Composite modification method for improving corrosion resistance and wear resistance of surface of oil well serial bearing

Through low-temperature plasma nitriding and oxidation treatment, the dense oxide layer is formed, combined with the sealing treatment, and the problems of cumbersome processes and environmental pollution in the bearing surface modification technology are solved, the wear resistance and corrosion resistance of the bearing are improved, and the service life is extended. Suitable for mass production.

CN119040795APending Publication Date: 2024-11-29HARBIN ENG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411174573.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing bearing surface modification technology has problems such as cumbersome process, easy deformation and cracking during service, and environmental pollution, and has little attention to corrosion resistance.

Method used

Low-temperature plasma nitriding treatment (LTPN) and low-temperature oxidation treatment (LTO) composite processes are used to form a dense mixed oxide layer of Fe3O4 phase and Fe2O3 phase, combined with pore sealing treatment, simplify process steps and improve the wear and corrosion resistance of the bearing.

Benefits of technology

It achieves the improvement of bearing surface hardness and wear resistance, while improving corrosion resistance, extending service life, and simplifying production steps, suitable for large-scale industrial production and without environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040795A_ABST
    Figure CN119040795A_ABST
Patent Text Reader

Abstract

The invention discloses a composite modification method for improving corrosion and wear resistance of an oil well serial bearing surface, and relates to a method for improving corrosion and wear resistance of a bearing surface. The problems that an existing bearing surface modification technology is tedious, deformation and cracking occur in the service process, and environmental pollution exists are solved. Through a low-temperature plasma nitriding and low-temperature oxidation composite process, an LTPN treatment modified layer with an epsilon-Fe2-3N phase and a gamma-Fe4N phase as main components and a small amount of nitrogen-containing supersaturated solid solution alpha phase is generated on the surface of the oil well serial bearing; the LTO treatment can generate a compact oxidation layer formed by mixing a Fe3O4 phase and a Fe2O3 phase on the surface of the nitriding bearing, the abrasion resistance of the bearing is maintained or improved, meanwhile, the corrosion resistance of the bearing is further improved, and good toughness is achieved. The composite heat treatment is performed in the same heat treatment furnace, so that the production steps are simplified, the method is suitable for industrial mass production, harmful substances such as cyanate salt are not used, and products in each process are non-toxic and harmless to the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for improving the corrosion and wear resistance of a bearing surface. Background Art

[0002] Chemical heat treatment technologies such as nitriding / nitrocarburizing can improve the hardness and wear resistance of the material surface while retaining its matrix strength and improving the corrosion resistance of the material to a certain extent. The main types include gas nitriding / nitrocarburizing, plasma nitriding / nitrocarburizing and salt bath nitriding / nitrocarburizing.

[0003] Nitriding treatment of bearings can significantly improve their wear resistance and corrosion resistance. Wang Jiawei (Wang Jiawei. Research on microstructure and wear properties of high-performance nitrided bearing steel [D]. Xi'an University of Architecture and Technology, 2013.), Li Lintao (Li Lintao. Research on microstructure, fatigue and friction and wear properties of high-performance nitrided bearing steel [D]. Xi'an University of Architecture and Technology, 2015.) and Guan Chenran et al. (Guan Chenran, Yang Maosheng, Gao Peng. Microstructure and rotary bending fatigue properties of nitrided layer of 32Cr3MoVE bearing steel [J]. Journal of Materials Heat Treatment, 2020, 41(06): 152-159.) conducted nitriding treatment on bearing steel at 530℃-550℃, 30h-3 5h ion nitriding treatment, Zhang Qiang et al. (Zhang Qiang, Sun Shiqing, Yang Maosheng. High stress rolling contact fatigue performance of 32Cr3MoVE nitrided bearing steel [J]. Mechanical Engineering Materials, 2019, 43 (09): 38-42 + 77.) carried out vacuum gas nitriding treatment on bearing steel at 550℃, Yi Cheng (Yi Cheng. Study on the influence of heat treatment on the wear resistance of heavy-load bearing materials [D]. Southwest Petroleum University, 2017.) carried out salt bath nitriding treatment on bearing steel at 570℃ for 2h. After nitriding treatment, the fatigue performance and wear resistance of bearing steel can be effectively enhanced. Based on the surface modification of bearing steel by different methods of nitriding / nitrocarburizing, the researchers also considered the influence of different nitriding parameters (such as temperature, time, atmosphere) on bearing steel. Xiao Yang (Xiao Yang. Microstructure and properties of plasma nitriding layer of M50NiL steel [D]. Harbin Institute of Technology, 2019.) and Wang Xinmin (Wang Xinmin. Research on active screen nitriding process of M50 steel [D]. Harbin Institute of Technology, 2020.) studied the effects of different temperatures, time and nitrogen-hydrogen ratio on the microstructure and properties of nitrided steel surface. The nitrogen-hydrogen ratio has a significant effect on the nitride particle size on the surface of nitrided bearing steel, which will change the nitrided surface morphology; appropriately lowering the nitriding temperature can reduce the generation of vein-like structure, and at higher temperatures, the generation of vein-like structure can be reduced by changing the nitrogen-hydrogen atmosphere to a nitrogen-argon atmosphere. The temperatures selected for the above nitriding processes are all above 500°C, although the hardness and wear resistance of the bearing surface are improved. However, thicker nitriding layers and higher temperatures will lead to reduced toughness of the steel and deformation during the treatment process, as well as changes in the microstructure of the bearing core. Low-temperature plasma nitriding treatment can improve the wear resistance and corrosion resistance of bearings, reduce the thermal diffusion temperature to below 450°C, ensure that the surface hardness and friction and wear resistance of the bearing itself are maintained or improved, and at the same time, improve the corrosion resistance of the bearing, achieve composite modification of bearing wear resistance and corrosion resistance, expand its application range and extend its service life.

