Laminated Film
A laminated film with a polybutylene terephthalate base layer, oxazoline-containing covering layer, and silicon-aluminum oxide composite inorganic layer addresses the challenge of maintaining barrier and toughness in high-temperature, high-humidity environments, ensuring durability and preventing content leakage.
Patent Information
- Application Number
- JP2020565153
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-10
- Filing Date
- 2020-01-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-01-07
AI Technical Summary
Existing laminated films fail to maintain excellent barrier properties, adhesive properties, and toughness in high-temperature, high-humidity environments, particularly during severe moist heat treatments like boiling, due to issues such as peeling, cracking, and reduced gas barrier performance.
A laminated film composed of at least three layers: a base layer made of 70% polybutylene terephthalate resin, a covering layer with a resin containing an oxazoline group, and an inorganic thin film layer of silicon oxide and aluminum oxide composite, with specific orientation and adhesion properties to ensure durability and gas barrier performance.
The laminated film maintains excellent barrier and adhesive properties under harsh conditions, preventing content deterioration and leakage, while offering high toughness and ease of processing, thus ensuring economic efficiency and production stability.
Smart Images

Figure 0007574646000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate used in the field of packaging food, medicine, industrial products, etc. More specifically, the present invention relates to a gas barrier laminate that is excellent in gas barrier property, dimensional stability, processability, and bag rupture resistance, and has excellent gas barrier property even in applications requiring storage or transportation in high-temperature and high-humidity environments or applications involving severe moist heat treatment such as boiling sterilization. [Background technology]
[0002] Packaging materials used for food, medicines, etc. are required to have gas barrier properties, that is, properties that block gases such as oxygen and water vapor, in order to inhibit oxidation of proteins and fats and oils, maintain flavor and freshness, and maintain the efficacy of medicines. In addition, gas barrier materials used in electronic devices and electronic components such as solar cells and organic electroluminescence (EL) devices require higher gas barrier properties than packaging materials for food, etc.
[0003] Conventionally, in food applications that require blocking various gases such as water vapor and oxygen, gas barrier laminates have been generally used in which a thin metal film made of aluminum or an inorganic thin film made of an inorganic oxide such as silicon oxide or aluminum oxide is formed on the surface of a base film made of plastic. Among these, those formed with a thin film (inorganic thin film layer) of an inorganic oxide such as silicon oxide, aluminum oxide, or a mixture thereof are widely used because they are transparent and allow the contents to be confirmed.
[0004] Transparent inorganic thin barrier films are being used in various situations due to their convenience and performance, and the quality required is also becoming higher. For example, there is a demand for high barrier properties to be maintained even in harsh environments, such as long-term transportation in hot and humid environments (e.g., export to overseas) and warehouse storage in hot and humid climates such as Japan. There is also a demand for barrier films that can withstand harsh sterilization treatments such as boiling and retorting, which are used to extend the expiration date of food packaging contents.
[0005] Among sterilization applications, boiling pouches in particular are subject to a large external load because the pressure of the contents increases during boiling sterilization. Therefore, in addition to sufficient water resistance, heat resistance, and gas barrier properties, high toughness (bag breakage resistance and puncture resistance) is also required. For these required performances, a laminated film in which a gas barrier layer is laminated on a general polyester film has excellent barrier performance, heat resistance, and processability, but has a problem of insufficient toughness. On the other hand, a conventional technology of laminating a gas barrier layer on a polyamide film has also been proposed (for example, Patent Document 1). This allows the production of a film that combines the toughness and barrier properties of a polyamide film. However, gas barrier laminated films using polyamide film as a base material have problems such as poor adhesion in a humid and hot environment due to the characteristics of the polyamide film, and the barrier properties may be significantly deteriorated due to expansion and contraction caused by moisture absorption of the polyamide film base material, making it difficult to use in the above-mentioned harsh environment. In addition, polyamide films are inferior in terms of heat resistance to polyester films, and there are also processing problems such as a tendency for heat shrinkage wrinkles to occur during coating and drying.
[0006] In response to this, a technology has been proposed in which a packaging material for boiling or retort treatment that is inexpensive and has low elution properties and excellent transparency can be obtained by biaxially stretching a multilayer film having a polyester-based resin layer and a polyamide-based resin layer, and using the layer having a biaxially oriented multilayer film as the base layer of a transparent gas barrier film (e.g., Patent Document 2). However, this conventional technology has the problem that peeling is likely to occur at the interface between the polyester-based resin layer and the polyamide-based resin layer, leading to the bag breaking when dropped and the contents easily leaking.
[0007] Furthermore, a technique was known in which a biaxially stretched polybutylene terephthalate film made of at least polybutylene terephthalate resin or a polyester resin composition in which polyethylene terephthalate (PET) resin is blended in a range of 30% by weight or less with polybutylene terephthalate (PBT) resin is formed with a vapor deposition film made of an inorganic oxide to obtain a biaxially stretched polybutylene terephthalate film excellent in compression resistance, impact resistance, and hot water resistance that can be used even under harsh retort conditions of 130°C or more (for example, Patent Document 3). However, the film-forming method by tubular simultaneous biaxial stretching disclosed in such a conventional technique has poor thickness accuracy due to the manufacturing method, and the plane orientation coefficient does not increase, so that not only is the impact resistance poor, but the film is easily stretched during processing such as adhesive coating, and has poor processability. In addition, PBT has a characteristic that the glass transition temperature is lower than that of PET, so that the film is easily stretched when tension is applied at high temperatures. For this reason, when tension is applied while being heated in each processing step, the film substrate stretches and cracks occur in the previously formed inorganic thin film layer, resulting in a problem of reduced barrier properties of the obtained barrier film.
[0008] In the above Patent Documents 1, 2 and 3, retort barrier performance is considered, but the compatibility of barrier performance and boil performance in a high-temperature and high-humidity environment with toughness is not considered.
[0009] Thus, it has not yet been possible to obtain a laminated film that is excellent in production stability, processing stability, and cost efficiency during manufacturing, that can maintain excellent barrier performance even in harsh environments such as high-temperature and high-humidity environments, and that can maintain its barrier properties, adhesion, and toughness even after sterilization treatment such as boiling. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Patent No. 4857482 [Patent Document 2] JP 2013-154605 A [Patent Document 3] JP 2012-214248 A Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention has been made against the background of the problems with the conventional technology, and has an object to provide a laminate that has excellent barrier performance even in a high-temperature and high-humidity environment, and can maintain excellent barrier properties and toughness even when used in applications in which a severe moist heat treatment such as boiling is performed. [Means for solving the problem]
[0012] The laminated film of the present invention, which has solved the above problems, has the following features.
