Metal particle-containing composition, joining paste, joined body, and method for producing joined body
A metal particle-containing composition with polyvalent fatty acids and polyamines addresses the issues of bonding strength and printability in high-temperature applications, ensuring stable bonding and durability under thermal cycles.
Patent Information
- Application Number
- JP2021161128
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-22
- Filing Date
- 2021-09-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-09-30
AI Technical Summary
Existing bonding materials for high-temperature applications, such as those used in next-generation power electronics, suffer from poor bonding strength due to void formation and degradation under cooling and heating cycles, and have issues with fluidity and printing suitability when high concentrations of metal particles are used.
A metal particle-containing composition comprising metal particles with specific diameters, polyvalent fatty acids, and polyamines, which form a bonding paste that maintains high bonding strength and fluidity, allowing for effective printing and resistance to thermal cycles.
The composition provides a bonding paste with high bonding strength that remains stable under long-term thermal cycles and allows for excellent printability even at high metal particle concentrations, resulting in a strong and durable joined body.
Smart Images

Figure 0007574773000001 
Figure 0007574773000002 
Figure 0007574773000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal particle-containing composition, a bonding paste, a bonded body, and a method for producing the bonded body. [Background technology]
[0002] Conventionally, solder has been used as a bonding material for bonding metal members together, between a metal member and a semiconductor element, between a metal member and a light-emitting diode (LED) element, etc. In recent years, in the technical field of next-generation power electronics, devices such as SiC capable of operating at high temperatures are in demand. As a bonding material for manufacturing such devices, a substitute material for solder is in demand from the viewpoint of high-temperature operation reliability, and for example, bonding materials such as bonding pastes using metal particles having sinterability as shown in Patent Documents 1 to 4 have been proposed.
[0003] Patent Document 1 discloses a bonding material containing metal submicron particles with an average primary particle size of 0.5 to 3.0 μm and metal nanoparticles with an average primary particle size of 1 to 200 nm that are coated with an organic compound having 6 to 8 carbon atoms. However, there is a problem in that the bonding strength at the bonded portion is poor, and the bonding strength decreases with thermal cycles.
[0004] Patent Document 2 discloses a bonding material containing silver nanoparticles having an average primary particle size of 1 to 200 nm and coated with an organic substance having 8 or less carbon atoms, and a flux component having at least two carboxyl groups. Patent Document 3 discloses a bonding material containing silver fine particles having an average primary particle size of 130 nm or less, and a cross-linked interparticle distance-maintaining agent that maintains the distance between the silver fine particles.
[0005] Patent Document 4 discloses a bonding material that contains metal particles including metal nanoparticles having an average particle size of 2 to 200 nm, a specific polyamide having a phenolic hydroxyl group in a side chain and a hydrocarbon group having 20 to 60 carbon atoms, and a tri- or higher functional compound that can react with the phenolic hydroxyl group.
[0006] However, the bonding materials described in Patent Documents 1 to 4 have the problem that defects such as voids (air gaps) are formed in the bonding portion, so that the strength of the bonded portion is poor and the bonding strength decreases with thermal cycles. Furthermore, when a bonding paste containing a high concentration of silver nanoparticles is prepared to achieve a dense and strong bond, the fluidity is significantly reduced. As a result, there are problems in that the printed portion is smudged or a portion that cannot be coated is generated (a non-coated portion is formed) in the process of printing the bonding paste on the bonded portion. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2011-80147 A [Patent Document 2] JP 2011-240406 A [Patent Document 3] JP 2018-109232 A [Patent Document 4] JP 2017-137375 A Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, the problem to be solved by the present invention is to provide a metal particle-containing composition that has high bonding strength at the bonded portion and suppresses the decrease in bonding strength due to thermal cycling. In addition to the above characteristics, the present invention is to provide a bonding paste that has excellent printability for the bonded portion even if it contains metal particles at a high concentration. Furthermore, the present invention is to provide a bonded body that does not deteriorate due to long-term thermal cycling of 1000 cycles or more. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention relates to a metal particle-containing composition comprising metal particles (A) having an average particle size of 1 nm to 1000 nm, a polyvalent fatty acid (B), and a polyamine (C).
