Method for processing niobium-containing austenitic heat-resistant stainless steel bar
The method optimizes the hot working process of niobium-containing austenitic heat-resistant stainless steel bars by controlling heating and forging parameters, addressing cracking issues and improving thermoplasticity, resulting in high-quality bars with uniform grain size.
Patent Information
- Application Number
- JP2023525499
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-14
- Filing Date
- 2022-05-11
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-05-11
AI Technical Summary
Traditional methods for manufacturing niobium-containing austenitic heat-resistant stainless steel bars face challenges such as high Cr and Ni contents leading to niobide formation, reduced thermoplasticity, and susceptibility to cracking during hot working, especially with smaller rod specifications, resulting in low manufacturing efficiency and quality defects.
A method involving heating the steel ingot to 1200°C to 1270°C, followed by blooming rolling with radial forging for a total compression ratio greater than 3, heating the billet at 1200°C to 1270°C, and hot rolling with controlled surface temperatures and deformation rates to produce a stainless steel bar, optimizing process parameters to prevent cracking and improve thermoplasticity.
The method enhances production efficiency, avoids surface cracks, and improves the surface quality and texture of the stainless steel bars, enabling the production of high-quality niobium-containing austenitic heat-resistant stainless steel bars with uniform grain size.
Smart Images

Figure 0007573743000002 
Figure 0007573743000001
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to a patent application filed on July 14, 2021, entitled "Hot working method for niobium-containing high alloy austenitic heat-resistant stainless steel bar material" and bearing Chinese patent application number "202110795237.3", the entire contents of which are incorporated herein by reference.
[0002] (Technical field) The present invention relates to the field of processing of steel materials, and in particular to a method for hot working of niobium-containing high alloy austenitic heat-resistant stainless steel bar stock. [Background technology]
[0003] In order to improve power generation efficiency and reduce emissions, the steam temperature and pressure parameters of thermal power plants are constantly improving, and traditional materials cannot meet the requirements of unit boilers, among which the boiler superheater and reheater piping are the parts with the most severe military service environment, and it is necessary to use a large amount of high-performance niobium-containing austenitic heat-resistant stainless steel materials. The addition of Nb element can precipitate nano-sized MX and NbCrN during military service, and these precipitates can be well dispersed in the substrate, inhibiting dislocation motion, enhancing the precipitation strengthening effect and creep resistance, and improving the high temperature resistance of austenitic stainless steel. However, such materials also have high Cr and Ni contents, which makes it easy to form large blocky niobium oxides during the solidification process, which greatly reduces the thermoplasticity of the material and makes it extremely prone to cracking during hot processing.
[0004] In recent years, in order to reduce production costs, Chinese tube enterprises have begun to develop hot piercing processes instead of traditional hot extrusion processes, so that the specifications of raw bar material are becoming smaller and smaller, gradually dropping from the original φ180-250mm to φ65-130mm. Originally, the manufacturing process of such bar material is to directly radial forge the steel ingot in one heat. If the finished product is directly forged in the original process after the specifications become smaller, there are too many passes in the forging process, the temperature drops too much, and multi-heat forging is required, which results in low manufacturing efficiency. According to the initial blooming + hot rolling or initial blooming + forging manufacturing of ordinary stainless steel small-gauge bar material, the surface crack phenomenon is serious.
[0005] At present, there is an urgent need for a hot working method for niobium-containing high alloy austenitic heat-resistant stainless steel bar to solve the above problems. Summary of the Invention [Problem to be solved by the invention]
[0006] In view of the above problems, the present invention provides a method for hot working niobium-containing high alloy austenitic heat resistant stainless steel bar that overcomes or at least partially solves the above problems. [Means for solving the problem]
[0007] According to one aspect, the present invention provides a method for producing a method for manufacturing a semiconductor device comprising: A step (1) of heating a steel ingot, the heating temperature being 1200°C to 1270°C; (2) performing radial forging and blooming to obtain a billet such that the total compression ratio is greater than 3; A step (3) of heating the billet, the heating temperature being 1200°C to 1270°C; (4) performing hot rolling to obtain a bar material; A method for processing stainless steel bar stock is provided.