[0013] (1) A laminate film comprising at least three layers, namely a substrate layer, a coating layer and an inorganic thin film layer, laminated in that order, the laminate film being characterized in that it satisfies the following requirements (a) to (d): (a) The substrate layer is made of a resin composition containing 70% by mass or more of a polybutylene terephthalate resin. (b) The puncture strength of the laminated film after boiling at 95°C for 30 minutes, measured in accordance with JIS Z 1707, is 0.6 N / μm or more. (c) The degree of planar orientation of the substrate layer is 0.144 to 0.160. (d) When the oxygen permeability value of the laminate film measured under conditions of 23°C × 65% RH is (A) and the oxygen permeability value measured under conditions of 40°C × 90% RH is (B), the barrier value deterioration rate under high temperature and high humidity conditions, expressed by the following formula, is 300% or less. Barrier value deterioration rate under high temperature and humidity conditions (%) = (B / A) x 100
[0014] (2) The laminate film according to (1), wherein the base layer further satisfies the following condition (e): (e) The thermal shrinkage rate of the base layer in both the longitudinal and transverse directions at 150° C. is 4.0% or less.
[0015] (3) The laminate film according to (1) or (2), wherein the inorganic thin film layer is a layer made of a composite oxide of silicon oxide and aluminum oxide.
[0016] (4) The laminate film according to any one of (1) to (3), wherein the coating layer is made of a resin composition containing a resin having an oxazoline group. Effect of the Invention
[0017] The laminated film of the present invention has excellent barrier performance even in a high-temperature and high-humidity environment. Therefore, deterioration of the contents can be suppressed even in a harsh transportation and storage environment. In addition, since it has excellent barrier properties and adhesive properties before and after boiling treatment, there is no problem of deterioration or leakage of the contents. Furthermore, since it has excellent toughness as a base material, there is little risk of the bag being punctured or torn. Moreover, since the laminated film of the present invention has excellent processability and can be easily manufactured, it is possible to provide a gas barrier film that is both economical and stable in production. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The laminate film of the present invention is a laminate film comprising at least three layers, namely a base layer, a coating layer, and an inorganic thin film layer, laminated in this order, and characterized in that the film satisfies the following requirements (a) to (d): (a) The substrate layer is made of a resin composition containing 70% by mass or more of a polybutylene terephthalate resin. (b) The puncture strength of the laminated film after boiling at 95°C for 30 minutes, measured in accordance with JIS Z 1707, is 0.6 N / μm or more. (c) The degree of planar orientation of the substrate layer is 0.144 to 0.160. (d) When the oxygen permeability value of the laminate film measured under conditions of 23°C × 65% RH is (A) and the oxygen permeability value measured under conditions of 40°C × 90% RH is (B), the barrier value deterioration rate under high temperature and high humidity conditions, expressed by the following formula, is 300% or less. Barrier value deterioration rate under high temperature and humidity conditions (%) = (B / A) x 100
[0019] The present inventors have found that when a biaxially stretched polyester film containing a predetermined amount of polybutylene terephthalate is used as a substrate layer and an inorganic thin film layer is laminated on the substrate layer to form a substrate laminate film, good barrier performance can be maintained even in a high-temperature and high-humidity environment. The present inventors have also found that by using the polybutylene terephthalate-based biaxially stretched polyester film having excellent moisture resistance as the substrate instead of a polyamide layer and further providing a coating layer between the inorganic thin film layer and the substrate, the barrier property and adhesiveness after boiling treatment are excellent, and the toughness as a substrate is also excellent, and have completed the present invention.
[0020] The base layer and each layer laminated thereon will be described below in order.
[0021] [Base material layer] The substrate layer used in the present invention is a biaxially stretched film made of a resin composition containing 70% by mass or more of PBT. The content of PBT is more preferably 75% by mass or more. If the content of PBT is less than 70% by mass, the puncture strength is reduced and the film properties are not sufficient. PBT preferably contains 90 mol % or more, more preferably 95 mol % or more, even more preferably 98 mol % or more, and most preferably 100 mol % of terephthalic acid as a dicarboxylic acid component, and preferably contains 90 mol % or more, more preferably 95 mol % or more, even more preferably 97 mol % or more of 1,4-butanediol as a glycol component, and most preferably contains no by-products other than those generated by ether bonds of 1,4-butanediol during polymerization.
[0022] The resin composition used in the present invention may contain a polyester other than PBT for the purpose of adjusting the film formability during biaxial stretching and the mechanical properties of the obtained film. Examples of polyesters other than PBT include at least one polyester selected from the group consisting of PET, polyethylene naphthalate, polybutylene naphthalate, and polypropylene terephthalate; PBT copolymerized with at least one dicarboxylic acid selected from the group consisting of isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyl dicarboxylic acid, cyclohexane dicarboxylic acid, adipic acid, azelaic acid, and sebacic acid; and PBT copolymerized with at least one diol component selected from the group consisting of ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, cyclohexanediol, polyethylene glycol, polytetramethylene glycol, and polycarbonate diol.
[0023] The upper limit of the amount of the polyester resin other than PBT added is preferably 30% by mass or less, more preferably 25% by mass or less. If the amount of the polyester resin other than PBT added exceeds 30% by mass, the mechanical properties of polybutylene terephthalate are impaired, and the impact strength, pinhole resistance, or bag rupture resistance becomes insufficient, and in addition, problems such as reduced transparency and gas barrier properties may occur.
[0024] The lower limit of the intrinsic viscosity of the polybutylene terephthalate (PBT) used in the present invention is preferably 0.9 dl / g, more preferably 0.95 dl / g, and further preferably 1.0 dl / g. If the intrinsic viscosity of the raw material polybutylene terephthalate (PBT) is less than 0.9 dl / g, the intrinsic viscosity of the film obtained by film formation will be low, and this may result in low puncture strength, impact strength, pinhole resistance, or bag rupture resistance. The upper limit of the intrinsic viscosity of polybutylene terephthalate is preferably 1.4 dl / g. If it exceeds the upper limit, the stress during stretching becomes too high, and film formability may deteriorate. When polybutylene terephthalate with a high intrinsic viscosity is used, the melt viscosity of the resin becomes high, so the extrusion temperature needs to be high, but extruding polybutylene terephthalate at a higher temperature may easily produce decomposition products.
[0025] The resin composition may contain conventionally known additives, such as a lubricant, a stabilizer, a colorant, an antistatic agent, and an ultraviolet absorbing agent, if necessary. As the lubricant type, inorganic lubricants such as silica, calcium carbonate, alumina, and organic lubricants are preferred, silica and calcium carbonate are more preferred, and silica is particularly preferred in terms of reducing haze. These lubricants can provide transparency and lubricity. The lower limit of the lubricant concentration is preferably 100 ppm, more preferably 500 ppm, and even more preferably 800 ppm. If it is less than the above, the slipperiness of the base film layer may decrease. The upper limit of the lubricant concentration is preferably 20000 ppm, more preferably 10000 ppm, and even more preferably 1800 ppm. If it exceeds the above, the transparency may decrease.
[0026] In the present invention, the lower limit of the thickness of the base layer is preferably 3 μm, more preferably 5 μm, and further preferably 8 μm. If it is 3 μm or more, the strength of the base film layer is sufficient. The upper limit of the thickness of the base film layer is preferably 100 μm, more preferably 75 μm, and further preferably 50 μm. If it is 100 μm or less, processing for the purpose of the present invention becomes easier.
