Metallic gloss prints
The printed matter with a metallic luster layer and surface protective layer, optimized for specular reflection, addresses the issue of reduced brightness by enhancing light reflection intensity and maintaining uniform appearance.
Patent Information
- Application Number
- JP2020169875
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-10-07
AI Technical Summary
Existing printed materials with metallic luster layers have reduced brightness when viewed from the specular reflection direction due to high anti-glare properties, resulting in uniform light intensity across different viewing angles.
A printed matter with a metallic luster layer and a surface protective layer, featuring specific roughness values and an anchor coat layer, configured to enhance light reflection intensity in the specular direction by controlling surface roughness and incorporating metal scales and a resin binder.
The solution achieves high brightness when observed from the specular reflection direction by optimizing surface roughness and layer configurations, enhancing the sense of brightness and maintaining uniform appearance across angles.
Smart Images

Figure 0007574601000002 
Figure 0007574601000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a printed matter having a metallic luster layer containing metal flakes. [Background technology]
[0002] Such a printed matter is described, for example, in US Pat. No. 5,399,633.
[0003] However, this print has high anti-glare properties, and therefore the light reflection intensity in the regular reflection direction is reduced while the light reflection intensity in other reflective and diffuse directions is increased to provide a uniform light intensity overall. Therefore, even when observed from the regular reflection direction, the perceived brightness is low. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-88095 A Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, an object of the present invention is to provide a printed matter having a metallic luster layer containing metal flakes, which has a high sense of brilliance when observed from a specular reflection direction. [Means for solving the problem]
[0006] That is, the invention described in claim 1 is a printed matter comprising a substrate on which a metallic luster layer containing metallic flakes is provided, and a surface protective layer is provided on the outermost surface of the metallic luster layer side, and the surface of the surface protective layer has an arithmetic mean roughness (Ra 0.08 ) and the arithmetic mean roughness (Ra 0.25) and the arithmetic mean roughness (Ra 0.8 ) and the value of X calculated according to the following formula (1) is in the range of 2.0 to 4.0. Located in Ra 0.08 is 0.10μm or more The metallic gloss printed matter is characterized by the above.
[0007] X=(Ra 0.8 -Ra 0.25 ) / (Ra 0.25 -Ra 0.08 ) (1) The invention described in claim 2 is the metallic gloss printed matter described in claim 1, characterized in that an anchor coat layer having a thickness of 1.0 to 3.0 μm is provided between the substrate and the metallic gloss layer. Effect of the Invention
[0008] According to the present invention, even though the printed matter has a metallic gloss layer containing metal flakes, the light reflection intensity in the direction of regular reflection is high, and therefore, when observed from this direction, a high sense of brightness can be observed. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view of a specific example of a metallic gloss printed matter of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, specific examples of the present invention will be described with reference to the accompanying drawings, in which: Fig. 1 is a cross-sectional view of a specific example of a metallic gloss printed matter of the present invention.
[0011] As can be seen from FIG. 1, the present invention provides a metallic luster layer 13 containing metallic flakes on a substrate 11. and a surface protective layer 14 is provided on the outermost surface on the side having the metallic gloss layer. In this example, an anchor coat layer 12 is provided between the substrate 11 and the metallic gloss layer 13. Another layer may be provided between the metallic gloss layer 13 and the surface protective layer 14, but it is necessary that the metallic gloss layer 13 can be seen through when the printed matter 10 is observed from the surface protective layer 14 side. An example of a layer provided between the metallic gloss layer 13 and the surface protective layer 14 is a partially printed picture print layer.
[0012] In the printed matter of the present invention, the value of X calculated on the surface of the surface protective layer 14 according to the following formula (1) is in the range of 2.0 to 4.0.
[0013] X=(Ra 0.8 -Ra 0.25 ) / (Ra 0.25 -Ra 0.08 ) (1) Here, Ra 0.8 means the arithmetic mean roughness of the surface of the surface protection layer when the cutoff value is 0.08 mm. Arithmetic mean roughness Ra 0.8 was measured according to JIS B0601:2001. Similarly, Ra 0.25 means the arithmetic mean roughness of the surface of the surface protection layer when the cutoff value is 0.25 mm. 0.08 means the arithmetic mean roughness of the surface of the surface protection layer when the cutoff value is set to 0.8 mm.