[0008] Optionally, in step (1), the incubation time is determined according to the following formula: T1 = 0.5D + 600 × w(Nb) × 100 Where: T1 is the heat retention time of the steel ingot, in minutes. D is the diameter of the steel block in millimeters. w(Nb) is the mass percent content of Nb.
[0009] Optionally, in step (2), the surface temperature of the initial forging is 1000°C to 1050°C, and the surface temperature of the forging process and final forging is 900°C to 950°C.
[0010] Optionally, in step (2), the forging process is performed in 4-10 passes, where the single pass deformation amount of the first and second passes is 4%-8%, and the forging frequency is 200-240 passes / min, and the single pass deformation amount of the subsequent passes is 15%-20%, and the forging frequency is 30-50 passes / min.
[0011] Optionally, in step (3), the incubation time is determined according to the following formula: T2 = 0.5L + 100 × w(Nb) × 100 Where: T2 is the billet warming time, in minutes. L is the side length of the billet in millimeters; w(Nb) is the mass percent content of Nb.
[0012] Optionally, in step (4), the surface temperature of the initial rolling is 1100°C to 1150°C, and the surface temperature of the rolling process and final rolling is 1000°C or higher.
[0013] Optionally, in step (4), the rolling process is carried out in 5-10 passes, the deformation amount in a single pass is 10%-15%, and the rolling speed is 1-1.2 m / s.
[0014] Optionally, the elemental composition of the stainless steel bar is: C 0.04%~0.10%, Si≦0.75%, Mn≦2.00%, P<0.03%, S<0.03%, Cr 24.0%~26.0%, Ni 17.0%~23.0%, Nb 0.20%~0.60%, N 0.15%~0.35%, and the balance Fe.
[0015] According to another aspect, the present invention provides a stainless steel bar produced by the above processing method. Effect of the Invention
[0016] Compared with the prior art, the method for processing stainless steel bars of the present invention has at least the following beneficial effects: The method for processing stainless steel bars of the present invention optimizes the process flow and controls key process parameters, thereby ensuring production efficiency, avoiding the occurrence of quality defects such as surface cracks, and producing niobium-containing high-alloy austenitic heat-resistant stainless steel bars with good surface quality and structure. The grain size of the bar structure was detected according to the standard test method for average grain size measurement of ASTM E112-2013, and the grain size was 3-7 grade, and the step difference was <2. [Brief description of the drawings]
[0017] [Figure 1] 1 shows the microstructure of a bar according to Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] In order to fully understand the objectives, features and effects of the present invention, the present invention will be described in detail with reference to the following specific embodiments. Except for the following content, the process method of the present invention adopts all other conventional methods or devices in the art. The following noun terms have the meanings commonly understood by those skilled in the art unless otherwise specified.
[0019] Regarding the technical difficulties encountered in the manufacturing process of small-gauge niobium-containing high-alloy austenitic heat-resistant stainless steel bar, the present inventors have deeply analyzed the hot working process and studied the process flow and key process parameters.
[0020] The elemental composition (wt%) of the target niobium-containing high alloy austenitic heat-resistant stainless steel is as follows: C 0.04%~0.10%, Si≦0.75%, Mn≦2.00%, P<0.03%, S<0.03%, Cr 24.0%~26.0%, Ni 17.0%~23.0%, Nb 0.20%~0.60%, N 0.15%~0.35%, the balance Fe and unavoidable impurities.
[0021] According to the inventor's research, the properties of this niobium-containing high alloy austenitic heat-resistant stainless steel bar are: (1) since the content of alloying elements is high, especially the N content, it has high resistance to thermal deformation, and its deformation resistance at 1100-1200°C is 1.5 to 2 times that of conventional austenitic stainless steel; (2) since it has a high Cr content and contains Nb, when the alloy solidifies, large lump niobium compounds are likely to be formed in areas where the Nb element is unevenly distributed, which leads to localized deterioration of forming and causes localized cracks.
