Cold-rolled steel sheet having hydrophilic functional groups on its surface and method for producing the same

Hydrophilic functional groups on cold-rolled steel sheets, introduced via low-pressure plasma treatment, address the challenge of spot rust prevention and enhance degreasing and chemical conversion properties, providing a solution for improved surface treatment without oil contamination.

JP7574674B2Active Publication Date: 2024-10-29JFE STEEL CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021015301
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-05
Filing Date
2021-02-02
Publication Date
2024-10-29
Estimated Expiration
2041-02-02

AI Technical Summary

Technical Problem

Existing cold-rolled steel sheets face challenges in preventing spot rust without increasing the amount of rust preventive oil, which can contaminate the production line and affect degreasing and chemical conversion treatment properties.

Method used

Introducing hydrophilic functional groups, such as carboxyl, silanol, or amino groups, onto the surface of cold-rolled steel sheets through low-pressure plasma treatment, enhancing wettability and suppressing rust spots without additional oil, while maintaining excellent degreasing and chemical conversion properties.

Benefits of technology

The method effectively prevents spot rust, improves degreasing and chemical conversion treatment properties, and avoids contamination issues associated with traditional rust preventive oils, ensuring high-quality coating adherence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574674000001
    Figure 0007574674000001
  • Figure 0007574674000002
    Figure 0007574674000002
  • Figure 0007574674000003
    Figure 0007574674000003
Patent Text Reader

Abstract

To provide a cold rolled steel sheet including a hydrophilic functional group, suppressed in generation of a point rust.SOLUTION: A cold rolled steel sheet has a hydrophilic functional group on a surface having a molecular ratio to an Fe atom of 0.20 or more and an oxide film having an automatic reduction time of 40 seconds or more, the hydrophilic functional group being selected from a carboxyl group, a silanol group, and an amino group. A manufacturing method of the cold rolled steel sheet having a hydrophilic functional group on a surface performs plasma irradiation for the cold rolled steel sheet in a reduced-pressure atmosphere at a pressure of 1 Pa or more and 100 Pa or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cold-rolled steel sheet having hydrophilic functional groups on its surface, in particular to a cold-rolled steel sheet having hydrophilic functional groups on its surface, which is suppressed from generating rust spots and has excellent degreasing and chemical conversion properties. The present invention also relates to a method for producing the cold-rolled steel sheet having hydrophilic functional groups on its surface. [Background technology]

[0002] Cold-rolled steel sheets have excellent workability and excellent surface quality, and are therefore used in a variety of applications, such as automobiles, electrical appliances, and building materials.

[0003] For example, cold-rolled steel sheets used as steel sheets for automobiles are processed into a desired shape by press forming, and then degreased, chemically treated, and painted by a method such as cationic electrodeposition coating to form a product. Cold-rolled steel sheets for other uses than automobiles are also generally degreased, chemically treated, and painted in the same manner.

[0004] Therefore, cold-rolled steel sheets are required to be able to be degreased, chemically treated, and then painted normally.

[0005] However, even in the short period between immediately after the production of the cold-rolled steel sheet and its use for chemical conversion treatment or the like by automobile manufacturers or other customers, spot-like initial rust (hereinafter referred to as "spot rust") may occur on the surface of the cold-rolled steel sheet.

[0006] When rust spots occur on the surface of a cold-rolled steel sheet, a chemical conversion coating cannot be formed on that portion, resulting in a defect. In addition, in the portion on which the chemical conversion coating is not formed, adhesion to the paint film formed in the subsequent painting cannot be ensured. For this reason, various techniques have been proposed to prevent the occurrence of rust spots on cold-rolled steel sheets.

[0007] For example, Patent Document 1 proposes that in order to prevent the occurrence of rust spots, a cold-rolled steel sheet is subjected to continuous annealing under specific conditions, and then treated with an acidic aqueous solution to form a P-containing coating on the surface of the cold-rolled steel sheet.