[0014] The cutoff value is a value indicating the degree to which the waviness component (low frequency component) is cut from a cross-sectional curve composed of a roughness component (high frequency component) and a waviness component (low frequency component). In other words, the cutoff value is a value indicating the fineness of a filter that cuts the waviness component (low frequency component). More specifically, when the cutoff value is large, the filter is coarse, so large waviness (low frequency component) among the waviness components is cut, but small waviness is not cut. In other words, when the cutoff value is large, the value includes the waviness component (low frequency component). On the other hand, when the cutoff value is small, the filter is fine, so most of the waviness component (low frequency component) is cut. In other words, when the cutoff value is small, the value includes almost no waviness component (low frequency component) and accurately reflects the roughness component (high frequency component).
[0015] Therefore, if the cutoff value is set to 0.08 mm, both the low frequency component and the mid frequency component are cut off as waviness, so the measured Ra 0.08 Reflects high frequency components.
[0016] In addition, if the cutoff value is set to 0.25 mm, the low frequency components are cut off as waviness, so the measured Ra 0.25 reflects both mid-frequency and high-frequency components.
[0017] In addition, when the cutoff value is set to 0.8 mm, the lower frequency components are cut off as swells, but the relatively low frequency components, mid frequency components and high frequency components are cut off as swells. 0.8 This is reflected in
[0018] Therefore, the numerator (Ra 0.8 -Ra 0.25 ) is a value that reflects relatively low-frequency components. On the other hand, the denominator (Ra 0.25 -Ra 0.08 ) is a value reflecting the mid-frequency component. Therefore, the value of X calculated according to formula (1) means the ratio of the value reflecting the relatively low-frequency component to the value reflecting the mid-frequency component among the irregularities on the surface of the surface protection layer 14.
[0019] The reflected light in the regular reflection direction is generated by the relatively low frequency components of the surface irregularities of the surface protective layer 14, and the scattered reflected light that is scattered to the surroundings is generated by the mid- and high-frequency components of the irregularities, so a large value of X means that the light reflection intensity in the regular reflection direction is high. Therefore, when observed from this regular reflection direction, a high sense of brightness can be observed.
[0020] As described later, the surface of the metallic luster layer 13 is also measured using an arithmetic mean roughness Ra with a cutoff value of 0.08 mm. 0.08 , arithmetic mean roughness Ra with a cutoff value of 0.25 mm 0.25 , arithmetic mean roughness Ra with a cutoff value of 0.8 mm 0.8 And these Ra 0.08 ,Ra 0.25 ,Ra 0.8 Considering the numerical value X calculated according to formula (1) from the above, the metallic gloss layer 13 is formed so that the numerical value X is in the range of 2.0 to 4.0, and then the surface protective layer 14 is formed so as to follow the surface irregularities of the metallic gloss layer 13, whereby it is possible to configure the surface of the surface protective layer 14 so that the value of X is also in the range of 2.0 to 4.0.
[0021] Incidentally, paper or a plastic film can be used as the substrate 11. Examples of paper include fine paper, medium-quality paper, coated paper, synthetic paper, impregnated paper, laminated paper, coated paper for printing, coated paper for recording, etc. Examples of plastic films include polyester film, polypropylene film, polystyrene film, nylon film, polycarbonate film, polyacrylonitrile film, polyimide film, etc. Furthermore, a multilayer film in which films or papers of these various materials are laminated may be used, and further, a film provided with a vapor deposition layer or a printing layer may be used as the substrate film.
[0022] Next, the light reflection intensity in the regular reflection direction can be increased by interposing an anchor coat layer 12 between the substrate 11 and the metallic luster layer 13. For this purpose, it is preferable that the anchor coat layer 12 has a thickness of 1.0 to 3.0 μm. As can be seen from a comparison between the examples and comparative examples described later, if the anchor coat layer 12 is thicker than this, the value X represented by formula (1) becomes smaller, and therefore the light reflection intensity in the regular reflection direction cannot be increased.