[0027] The upper limit of the heat shrinkage rate of the biaxially stretched polyester film constituting the base layer in the present invention after heating at 150°C for 15 minutes in the longitudinal stretching (machine direction) direction (MD) and transverse stretching (width) direction (TD) is preferably 4.0%, more preferably 3.0%, and even more preferably 2%. If the upper limit is exceeded, not only may cracks occur in the inorganic thin film layer due to dimensional changes in the base film layer that occur in the process of forming the inorganic thin film layer / protective layer or in high-temperature treatment such as retort sterilization treatment, resulting in a decrease in gas barrier properties, but also pitch deviation may occur due to dimensional changes during processing such as printing.
[0028] The lower limit of the heat shrinkage rate of the biaxially oriented polyester film constituting the base layer in the present invention after heating at 150° C. for 15 minutes in both the longitudinal stretching direction (MD) and the transverse stretching direction (TD) is preferably 0%. If it is below the lower limit, the improvement effect will not be further obtained (saturation will occur) and the film may become mechanically brittle.
[0029] The lower limit of the impact strength of the biaxially oriented polyester film constituting the base layer in the present invention is preferably 0.05 J / μm. If it is 0.05 J / μm or more, the strength is sufficient when used as a bag. The upper limit of the impact strength of the biaxially oriented polyester film constituting the base layer in the present invention is preferably 0.2 J / μm. Even if the upper limit is exceeded, the effect of improvement is not obtained any more (it becomes saturated).
[0030] The lower limit of the planar orientation degree (ΔP) of the PBT film of the polyester film of the present invention is preferably 0.144, more preferably 0.148, and further preferably 0.15. If it is less than the above, the orientation is weak, so not only is sufficient strength not obtained and the puncture strength may decrease, but also, when an inorganic thin film layer is provided on a base film layer to form a laminate film, the inorganic thin film layer is easily stretched due to the tension and temperature applied during formation, and the inorganic thin film layer may crack, resulting in a decrease in gas barrier properties. The upper limit of the planar orientation degree (ΔP) of the polyester film in the present invention is preferably 0.160, more preferably 0.158. If it exceeds the above, the orientation becomes too strong and the film is easily broken during film formation. In addition, the higher the orientation, the higher the heat fixation temperature is required to reduce the heat shrinkage rate, and there is a risk that the strength of the film will be reduced due to crystallization.
[0031] The upper limit of the haze per thickness of the biaxially oriented polyester film constituting the base layer in the present invention is preferably 0.66% / μm, more preferably 0.60% / μm, and even more preferably 0.53% / μm. When printing is performed on a base layer having a haze of 0.66% / μm or less, the quality of the printed characters and images is improved.
[0032] The upper limit of the intrinsic viscosity (IV) of the biaxially oriented polyester film constituting the base layer in the present invention is preferably 1.20 dl / g, more preferably 1.15 dl / g, and even more preferably 1.10 dl / g. If it exceeds the upper limit, the strength of the film is improved, but the pressure load on the filter during extrusion becomes large, making production difficult. The lower limit is preferably 0.60 dl / g, more preferably 0.65 dl / g, and even more preferably 0.70 dl / g. If it is below the lower limit, the strength of the film may decrease.
[0033] In addition, the biaxially oriented polyester film constituting the base layer in the present invention may be subjected to a corona discharge treatment, a glow discharge treatment, a flame treatment, or a surface roughening treatment, and may also be subjected to a known anchor coat treatment, printing, decoration, etc., as long as the object of the present invention is not impaired.
[0034] Next, the production methods for obtaining the polyester film of the present invention will be specifically described, although the methods are not limited thereto. The manufacturing method for obtaining the polyester film of the present invention includes a step of melt-extruding a polyester raw material resin into a sheet form and cooling it on a casting drum to form an unstretched sheet, a longitudinal stretching step of stretching the formed unstretched sheet in the longitudinal direction, a preheating step of preheating to a temperature at which the unstretched sheet can be stretched laterally after the longitudinal stretching, a transverse stretching step of stretching the unstretched sheet in the width direction perpendicular to the longitudinal direction, a heat setting step of heating and crystallizing the film after the longitudinal and transverse stretching steps, a heat relaxation step of removing residual strain in the heat-set film, and a cooling step of cooling the film after the heat relaxation step. [Unstretched sheet molding process] First, the film raw materials are dried or hot air dried, then the raw materials are weighed, mixed, and fed into an extruder, where they are heated and melted, and then melt-cast into a sheet. The molten resin sheet is then brought into contact with a cooling roll (casting roll) using an electrostatic application method, and cooled and solidified to obtain an unstretched sheet. The electrostatic application method is a method in which a voltage is applied to an electrode disposed near the surface of the resin sheet opposite to the surface that contacts the rotating metal roll near where the molten resin sheet contacts the rotating metal roll, thereby charging the resin sheet and bringing the resin sheet into close contact with the rotating cooling roll.
[0035] The lower limit of the resin heat melting temperature is preferably 200°C, more preferably 250°C, and even more preferably 260°C. If the temperature is lower than the above, extrusion may become unstable. The upper limit of the resin melting temperature is preferably 280°C, more preferably 270°C. If the temperature exceeds the above, decomposition of the resin proceeds, and the film becomes brittle.
[0036] It is preferable to reduce the difference in crystallinity in the width direction when the molten polyester resin is extruded and cast onto a cooling roll. Specific methods for this purpose include casting raw materials of the same composition in a multi-layered form when the molten polyester resin is extruded and cast onto a cooling roll, and further lowering the cooling roll temperature. PBT resin has a fast crystallization rate, so crystallization continues even during casting. In this case, if the film is cast in a single layer without being multi-layered, the crystals will grow into large spherulites because there is no barrier that can suppress the growth of the crystals. As a result, the yield stress of the obtained unstretched sheet will be high, and not only will it be easily broken during biaxial stretching, but the impact strength, pinhole resistance, or bag breakage resistance of the obtained biaxially stretched film will be insufficient. On the other hand, by laminating the same resin in multiple layers, the stretching stress of the unstretched sheet can be reduced, and the subsequent biaxial stretching can be stably performed.
[0037] The method of extruding molten polyester resin and casting raw materials of the same composition into multiple layers specifically includes at least a step (1) of melting a resin composition containing 70% by weight or more of PBT resin to form a molten fluid, a step (2) of forming a laminated fluid having 60 or more layers from the formed molten fluid, a step (3) of discharging the formed laminated fluid from a die and bringing it into contact with a cooling roll to solidify it to form a laminated unstretched sheet, and a step (4) of biaxially stretching the laminated unstretched sheet. Other steps may be inserted between step (1) and step (2) and between step (2) and step (3). For example, a filtration step, a temperature change step, etc. may be inserted between step (1) and step (2). Furthermore, a temperature change step, a charge application step, etc. may be inserted between step (2) and step (3). However, there must be no step between step (2) and step (3) that destroys the laminated structure formed in step (2).
[0038] In step (1), the method for melting the polyester resin composition to form a molten fluid is not particularly limited, but a suitable method is to heat and melt the composition using a single-screw extruder or a twin-screw extruder.