[0008] Moreover, Patent Document 2 proposes removing the oxide film formed in the continuous annealing process by pickling, and then rinsing with water to regenerate the oxide film.

[0009] On the other hand, Patent Document 3 proposes forming an oxide film on the surface of a cold-rolled steel sheet in order to prevent the occurrence of an interference color called "blue color" during chemical conversion treatment. Specifically, the cold-rolled steel sheet after continuous annealing is brought into contact with an alkaline aqueous solution, and then washed with water and dried to form an oxide film on the surface of the cold-rolled steel sheet. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2007-084868 A [Patent Document 2] JP 2004-269919 A [Patent Document 3] JP 2014-005522 A Summary of the Invention [Problem to be solved by the invention]

[0011] The technology proposed in Patent Document 1 aims to ensure rust prevention in an uncoated state where no rust-preventive oil is applied in order to omit the degreasing process. However, it is common for cold-rolled steel sheets to be coated with rust-preventive oil for initial rust prevention at the time of shipment. Patent Document 1 does not take into consideration the prevention of spot rust occurrence in a state where rust-preventive oil is applied.

[0012] Since anti-rust oil itself has an anti-rust effect, applying the anti-rust oil can suppress the occurrence of rust spots to a certain extent. However, depending on the circumstances of distribution and the operation status of the customer's production line, cold-rolled steel sheets may be stored for a certain period of time with anti-rust oil or press oil applied, and in such cases, it is difficult to prevent the occurrence of rust spots with only anti-rust oil or press oil. Furthermore, with the recent global warming and the increase in exports to hot and humid regions, the problem of rust spots occurring even in cold-rolled steel sheets applied with anti-rust oil has become apparent.

[0013] Although the rust prevention effect can be improved by increasing the amount of anti-rust oil applied, degreasing becomes difficult when the amount of anti-rust oil applied is increased. Therefore, there is a demand for a method to prevent the occurrence of rust spots without increasing the amount of anti-rust oil applied.

[0014] In addition, in the technology proposed in Patent Document 1, a P-containing film is formed on the surface of a cold-rolled steel sheet. Therefore, there is a concern that P may be released from the film during a degreasing process or the like, contaminating the production line. There is also a concern that P remaining on the steel sheet surface after the degreasing process may affect the formation of phosphate crystals in the chemical conversion treatment process.

[0015] In addition, the technology proposed in Patent Document 2 can suppress the occurrence of rust spots by regenerating an oxide film by washing with water. However, in the method described in Patent Document 2, in order to enhance the rust spot suppression effect, it is necessary to increase the thickness of the oxide film, and increasing the thickness of the oxide film reduces the chemical conversion treatability (see Figure 2 in Patent Document 2).

[0016] Thus, prevention of rust spot formation and improvement of degreasing ability and chemical conversion treatability are contradictory issues, and it has been difficult to achieve both at a high level.

[0017] Furthermore, the technology proposed in Patent Document 3 is merely for forming an oxide film to prevent the occurrence of interference colors during chemical conversion treatment, and does not take into consideration chemical conversion treatability in the general sense, nor does it consider the prevention of rust spots or the improvement of degreasing properties.

[0018] The present invention has been made in consideration of the above circumstances, and has an object to provide a cold-rolled steel sheet in which the occurrence of rust spots is suppressed and which has both excellent degreasing properties and chemical conversion treatability. [Means for solving the problem]

[0019] As a result of investigations conducted by the inventors to solve the above problems, they discovered that by subjecting a cold-rolled steel sheet to a reduced pressure plasma treatment and introducing hydrophilic functional groups onto the surface of the cold-rolled steel sheet, it is possible to prevent the occurrence of rust spots without increasing the amount of rust-preventive oil applied, and also to obtain excellent degreasing properties and chemical conversion properties.

[0020] The present invention has been completed based on these findings, and the gist of the present invention is as follows.

