Hydrogen station and hydrogen generation method
The hydrogen station employs a PSA device and catalytic combustion to heat the dehydrogenation reaction safely and reduce CO2 emissions by using a platinum-supported alumina catalyst, addressing the challenges of flame use and emissions in hydrogen station heating processes.
Patent Information
- Application Number
- JP2023514315
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-16
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-04-16
AI Technical Summary
Hydrogen stations face challenges in safely heating the dehydrogenation reaction of hydrogenated aromatics without using open flames, which can be ignition sources, and in reducing CO2 emissions from heating processes.
A hydrogen station design that uses a PSA device to purify reaction product gas and regenerate adsorbents, employing a catalytic combustion tube to heat a heat medium with a platinum-supported alumina catalyst, avoiding direct flames and minimizing CO2 emissions.
The system effectively heats the dehydrogenation reaction without open flames, reducing CO2 emissions and ensuring safe operation by utilizing a highly active platinum catalyst for spontaneous ignition, thereby enhancing safety and environmental sustainability.
Smart Images

Figure 0007573732000006 
Figure 0007573732000007 
Figure 0007573732000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydrogen station that supplies hydrogen to fuel cell-equipped mobile objects such as fuel cell vehicles (FCVs) and fuel cell forklifts, and to a hydrogen generation method. [Background technology]
[0002] Hydrogen stations that fill fuel cell vehicles and other mobile vehicles with hydrogen are being developed based on the Japanese government's basic hydrogen strategy. Currently, there are about 110 hydrogen stations for FCVs in operation, and the goal is to have 900 by 2030, mainly in the four major metropolitan areas. Ultimately, about 15,000 hydrogen stations, equivalent to the current number of gas stations, are needed. After 2030, it will be necessary to spread hydrogen stations not only to the four major metropolitan areas but also throughout the country, including remote islands. Currently, hydrogen stations in practical use use compressed hydrogen and liquid hydrogen methods for storing and transporting hydrogen.
[0003] On the other hand, one of the methods for storing and transporting hydrogen is the organic chemical hydride method (see Non-Patent Documents 1 and 2). The organic chemical hydride method (OCH method) is a method in which hydrogen is converted into saturated cyclic compounds (hydrogenated aromatics) such as methylcyclohexane (MCH) that incorporate hydrogen into the molecule by hydrogenation reaction with aromatics such as toluene (TOL), thereby "storing" and "transporting" in a liquid state at room temperature and pressure, and at the same time, the required amount of hydrogen is extracted and used at the usage site by a dehydrogenation reaction of the saturated cyclic compounds. That is, the OCH method includes, for example, a hydrogenation reaction (hydrogen storage reaction) in which hydrogen is reacted with TOL, and a dehydrogenation reaction (hydrogen generation reaction) in which hydrogen is generated from MCH and TOL is recovered, and the TOL generated after hydrogen is extracted can be recovered as a hydrogen container (carrier) and reused.
[0004] In the OCH method, the dehydrogenation reaction that generates hydrogen from the saturated cyclic compounds after transportation is an endothermic reaction, and therefore requires heat input from the outside. Therefore, in the dehydrogenation reaction, in order to input the required amount of heat and maintain a predetermined reaction temperature condition (for example, a reaction temperature of 300 to 400°C), a method is used in which a liquid heat medium such as heated hot oil is circulated around the outside of a reaction tube filled with a dehydrogenation catalyst. Here, as a method for heating the hot oil, a method in which the pipe through which the hot oil flows is heated by a direct flame generated by burning fuel in a heating furnace is considered (see Patent Document 1). However, it is preferable for safety reasons to avoid the use of direct flames as much as possible within the premises of a hydrogen station that handles flammable hydrogen.
[0005] In addition, if fossil fuels such as natural gas or kerosene are used to heat the hot oil, the carbon derived from the fuel is emitted as CO2, which reduces the significance of using hydrogen.Furthermore, since an ignition source is required to burn the fuel, there is also the problem that the danger of ignition cannot be avoided simply by avoiding the use of the burner of the heating furnace. [Prior art documents] [Patent documents]
[0006] [Non-Patent Document 1] Yoshimi Okada, Energy and Resources, Vol.33, No.3, 168(2018) [Non-Patent Document 2] Yoshimi Okada, Tokyo High Pressure Gas Association Newsletter, August and September 2019 issues [Patent Document 1] JP 2015-182919 A Summary of the Invention [Problem to be solved by the invention]
[0007] In light of the above-mentioned background, the present inventors have conducted extensive research into a method for avoiding the use of direct flame and suppressing CO2 emissions when using a heated heat transfer medium to input heat into the dehydrogenation reaction of hydrogenated aromatics carried out in a hydrogen station.
[0008] As a result, the inventors discovered that the reaction product gas containing hydrogen obtained by the dehydrogenation reaction is purified by a PSA apparatus using the PSA method (pressure swing method), and that the heat medium can be heated without generating flames by catalytically combusting the purge gas (containing a high concentration of hydrogen) used to perform the regeneration operation of the column (adsorption tower) of the PSA apparatus (i.e., to remove impurities adsorbed to the adsorbent packed in the column). This makes it possible to suppress the CO2 emissions from the hydrogen station while avoiding the use of open flames, which can be a source of ignition in the hydrogen station. Furthermore, the inventors discovered that it is preferable to use a highly active platinum catalyst in combination with the combustion catalyst for catalytically combusting the purge gas so that the purge gas can be spontaneously ignited even in cold regions.
[0009] Therefore, an object of the present invention is to provide a hydrogen station and a hydrogen generation method that, when a heated heat transfer medium is used to input heat into the dehydrogenation reaction of hydrogenated aromatics, can avoid the use of direct flame in heating the heat transfer medium and reduce CO2 emissions. [Means for solving the problem]
[0010] One aspect of the present invention is a hydrogen station (1) comprising: a dehydrogenation reactor (23) that produces hydrogen by a dehydrogenation reaction of hydrogenated aromatics in the presence of a dehydrogenation catalyst; a heat supply device (26) that supplies heat to the dehydrogenation reactor via a heat medium heated by fuel; and a PSA device (33) that purifies the reaction product gas containing hydrogen produced by the dehydrogenation reactor using an adsorbent based on a pressure swing method, wherein the PSA device is supplied with a purge gas containing hydrogen used to regenerate the adsorbent, and the heat supply device has a storage tank (27) that contains the heat medium, and a catalytic combustion tube (28) that is disposed in the storage tank and performs catalytic combustion of the fuel in the presence of a combustion catalyst, and the purge gas discharged from the PSA device is supplied to the catalytic combustion tube together with air as the fuel.
[0011] According to this embodiment, when a heated heat transfer medium is used for heat input to the dehydrogenation reaction of hydrogenated aromatics, the heat transfer medium is heated by catalytic combustion of the purge gas used for regenerating the adsorbent in the PSA unit. This makes it possible to avoid the use of direct flame in heating the heat transfer medium and to suppress CO2 emissions.
[0012] In the above aspect, the dehydrogenation catalyst includes a platinum-supported alumina catalyst, the platinum-supported alumina catalyst having an alumina carrier and platinum supported on the alumina carrier, the alumina carrier having a surface area of 200 m 2 / g or more, pore volume is 0.50m 3 The γ-alumina carrier has a γ-alumina content of 0.1 wt % to 1.5 wt % of platinum particles as elemental platinum (Pt), and direct observation using a transmission electron microscope reveals that 70% or more of the platinum particles have a size of 8 Å to 15 Å.
[0013] According to this embodiment, a platinum-supported alumina catalyst containing platinum particles with an appropriately set particle size (platinum with an appropriately controlled particle distribution) is used for the dehydrogenation reaction of hydrogenated aromatics, and therefore the dehydrogenation reaction of hydrogenated aromatics (i.e., hydrogen production) can be stably carried out due to the effect of improving the catalyst life.
[0014] In the above aspect, the combustion catalyst may include a catalyst having the same configuration as the dehydrogenation catalyst.
[0015] According to this embodiment, a relatively highly active catalyst (e.g., platinum-supported alumina catalyst) having the same structure as the dehydrogenation catalyst is used as the combustion catalyst, so that the heat transfer medium can be heated well. In particular, by using a platinum-supported alumina catalyst containing platinum particles with an appropriately set particle size (platinum with an appropriately controlled particle distribution) for catalytic combustion, the heat transfer medium can be heated stably due to the effect of improving the catalyst life.
[0016] In the above aspect, the combustion catalyst may include a first catalyst that is filled in a fuel inlet portion (28A) of the catalytic combustion tube through which the fuel is introduced and has the same configuration as the dehydrogenation catalyst, and a second catalyst that has a different configuration from the first catalyst and is filled downstream of the fuel inlet portion of the catalytic combustion tube.
[0017] According to this embodiment, the fuel can be spontaneously ignited satisfactorily by the first catalyst at the fuel inlet of the catalytic combustion tube. Also, since the second catalyst having a different configuration from the first catalyst is filled downstream of the fuel inlet of the catalytic combustion tube, a catalyst (general-purpose catalyst) that is less expensive than the first catalyst can be used as the second catalyst, thereby reducing catalyst costs.
[0018] In the above aspect, the heat transfer medium may be hot oil.
[0019] According to this embodiment, heat can be easily supplied to the dehydrogenation reactor by an appropriate heat medium.
[0020] In the above aspect, the air may be divided and supplied to a plurality of different portions of the catalytic combustion tube.
[0021] According to this embodiment, the catalytic combustion reaction can be made uniform over a wide area within the catalytic combustion tube, and the occurrence of hot spots can be suppressed.
[0022] In the above aspect, the system may further include a dispenser (15) that supplies the hydrogen purified by the PSA device to a mobile body equipped with a fuel cell, a precooler (17) that cools the hydrogen supplied from the dispenser with a refrigerant, and a gas-liquid separator (31) that separates the reaction product gas into gas and liquid, and the reaction product gas is cooled in the gas-liquid separator by the refrigerant supplied from the precooler.
[0023] According to this embodiment, the reaction product gas can be cooled to a temperature lower than the atmospheric temperature by using the refrigerant of the precooler, so that aromatic compounds (e.g., toluene) and unreacted raw materials (e.g., cyclohexane) contained in the reaction product gas can be satisfactorily condensed in the gas-liquid separator.
[0024] In the above aspect, in the dehydrogenation reaction, hydrogen and toluene are produced by dehydrogenating cyclohexane as the hydrogenated aromatic compound, and the system may further include a first tank (4) for accommodating the cyclohexane and a second tank (6) for accommodating the toluene, and the first tank and the second tank may each be disposed underground.
[0025] This embodiment allows greater freedom in the use of aboveground space at hydrogen stations and makes it possible to make hydrogen stations more compact. In this case, it is also possible to use (repurpose) underground tanks for storing gasoline and the like at existing gas stations to store cyclohexane and toluene.
[0026] In the above aspect, at least one of the gas phase gas in the first tank and the gas phase gas in the second tank may be supplied to the catalytic combustion tube as the fuel together with the purge gas discharged from the PSA device.
[0027] According to this embodiment, hydrogen that may be contained in at least one of the gas phase in the first tank and the gas phase in the second tank can be safely removed.
[0028] In the above aspect, at least one of the gas phase gas in the first tank and the gas phase gas in the second tank may be introduced together with air into a fuel inlet portion (28A) through which the fuel is introduced in the catalytic combustion tube.
[0029] According to this embodiment, the hydrogen contained in at least one of the gas phase in the first tank and the gas phase in the second tank can be used as fuel for ignition in the catalytic combustion tube.
[0030] In the above aspect, the catalytic combustion tube may be a coil filled with the combustion catalyst.
[0031] According to this aspect, the heating medium can be uniformly heated by catalytic combustion.
[0032] In the above embodiment, the hydrogenated aromatic compound may be one or a mixture of two or more selected from the group consisting of hydrogenated monocyclic aromatic compounds, hydrogenated bicyclic aromatic compounds, and hydrogenated compounds having three or more aromatic rings.
[0033] According to this embodiment, the dehydrogenation reaction can be carried out satisfactorily using an appropriate hydrogenated aromatic compound.
[0034] In the above embodiment, the hydrogenated aromatic compound may be one or a mixture of two or more selected from the group consisting of methylcyclohexane, cyclohexane, trimethylcyclohexane, decalin, and dibenzotriol.
[0035] According to this embodiment, the dehydrogenation reaction can be carried out satisfactorily using an appropriate hydrogenated aromatic compound.
[0036] One aspect of the present invention is a method for generating hydrogen at a hydrogen station, comprising: generating hydrogen by a dehydrogenation reaction of hydrogenated aromatics in the presence of a dehydrogenation catalyst; supplying heat to the dehydrogenation reaction via a heat transfer medium heated with a fuel; purifying a reaction product gas containing hydrogen produced by the dehydrogenation reaction using an adsorbent based on a pressure swing method; regenerating the adsorbent using a purge gas containing hydrogen; and supplying the purge gas used for regenerating the adsorbent together with air as the fuel when heating the heat transfer medium.
[0037] According to this embodiment, when a heated heat transfer medium is used for heat input to the dehydrogenation reaction of hydrogenated aromatics, the heat transfer medium is heated by catalytic combustion of the purge gas that has been used for regenerating the adsorbent based on the pressure swing method. This makes it possible to avoid the use of direct flame in heating the heat transfer medium and to suppress CO2 emissions.