[0004] After nitriding / nitrocarburizing treatment, other heat treatment methods can be added to further improve the surface hardness of the nitrided layer, reduce the hardness gradient, fatigue resistance, corrosion resistance and other comprehensive properties. Patent CN109881144A uses salt bath nitrocarburizing-gas phase nitrocarburizing-heat treatment composite treatment on bearing steel, which can significantly reduce the friction coefficient after treatment; Zhang Guosong et al. (Zhang Guosong, Cui Hongzhi, Cheng Guiqin. GCr15 steel gas nitriding + quenching composite treatment and dry friction behavior [J]. China Surface Engineering, 2016, 29 (06): 30-37.) uses gas nitriding + laser quenching treatment on GCr15 bearing steel, which effectively reduces the friction coefficient and improves wear resistance. Composite treatment can further improve the performance of bearing steel, but the process is relatively complicated. The nitriding / nitrocarburizing + oxidation composite treatment technology is a novel chemical heat treatment composite technology, which originated from the QPQ technology. QPQ is a composite process in which the nitriding / nitrocarburizing process is followed by oxidation treatment with an oxygen-containing source, and finally a uniform and dense oxide layer is generated on the nitrided layer. In many production fields, this oxide layer can be used as a wear-resistant and corrosion-resistant coating. Due to the superior properties of the oxide layer, it has gradually attracted people's attention. At present, researchers have explored the nitriding-oxidation composite treatment process of more carbon steel and alloy steel workpieces, and used it as a surface strengthening treatment, but this composite modification technology is less used in the bearing field.

[0005] Zhang Xin et al. (Zhang Xin, Meng Zhengbing, Zhou Ying, et al. Effect of rare earth nitriding on the QPQ salt bath composite treatment performance of 9Cr18Mo steel [J]. Metal Heat Treatment, 2024, 49(03): 63-67.) 9Cr18Mo bearing steel was subjected to salt bath nitriding at 610℃ for 3h and subsequent oxidation treatment at 420℃ for 2h. The corrosion resistance and wear resistance of the bearing steel were enhanced after QPQ treatment. In addition, the addition of rare earth to the molten salt can further improve the performance of the QPQ treated bearing steel. After adding rare earth, the self-corrosion potential of the material increased from -0.2134V to -0-0975V, and the self-corrosion current density increased from 0.62μA / cm 2 Reduced to 0.41μA / cm 2 However, the molten salt used in the salt bath nitriding process has environmental pollution problems.

[0006] After the composite treatment, the use of sealing (such as oil seal) treatment can further improve the wear and corrosion resistance of bearing steel. Du Yingjun (Du Yingjun. Research on the tribological properties of ion nitrided GCr15 bearing steel under dry friction and oil lubrication conditions [D]. China University of Geosciences (Beijing), 2020.) ion nitrided GCr15 bearing steel at 520℃ for 5h. The addition of lubricating oil can further reduce the friction coefficient and wear volume of bearing steel and enhance its anti-wear performance.

[0007] The surface modification technologies used for bearing steel mentioned above are mainly conventional nitriding treatment, post-nitriding heat treatment and QPQ process treatment. Researchers have conducted a relatively detailed study on the wear resistance of bearing steel, but have paid less attention to the corrosion resistance of bearing steel. In addition, the temperature used in conventional nitriding is relatively high, and the white bright layer on the surface after nitriding is relatively thick, which can easily cause deformation and cracking of the surface of the workpiece during service; the post-nitriding heat treatment process is relatively cumbersome and not suitable for large-scale industrial production; although the QPQ treatment technology can improve the performance of bearing steel, molten salts (such as cyanate-based salts) have environmental pollution and other problems; therefore, it is necessary to develop a new, simple, green and environmentally friendly composite treatment technology to improve its surface hardness and obtain good anti-friction and wear performance without affecting corrosion resistance, realize the composite modification of bearing steel wear resistance and corrosion resistance, expand the application range of bearing steel, and extend the service life of bearing steel. Summary of the invention

[0008] In order to solve the problems of complicated process, deformation and cracking during service and environmental pollution in existing bearing surface modification, the present invention proposes a composite modification method for improving the corrosion and wear resistance of the oil well serial bearing surface.

