularly preferred.

[0113] As the organomagnesium compound, an organomagnesium compound which is soluble in an inert hydrocarbon solvent and is represented by the above formula 3 is preferred.

[0114] (M 2 )γ(Mg)δ(R 8 ) e (R 9 ) f (OR 10 ) g ...Formula 3 (In formula 3, M 2 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 8 , R 9 and R 10are hydrocarbon groups having 1 to 20 carbon atoms, and γ, δ, e, f, and g are real numbers that satisfy the following relationships: 0≦γ, 0<δ, 0≦e, 0≦f, 0≦g, 0 <e+f、0≦g / (γ+δ)≦2、kγ+2δ=e+f+g(ここで、kはM 2 Represents the valence of .

[0115] The organomagnesium compound is shown in the form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, but includes all dihydrocarbylmagnesium compounds and complexes of this compound with other metal compounds. 2 , R 8 , R 9 , OR 10 As already mentioned, it is preferable that the organomagnesium compound has high solubility in an inert hydrocarbon solvent, so that δ / γ is preferably in the range of 0.5 to 10. 2 More preferred are compounds in which is aluminum. The combination ratio of the solid catalyst component and the organometallic compound component [B] is not particularly limited, but it is preferable that the organometallic compound component [B] is 1 mmol or more and 3,000 mmol or less per 1 g of the solid catalyst component.

[0116] <Metallocene catalyst> As an example of using a metallocene catalyst, a general transition metal compound is used. The method for producing the metallocene catalyst is not particularly limited, but for example, the method described in Japanese Patent No. 4868853 can be mentioned. Such a metallocene catalyst is composed of two catalyst components: (a) a transition metal compound having a cyclic η-bonding anion ligand, and (b) an activator capable of forming a complex that expresses catalytic activity by reacting with the transition metal compound.

[0117] The transition metal compound having a cyclic η-bonding anion ligand used in this embodiment can be represented, for example, by the following formula 8. L 1 j W k M 3 X2 p X 3 q ...Formula 8

[0118] In Equation 8, L 1 each independently represents an η-bonding cyclic anionic ligand selected from the group consisting of a cyclopentadienyl group, an indenyl group, a tetrahydroindenyl group, a fluorenyl group, a tetrahydrofluorenyl group, and an octahydrofluorenyl group, and the ligand optionally has 1 to 8 substituents, each independently being a substituent having up to 20 non-hydrogen atoms selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-substituted hydrocarbon group having 1 to 12 carbon atoms, an aminohydrocarbyl group having 1 to 12 carbon atoms, a hydrocarbyloxy group having 1 to 12 carbon atoms, a dihydrocarbylamino group having 1 to 12 carbon atoms, a hydrocarbylphosphino group having 1 to 12 carbon atoms, a silyl group, an aminosilyl group, a hydrocarbyloxysilyl group having 1 to 12 carbon atoms, and a halosilyl group.

[0119] In Equation 8, M 3 is a transition metal selected from the group of transition metals belonging to Group 4 of the periodic table having a formal oxidation number of +2, +3 or +4, and has at least one ligand L 1 To 5 Represents a bound transition metal.

[0120] In formula 8, W is a divalent substituent having up to 50 non-hydrogen atoms, L 1 and M. 3 Each bond has a valence of 1, resulting in L 1 and M 3 represents a divalent substituent which cooperates with X to form a metallocycle; 2 are each independently a monovalent anionic σ-bonded ligand; M 3 and a divalent anionic σ-bonded ligand that is divalently bonded to L 1 and M. 3 and divalent anionic σ-bonded ligands each having a valence of 1 to 1 and each having a valence of 1 to 1, and each having a valence of 1 to 1.

[0121] In Equation 8, X 2 each independently represents a neutral Lewis base coordinating compound having up to 40 non-hydrogen atoms; X 3 represents a neutral Lewis base coordinating compound.

[0122] j is 1 or 2, provided that when j is 2, two ligands L 1 are bonded to each other via a divalent group having up to 20 non-hydrogen atoms, and the divalent group is a group selected from the group consisting of hydrocarbadiyl groups having 1 to 20 carbon atoms, halohydrocarbadiyl groups having 1 to 12 carbon atoms, hydrocarbyleneoxy groups having 1 to 12 carbon atoms, hydrocarbyleneamino groups having 1 to 12 carbon atoms, silanediyl groups, halosilanediyl groups, and silyleneamino groups.

[0123] k is 0 or 1, p is 0, 1 or 2, provided that X 2 is a monovalent anionic σ-bonded ligand, or L 1 and M. 3 If p is a divalent anionic σ-bonded ligand bound to M 3 is an integer that is one or more smaller than the formal oxidation number of X 2 M 3 If the ligand is a divalent anionic σ-bonded ligand bound only to M, then p is M 3 is an integer that is (j+1) or more smaller than the formal oxidation number of

[0124] Ligand X in the compound of formula 8 above 2 Examples of the alkyl group include halides, hydrocarbon groups having 1 to 60 carbon atoms, hydrocarbyloxy groups having 1 to 60 carbon atoms, hydrocarbylamide groups having 1 to 60 carbon atoms, hydrocarbyl phosphide groups having 1 to 60 carbon atoms, hydrocarbyl sulfide groups having 1 to 60 carbon atoms, silyl groups, and composite groups thereof.

[0125] The neutral Lewis base coordinating compound X in the compound of formula 8 3Examples of the substituent include phosphines, ethers, amines, olefins having 2 to 40 carbon atoms, dienes having 3 to 40 carbon atoms, and divalent groups derived from these compounds.

[0126] In this embodiment, the transition metal compound having a cyclic η-bonding anion ligand is preferably a transition metal compound represented by the above formula 8 (where j is 1). A preferred example of the compound represented by the above formula 8 (where j is 1) is a compound represented by the following formula 9.

[0127] [ka]

[0128] In Equation 9, M 4 represents a transition metal selected from the group consisting of titanium, zirconium, nickel, and hafnium, the formal oxidation number of which is +2, +3, or +4; R 13 each independently represents a substituent having up to 20 non-hydrogen atoms selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a silyl group, a germyl group, a cyano group, a halogen atom, and a composite group thereof, provided that the substituent R 13 is a hydrocarbon group having 1 to 8 carbon atoms, a silyl group, or a germyl group, two adjacent substituents R 13 are bonded to each other to form a divalent group, whereby the two adjacent substituents R 13 can cooperate with the bonds between the two carbon atoms of the cyclopentadienyl ring to form a ring.

[0129] In Equation 9, X 4each independently represents a substituent having up to 20 non-hydrogen atoms selected from the group consisting of a halide, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbyloxy group having 1 to 18 carbon atoms, a hydrocarbylamino group having 1 to 18 carbon atoms, a silyl group, a hydrocarbylamide group having 1 to 18 carbon atoms, a hydrocarbyl phosphide group having 1 to 18 carbon atoms, a hydrocarbyl sulfide group having 1 to 18 carbon atoms, and composite groups thereof, provided that in some cases two substituents X 4 can cooperate to form a neutral conjugated diene or divalent group having 4 to 30 carbon atoms.

[0130] In Equation 9, Y 2 -O-, -S-, -NR * -OR-PR * -, where R * represents a hydrogen atom, a hydrocarbon group having 1 to 12 carbon atoms, a hydrocarbyloxy group having 1 to 8 carbon atoms, a silyl group, a halogenated alkyl group having 1 to 8 carbon atoms, a halogenated aryl group having 6 to 20 carbon atoms, or a composite group thereof.

[0131] In formula 9, Z 2 is SiR * 2. CR * 2. SiR * 2SiR * 2. CR * 2CR *2 , C.R. * =CR * , C.R. * 2SiR * 2 or GeR * 2, where R * is as defined above and n is 1, 2 or 3.

[0132] Examples of the transition metal compound having a cyclic η-bonding anion ligand used in this embodiment include the following compounds. The zirconium-based compound is not particularly limited, but specifically includes, for example, bis(methylcyclopentadienyl)zirconium dimethyl, bis(n-butylcyclopentadienyl)zirconium dimethyl, bis(indenyl)zirconium dimethyl, bis(1,3-dimethylcyclopentadienyl)zirconium dimethyl, (pentamethylcyclopentadienyl)(cyclopentadienyl)zirconium dimethyl, bis(cyclopentadienyl)zirconium dimethyl, bis(pentamethylcyclopentadienyl)zirconium dimethyl, bis(fluorenyl)zirconium dimethyl, ethylenebis(indenyl)zirconium dimethyl, ethylenebis(4,5,6,7-tetrahydro-1-indenyl)zirconium dimethyl, ethylenebis(4-methyl-1-indenyl)zirconium dimethyl, ethylenebis(5-methyl-1-indenyl)zirconium dimethyl, ) zirconium dimethyl, ethylene bis (6-methyl-1-indenyl) zirconium dimethyl, ethylene bis (7-methyl-1-indenyl) zirconium dimethyl, ethylene bis (5-methoxy-1-indenyl) zirconium dimethyl, ethylene bis (2,3-dimethyl-1-indenyl) zirconium dimethyl, ethylene bis (4,7-dimethyl-1-indenyl) zirconium dimethyl, ethylene bis (4,7-dimethoxy-1-indenyl) zirconium dimethyl, methylene bis (cyclopentadienyl) zirconium dimethyl, isopropylidene (cyclopentadienyl) zirconium dimethyl, isopropylidene (cyclopentadienyl-fluorenyl) zirconium dimethyl, silylene bis (cyclopentadienyl) zirconium dimethyl, dimethylsilylene (cyclopentadienyl) zirconium dimethyl, and the like.