[0039] The method for forming the laminated fluid in step (2) is not particularly limited, but from the viewpoints of facility simplicity and maintainability, a static mixer and / or a multi-layer feed block is more preferred. From the viewpoint of uniformity in the sheet width direction, a device having a rectangular melt line is more preferred. It is further preferred to use a static mixer or a multi-layer feed block having a rectangular melt line. The resin composition consisting of multiple layers formed by joining multiple resin compositions may be passed through one or more of a static mixer, a multi-layer feed block, and a multi-layer manifold.
[0040] The theoretical number of layers in step (2) is preferably 60 or more. The lower limit of the theoretical number of layers is more preferably 500. If the theoretical number of layers is too small, or the distance between the layer interfaces is long and the crystal size becomes too large, the effect of the present invention tends not to be obtained. In addition, the crystallinity increases near both ends of the sheet, making film formation unstable and reducing transparency after molding. The upper limit of the theoretical number of layers in step (2) is not particularly limited, but is preferably 100,000, more preferably 10,000, and even more preferably 7,000. Even if the theoretical number of layers is extremely large, the effect may become saturated.
[0041] When the lamination in step (2) is performed using a static mixer, the theoretical number of layers can be adjusted by selecting the number of elements of the static mixer. A static mixer is generally known as a stationary mixer (line mixer) without a drive unit, and the fluid that enters the mixer is stirred and mixed sequentially by the elements. However, when a high-viscosity fluid is passed through a static mixer, the high-viscosity fluid is divided and layered, forming a layered fluid. Each time the high-viscosity fluid passes through one element of the static mixer, it is divided into two, which then merge and are layered. For this reason, when a high-viscosity fluid is passed through a static mixer with n elements, a layered fluid with a theoretical number of layers N = 2n is formed.
[0042] A typical static mixer element has a rectangular plate twisted 180 degrees, with right and left elements depending on the direction of twist, and the dimensions of each element are basically 1.5 times the length compared to the diameter. Static mixers that can be used in the present invention are not limited to this type.
[0043] When the lamination in step (2) is performed in a multi-layer feedblock, the theoretical number of layers can be adjusted by selecting the number of divisions and laminations of the multi-layer feedblock. Multiple multi-layer feedblocks can be installed in series. It is also possible for the high-viscosity fluid supplied to the multi-layer feedblock itself to be the lamination fluid. For example, if the number of layers of the high-viscosity fluid supplied to the multi-layer feedblock is p, the number of divisions and layers of the multi-layer feedblock is q, and the number of installed multi-layer feedblocks is r, the number of layers N of the lamination fluid is N = p × qr.
[0044] In step (3), the laminating fluid is discharged from the die and solidified by contacting it with a chill roll. The lower limit of the cooling roll temperature is preferably -10°C. If the temperature is lower than this, the effect of suppressing crystallization may become saturated. The upper limit of the cooling roll temperature is preferably 40°C. If the temperature exceeds this, the crystallinity may become too high, making stretching difficult. The upper limit of the cooling roll temperature is preferably 25°C. Furthermore, when the cooling roll temperature is in the above range, it is preferable to lower the humidity of the environment near the cooling roll to prevent condensation. It is preferable to reduce the temperature difference in the width direction of the cooling roll surface. In this case, the thickness of the unstretched sheet is preferably in the range of 15 to 2500 μm. The above-mentioned multi-layered unstretched sheet has at least 60 layers, preferably at least 250 layers, and more preferably at least 1000 layers. If the number of layers is too small, the effect of improving stretchability is lost.
[0045] [Longitudinal and transverse stretching processes] The stretching method can be either simultaneous biaxial stretching or sequential biaxial stretching, but in order to increase the piercing strength, it is necessary to increase the degree of planar orientation, and sequential biaxial stretching is most preferable in terms of high productivity and high film production speed.
[0046] The lower limit of the stretching temperature in the longitudinal stretching direction is preferably 55°C, more preferably 60°C. At 55°C or higher, breakage is unlikely to occur. In addition, since the longitudinal orientation of the film is not too strong, shrinkage stress during heat setting treatment can be suppressed, and a film with less distortion of molecular orientation in the width direction can be obtained. The upper limit of the stretching temperature in the longitudinal stretching direction is preferably 100°C, more preferably 95°C. If it is 100°C or lower, the orientation of the film is not too weak, so the mechanical properties of the film are not reduced.
[0047] The lower limit of the stretching ratio in the longitudinal stretching direction is preferably 2.8 times, and particularly preferably 3.0 times. If it is 2.8 times or more, the degree of planar orientation increases, and the puncture strength of the film improves. The upper limit of the stretching ratio in the longitudinal stretching direction is preferably 4.3 times, more preferably 4.0 times, and particularly preferably 3.8 times. If it is 4.3 times or less, the orientation degree in the transverse direction of the film is not too strong, the shrinkage stress during heat setting is not too large, and the distortion of the molecular orientation in the transverse direction of the film is small, resulting in improved linear tearability in the longitudinal direction. In addition, the effect of improving the mechanical strength and thickness unevenness is saturated within this range.
[0048] The lower limit of the stretching temperature in the transverse stretching direction is preferably 60° C., and if it is 60° C. or higher, breakage may be less likely to occur. The upper limit of the stretching temperature in the transverse stretching direction is preferably 100° C., and if it is 100° C. or lower, the degree of orientation in the transverse direction increases, improving the mechanical properties.
[0049] The lower limit of the stretching ratio in the transverse stretching direction is preferably 3.5 times, more preferably 3.6 times, and particularly preferably 3.7 times. If it is 3.5 times or more, the degree of orientation in the transverse direction is not too weak, and the mechanical properties and thickness unevenness are improved. The upper limit of the stretching ratio in the transverse stretching direction is preferably 5 times, more preferably 4.5 times, and particularly preferably 4.0 times. If it is 5.0 times or less, the effect of improving the mechanical strength and thickness unevenness is maximized (saturated) even in this range.
[0050] [Heat setting process] The lower limit of the heat setting temperature in the heat setting step is preferably 195° C., more preferably 200° C. If the temperature is 195° C. or higher, the heat shrinkage rate of the film is small, and even after boiling treatment, the inorganic thin film layer is less likely to be damaged, improving the gas barrier property. The upper limit of the heat setting temperature is preferably 220° C., and if the temperature is 220° C. or lower, the base film layer does not melt and is less likely to become brittle.
[0051] [Thermal relaxation section process] The lower limit of the relaxation rate in the heat relaxation section is preferably 0.5%. If it is 0.5% or more, breakage may be less likely to occur during heat setting. The upper limit of the relaxation rate is preferably 10%. If it is 10% or less, shrinkage in the longitudinal direction during heat setting is reduced, resulting in less distortion of the molecular orientation at the film edge, and improved straight tearability. In addition, sagging of the film is less likely to occur, and thickness unevenness is less likely to occur.
[0052] [Cooling process] In the cooling step after the relaxation in the heat relaxing section, the temperature of the surface of the edge of the polyester film is preferably set to 80° C. or lower. If the temperature of the film ends after passing through the cooling process exceeds 80°C, the ends will be stretched by the tension applied when the film is wound up, resulting in a high thermal shrinkage rate in the longitudinal direction of the ends, and the distribution of thermal shrinkage rate in the width direction of the roll will be non-uniform. When such a roll is heated and transported for deposition processing, etc., streaky wrinkles will occur, and the physical properties of the final gas barrier film may be non-uniform in the width direction.