[0009] The composite modification method for improving the corrosion and wear resistance of the surface of the oil well serial bearing of the present invention is carried out according to the following steps:

[0010] Step 1: Degrease and clean the bearing surface;

[0011] Step 2: Plasma cleaning before low-temperature plasma nitriding treatment of the bearing; placing the bearing treated in step 1 into a plasma thermal diffusion device for plasma cleaning to remove the surface passivation film or burrs;

[0012] Step 3: Perform low temperature plasma nitriding (LTPN) on the bearing surface;

[0013] The process of low-temperature plasma nitriding treatment is as follows: in a plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650-750V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is set to 100-400Pa, the plasma nitriding temperature is set to 390-450℃, and the treatment time is set to 4-12h;

[0014] The volume ratio of nitrogen to hydrogen in the nitrogen and hydrogen mixed atmosphere is 1:1-4; after the low-temperature plasma nitriding treatment on the bearing surface, a white bright layer is formed on the bearing surface, and the white bright layer contains ε-Fe 2-3 N phase, γ`-Fe4N phase and nitrogen-supersaturated solid solution α phase, with the white bright layer as the bearing layer;

[0015] Step 4: Low-temperature oxidation treatment (LTO) of the bearing surface: After the low-temperature plasma nitriding treatment in step 3 is completed, the vacuum in the plasma thermal diffusion device is evacuated to below 50Pa, the low-temperature plasma power supply is turned off to stop plasma heating, and then the bearing surface is subjected to low-temperature oxidation treatment; after the low-temperature oxidation treatment of the bearing surface, a dense Fe3O4 phase and Fe2O3 phase mixed oxide layer is generated on the surface of the white bright layer as an anti-corrosion functional layer;

[0016] The process of low-temperature oxidation treatment of the bearing surface is as follows: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is not higher than the plasma nitriding temperature and is within the range of 300 to 450°C, and the time of the low-temperature oxidation treatment is 0.5 to 6 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C with the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing;

[0017] Step 5: seal the bearing after the surface low-temperature oxidation treatment.

[0018] The principles and beneficial effects of the present invention are:

[0019] 1. After low-temperature plasma nitriding treatment on the bearing surface, a thin white bright layer is formed on the bearing surface, which contains ε-Fe 2-3 N phase, γ`-Fe4N phase and nitrogen supersaturated solid solution α phase (α N ) as the bearing layer; the bearing layer can effectively reduce brittleness and has good toughness, while significantly improving the surface hardness and wear resistance of the bearing without reducing or even improving the corrosion resistance of the bearing. After LTO treatment, a dense Fe3O4 phase and Fe2O3 mixed oxide layer is generated on the surface of the white bright layer as an anti-corrosion functional layer; while maintaining or improving the wear resistance of the bearing, the corrosion resistance of the bearing is further improved, and it has good toughness. Due to the high residual compressive stress and microcrack defects after LTPN modification, the bearings treated with LTPN are at risk of deformation or cracking during service. The LTO treatment process can anneal the LTPN modified layer to make the surface low nitrogen compound phase (such as α N Or γ`-Fe4N) decomposes into α-Fe and active nitrogen atoms, α-Fe reacts with O to generate iron oxide, and the active nitrogen atoms continue to diffuse into the bearing, which can effectively eliminate micro stress and reduce or eliminate the brittleness of the LTPN modified layer. Therefore, the modified layer obtained by the method of the present invention has the advantages of wear resistance, corrosion resistance, high toughness, etc., and realizes the composite modification of oil well serial bearings for corrosion resistance and wear resistance, so that the friction coefficient of the bearing is reduced, the wear rate is reduced, the corrosion potential is increased, the corrosion current is reduced, and the corrosion polarization resistance is increased, which significantly improves the wear resistance of the oil well serial bearings while improving their corrosion resistance, and prolongs the service life of the bearings in harsh environments.

[0020] 2. Compared with the composite heat treatment after nitriding / nitrocarburizing, the composite heat treatment of the present invention is carried out in the same heat treatment furnace, which simplifies the production steps and is suitable for industrial mass production.