[0133] The titanium-based compound is not particularly limited, but specifically includes, for example, [(Nt-butylamido)(tetramethyl-η 5 -cyclopentadienyl)-1,2-ethanediyl]titanium dimethyl, [(Nt-butylamido)(tetramethyl-η 5-Cyclopentadienyl)dimethylsilane]titanium dimethyl, [(N-methylamido)(tetramethyl-η 5 -Cyclopentadienyl)dimethylsilane]titanium dimethyl, [(N-phenylamido)(tetramethyl-η 5 -Cyclopentadienyl)dimethylsilane]titanium dimethyl, [(N-benzylamido)(tetramethyl-η 5 -Cyclopentadienyl)dimethylsilane]titanium dimethyl, [(Nt-butylamido)(η 5 -cyclopentadienyl)-1,2-ethanediyl]titanium dimethyl, [(Nt-butylamido)(η 5 -Cyclopentadienyl)dimethylsilane]titanium dimethyl, [(N-methylamido)(η 5 -cyclopentadienyl)-1,2-ethanediyl]titanium dimethyl, [(N-methylamido)(η 5 -Cyclopentadienyl)dimethylsilane]titanium dimethyl, [(Nt-butylamido)(η 5 -indenyl)dimethylsilane]titanium dimethyl, [(N-benzylamide)(η 5 -indenyl)dimethylsilane]titanium dimethyl, and the like.

[0134] The nickel-based compound is not particularly limited, but specific examples thereof include dibromobistriphenylphosphine nickel, dichlorobistriphenylphosphine nickel, dibromodiacetonitrile nickel, dibromodibenzonitrile nickel, dibromo(1,2-bisdiphenylphosphinoethane)nickel, dibromo(1,3-bisdiphenylphosphinopropane)nickel, dibromo(1,1'-diphenylbisphosphinoferrocene)nickel, dimethylbisdiphenylphosphine nickel, dimethyl(1,2-bisdiphenylphosphinoethane)nickel, methyl(1,2-bisdiphenylphosphinoethane)nickel tetrafluoroborate, (2-diphenylphosphino-1-phenylethyleneoxy)phenylpyridine nickel, and the like.

[0135] The hafnium-based compound is not particularly limited, but specifically includes, for example, [(Nt-butylamido)(tetramethyl-η 5 -cyclopentadienyl)-1,2-ethanediyl]hafnium dimethyl,[(Nt-butylamido)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]hafnium dimethyl,[(N-methylamido)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]hafnium dimethyl,[(N-phenylamido)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]hafnium dimethyl,[(N-benzylamido)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]hafnium dimethyl,[(Nt-butylamido)(η5- [(N-butylamido)(η5-cyclopentadienyl)dimethylsilane]hafnium dimethyl, [(N-methylamido)(η5-cyclopentadienyl)-1,2-ethanediyl]hafnium dimethyl, [(N-methylamido)(η5-cyclopentadienyl)dimethylsilane]hafnium dimethyl, [(N-butylamido)(η5-indenyl)dimethylsilane]hafnium dimethyl, [(N-benzylamido)(η5-indenyl)dimethylsilane]hafnium dimethyl and the like.

[0136] Further specific examples of the transition metal compound having a cyclic η-bonding anion ligand used in this embodiment include the "dimethyl" portion of the name of each of the zirconium-based compounds and titanium-based compounds listed above (this appears immediately after the end of the name of each compound, i.e., "zirconium" or "titanium" portion, and X in the above formula 9 4 (The name corresponds to the part of the formula (a)) can be used to refer to, for example, "dichloro," "dibromo," "diiodo," "diethyl," "dibutyl," "diphenyl," "dibenzyl," "2-(N,N-dimethylamino)benzyl," "2-butene-1,4-diyl," "s-trans-η 4 -1,4-diphenyl-1,3-butadiene", "s-trans-η 4 -3-Methyl-1,3-pentadiene", "s-trans-η4 -1,4-dibenzyl-1,3-butadiene", "s-trans-η 4 -2,4-Hexadiene", "s-trans-η 4 -1,3-pentadiene", "s-trans-η 4 -1,4-ditolyl-1,3-butadiene", "s-trans-η 4 -1,4-Bis(trimethylsilyl)-1,3-butadiene, s-cis-η 4 -1,4-diphenyl-1,3-butadiene", "s-cis-η 4 -3-methyl-1,3-pentadiene", "s-cis-η 4 -1,4-dibenzyl-1,3-butadiene", "s-cis-η 4 -2,4-hexadiene", "s-cis-η 4 -1,3-pentadiene", "s-cis-η 4 -1,4-ditolyl-1,3-butadiene", "s-cis-η 4 Also included are compounds with names that can be arbitrarily substituted, such as "-1,4-bis(trimethylsilyl)-1,3-butadiene."

[0137] The transition metal compounds having a cyclic η-bonding anion ligand used in this embodiment can be synthesized by a generally known method. In this embodiment, these transition metal compounds may be used alone or in combination.

[0138] Next, the activator (b) capable of reacting with a transition metal compound to form a complex that exhibits catalytic activity (hereinafter, simply referred to as "activator") used in this embodiment will be described. An example of the activator used in this embodiment is a compound defined by the following formula 10. [L 2 -H] d+ [M 5 m Q p ] d- ...Formula 10 (In formula 10, [L 2 -H] d+ represents a proton-donating Bronsted acid, where L2 represents a neutral Lewis base, d is an integer from 1 to 7; [M 5 m Q p ] d- represents a compatible non-coordinating anion, where M 5 represents a metal or metalloid belonging to any one of Groups 5 to 15 of the periodic table, and each Q is independently selected from the group consisting of a hydride, a halide, a dihydrocarbylamide group having 2 to 20 carbon atoms, a hydrocarbyloxy group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms, and a substituted hydrocarbon group having 1 to 40 carbon atoms, wherein the number of Qs that are halides is 1 or less, m is an integer from 1 to 7, p is an integer from 2 to 14, d is as defined above, and pm=d.

[0139] The non-coordinating anion is not particularly limited, but specific examples thereof include tetrakisphenylborate, tri(p-tolyl)(phenyl)borate, tris(pentafluorophenyl)(phenyl)borate, tris(2,4-dimethylphenyl)(hydroxyphenyl)borate, tris(3,5-dimethylphenyl)(phenyl)borate, tris(3,5-di-trifluoromethylphenyl)(phenyl)borate, tris(pentafluorophenyl)(cyclohexyl)borate, tris(pentafluorophenyl)(naphthyl)borate, tetrakis(pentafluorophenyl)borate, triphenyl(hydroxyphenyl)borate, diphenyl-di(hydroxyphenyl)borate, triphenyl(2,4-dihydroxyphenyl)borate, tri(p-tolyl)borate, tris(pentafluorophenyl)(naphthyl)borate, tris(pentafluorophenyl)(naphthyl)borate, tris(pentafluorophenyl)borate, tris(pentafluorophenyl)(hydroxyphenyl)borate, tris(pentafluorophenyl)(naphthyl)borate, tris(pentafluorophenyl ... tris(pentafluorophenyl)(hydroxyphenyl)borate, tris(pentafluorophenyl)(hydroxyphenyl)borate, tris(2,4-dimethylphenyl)(hydroxyphenyl)borate, tris(3,5-dimethylphenyl)(hydroxyphenyl)borate, tris(3,5-di-trifluorimethylphenyl)(hydroxyphenyl)borate, tris(pentafluorophenyl)(2-hydroxyethyl)borate, tris(pentafluorophenyl)(4-hydroxybutyl)borate, tris(pentafluorophenyl)(4-hydroxy-cyclohexyl)borate, tris(pentafluorophenyl)(4-(4'-hydroxyphenyl)phenyl)borate, tris(pentafluorophenyl)(6-hydroxy-2-naphthyl)borate, and the like.

[0140] Other preferred examples of non-coordinating anions include borates in which the hydroxy group of the above exemplary borates is replaced with an NHR group, where R is preferably a methyl group, an ethyl group, or a tert-butyl group.

[0141] In addition, the proton-donating Bronsted acid is not particularly limited, but specific examples thereof include trialkyl group-substituted ammonium cations such as triethylammonium, tripropylammonium, tri(n-butyl)ammonium, trimethylammonium, tributylammonium, and tri(n-octyl)ammonium; N,N-dialkylanilinium cations such as N,N-dimethylanilinium, N,N-diethylanilinium, N,N-2,4,6-pentamethylanilinium, and N,N-dimethylbenzylanilinium; dialkylammonium cations such as di-(i-propyl)ammonium and dicyclohexylammonium; triarylphosphonium cations such as triphenylphosphonium, tri(methylphenyl)phosphonium, and tri(dimethylphenyl)phosphonium; and dimethylsulfonium, diethylsulfonium, and diphenylsulfonium.