[0022] Based on the above research, the inventor further considered that in the design of the process flow, this stainless steel material has very poor thermoplasticity in the form of as-cast structure, so if blooming is adopted, the metal in the rolling direction will be deformed by tensile stress, the deformation conditions are poor, and the plasticity of the metal cannot be fully exerted, which will cause surface cracks. Therefore, the radial forging process is selected to carry out blooming, and the metal is mainly subjected to compressive stress during the deformation process, which has good plasticity. After forging, the thermoplasticity is greatly improved after forming the deformation recrystallization structure, and the rolling process is used to form the material in order to improve the manufacturing efficiency. Therefore, the deformation is manufactured by the process of "radial forging blooming + rolling to make material".
[0023] Based on the findings and process concepts of the above studies, the present inventors propose a hot working method for niobium-containing high alloy austenitic heat-resistant stainless steel bars, the overall process of which is as follows: ingot → heating → radial forging billet → surface inspection and thinning → heating → hot rolling → straightening → verification.
[0024] Specifically, the method for processing a stainless steel bar of the present invention includes the following steps (1) to (4).
[0025] (1) Heating the steel ingot The steel ingot is heated to a heating temperature of 1200°C to 1270°C, for example, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C, 1250°C, 1260°C, or 1270°C, and the heat-retention time is determined according to the following formula: T1 = 0.5D + 600 × w(Nb) × 100 Where: T1 is the heat retention time of the steel ingot, in minutes. D is the diameter of the steel block in millimeters. w(Nb) is the mass percent content of Nb. The inventor analyzed the phase diagram of the above-mentioned niobium-containing high alloy austenitic heat-resistant stainless steel and supplemented experimental observations. As a result, when this stainless steel material is heated to 1270°C or higher, a low melting point eutectic phase of niobium appears, and the NbC phase begins to precipitate at 1200°C or lower. However, due to uneven distribution of Nb element during solidification, the NbC phase precipitated in the steel ingot often exhibits a large block shape. Therefore, by selecting a target heating temperature of 1200 to 1270°C, the inventor can prevent the influence of NbC precipitation on thermoplasticity and avoid the occurrence of a low melting point eutectic phase at high temperatures. In addition, according to the inventor's research, in the conventional heating system, the warming time after the temperature rises is usually 0.5 to 0.8 min / mm depending on the diameter D of the steel ingot, and although the heat transmission of the steel ingot is ensured within this time, NbC cannot be dissolved. In order to eliminate large agglomerated NbC as much as possible, it is necessary to appropriately lengthen the warming time, but if the warming time is too long, the crystal grains become too coarse and grain boundary cracks are likely to occur. Therefore, the inventor proposes to determine the warming time of the steel ingot using the above formula, which can eliminate large agglomerated NbC as much as possible and avoid the crystal grains becoming too coarse and the formation of grain boundary cracks.
[0026] (2) Radial forging and blooming The heated steel ingot is then subjected to radial forging to be bloomed, and the total compression ratio of the entire radial forging process must be greater than 3 to ensure that the as-cast structure of the steel ingot is crushed. The surface temperature during the initial forging is controlled to 1000-1050°C, for example, 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, or 1050°C, and the surface temperature during the forging process and final forging is controlled to 900-950°C, for example, 900°C, 910°C, 920°C, 930°C, 940°C, or 950°C, to prevent grain growth after dynamic recrystallization at a low temperature and ensure a fine crystal structure on the surface. Forging is performed in 4-10 passes, for example, 4 passes, 5 passes, 6 passes, 7 passes, 8 passes, 9 passes or 10 passes. The first two passes are high-frequency forging with a small deformation amount, the deformation amount of a single pass is 4-8%, for example, 4%, 5%, 6%, 7% or 8%, and the forging frequency is 200-240 times / min, for example, 200 times / min, 210 times / min, 220 times / min, 230 times / min or 240 times / min. This allows the as-cast structure on the surface to be rapidly fractured with a small strain, making the surface into a uniform and fine grain recrystallized structure, forming a surface hardened layer, and preventing cracks due to poor plasticity of the slab during the blooming process. The subsequent passes adopt low-frequency forging with large deformation, and in the state of low strain rate and large deformation, the recrystallization in the deformation process of the center is fully ensured, and the structure of the center is improved; the deformation amount of a single pass is 15-20%, for example, 15%, 16%, 17%, 18%, 19% or 20%, and the forging frequency is 30-50 times / min, for example, 30 times / min, 31 times / min, 32 times / min, 33 times / min, 34 times / min, 35 times / min, 36 times / min, 37 times / min, 38 times / min, 39 times / min, 40 times / min, 41 times / min, 42 times / min, 43 times / min, 44 times / min, 45 times / min, 46 times / min, 47 times / min, 48 times / min, 49 times / min or 50 times / min. The final product is a billet.