[0021] 3. Compared with the QPQ process, the present invention does not use harmful substances such as cyanate radical salts, and the products of each process are non-toxic and harmless to the environment;

[0022] 4. The modified material of the present invention is treated with a sealing agent to improve the lubrication effect of the oil well serial bearing and further improve the corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a relationship diagram between the friction coefficient and the sliding time of the bearing surface after treatment in Example 1;

[0024] Figure 2 is a histogram of the wear rate of the bearing surface after treatment in Example 1;

[0025] Figure 3 is a polarization curve diagram of the bearing surface after treatment in Example 1;

[0026] Figure 4 is a surface morphology diagram of the indentation of the bearing surface after treatment in Example 1;

[0027] Figure 5 This is the phase composition analysis diagram (XRD) of the bearing surface after treatment in Example 1. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0029] Specific implementation method 1: The composite modification method for improving the corrosion and wear resistance of the oil well serial bearing surface in this implementation method is carried out according to the following steps:

[0030] Step 1: Degrease and clean the bearing surface;

[0031] Step 2: Plasma cleaning before low-temperature plasma nitriding treatment of the bearing; placing the bearing treated in step 1 into a plasma thermal diffusion device for plasma cleaning to remove the surface passivation film or burrs;

[0032] Step 3: Perform low temperature plasma nitriding (LTPN) on the bearing surface;

[0033] The process of low-temperature plasma nitriding treatment is as follows: in a plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650-750V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is set to 100-400Pa, the plasma nitriding temperature is set to 390-450℃, and the treatment time is set to 4-12h;

[0034] The volume ratio of nitrogen to hydrogen in the nitrogen and hydrogen mixed atmosphere is 1:1-4; after the low-temperature plasma nitriding treatment on the bearing surface, a white bright layer is formed on the bearing surface, and the white bright layer contains ε-Fe 2-3 N phase, γ`-Fe4N phase and nitrogen-supersaturated solid solution α phase, with the white bright layer as the bearing layer;

[0035] Step 4: Low-temperature oxidation treatment (LTO) of the bearing surface: After the low-temperature plasma nitriding treatment in step 3 is completed, the vacuum in the plasma thermal diffusion device is evacuated to below 50Pa, the low-temperature plasma power supply is turned off to stop plasma heating, and then the bearing surface is subjected to low-temperature oxidation treatment; after the low-temperature oxidation treatment of the bearing surface, a dense Fe3O4 phase and Fe2O3 phase mixed oxide layer is generated on the surface of the white bright layer as an anti-corrosion functional layer;

[0036] The process of low-temperature oxidation treatment of the bearing surface is as follows: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is not higher than the plasma nitriding temperature and is within the range of 300 to 450°C, and the time of the low-temperature oxidation treatment is 0.5 to 6 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C with the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing;

[0037] Step 5: seal the bearing after the surface low-temperature oxidation treatment.

[0038] This embodiment has the following beneficial effects:

[0039] 1. After low-temperature plasma nitriding treatment on the bearing surface, a thin white bright layer is formed on the bearing surface, which contains ε-Fe 2-3 N phase, γ`-Fe4N phase and nitrogen supersaturated solid solution α phase (α N) as the bearing layer; the bearing layer can effectively reduce brittleness and has good toughness, while significantly improving the surface hardness and wear resistance of the bearing without reducing or even improving the corrosion resistance of the bearing. After LTO treatment, a dense Fe3O4 phase and Fe2O3 mixed oxide layer is generated on the surface of the white bright layer as an anti-corrosion functional layer; while maintaining or improving the wear resistance of the bearing, the corrosion resistance of the bearing is further improved, and it has good toughness. Due to the high residual compressive stress and microcrack defects after LTPN modification, the bearings treated with LTPN are at risk of deformation or cracking during service. The LTO treatment process can anneal the LTPN modified layer to make the surface low nitrogen compound phase (such as α N Or γ`-Fe4N) decomposes into α-Fe and active nitrogen atoms, α-Fe reacts with O to generate iron oxide, and the active nitrogen atoms continue to diffuse into the bearing, which can effectively eliminate micro stress and reduce or eliminate the brittleness of the LTPN modified layer. Therefore, the modified layer obtained by the method of this embodiment has the advantages of wear resistance, corrosion resistance, high toughness, etc., and realizes the composite modification of oil well serial bearings for corrosion resistance and wear resistance, so that the friction coefficient of the bearing is reduced, the wear rate is reduced, the corrosion potential is increased, the corrosion current is reduced, and the corrosion polarization resistance is increased, which significantly improves the wear resistance of the oil well serial bearings while improving their corrosion resistance, and prolongs the service life of the bearings in harsh environments.

[0040] 2. Compared with the composite heat treatment after nitriding / nitrocarburizing, the composite heat treatment in this embodiment is carried out in the same heat treatment furnace, which simplifies the production steps and is suitable for industrial mass production.

[0041] 3. Compared with the QPQ process, this implementation method does not use harmful substances such as cyanate radical salts, and the products of each process are non-toxic and harmless to the environment;

[0042] 4. The modified embodiment is treated with a sealing agent to improve the lubrication of the oil well serial bearing and further improve the corrosion resistance.

[0043] Specific implementation method 2: The difference between this implementation method and specific implementation method 1 is that the bearing described in step 1 is high-carbon bearing steel or medium-carbon bearing.