[0142] In this embodiment, an organometallic oxy compound having a unit represented by the following formula 11 can also be used as the activator. [ka] (Here, in Equation 11, M 6 is a metal or metalloid of Groups 13 to 15 of the periodic table, and R 14 are each independently a hydrocarbon group or a substituted hydrocarbon group having 1 to 12 carbon atoms, and n is a metal M 6 where m is an integer of 2 or greater.)

[0143] A preferred example of the activator used in this embodiment is an organoaluminum oxy compound containing a unit represented by the following formula 12: [ka] (Here, in Equation 12, R 15 is an alkyl group having 1 to 8 carbon atoms, and m is an integer of 2 to 60.

[0144] A more preferred example of the activator used in this embodiment is methylalumoxane containing a unit represented by the following formula 13: [ka] (In formula 13, m is an integer from 2 to 60.) In this embodiment, the activator components may be used alone or in combination.

[0145] In the present embodiment, these catalyst components can also be used as supported catalysts by being supported on a solid component. Such solid components are not particularly limited, but specific examples thereof include at least one inorganic solid material selected from porous polymeric materials such as polyethylene, polypropylene, and styrene-divinylbenzene copolymers; inorganic solid materials of elements in Groups 2, 3, 4, 13, and 14 of the Periodic Table, such as silica, alumina, magnesia, magnesium chloride, zirconia, titania, boron oxide, calcium oxide, zinc oxide, barium oxide, vanadium pentoxide, chromium oxide, and thorium oxide, and mixtures thereof; and double oxides thereof.

[0146] The composite oxide of silica is not particularly limited, but specifically includes, for example, composite oxides of silica, such as silica magnesia and silica alumina, and an element of Group 2 or Group 13 of the periodic table. In addition to the above two catalyst components, an organoaluminum compound can be used as a catalyst component in this embodiment, if necessary. The organoaluminum compound that can be used in this embodiment is, for example, a compound represented by the following formula 14. [ka] (Here, in Equation 14, R 16 is an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 20 carbon atoms, and X 5 is a halogen, hydrogen or an alkoxyl group, the alkyl group is linear, branched or cyclic, and n is an integer of 1 to 3.

[0147] Here, the organoaluminum compound may be a mixture of compounds represented by the above formula 14. The organoaluminum compound that can be used in this embodiment is, for example, a compound represented by the above formula R 16 X is a methyl group, an ethyl group, a butyl group, an isobutyl group, a hexyl group, an octyl group, a decyl group, a phenyl group, a tolyl group, etc. 5 Examples of the alkyl group include a methoxy group, an ethoxy group, a butoxy group, and a chlorine group.

[0148] The organoaluminum compound that can be used in the present embodiment is not particularly limited, but specific examples include trimethylaluminum, triethylaluminum, tributylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, tridecylaluminum, and the like, as well as reaction products of these organoaluminum compounds with alcohols such as methyl alcohol, ethyl alcohol, butyl alcohol, pentyl alcohol, hexyl alcohol, octyl alcohol, and decyl alcohol, such as dimethylmethoxyaluminum, diethylethoxyaluminum, and dibutylbutoxyaluminum.

[0149] (Polymerization conditions) The polymerization temperature in the method for producing ultra-high molecular weight polyethylene powder of this embodiment is usually 30°C or higher and 100°C or lower. A polymerization temperature of 30°C or higher tends to enable more efficient industrial production. On the other hand, a polymerization temperature of 100°C or lower tends to enable more continuous and stable operation. In addition, the intrinsic viscosity IV of the ultra-high molecular weight polyethylene powder tends to decrease as the polymerization temperature is increased, and tends to increase as the polymerization temperature is decreased.

[0150] The polymerization pressure in the method for producing the ultra-high molecular weight polyethylene powder of this embodiment is usually normal pressure or more and 2 MPa or less. The polymerization pressure is preferably 0.1 MPa or more, more preferably 0.12 MPa or more, and is preferably 1.5 MPa or less, more preferably 1.0 MPa or less. A polymerization pressure of normal pressure or more tends to enable industrially more efficient production, and a polymerization pressure of 2 MPa or less tends to suppress partial heat generation due to a rapid polymerization reaction when the catalyst is introduced, and polyethylene tends to be produced stably.

[0151] The polymerization reaction can be carried out in any of a batch system (batch system), semi-continuous system, and continuous system. From the viewpoint of controlling the voids of the ultra-high molecular weight polyethylene powder of the present embodiment within the above-mentioned range, a batch system (batch system) is preferred. On the other hand, from the viewpoint of making the polymerization system more uniform, a continuous system is preferred. By continuously supplying ethylene gas, a solvent, a catalyst, and the like into the polymerization system and continuously discharging them together with the produced polyethylene, it is possible to suppress a partial high temperature state caused by a sudden reaction of ethylene, and the polymerization system is more stabilized. When ethylene reacts in a uniform state within the system, the generation of branches and double bonds in the polymer chain is suppressed, and the molecular weight of polyethylene is reduced and crosslinking is less likely to occur, so that the amount of unmelted material remaining when the ultra-high molecular weight polyethylene powder is melted or dissolved is reduced, coloring is suppressed, and problems such as a decrease in mechanical properties are less likely to occur.

[0152] It is also possible to carry out the polymerization in two or more stages with different reaction conditions. Furthermore, as described in, for example, West German Patent Application Publication No. 3127133, the intrinsic viscosity of the resulting polyethylene can be adjusted by making hydrogen present in the polymerization system or by changing the polymerization temperature. By adding hydrogen as a chain transfer agent to the polymerization system, it is possible to control the intrinsic viscosity within an appropriate range. By adding a chain transfer agent, the intrinsic viscosity IV of the ultra-high molecular weight polyethylene produced at the same polymerization temperature tends to be lower. When hydrogen is added to the polymerization system, the molar fraction of hydrogen is preferably 0 mol% or more and 30 mol% or less, more preferably 0 mol% or more and 25 mol% or less, and even more preferably 0 mol% or more and 20 mol% or less. In this embodiment, in addition to the above-mentioned components, other known components useful for the production of polyethylene can be included.

[0153] As described above, the ultra-high molecular weight polyethylene powder of this embodiment is prepared by polymerizing under high pressure conditions using a polymer obtained by prepolymerization as a prepolymerization catalyst (control method 1), polymerizing using a precipitation-type catalyst having a fine catalyst particle size with little variation in particle size, and then drying at high temperature while rotating at high speed (control method 2), and collecting only the fine powder polymer by classification and drying again while rotating at high temperature while rotating at high speed, thereby controlling the proportion of thin parts or void parts of the ultra-high molecular weight polyethylene powder within the above range (control method 3).

[0154] When ultra-high molecular weight polyethylene powder is produced by the above-mentioned control method 1, the prepolymerization temperature is preferably 5°C or more and 40°C or less, the prepolymerization pressure is preferably 0.1 MPa or more and 0.5 MPa or less, the prepolymerization time is preferably 0.5 hours or more and 3.0 hours or less, and the main polymerization pressure is preferably 0.5 MPa or more and 1.0 MPa or less.

[0155] When producing ultra-high molecular weight polyethylene powder using the above control method 2, the average particle diameter of the catalyst (D 50) is preferably 1 μm or more and 3 μm or less, the particle size distribution of the catalyst particle diameter is preferably 0.5 μm or more and 5 μm or less, the drying temperature is preferably 110° C. or more and 120° C. or less, the drying time is preferably 1 hour or more and 3 hours or less, and the rotation speed during drying is preferably 100 rpm or more and 300 rpm or less.

[0156] When ultra-high molecular weight polyethylene powder is produced using the above-mentioned control method 3, it is preferable to use 75 μm pass products (less than 75 μm) in the classification process, the drying temperature is preferably 110° C. or higher and 120° C. or lower, the drying time is preferably 1 hour or higher and 3 hours or lower, and the rotation speed during drying is preferably 100 rpm or higher and 300 rpm or lower.

[0157] When polymerizing the ultra-high molecular weight polyethylene powder of this embodiment, an antistatic agent such as Stadis 450 manufactured by The Associated Octel Company (distributor: Maruwa Bussan) can be used to suppress adhesion of the polymer to the polymerization reactor. Stadis 450 can also be diluted in an inert hydrocarbon medium and added to the polymerization reactor by a pump or the like. The amount of addition is preferably in the range of 0.10 ppm to 20 ppm, more preferably 0.20 ppm to 10 ppm, relative to the amount of polyethylene produced per unit time.

[0158] [Additives] Additives such as slip agents, neutralizing agents, antioxidants, light resistance stabilizers, antistatic agents, and pigments may be added to the ultra-high molecular weight polyethylene powder of this embodiment as necessary.

[0159] The slip agent or neutralizing agent is not particularly limited, but may be, for example, an aliphatic hydrocarbon, a higher fatty acid, a higher fatty acid metal salt, a fatty acid ester of alcohol, a wax, a higher fatty acid amide, a silicone oil, or a rosin. A specific example may be, but is not particularly limited, calcium stearate. The content of the slip agent or neutralizing agent is not particularly limited, but is preferably 5000 ppm or less, more preferably 4000 ppm or less, and even more preferably 3000 ppm or less.