[0023] The anchor coat layer 12 can be formed by applying an ionizing radiation curable resin composition and curing it by irradiating it with ionizing radiation.
[0024] The ionizing radiation curable resin composition is a composition containing a compound having an ionizing radiation curable functional group (hereinafter, also referred to as "ionizing radiation curable compound"). Examples of the ionizing radiation curable functional group include ethylenically unsaturated bond groups such as (meth)acryloyl group, vinyl group, and allyl group, as well as epoxy group, oxetanyl group, and the like. As the ionizing radiation curable compound, a compound having an ethylenically unsaturated bond group is preferred, a compound having two or more ethylenically unsaturated bond groups is more preferred, and among them, a polyfunctional (meth)acrylate-based compound having two or more ethylenically unsaturated bond groups is even more preferred. As the polyfunctional (meth)acrylate-based compound, both a monomer and an oligomer can be used, but a monomer is preferred from the viewpoint of improving scratch prevention and penetration prevention due to high crosslinking density.
[0025] Here, ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules. Usually, ultraviolet rays (UV) or electron beams (EB) are used, but other types of radiation, such as electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion beams, can also be used.
[0026] When the ionizing radiation curable compound is an ultraviolet ray curable compound, the ionizing radiation curable composition (ultraviolet ray curable resin composition) preferably contains a photopolymerization initiator, such as cetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl methyl ketal, benzoyl benzoate, α-acyloxime ester, or thioxanthones.
[0027] Next, the metallic luster layer 13 can be formed by mixing metal flakes, a resin binder and other additives in a solvent to prepare a paint, and then applying the paint.
[0028] Examples of materials for the metal flakes include metals and alloys such as aluminum, gold, silver, brass, titanium, chromium, nickel, nickel chromium, and stainless steel.
[0029] The average length of the metal flakes is preferably 5.0 to 30 μm, and more preferably 8.0 to 20 μm, and the average thickness of the metal flakes is preferably 0.10 μm or less, and more preferably 0.08 μm or less.
[0030] Such metal flakes can be produced, for example, by peeling off a thin metal film formed by vacuum-depositing the metal or alloy on a plastic film from the plastic film, and then crushing and stirring the peeled thin metal film.
[0031] Examples of the resin binder include thermoplastic resins and thermosetting resins such as polyester resin, urethane resin, epoxy resin, melamine resin, alkyd resin, phenol resin, acrylic resin, cellulose resin, etc. Furthermore, a cured product of an ultraviolet-curable resin composition may be used as the resin binder.
[0032] The compounding ratio of the resin binder to the metal flakes is preferably 55:45 to 30:70, more preferably 50:50 to 35:65, in terms of solid mass ratio. By making the ratio of metal flakes 45 or more to resin binder 55, it becomes easier to obtain a sufficient metallic luster, and by making the ratio of metal flakes 70 or less to resin binder 30, it becomes easier to improve the printability of the metallic luster layer and the processability of the printed matter.
[0033] Examples of other additives include colorants such as titanium oxide, zinc oxide, carbon black, iron oxide, iron yellow, ultramarine blue, metallic pigments, pearl pigments, etc. In addition, additives such as defoamers and thickeners can be added in the usual manner.
[0034] As the solvent, ethanol, isopropyl alcohol, ethyl acetate, normal propyl acetate, etc. can be used.
[0035] The thickness of the metallic luster layer 13 is preferably 0.15 to 1.5 μm, and more preferably 0.20 to 1.0 μm.
[0036] As the coating method, for example, a known coating method such as a gravure coating method, a roll coating method, a die coating method, etc. can be used.
[0037] The surface unevenness of the metallic gloss layer 13 thus formed is desirably configured so that the numerical value X is in the range of 2.0 to 4.0. By forming a surface protective layer 14 on the metallic gloss layer 13, which conforms to the surface unevenness of the metallic gloss layer 13, the surface unevenness of the surface protective layer 14 is also configured so that the value of X calculated according to formula (1) is in the range of 2.0 to 4.0.