[0053] In the cooling process, methods for keeping the surface temperature of the film ends at 80°C or below can include adjusting the temperature and air volume in the cooling process, providing a shielding plate at the center in the width direction of the cooling zone to selectively cool the ends, or blowing cold air locally against the ends of the film.
[0054] [Coating layer]
[0055] In the laminate film of the present invention, a coating layer can be provided between the substrate layer and the inorganic thin film layer for the purpose of ensuring the barrier property and laminate strength after boiling retort treatment. Examples of the coating layer include resins such as urethane, polyester, acrylic, titanium, isocyanate, imine, and polybutadiene, to which curing agents such as epoxy, isocyanate, and melamine are added. Examples of the solvent (solvent) include aromatic solvents such as benzene and toluene; alcohol solvents such as methanol and ethanol; ketone solvents such as acetone and methyl ethyl ketone; ester solvents such as ethyl acetate and butyl acetate; and polyhydric alcohol derivatives such as ethylene glycol monomethyl ether. The resin composition used for these coating layers preferably contains a silane coupling agent having at least one type of organic functional group. Examples of the organic functional group include an alkoxy group, an amino group, an epoxy group, and an isocyanate group. The addition of the silane coupling agent further improves the laminate strength after retort treatment.
[0056] Among the resin compositions used for the coating layer, it is preferable to use a resin containing an oxazoline group. The oxazoline group has a high affinity with the inorganic thin film, and can react with the oxygen-deficient portion of the inorganic oxide or the metal hydroxide generated during the formation of the inorganic thin film layer, and shows strong adhesion with the inorganic thin film layer. In addition, the unreacted oxazoline group present in the coating layer can react with the carboxylic acid terminal generated by hydrolysis of the substrate film and the coating layer to form a crosslink.
[0057] The coating layer may be mixed with any one of polyester resin, urethane resin, and acrylic resin for the purpose of improving adhesion with the base layer. In particular, urethane resin is preferred in terms of adhesion, and acrylic resin is preferred in terms of water resistance.
[0058] The method for forming the coating layer is not particularly limited, and a conventionally known method such as a coating method can be adopted. Among the coating methods, preferred methods include an offline coating method and an in-line coating method. For example, in the case of an in-line coating method carried out in the process of manufacturing a biaxially stretched polyester film substrate constituting a substrate layer, the conditions of drying and heat treatment during coating depend on the coating thickness and the device conditions, but it is preferable to feed the film immediately after coating into a stretching process in the perpendicular direction and dry it in the preheating zone or stretching zone of the stretching process, and in such a case, it is usually preferable to set the temperature at about 50 to 250 ° C. A method of adopting a sequential biaxial stretching method, coating the film after MD stretching, and then TD stretching is more preferable.
[0059] In the present invention, the coating weight of the coating layer is 0.010 to 0.200 g / m 2 It is preferable that the coating layer is made uniform, and as a result, the inorganic thin film layer can be densely deposited. In addition, the cohesive force inside the coating layer is improved, and the adhesion between the substrate layer, coating layer, and inorganic thin film layer is also increased, so that the water-resistant adhesion of the coating layer can be improved. The coating layer preferably has a deposition weight of 0.015 g / m 2 More preferably, 0.020 g / m 2 More preferably, 0.025 g / m 2 or more, preferably 0.190 g / m 2 Less than or equal to 0.180 g / m 2 or less, more preferably 0.170 g / m 2 The coating weight is 0.200g / m or less. 2If the thickness of the coating layer exceeds 0.010 g / m, the cohesive force inside the coating layer becomes insufficient, and good adhesion may not be achieved. In addition, the uniformity of the coating layer is reduced, which may cause defects in the inorganic thin film layer and reduce the gas barrier properties. Moreover, the manufacturing cost increases, which is economically disadvantageous. On the other hand, if the thickness of the coating layer is 0.010 g / m 2 If the thickness is less than this, the substrate cannot be sufficiently covered, and there is a risk that sufficient gas barrier properties and interlayer adhesion cannot be obtained.
[0060] The resin composition for the covering layer may contain various known inorganic and organic additives such as antistatic agents, slipping agents, and antiblocking agents, if necessary, within the scope of the present invention.
[0061] [Inorganic thin film layer] The substrate laminated film of the present invention has an inorganic thin film layer laminated thereon. The inorganic thin film layer is a thin film made of an inorganic oxide. There is no particular limitation on the material forming the inorganic thin film layer as long as it can be made into a thin film, but from the viewpoint of gas barrier properties, inorganic oxides such as silicon oxide (silica), aluminum oxide (alumina), and a mixture of silicon oxide and aluminum oxide (composite oxide) are preferred. In particular, a composite oxide of silicon oxide and aluminum oxide is preferred from the viewpoint of achieving both flexibility and denseness of the thin film layer. In this composite oxide, the mixture ratio of silicon oxide and aluminum oxide is preferably in the range of 20 to 70 mass% Al in terms of the mass ratio of the metal content. If the Al concentration is less than 20 mass%, the barrier property may be reduced, while if it exceeds 70 mass%, the inorganic thin film layer tends to become hard, and there is a risk that the film will be destroyed during secondary processing such as printing or lamination, resulting in a reduction in barrier property. The silicon oxide referred to here is various silicon oxides such as SiO and SiO2 or a mixture thereof, and the aluminum oxide is various aluminum oxides such as AlO and Al2O3 or a mixture thereof.
[0062] The inorganic thin film layer has a thickness of usually 1 to 100 nm, preferably 5 to 50 nm. If the inorganic thin film layer has a thickness of less than 1 nm, it may be difficult to obtain satisfactory gas barrier properties, while if the inorganic thin film layer has a thickness exceeding 100 nm, the corresponding improvement in gas barrier properties cannot be obtained, and it is rather disadvantageous in terms of flex resistance and production costs.
[0063] The method for forming the inorganic thin film layer is not particularly limited, and any known deposition method, such as physical deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, or chemical deposition (CVD), may be appropriately adopted. A typical method for forming the inorganic thin film layer will be described below using a silicon oxide / aluminum oxide thin film as an example. For example, when the vacuum deposition method is adopted, a mixture of SiO2 and Al2O3, or a mixture of SiO2 and Al, is preferably used as the deposition raw material. Particles are usually used as these deposition raw materials, and in this case, it is desirable that the size of each particle is large enough that the pressure during deposition does not change, and the preferred particle diameter is 1 mm to 5 mm. Heating can be performed by resistance heating, high-frequency induction heating, electron beam heating, laser heating, or other methods. It is also possible to introduce oxygen, nitrogen, hydrogen, argon, carbon dioxide, water vapor, or other reactive gases as reaction gases, or to adopt reactive deposition using means such as ozone addition and ion assist. Furthermore, the film formation conditions can be changed arbitrarily, such as applying a bias to the deposition target (laminated film to be subjected to deposition), or heating or cooling the deposition target. The deposition material, reaction gas, bias of the deposition target, heating / cooling, etc. can be changed in the same manner when the sputtering method or the CVD method is adopted.