[0021] 1. A cold-rolled steel sheet having a hydrophilic functional group on its surface, A cold-rolled steel sheet having hydrophilic functional groups on its surface, the molar ratio of the hydrophilic functional groups to Fe atoms on the surface of the cold-rolled steel sheet being 0.20 or more.

[0022] 2. The cold-rolled steel sheet having hydrophilic functional groups on its surface as described in 1 above, in which the self-reduction time of the oxide film is 40 seconds or more.

[0023] 3. The cold-rolled steel sheet having a hydrophilic functional group on its surface according to 1 or 2 above, wherein the hydrophilic functional group is at least one selected from a carboxyl group, a silanol group, and an amino group.

[0024] 4. A method for producing a cold-rolled steel sheet having hydrophilic functional groups on its surface, comprising irradiating the cold-rolled steel sheet with plasma in a reduced pressure atmosphere having a pressure of 1 Pa or more and 100 Pa or less.

[0025] 5. The method for producing a cold-rolled steel sheet having hydrophilic functional groups on its surface according to 4 above, wherein the reduced pressure atmosphere contains at least one selected from the group consisting of CO, CO2, and N2 in a total amount of 5 volume % or more.

[0026] 6. The method for producing a cold-rolled steel sheet having hydrophilic functional groups on its surface according to 4 or 5 above, wherein the plasma irradiation generates plasma using an AC voltage.

[0027] 7. The method for producing a cold-rolled steel sheet having hydrophilic functional groups on the surface thereof according to any one of the above 4 to 6, wherein the plasma voltage is 500V or more and 4000V or less. Effect of the Invention

[0028] According to the present invention, the occurrence of rust spots on a cold-rolled steel sheet can be prevented without increasing the amount of anti-rust oil applied. The cold-rolled steel sheet having hydrophilic functional groups of the present invention does not cause rust spots even when stored in a state before chemical conversion treatment or painting is applied. In addition, the cold-rolled steel sheet having hydrophilic functional groups of the present invention has both excellent degreasing properties and chemical conversion treatability. In addition, since the desired effect can be obtained by forming hydrophilic functional groups on the surface of the cold-rolled steel sheet in the present invention, there is no need to form a P-containing film that may cause contamination as in the technology proposed in Patent Document 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Next, a method for carrying out the present invention will be specifically described. Note that the following description shows a preferred embodiment of the present invention, and the present invention is not limited to the following description in any way.

[0030] In one embodiment of the present invention, the cold-rolled steel sheet having hydrophilic functional groups is prevented from generating rust spots by introducing hydrophilic functional groups into the surface. This is believed to be due to the following mechanism.

[0031] That is, by introducing a hydrophilic functional group into the surface of a cold-rolled steel sheet, the wettability of the surface of the cold-rolled steel sheet is improved, and the surface is uniformly wetted. The presence of an interface between the air and moisture (gas-liquid interface) on the surface of the cold-rolled steel sheet plays an important role in the occurrence of initial rust. Therefore, the occurrence of spot rust is prevented by the surface being uniformly wetted. However, the present invention is not limited to the above theory.

[0032] (cold rolled steel plate) Since the effects of the present invention are obtained by hydrophilic functional groups formed on the surface of the cold-rolled steel sheet, the cold-rolled steel sheet is not particularly limited and any cold-rolled steel sheet can be used.

[0033] The cold-rolled steel sheet is not particularly limited, and a cold-rolled steel sheet having any chemical composition can be used. For example, in one embodiment of the present invention, a cold-rolled steel sheet (low carbon steel sheet) made of low carbon steel can be used as the cold-rolled steel sheet. The chemical composition of the cold-rolled steel sheet can optionally contain alloy elements (e.g., Mn) added to improve strength in the production of ordinary low carbon steel sheets, and elements such as Al added as a decarburizing agent. The chemical composition may also contain Si, P, S, etc. as inevitable impurities. The preferred amounts or contents of these elements are as follows. The balance of the chemical composition may be Fe and inevitable impurities, but may also optionally contain other alloy elements.