[0038] Next, the surface protective layer 14 is located on the outermost surface of the printed matter 10, and improves its scratch resistance and weather resistance. In addition, the unevenness of the surface of the surface protective layer 14 controls the reflection direction of light incident on the printed matter 10, and increases the light reflection intensity in the regular reflection direction. Therefore, as described above, by forming the surface protective layer 14 following the metallic gloss layer 13 having surface unevenness with a numerical value X in the range of 2.0 to 4.0, the value of X on the surface can also be in the range of 2.0 to 4.0.
[0039] The surface protection layer 14 is formed by applying a thermoplastic resin, a thermosetting resin, or an ultraviolet-curing resin. The insulating layer can be formed by carrying out a necessary drying treatment, heat curing treatment, or ultraviolet ray irradiation treatment.
[0040] Examples of the thermoplastic resin or thermosetting resin that can be used include acrylic resin, urethane resin, polyester resin, etc. Examples of the ultraviolet-curable resin that can be used include a monomer having an ethylenically unsaturated bond group such as a (meth)acryloyl group, a vinyl group, or an allyl group, and an additive such as a photopolymerization initiator or a photopolymerization accelerator is added to the monomer.
[0041] The surface protective layer 14 can be applied by a known application method such as gravure coating, roll coating, or die coating. EXAMPLES
[0042] Example 1 Paper was used as the substrate 11, and an anchor coat layer 12, a metallic luster layer 13, and a surface protective layer 14 were applied thereon in this order to produce a metallic luster printed matter 10. The thickness of the anchor coat layer 12 was 2.2 μm. The Ra of the surface of the surface protective layer of this printed matter 10 was 0.8 is 0.39, Ra 0.25 is 0.18, Ra 0.08 was 0.10 and the value of X was 2.63.
[0043] (Examples 2 to 3, Comparative Examples 1 to 4) Metallic gloss printed matter 10 was produced in the same manner as in Example 1, except that the thickness of the anchor coat layer 12 was changed. The thickness of the anchor coat layer 12 of these metallic gloss printed matter 10 and the Ra of the surface of the surface protective layer were 0.8 , Ra 0.25 , Ra 0.08 and the values of X are shown in Table 1.
[0044] [Table 1]
[0045] When the printed matter of Examples 1 to 3 and Comparative Examples 1 to 4 was picked up and observed from various angles, the printed matter of Comparative Examples 1 to 4 did not change in brilliance even when the observation angle was changed, and showed a uniform and stable metallic luster from any angle, whereas the printed matter of Examples 1 to 3 changed in brilliance depending on the observation angle. When observed from the direction of regular reflection, a metallic luster with a particularly strong brilliance was observed. [Explanation of symbols]
[0046] 10: Metallic gloss printed matter 11: Substrate 12: Anchor coat layer 13: Metallic gloss layer 14: Surface protective layer
Claims
1. A printed matter comprising a substrate having a metallic luster layer containing metallic flakes and a surface protective layer on the outermost surface of the metallic luster layer side, the surface of the surface protective layer having a cutoff value of 0.08 mm and a surface roughness of JIS B0601:2001 (Ra 0.08 ) and the arithmetic average roughness (Ra 0.25 ) and the arithmetic average roughness (Ra 0.8 ) and the value of X calculated according to the following formula (1) is in the range of 2.0 to 4.0, The Ra0.08 is 0.10 μm or more; Metallic gloss print. X=(Ra 0.8 -Ra 0.25 ) / (Ra 0.25 -Ra 0.08 ) (1)
2. The Ra 0.8 is 0.47 μm or more, The metallic gloss printed matter according to claim 1.
3. The Ra 0.25 is 0.21 μm or more.
3. The metallic gloss printed matter according to claim 1 or 2.
4. 2. The metallic gloss printed matter according to claim 1, further comprising an anchor coat layer having a thickness of 1.0 to 3.0 μm between the substrate and the metallic gloss layer.
Citation Information
Patent Citations
Magnetic card
JP1992270682A
Decorative sheet, decorative material, and method for producing decorative sheet
JP2016068344A
Printed matter, container using the printed matter, manufacturing method of printed matter and selection method of printed matter
JP2016088095A
Printed matter and container using the same
JP2019018445A
Printed matter and container using the printed matter
JP2020011515A