[0027] (3) Heating the billet The billet is heated to a heating temperature of 1200°C to 1270°C, for example, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C, 1250°C, 1260°C, or 1270°C. The heat-retention time is determined according to the following formula: T2 = 0.5L + 100 × w(Nb) × 100 Where: T2 is the billet warming time, in minutes. L is the side length of the billet in millimeters; w(Nb) is the mass percent content of Nb. In this formula, 0.5L is the minimum time for the billet to be uniformly sintered, and the warming time after the temperature rises is usually 0.5-0.8min / mm depending on the diameter D of the steel ingot. In the present invention, the time is extended to 1.0min / mm to ensure the effect. In actual production, considering that the billet of the heated batch is stacked in three-sided heating, one of which is at the bottom of the furnace, according to the inventor's research, the time is taken into consideration at half the side length, and 0.5mm is adopted as the coefficient to ensure that the inside and outside temperature of the billet after heating is uniform and reaches within 10°C. In order to maximize the dissolution of NbC, 100×w(Nb)×100 is the minimum warming time to be increased, which maximizes the dissolution of NbC, reduces the segregation of other alloy elements, and enhances the natural plasticity of the material.
[0028] (4) Hot rolling In the forging process of step (2), the as-cast structure is fractured, so the hot rolling process is mainly controlled to prevent the surface from cracking. The surface temperature of the initial rolling is controlled to 1100-1150°C (for example, 1100°C, 1110°C, 1120°C, 1130°C, 1140°C or 1150°C, etc.). This stainless steel material has a rapid decrease in thermoplasticity below 1000°C, and if there is tensile stress in the rolling process, the rolling is more likely to crack, so the surface temperature of the rolling process and final rolling is controlled to above 1000°C to ensure that the temperature range is in the optimal thermoplastic region. According to the specifications of the finished product, the rolling is performed in 5 to 10 passes, for example, 5 passes, 6 passes, 7 passes, 8 passes, 9 passes or 10 passes, the deformation amount in a single pass is 10 to 15%, for example, 10%, 11%, 12%, 13%, 14% or 15%, and the rolling speed is 1 to 1.2 m / s, for example, 1 m / s, 1.1 m / s or 1.2 m / s. Subsequent correction and verification can be performed in the usual manner, which will not be described here. The hot rolling step is mainly a forming process, that is, in the manufacturing process, the stainless steel material is made into a product of the desired specifications within the deformation temperature range (optimum deformation temperature range) to prevent the generation of scrap due to hot rolling cracks.
[0029] (Example) The present invention will be further described below with reference to examples, but the present invention is not limited to the scope of these examples. In the following examples, experimental methods for which specific conditions are not specified are selected based on conventional methods and conditions or product instructions.
[0030] Example 1 The elemental composition of the stainless steel of this example is 0.05% C, 0.23% Si, 0.78% Mn, 0.021% P, 0.001% S, 25.1% Cr, 21.2% Ni, 0.5% Nb, 0.26% N, and the balance Fe.