[0038] Hydrogen has been attracting attention as a clean secondary energy since the 1970s, and in Japan, research and development of hydrogen production technology and fuel cells was promoted in the Sunshine Project from 1974 to 1992, the Moonlight Project from 1978 to 1992, and the New Sunshine Project from 1993 to 2001. Development of the liquefied hydrogen method for large-scale hydrogen storage and transportation technology began in the WE-NET Project from 1992 to 2002. Meanwhile, the development of the organic chemical hydride method (OCH method) has a long history, dating back to the Euro-Quebec Project, an international research and development project implemented in the 1980s by the Quebec government in Canada and 12 European countries. This project was to produce hydrogen by electrolyzing water using surplus hydroelectric power abundantly available in Quebec, and to transport it across the Atlantic Ocean for use in Europe. The first candidate for hydrogen transportation methods is the liquid hydrogen method, the second is the liquid ammonia method, and the third is the OCH method. At the time, the organic chemical hydride method was called the MCH method. The EuroQuebec project ran for about 10 years until around 1992, but none of the methods were put to practical use and the project was terminated, and since then, the technology for storing and transporting hydrogen on a large scale has not been put to practical use.
[0039] In Japan, the WE-NET project, which was carried out from 1992 to 2002, saw the development of the liquefied hydrogen method, while research on the OCH method was mainly conducted at Japanese universities. After starting the development of dehydrogenation catalysts in 2002, the applicant made his first academic presentation at the World Hydrogen Congress held in Yokohama in 2004. From this period onwards, examples of research and development by companies began to be presented, and at present, the only technologies that have progressed to the demonstration level in the research and development of large-scale hydrogen storage and transportation technology are the liquefied hydrogen method and the OCH method proposed by the applicant.
[0040] The OCH process is a method in which hydrogen is hydrogenated with aromatics such as toluene (TOL) to convert it into saturated cyclic compounds such as methylcyclohexane (MCH) that incorporate hydrogen into the molecule, allowing it to be stored and transported in a liquid state at room temperature and pressure, and the required amount of hydrogen is extracted and used at the usage site through a dehydrogenation reaction. This method consists of a hydrogenation reaction (hydrogen storage reaction) in which hydrogen reacts with TOL, and a dehydrogenation reaction (hydrogen generation reaction) in which hydrogen is generated from MCH and TOL is recovered. The TOL generated after hydrogen is extracted is recovered as a hydrogen container (carrier) and reused repeatedly.
[0041] Hydrogen is an explosive gas, and therefore poses a high potential risk when stored and transported on a large scale as is. In the OCH method, hydrogen is incorporated into the molecules of MCH, a component of gasoline and diesel that is in a liquid state at room temperature and pressure, and is then stored and transported, making it a method that is theoretically very safe. Specifically, even if a tank or reactor in a system based on the OCH method were to catch fire, it would be similar to a conventional refinery fire, and it is considered extremely unlikely that it would cause severe damage to the surrounding urban areas. The idea that "accidents are bound to happen" is extremely important in safety measures, and this is why fundamental safety is required.
[0042] In the OCH process, about 530L of hydrogen gas can be stored in 1L of MCH liquid. To physically reduce the volume of hydrogen gas to 1 / 500 or less, it is necessary to compress it to 500 atmospheres or more, or to cool it to -253℃ or less to make it into 1 / 800 of its volume of liquid hydrogen. However, in the OCH process, a chemical reaction is used to reduce the volume to 1 / 500 at room temperature and pressure. In addition, since TOL and MCH are in a liquid state over a wide temperature range from -95℃ to 101℃, they can be handled as liquids like water in any environment on Earth. To build a large-scale supply chain, it is necessary to procure TOL in hundreds of thousands of tons. TOL is a fuel base material that is contained in high-octane gasoline at 10% by weight or more, and is also widely used as an industrial solvent. Furthermore, since TOL is a general-purpose chemical product with more than 20 million tons produced annually worldwide, it is easy to procure large quantities.
[0043] From the above, the first feature of the OCH process is that it can, in principle, reduce the potential risks involved in the large-scale storage and transportation of hydrogen to the same level of danger as conventional gasoline storage and transportation (i.e., it is a highly safe method), and this is the first reason why the applicant focused on this method. In addition, the storage of TOL and MCH in large tanks and the transportation of TOL and MCH in chemical tankers and chemical lorries have long been in practical use as chemical products. With the future trend toward electrification of automobiles, it is expected that demand for automobile fuels such as gasoline and diesel will decrease, and a major advantage of the OCH process is that it allows the repurposing of existing infrastructure such as storage tanks.
[0044] Furthermore, if hydrogen comes to be used on a large scale as a power generation fuel in the future, it is expected that there will come a time when hydrogen fuel stockpiles will be necessary, similar to the current oil stockpiles. Because TOL and MCH do not undergo chemical changes even when stored on a large scale for long periods of time, and long-term storage does not involve any particular energy consumption or loss, it is possible to convert current oil stockpiles into hydrogen energy stockpiles by storing MCH in their tanks.
[0045] The applicant focused on the OCH method, which is the safest method and is cost-effective because it allows the repurposing of existing infrastructure, and began developing a new dehydrogenation catalyst, which is the key to practical application, in 2002, and succeeded in developing the world's first new dehydrogenation catalyst that is industrially applicable to the OCH method. Thereafter, with the aim of establishing the technology for the entire system, a demonstration plant was constructed in 2013 that utilizes the catalyst developed for the dehydrogenation process and combines it with the TOL hydrogenation process, which is the hydrogen storage reaction, to continuously repeat hydrogen storage and hydrogen generation at the same location. Demonstration operation was performed for a total of approximately 10,000 hours from April of that year to November 2014, and it was confirmed that the high performance could be stably maintained as designed, completing the establishment of the technology.
[0046] As the final stage of development, a world-leading international hydrogen supply chain demonstration was carried out in 2020 as a NEDO (New Energy and Industrial Technology Development Organization) project, in which approximately 200 tons of hydrogen were transported from Brunei in Southeast Asia to the coastal area of Kawasaki City, Japan, using a system based on the OCH method, and a demonstration of transporting more than 100 tons of hydrogen per year using this system was completed.
[0047] Japanese Patent No. 4652695 (hereinafter referred to as Patent Document 3) and Japanese Patent No. 4142733 (hereinafter referred to as Patent Document 4) disclose dehydrogenation catalysts that can be used in the dehydrogenation reaction in the above-mentioned OCH process. Several specific methods have been proposed around the world for this dehydrogenation method, but in order to put into practical use on a large scale facilities for supplying fuel for power generation, not only a high yield but also a sufficient catalyst life is required. Therefore, it is preferable to use such a long-life and economical dehydrogenation catalyst in the hydrogen station and hydrogen generation method using the OCH process according to the present invention.
[0048] Patent document 3 describes a surface area of 150 m 2 / g or more, pore volume 0.55 cm 3 Patent Document 4 discloses a platinum-supported alumina catalyst characterized in that platinum is supported on a porous γ-alumina carrier having a molecular weight of 100000000 / g or more, an average pore diameter of 90 Å to 300 Å, and a ratio of pores with a pore diameter of 90 Å to 300 Å or less to the total pore volume of 60% or more. Patent Document 4 also discloses a homogeneous platinum-supported alumina catalyst in which the dispersion form of the supported platinum becomes homogeneous and the decomposition reaction is suppressed by incorporating sulfur into the alumina carrier, thereby improving the catalyst life. The disclosures of all documents cited in this specification, including Patent Documents 3 and 4, constitute a part of this specification, and detailed explanations are omitted.
[0049] Here, the feature of the dehydrogenation catalysts disclosed in Patent Documents 3 and 4 is that the particle size of the platinum particles supported on the alumina carrier is significantly smaller than that of conventional platinum catalysts. The average particle size of the platinum particles in a typical platinum-supported alumina catalyst is 20 Å or more. Conventionally, the OCH method was a method that could not be put into practical use because a dehydrogenation catalyst had not been developed. However, the applicant established the technology of this method by finding that the catalytic activity of the platinum-supported alumina catalyst is significantly improved by highly dispersing the platinum particles to small particles of about 10 Å, and by the end of 2020, the applicant completed the world's first international hydrogen supply chain demonstration using this method.
[0050] The platinum particle diameter of the dehydrogenation catalysts disclosed in Patent Documents 3 and 4 is 10 Å or less, and most of the platinum particle diameters are 20 Å or less. As described above, the minimum platinum particle diameter of existing platinum-supported alumina catalysts is about 20 Å, and the average particle diameter is 20 Å or more. In the hydrogen station according to the present invention based on the OCH method, it is preferable to use the dehydrogenation catalysts disclosed in Patent Documents 3 and 4, which contain platinum particles with an average particle diameter of 20 Å or less.
[0051] Regarding the catalysts that can be used as the dehydrogenation catalyst in the present invention, the homogeneous catalyst is effective when the diffusion of the raw material into the catalyst is sufficient, and the eggshell catalyst is effective when the diffusion into the catalyst is limited and not sufficient, so these two types of catalysts can be used depending on the diffusion state in the reaction field. In addition, even for the same reaction, the diffusion state of the raw material into the catalyst may differ depending on the position in the dehydrogenation reactor, and the raw material concentration is low near the outlet where the reaction has progressed, so the diffusion into the catalyst may be limited. In such a case, the homogeneous and eggshell catalysts can be used together in the reactor.
[0052] In addition, the degree of diffusion of raw materials inside a catalyst is generally expressed as the catalytic effectiveness factor, but it is possible to control the catalytic effectiveness factor by changing the size and shape of the catalyst pellets. Therefore, by changing the size and shape of the catalyst pellets for both uniform and eggshell type catalysts, it is possible to manufacture platinum-alumina catalysts with various catalytic effectiveness factors.
[0053] In the platinum-supported alumina catalyst that can be used as the dehydrogenation catalyst in the present invention, the alumina carrier on which platinum is supported is preferably one in which the pore size is controlled as uniformly as possible so that the pore distribution is sharp. 2 / g or more, pore volume is 0.5m 3 / g or more, an average pore diameter of 60 Å to 150 Å, and the ratio of pores with a diameter of the average pore diameter ±30 Å to the total pore volume is 60% or more. 2 If the amount is less than 0.5 m / g, the activity after catalysis will be insufficient, and the pore volume will be less than 0.5 m 3 If the average pore diameter is less than 150 Å, it is difficult to uniformly support the active metal component, and if the average pore diameter is smaller than 60 Å, the surface area is large but the pore volume is small, and conversely, if the average pore diameter is larger than 150 Å, the surface area is small and the pore volume is large. As a result of comprehensively considering these correlations, the average pore diameter is appropriate to be 60 Å to 150 Å. Also, if the ratio of pores with an average pore diameter of ±30 Å is less than 60%, the effect of the present invention in terms of catalytic performance is reduced. As a result of the pore size being uniform in this way, the alumina carrier has a uniform pore size throughout its powder and molded body. As a result, the process of dispersing and supporting platinum on the alumina carrier and the process of dispersing and supporting platinum throughout in accordance with the distribution of sulfur can be appropriately performed.
[0054] The hydrogen station according to the present invention may include a dehydrogenation reactor that generates hydrogen by a dehydrogenation reaction of hydrogenated aromatics (e.g., methylcyclohexane) that is a hydrogen carrier, and a PSA (Pressure Swing Adsorption) device that refines the generated hydrogen to a purity sufficient for filling fuel cell vehicles (FCVs), etc. The hydrogen station may also be equipped with a system that recovers TOL generated by the dehydrogenation reaction and unreacted MCH.
[0055] The dehydrogenation reactor in the present invention is preferably a multi-tubular fixed-bed reactor having a structure similar to that of a heat exchanger. That is, in the dehydrogenation reactor, catalytic reaction tubes filled with a dehydrogenation catalyst are arranged in parallel inside the reactor, and MCH gas heated to the reaction temperature is supplied to the catalytic reaction tubes, and a liquid heat transfer medium is supplied to the outside of the catalytic reaction tubes, thereby supplying heat necessary for the endothermic reaction of the dehydrogenation reaction and maintaining the reaction temperature.
[0056] In the present invention, a liquid with a large heat capacity is preferable as a heat medium for supplying heat to the catalytic reaction tube. When a gas is used as a heat medium, the heat transfer area becomes large due to its small heat capacity, and it is necessary to increase the external surface area of the catalytic reaction tube, which has the disadvantage of making the reactor larger than necessary. As a liquid heat medium, existing molten salt or hot oil can be used. However, many molten salts contain oxygen atoms in their molecules, and if the MCH gas in the reaction tube comes into contact with the molten salt due to an unexpected earthquake or the like, there is a possibility that it will ignite even in the reaction temperature range of 300 to 400 ° C. Therefore, it is preferable to use hot oil, which will not ignite even in the unlikely event of an accident, as a heat medium, because it is safer and will not lead to a fire in principle.
[0057] In the present invention, the hot oil may be a commercially available general heat transfer oil. Since the hot oil is a hydrocarbon with a large molecular weight, it may be thermally decomposed at about 400°C and lose heat. Therefore, it is preferable to use a hot oil that can minimize the thermal decomposition loss as the hot oil for supplying heat to the catalytic reaction tube.
[0058] In the present invention, the hot oil is heated by transferring heat from a catalytic combustion tube (catalytic combustion coil) filled with a combustion catalyst to the hot oil in a hot oil storage tank. The metallic material constituting the catalytic combustion tube can be inexpensive steel, since hot oil is not corrosive to the catalytic combustion tube.