[0044] Specific implementation method three: The difference between this implementation method and specific implementation method one or two is that the high carbon bearing steel described in step one is GCr15 steel or M50 steel, etc.

[0045] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that: the medium carbon bearing in step 1 is made of 55SiMoV steel or the like.

[0046] Specific embodiment five: This embodiment differs from any one of specific embodiments one to four in that: the plasma cleaning process described in step two is: evacuating the plasma thermal diffusion device to a vacuum level below 5 Pa, then introducing hydrogen and applying a voltage of 500 to 650 V, and the cleaning time is 15 to 30 minutes.

[0047] Specific implementation method 6: This implementation method is different from any one of specific implementation methods 1 to 5 in that the volume fraction of oxygen in the oxidizing atmosphere in step 4 is 10-30%.

[0048] Specific implementation method 7: This implementation method is different from any one of specific implementation methods 1 to 6 in that: the process of the sealing treatment in step 5 is: soaking the bearing in the sealing agent for 1-5 hours, and then naturally drying it.

[0049] Specific implementation eight: This implementation differs from any one of specific implementations one to seven in that: the sealing agent in step five is anti-rust oil or nano-sealing agent, etc.

[0050] Specific embodiment nine: The difference between this embodiment and any one of specific embodiments one to eight is that: the process of low-temperature plasma nitriding treatment described in step one is: in the plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is 200Pa, the plasma nitriding temperature is 420℃, and the treatment time is 8h.

[0051] Specific embodiment ten: The difference between this embodiment and any one of specific embodiments one to nine is that: the process of low-temperature oxidation treatment of the bearing surface described in step four is: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is 380°C, and the time of the low-temperature oxidation treatment is 2 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C in the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing.

[0052] Embodiment 1:

[0053] The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface in this embodiment is carried out according to the following steps:

[0054] Step 1: Degrease and clean the bearing surface;

[0055] The bearing is made of 55SiMoV steel;

[0056] Step 2: Plasma cleaning before low-temperature plasma nitriding treatment of the bearing; placing the bearing treated in step 1 into a plasma thermal diffusion device for plasma cleaning to remove the surface passivation film or burrs;

[0057] The plasma cleaning process is as follows: the vacuum in the plasma thermal diffusion device is evacuated to below 5 Pa, and then hydrogen is introduced and a voltage of 650 V is applied, and the cleaning time is 30 minutes;

[0058] Step 3: Perform low temperature plasma nitriding (LTPN) on the bearing surface;

[0059] The process of low-temperature plasma nitriding treatment is as follows: in a plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is 200Pa, the plasma nitriding temperature is 420℃, and the treatment time is 8h;

[0060] The volume ratio of nitrogen to hydrogen in the mixed atmosphere of nitrogen and hydrogen is 1:3;

[0061] Step 4: Low-temperature oxidation treatment (LTO) of the bearing surface: After the low-temperature plasma nitriding treatment in step 3 is completed, the vacuum in the plasma thermal diffusion device is evacuated to below 50 Pa, the low-temperature plasma power supply is turned off to stop plasma heating, and then the low-temperature oxidation treatment of the bearing surface is performed;

[0062] The process of low-temperature oxidation treatment of the bearing surface is as follows: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is 380°C, and the time of the low-temperature oxidation treatment is 2 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C with the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing;

[0063] The oxidizing atmosphere is air, and the volume fraction of oxygen is 21%;

[0064] Step 5: sealing the bearing after the surface low-temperature oxidation treatment, and the process is completed;

[0065] The sealing process is as follows: immersing the bearing in the sealing agent for 2 hours and then air-drying it naturally;

[0066] The sealing agent is anti-rust oil.

[0067] The relationship between the friction coefficient and the sliding time of the bearing surface after treatment in Example 1; the average friction coefficient of the sample after treatment is reduced from 0.5394 to 0.2954, which has good anti-friction performance; Figure 2 is a histogram of the wear rate of the bearing surface after treatment in Example 1; the wear rate is 7.9618 on the surface. -10 kg06 -1 1 -1 Reduced to 8.8464 surface -11 kg14 -1 1 -1, has good wear resistance. Figure 3 is the polarization curve of the bearing surface after treatment in Example 1; after the sample was treated with the composite, the sample was immersed in the sealing agent for 2 hours, and the corrosion potential was measured to increase from -0.668V to -0.205V, and the corrosion current density increased from 10.57 to 1.08V. 2 The polarization is reduced to 0.7825 degrees by 2 , the polarization resistance is 2617 and the resistance is 2 Increased to 54328 degrees 2 . Figure 4 This is a surface morphology image of the indentation on the bearing surface after treatment in Example 1. After the load is applied, no large cracks appear at the edge of the indentation. Figure 5 The phase composition analysis diagram (XRD) of the bearing surface after treatment in Example 1 shows that the surface of the workpiece after LTPN treatment is mainly composed of ε 2-3 N phase and γ and 3 workpiece 4N phase, a small amount of α N Phase, after LTO treatment, Fe3O4 phase and Fe2O3 phase are further generated on the workpiece surface.