[0034] C: 0.2% or less C is an element effective for adjusting the strength of steel. From the viewpoint of improving weldability, the C content is preferably set to 0.2% or less.

[0035] Mn:3.0% or less Mn concentrates on the steel sheet surface during continuous annealing to form Mn-based oxides. Since coarse Mn-based oxides take a long time to dissolve, they may not be completely dissolved and remain in the chemical conversion treatment process. However, if the Mn content is 3.0% or less, the formation of coarse Mn-based oxides can be prevented. Therefore, from the viewpoint of further improving the chemical conversion treatment property, it is preferable to set the Mn content to 3.0% or less.

[0036] P:0.05% or less P is an element that impairs weldability, and therefore, from the viewpoint of improving weldability, the P content is preferably set to 0.05% or less.

[0037] S: 0.05% or less S is an unavoidable impurity element. P precipitates as MnS in steel and is a harmful component that reduces the stretch flangeability of the steel sheet. Therefore, from the viewpoint of improving the stretch flangeability, the S content is preferably 0.05% or less.

[0038] Si: 2.0% or less Silicon forms silicon-based oxides on the steel sheet surface during continuous annealing. These silicon-based oxides are poorly soluble in chemical conversion treatment solutions. Therefore, from the viewpoint of further improving chemical conversion treatability, the silicon content is preferably set to 2.0% or less.

[0039] Al: 0.005 to 0.2% Al is an element added as a deoxidizer in the steelmaking process. Furthermore, Al is an element that is effective in separating nonmetallic inclusions that reduce stretch flangeability as slag. Therefore, the Al content is preferably set to 0.01 to 0.15%.

[0040] (molar ratio) The above effect can be obtained if the molar ratio of hydrophilic functional groups to Fe elements on the surface of the cold-rolled steel sheet is 0.20 or more. The molar ratio is preferably 0.50 or more, more preferably 1.0 or more, and even more preferably 3.0 or more. On the other hand, the upper limit of the molar ratio is not particularly limited, but may be, for example, 20.0 or less, or 10.0 or less.

[0041] The molar ratio can be measured by X-ray photoelectron spectroscopy (XPS), specifically, by the method described in the Examples.

[0042] The hydrophilic functional group is not particularly limited and may be any hydrophilic functional group. For example, at least one selected from the group consisting of a carboxyl group (COOH), a carbonyl group (CO), a hydroxyl group (OH), an amino group (NH2), and a silanol group (SiOH) may be used as the hydrophilic functional group.

[0043] (Automatic redemption time) In the cold-rolled steel sheet of the present invention, the presence of an oxide film is also believed to contribute to the prevention of rust spot formation. Therefore, by increasing the stability of the oxide film, the occurrence of rust spots can be further effectively suppressed. Specifically, the automatic reduction time, which is one of the indicators of the stability of the oxide film, is preferably 40 seconds or more. On the other hand, from the viewpoint of further improving the chemical conversion treatability, the automatic reduction time is preferably 80 seconds or less.

[0044] Here, the auto-reduction time is defined as the time corresponding to the inflection point when a cold-rolled steel sheet is immersed in a nitrogen-substituted sodium borate-hydrochloric acid buffer solution of pH 6.65 and the change with time of the natural potential (immersion potential) is measured. The inflection point is the point at which the natural potential of the oxide film changes to the natural potential of the steel, and more specifically, it can be measured by the method described in the Examples.

[0045] [Manufacturing method] Next, a method for producing a cold-rolled steel sheet having hydrophilic functional groups according to another embodiment of the present invention will be described.

[0046] The cold-rolled steel sheet having hydrophilic functional groups of the present invention can be produced by irradiating the cold-rolled steel sheet with plasma in a reduced pressure atmosphere having a pressure of 1 Pa or more and 100 Pa or less. By using a reduced pressure atmosphere, O2 contained in the air can be eliminated.