[0031] The steel ingot has a diameter of 600 mm, and the target bar has a diameter of 140 mm. The overall process is as follows: steel ingot → heating → billet by radial forging → surface inspection and thinning → heating → hot rolling → straightening → verification. Specifically, the process is as follows: 1. Heating the steel ingot: the target temperature is 1230℃, and the heat retention time is 600min. 2. Blooming and rolling by forging: the initial forging temperature is 1030℃, 9 passes are performed, the first 2 passes have a single pass deformation of 6%, the forging frequency is 210 times / min, the last 7 passes have a single pass deformation of 16%, the forging frequency is 45 times / min. The final forging temperature is 920℃, and the billet size is 271×271mm. 3. Heating the billet: the heating temperature is 1250℃, and the heat retention time is 185min. 4. Hot rolling: the surface temperature of the initial rolling is 1120℃, the surface temperature of the final rolling is 1050℃, the rolling is carried out in 8 passes, the single-pass deformation amount of the first 4 passes is 13%, and the single-pass deformation amount of the last 4 passes is 11%, and the rolling speed is 1m / s. The microstructure of the obtained bar is shown in Figure 1. As can be seen from Figure 1, the bar has a good structure and a uniform grain size.
[0032] Example 2 The Nb content of the steel grade is 0.4%, the steel ingot size is Φ500mm, and the target bar size is Φ140mm. The overall process is as follows: ingot → heating → billet by radial forging → surface inspection and thinning → heating → hot rolling → straightening → verification. Specifically, it is as follows: 1. Heating the steel ingot: the target temperature is 1230℃, and the heat retention time is 490min. 2. Blooming and rolling by forging: the initial forging temperature is 1040℃, 9 passes are performed, the first 2 passes have a single pass deformation of 7%, the forging frequency is 215 times / min, the last 7 passes have a single pass deformation of 20%, the forging frequency is 50 times / min. The final forging temperature is 930℃, and the billet size is 220×220mm. 3. Heating the billet: the heating temperature is 1260℃, and the heat retention time is 150min. 4. Hot rolling: the surface temperature of the initial rolling is 1130℃, the surface temperature of the final rolling is 1030℃, the rolling is carried out in 7 passes, the single-pass deformation amount of the first 5 passes is 15%, the single-pass deformation amount of the last 2 passes is 13%, and the rolling speed is 1.1m / s.
[0033] Testing the effectiveness According to the standard test method for measuring average grain size of ASTM E112-2013, the grain size of the bars obtained in Examples 1 and 2 was detected, and the results are as follows:
[0034] [Table 1]
[0035] The above examples are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above examples. Any other alternatives, modifications, combinations, changes, simplifications, etc. that do not deviate from the spirit and principles of the present invention are all equivalent replacement methods and fall within the protection scope of the present invention.
[0036] (Additional Note) (Appendix 1) A method for processing stainless steel bars, comprising the steps of: A step (1) of heating a steel ingot, the heating temperature being 1200°C to 1270°C; (2) performing radial forging and blooming to obtain a billet such that the total compression ratio is greater than 3; A step (3) of heating the billet, the heating temperature being 1200°C to 1270°C; (4) performing hot rolling to obtain a bar material; A method for processing stainless steel bar material, comprising:
[0037] (Appendix 2) In step (1), the incubation time is determined according to the following formula: T1 = 0.5D + 600 × w(Nb) × 100 Where: T1 is the heat retention time of the steel ingot, in minutes. D is the diameter of the steel block in millimeters. w(Nb) is the mass% content of Nb; 2. A method for processing a stainless steel bar as described in claim 1.
[0038] (Appendix 3) In step (2), the surface temperature of the initial forging is 1000°C to 1050°C, and the surface temperature of the forging process and final forging is 900°C to 950°C; 2. A method for processing a stainless steel bar as described in claim 1.
[0039] (Appendix 4) In step (2), the forging process is carried out in 4-10 passes, where the single pass deformation amount of the first and second passes is 4%-8%, and the forging frequency is 200-240 times / min, and the single pass deformation amount of the subsequent passes is 15%-20%, and the forging frequency is 30-50 times / min; 2. A method for processing a stainless steel bar as described in claim 1.
[0040] (Appendix 5) In step (3), the incubation time is determined according to the following formula: T2 = 0.5L + 100 × w(Nb) × 100 Where: T2 is the billet warming time, in minutes. L is the side length of the billet in millimeters; w(Nb) is the mass% content of Nb; 2. A method for processing a stainless steel bar as described in claim 1.