[0068] Embodiment 2:

[0069] The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface in this embodiment is carried out according to the following steps:

[0070] Step 1: Degrease and clean the bearing surface;

[0071] The bearing is made of 55SiMoV steel;

[0072] Step 2: Plasma cleaning before low-temperature plasma nitriding treatment of the bearing; placing the bearing treated in step 1 into a plasma thermal diffusion device for plasma cleaning to remove the surface passivation film or burrs;

[0073] The plasma cleaning process is as follows: the vacuum in the plasma thermal diffusion device is evacuated to below 5 Pa, and then hydrogen is introduced and a voltage of 650 V is applied, and the cleaning time is 30 minutes;

[0074] Step 3: Perform low temperature plasma nitriding (LTPN) on the bearing surface;

[0075] The process of low-temperature plasma nitriding treatment is as follows: in a plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is set to 200Pa, the plasma nitriding temperature is set to 440℃, and the treatment time is set to 8h;

[0076] The volume ratio of nitrogen to hydrogen in the mixed atmosphere of nitrogen and hydrogen is 1:3;

[0077] Step 4: Low-temperature oxidation treatment (LTO) of the bearing surface: After the low-temperature plasma nitriding treatment in step 3 is completed, the vacuum in the plasma thermal diffusion device is evacuated to below 50 Pa, the low-temperature plasma power supply is turned off to stop plasma heating, and then the low-temperature oxidation treatment of the bearing surface is performed;

[0078] The process of low-temperature oxidation treatment of the bearing surface is as follows: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is 380°C, and the time of the low-temperature oxidation treatment is 2 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C with the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing;

[0079] The oxidizing atmosphere is air, and the volume fraction of oxygen is 21%;

[0080] Step 5: sealing the bearing after the surface low-temperature oxidation treatment, and the process is completed;

[0081] The sealing process is as follows: immersing the bearing in the sealing agent for 2 hours and then air-drying it naturally;

[0082] The sealing agent is a nano-sealing agent, the manufacturer of the nano-sealing agent is Sichuan Xingrongke Technology Co., Ltd., and the model is RK-315N.

[0083] After composite treatment, the average friction coefficient of the material decreased from 0.5394 to 0.2939, and the wear rate decreased from 7.9618×10 -10 kg·N -1 ·m -1 Reduced to 8.8464×10 -11 kg·N -1 ·m -1 The wear resistance and anti-friction properties were improved; the corrosion potential increased from -0.668V to -0.310V, and the corrosion current density increased from 10.57μA / cm 2 Reduced to 2.683μA / cm 2 , the polarization resistance is 2617Ω·cm 2 Increased to 15539Ω·cm 2 , the corrosion resistance is greatly improved.

[0084] Embodiment 3:

[0085] The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface in this embodiment is carried out according to the following steps:

[0086] Step 1: Degrease and clean the bearing surface;

[0087] The bearing is made of 55SiMoV steel;

[0088] Step 2: Plasma cleaning before low-temperature plasma nitriding treatment of the bearing; placing the bearing treated in step 1 into a plasma thermal diffusion device for plasma cleaning to remove the surface passivation film or burrs;

[0089] The plasma cleaning process is as follows: the vacuum in the plasma thermal diffusion device is evacuated to below 5 Pa, and then hydrogen is introduced and a voltage of 650 V is applied, and the cleaning time is 30 minutes;

[0090] Step 3: Perform low temperature plasma nitriding (LTPN) on the bearing surface;

[0091] The process of low-temperature plasma nitriding treatment is as follows: in a plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is set to 200Pa, the plasma nitriding temperature is set to 440℃, and the treatment time is set to 8h;

[0092] The volume ratio of nitrogen to hydrogen in the mixed atmosphere of nitrogen and hydrogen is 1:3;

[0093] Step 4: Low-temperature oxidation treatment (LTO) of the bearing surface: After the low-temperature plasma nitriding treatment in step 3 is completed, the vacuum in the plasma thermal diffusion device is evacuated to below 50 Pa, the low-temperature plasma power supply is turned off to stop plasma heating, and then the low-temperature oxidation treatment of the bearing surface is performed;

[0094] The process of low-temperature oxidation treatment of the bearing surface is as follows: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is 440°C, and the time of the low-temperature oxidation treatment is 2 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C in the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing;

[0095] The oxidizing atmosphere is air, and the volume fraction of oxygen is 21%;

[0096] Step 5: sealing the bearing after the surface low-temperature oxidation treatment, and the process is completed;

[0097] The sealing process is as follows: immersing the bearing in the sealing agent for 2 hours and then air-drying it naturally;

[0098] The sealing agent is a nano sealing agent.