[0047] (pressure) By performing plasma treatment, hydrophilic functional groups can be introduced into the surface of the cold-rolled steel sheet. However, if the pressure during plasma treatment is less than 1 Pa, the molar ratio of the hydrophilic functional groups on the surface of the cold-rolled steel sheet cannot be sufficiently increased. Therefore, the pressure during plasma treatment is set to 1 Pa or more. On the other hand, if the pressure exceeds 100 Pa, collisions between gas molecules are likely to occur, and as a result, the molar ratio of the hydrophilic functional groups cannot be sufficiently increased. Therefore, the pressure is set to 100 Pa or less.

[0048] The atmosphere in which the plasma treatment is performed is not particularly limited, and can be any atmosphere. From the viewpoint of effectively forming hydrophilic functional groups, the atmosphere preferably contains one or more gases selected from CO, CO2, and N2, and more preferably contains one or more gases selected from CO, CO2, and N2 in a total of 5 volume % or more. When plasma irradiation is performed in an atmosphere containing one or both of CO and CO2, a carboxyl group can be introduced. Also, when plasma irradiation is performed in an atmosphere containing N2, an amino group can be introduced. The atmosphere can further contain a rare gas such as Ar, He, or Ne.

[0049] Moreover, Si can be added to the above atmosphere. By carrying out plasma irradiation in the above reduced pressure atmosphere containing Si, silanol groups, which are hydrophilic functional groups, can be introduced into the surface of the cold rolled steel sheet.

[0050] Addition of Si to the atmosphere can be performed by any method. For example, CO2 gas may be introduced into the chamber after being passed through the Si solution. Alternatively, plasma irradiation may be performed with a Si source (e.g., silicone rubber) placed in the chamber.

[0051] The energy of the plasma treatment is not particularly limited, but by setting it to 50 W or more, carboxyl groups can be introduced more effectively. This is thought to be because by performing plasma treatment with an energy of 50 W or more, the Fe-O bonds of the natural oxide film present on the steel sheet surface are broken, improving the reactivity with CO2 and CO in the atmosphere. Therefore, it is preferable that the energy of the plasma treatment is 50 W or more. On the other hand, if the energy of the plasma treatment is higher than 10,000 W, the introduction of carboxyl groups may not progress. Therefore, it is preferable that the energy of the plasma treatment is 10,000 W or less.

[0052] Although either a DC voltage or an AC voltage can be used to generate the plasma used in the plasma irradiation, it is preferable to use an AC voltage. By using an AC voltage, particularly a high frequency voltage, plasma can be generated more efficiently at a lower voltage than when a DC voltage is used. EXAMPLES

[0053] Example 1 Plasma-treated cold-rolled steel sheets were produced according to the procedure described below, and their properties were evaluated.

[0054] 1. Sample Preparation A cold-rolled steel strip with a tensile strength (TS) of 270 MPa, which is often used for the outer panels of automobiles (doors, roofs, etc.), was annealed in a continuous annealing furnace and then wound into a coil. A number of cold-rolled steel sheets of 70 × 150 mm were cut out from the coil to be used as test materials. The chemical composition of the cold-rolled steel sheet is as shown in Table 1. In the manufacturing process of the cold-rolled steel sheet, a rust-preventive oil (Antirust P-2800, JTXG Energy Corporation) was applied to the surface of the cold-rolled steel sheet in an amount of 1.0 g / m. 2 It was applied with.

[0055] Next, the cold-rolled steel sheet as the test material was degreased to remove the rust-preventive oil applied to the surface of the cold-rolled steel sheet. The degreasing was performed using a solvent.