[0064] In the present invention, a protective layer may be provided on the inorganic thin film layer as necessary. The inorganic thin film layer is not a completely dense film, but has minute defects scattered therein. By forming a protective layer by applying a resin composition for a protective layer on the inorganic thin film layer, the resin in the resin composition for a protective layer penetrates into the defective parts of the inorganic thin film layer, resulting in an effect of stabilizing the gas barrier properties. In addition, since the deterioration of the barrier properties when a printing layer is laminated can be suppressed, printing becomes possible. In addition, by using a material having gas barrier properties for the protective layer itself, the gas barrier performance of the laminated film can also be greatly improved.
[0065] Examples of the protective layer formed on the surface of the laminated film of the present invention include resins such as urethane, polyester, acrylic, titanium, isocyanate, imine, polybutadiene, etc., to which curing agents such as epoxy, isocyanate, melamine, etc. are added. Examples of the solvent (solvent) include aromatic solvents such as benzene and toluene, alcohol solvents such as methanol and ethanol, ketone solvents such as acetone and methyl ethyl ketone, ester solvents such as ethyl acetate and butyl acetate, polyhydric alcohol derivatives such as ethylene glycol monomethyl ether, etc.
[0066] [Lamination with heat-sealable resin layer] The laminated film of the present invention is preferably used by laminating it with a heat-sealable resin layer called a sealant. The heat-sealable resin layer is usually provided on the inorganic thin film layer side (on the protective layer surface when a protective layer is formed on the inorganic thin film layer), but may also be provided on the outside of the base film (on the surface opposite to the surface on which the coating layer is formed). The heat-sealable resin layer is usually formed by extrusion lamination or dry lamination using a sealant film. The thermoplastic polymer forming the heat-sealable resin layer may be any polymer that can fully exhibit sealant adhesion, and may be polyethylene resins such as HDPE, LDPE, and LLDPE, polypropylene resin, ethylene-vinyl acetate copolymer, ethylene-α-olefin random copolymer, ionomer resin, etc. The thickness of the heat-sealable resin layer is preferably 20 μm or more, more preferably 25 μm or more, and even more preferably 30 μm or more, and is preferably 80 μm or less, more preferably 75 μm or less, and even more preferably 70 μm or less. If the thickness is 20 μm or less, productivity is poor. On the other hand, if it is more than 80 μm, the cost increases and the transparency deteriorates.
[0067] [Other layers] In the laminate film of the present invention, a printed layer, other plastic substrate and / or paper substrate may be laminated between the heat-sealable resin layer and at least one other layer.
[0068] [Adhesive layer] The adhesive layer used in the present invention can be a general-purpose adhesive for lamination. For example, (non-)solvent type, water-based type, or hot melt type adhesives mainly composed of poly(ester)urethane, polyester, polyamide, epoxy, poly(meth)acrylic, polyethyleneimine, ethylene-(meth)acrylic acid, polyvinyl acetate, (modified) polyolefin, polybutadiene, wax, or casein can be used. Among these, urethane or polyester types are preferred in consideration of the moisture and heat resistance that can withstand retort treatment and the flexibility that can follow the dimensional changes of each substrate. The adhesive layer can be applied by, for example, direct gravure coating, reverse gravure coating, kiss coating, die coating, roll coating, dip coating, knife coating, spray coating, fountain coating, or other methods, and the coating amount after drying is 1 to 8 g / m in order to exhibit sufficient adhesion after retort. 2 More preferably, the thickness is 2 to 7 g / m 2 , and more preferably 3 to 6 g / m 2 The coating amount is 1g / m 2 If it is less than 8g / m, it becomes difficult to bond the entire surface, and the adhesive strength decreases. 2 If the temperature exceeds this range, it will take a long time for the film to completely cure, unreacted material will be likely to remain, and adhesive strength will decrease.
[0069] As the printing ink for forming the printing layer, water-based and solvent-based resin-containing printing inks can be preferably used. Examples of the resin used in the printing ink include acrylic resins, urethane resins, polyester resins, vinyl chloride resins, vinyl acetate copolymer resins, and mixtures thereof. The printing ink may contain known additives such as antistatic agents, light blocking agents, ultraviolet absorbers, plasticizers, lubricants, fillers, colorants, stabilizers, lubricants, defoamers, crosslinking agents, antiblocking agents, and antioxidants. The printing method for providing the printing layer is not particularly limited, and known printing methods such as offset printing, gravure printing, and screen printing can be used. To dry the solvent after printing, known drying methods such as hot air drying, hot roll drying, and infrared drying can be used.
[0070] In the laminated film of the present invention, when the oxygen transmission rate under the condition of 23°C x 65% RH is (A) and the oxygen transmission rate under the condition of 40°C x 90% RH is (B), the barrier value deterioration rate under high temperature and high humidity conditions is expressed by the formula (b)B / A x 100 [%], and the value must be 300% or less. The deterioration rate can be preferably 250% or less, more preferably 200% or less. If the deterioration rate exceeds 300%, it becomes difficult to meet the needs of applications requiring gas barrier properties under high temperature and high humidity environments.
[0071] The laminate of the present invention has an oxygen permeability of 30 ml / m before and after the boiling treatment. 2 d MPa or less, and more preferably 25 ml / m 2 ·d·MPa or less, more preferably 20ml / m 2 ·d·MPa or less. Oxygen permeability is 30ml / m 2 If the pressure exceeds d MPa, there is a risk of the contents deteriorating due to oxidation.
[0072] The laminate of the present invention has a water vapor transmission rate of 2.5 g / m2 both before and after boiling treatment. 2 d or less, and more preferably 2.0 g / m 2 d or less, more preferably 1.5 g / m 2 ·d or less. Water vapor permeability is 2.5g / m 2 If it exceeds d, there is a risk of a decrease in quality and aroma retention due to a loss of moisture in the contents.
[0073] The laminate of the present invention preferably has a water-lamination strength of 2.0 N / 15 mm or more under conditions of 23°C x 65% RH before and after boiling treatment, more preferably 2.5 N / 15 mm or more, and even more preferably 3.0 N / 15 mm or more. If the lamination strength is less than 2.0 N / 15 mm, peeling may occur due to bending load or liquid contents, resulting in deterioration of barrier properties or leakage of contents. Furthermore, there is a risk of deterioration in hand tearability.
[0074] The laminated film of the present invention preferably has a puncture strength of 0.6 N / μm or more, more preferably 0.7 N / μm or more, and even more preferably 0.8 N / μm or more after boiling at 95° C. for 30 minutes, as measured in accordance with JIS Z 1707. If the puncture strength is less than 0.6 N / μm, there is a risk that the film will be punctured by an external load when used as a bag, causing the contents to leak out. EXAMPLES
[0075] Next, the present invention will be described in detail using examples and comparative examples, but the present invention is not limited to the following examples. Unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass." The evaluation methods used in the present invention are as follows.
[0076] (1) Thickness of laminated film The measurement was performed using a dial gauge in accordance with JIS K7130-1999 Method A.