[0099] After composite treatment, the average friction coefficient of the sample decreased from 0.5394 to 0.2937, and the wear rate decreased from 7.9618×10 -10 kg·N -1 ·m -1 Reduced to 1.7963×10 -10kg·N -1 ·m -1 The wear resistance and anti-friction properties were improved; the corrosion potential increased from -0.668V to -0.285V, and the corrosion current density increased from 10.57μA / cm 2 Reduced to 2.852μA / cm 2 , the polarization resistance is 2617Ω·cm 2 Increased to 15735Ω·cm 2 , the corrosion resistance is greatly improved.

[0100] Embodiment 4:

[0101] The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface in this embodiment is carried out according to the following steps:

[0102] Step 1: Degrease and clean the bearing surface;

[0103] The bearing is made of 55SiMoV steel;

[0104] Step 2: Plasma cleaning before low-temperature plasma nitriding treatment of the bearing; placing the bearing treated in step 1 into a plasma thermal diffusion device for plasma cleaning to remove the surface passivation film or burrs;

[0105] The plasma cleaning process is as follows: the vacuum in the plasma thermal diffusion device is evacuated to below 5 Pa, and then hydrogen is introduced and a voltage of 650 V is applied, and the cleaning time is 30 minutes;

[0106] Step 3: Perform low temperature plasma nitriding (LTPN) on the bearing surface;

[0107] The process of low-temperature plasma nitriding treatment is as follows: in a plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is 200Pa, the plasma nitriding temperature is 420℃, and the treatment time is 8h;

[0108] The volume ratio of nitrogen to hydrogen in the mixed atmosphere of nitrogen and hydrogen is 1:3;

[0109] Step 4: Low-temperature oxidation treatment (LTO) of the bearing surface: After the low-temperature plasma nitriding treatment in step 3 is completed, the vacuum in the plasma thermal diffusion device is evacuated to below 50 Pa, the low-temperature plasma power supply is turned off to stop plasma heating, and then the low-temperature oxidation treatment of the bearing surface is performed;

[0110] The process of low-temperature oxidation treatment of the bearing surface is as follows: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is within the range of 400°C, and the time of the low-temperature oxidation treatment is 2 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C with the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing;

[0111] The oxidizing atmosphere is air, and the volume fraction of oxygen is 21%;

[0112] Step 5: sealing the bearing after the surface low-temperature oxidation treatment, and the process is completed;

[0113] The sealing process is as follows: immersing the bearing in the sealing agent for 2 hours and then air-drying it naturally;

[0114] The sealing agent is a nano sealing agent.

[0115] After composite treatment, the average friction coefficient of the sample decreased from 0.5394 to 0.3593, and the wear rate decreased from 7.9618×10 -10 kg·N -1 ·m -1 Reduced to 1.7963×10 -10 kg·N -1 ·m -1 The wear resistance and anti-friction properties were improved; the corrosion potential increased from -0.668V to -0.339V, and the corrosion current density increased from 10.57μA / cm 2 Reduced to 1.779μA / cm 2 , the polarization resistance is 2617Ω·cm 2 Increased to 19366Ω·cm 2 , the corrosion resistance is greatly improved.

[0116] Embodiment 5:

[0117] The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface in this embodiment is carried out according to the following steps:

[0118] Step 1: Degrease and clean the bearing surface;

[0119] The bearing is made of 55SiMoV steel;

[0120] Step 2: Plasma cleaning before low-temperature plasma nitriding treatment of the bearing; placing the bearing treated in step 1 into a plasma thermal diffusion device for plasma cleaning to remove the surface passivation film or burrs;

[0121] The plasma cleaning process is as follows: the vacuum in the plasma thermal diffusion device is evacuated to below 5 Pa, and then hydrogen is introduced and a voltage of 650 V is applied, and the cleaning time is 30 minutes;

[0122] Step 3: Perform low temperature plasma nitriding (LTPN) on the bearing surface;

[0123] The process of low-temperature plasma nitriding treatment is as follows: in a plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is 200Pa, the plasma nitriding temperature is 420℃, and the treatment time is 8h;

[0124] The volume ratio of nitrogen to hydrogen in the mixed atmosphere of nitrogen and hydrogen is 1:3;

[0125] Step 4: Low-temperature oxidation treatment (LTO) of the bearing surface: After the low-temperature plasma nitriding treatment in step 3 is completed, the vacuum in the plasma thermal diffusion device is evacuated to below 50 Pa, the low-temperature plasma power supply is turned off to stop plasma heating, and then the low-temperature oxidation treatment of the bearing surface is performed;

[0126] The process of low-temperature oxidation treatment of the bearing surface is as follows: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is 420°C, and the time of the low-temperature oxidation treatment is 2 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C with the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing;

[0127] The oxidizing atmosphere is air, and the volume fraction of oxygen is 21%;

[0128] Step 5: sealing the bearing after the surface low-temperature oxidation treatment, and the process is completed;

[0129] The sealing process is as follows: immersing the bearing in the sealing agent for 2 hours and then air-drying it naturally;

[0130] The sealing agent is a nano sealing agent.