[0160] The antioxidant is not particularly limited, but for example, a phenol-based compound or a phenol-phosphorus-based compound is preferable. Specific examples of the antioxidant include phenol-based antioxidants such as 2,6-di-t-butyl-4-methylphenol (dibutylhydroxytoluene), n-octadecyl-3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, and tetrakis(methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate))methane; phenol-phosphorus-based antioxidants such as 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine; and phosphorus-based antioxidants such as tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenylene-diphosphonite, tris(2,4-di-t-butylphenyl)phosphite, and cyclic neopentanetetraylbis(2,4-t-butylphenylphosphite).

[0161] In the ultra-high molecular weight polyethylene powder according to this embodiment, the amount of the antioxidant is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, and particularly preferably 2 parts by mass or less, when the total amount of the ultra-high molecular weight polyethylene powder and liquid paraffin is 100 parts by mass. When the amount of the antioxidant is 5 parts by mass or less, deterioration of the polyethylene is suppressed, and embrittlement, discoloration, deterioration of mechanical properties, etc. are less likely to occur, resulting in more excellent long-term stability.

[0162] Examples of the light resistance stabilizer include, but are not limited to, benzotriazole-based light resistance stabilizers such as 2-(5-methyl-2-hydroxyphenyl)benzotriazole and 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole; and hindered amine-based light resistance stabilizers such as bis(2,2,6,6-tetramethyl-4-piperidine)sebacate and poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}]. The content of the light resistance stabilizer is not particularly limited, but is 5000 ppm or less, preferably 3000 ppm or less, and more preferably 2000 ppm or less.

[0163] The antistatic agent is not particularly limited, but examples thereof include aluminosilicates, kaolin, clay, natural silica, synthetic silica, silicates, talc, diatomaceous earth, and glycerin fatty acid esters.

[0164] [Molded body] The ultra-high molecular weight polyethylene powder of this embodiment can be molded by various methods. The molded article of this embodiment is obtained by molding the ultra-high molecular weight polyethylene powder described above. The molded article of this embodiment can be used for various applications. Specific examples of the molded article of this embodiment include, but are not limited to, separators for secondary batteries (e.g., microporous membranes) and fibers (e.g., high-strength fibers), and among these, the molded article is suitable as a microporous membrane and high-strength fiber for lithium-ion secondary battery separators.

[0165] The method for producing the molded article of the present embodiment may be a conventionally known method, and examples of such a method include, but are not limited to, compression molding (press molding), extrusion molding, stretch molding, etc. In addition, when the molded article is a separator for a secondary battery or a fiber, the manufacturing method is as follows.

[0166] The method for producing a separator for a secondary battery (e.g., a microporous membrane) is not particularly limited, but for example, a processing method using a solvent in a wet process in which an extruder equipped with a T-die is used for extrusion, stretching, extraction, and drying. Specifically, for example, the method is not particularly limited, but for example, a manufacturing method under the following general swelling conditions and a manufacturing method under the following low-temperature swelling conditions.

[0167] (Swelling conditions) Ultra-high molecular weight polyethylene powder is mixed with liquid paraffin, and additives such as antioxidants are added as necessary. The melting point (T m2 ) and stir at a temperature 30°C lower than the recommended temperature to prepare a slurry liquid. The obtained slurry liquid is put into a kneading machine, kneaded at a constant temperature, and then hot-pressed and cold-pressed to form a gel sheet. The thickness of the gel sheet is adjusted using a metal frame. The gel sheet was stretched using a simultaneous biaxial stretching machine, and the stretched film was cut out and fixed on a metal frame. It was then immersed in hexane to extract and remove the liquid paraffin, and then dried. It was further heat-set to obtain a microporous membrane for a secondary battery separator.

[0168] The method for producing fibers (e.g., high-strength fibers) is not particularly limited, but examples thereof include a method in which liquid paraffin and the above-mentioned ultra-high molecular weight polyethylene powder are kneaded and spun, followed by heating and drawing.Specific examples thereof include, but are not particularly limited to, a production method under the following general swelling conditions and a production method under the following low-temperature swelling conditions.

[0169] (Swelling conditions) Ultra-high molecular weight polyethylene powder is mixed with liquid paraffin, and additives such as antioxidants are added as necessary. The melting point (T m2 ) and stir at a temperature 30°C lower than the recommended temperature to prepare a slurry liquid. Next, the slurry liquid is charged into a kneading machine and kneading is carried out at a constant temperature. The mixture is then spun through a spinneret attached to a Capillograph 1D. At this time, the yarn containing the discharged liquid paraffin is wound up at a location away from the spinneret. Next, in order to remove the liquid paraffin from the wound yarn, the yarn is immersed in hexane for extraction, and then dried. The obtained yarn is first drawn in a thermostatic chamber, and then secondly drawn in the thermostatic chamber until the yarn breaks, to obtain a high-strength fiber (drawn yarn). EXAMPLES

[0170] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples in any way.

[0171] Here, the ethylene and hexane used in the examples and comparative examples were dehydrated using MS-3A (manufactured by Showa Union), and hexane was further deoxygenated by degassing under reduced pressure using a vacuum pump before use.

[0172] [Measurement method and conditions] The physical properties of the ultra-high molecular weight polyethylene powders of the Examples and Comparative Examples were measured by the following methods.

[0173] (Measurement 1) Intrinsic viscosity IV The intrinsic viscosity IV of the ultra-high molecular weight polyethylene powders obtained in the Examples and Comparative Examples was measured in accordance with ISO1628-3 (2010) as follows. Polyethylene powder was weighed out in the range of 4.0 to 4.5 mg, and dissolved in 20 mL of decahydronaphthalene (2,6-di-t-butyl-4-methylphenol added at 1 g / L, hereafter referred to as Decalin) that had been degassed with a vacuum pump and replaced with nitrogen, stirred at 150°C for 90 minutes in a dissolution tube whose internal air had been degassed with a vacuum pump and replaced with nitrogen to obtain a solution. A Cannon-Fenske viscometer (manufactured by Shibata Scientific Instruments Co., Ltd.: product number -100) was used as the viscosity tube.

[0174] (Measurement 2) Percentage of voids in ultra-high molecular weight polyethylene powder The ratio of voids in the ultra-high molecular weight polyethylene powders obtained in the Examples and Comparative Examples was calculated by carrying out the following procedures 1, 2, and 3 in this order. [Step 1; Preparation of embedded resin sample] 100 g of ultra-high molecular weight polyethylene powder was classified using 10 types of sieves (mesh size: 710 μm, 500 μm, 425 μm, 355 μm, 300 μm, 212 μm, 150 μm, 106 μm, 75 μm, 53 μm) specified in JIS Z8801. The weight of the particles remaining on each sieve was integrated from the smaller mesh side, and the particle size at 50% of the weight on the integral curve was defined as the average particle size (D 50 ) and D 50 The fraction containing the particle size of was collected. The collected powder was embedded in the high-performance adhesive Araldite Standard (Nichiban Co., Ltd.) and dried at 30°C for 24 hours to prepare an embedded resin sample. The epoxy resin, which is the base material, and the modified polyamine, which is the hardener, were mixed in a 1:1 ratio. [Step 2: Optical microscope observation] The embedded resin sample was cut into 10 μm thick sections using a microtome manufactured by Japan Microtome Laboratory Co., Ltd., the cut sample was placed on a slide glass, a small amount (0.05 mL) of liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Co., Ltd. was added, and a cover glass was placed on top of it. Next, transmission differential interference observation was performed using an optical microscope BX51 manufactured by Olympus Co., Ltd. (the light intensity of the microscope was fixed at memory 9), and D 50 Ten particles of ±5 μm were randomly observed, and cross-sectional images of the powder were taken. [Step 3; Image analysis] Using image analysis software (Asahi Kasei Corporation, A-zo-kun ver.2.50), the powder cross-sectional image photographed under a microscope was binarized (white: polymer part, black: void part). An arbitrary rectangle circumscribing the polymer part (white) was drawn, and the intersection of the diagonal lines of the rectangle was taken as the center of the powder. The proportion of the polymer part (white) in the rectangle was set to 20% or more. Next, a 20 μm × 20 μm square was drawn parallel to the rectangle with the powder center as its axis, and the proportion of void parts (black) in the square was determined. A similar image analysis was performed on all 10 points photographed under an optical microscope, and the average value was taken as the proportion of void parts (black).

[0175] (Measurement 3) Crystallinity of ultra-high molecular weight polyethylene powder The crystallinity of the ultra-high molecular weight polyethylene powders obtained in the Examples and Comparative Examples was measured by wide-angle X-ray scattering (WAXS) under the following conditions. A Rigaku Ultima-IV was used for the measurements. Cu-Kα radiation was incident on the ultra-high molecular weight polyethylene powder sample, and the diffracted light was detected by D / tex Ultra. The measurement conditions were: distance between sample and detector 285 mm, excitation voltage 40 kV, and current 40 mA. A focusing optical system was used, and the slit conditions were DS=1 / 2°, SS=open, and vertical slit=10 mm.