[0059] In the present invention, the combustion catalyst filled in the catalytic combustion tube can be an existing combustion catalyst known as a catalyst used in catalytic combustion. However, the combustion catalyst must be able to reliably ignite the fuel spontaneously, and since spontaneous ignition at sub-freezing points is required at hydrogen stations in cold regions, it is desirable to use a highly active platinum catalyst. On the other hand, the dehydrogenation catalyst that can be used in the dehydrogenation reactor in the present invention is extremely active and can lower the dehydrogenation temperature that requires existing dehydrogenation catalysts by 100°C or more. Therefore, in the present invention, in addition to the existing combustion catalyst, a catalyst that can be used as a dehydrogenation catalyst is used as a higher performance combustion catalyst, so that the fuel can be reliably ignited spontaneously. In addition, if a catalyst that can be used as a dehydrogenation catalyst is used for all the combustion catalysts, it is believed that the fuel can be spontaneously ignited in any cold region on the earth.
[0060] In the present invention, catalysts that can be used as dehydrogenation catalysts or combustion catalysts include the platinum-supported alumina catalysts disclosed in the above-mentioned Patent Documents 3 and 4, as well as a novel platinum-supported alumina catalyst in which the particle size of the platinum particles supported on the carrier has been more appropriately set (the platinum particle distribution is appropriately controlled), as revealed by direct observation using a transmission electron microscope, as will be described in detail later.
[0061] In the present invention, existing combustion catalysts (second catalysts described later) that can be used as the combustion catalyst include combustion catalysts in which at least one of precious metals such as platinum, palladium, and iridium is supported on a carrier, and metal-supported catalysts in which at least one of metals such as nickel, cobalt, molybdenum, chromium, vanadium, and molybdenum is supported on a carrier. Precious metals are expensive but have high ignition properties, while non-precious metals have the advantage of being inexpensive but have low ignition properties.
[0062] In the present invention, the PSA apparatus has a plurality of columns (adsorption tanks) filled with adsorbents, and the reaction product gas is supplied to these columns to adsorb and remove impurities. The PSA apparatus supplies the reaction product gas to, for example, one of two columns, adsorbs the impurities with the adsorbent, and extracts hydrogen gas. Since the adsorption capacity of the adsorbent decreases over time, the supply destination of the reaction product gas is switched to the other column at an appropriate timing. The adsorbent is regenerated by lowering the pressure of the column to desorb the adsorbed impurities, and then purging the impurities by supplying product hydrogen gas that does not contain impurities. The PSA method is called the pressure swing method because the impurities are desorbed by changing the pressure. The purge gas used in the regeneration operation of the PSA apparatus uses product hydrogen, so it contains a high concentration of hydrogen even after the impurities are removed.
[0063] In the present invention, the fuel to be supplied to the catalytic combustion coil can be the purge gas discharged from the PSA device (i.e., after purging of impurities). The purge gas of the PSA device is supplied from a column in regeneration mode (regenerating the adsorbent) among a plurality of columns. Here, it is preferable that the regeneration process is carried out without interruption by sequentially switching the columns to be regenerated in the PSA device so that the purge gas as fuel is continuously supplied (discharged) without interruption. However, it is preferable to provide a hydrogen holder for storing the pressurized purge gas as necessary. For example, by supplying all the purge gas discharged from the PSA device to the hydrogen holder and storing it once, the purge gas can be stably supplied from the hydrogen holder to the catalytic combustion coil, and the entire amount of the purge gas discharged from the PSA device can be used without waste.
[0064] In the present invention, a gas-liquid separator can be provided between the dehydrogenation reactor and the PSA unit as a system for recovering TOL produced by the dehydrogenation reaction and unreacted MCH. In the gas-liquid separator, the reaction product gas taken out of the dehydrogenation reactor is cooled to 100°C or less, whereby liquid phase components (including TOL, MCH, etc. condensed into liquid) can be recovered. Furthermore, in the gas-liquid separator according to the present invention, it is preferable to cool the reaction product gas to 10°C or less in order to improve the recovery rate of TOL, MCH, etc.
[0065] In this way, recovering TOL, MCH, etc., to the extent possible from the reaction product gas before it is introduced into the PSA unit not only reduces the toluene loss calculated as the unrecovered amount, but also contributes to reducing the processing load of the PSA unit. In addition, an increase in the amount of impurities adsorbed and removed by the PSA unit can lead to an increase in CO2 emissions generated during catalytic combustion, so this also has the effect of reducing this.
[0066] When cooling the reaction product gas containing TOL and MCH, it can usually be cooled naturally to about 50°C without any particular energy consumption, and cooling water can be used to further cool it to about ambient temperature. However, it is difficult to cool the reaction product gas to below 10°C, especially in the summer when temperatures are high, so a new cold source is required for this purpose. At a hydrogen station, 5 kg of hydrogen can be filled into the hydrogen tank of an FCV within 3 minutes, but the hydrogen is cooled in advance to about -40°C by a precooler so that the temperature of the FCV hydrogen tank does not rise to 80°C or higher due to frictional heat generated during this process. Therefore, in the present invention, the cold source of the precooler can be used to cool the reaction product gas containing TOL and MCH.
[0067] Hydrogen stations where the dehydrogenation reaction takes place require tanks to store MCH, the raw material for the dehydrogenation reaction, and TOL, the product of the dehydrogenation reaction. Existing gas stations are equipped with underground tanks for gasoline, kerosene, heavy oil, etc. MCH and TOL are classified as Class 4, Class 1 petroleum, the same hazardous material classification as gasoline and kerosene. In addition, MCH and TOL are compounds with seven carbon atoms, and have a lower vapor pressure and less volatility than gasoline, which contains hydrocarbon components with four or more carbon atoms.
[0068] On the other hand, MCH and TOL stored at hydrogen stations contain hydrogen gas to the extent that it is dissolved, but the amount is so small that it is not normally possible for the gas phase components in the underground tank to reach a concentration above the explosion limit. However, it is preferable to install a system to remove dissolved hydrogen from the underground tank.
[0069] In order to remove the dissolved hydrogen, the present invention can subject the gas (tank gas) exhausted from the gas phase components of the tank (MCH tank) storing MCH and the tank (TOL tank) storing TOL to catalytic combustion treatment. In this case, the tank gas contains not only hydrogen but also MCH and TOL in amounts whose vapor pressures are undesirable for release into the atmosphere, and this has the advantage that these can also be subjected to catalytic combustion treatment. If the increase in cost is tolerable, it is also possible to exhaust the gas phase components by bubbling an inert gas such as nitrogen into the liquid in the tank.
[0070] Air can be used as the oxygen required for catalytic combustion of the tank gas. The catalytic combustion of the tank gas can also be performed using a similar catalytic combustion coil separately from the purge gas discharged from the PSA device. However, by mixing the tank gas with the purge gas and catalytically combusting it, there is an advantage that the hydrogen in the tank can be treated with a simple configuration. The tank gas can be catalytically combusted by spontaneous ignition when it is introduced together with air into the inlet of the catalytic combustion coil filled with a platinum-supported alumina catalyst.
[0071] The hydrogenated aromatic compound that can be used in the dehydrogenation reaction according to the present invention is not limited to MCH, and may be one or a mixture of two or more selected from the group consisting of hydrogenated monocyclic aromatic compounds such as cyclohexane, dimethylcyclohexane, and trimethylcyclohexane, hydrogenated bicyclic aromatic compounds such as tetralin, decalin, methyldecalin, biphenyl, and diphenylmethyl, and hydrogenated compounds having three or more aromatic rings such as dibenzotriol and tetradecahydroanthracene. Effect of the Invention
[0072] According to the above configuration, in the hydrogen station and the hydrogen generation method, when a heated heat transfer medium is used to input heat to the dehydrogenation reaction of hydrogenated aromatics, the use of direct flame in heating the heat transfer medium can be avoided and CO2 emissions can be suppressed. [Brief description of the drawings]
[0073] [Figure 1] Diagram of a conventional hydrogen station [Diagram 2] Configuration diagram of a hydrogen station according to the first embodiment [Diagram 3] FIG. 1 is a diagram showing a detailed configuration of a dehydrogenation unit according to a first embodiment. [Figure 4] Configuration diagram of a hydrogen station according to the second embodiment [Diagram 5] (A) Transmission electron microscope photograph of a catalyst taken in the 2000s, and (B) a diagram showing a transmission electron microscope photograph taken in recent years [Figure 6] Illustration of platinum particle size measurement based on transmission electron micrographs DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0074] Hereinafter, a hydrogen station and a hydrogen generating method according to an embodiment will be described with reference to the drawings.
[0075] Existing hydrogen stations are broadly divided into on-site and off-site types. The on-site type is a general term for a type in which hydrogen is produced within the hydrogen station. The off-site type is a general term for a type in which highly pure hydrogen is transported directly to the hydrogen station as compressed hydrogen or liquid hydrogen, and the hydrogen stored there is pressurized for use. The hydrogen station according to the present invention, which will be described in detail later, is expected to be classified as an on-site type since it generates hydrogen through a dehydrogenation reaction on-site and is similar to an on-site reforming hydrogen station. However, at present, the hydrogen station according to the present invention is in the research and development stage and no actual hydrogen stations exist, so it is unclear as to which classification it will ultimately be classified as.
[0076] (Prior Art) As shown in FIG. 1, a conventional on-site hydrogen station 101 includes a hydrogen production device 103 required for hydrogen production. As the hydrogen production device 103, a water electrolysis device or a reforming type hydrogen production device is used. In a reforming type hydrogen production device, fossil fuels such as city gas are steam reformed and then converted into hydrogen and carbon dioxide by a shift reaction. A water electrolysis device has a cost issue because it uses electricity to electrolyze water, and a reforming type hydrogen production device generates carbon dioxide, so they are not mainstream as hydrogen stations actually operating as commercial stations. Currently, there are about 50 off-site hydrogen stations using the compressed hydrogen method and the liquid hydrogen method as commercial stations.
[0077] The hydrogen produced by the hydrogen production device 103 is sent to the hydrogen storage tank 105 and temporarily stored there. The hydrogen stored in the hydrogen storage tank 105 is then sent to a compressor 109, where it is pressurized to about 800 atmospheres, and then sent to a pressure accumulator 111, where it is stored as product hydrogen.
[0078] The product hydrogen stored in the accumulator 111 is supplied via a dispenser 115 to a fuel cell vehicle (FCV) 113 that uses the hydrogen station 101 .
[0079] The requirement for hydrogen filling into the on-board tank of FCV113 is, for example, that 5 kg of hydrogen be filled in 3 minutes, and the frictional heat generated when hydrogen is filled at this rate increases the temperature inside the on-board tank of FCV113. Therefore, in order to keep the temperature inside the on-board tank below 80°C, the hydrogen supplied from dispenser 115 is cooled to about -40°C by a refrigerant supplied from pre-cooler 117 before being sent to FCV113.
[0080] (First embodiment) Next, the hydrogen station 1 and the hydrogen generation method thereof according to the first embodiment of the present invention will be described with reference to FIGS.
[0081] As shown in Fig. 2, the hydrogen station 1 according to the first embodiment includes a dehydrogenation unit 3 that produces hydrogen by a dehydrogenation reaction of hydrogenated aromatics. As will be described in detail later, the dehydrogenation unit 3 uses methylcyclohexane (MCH) as the raw material hydrogenated aromatics, and produces a reaction product gas (reaction product) containing hydrogen, toluene (TOL), and the like, by a dehydrogenation reaction of MCH in the presence of a dehydrogenation catalyst. This reaction product gas contains unreacted MCH, and the like.
[0082] MCH is stored in an MCH tank 4 and supplied to the dehydrogenation unit 3 via a raw material supply line L1. TOL is sent from the dehydrogenation unit 3 via a toluene discharge line L3 to a toluene tank 6, where it is stored. Supply of MCH to the MCH tank 4 and collection of TOL from the toluene tank 6 are carried out by a chemical tanker (not shown).
[0083] The MCH tank 4 and the toluene tank 6 may each be placed in an appropriate location within the hydrogen station 1, but it is preferable to place them underground within the hydrogen station 1. This allows greater freedom in the use of aboveground space in the hydrogen station 1 and also enables the hydrogen station 1 to be made more compact. In this case, underground tanks for storing gasoline and the like at existing gas stations can also be used to store MCH and TOL (i.e., they can be reused as the MCH tank 4 and the toluene tank 6).
[0084] The hydrogen produced by the dehydrogenation unit 3 is sent to the compressor 9 via a hydrogen transport line L5. The hydrogen sent to the compressor 9 has been purified to an extent that it can be used as product hydrogen in the dehydrogenation unit 3.
[0085] As with the conventional hydrogen station 101 shown in FIG. 1, hydrogen pressurized to about 800 atmospheres in the compressor 9 is sent to the pressure accumulator 11 via the hydrogen transport line L6. The hydrogen sent to the pressure accumulator 11 is stored there as product hydrogen. The product hydrogen stored in the pressure accumulator 11 is sent to the dispenser 15 via the hydrogen transport line L7, and is supplied to a fuel cell vehicle (FCV) 13 via a filling hose L11. The hydrogen supplied from the dispenser 15 is cooled to about -40°C by a refrigerant supplied from a precooler 17 before being sent to the FCV 13. It should be noted that the hydrogen station 1 can be used not only by the FCV 13, but also by any mobile object equipped with a fuel cell.
[0086] The refrigerant used to cool hydrogen circulates through a first refrigerant circulation line L13 provided between the dispenser 15 and the precooler 17, and exchanges heat with hydrogen in a heat exchanger for cooling hydrogen provided in the dispenser 15. Alternatively, the hydrogen in the dispenser 15 may be sent to the FCV 13 after passing through a heat exchanger for cooling hydrogen provided in the precooler 17 (i.e., after exchanging heat with the refrigerant).
[0087] Next, the detailed configuration of the dehydrogenation unit 3 will be described with reference to FIG.