[0056] Next, the cold-rolled steel sheet was subjected to plasma irradiation under the conditions shown in Table 2. The plasma irradiation was performed using a plasma irradiation device (manufactured by Estec Co., Ltd.). The power during plasma irradiation was 1250 W (2.5 kV x 500 mA) in all examples. However, for comparison, some test pieces were not subjected to plasma irradiation (Nos. 1 and 2).

[0057] 2.Analysis of surface condition The surface condition of each of the obtained cold-rolled steel sheets was analyzed by the following procedure. The measurement results are shown in Table 2.

[0058] Molar ratio of carboxyl groups to Fe atoms The molar ratio of carboxyl groups to Fe atoms on the surface of the cold-rolled steel sheet immediately after plasma irradiation was measured by X-ray photoelectron spectroscopy (XPS). Specifically, a wide-range photoelectron spectrum was first obtained for the qualitative analysis of the outermost surface of the cold-rolled steel sheet, and a narrow-range photoelectron spectrum was obtained to measure the bonding state of the elements detected in the wide-range photoelectron spectrum. Next, the elemental composition ratio (at.%) was calculated from the peak area and relative intensity coefficient in the obtained narrow-range photoelectron spectrum. Furthermore, the narrow-range photoelectron spectrum was subjected to waveform analysis to calculate the ratio of each bonding state of C, N, and O. In the waveform analysis, the background was subtracted by the Shirley method, and then fitting was performed using a Gauss-Lorentz mixed function. Then, the composition ratio by bonding state was obtained from the obtained elemental composition ratio and the result of the waveform analysis. At that time, the molar ratio of carboxyl groups (OC=O) to Fe atoms was calculated as carboxyl groups (OC=O) (at.%) / Fe (at.%).

[0059] The measurements were performed using a PHI 5000Versa Probe III manufactured by ULVAC-PHI. Monochromatic AlKα rays (1486.6 eV) were used as the X-ray source, and measurements were performed with an X-ray beam diameter of 100 μm. For No. 1 and No. 2, which were not exposed to plasma, measurements were performed immediately after removing the rust-preventive oil with a solvent.

[0060] Automatic redemption time To evaluate the stability of the oxide film, the auto-reduction time of the oxide film was measured for the cold-rolled steel sheet immediately after plasma exposure. The cold-rolled steel sheet was immersed in a nitrogen-substituted sodium borate-hydrochloric acid buffer solution of pH 6.65 to measure the time change in natural potential (immersion potential). The time from the start of immersion until the natural potential reached the inflection point was taken as the auto-reduction time (τ value). For No. 1 and 2, which were not exposed to plasma, the measurement was performed immediately after removing the rust-preventive oil with a solvent.

[0061] ·Water droplet contact angle In order to evaluate the wettability of the surface of the cold-rolled steel sheet, the contact angle with water was measured. An automatic contact angle meter SImage AUTO 100 manufactured by Excimer Corporation was used to measure the contact angle. In the measurement, the angle θ1 of the line connecting the left and right end points of the water droplet and the apex with the solid surface was obtained, and the contact angle θ was obtained by doubling this. The measurement was performed under two conditions: immediately after plasma irradiation and after leaving the test piece in the air for one week outdoors without adhesion of dust or water droplets (rainwater).

[0062] 3. Characterization Next, the susceptibility to rust spot formation, degreasing properties, and chemical conversion treatability of each of the obtained cold-rolled steel sheets were evaluated by the following procedures.

[0063] ·Spot rust The surface of the cold-rolled steel sheet having the above hydrophilic functional groups was coated with anti-rust oil (Antirust P2500, Sugimura Chemical Industry Co., Ltd., application amount 1.0 g / m 2 After applying the anti-rust oil, the specimens were left outdoors for one week to avoid the effects of dust and water droplets (rainwater), and then the occurrence of rust spots was examined. The application conditions for the anti-rust oil were a coating amount of 0.5 g / m 2 A light coating of oil and a coating amount of 1.0g / m 2 The number of rust spots that appeared after one week was 1 cm 2 If there were less than 15 hits, it was marked as "○ (pass)", and if there were 15 or more hits, it was marked as "× (fail)".