[0176] (Measurement 4) Apparent density of ultra-high molecular weight polyethylene powder The apparent density of the ultra-high molecular weight polyethylene powder obtained in the examples and comparative examples was calculated by the following method. First, the ultra-high molecular weight polyethylene powder was allowed to flow down through the orifice of a funnel calibrated to standard dimensions in accordance with JIS K 6891 into a 100 cc cylindrical container until it overflowed. Next, in order to prevent compaction or the powder overflowing from the cup, a blade such as a spatula was placed vertically in contact with the top surface of the container and moved smoothly to carefully scrape off the excess powder from the top surface of the container. All of the powder was also removed from the sides of the container, and the mass of the powder including the container was measured, and the mass of the powder was calculated by subtracting the mass of the empty measuring container that had been measured in advance. After the above operation was performed three times in succession, the apparent density (g / cm 3 ) was calculated according to the following formula A. 3 ) was calculated and the average value was recorded. 3 ) = mass of the powder (g) / volume of the cylindrical container (cm 3 )…Formula A

[0177] (Measurement 5) Ti content in ultra-high molecular weight polyethylene powder The ultra-high molecular weight polyethylene powders obtained in the Examples and Comparative Examples were pressure-decomposed using a microwave decomposition apparatus (model ETHOS TC, manufactured by Milestone General Co., Ltd.), and the elemental concentration of titanium (Ti) as a metal contained in the ultra-high molecular weight polyethylene powder was measured using an ICP-MS (inductively coupled plasma mass spectrometer, model X-series X7, manufactured by Thermo Fisher Scientific Co., Ltd.) by the internal standard method.

[0178] (Method 1 for producing molded body) Method for producing separator (microporous membrane) for secondary battery with high polymer concentration Using the ultra-high molecular weight polyethylene powders obtained in the Examples and Comparative Examples, secondary battery separators were produced as follows. When the total amount of the ultra-high molecular weight polyethylene powder and the liquid paraffin is 100 parts by mass, 40 parts by mass of the ultra-high molecular weight polyethylene powder, 60 parts by mass of liquid paraffin (liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of an antioxidant (tetrakis[methylene(3,5-di-t-butyl-4-hydroxy-hydrocinnamate)]methane (product name: ANOX20) manufactured by Great Lakes Chemical Japan Co., Ltd.) are mixed together, and the melting point (T m2 ) and stirred for 30 minutes at a temperature 30° C. lower than the reaction temperature. A slurry liquid was prepared. The obtained slurry liquid was put into a Labo Plastomill (body model: 4C150-01) manufactured by Toyo Seiki Co., Ltd., and kneaded at a constant temperature of 200°C for 10 minutes with a screw rotation speed of 50 rpm, and then heat-pressed at 180°C / 1 MPa / 3 minutes, further heat-pressed at 180°C / 10 MPa / 2 minutes, and then cooled and pressed at 25°C / 10 MPa / 5 minutes to form a gel sheet. The thickness of the gel sheet was adjusted to 1.0 mm by using a metal frame with a thickness of 1.0 mm. The gel sheet was stretched 7x7 times at 115°C using a simultaneous biaxial stretching machine, and the stretched film was cut into approximately 30cm squares and fixed to a metal frame with an inner dimension of 25cm square. It was then immersed in hexane to extract and remove the liquid paraffin, and then dried for 24 hours or more. It was then heat-set at 134°C for 1 minute to obtain a separator for secondary batteries.

[0179] (Method 2 for producing molded body) A method for producing a separator for a secondary battery with a general polymer concentration and a general kneading time A secondary battery separator was obtained in the same manner as described above (Method 1 for producing molded bodies), except that, when the total amount of the ultra-high molecular weight polyethylene powder and liquid paraffin was 100 parts by mass, 25 parts by mass of the ultra-high molecular weight polyethylene powder, 75 parts by mass of liquid paraffin (liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of an antioxidant (tetrakis[methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate)]methane (product name: ANOX20) manufactured by Great Lakes Chemical Japan Co., Ltd.) were blended.

[0180] (Method 3 for producing a molded body) A method for producing a microporous membrane for a secondary battery separator in a short kneading time Using the ultra-high molecular weight polyethylene powders obtained in the Examples and Comparative Examples, secondary battery separators were produced as follows. When the total amount of the ultra-high molecular weight polyethylene powder and the liquid paraffin is 100 parts by mass, 25 parts by mass of the ultra-high molecular weight polyethylene powder, 75 parts by mass of liquid paraffin (liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of an antioxidant (tetrakis[methylene(3,5-di-t-butyl-4-hydroxy-hydrocinnamate)]methane (product name: ANOX20) manufactured by Great Lakes Chemical Japan Co., Ltd.) are mixed together, and the melting point (T m2 ) and stirred for 30 minutes at a temperature 30° C. lower than the reaction temperature. A slurry liquid was prepared. The obtained slurry liquid was put into a Labo Plastomill (body model: 4C150-01) manufactured by Toyo Seiki Co., Ltd., and kneaded at a constant temperature of 200°C for 5 minutes with a screw rotation speed of 50 rpm, and then heat-pressed at 180°C / 1 MPa / 3 minutes, further heat-pressed at 180°C / 10 MPa / 2 minutes, and then cooled and pressed at 25°C / 10 MPa / 5 minutes to form a gel sheet. The thickness of the gel sheet was adjusted to 1.0 mm by using a metal frame with a thickness of 1.0 mm. The gel sheet was stretched 7x7 times at 115°C using a simultaneous biaxial stretching machine, and the stretched film was cut into approximately 30cm squares and fixed to a metal frame with an inner dimension of 25cm square. It was then immersed in hexane to extract and remove the liquid paraffin, and then dried for 24 hours or more. It was then heat-set at 134°C for 1 minute to obtain a separator for secondary batteries.

[0181] (Evaluation method 1) Thickness variation of secondary battery separator Microporous membranes serving as separators for secondary batteries were produced by the methods described in (Production method 1 for molded article) to (Production method 3 for molded article) above, and the thicknesses of the resulting microporous membranes were measured using a film thickness meter based on JIS K7130. For the measurement points, one 25 cm square microporous membrane was cut into 25 5 cm square microporous membranes, and the center of each was measured to calculate the average membrane thickness. Using the average membrane thickness as a standard, the thickness variation (hereinafter also referred to as membrane thickness unevenness), which is one index of the quality of the microporous membrane, was evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 3 and 4. (Evaluation Criteria) ⊚: The film thickness varies by less than ±1.5 μm from the average film thickness. ◯: The film thickness varies by more than ±1.5 μm and less than ±3.0 μm from the average film thickness. ×: The film thickness varies by ±3.0 μm or more from the average film thickness.

[0182] (Evaluation method 2) Puncture strength converted into basis weight (gf / (g / m 2 )) Using a handy compression tester "KES-G5" manufactured by Kato Tech Co., Ltd., the microporous membranes that are separators for secondary batteries described in (Production method 1 for molded body) to (Production method 3 for molded body) above were fixed with a sample holder with an opening diameter of 10 mm. Next, a puncture test was performed on the center of the fixed microporous membrane with a needle tip curvature radius of 0.5 mm and a puncture speed of 10 mm / min to obtain the puncture strength (gf) as the maximum puncture load. The obtained puncture strength (gf) was divided by the basis weight to obtain the basis weight converted puncture strength (gf / (g / m 2 This operation was carried out eight times for eight microporous membranes, and the average of the eight measurements was calculated as the basis weight converted puncture strength (gf / (g / m 2 The evaluation results are shown in Tables 3 and 4. (Evaluation Criteria) ◎: The puncture strength converted into basis weight is 80gf / (g / m 2 )That's all. ○: The puncture strength converted to basis weight is 60gf / (g / m 2 ) or more 80gf / (g / m 2 ) or less. ×: The puncture strength converted to basis weight is 60gf / (g / m2 ) or less.

[0183] (Method 4 for manufacturing molded products) Method for manufacturing high-strength fibers with high polymer concentration A high-strength fiber was produced using ultra-high molecular weight polyethylene powder as follows. When the total amount of the ultra-high molecular weight polyethylene powder and liquid paraffin was 100 parts by mass, 15 parts by mass of the ultra-high molecular weight polyethylene powder, 85 parts by mass of liquid paraffin (liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of an antioxidant (tetrakis[methylene(3,5-di-t-butyl-4-hydroxy-hydrocinnamate)]methane (product name: ANOX20) manufactured by Great Lakes Chemical Japan Co., Ltd.) were blended to obtain a fiber having a melting point (T m2 ) and stirred for 30 minutes at a temperature 30° C. lower than the reaction temperature. A slurry liquid was prepared. Next, the slurry liquid was put into a Labo Plastomill (main unit type: 4C150-01) manufactured by Toyo Seiki Co., Ltd., and kneaded at a constant temperature of 200°C for 10 minutes with a screw rotation speed of 50 rpm, and then spun using a Capilograph 1D (main unit type: PMD-C) manufactured by Toyo Seiki Co., Ltd. The orifice used had a diameter of 0.5 mm, a length of 5 mm, and an inlet angle of 90°. The spinning conditions were a temperature of 200°C, an extrusion speed of 20 mm / min, and a winding speed of 50 m / min. Next, in order to remove the liquid paraffin from the wound yarn, the yarn was immersed in hexane for extraction, and then dried for 24 hours or more. The obtained yarn was first drawn at a speed of 20 mm / min in a thermostatic chamber set at 120°C, and then secondarily drawn at a speed of 10 mm / min in a thermostatic chamber set at 140°C until the yarn broke, to obtain a high-strength fiber (drawn yarn).