[0041] (Appendix 6) In step (4), the surface temperature of the initial rolling is 1100°C to 1150°C, and the surface temperature of the rolling process and final rolling is above 1000°C; 2. A method for processing a stainless steel bar as described in claim 1.
[0042] (Appendix 7) In step (4), the rolling process is carried out in 5-10 passes, the deformation amount of a single pass is 10%-15%, and the rolling speed is 1-1.2 m / s; 2. A method for processing a stainless steel bar as described in claim 1.
[0043] (Appendix 8) The elemental composition of the stainless steel bar is: C 0.04%~0.10%, Si≦0.75%, Mn≦2.00%, P<0.03%, S<0.03%, Cr 24.0%~26.0%, Ni 17.0%~23.0%, Nb 0.20%~0.60%, N 0.15%~0.35%, and the balance Fe. 2. A method for processing a stainless steel bar as described in claim 1.
[0044] (Appendix 9) Produced by the processing method according to any one of appendix 1 to 8, 1. A stainless steel bar material comprising:
Claims
1. A method for processing a niobium-containing austenitic heat-resistant stainless steel bar, comprising the steps of: A step (1) of heating the steel ingot, the heating temperature being 1200°C to 1270°C; (2) performing radial forging and blooming to obtain a billet so that the total compression ratio is greater than 3; A step (3) of heating the billet, the heating temperature being between 1200°C and 1270°C; (4) performing hot rolling to obtain a bar stock, In step (1), the warming time is determined according to the following formula: T1=0.5D+600×w(Nb)×100 Where: T1 is the warming time of the steel ingot, in minutes. D is the diameter of the steel ingot in millimeters; w(Nb) is the mass% content of Nb, In step (3), the warming time is determined according to the following formula: T2=0.5L+100×w(Nb)×100 Where: T2 is the billet warming time, in minutes; L is the side length of the billet in millimeters; w (Nb) is the mass% content of Nb; 2. A method for processing a niobium-containing austenitic heat-resistant stainless steel bar material, comprising the steps of:
2. In step (2), the surface temperature of the initial forging is 1000°C to 1050°C, and the surface temperature of the forging process and final forging is 900°C to 950°C; 2. The method for processing a niobium-containing austenitic heat-resistant stainless steel bar according to claim 1.
3. In step (2), the forging process is carried out in 4-10 passes, where the single pass deformation amount of the first and second passes is 4%-8%, and the forging frequency is 200-240 times / min, and the single pass deformation amount of the subsequent passes is 15%-20%, and the forging frequency is 30-50 times / min; 2. The method for processing a niobium-containing austenitic heat-resistant stainless steel bar according to claim 1.
4. In step (4), the surface temperature of the initial rolling is 1100°C to 1150°C, and the surface temperature of the rolling process and final rolling is 1000°C or higher; 2. The method for processing a niobium-containing austenitic heat-resistant stainless steel bar according to claim 1.
5. In step (4), the rolling process is carried out in 5-10 passes, the deformation amount of a single pass is 10%-15%, and the rolling speed is 1-1.2 m / s; 2. The method for processing a niobium-containing austenitic heat-resistant stainless steel bar according to claim 1.
6. The elemental composition of the stainless steel bar is: C 0.04% to 0.10%, Si≦0.75%, Mn≦2.00%, P<0.03%, S<0.03%, Cr 24.0% to 26.0%, Ni 17.0% to 23.0%, Nb 0.20% to 0.60%, N 0.15% to 0.35%, and the balance Fe.
2. The method for processing a niobium-containing austenitic heat-resistant stainless steel bar according to claim 1.
Citation Information
Patent Citations
Preparation method of micro / nano-structure ultrahigh-strength plastic stainless steel containing Nb
CN102994905A
Austenite heat-resistance stainless steel resisting high temperature oxidation
CN103741065A
Manufacturing method of stainless steel large forging for thermonuclear fusion reactor
CN104174796A
Hot rolling technique for heat-resistant niobium-contained austenitic stainless steel
CN105648360A
Forging method of tungsten austenite-containing heat-resisting steel tube blank
CN106623711A