[0064] - Degreasing and chemical treatment properties Next, in order to evaluate the degreasing property and chemical conversion treatability, the cold-rolled steel sheet used in the above rust spot evaluation after one week was subjected to degreasing, surface conditioning, and chemical conversion treatment. Each of the above treatments was carried out under the following two conditions using a degreaser: FC-E2011, a surface conditioner: PL-X, and a chemical conversion treatment agent: Palbond PB-L3065, all of which are manufactured by Nihon Parkerizing Co., Ltd. <Standard conditions> Degreasing process: Processing temperature 40°C, processing time 120 seconds, spray degreasing Surface conditioning process: pH 9.5, treatment temperature room temperature, treatment time 20 seconds Chemical conversion treatment process: Chemical conversion treatment solution temperature 35℃, treatment time 120 seconds <Short-time conditions> Degreasing process: Processing temperature 40°C, processing time 60 seconds, spray degreasing Surface conditioning process: pH 9.5, treatment temperature room temperature, treatment time 20 seconds Chemical conversion treatment process: Chemical conversion treatment solution temperature 35℃, treatment time 60 seconds

[0065] After the above degreasing step, the steel sheet was spray washed with water and the water-wet area ratio (%) of the steel sheet surface was visually determined. A water-wet area ratio of 80 to 100% was rated as "◯ (pass)" and less than 80% was rated as "× (fail)".

[0066] After the chemical conversion treatment process, the steel sheets were spray-washed and dried, and the surfaces were observed with a scanning electron microscope (accelerating voltage 15 kV, magnification 1000). A state in which the steel sheet base surface was completely covered with phosphate crystals was judged as "good (pass)", and a state in which the steel sheet base surface was exposed in some areas was judged as "bad (pass)".

[0067] As shown in Table 1, in the cold-rolled steel sheet satisfying the conditions of the present invention, the water droplet contact angle was reduced and wettability was improved. Furthermore, even under light oiling conditions where the amount of rust-preventive oil applied was small, the occurrence of rust spots was sufficiently suppressed. In addition, excellent degreasing properties and chemical conversion treatability were obtained under both standard conditions and short-time conditions. Therefore, the cold-rolled steel sheet of the present invention also contributes to shortening the treatment time in a chemical conversion line, and is extremely useful industrially.

[0068] [Table 1]

[0069] [Table 2]

[0070] Example 2 A plasma-treated cold-rolled steel sheet was produced under the same procedures and conditions as in Example 1, except that a Si source was installed in the chamber when performing the plasma treatment, and its characteristics were evaluated. A silicone rubber sheet (SN50, manufactured by Osaka Rubber Co., Ltd.) cut to 20 mm x 100 mm x 1 mm thick was used as the Si source. Specific production conditions and evaluation results are shown in Table 3.

[0071] As mentioned above, by performing plasma irradiation with a Si source installed in the chamber, silanol groups, which are hydrophilic functional groups, are introduced onto the surface of the cold-rolled steel sheet. In this example, CO2 is used as the atmospheric gas, so that carboxyl groups and silanol groups are present as hydrophilic functional groups on the surface of the final cold-rolled steel sheet. Therefore, the molar ratio of the carboxyl groups and the molar ratio of the silanol groups were measured, and the sum was taken as the molar ratio of the hydrophilic functional groups. The molar ratio of the carboxyl groups was measured in the same manner as in Example 1. The molar ratio of the silanol groups was also measured by the following method.

[0072] Molar ratio of silanol groups to Fe atoms The molar ratio of silanol groups introduced onto the surface of cold-rolled steel sheets was measured using a method similar to that used to measure the molar ratio of carboxyl groups. Narrow-range photoelectron spectra of B, N, C, O, and Si were obtained, and the elemental composition ratios were calculated. The molar ratio of silanol groups to Fe atoms was calculated using the obtained Si element ratio.