[0184] (Method 5 for producing molded products) A method for producing high-strength fibers at a typical polymer concentration and for a typical kneading time A high-strength fiber (drawn yarn) was obtained in the same manner as described above (Method 5 for producing molded bodies), except that, when the total amount of the ultra-high molecular weight polyethylene powder and liquid paraffin was 100 parts by mass, 7 parts by mass of the ultra-high molecular weight polyethylene powder, 93 parts by mass of liquid paraffin (liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of an antioxidant (tetrakis[methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate)]methane (product name: ANOX20) manufactured by Great Lakes Chemical Japan Co., Ltd.) were blended.

[0185] (Method 6 for manufacturing molded products) A method for manufacturing high-strength fibers in a short kneading time A high-strength fiber was produced using ultra-high molecular weight polyethylene powder as follows. When the total amount of the ultra-high molecular weight polyethylene powder and liquid paraffin was 100 parts by mass, 7 parts by mass of the ultra-high molecular weight polyethylene powder, 93 parts by mass of liquid paraffin (liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of an antioxidant (tetrakis[methylene(3,5-di-t-butyl-4-hydroxy-hydrocinnamate)]methane (product name: ANOX20) manufactured by Great Lakes Chemical Japan Co., Ltd.) were blended to obtain a fiber having a melting point (T m2 ) and stirred for 30 minutes at a temperature 30° C. lower than the reaction temperature. A slurry liquid was prepared. Next, the slurry liquid was put into a Labo Plastomill (main unit type: 4C150-01) manufactured by Toyo Seiki Co., Ltd., and kneaded at a constant temperature of 200°C for 5 minutes with a screw rotation speed of 50 rpm, and then spun using a Capilograph 1D (main unit type: PMD-C) manufactured by Toyo Seiki Co., Ltd. The orifice used had a diameter of 0.5 mm, a length of 5 mm, and an inlet angle of 90°. The spinning conditions were a temperature of 200°C, an extrusion speed of 20 mm / min, and a winding speed of 50 m / min. Next, in order to remove the liquid paraffin from the wound yarn, the yarn was immersed in hexane for extraction, and then dried for 24 hours or more. The obtained yarn was first drawn at a speed of 20 mm / min in a thermostatic chamber set at 120°C, and then secondarily drawn at a speed of 10 mm / min in a thermostatic chamber set at 140°C until the yarn broke, to obtain a high-strength fiber (drawn yarn).

[0186] (Evaluation method 3) Unevenness in yarn diameter of high-strength fibers The diameter of 10 m of high strength fiber (drawn yarn) spun by the methods described in (Production method 4 for molded body) to (Production method 6 for molded body) was measured at 0.5 m intervals using an optical microscope, and the average yarn diameter was calculated. Using this average yarn diameter as a standard, the unevenness of the yarn diameter, which is one of the indicators of the quality of high strength fiber, was evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 3 and 4. (Evaluation Criteria) ◎: Variation is less than ±5 μm from the average fiber diameter. ◯: The variation is between ±5 μm and ±8 μm from the average fiber diameter. ×: The average yarn diameter varies by ±8 μm or more.

[0187] (Evaluation method 4) Evaluation of high-speed winding properties of high-strength fibers The gel kneaded by the methods described in (Production method 4 for molded body) to (Production method 6 for molded body) above was spun using a Capillograph 1D (main body type: PMD-C) manufactured by Toyo Seiki Co., Ltd. The orifice used had an aperture of 0.5 mm, a length of 5 mm, and an inlet angle of 90°. The spinning conditions were fixed at a temperature of 200°C and an extrusion speed of 20 mm / min, and the winding speed was increased from 3 m / min to 200 m / min by 19.7 m / min. 2 The winding speed was gradually increased, and the speed at which the film broke was measured as the high winding speed. The average value of five measurements was used to evaluate the film according to the following evaluation criteria. The evaluation results are shown in Tables 3 and 4. (Evaluation Criteria) ◎: High-speed winding speed is 100 m / min or more. ◯: The high-speed winding speed is 50 m / min or more and less than 100 m / min. ×: The high-speed winding speed is less than 50 m / min.

[0188] (Measurement 6) Melting point (T m2) The melting points (T m2 ) was measured using a Perkin Elmer DSC8000 differential scanning calorimeter (DSC) as follows. 8.3-8.5 mg of ultra-high molecular weight polyethylene powder was weighed out and placed in an aluminum sample pan. An aluminum cover was attached to this pan and placed in the differential scanning calorimeter. Measurements were performed under the following conditions while purging with nitrogen at a flow rate of 20 mL / min. Pure indium was used for temperature calibration. 1) After holding at 50°C for 1 minute, the temperature was increased to 180°C at a rate of 10°C / min. 2) After holding at 180°C for 5 minutes, the temperature was lowered to 50°C at a rate of 10°C / min. 3) After holding at 50°C for 5 minutes, the temperature was increased to 180°C at a rate of 10°C / min. The temperature at the peak top of the melting curve obtained during the temperature rise process in the above step 3 is called the melting peak temperature (T m2 ) was decided.

[0189] (Measurement 7) Proportion of particles larger than 300 μm 100 g of ultra-high molecular weight polyethylene powder was classified using 10 types of sieves specified in JIS Z8801 (mesh openings: 710 μm, 500 μm, 425 μm, 355 μm, 300 μm, 212 μm, 150 μm, 106 μm, 75 μm, 53 μm), and the ratio was calculated from the weight (g) of particles deposited on a sieve with an opening of 300 μm or more relative to the weight of the total particles. Percentage of particles with a particle diameter of 300 μm or more (%) = [Weight of particles deposited on a sieve with an opening of 300 μm or more (g)] / [Weight of total particles 100 (g)] × 100

[0190] (Measurement 8) Proportion of particles smaller than 53 μm 100 g of ultra-high molecular weight polyethylene powder was classified using 10 types of sieves specified in JIS Z8801 (mesh openings: 710 μm, 500 μm, 425 μm, 355 μm, 300 μm, 212 μm, 150 μm, 106 μm, 75 μm, 53 μm), and the ratio was calculated from the weight (g) of the particles that passed through the sieve with a 53 μm opening to the weight of the total particles. Percentage of particles with a particle diameter of less than 53 μm (%) = [Weight of particles passing through a sieve with a mesh size of 53 μm (g)] / [Weight of all particles 100 (g)] × 100

[0191] [Catalyst synthesis method] [Catalyst Production Example 1] (Preparation of Supported Metallocene Catalyst Component [A]) (1) Synthesis of raw material [a-1] Average particle size is 7μm, specific surface area is 700m 2 Spherical silica with a particle size of 1.9 mL / g and an intraparticle pore volume of 1.9 mL / g was calcined at 500°C for 5 hours in a nitrogen atmosphere and dehydrated. In a nitrogen atmosphere, 40 g of this dehydrated silica was dispersed in 800 mL of hexane in a 1.8 L capacity autoclave to obtain a slurry. While keeping the obtained slurry at 20° C. under stirring, 100 mL of a hexane solution of triethylaluminum (concentration: 1 mol / L) was added dropwise over 1 hour, and then the mixture was stirred at the same temperature for 2 hours. Thereafter, the resulting reaction mixture was decanted to remove the unreacted triethylaluminum in the supernatant, thus obtaining 800 mL of a hexane slurry of the silica component [a-1] treated with triethylaluminum. (2) Preparation of raw material [a-2] 200 mmol of [(Nt-butylamido)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]titanium-1,3-pentadiene (hereinafter referred to as "titanium complex") was dissolved in 1250 mL of Isopar E [a trade name for a hydrocarbon mixture manufactured by Exxon Chemical Company (USA)], 25 mL of a 1 mol / L hexane solution of commercially available butylethylmagnesium was added, and further hexane was added to adjust the titanium complex concentration to 0.1 mol / L, thereby obtaining titanium complex [a-2]. (3) Preparation of raw material [a-3] 5.7 g of bis(hydrogenated tallow alkyl)methylammonium-tris(pentafluorophenyl)(4-hydroxyphenyl)borate (hereinafter referred to as "borate") was added and dissolved in 50 mL of toluene to obtain a 100 mmol / L toluene solution of borate. 5 mL of a 1 mol / L hexane solution of ethoxydiethylaluminum was added to this toluene solution of borate at room temperature, and further hexane was added so that the borate concentration in the solution became 70 mmol / L. After that, the mixture was stirred at room temperature for 1 hour to obtain a reaction mixture [a-3] containing borate. (4) Synthesis of supported metallocene catalyst [A] 800 mL of the silica component [a-1] slurry obtained in (1) above was stirred at 20°C, and 32 mL of the titanium complex [a-2] obtained in (2) above and 46 mL of the reaction mixture [a-3] containing borate obtained in (3) above were added simultaneously over 1 hour, and the mixture was stirred at the same temperature for another 1 hour to react the titanium complex with the borate. The catalytic activity can be controlled by adjusting the amounts of the titanium complex [a-2] and the reaction mixture [a-3] containing borate. Specifically, increasing the amounts of these components tends to increase the catalytic activity. After the reaction was completed, the supernatant was removed, and unreacted catalyst raw materials were removed with hexane to obtain a supported metallocene catalyst [A] (hereinafter also referred to as solid catalyst component [A] or solid catalyst A) in which catalytically active species were formed on the silica. (5) Synthesis of raw material (a-4) In an 8L stainless steel autoclave that had been thoroughly purged with nitrogen, 1 mol / L of Mg6(C4H9) 12 2,000mL of hexane solution of Al(C2H5)3 (equivalent to 2000mmol in total of magnesium and aluminum) was charged, and 240mL of hexane solution of 8.33mol / L methylhydrogenpolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.) was pumped in while stirring at 80℃, and stirring was continued for another 2 hours at 80℃. After the reaction was completed, the mixture was cooled to room temperature and used as raw material (a-4). Raw material (a-4) had a total concentration of magnesium and aluminum of 0.786mol / L.