[0088] In the dehydrogenation unit 3, MCH as a raw material stored in an MCH tank 4 is supplied to a dehydrogenation reactor 23 by a liquid pump (MCH transport pump) 21 provided in a raw material supply line L1. A heat exchanger 25 is provided in the raw material supply line L1 for exchanging heat between the MCH sent toward the dehydrogenation unit 3 and the reaction product gas extracted from the dehydrogenation reactor 23. More specifically, the MCH flowing through the raw material supply line L1 is heated to approximately the reaction temperature of the dehydrogenation reaction by heat exchange with the reaction product gas flowing through the reaction product gas line L21 in the heat exchanger 25, and is introduced in a gaseous state into the upper part of the dehydrogenation reactor 23.
[0089] The hydrogen station 1 includes a heat supply device 26 that supplies heat to the dehydrogenation reactor 23 via a heat medium heated by using fuel. The heat supply device 26 includes a storage tank 27 that stores the heat medium, and a catalytic combustion coil 28 (catalytic combustion tube) that is disposed in the storage tank 27 and filled with a combustion catalyst. In the catalytic combustion coil 28, catalytic combustion of the fuel is performed in the presence of the combustion catalyst, and the heat generated by the catalytic combustion coil 28 is transferred from the catalytic combustion coil 28 to the heat medium in the storage tank 27, thereby heating the heat medium. The heated heat medium circulates through a heat medium circulation line L23 installed between the dehydrogenation reactor 23 and the heat supply device 26. In this way, heat is supplied from the heat supply device 26 to the dehydrogenation reactor 23. As will be described in detail later, the heat supply device 26 uses a purge gas discharged from the PSA unit 33 (hereinafter referred to as discharge purge gas) as fuel.
[0090] The reaction product gas taken out from the dehydrogenation reactor 23 flows through the reaction product gas line L21, undergoes heat exchange with MCH in the heat exchanger 25, and is then introduced into the gas-liquid separator 31.
[0091] The gas-liquid separator 31 has a known configuration and separates the reaction product gas into a gas phase component and a liquid phase component by cooling the reaction product gas. In this embodiment, the reaction product gas introduced into the gas-liquid separator 31 is naturally cooled to a temperature of 100°C or less. In the gas-liquid separator 31, TOL and MCH contained in the reaction product gas are condensed into liquid to form a liquid phase component. The liquid phase component is extracted from the bottom of the gas-liquid separator 31 and introduced into the toluene tank 6 via the toluene discharge line L3 and stored therein.
[0092] On the other hand, the hydrogen constituting the gas phase components in the gas-liquid separator 31 is crude hydrogen containing TOL and MCH in amounts of vapor pressure according to the temperature. This crude hydrogen is extracted from the top of the gas-liquid separator 31 and sent to the PSA unit 33 via the crude hydrogen transport line L25.
[0093] The PSA unit 33 is a device that purifies the crude hydrogen (gas phase component of the reaction product gas) supplied from the gas-liquid separator 31. The PSA unit 33 supplies crude hydrogen to a column (adsorption tank) filled with an adsorbent based on the PSA (Pressure Swing Adsorption) method, and adsorbs and removes impurities contained in the crude hydrogen. The PSA unit 33 has multiple columns arranged in parallel, and performs continuous purification by alternately switching between a column for a regeneration process and a column for a purification process among the multiple columns.
[0094] In the purification step column to which the reaction product gas is supplied, the impurities are removed by adsorbing them to the adsorbent under high pressure. Meanwhile, in the regeneration step column, the pressure inside the column is lowered to desorb the adsorbed impurities, and high-purity hydrogen is supplied as a purge gas to purge the desorbed impurities. Product hydrogen is used as the purge gas used for the regeneration operation of the regeneration step column. The purge gas (hereinafter referred to as discharge purge gas) discharged from the PSA device 33 after the impurities have been removed contains the impurities desorbed from the adsorbent, but the hydrogen concentration is significantly higher than the impurity concentration. The discharge purge gas has a hydrogen concentration of, for example, 80% or more.
[0095] However, the hydrogen concentration of the discharged purge gas can be adjusted by the design of the column of the PSA device 33. That is, if the column (i.e., the amount of adsorbent) is made larger and the purification process time is lengthened, the amount of impurities adsorbed and removed increases, and the hydrogen concentration of the purge gas decreases. On the other hand, if the column is made smaller and the switching time (purification process time) is designed to be shorter, the amount of impurities adsorbed and removed is smaller, and the hydrogen concentration in the purge gas increases.
[0096] Here, the calorific value of hydrogen is very high at 120 MJ / kg per weight, but because hydrogen has a small molecular weight and is light, it is only 12 MJ / Nm 3It is a substance with a low calorific value. On the other hand, hydrocarbons such as gasoline and kerosene contain the heat of combustion of carbon, so their calorific value per unit weight is about 40 MJ / kg, which is about one-third that of hydrogen. As the ratio of hydrogen atoms to carbon atoms is not significantly different for TOL, its heat of combustion (39.5 MJ / kg) is roughly the same as that of gasoline, kerosene, etc.
[0097] Since the impurities in the exhaust purge gas are mainly TOL, if we assume that the hydrogen concentration in the exhaust purge gas is 80% and the remaining 20% is TOL, then 1 Nm 3 The calorific value of the exhaust purge gas is about 10 MJ for hydrogen and about 80 MJ for TOL. Therefore, the total calorific value of the exhaust purge gas is 90 MJ / Nm 3 In addition, if we assume that the TOL concentration in the exhaust purge gas is 10%, the TOL content is about 40 MJ, so the calorific value of the exhaust purge gas, including the hydrogen content, is 50 MJ / Nm 3 It becomes.
[0098] The hydrogen contained in the exhaust purge gas is valuable because it is product hydrogen. For example, 800L of hydrogen gas has a calorific value of 8.6MJ, and 200L of TOL gas has a calorific value of 34.6MJ, so 1000L of exhaust purge gas with a hydrogen concentration of 80% has a calorific value of 43.2MJ. On the other hand, the calorific value required to generate 800L of hydrogen by dehydrogenation reaction is 2.6MJ, so if the hydrogen used for the exhaust purge gas is generated by dehydrogenation reaction, the exhaust purge gas can be a heat source to generate about 17 times the volume of hydrogen.
[0099] On the other hand, when exhaust purge gas is generated with a hydrogen concentration of 90% and a TOL gas concentration of 10%, the sum of the calorific value of the TOL gas (17.3 MJ) and the calorific value of the hydrogen gas (9.6 MJ) is 26.9 MJ, so the calorific value of the exhaust purge gas will be reduced.
[0100] Furthermore, if the TOL concentration in the exhaust purge gas that provides the necessary calorific value becomes high, the amount of carbon dioxide emitted increases and the LCACO2 value becomes large, making the hydrogen station less useful. For this reason, it is essential to design an optimal system for hydrogen station 1 from the standpoints of the calorific value of the exhaust purge gas, economic efficiency based on hydrogen concentration, and the environmental impact of LCACO2.
[0101] The discharge purge gas from the PSA device 33 is sent to a purge gas tank 39 by a purge gas pump 37 installed in a line L31 for discharge purge gas, and stored there. Regarding the storage pressure of the purge gas tank 39, if the pressure is relatively low, a problem occurs in that the discharge purge gas cannot be appropriately supplied to the catalytic combustion coil 28 due to pressure loss during supply to the catalytic combustion coil 28. On the other hand, if the storage pressure of the purge gas tank 39 is relatively high, there is an advantage that the size of the purge gas tank 39 can be reduced, but the required power of the purge gas pump 37 increases, and the increased energy loss leads to a decrease in the energy efficiency of the hydrogen station 1. Therefore, the storage pressure of the purge gas tank 39 is determined in consideration of such pressure loss and required power as well as economic efficiency and energy efficiency, and is preferably in the range of 1 atm to 20 atm, and more preferably in the range of 3 atm to 9 atm.
[0102] The exhaust purge gas is introduced as fuel from the purge gas tank 39 to the catalytic combustion coil 28 of the heat supply device 26 via the purge gas supply line L33. It is preferable that the catalytic combustion coil 28 is filled with a highly active platinum-supported alumina catalyst (hereinafter referred to as the first catalyst) that is also used as a dehydrogenation catalyst for ignition, together with an existing combustion catalyst (hereinafter referred to as the second catalyst). The first catalyst is filled in the fuel inlet portion 28A of the catalytic combustion coil 28, and the amount of the first catalyst filled is small compared to that of the second catalyst. The fuel inlet portion 28A (i.e., the filling area of the first catalyst in the catalytic combustion coil 28) can be set to an appropriate range (length) from the upstream end of the catalytic combustion coil 28 depending on the surrounding environment (particularly the atmospheric temperature) of the hydrogen station 1, etc. This allows the exhaust purge gas to be satisfactorily spontaneously ignited by the first catalyst at the fuel inlet portion 28A of the catalytic combustion coil 28. In addition, since the downstream side of the fuel inlet 28A of the catalytic combustion coil 28 (i.e., other than the fuel inlet 28A) is filled with a second catalyst having a different configuration from the first catalyst, the catalyst cost can be reduced by using a catalyst (general-purpose catalyst) that is less expensive than the first catalyst as the second catalyst. However, in the hydrogen station 1, the use of only the first catalyst as the combustion catalyst is not prevented.
[0103] Ignition of fuel in catalytic combustion coil 28 can be achieved by providing an ignition source of approximately 700°C by heating a nichrome wire at fuel inlet portion 28A. However, when used at a hydrogen station 1, providing an open flame or a high-temperature portion of the nichrome wire is not desirable from a safety perspective.
[0104] On the other hand, the first catalyst has a feature that it has excellent ignition properties and can ignite the exhaust purge gas even at room temperature. In cold regions, moisture produced by combustion adheres to the combustion catalyst and freezes, which causes a problem of poor combustibility below freezing. The platinum-supported alumina catalyst used in the dehydrogenation reaction in the present invention is estimated to have activity 400 times or more higher than that of a normal platinum catalyst, and has extremely high ignition properties. By using the platinum-supported alumina catalyst as the combustion catalyst, the catalytic combustion coil 28 can quickly spontaneously ignite the exhaust purge gas without providing an ignition source such as a direct flame or an electric heating wire. In particular, by increasing the ratio of particles having a particle diameter of 8 Å to 15 Å among the platinum particles supported on the carrier in the first catalyst, the dispersibility of the reaction is increased, and even if moisture on the combustion catalyst freezes below freezing, the surface of the platinum is not completely covered with ice and the exhaust purge gas can quickly spontaneously ignite.
[0105] In addition, oxygen needs to be supplied when catalytically combusting the exhaust purge gas. Air containing oxygen required for catalytic combustion is supplied to the catalytic combustion coil 28 by an air pump 41 installed in an air supply line L37. The air supply line L37 is connected to a connection part 43 of a purge gas supply line L33. As a result, the exhaust purge gas flowing through the line L33 is mixed with air at the connection part 43 and then introduced into the fuel inlet part 28A of the catalytic combustion coil 28. In this way, the mixture of the exhaust purge gas and the required amount of air spontaneously ignites when it comes into contact with a first catalyst filled in the fuel inlet part 28A for spontaneous ignition.
[0106] The amount of air supplied to the line L33 should be more than the theoretical amount required for the combustion of the exhaust purge gas. However, if too much air is supplied, it may hinder the catalytic combustion reaction, and if too little air is supplied, gas diffusion in the combustion catalyst layer may be stagnated, making it difficult to maintain a good combustion reaction.
[0107] Moreover, the entire amount of air required for catalytic combustion in the catalytic combustion coil 28 does not necessarily have to be mixed with the exhaust purge gas introduced into the fuel inlet portion 28A (i.e., introduced into the connection portion 43 of the line L33). For example, at least a portion of the air introduced into the connection portion 43 as described above can also be introduced into an intermediate portion of the catalytic combustion coil 28 (i.e., downstream of the fuel inlet portion 28A) via a divided air supply line L37A (see the dashed line in FIG. 3). Such introduction of air into intermediate portions of the catalytic combustion coil 28 can be performed for at least one intermediate portion.
[0108] By dividing the air supply to the catalytic combustion coil 28 in this manner, it is possible to avoid problems such as the catalytic combustion reaction progressing rapidly near the fuel inlet 28A, forming hot spots, which hinder uniform heating of the heat medium in the storage tank 27, and the occurrence of sintering of metal particles (agglomeration of the active metal of the combustion catalyst) due to the formation of hot spots, which reduces the surface area of the active metal and reduces the performance of the combustion catalyst.
[0109] In addition, at least one of the gas constituting the gas phase components in the MCH tank 4 (hereinafter referred to as MCH tank gas) and the gas constituting the gas phase components in the toluene tank 6 (hereinafter referred to as toluene tank gas) can be supplied as fuel to the catalytic combustion coil 28 together with the discharge purge gas. More specifically, as shown by the dashed line in FIG. 3, the MCH tank gas discharged from the MCH tank 4 is sent to the connection part 43 of the purge gas supply line L33 by the gas discharge pump 44 installed in the tank gas discharge line L38. As a result, the MCH tank gas is mixed with the discharge purge gas at the connection part 43 located at the downstream end of the tank gas discharge line L38. Similarly, the toluene tank gas discharged from the toluene tank 6 is sent to the connection part 43 of the line L33 via the branch line L38A connected to the middle part of the tank gas discharge line L38. As a result, the toluene tank gas is mixed with the discharge purge gas at the connection part 43 located at the downstream end of the tank gas discharge line L38. The toluene tank gas may be introduced into the line L33 through a line (piping) different from that for the MCH tank gas. In addition, the position where the MCH tank gas and the toluene tank gas are introduced into the line L33 is not limited to the connection part 43 and can be changed as appropriate.