[0077] (2) Planar orientation degree of laminated film ΔP The refractive index (Nx) in the longitudinal direction and the refractive index (Ny) in the width direction of the sample were measured using an Abbe refractometer with sodium D line as a light source according to JIS K 7142-1996 A method, and the degree of planar orientation ΔP was calculated according to formula (1). Planar orientation degree (ΔP)=(Nx+Ny) / 2-Nz (1)
[0078] (3) Thermal shrinkage rate of laminated film The heat shrinkage of the polyester film constituting the base layer was measured by the dimensional change test method described in JIS-C-2151-2006.21, except that the test temperature was 150°C and the heating time was 15 minutes. The test specimen was used as described in 21.1(a).
[0079] (4) Intrinsic viscosity IV of raw resin or laminated film The sample was dried in a vacuum at 130°C for a day and night, crushed or cut, and 80 mg of the crushed sample was precisely weighed and dissolved in a mixed solution of phenol / tetrachloroethane = 60 / 40 (volume ratio) at 80°C for 30 minutes by heating. The same mixed solution was added to make 20 ml, and then the measurement was performed at 30°C.
[0080] (5) Puncture strength of laminated film after boiling The films obtained in the examples and comparative examples were subjected to boiling treatment by keeping them in hot water at 95°C for 30 minutes, and the resulting boiled films were sampled into 5 cm squares, and the puncture strength of the films (after boiling) was measured in accordance with JIS Z1707 using a digital force gauge "ZTS-500N", a motorized test stand "MX2-500N", and a puncture jig "TKS-250N" manufactured by Imada Co., Ltd. The unit is N / μm.
[0081] (6) Deterioration rate of barrier value of laminated film under high temperature and high humidity conditions The laminated films obtained in the examples and comparative examples were measured for oxygen permeability (A) in an atmosphere of temperature 23° C. and humidity 65% RH using an oxygen permeability measuring device ("OX-TRAN (registered trademark) 1 / 50" manufactured by MOCON) in accordance with JIS-K7126 B method. The permeability was measured in the direction in which oxygen permeated from the side of the film that did not have an inorganic thin film layer to the inorganic thin film side. Similarly, the oxygen permeability (B) was measured in an atmosphere with a temperature of 40°C and a humidity of 90% RH, and the barrier value deterioration rate (b) B / A x 100 [%] was calculated. (7) Preparation of Laminate for Evaluation A polyurethane adhesive (TM569 manufactured by Toyo-Morton Co., Ltd.) was applied to the protective layer surface of the laminated film obtained in the Examples and Comparative Examples so that the thickness after drying treatment at 80°C would be 3 μm. A linear low-density polyethylene film (L4102 manufactured by Toyobo Co., Ltd.; thickness 40 μm; referred to as LL) was then dry-laminated on a metal roll heated to 60°C, and aging was carried out at 40°C for 4 days to obtain a laminated gas barrier laminate for evaluation (hereinafter sometimes referred to as a "laminate laminate").
[0082] (8) Evaluation method for pre- and post-boil oxygen transmission rate (OTR) of laminated materials The laminated body prepared in (5) above was measured for oxygen permeability under normal conditions in an atmosphere of 23°C and 65%RH humidity using an oxygen permeability measuring device ("OX-TRAN (registered trademark) 1 / 50" manufactured by MOCON) in accordance with JIS-K7126 B method. The oxygen permeability was measured in the direction in which oxygen permeates from the base film side of the laminated body to the heat-sealable resin layer side. On the other hand, the laminated body prepared in (5) above was subjected to a moist heat treatment in hot water at 95°C for 30 minutes, and dried at 40°C for 1 day (24 hours). The oxygen permeability (after boiling) of the resulting laminated body after moist heat treatment was measured in the same manner as above.
[0083] (9) Evaluation method for pre- and post-boil water vapor transmission rate (WVTR) of laminated materials The laminated product prepared in (5) above was measured for water vapor permeability under normal conditions in an atmosphere of temperature 40° C. and humidity 90% RH using a water vapor permeability measuring device ("PERMATRAN-W 3 / 33MG" manufactured by MOCON) in accordance with JIS-K7129 Method B. The water vapor permeability was measured in the direction in which water vapor permeates from the heat sealable resin layer side of the laminated product to the base film side. On the other hand, the laminate prepared in (5) above was subjected to a wet heat treatment by being kept in hot water at 95°C for 30 minutes, and then dried at 40°C for 1 day (24 hours). The water vapor permeability (after boiling) of the obtained wet heat treated laminate was measured in the same manner as above.
[0084] (10) Evaluation method for laminate strength before and after boiling The laminated laminate prepared in (5) above was cut into a test piece having a width of 15 mm and a length of 200 mm, and the laminate strength (normal state) was measured using a Tensilon universal material testing machine (Tensilon UMT-II-500 model, manufactured by Toyo Baldwin Co., Ltd.) under conditions of a temperature of 23° C. and a relative humidity of 65%. The laminate strength was measured at a tensile speed of 200 mm / min, and the strength was measured when water was applied between the laminated film layer and the heat-sealable resin layer of each laminated film obtained in the examples and comparative examples and the layer was peeled off at a peel angle of 90 degrees. On the other hand, the laminate prepared above was subjected to a boiling treatment in which it was kept in hot water at a temperature of 95°C for 30 minutes, and then immediately a test piece was cut out from the resulting laminate after the boiling treatment in the same manner as described above, and the laminate strength (after boiling treatment) was measured in the same manner as described above.
[0085] The raw material resins and coating solutions used in the present examples and comparative examples are described in detail below. The raw material resins and coating solutions used in the present examples and comparative examples are shown in Table 1. 1) Base film layer A Polybutylene terephthalate (PBT): The polybutylene terephthalate used in the film production described below was 1100-211XG (CHANG CHUN PLASTICS CO., LTD., intrinsic viscosity 1.28 dl / g). Polyethylene terephthalate (PET): The polyethylene terephthalate used in the film production described below was terephthalic acid / ethylene glycol=100 / / 100 (mol %) (manufactured by Toyobo Co., Ltd., intrinsic viscosity 0.62 dl / g).
[0086] 2) Resin having an oxazoline group (A): A commercially available water-soluble acrylate containing an oxazoline group ("Epocross (registered trademark) WS-300" manufactured by Nippon Shokubai Co., Ltd.; solid content 10%) was prepared as a resin having an oxazoline group. The amount of oxazoline groups in this resin was 7.7 mmol / g.
[0087] 3) Acrylic resin (B): A 25% by mass emulsion of a commercially available acrylic acid ester copolymer ("Mowinyl (registered trademark) 7980" manufactured by Nichigo Mowinyl Co., Ltd.) was prepared as the acrylic resin. The acid value (theoretical value) of this acrylic resin was 4 mgKOH / g.
[0088] 4) Urethane resin (C): A commercially available polyester urethane resin dispersion (Mitsui Chemicals' "Takelac (registered trademark) W605"; solid content 30%) was prepared as the urethane resin. The acid value of this urethane resin was 25 mgKOH / g, and the glass transition temperature (Tg) measured by DSC was 100°C. The ratio of aromatic or aromatic aliphatic diisocyanate to the entire polyisocyanate component measured by 1H-NMR was 55 mol%.