[0192] [Catalyst Production Example 2] (Preparation of solid catalyst component [B]) (1) Synthesis of raw material (b-1) In an 8L stainless steel autoclave that had been thoroughly purged with nitrogen, 1 mol / L of Mg6(C4H9) 12 2,000mL of hexane solution of Al(C2H5)3 (equivalent to 2000mmol in total of magnesium and aluminum) was charged, and 146mL of 5.47mol / L n-butanol hexane solution was added dropwise over 3 hours while stirring at 50℃. After the addition was completed, the line was washed with 300mL of hexane. The reaction was continued while stirring at 50℃ for another 2 hours. After the reaction was completed, the mixture was cooled to room temperature and used as raw material (b-1). The magnesium and aluminum concentrations of raw material (b-1) were 0.704mol / L. (2) Synthesis of raw material (b-2) In an 8L stainless steel autoclave that had been thoroughly purged with nitrogen, 1 mol / L of Mg6(C4H9) 12 2,000mL of hexane solution of Al(C2H5)3 (equivalent to 2000mmol in total of magnesium and aluminum) was charged, and 240mL of hexane solution of 8.33mol / L methylhydrogenpolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.) was pumped in while stirring at 80℃, and the reaction was continued for another 2 hours at 80℃ while stirring. After the reaction was completed, the mixture was cooled to room temperature and used as raw material (b-2). Raw material (b-2) had a total concentration of magnesium and aluminum of 0.786mol / L. (3) (B-1) Synthesis of Carrier 1,000mL of 1mol / L hydroxytrichlorosilane hexane solution was charged into an 8L stainless steel autoclave that had been fully purged with nitrogen, and 1340mL of the hexane solution of the organic magnesium compound (b-1) (equivalent to 943mmol of magnesium) was added dropwise over 3 hours at 65°C, and the reaction was continued for another 1 hour at 65°C with stirring. After the reaction was completed, the supernatant was removed and the mixture was washed four times with 1,800mL of hexane to obtain the (B-1) carrier. Analysis of this carrier showed that the magnesium content per 1g of solid was 7.5mmol. (4) Preparation of solid catalyst component [B] 103 mL of a 1 mol / L hexane solution of titanium tetrachloride and 131 mL of raw material (b-2) were added simultaneously over 3 hours to 1,970 mL of hexane slurry containing 110 g of the above (B-1) carrier while stirring at 10°C. The catalytic activity can be controlled by adjusting the amount of the hexane solution of titanium tetrachloride and raw material (b-2) here. Specifically, increasing the amount of these tends to increase the catalytic activity. After the addition, the reaction was continued for 1 hour at 10°C. After the reaction was completed, the supernatant was removed and the unreacted raw material components were removed by washing four times with hexane to prepare a solid catalyst component [B] (hereinafter also referred to as solid catalyst B).

[0193] [Catalyst Production Example 3] (Preparation of solid catalyst component [C]) (1) Synthesis of raw material (c-1) In an 8L stainless steel autoclave that had been thoroughly purged with nitrogen, 1 mol / L of Mg6(C4H9) 12 2,000mL of hexane solution of Al(C2H5)3 (equivalent to 2000mmol in total of magnesium and aluminum) was charged, and 240mL of hexane solution of 8.33mol / L methylhydrogenpolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.) was pumped in while stirring at 80℃, and the reaction was continued for another 2 hours at 80℃ while stirring. After the reaction was completed, the mixture was cooled to room temperature and used as raw material (c-1). Raw material (c-1) had a total concentration of magnesium and aluminum of 0.786mol / L. (2) Preparation of solid catalyst component [C] 1,600 mL of hexane was added to an 8 L stainless steel autoclave purged with nitrogen. While stirring at 10°C, 800 mL of a 1 mol / L hexane solution of titanium tetrachloride and 800 mL of raw material (c-1) were added simultaneously over 5 hours. The reaction was continued at 10°C for 1 hour. After the reaction was completed, the supernatant was removed and the unreacted raw material components were removed by washing with hexane four times to prepare a solid catalyst component [C] (hereinafter also referred to as solid catalyst C). The catalytic activity of this catalyst can be adjusted by the polymerization pressure during polymerization.

[0194] [Co-catalyst] As the cocatalysts, the following cocatalysts 1 to 3 were used. Cocatalyst 1: A mixture of commercially available triisobutylaluminum and diisobutylaluminum hydride (a 9:1 mixture by mass). Cocatalyst 2: Mg6(C4H9) 12 AL(C2H5)3 Co-catalyst 3: the above-synthesized raw material (a-4), raw material (b-2), or raw material (c-1)

[0195] [Example 1] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst (hereinafter also referred to as prepolymerization catalyst 1) was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst. After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component (hereinafter also referred to as a low molecular weight PE component) was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 78°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen for adjusting the intrinsic viscosity IV (molecular weight) was introduced so that the pressure in the polymerization reactor became 0.00035MPa, and ethylene was further introduced so that the pressure in the polymerization reactor became 0.7MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately additionally introducing ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid components. The obtained solid component was placed in a stainless steel beaker with a diameter of 68 mm and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm, yielding ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 82.0 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 15,000 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0196] [Example 2] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 78°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen was introduced to adjust the intrinsic viscosity IV (molecular weight) so that the pressure in the polymerization reactor became 0.00035MPa, and ethylene was further introduced so that the pressure in the polymerization reactor became 0.35MPa. Then, 5.0mg of the solid catalyst component [C], which was collected using a wet classification device (SATAKE i-Classifier manufactured by Satake Multimix Co., Ltd.), and only particles with a particle diameter of 2.0μm or less were dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing ethylene into the polymerization reactor. After that, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powdery solid components. The obtained solid components were placed in a stainless steel beaker with a diameter of 68 mm, and dried at 115°C for 2.0 hours while stirring at a stirring speed of 300 rpm to obtain ultra-high molecular weight polyethylene powder. The yield of the ultra-high molecular weight polyethylene powder was 131.6 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 26,300 (g-PE / g-catalyst). After removing scale and extremely coarse powder using a sieve with 425 μm openings, the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0197] [Example 3] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 78°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen was introduced to adjust the intrinsic viscosity IV (molecular weight) so that the pressure in the polymerization reactor was 0.00035MPa, and ethylene was further introduced so that the pressure in the polymerization reactor was 0.35MPa. Then, 5.0mg of solid catalyst component [C] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid components. The obtained solid component was placed in a stainless steel beaker with a diameter of 68 mm, and dried at 100 ° C for 2.5 hours while stirring at a stirring speed of 50 rpm to obtain ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 128.5 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 25,680 (g-PE / g-catalyst). Next, after removing scale and coarse powder using a sieve with 75 μm openings, the mixture was stirred at 115 ° C for 2.0 hours at a stirring speed of 300 rpm to obtain the final ultra-high molecular weight polyethylene powder. The physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0198] [Example 4] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst (hereinafter also referred to as prepolymerization catalyst 4) was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst. After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500 mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 0.6 mL of cocatalyst 1 was dispersed in 100 mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 78°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen for adjusting the intrinsic viscosity IV (molecular weight) was introduced so that the pressure in the polymerization reactor was 0.00035 MPa, and further, ethylene and 0.05 mol% of 1-butene (hereinafter also referred to as comonomer) were introduced from separate lines so that the pressure in the polymerization reactor was 0.7 MPa. Then, 40.0 mg of prepolymerization catalyst was dispersed in 200 mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by additionally introducing ethylene and comonomer into the polymerization reactor as appropriate. The polymerization reactor was then opened, and the contents were filtered under reduced pressure to separate and recover the powdery solid components. The obtained solid components were placed in a stainless steel beaker with a diameter of 68 mm, and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm to obtain ultra-high molecular weight polyethylene powder. The yield of the ultra-high molecular weight polyethylene powder was 80.3 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 14,290 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0199] [Example 5] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst (hereinafter also referred to as prepolymerization catalyst 5) was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst. After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 80°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen was introduced to adjust the intrinsic viscosity IV (molecular weight) so that the pressure in the polymerization reactor was 0.045MPa, and ethylene was further introduced so that the pressure in the polymerization reactor was 0.8MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid components. The obtained solid component was placed in a stainless steel beaker with a diameter of 68 mm and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm, yielding ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 94.5 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 16,730 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce microporous membranes for secondary battery separators by the methods described in the above (Molded body production method 1) to (Molded body production method 3), and evaluated by the above Evaluation methods 1 and 2. The evaluation results of the obtained microporous membranes are shown in Tables 3 and 4.