[0110] The fuel (including exhaust purge gas) catalytically combusted in the catalytic combustion coil 28 is discharged as exhaust gas from its downstream end. The exhaust gas is discharged into the atmosphere through an exhaust line L39 equipped with an exhaust control valve 45 while maintaining a temperature of 100°C or higher, at which moisture does not condense. Since the exhaust gas is a gas after complete combustion, its main components are water vapor and nitrogen, and it is converted into a gas containing low concentrations of CO2 and unreacted oxygen, so it is a harmless gas that can be discharged into the atmosphere.
[0111] The product hydrogen obtained by refining the crude hydrogen in the PSA unit 33 has, for example, a purity of 99.7% or more and a carbon content of 2 ppm or less. The product hydrogen is sent from the PSA unit 33 to the compressor 9 via a hydrogen transport line L5.
[0112] Second embodiment Next, a hydrogen station 1 and a hydrogen generation method thereof according to a second embodiment of the present invention will be described with reference to Fig. 4. In Fig. 4, the same components as those in the above-mentioned first embodiment are given the same reference numerals. Furthermore, with regard to the hydrogen station 1 according to the second embodiment, matters that are not specifically mentioned below are the same as those in the first embodiment. The hydrogen station 1 and the hydrogen generation method thereof according to the second embodiment are particularly suitable for improving the recovery rate of TOL contained in the reaction product gas.
[0113] As in the first embodiment, impurities other than hydrogen contained in the reaction product gas of the dehydrogenation reaction in the dehydrogenation reactor 23 are mainly TOL, and further include unreacted MCH and methane gas generated by decomposition side reactions. Of these impurities, TOL and MCH can be repeatedly used as hydrogen carriers in the OCH method, so it is preferable to recover as much of them as possible within the scope that ensures economic efficiency.
[0114] As in the first embodiment, the reaction product gas flowing through the reaction product gas line L21 is cooled by passing through the heat exchanger 25 to give heat to the raw material gas in the raw material supply line L1, and then cooled naturally to a temperature of 100° C. or less (for example, about 50° C.) in the gas-liquid separator 31. However, in hot seasons such as summer, the temperature in the gas-liquid separator 31 may exceed 60° C. The crude hydrogen, which is the gas phase component in the gas-liquid separator 31, contains TOL and MCH in a vapor pressure amount corresponding to the temperature. Therefore, further cooling the gas-liquid separator 31 to lower the temperature of the crude hydrogen is effective in lowering the concentrations of TOL and MCH in the crude hydrogen sent to the PSA unit 33.
[0115] Therefore, in the hydrogen station 1 according to the second embodiment, as shown in FIG. 4, the cold energy of the refrigerant in the precooler 17 is used to cool the crude hydrogen. More specifically, the inside of the gas-liquid separator 31 is cooled by circulating the refrigerant in the second refrigerant circulation line L41 provided between the precooler 17 and the gas-liquid separator 31. In this way, by supplying both the cold energy to be supplied to the dispenser 15 (see FIG. 2) and the cold energy to be supplied to the gas-liquid separator 31 by the precooler 17, it is possible to cool the crude hydrogen with a simple configuration. Since the refrigerant supplied to the gas-liquid separator 31 is at a relatively low temperature (for example, −40° C.), the supply amount can be reduced, and the piping size of the second refrigerant circulation line L41 can be reduced to facilitate insulation. The crude hydrogen in the gas-liquid separator 31 can be cooled to about −10° C. to 0° C. by cooling with the refrigerant. This makes it possible to drastically reduce the concentrations of TOL and MCH at their vapor pressures contained in the crude hydrogen, thereby reducing the processing load of the PSA device 33 and reducing the loss of TOL and MCH used as hydrogen carriers.
[0116] The second refrigerant circulation line L41 can be provided separately from the first refrigerant circulation line L13. Alternatively, the first refrigerant circulation line L13 and the second refrigerant circulation line L41 may be provided so as to be continuous with each other. In this case, the refrigerant after cooling the hydrogen in the dispenser 15 can be used for cooling the inside of the gas-liquid separator 31.
[0117] (dehydrogenation catalyst) Next, a novel dehydrogenation catalyst (platinum-supported alumina catalyst) that can be used in the hydrogen station 1 and the hydrogen generation method according to the first and second embodiments of the present invention will be described. As described above, this dehydrogenation catalyst can also be used as a combustion catalyst.
[0118] FIG. 5 shows (A) a transmission electron microscope photograph from the 2000s, and (B) a transmission electron microscope photograph from recent years, each of which was taken of a catalyst. FIG. 5(A) is a photograph of the eggshell-type catalyst disclosed in Patent Document 3. The photograph in FIG. 5(A) was taken in 2006 at a magnification of 1.8 million times using a Hitachi HD-200 type electron microscope, which was the most advanced transmission electron microscope at the time. FIG. 5(B) is a photograph of the homogeneous platinum-supported alumina catalyst disclosed in Patent Document 4. The photograph in FIG. 5(B) was taken in 2018 at a magnification of 2 million times using a JEM-ARM200 type electron microscope manufactured by JEOL.
[0119] The resolution of typical transmission electron microscopes in the 2000s was not sufficient to directly observe and measure platinum particle diameters of a few nanometers, so at the time it was common to estimate particle diameters using the CO pulse method (CO pulse adsorption method).Currently, advances in electron microscope performance have made it possible to directly observe particles of a few Å in size and molecules such as benzene rings with a resolution of around 1 Å.
[0120] In the transmission electron microscope photograph from the 2000s shown in Figure 5(A), it is clear that multiple platinum particles are independently supported, but because the outlines of the white dots (i.e., platinum particles) are not clear, the particles tend to appear larger than they actually are.
[0121] It can be seen that the outline of the white dots (platinum particles) can be observed more clearly with a recent transmission electron microscope shown in FIG. 5(B). Therefore, the particle size of platinum supported on the alumina carrier can be measured with higher accuracy by direct observation with a recent transmission electron microscope. The average particle size of platinum particles in the platinum-supported alumina catalyst according to the present invention can be calculated by measuring the particle sizes of a predetermined number of platinum particles (usually about 50 particles) in a transmission electron microscope photograph as shown in FIG. 5(B) and averaging them. In the transmission electron microscope, it is preferable to set the magnification so that the predetermined number of platinum particle sizes fit in the photograph (for example, 40 to 50 platinum particles can be observed in the field of view by observing the platinum-supported alumina catalyst of the present invention at 2 million times). The size of each platinum particle can be measured by aligning a measurement line with the particle outline on a computer screen provided in the electron microscope system. In this case, if the shape of the platinum particles has a major axis and a minor axis, the major axis can be measured by matching it to the outline of the major axis, and the minor axis can be measured in the same way. Since the platinum particles on the platinum-supported alumina catalyst of the present invention have almost no difference between the major axis and the minor axis, the major axis can be used as a representative value. In addition, the particle size can also be measured by printing an image, measuring the particle size with a ruler, and comparing it with the scale on the image.
[0122] In contrast, the platinum particle diameters disclosed in the above Patent Documents 3 and 4 are estimated values using the CO pulse method. It is considered that there is an error between the particle diameters estimated using the CO pulse method and those measured by direct observation using a transmission electron microscope. This is because the CO pulse method is more likely to estimate the particles as small particles than those measured by direct observation. In the CO pulse method, one molecule of CO is adsorbed per platinum atom on the platinum particle surface, so the total CO adsorption amount is measured, and the shape of the platinum particle is assumed to be a cube, and the length of one side is estimated as the particle diameter. At this time, the estimation is made under the assumption that CO is not adsorbed on the support. In the case of a platinum-supported alumina catalyst, CO is preferentially adsorbed on platinum, and the injection of CO is immediately stopped when the distilled CO becomes equal to the amount of injected CO, but in the case of an alumina support, the surface area is large and a certain amount of CO is adsorbed on the support, so this amount of CO is estimated as being adsorbed on the platinum surface.
[0123] Here, the CO pulse method is explained. When CO is injected into a sample in a pulsed manner, CO is adsorbed onto the supported metal surface at the beginning of the injection, and only a small amount of CO is eluted. Eventually, when most of the supported metal surface is adsorbed and a steady state is reached, most of the injected CO is discharged. At this time, the amount of CO discharged during adsorption is subtracted from the amount of CO discharged at the steady state, and the sum of these differences is calculated as the amount of CO adsorption. The CO pulse method is a method for calculating the metal surface area, dispersion rate, and particle size from this amount of adsorption and the supported metal content. The specific calculation method is explained below.
[0124] The amount of gas adsorbed per 1 g of catalyst at 0° C., V, was calculated from the amount of CO gas adsorbed at the measurement temperature, Vt, by the following formula (1). V=(Vt / W)×{273 / (273+t)} (ml / g·cat) ... (1) Here, assuming that the metal content of the sample is C (%) and the atomic weight of the supported metal is M, the number of moles of supported metal per 1 g of sample, R, can be calculated from formula (2). R=(C / 100)×(1 / M) (mol / g·cat) ... (2) The number of moles K of gas adsorbed per 1 g of sample can be calculated using equation (3). K = V / (22.4×10 -3 ×10 6 ) (mol / g cat) ...(3) From these, the degree of dispersion B (the ratio of effectively supported metal to the supported metal) can be calculated from the formula (4). B = (K / R) × 100 (%) ... (4) When the lattice constant of the supported metal catalyst is a (Å), the lattice constant area a 2 If one gas molecule is adsorbed per metal, the specific surface area S of the metal can be calculated using equation (5). S = number of gas molecules adsorbed per 1 g of sample × a 2 =K x 6.02 x 10 23 ×(a×10 -10 ) 2 ... (5)
[0125] In addition, if we assume that the supported metal particle is a cube with a side length of D (m), five of the six faces of the particle are effective faces, so Effective area of one particle S=5D 2 (m 2 ) ... (6) Volume of one particle v=D 3 (m 3 ) ... (7) If the number of supported metal particles per gram of sample is n, Specific surface area of supported metal S=ns=n5D 2 (m 2 ) ... (8) Volume of supported metal Vc=nv=Nd 3 (m 3 ) ... (9) From equations (6) to (9), the length of one side D (m) is expressed as in equation (10). S / Vc=5 / D ∴D=5Vc / S (m) ... (10) Here, the content of the supported metal C (%) and the specific gravity d (g / cm 3 ), the volume Vc of the supported metal per gram of sample is expressed by equation (11). Vc = weight of supported metal per 1 g of sample (g / g) / specific gravity of supported metal (g / cm 3 ) = C / 100 / d (g / cm 3 ) ... (11) Therefore, the particle size is calculated from equation (12). Particle size=5Vc / S = {5(C / 100 / d)×10 -6} / S (m) = {5(C / 100 / d)×10 -6 ×10 10} / S (Å) ... (12)
[0126] Thus, in conventional platinum-supported alumina catalysts, the particle size of platinum supported on the alumina carrier was measured (calculated) based on the CO pulse method, which had a relatively large error, or on transmission electron microscope photographs taken at the time (see FIG. 5(A)). Therefore, in conventional platinum-supported alumina catalysts, it was difficult to control the platinum particle size with high accuracy, and the suitable range of the platinum particle size was set to a relatively wide range.
[0127] In contrast, in the present invention, a platinum particle size range (platinum particle size distribution) that can significantly improve catalyst life compared to conventional platinum-supported alumina catalysts is set based on the platinum particle size value measured with relatively high accuracy based on recent transmission electron microscope photographs (see FIG. 5(B)). In the platinum-supported alumina catalyst according to the present invention, it is preferable that 70% or more of the platinum particles supported on the γ-alumina carrier have a size of 8 Å to 15 Å when directly observed with a transmission electron microscope. More preferably, it is preferable that 80% or more of the platinum particles supported on the γ-alumina carrier have a size of 8 Å to 15 Å. Even more preferably, it is preferable that 90% or more of the platinum particles supported on the γ-alumina carrier have a size of 8 Å to 15 Å.
[0128] Next, the eggshell-type metal-supported catalyst and the homogeneous metal-supported catalyst in the present invention will be described. The eggshell-type metal-supported catalyst refers to a state in which the metal species supported in the cross section of the molded catalyst are dispersed and supported only in the outer shell part of the cross section. That is, a metal-supported part in which the metal species is supported is formed in the outer shell part of the porous carrier. The homogeneous metal-supported catalyst refers to a state in which the metal species is dispersed throughout the entire cross section of the catalyst, and a metal-supported part in which the metal species is supported is formed throughout the entire inside of the molded body of the porous carrier.
[0129] The platinum-supported alumina catalyst according to the present invention comprises an alumina support and platinum supported on the alumina support.
[0130] Next, the alumina carrier used in the platinum-supported alumina catalyst according to the present invention will be described.
[0131] The alumina carrier may be a porous γ-alumina carrier. More specifically, the alumina carrier may be a porous γ-alumina carrier obtained by filtering and washing an aluminum hydroxide slurry produced by neutralizing an aluminum salt, dehydrating and drying the obtained alumina hydrogel, and then calcining the resulting alumina hydrogel at 400°C to 800°C for about 1 to 6 hours, as disclosed in, for example, JP-B-6-72005. More preferably, the alumina carrier may be a porous γ-alumina carrier obtained through a pH swing process in which the pH value of the alumina hydrogel is alternately changed between an alumina hydrogel dissolution pH region and a boehmite gel precipitation pH region, and an alumina hydrogel forming substance is added during the pH change from at least one of the pH regions to the other pH region to grow the crystals of the alumina hydrogel. The porous γ-alumina carrier obtained through this pH swing process is excellent in uniformity of pore distribution, has little variation in physical properties even in the alumina carrier pellets after molding, and has stable physical properties for each individual pellet.