[0073] [Table 3]

[0074] Example 3 Except for the fact that the plasma treatment was carried out in a 100% nitrogen gas atmosphere, plasma-treated cold-rolled steel sheets were produced under the same procedures and conditions as in Example 1 above, and their properties were evaluated. Specific production conditions and evaluation results are shown in Table 4.

[0075] In this embodiment, since the plasma treatment was performed in a nitrogen gas atmosphere, amino groups were introduced as hydrophilic functional groups to the surface of the cold-rolled steel sheet. In addition, as a result of the measurement, it was found that carboxyl groups were also introduced to the surface of the cold-rolled steel sheet. It is considered that the carboxyl groups originate from CO2 in the air that entered the chamber when the chamber was opened to the atmosphere. Therefore, in this embodiment, the molar ratio of amino groups to Fe atoms and the molar ratio of carboxyl groups to Fe atoms on the surface of the cold-rolled steel sheet were measured, and the sum was taken as the molar ratio of the hydrophilic functional groups. The molar ratio of the carboxyl groups was measured in the same manner as in Example 1 above. In addition, the molar ratio of the amino groups was measured by the following procedure.

[0076] Molar ratio of amino groups to Fe atoms The molar ratio of amino groups introduced onto the surface of the cold-rolled steel sheet was measured using a method similar to that used to measure the molar ratios of carboxyl groups and silanol groups. Narrow-range photoelectron spectra of B, N, C, O, and Si were obtained, and the elemental composition ratios were calculated. The molar ratio of amino groups to Fe atoms was calculated using the obtained N element ratio.

[0077] [Table 4]

[0078] Example 5 In order to confirm the influence of the voltage application method in the plasma treatment, cold-rolled steel sheets were produced under the same procedures and conditions as in Example 1, except that the plasma treatment was carried out at the same voltage using both AC and DC, and the properties of the cold-rolled steel sheets were evaluated. Specific production conditions and evaluation results are shown in Table 5.

[0079] [Table 5]

Claims

1. A cold-rolled steel sheet having a hydrophilic functional group on a surface thereof, the hydrophilic functional group is at least one selected from a carboxyl group, a silanol group, and an amino group; A cold-rolled steel sheet having hydrophilic functional groups on a surface thereof, the molar ratio of the hydrophilic functional groups to Fe atoms on the surface of the cold-rolled steel sheet being 0.20 or more.

2. The cold-rolled steel sheet having hydrophilic functional groups on its surface according to claim 1, wherein the self-reduction time of the oxide film is 40 seconds or more.

3. A method for producing a cold-rolled steel sheet having hydrophilic functional groups on its surface, comprising irradiating the cold-rolled steel sheet with plasma in a reduced pressure atmosphere having a pressure of 1 Pa or more and 100 Pa or less.

4. The reduced pressure atmosphere is 2 , and N 2 The method for producing a cold-rolled steel sheet having hydrophilic functional groups on a surface thereof according to claim 3, wherein the cold-rolled steel sheet contains at least one selected from the group consisting of:

5. The method for producing a cold-rolled steel sheet having hydrophilic functional groups on its surface according to claim 3 or 4, wherein the plasma is generated by using an AC voltage in the plasma irradiation.

6. The method for producing a cold-rolled steel sheet having a hydrophilic functional group on a surface thereof according to any one of claims 3 to 5, wherein the plasma voltage is 500V or more and 4000V or less.

Citation Information

Patent Citations

  • Method of producing cold rolled steel sheet, and cold rolled steel sheet

    JP2004269919A

  • Cold-rolled steel sheet and manufacturing method therefor

    JP2007084868A

  • Manufacturing method of surface-treated cold-rolled steel plate

    JP2010070808A

  • Method of manufacturing cold rolled steel sheet with superior chemical conversion property

    JP2014005522A