[0200] [Example 6] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst (hereinafter also referred to as prepolymerization catalyst 6) was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst. After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 80°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen was introduced to adjust the intrinsic viscosity IV (molecular weight) so that the pressure in the polymerization reactor was 0.016MPa, and ethylene was further introduced so that the pressure in the polymerization reactor was 0.8MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid components. The obtained solid component was placed in a stainless steel beaker with a diameter of 68 mm and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm, yielding ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 92.5 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 16,230 (g-PE / g-catalyst). Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce microporous membranes for secondary battery separators by the methods described in the above (Molded body production method 1) to (Molded body production method 3), and evaluated by the above Evaluation methods 1 and 2. The evaluation results of the obtained microporous membranes are shown in Tables 3 and 4.

[0201] [Example 7] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst (hereinafter also referred to as prepolymerization catalyst 7) ​​was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst. After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 80°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen was introduced to adjust the intrinsic viscosity IV (molecular weight) so that the pressure in the polymerization reactor was 0.0036MPa, and ethylene was further introduced so that the pressure in the polymerization reactor was 0.8MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid components. The obtained solid component was placed in a stainless steel beaker with a diameter of 68 mm and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm, yielding ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 96.5 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 16,980 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce microporous membranes for secondary battery separators by the methods described in the above (Molded body production method 1) to (Molded body production method 3), and evaluated by the above Evaluation methods 1 and 2. The evaluation results of the obtained microporous membranes are shown in Tables 3 and 4.

[0202] [Example 8] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 2 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst (hereinafter also referred to as prepolymerization catalyst 8) was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst. After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 2 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 70°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene gas was introduced so that the pressure in the polymerization reactor was 0.7MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid component. The obtained solid component was placed in a stainless steel beaker with a diameter of 68mm, and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm to obtain ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 79.5g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 11,000 (g-PE / g-catalyst). Scale and extremely coarse particles were removed using a sieve with 425μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0203] [Example 9] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 2 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst (hereinafter also referred to as prepolymerization catalyst 9) was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst. After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 2 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 58°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene gas was introduced so that the pressure in the polymerization reactor was 0.7MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid component. The obtained solid component was placed in a stainless steel beaker with a diameter of 68mm, and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm to obtain ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 72.5g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 8,980 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0204] [Example 10] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of the cocatalyst 3 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of the solid catalyst component [A] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst (hereinafter also referred to as prepolymerization catalyst 10) was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst. After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 3 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 70°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene gas was introduced so that the pressure in the polymerization reactor was 0.8MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid component. The obtained solid component was placed in a stainless steel beaker with a diameter of 68mm, and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm to obtain ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 70.3 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 8,520 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0205] [Comparative Example 1] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 78°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen was introduced to adjust the intrinsic viscosity IV (molecular weight) so that the pressure in the polymerization reactor was 0.00035MPa, and ethylene was further introduced so that the pressure in the polymerization reactor was 0.35MPa. Then, 5.0mg of solid catalyst component [C] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid components. The obtained solid component was placed in a stainless steel beaker with a diameter of 68 mm and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm, yielding ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 125.5 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 21,280 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0206] [Comparative Example 2] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 2 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 58°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene gas was introduced so that the pressure in the polymerization reactor was 0.35MPa. Then, 5.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid component. The obtained solid component was placed in a stainless steel beaker with a diameter of 68mm, and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm to obtain ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 52.5g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 4,230 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0207] [Comparative Example 3] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [B] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst (hereinafter, also referred to as prepolymerized catalyst H-3). After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 1 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 80°C, and stirring was started at a rotation speed of 1,000 rpm. Next, hydrogen was introduced to adjust the intrinsic viscosity IV (molecular weight) so that the pressure in the polymerization reactor was 0.24MPa, and ethylene was further introduced so that the pressure in the polymerization reactor was 0.8MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid components. The obtained solid component was placed in a stainless steel beaker with a diameter of 68 mm and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm, yielding ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 93.5 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 16,500 (g-PE / g-catalyst). Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce microporous membranes for secondary battery separators by the methods described in the above (Molded body production method 1) to (Molded body production method 3), and evaluated by the above Evaluation methods 1 and 2. The evaluation results of the obtained microporous membranes are shown in Tables 3 and 4.

[0208] [Comparative Example 4] After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane was introduced into the polymerization reactor. Then, 5.0mL of cocatalyst 3 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 25°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene was adjusted to 30NL with a flow meter, 750.0mg of solid catalyst component [A] was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch-type prepolymerization reaction was carried out for 1.0 hour. After the reaction was completed, the obtained prepolymerization catalyst was extracted into a nitrogen glove and collected. Next, main polymerization was carried out using the collected prepolymerized catalyst (hereinafter, also referred to as prepolymerized catalyst H-4). After evacuating the inside of a vessel-type 1.5L polymerization reactor equipped with a stirring device, 500mL of dehydrated normal hexane containing a low molecular weight polyethylene component was introduced into the polymerization reactor. Then, 0.6mL of cocatalyst 3 was dispersed in 100mL of dehydrated normal hexane and introduced into the polymerization reactor, the temperature of the polymerization reactor was adjusted to 60°C, and stirring was started at a rotation speed of 1,000 rpm. Then, ethylene gas was introduced so that the pressure in the polymerization reactor was 0.8MPa. Then, 40.0mg of prepolymerization catalyst was dispersed in 200mL of dehydrated normal hexane and introduced into the polymerization reactor, and a batch polymerization reaction was carried out for 1.0 hour. During the polymerization reaction, the pressure in the polymerization reactor was maintained by appropriately introducing additional ethylene into the polymerization reactor. Then, the polymerization reactor was opened, and the contents were filtered under reduced pressure to separate and recover the powder-like solid component. The obtained solid component was placed in a stainless steel beaker with a diameter of 68mm, and dried at 100°C for 2.5 hours while stirring at a stirring speed of 50 rpm to obtain ultra-high molecular weight polyethylene powder. The yield of ultra-high molecular weight polyethylene powder was 66.3 g, and the catalytic activity (amount of polyethylene obtained per unit catalyst weight) was 7,780 (g-PE / g-catalyst). Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the ultra-high molecular weight polyethylene powder were evaluated. The evaluation results of the ultra-high molecular weight polyethylene powder are shown in Tables 1 and 2. The obtained ultra-high molecular weight polyethylene powder was used to produce high strength fibers by the methods described in the above (Molded body production method 4) to (Molded body production method 6), and the fibers were evaluated by the above evaluation methods 3 and 4. The evaluation results of the obtained high strength fibers are shown in Tables 3 and 4.

[0209] [Table 1]

[0210] [Table 2]

[0211] [Table 3]

[0212] [Table 4] [Industrial Applicability]

[0213] INDUSTRIAL APPLICABILITY The ultra-high molecular weight polyethylene powder of the present invention has excellent moldability due to the presence of voids in the center of the powder, and can provide high-quality molded articles, such as separators and fibers for secondary batteries, and has industrial applicability.

Claims

1. A titanium-containing ultra-high molecular weight polyethylene powder, The titanium content is 10 ppm or less, The intrinsic viscosity IV is 1.0 dL / g or more and 33.0 dL / g or less, The ultra-high molecular weight polyethylene powder has voids therein, In the cross-sectional structure of the powder, a ratio of an area occupied by the void portion to a cross-sectional area A is 5% or more, The cross-sectional structure is such that the particle diameter of the powder is D 50 The cross-sectional structure of the powder P, which is in the range of ±5 μm, The cross-sectional area A is a 20 μm × 20 μm square area centered on the intersection of the diagonals of a rectangle circumscribing the powder P, Ultra-high molecular weight polyethylene powder.

2. a proportion of ultra-high molecular weight polyethylene powder having a particle diameter of 300 μm or more is 10 mass% or less based on the total amount of the ultra-high molecular weight polyethylene powder; The proportion of ultra-high molecular weight polyethylene powder having a particle diameter of less than 53 μm is 20 mass% or less based on the total amount of the ultra-high molecular weight polyethylene powder. The ultra-high molecular weight polyethylene powder according to claim 1.

3. The crystallinity is 70% or more and 85% or less. The ultra-high molecular weight polyethylene powder according to claim 1.

4. The apparent density, which means the density when a powder is filled into a container of a certain volume and the internal volume is taken as the volume, is 0.45 g / cm 3 Below is the The ultra-high molecular weight polyethylene powder according to claim 1.

5. The titanium content is 1.5 ppm or more. The ultra-high molecular weight polyethylene powder according to claim 1.

6. The titanium content is 3 ppm or less. The ultra-high molecular weight polyethylene powder according to claim 1.

7. A product obtained by molding the ultra-high molecular weight polyethylene powder according to any one of claims 1 to 6. Molded body.

8. The molded article is a separator for a secondary battery. The molded article according to claim 7.

9. The molded body is a fiber. The molded article according to claim 7.

Citation Information

Patent Citations

  • Powder of ultra-high-molecular-weight polyolefin and composition thereof

    JP1988033403A

  • Crystalline olefin polymer and copolymer in the form of spherical particles of high porosity

    JP1993194620A

  • Impregnated product, polyolefin composition containing the impregnated product and method for manufacturing the same, and molded product obtained from the composition

    JP2003026851A

  • High molecular weight polyolefin-based particle

    JP2007161896A

  • Polyethylene powder

    JP2015120784A