[0132] The present inventors further investigated the relationship between the drying and calcination conditions of the alumina hydrogel (boehmite) and the particle size of the supported platinum, and as a result, found that in order to stably support most of the platinum particles with a size in the range of 8 Å to 15 Å on the γ-alumina support, it is particularly preferable that the drying temperature be 200°C or lower, the subsequent calcination temperature be 250°C or higher and 400°C or lower, and the calcination time be 1 hour or higher and 12 hours or lower.
[0133] When preparing the homogeneous platinum-supported alumina catalyst according to the present invention, the sulfur or sulfur compound to be dispersed and contained in the alumina carrier in advance is not particularly limited as long as it has sulfur element and can be contained in the catalyst carrier in a homogeneously dispersed state during or after the preparation of the catalyst carrier. For example, examples of sulfur or sulfur compounds include sulfur crystal powder, sulfuric acid, ammonium sulfate, and other sulfur-containing compounds, and sulfur compounds that are soluble in water or organic solvents are preferred from the viewpoint of easy dispersion of sulfur on the carrier, and examples of such sulfur compounds include sulfuric acid, ammonium sulfate, and the like.
[0134] The amount of sulfur contained in the carrier is preferably 0.15% by weight (wt%) or more and 5.0% by weight or less, more preferably 0.15% by weight or more and 3.0% by weight or less, in terms of elemental sulfur (S). If the sulfur content is less than 0.15% by weight, the effect of uniformly supporting the metal all the way to the center of the catalyst is low, and if the sulfur content exceeds 5% by weight, the sulfur tends to aggregate locally, and the problem of the metal not being dispersed and supported in such local areas is likely to occur. For these reasons, the most suitable range of the sulfur content in terms of the effect of uniformly dispersing and supporting the metal is 0.15% by weight or more and 5.0% by weight or less.
[0135] As a result of further investigations into the relationship between the sulfur concentration and the particle size of the supported platinum, the present inventors have found that in order to stably support most of the platinum particles with a size in the range of 8 Å to 15 Å on the γ-alumina support, it is particularly preferable that the sulfur content be in the range of 0.5 to 1.2 wt % in terms of elemental sulfur (S), including sulfur or a sulfur compound.
[0136] In the present invention, the method for preparing the sulfur-containing catalyst carrier containing the above-mentioned sulfur or sulfur compound may be any method as long as it can contain sulfur or a sulfur compound in a state where it is dispersed throughout the entire cross section of the carrier. For example, the following methods may be used: A: A method in which a metal hydroxide gel, which is a precursor of a metal oxide obtained during the preparation of the catalyst carrier, is kneaded with sulfur powder, molded into a predetermined shape, and then dried and fired; B: A method in which a metal hydroxide gel, which is a precursor of a metal oxide containing sulfur, is prepared using a metal sulfate and / or sulfuric acid during the preparation of the catalyst carrier, molded into a predetermined shape, and then dried and fired; C: A method in which a metal hydroxide gel, which is a precursor of a metal oxide, is molded into a predetermined shape during the preparation of the catalyst carrier, and then dried and fired to prepare a metal hydroxide gel; C: a method in which a metal hydroxide gel that will be a precursor of the metal oxide during preparation of the catalyst support is formed into a predetermined shape, then dried to obtain a dry metal hydroxide, this dry metal hydroxide is impregnated with a sulfur compound solution and then fired to prepare a catalyst support; D: a method in which a metal hydroxide gel that will be a precursor of the metal oxide during preparation of the catalyst support is formed into a predetermined shape, then dried to obtain a dry metal hydroxide gel, this dry metal hydroxide gel is then fired to obtain a fired metal oxide, this fired metal oxide is impregnated with a sulfur compound solution such as an aqueous sulfuric acid solution or an aqueous ammonium sulfate solution, and then fired again to prepare a catalyst support.
[0137] As a result of further investigations into the method for preparing a sulfur-containing catalyst support, the present inventors have found that in order to stably support most of the platinum particles with a size in the range of 8 Å to 15 Å on the γ-alumina support, it is particularly preferable to disperse and support sulfur on the surface of the γ-alumina support using the above method E.
[0138] Regarding the calcination conditions for preparing this sulfur-containing catalyst carrier, the calcination temperature is usually 100° C. to 1000° C., preferably 350° C. to 800° C., and the calcination time is 0.5 hours to 48 hours, preferably 1 hour to 24 hours. If the calcination temperature is lower than 350° C., the conversion from hydroxide to oxide may not be sufficient, and conversely, if it is higher than 800° C., the surface area after calcination may be significantly reduced.
[0139] The present inventors further investigated the drying and calcination conditions in preparing the sulfur-containing γ-alumina support and found that, in order to stably support most of the platinum particles in the size range of 8 Å to 15 Å on the γ-alumina support, it is particularly preferable that the drying temperature be 100° C. or higher and 200° C. or lower and the drying time be 3 hours or higher and 12 hours or shorter, and that the calcination temperature be 250° C. or higher and 400° C. or lower and the calcination time be 1 hour or higher and 12 hours or shorter.
[0140] In the present invention, the amount of platinum supported on the sulfur-containing catalyst carrier is 0.05% by weight or more and 5.0% by weight or less, preferably 0.1% by weight or more and 3.0% by weight or less, in terms of platinum element. If the amount of platinum supported is less than 0.05% by weight, there is a problem of low activity, while if it is more than 5.0% by weight, there is a problem of large platinum particle size, low selectivity, and easy sintering and easy deterioration.
[0141] As a result of further investigations into the suitable amount of platinum supported, the inventors of the present application have found that in order to stably support most of the platinum particles with a size in the range of 8 Å to 15 Å on the γ-alumina support, the amount of platinum supported is preferably 0.1 wt % or more and 1.5 wt % or less in terms of the platinum element content, and more preferably 0.5 wt % or more and 1.5 wt % or less in terms of improving the life of the prepared platinum-supported alumina catalyst.
[0142] In the present invention, when platinum metal is supported on a γ-alumina carrier, the above-mentioned γ-alumina carrier may be impregnated with a solution of a platinum compound, dried, and then calcined at a predetermined temperature. Examples of the platinum compound include platinum chloride, bromide, ammonium salt, carbonyl compound, amine and ammine complexes, acetylacetonato complexes, and various other complex compounds. Examples of the platinum compound include chloroplatinic acid, acetylacetonato platinum, ammonium platinate, bromoplatinic acid, platinum dichloride, platinum tetrachloride hydrate, carbonyl platinum dichloride dichloride, and dinitrodiamineplatinate.
[0143] As a result of further investigations into the platinum compound to be impregnated, the inventors of the present application have found that, from the viewpoint of improving the life of the prepared platinum-supported alumina catalyst, it is particularly preferable to impregnate the calcined γ-alumina carrier with platinum using an aqueous solution of chloroplatinic acid as the aqueous platinum reagent solution.
[0144] After the alumina support is impregnated with the platinum compound solution, the alumina support to which the platinum compound is attached is dried under conditions of 50°C to 200°C for 0.5 to 48 hours, and then calcined under conditions of 350°C to 600°C for 0.5 to 48 hours, more preferably 350°C to 450°C for 0.5 to 5 hours.
[0145] The present inventors further investigated suitable drying and calcination conditions after platinum impregnation of the alumina carrier (for example, when the platinum element content is in the range of 0.5% by weight to 1.5% by weight), and found that, in order to stably support most of the platinum particles with a size in the range of 8 Å to 15 Å on the γ-alumina carrier, the particularly preferred drying conditions are a drying temperature of 100° C. or higher and 200° C. or lower, and a drying time of 3 hours or higher and 12 hours or lower, and the particularly preferred calcination conditions are a calcination temperature of 250° C. or higher and 450° C. or lower, and a calcination time of 1 hour or higher and 8 hours or lower.
[0146] Next, as the final step of the platinum carrying step, the alumina carrier to which the platinum compound is attached is subjected to hydrogen reduction treatment in a hydrogen gas atmosphere under reduction conditions of 350° C. to 600° C. and 0.5 hours to 48 hours, preferably 350° C. to 550° C. and 3 hours to 24 hours. If the temperature during this hydrogen reduction is less than 350° C., there is a problem that platinum is not sufficiently reduced, and if it exceeds 600° C., there is a problem that platinum particles are sintered during reduction, decreasing the degree of metal dispersion.
[0147] As a result of further investigations into suitable temperature conditions for hydrogen reduction after platinum impregnation and calcination, the inventors of the present application have found that in order to stably support most of the platinum particles with a size in the range of 8 Å to 15 Å on the γ-alumina support, the hydrogen reduction temperature is particularly preferably 300°C or higher and 450°C or lower, and is particularly preferably equal to or lower than the temperature at which calcination is performed after platinum impregnation, and the hydrogen reduction time is particularly preferably 1 hour or higher and 15 hours or shorter.
[0148] The amount of alkali added to the eggshell type platinum-supported alumina catalyst and the homogeneous platinum-supported alumina catalyst prepared by incorporating sulfur into the γ-alumina carrier is 0.1% by weight to 5% by weight, preferably 0.3% by weight to 3.0% by weight, and more preferably 0.5% by weight to 1.5% by weight. If the amount of alkali metal supported is less than 0.1% by weight, there is a problem that the catalyst life is short and the effect is low, while if it is more than 5.0% by weight, there is a problem that the activity decreases and the catalyst life is shortened.
[0149] The present inventors further investigated the appropriate amount of alkali to be added in order to support most of the platinum particles with a size in the range of 8 Å to 15 Å on the γ-alumina support, and found that an alkali addition amount of 0.5 wt % or more and 1.5 wt % or less does not significantly affect the size of the prepared platinum particles.
[0150] Examples of the alkaline metal compound used when supporting an alkaline metal on the eggshell type platinum-supported alumina catalyst and the homogeneous platinum-supported alumina catalyst prepared by incorporating sulfur into a γ-alumina carrier include chlorides, bromides, iodides, nitrates, sulfates, acetates, propionates, etc. of alkaline metals, and preferably those that are water-soluble and / or soluble in organic solvents such as acetone, etc., include sodium chloride, sodium bromide, sodium iodide, sodium nitrate, sodium sulfate, sodium acetate, sodium propionate, potassium chloride, potassium bromide, potassium iodide, potassium nitrate, potassium sulfate, potassium acetate, potassium propionate, calcium chloride, calcium bromide, calcium iodide, calcium nitrate, calcium sulfate, calcium acetate, calcium propionate, calcium chloride, calcium bromide, calcium iodide, calcium nitrate, calcium sulfate, calcium acetate, calcium propionate, etc.
[0151] In addition, when an alkaline metal is supported on an eggshell type platinum-supported alumina catalyst or a homogeneous platinum-supported alumina catalyst prepared by incorporating sulfur into a γ-alumina carrier, the catalyst is impregnated with a solution of an alkaline metal compound, and then dried under drying conditions of room temperature to 200°C and for 0.5 to 48 hours, preferably 50°C to 150°C and for 0.5 to 24 hours, more preferably 80°C to 120°C and for 0.5 to 5 hours, and then calcined under conditions of 350°C to 600°C and for 0.5 to 48 hours, preferably 350°C to 450°C and for 0.5 to 5 hours.
[0152] The present inventors further investigated suitable drying conditions after impregnation with a solution of an alkaline compound in order to support most of the platinum particles with a size in the range of 8 Å to 15 Å on a γ-alumina support, and found that the size of the supported platinum particles is not affected as long as the drying temperature is from room temperature to 200°C, regardless of the drying time.
[0153] The eggshell-type platinum-supported alumina catalyst and the homogeneous platinum-supported alumina catalyst prepared by adding sulfur to a γ-alumina carrier are impregnated with an alkali metal, and the alkali metal-supported dried product obtained by drying is directly subjected to final hydrogen reduction without subsequent calcination. The reduction conditions for this hydrogen reduction are 350°C to 600°C and 0.5 hours to 48 hours, preferably 350°C to 550°C and 3 hours to 24 hours, in a hydrogen gas atmosphere. If the alkali metal-supported dried product is calcined prior to hydrogen reduction, the catalytic performance in terms of activity, selectivity, and life will be reduced. In addition, if the temperature during hydrogen reduction is less than 350°C, platinum will not be sufficiently reduced, and if it exceeds 600°C, platinum particles will be sintered during reduction, resulting in a decrease in metal dispersion.
[0154] The present inventors further investigated suitable conditions for hydrogen reduction after impregnation with a solution of an alkali compound and drying in order to support most of the platinum particles in the size range of 8 Å to 15 Å on a γ-alumina support, and found that the size of the supported platinum particles is not affected so long as the temperature and reduction time are equal to or less than those of the hydrogen reduction, which is the final step in the platinum support process before the addition of the alkali metal.
[0155] Hereinafter, preferred embodiments of the dehydrogenation catalyst of the present invention will be specifically described based on examples and comparative examples.
[0156] [Comparative Example 1] (Comparison of particle size measurement results by direct observation using a transmission electron microscope and measurement results by a CO pulse method for the eggshell catalyst described in Patent Document 3 and the homogeneous platinum-supported alumina catalyst described in Patent Document 4)
[0157] The platinum particle diameter of the eggshell catalyst described in Patent Document 3 is a particle diameter estimated based on the degree of dispersion estimated from the CO adsorption amount measured by a CO pulse method and on the assumption that the platinum particles have a cubic shape, and as shown in Table 2 (Experimental Example 1) and Table 3 (Experimental Example 2) of Patent Document 3, the particle diameter was estimated to be in the range of 5.5 Å to 14 Å.