[0089] 5) Coating liquid 1 used for coating layer The materials were mixed in the following ratio to prepare a coating liquid (resin composition for coating layer). Water 50.53% by mass Isopropanol 22.00% by mass Oxazoline group-containing resin (A) 20.00% by mass Acrylic resin (B) 4.80% by mass Urethane resin (C) 2.67% by mass
[0090] The method for producing the base film layer A used in Examples 1 to 6 and Comparative Examples 1 to 5 will be described below. Using a single screw extruder, a mixture of 80% by mass of PBT resin and 20% by mass of PET resin was mixed with silica particles with an average particle size of 2.4 μm as inactive particles at a silica concentration of 900 ppm relative to the mixed resin. The mixture was then melted at 290°C, and the melt line was introduced into a 12-element static mixer. This allowed the polyester resin melt to be divided and laminated, resulting in a multi-layer melt made from the same raw materials. The mixture was cast from a T-die at 265°C and adhered to a cooling roll at 15°C by electrostatic adhesion to obtain an unstretched sheet. The film was then stretched 2.9 times in the machine direction at 60°C, and after the machine direction stretching, the adhesive layer resin composition (coating liquid 1) was applied by the fountain bar coating method. The film was then guided to a tenter while drying, and then passed through the tenter to stretch 4.0 times in the machine direction at 90°C. After performing a tension heat treatment at 200°C for 3 seconds and a 9% relaxation treatment for 1 second, the film was cooled at 50°C for 2 seconds. The surface temperature of the film end at this time was 75°C. Next, 9% of the gripped parts on both ends were cut off and removed to leave a polyester film with a thickness of 15 μm and a thickness of 0.030 g / m 2 The physical properties of the obtained film are shown in Table 1.
[0091] <Examples 2 to 6 and Comparative Examples 1 to 5> The film-forming process of the base film layer A was carried out in the same manner as in Example 1, except that the presence or absence of a coating layer, the PBT ratio, the longitudinal stretching ratio, the heat setting temperature, the relaxation rate, and the tenter cooling step zone temperature were as shown in Table 1. The physical properties of the obtained biaxially stretched polyester film are also shown in Table 1.
[0092] The method for producing the base film layer B used in Comparative Example 6 will be described below. <Comparative Example 6> Polyethylene terephthalate resin with an intrinsic viscosity of 0.62 dl / g (30°C, phenol / tetrachloroethane=60 / 40) was pre-crystallized, then dried, extruded at 280°C using an extruder with a T-die, and quenched and solidified on a drum with a surface temperature of 40°C to obtain an amorphous sheet. The sheet obtained was then stretched 4.0 times in the machine direction at 100°C between a heating roll and a cooling roll. Then, the above-mentioned coating liquid 1 was coated on one side of the obtained uniaxially stretched film by the fountain bar coating method. The film was introduced into a tenter while drying, preheated at 100°C, stretched 4.0 times in the transverse direction at 120°C, and heat-treated at 225°C while performing 6% relaxation in the transverse direction, to produce a biaxially stretched polyester film with a thickness of 12 μm. 2 A coating layer of A laminated film was obtained. The physical properties of the obtained film are shown in Table 1.
[0093] The method for producing the base film layer C used in Comparative Example 7 will be described below. <Comparative Example 7> Polycaproamide was heated and melted at 260°C in a screw extruder and extruded into a sheet from a T-die. The unstretched sheet was then stretched 3.3 times longitudinally at 80°C between a heating roll and a cooling roll. The above-mentioned coating liquid 1 was then applied to one side of the resulting uniaxially stretched film by a fountain coat method. The film was then introduced into a tenter, stretched 4.0 times in the transverse direction at 120°C, and heat-set at 215°C to produce a biaxially stretched polyamide film having a thickness of 15 μm. 2 The physical properties of the obtained film are shown in Table 1.
[0094] The method of forming the inorganic thin film layer in each of the examples and comparative examples will be described below. <Formation of inorganic thin film layer> As the inorganic thin film layer, a composite oxide layer of silicon dioxide and aluminum oxide was formed on the base film layer A, base film layer B, or C by electron beam deposition. Particulate SiO2 (purity 99.9%) and Al2O3 (purity 99.9%) of about 3 mm to 5 mm were used as the deposition source. The film thickness of the inorganic thin film layer (SiO2 / Al2O3 composite oxide layer) in the film thus obtained (film containing inorganic thin film layer / coating layer) was 13 nm. The composition of this composite oxide layer was SiO2 / Al2O3 (mass ratio) = 55 / 45.
[0095] A total of 13 types of substrate-laminated films and their laminates were obtained, and the evaluation results are shown in Table 1.
[0096] [Table 1] [Industrial Applicability]
[0097] The present invention provides excellent barrier performance even in high-temperature and high-humidity environments. Therefore, deterioration of the contents can be suppressed even in harsh transport and storage environments. In addition, since the film has excellent barrier and adhesive properties before and after boiling, there is no problem of deterioration or leakage of the contents. Furthermore, since the film has excellent toughness as a base material, there is little risk of the bag being punctured or torn. Moreover, since the laminated film of the present invention has excellent processability and can be easily manufactured, it is excellent in both economy and production stability, and a gas barrier film with uniform characteristics can be provided.
Claims
1. A laminate film comprising at least three layers, namely a base layer, a coating layer and an inorganic thin film layer, laminated in this order, the laminate film satisfying the following requirements (a) to (d) and (f): (a) The substrate layer is made of a resin composition containing 70 mass % or more of a polybutylene terephthalate resin. (b) The puncture strength of the laminated film after boiling at 95° C. for 30 minutes, measured in accordance with JIS Z 1707, is 0.6 N / μm or more. (c) the degree of planar orientation of the substrate layer is 0.15 to 0.160; (d) When the oxygen permeability value of the laminate film measured under conditions of 23°C x 65% RH is (A) and the oxygen permeability value measured under conditions of 40°C x 90% RH is (B), the barrier value deterioration rate under high temperature and high humidity conditions represented by the following formula is 300% or less. Barrier value deterioration rate under high temperature and high humidity conditions (%) = (B / A) x 100 (f) The thermal shrinkage rate of the base layer in the longitudinal direction at 150° C. is 2.4% or more and 4.0% or less.
2. 2. The laminated film according to claim 1, wherein the base layer further satisfies the following requirement (e): (e) The thermal shrinkage rate at 150° C. in the width direction of the base layer is 4.0% or less.
3. 3. The laminated film according to claim 1, wherein the inorganic thin film layer is a layer made of a composite oxide of silicon oxide and aluminum oxide.
4. 4. The laminated film according to claim 1, wherein the coating layer is made of a resin composition containing a resin having an oxazoline group.
Citation Information
Patent Citations
JP1973057482A
Retort packaging material including biaxially stretched polybutylene terephthalate film
JP2012214248A
Packaging material for boil / retort treatment and pouch
JP2013154605A
Packaging bag using polybutylene terephthalate film