[0131] After composite treatment, the average friction coefficient of the sample decreased from 0.5394 to 0.4171, and the wear rate decreased from 7.9618×10 -10 kg·N -1 ·m -1 Reduced to 2.6539×10 -10 kg·N -1 ·m -1 The wear resistance and anti-friction properties were improved; the corrosion potential increased from -0.668V to -0.350V, and the corrosion current density increased from 10.57μA / cm 2Reduced to 1.131μA / cm 2 , the polarization resistance is 2617Ω·cm 2 Increased to 20034Ω·cm 2 , the corrosion resistance is greatly improved.

Claims

1. A composite modification method for improving the corrosion and wear resistance of the surface of oil well serial bearings. Features: The composite modification method for improving the corrosion and wear resistance of the oil well serial bearing surface is carried out in the following steps: Step 1: Degrease and clean the bearing surface; Step 2: Plasma cleaning of the bearing before low-temperature plasma nitriding treatment; Step 3: Perform low temperature plasma nitriding (LTPN) on the bearing surface; The process of low-temperature plasma nitriding treatment is as follows: in a plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650-750V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is set to 100-400Pa, the plasma nitriding temperature is set to 390-450°C, and the treatment time is set to 4-12h; The volume ratio of nitrogen to hydrogen in the mixed atmosphere of nitrogen and hydrogen is 1:1-4; Step 4: Low-temperature oxidation treatment (LTO) of the bearing surface: After the low-temperature plasma nitriding treatment in step 3 is completed, the vacuum in the plasma thermal diffusion device is evacuated to below 50 Pa, the low-temperature plasma power supply is turned off to stop plasma heating, and then the low-temperature oxidation treatment of the bearing surface is performed; The process of low-temperature oxidation treatment of the bearing surface is as follows: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is not higher than the plasma nitriding temperature and is within the range of 300 to 450° C., and the time of the low-temperature oxidation treatment is 0.5 to 6 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200° C. with the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing; Step 5: seal the bearing after the surface low-temperature oxidation treatment.

2. The composite modification method for improving the corrosion and wear resistance of the surface of oil well serial bearings according to claim 1, Features: The bearing described in step 1 is high carbon bearing steel or medium carbon bearing.

3. The composite modification method for improving the corrosion and wear resistance of the surface of oil well serial bearings according to claim 1, Features: The high carbon bearing steel in step 1 is GCr15 steel or M50 steel.

4. The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface according to claim 1, Features: The medium carbon bearing described in step 1 is 55SiMoV steel.

5. The composite modification method for improving the corrosion and wear resistance of the surface of oil well serial bearings according to claim 1, Features: The plasma cleaning process in step 2 is as follows: the vacuum in the plasma thermal diffusion device is evacuated to below 5 Pa, and then hydrogen is introduced and a voltage of 500 to 650 V is applied, and the cleaning time is 15 to 30 minutes.

6. The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface according to claim 1, Features: The oxygen volume fraction in the oxidizing atmosphere in step 4 is 10-30%.

7. The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface according to claim 1, Features: The sealing process in step 5 is as follows: immerse the bearing in the sealing agent for 1-5 hours, and then allow it to dry naturally.

8. The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface according to claim 1, Features: The sealing agent in step 5 is anti-rust oil or nano-sealing agent.

9. The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface according to claim 1, Features: The process of low-temperature plasma nitriding treatment in step 1 is: in the plasma thermal diffusion device, the low-temperature plasma power supply voltage is set to 650V, the working atmosphere is a mixed atmosphere of nitrogen and hydrogen, the working gas pressure is 200Pa, the plasma nitriding temperature is 420°C, and the treatment time is 8h.

10. The composite modification method for improving the corrosion resistance and wear resistance of the oil well serial bearing surface according to claim 1, Features: The process of low-temperature oxidation treatment of the bearing surface described in step 4 is: the atmosphere of the low-temperature oxidation treatment is an oxidizing atmosphere, the temperature of the low-temperature oxidation treatment is 380°C, and the time of the low-temperature oxidation treatment is 2 hours; after the low-temperature oxidation treatment is completed, the gas supply is stopped, the vacuum is drawn, and the power is turned off; after the bearing is cooled to below 200°C in the furnace, it is taken out to obtain a low-temperature plasma nitriding-low-temperature oxidation composite modified bearing.

Citation Information

Cited By

  • Plasma nitrogen oxidation composite treatment process method for piston rod of hydraulic oil cylinder

    CN121204599A

  • A plasma nitride-oxide composite treatment process method for a hydraulic cylinder piston rod

    CN121204599B