[0158] On the other hand, the particle diameter of the homogeneous platinum-supported alumina catalyst described in Patent Document 4 was estimated to be 6.5 to 11 Å, as shown in Table 1 (Example 4) of Patent Document 4.
[0159] As shown in Figure 6, the particle diameters of 42 platinum particles (see numbers 1-42 in Figure 6) in the uniform platinum-supported alumina catalyst described in Patent Document 4 were measured by direct observation using a transmission electron microscope. The image of the catalyst shown in Figure 6 corresponds to the transmission electron microscope photograph shown in Figure 5(B). This catalyst corresponds to catalyst No. 6 (particle diameter 6.5 Å) described in Patent Document 4 (Table 1).
[0160] Platinum particle size can be measured using the particle size measurement function on the electron microscope screen. However, similar measurement results can also be obtained by comparing the scale shown in the electron microscope photograph with the length of the part showing the largest particle size. The particle size measurement results are shown in Table 1. The average particle size of the 42 particles shown in Table 1 was 16.8 Å (1.68 nm).
[0161] [Table 1]
[0162] In addition, according to the platinum particle size measurement results shown in Table 1, 19 out of 42 platinum particles measured (approximately 45%) had a size range of 8 Å to 15 Å (0.8 to 1.5 nm), and 23 platinum particles had a size greater than 15 Å (1.5 nm) and greater than 16 Å (1.6 nm).
[0163] Thus, when the homogeneous platinum-supported alumina catalyst described in Patent Document 4 (Catalyst No. 6 in Table 1 of Patent Document 4) was measured from an image directly observed with an electron microscope, the average platinum particle size was 1.68 nm (16.8 Å). This shows that the estimated platinum particle size (6.5 Å) by the CO pulse method described in Patent Document 4 is significantly smaller than the value measured by direct observation of an electron microscope photograph.
[0164] As described above, for the eggshell catalyst described in Patent Document 3 and the uniform platinum-supported alumina catalyst described in Patent Document 4, the particle diameters were estimated to be 5.5 to 14 Å based on the degree of dispersion estimated from the CO adsorption amount measured by the CO pulse method and on the assumption that the platinum particles have a cubic shape. However, these particle diameters are also considered to be significantly smaller values when directly observed using an electron microscope.
[0165] This large error in the particle size estimation value by the CO pulse method is thought to be due to the following: In the CO pulse method, estimations are made under the assumption that the introduced CO is adsorbed to platinum atoms exposed on the surface of the platinum particles; however, in reality, a large amount of CO is also adsorbed on the alumina support, resulting in the observed amount of CO adsorption being large; and the shape of the platinum particles is assumed to be a cube, and one side of the cube is estimated as the particle size.
[0166] [Comparative Example 2] (Preparation method described in the examples of Patent Document 3)
[0167] A method for preparing the eggshell-type platinum-supported γ-alumina catalyst described in the examples of Patent Document 3 will be described below.
[0168] As in the examples of Patent Document 3, a porous γ-alumina carrier was produced based on the prior art described in Example 1 of JP-B-6-72005. The outline of this method is that an aqueous solution of sodium aluminate was added instantaneously to hot dilute sulfuric acid while vigorously stirring, to obtain an aluminum hydroxide slurry suspension (pH 10). This was used as seed aluminum hydroxide, and the operation of alternately adding hot dilute sulfuric acid and an aqueous solution of sodium aluminate at regular intervals while continuing to stir was repeated, to obtain a filtered and washed cake. This was extruded, dried, and then calcined at 500°C for 3 hours.
[0169] The gamma-alumina support thus prepared has a surface area of 240 m 2 / g, pore volume 0.713 cm 3The physical properties are pore size (g), average pore size (A) of 119 Å, and pore size (A) of 90-300 Å of 90%. 79 g of 0.4 wt%-chloroplatinic acid aqueous solution prepared so that the pH value is 2.0 was added to 20 g of this porous γ-alumina carrier, and the carrier was allowed to stand for 3 hours for impregnation, after which water was removed by decantation, and the carrier was dried at 120°C for 3 hours and then calcined in a muffle furnace at 400°C for 3 hours under air flow. The calcined product thus obtained was cooled to room temperature in a desiccator, and then reduced at 400°C for 15 hours under hydrogen flow to prepare a dehydrogenation catalyst (corresponding to catalyst No. 2 described in Table 2 in the examples of Patent Document 3). The estimated platinum particle size of this catalyst by the CO pulse method was 5.5 Å.
[0170] [Comparative Example 3] (Preparation method described in the Examples of Patent Document 4)
[0171] A method for preparing a homogeneous platinum-supported γ-alumina catalyst described in the examples of Patent Document 4 will be described below.
[0172] 3900cc of an aluminum nitrate aqueous solution with a concentration of 2.67mol / L was prepared, and 3900cc of a 14% ammonia aqueous solution was prepared. 20L of pure water was placed in a 30L enamel container and heated to 70°C while stirring. While continuing to stir, 1300cc of aluminum nitrate aqueous solution was added and stirred for 5 minutes (pH=2.0), and then 1300cc of ammonia aqueous solution was added and stirred for 5 minutes (pH=7.4), performing a pH swing operation four times. The resulting aluminum hydroxide slurry aqueous solution was filtered to recover a cake, and then the cake was redispersed in 20L of pure water and filtered again, performing a washing operation three times to obtain a washed gel.
[0173] The washed cake was air-dried to adjust the moisture content, and then molded into a rod shape with a diameter of 1.6 mm using an extruder. After drying (120°C, 3 hours), it was crushed to a length of about 1 cm and calcined in a muffle furnace (500°C, 3 hours) to obtain alumina carrier A that does not contain sulfur. The obtained alumina carrier A had a BET surface area of 275 m 2 / g, mercury porosimetry pore volume 0.65 cm 3 / g. The obtained alumina carrier A had a mean pore size of 8.9 nm, a sharp pore size distribution in which most of the pores were concentrated near the mean pore size, and the volume of pores having a pore size of 7 to 10 nm was 80% or more of the total pore volume.
[0174] Alumina carrier A was impregnated with an aqueous solution of ammonium sulfate with a concentration of 0.38 mol / L so that the sulfur content after calcination was 0.5% by weight, and the solvent was removed using an evaporator. Thereafter, alumina carrier A was dried (120°C, 3 hours) and calcined (500°C, 3 hours) to obtain an alumina carrier containing 0.5% by weight of sulfur.
[0175] The alumina carrier thus prepared was impregnated with a chloroplatinic acid aqueous solution adjusted to pH=2.0 so that the platinum loading after calcination would be 0.6% by weight, then the water was removed using an evaporator, dried (120°C, 3 hours), and calcined (400°C, 3 hours), after which it was loaded into a flow-type hydrogen reduction device and hydrogen-reduced under a hydrogen stream at 450°C for 15 hours to obtain a 0.6wt% platinum-loaded alumina catalyst. The platinum particle diameter of this platinum-loaded alumina catalyst was estimated to be 6.5Å by the CO pulse method.
[0176] [Comparative Example 4] (Reaction test method for the eggshell catalyst described in Patent Document 3 and the homogeneous catalyst described in Patent Document 4)
[0177] A comparison of the dehydrogenation reaction test method and reaction test results for the eggshell catalyst described in Patent Document 3 and the homogeneous catalyst described in Patent Document 4 is shown. Here, the dehydrogenation reaction test described in Patent Document 3 and the dehydrogenation reaction test described in Patent Document 4 are different in the reaction temperature and the concentration of hydrogen supplied together with the raw material MCH. This is because the dehydrogenation catalyst described in Patent Document 3 and the dehydrogenation catalyst described in Patent Document 4 have different deterioration rates. The reaction test conditions for the deterioration rate at the time of development of the dehydrogenation catalyst described in Patent Document 3 were conditions under which deterioration was relatively difficult. Specifically, the reaction test conditions described in Patent Document 3 are conditions of a reaction temperature of 300°C and a hydrogen co-supply concentration of 20%, while the reaction conditions described in Patent Document 4 are conditions of a reaction temperature of 320°C and a hydrogen co-supply concentration of 5%. This is because the dehydrogenation catalyst described in Patent Document 4 is a catalyst with a small deterioration rate and is difficult to deteriorate, so the reaction test was performed under accelerated conditions under which deterioration is likely to proceed.
[0178] In this comparative example, the results of a dehydrogenation reaction test of methylcyclohexane (MCH) are shown, in which the dehydrogenation catalyst described in Patent Document 3 was used as Catalyst No. 1 and the dehydrogenation catalyst described in Patent Document 4 was used as Catalyst No. 2.
[0179] 10cc of each of the above catalysts was filled in the longitudinal center of a stainless steel reaction tube with an inner diameter of 12.6mmφ×300mm and a thermocouple protection tube with an outer diameter of 1 / 8 inch in the center of the reaction tube cross section, so that the center of the catalyst layer was located, and 10cc of spherical α-alumina beads with a diameter of 1mm were filled on the upper side of the catalyst as a preheating layer. The temperature was raised to 320°C under hydrogen flow (LHSV=5.0; 50cc / hr). Next, methylcyclohexane (MCH) was supplied to the reactor in an amount equivalent to LHSV=2.0 (20cc / hr) by a high-performance liquid chromatography (HPLC) liquid delivery pump (HPLC pump), and the flow rate of hydrogen was immediately adjusted so that the amount of hydrogen gas was 5mol% of the total amount of MCH and hydrogen gas. The output of the electric furnace was adjusted so that the temperature of the center of the catalyst layer was 320°C during the reaction, and the reaction test was performed.
[0180] A gas-liquid separator was provided at the outlet of the reaction tube to separate liquid products such as toluene produced by the dehydrogenation reaction from gases such as hydrogen gas, and the recovered liquid products and gases were each analyzed by gas chromatography.
[0181] The MCH conversion rate (%), toluene selectivity (%), toluene yield (%), and methane concentration (ppm) were determined 2 hours and 300 hours after the start of the reaction. The results are shown in Table 2.
[0182] [Table 2]
[0183] [Example 1] (Method of preparing eggshell-type catalyst according to the present invention and measurement results of particle size)
[0184] 3900cc of an aluminum nitrate aqueous solution with a concentration of 2.67mol / L was prepared, and 3900cc of a 14% ammonia aqueous solution was prepared. 20L of pure water was placed in a 30L enamel container and heated to 70°C while stirring. While continuing to stir, 1300cc of aluminum nitrate aqueous solution was added and stirred for 5 minutes (pH=2.0), and then 1300cc of ammonia aqueous solution was added and stirred for 5 minutes (pH=7.4). This pH swing operation was performed four times. The resulting aluminum hydroxide slurry aqueous solution was filtered to recover a cake, and then this cake was redispersed in 20L of pure water and filtered again, and this washing operation was performed three times to obtain a washed gel.
[0185] The washed cake was air-dried to adjust the moisture content, and then molded into a rod shape with a diameter of 1.6 mm using an extruder. After drying (120°C, 3 hours), it was crushed to a length of about 1 cm and calcined in a muffle furnace (350°C, 3 hours) to obtain alumina carrier A that does not contain sulfur. The obtained alumina carrier A had a BET surface area of 290 m 2 / g, mercury intrusion pore volume of 0.61 cm 3 / g. The obtained alumina carrier A had a mean pore size of 9.5 nm (95 Å), a sharp pore size distribution in which most of the pores were concentrated near the mean pore size, and the volume of pores with a pore size of 7 to 11 nm (70 to 110 Å) was 80% or more of the total pore volume.
[0186] The alumina carrier thus prepared was impregnated with an aqueous solution of chloroplatinic acid adjusted to pH=2.0 so that the amount of platinum supported after calcination would be 0.6 wt%, and then the water was removed using an evaporator, dried (120°C, 3 hours), and calcined (350°C, 3 hours). The alumina carrier was then loaded into a flow-type hydrogen reduction device and reduced with hydrogen at 400°C for 15 hours under a hydrogen stream to obtain an alumina catalyst carrying 0.6 wt% platinum (hereinafter referred to as catalyst NO.3). The average particle diameter of the platinum particles in the catalyst NO.3 thus obtained was 11.27 Å, as measured by direct observation using an electron microscope. The measurement results of the platinum particle diameter are shown in Table 3.
[0187] [Table 3]
[0188] In Table 3, the smallest platinum particle is 8 Å (0.8 nm) and the largest platinum particle is 21 Å (2.1 nm). It can also be seen that 40 of the 45 platinum particles measured (about 89%) are in the size range of 8 Å to 15 Å (0.8 to 1.5 nm), and only 5 platinum particles are larger than 15 Å (1.5 nm) and 16 Å (1.6 nm) or more.
[0189] [Example 2] (Preparation method of homogeneous catalyst according to the present invention and measurement results of particle size)
[0190] 3900cc of an aluminum nitrate aqueous solution with a concentration of 2.67mol / L was prepared, and 3900cc of a 14% ammonia aqueous solution was prepared. 20L of pure water was placed in a 30L enamel container and heated to 70°C while stirring. While continuing to stir, 1300cc of aluminum nitrate aqueous solution was added and stirred for 5 minutes (pH=2.0), and then 1300cc of ammonia aqueous solution was added and stirred for 5 minutes (pH=7.4). This pH swing operation was performed four times. The resulting aluminum hydroxide slurry aqueous solution was filtered to recover a cake, and then this cake was redispersed in 20L of pure water and filtered again, and this washing operation was performed three times to obtain a washed gel.
[0191] The washed cake was air-dried to adjust the moisture content, and then molded into a rod shape with a diameter of 1.6 mm using an extruder. After drying (120°C, 3 hours), it was crushed to a length of about 1 cm and calcined in a muffle furnace (350°C, 3 hours) to obtain alumina carrier A that does not contain sulfur. The obtained alumina carrier A had a BET surface area of 290 m 2 / g, mercury intrusion pore volume of 0.61 cm 3 / g. The obtained alumina carrier A had a mean pore size of 9.5 nm (95 Å), a sharp pore size distribution in which most of the pores were concentrated near the mean pore size, and the volume of pores with a pore size of 7 to 11 nm (70 to 110 Å) was 80% or more of the total pore volume.
[0192] The gamma-alumina carrier thus prepared was impregnated with an aqueous solution of ammonium sulfate with a concentration of 0.38 mol / L so that the sulfur content after calcination would be 0.5% by weight. The solvent was removed using an evaporator, and the carrier was then dried (120°C, 3 hours) and calcined (350°C, 3 hours) to obtain an alumina carrier containing sulfur.
[0193] The obtained alumina carrier was impregnated with a chloroplatinic acid aqueous solution adjusted to pH=2.0 so that the platinum loading after calcination would be 0.6 wt%. The water was removed using an evaporator, dried (120°C, 3 hours), and calcined (350°C, 3 hours). The alumina carrier was then loaded into a flow-type hydrogen reduction device and reduced with hydrogen at 400°C for 15 hours under a hydrogen stream to obtain a 0.6 wt% platinum-loaded alumina catalyst (hereinafter referred to as catalyst NO.4). The average particle diameter of the platinum particles in the thus obtained catalyst NO.4 was measured by direct observation using an electron microscope and was 11.27 Å. The measurement results of the platinum particle diameter are shown in Table 4.
[0194] [Table 4]
[0195] In Table 4, the smallest platinum particle is 8 Å (0.8 nm) and the largest platinum particle is 22 Å (2.2 nm). It can also be seen that 41 of the 47 platinum particles measured (about 87%) are in the size range of 8 Å to 15 Å (0.8 to 1.5 nm), and only 6 platinum particles are larger than 15 Å (1.5 nm) and 16 Å (1.6 nm) or more.
[0196] [Example 3] (Reaction test results of eggshell catalyst and homogeneous catalyst according to the present invention)
[0197] For the eggshell-type platinum-supported γ-alumina catalyst (Catalyst No. 3) prepared under the preparation conditions of the present invention shown in Example 1, and the homogeneous platinum-supported γ-alumina catalyst (Catalyst No. 4) prepared under the preparation conditions of the present invention shown in Example 2, a dehydrogenation reaction test of methylcyclohexane was carried out by the same method and reaction conditions as those shown in Comparative Example 4. Table 5 shows the results of the dehydrogenation reaction test, as well as the average particle size of platinum particles measured based on direct observation of electron microscope images, and the calculated percentage of the number of platinum particles having a size range of 8 Å to 15 Å among the measured platinum particles.
[0198] [Table 5]
[0199] As can be seen from the reaction test results in Table 5, by optimizing the catalyst preparation conditions according to the present invention, a platinum-supported alumina catalyst with excellent performance, especially in terms of catalyst life, was obtained. Compared with the eggshell-type platinum-supported γ-alumina catalyst (Catalyst No. 1) prepared under conventional preparation conditions, the eggshell-type platinum-supported γ-alumina catalyst (Catalyst No. 3) prepared under the preparation conditions of the present invention has a longer life with less decline in toluene yield. Also, compared with the homogeneous platinum-supported γ-alumina catalyst (Catalyst No. 2) prepared under conventional preparation conditions, the homogeneous platinum-supported γ-alumina catalyst (Catalyst No. 4) prepared under the preparation conditions of the present invention has a longer life with less decline in toluene yield.
[0200] The reaction tests in Table 5 were conducted under accelerated test conditions, so the deterioration of the toluene yield after about 300 hours appears small. However, the deterioration under the accelerated test conditions is significantly larger than the deterioration under the reaction conditions in actual commercial practice. Roughly speaking, the lifespan of catalyst No. 1 in Table 5 is about 1 year, and that of catalyst No. 2 is about 2 years, while that of catalyst No. 3 can be expected to be about 3 years, and that of catalyst No. 4 can be expected to be about 4 years.
[0201] In addition, in the catalysts (Catalyst No. 3, Catalyst No. 4) according to the present invention, in which the catalyst life is improved by the preparation method shown in Example 1 and Example 2, more than 80% of all platinum particles measured have a particle diameter in the range of 8 Å to 15 Å in terms of the platinum particle diameter measured by direct observation of the observation image by electron microscope. Compared with Catalyst No. 2, in which the ratio of particle diameters in the range of 8 Å to 15 Å is about 45%, in the catalysts according to the present invention, the ratio of platinum particles having a particle diameter in the range of 8 Å to 15 Å is remarkably high, and the ratio of platinum particles having a large size of 16 Å or more is significantly reduced.
[0202] The reason why the catalyst life of the catalysts (Catalyst No. 3, Catalyst No. 4) prepared by the preparation methods shown in Examples 1 and 2 of the present invention was significantly improved is believed to be due to the optimization of the calcination conditions during the preparation of the γ-alumina support, the calcination conditions after impregnation with platinum (and sulfur, if necessary) and drying, and the conditions during the final hydrogen reduction.
[0203] The reason why the life of conventional catalysts (i.e., the dehydrogenation catalysts described in Patent Documents 3 and 4) was impaired is believed to be that in the conventional preparation methods, the calcination conditions for preparing the γ-alumina support exceeded 400°C, the calcination conditions after impregnation with platinum (and sulfur as required) and drying were also similarly high, and further, the final hydrogen reduction temperature was as high as the calcination conditions after impregnation of the support and platinum (and sulfur as required) and drying. In particular, it was found that in preparing the catalyst, it is more preferable to set the final hydrogen reduction temperature to 400°C or lower and to carry out the calcination temperature conditions for the thermal history before hydrogen reduction at a temperature lower than the final hydrogen reduction conditions.
[0204] The catalyst of the present invention could not have been completed using the electron microscope technology that was available for conventional catalysts (i.e., at the time of the patent applications for the dehydrogenation catalysts described in Patent Documents 3 and 4). However, the catalyst of the present invention was only completed thanks to the subsequent evolution of electron microscope technology, which has progressed to the point where the catalyst preparation conditions and the size of the platinum particles in the prepared catalyst can be accurately measured by direct observation. [Industrial Applicability]
[0205] The hydrogen station using the OCH method of the present invention is highly safe and can be suitably used as a hydrogen station for filling hydrogen into mobile bodies equipped with fuel cells, such as FCVs, fuel cell forklifts, and fuel cell ships. The OCH method is a highly safe method for storing and transporting hydrogen using MCH, which is liquid at room temperature and pressure, and since there is a high possibility that a large-scale supply chain for hydrogen for hydrogen-fired power generation will be established, there is a possibility that inexpensive MCH can be used on a large scale for hydrogen stations. Since hydrogen carriers can be delivered to areas, including rural areas and remote islands, using rail transport, lorry transport, and ship transport, which are the existing transport infrastructure for gasoline and kerosene, hydrogen stations using the OCH method are suitable for the nationwide deployment of hydrogen stations after 2030, and the hydrogen generation method is also applicable to future national stockpiles, so there is a possibility that it can be widely applied to the spread and expansion of hydrogen, making this an invention with extremely high industrial applicability. [Explanation of symbols]
[0206] 1: Hydrogen station 3: Dehydrogenation unit 4: MCH tank 6: Toluene tank 9: Compressor 11: Pressure accumulator 15: Dispenser 17: Pre-cooler 23: Dehydrogenation reactor 25: Heat exchanger 26: Heat supply device 27:Storage tank 28: Catalytic combustion coil 28A: Fuel inlet 31: Gas-liquid separator 33:PSA device 37: Purge gas pump 39: Purge gas tank 41: Air supply pump 43: Connection part 45: Exhaust control valve L1: Raw material supply line L3: Toluene discharge line L5-L7: Hydrogen transport line L11: Filling hose L13: First refrigerant circulation line L21: Reaction product gas line L23: Heat transfer medium circulation line L25: Crude hydrogen transport line L31: Exhaust purge gas line L33: Purge gas supply line L37: Air supply line L37A: Split air supply line L38: Tank gas discharge line L38A: Branch line L39: Exhaust line L41: Second refrigerant circulation line
Claims
1. A hydrogen station, a dehydrogenation reactor for producing hydrogen by dehydrogenating hydrogenated aromatic compounds in the presence of a dehydrogenation catalyst; a heat supply device that supplies heat to the dehydrogenation reactor via a heat medium heated by using a fuel; a PSA apparatus for purifying the reaction product gas containing hydrogen produced by the dehydrogenation reactor using an adsorbent based on a pressure swing method; the PSA apparatus is supplied with a purge gas containing hydrogen used to regenerate the adsorbent; The heat supply device includes a storage tank that contains the heat medium, and a catalytic combustion tube that is disposed in the storage tank and performs catalytic combustion of the fuel in the presence of a combustion catalyst; a catalytic combustion tube that is supplied with the purge gas discharged from the PSA device together with air as the fuel, and the heat medium is heated by heat generated by the catalytic combustion of the fuel.
2. A hydrogen station as described in claim 1, wherein the heat transfer medium is heated only by the heat generated by the catalytic combustion.
3. The dehydrogenation catalyst comprises a platinum-supported alumina catalyst; The platinum-supported alumina catalyst is An alumina support; and platinum supported on the alumina support, The alumina support has a surface area of 200 m 2 / g or more, a pore volume of 0.50 m3 / g or more, an average pore diameter in the range of 60 Å to 150 Å, and a ratio of pores having an average pore diameter of ±30 Å to the total pore volume of 60% or more, The platinum particles are supported on the γ-alumina carrier in an amount of 0.1% by weight to 1.5% by weight as platinum element (Pt), 3. The hydrogen station according to claim 1, wherein 70% or more of the platinum particles have a size of 8 Å to 15 Å when directly observed using a transmission electron microscope.
4. 4. The hydrogen station according to claim 1, wherein the combustion catalyst includes a catalyst having the same configuration as the dehydrogenation catalyst.
5. 5. The hydrogen station according to claim 4, wherein the combustion catalyst includes a first catalyst which is filled in a fuel inlet portion of the catalytic combustion tube through which the fuel is introduced and has the same configuration as the dehydrogenation catalyst, and a second catalyst which has a different configuration from the first catalyst and is filled downstream of the fuel inlet portion of the catalytic combustion tube.
6. 6. The hydrogen station according to claim 1, wherein the heat medium is hot oil.
7. 7. The hydrogen station according to claim 1, wherein the air is divided and supplied to a plurality of different portions of the catalytic combustion tube.
8. a dispenser that supplies the hydrogen purified by the PSA device to a mobile body equipped with a fuel cell; A precooler that cools the hydrogen supplied from the dispenser with a refrigerant; A gas-liquid separator that separates the reaction product gas into gas and liquid, 8. The hydrogen station according to claim 1, wherein in the gas-liquid separator, the reaction product gas is cooled by the refrigerant supplied from the precooler.
9. In the dehydrogenation reaction, hydrogen and toluene are produced by dehydrogenating cyclohexane as the hydrogenated aromatic compound, a first tank containing the cyclohexane; and a second tank for containing the toluene, 9. The hydrogen station according to claim 1, wherein the first tank and the second tank are each disposed underground.
10. 10. The hydrogen station according to claim 9, wherein at least one of the gas phase gas in the first tank and the gas phase gas in the second tank is supplied to the catalytic combustion tube as the fuel together with the purge gas discharged from the PSA device.
11. 11. The hydrogen station according to claim 10, wherein at least one of the gas in the gas phase in the first tank and the gas in the gas phase in the second tank is introduced together with air into a fuel inlet port in the catalytic combustion tube through which the fuel is introduced.
12. 11. The hydrogen station according to claim 1, wherein the catalytic combustion tube is a coil filled with the combustion catalyst.
13. 9. The hydrogen station according to claim 1, wherein the hydrogenated aromatic compound is one or a mixture of two or more selected from the group consisting of hydrogenated monocyclic aromatic compounds, hydrogenated bicyclic aromatic compounds, and hydrogenated compounds having three or more aromatic rings.
14. 9. The hydrogen station according to claim 1, wherein the hydrogenated aromatic compound is one or a mixture of two or more selected from the group consisting of methylcyclohexane, cyclohexane, trimethylcyclohexane, and decalin.
15. A method for generating hydrogen at a hydrogen station, comprising the steps of: generating hydrogen by dehydrogenating aromatic compounds in the presence of a dehydrogenation catalyst; supplying heat to the dehydrogenation reaction via a heat transfer medium heated by using a fuel; Purifying a reaction product gas containing hydrogen produced by the dehydrogenation reaction using an adsorbent based on a pressure swing method; A purge gas containing hydrogen is used to regenerate the adsorbent; In the heating of the heat transfer medium, catalytic combustion of the fuel is performed in the presence of a combustion catalyst filled in a catalytic combustion tube; A method for generating hydrogen at a hydrogen station, wherein the purge gas used for regenerating the adsorbent is supplied to the catalytic combustion tube together with air as the fuel, and the heat medium is heated by heat generated by the catalytic combustion of the fuel.
Citation Information
Patent Citations
Fuel gas generation apparatus
JP2004277189A
Pure hydrogen production device
JP2004352511A
Hydrogen production system and hydrogen production method
JP2015182919A
Hydrogen production apparatus and hydrogen production method
JP2017065937A