[0010] The present invention also relates to the metal particle-containing composition, wherein the polyvalent fatty acid (B) has 20 to 80 carbon atoms and the polyamine (C) has 20 to 80 carbon atoms.
[0011] The present invention also relates to the above metal particle-containing composition, wherein the polyvalent fatty acid (B) contains a divalent and / or trivalent fatty acid.
[0012] The present invention also relates to the metal particle-containing composition, wherein the polyamine (C) contains a diamine and / or a triamine.
[0013] The present invention also relates to the metal particle-containing composition, wherein the polyvalent fatty acid (B) and / or the polyamine (C) have a branched and / or cyclic structure.
[0014] The present invention also relates to the above metal particle-containing composition, in which the polyvalent fatty acid (B) has a hydrocarbon group (D) with a valence of m, or the polyamine (C) has a hydrocarbon group (E) with a valence of n, where m is the valence of the polyvalent fatty acid (B) and n is the valence of the polyamine (C).
[0015] The present invention also relates to the above metal particle-containing composition, wherein the m-valent hydrocarbon group (D) and / or the n-valent hydrocarbon group (E) have 30-60 carbon atoms.
[0016] The present invention also relates to the above metal particle-containing composition, which contains 0.05 to 1 part by mass of polyvalent fatty acid (B) and / or 0.05 to 1 part by mass of polyamine (C) per 100 parts by mass of metal particles (A).
[0017] The present invention also relates to the metal particle-containing composition, which contains 0.1 to 0.5 parts by mass of polyvalent fatty acid (B) and / or 0.1 to 0.5 parts by mass of polyamine (C) per 100 parts by mass of metal particles (A).
[0018] The present invention also relates to the metal particle-containing composition, wherein the metal particles (A) have an average particle size of 180 nm to 400 nm.
[0019] The present invention also relates to the metal particle-containing composition, wherein the metal particles (A) have an average particle size of 200 nm to 300 nm.
[0020] The present invention also relates to a bonding paste containing the above metal particle-containing composition and a dispersion medium (F).
[0021] The present invention also relates to the above bonding paste, in which the proportion of the mass of the metal particles (A) to the sum of the masses of the metal particles (A), the polyvalent fatty acid (B), the polyamine (C) and the dispersion medium (F) is 80 mass% to 95 mass%.
[0022] The present invention also relates to a bonded body in which a first bonded part and a second bonded part are bonded via a bonding layer, the bonding layer being a layer formed from the above-mentioned bonding paste.
[0023] The present invention also relates to a method for producing a bonded body in which a first bonded part and a second bonded part are bonded via a bonding layer, the method comprising the steps of applying a bonding paste to the first bonded part, the bonding paste containing metal particles (A) having an average particle diameter of 1 nm to 1000 nm, a polyvalent fatty acid (B), a polyamine (C), and a dispersion medium (F), placing the second bonded part on the bonding paste, and sintering the resulting product. Effect of the Invention
[0024] The present invention provides a metal particle-containing composition that provides high bonding strength at the bonded portion and does not decrease with long-term thermal cycles, and a bonding paste that has these effects and is also excellent in printability. It also provides a bonded body that does not deteriorate with thermal cycles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The metal particle-containing composition of the present invention contains metal particles (A) having an average particle size of 1 nm to 1000 nm, a polyvalent fatty acid (B), and a polyamine (C). The bonding paste of the present invention contains a dispersion medium (F) in addition to the metal particle-containing composition. The metal particle-containing composition may be formed by volatilizing a part or all of the dispersion medium (F) from the bonding paste during the bonding process. In this specification, "metal particles (A) having an average particle size of 1 nm to 1000 nm" may be abbreviated as "metal particles (A)".
[0026] The metal particles (A) are within a specific average particle size range, so that when heated or sintered, the particles melt or bond together (hereinafter also referred to as sintering) and change into bulk metal. As a result, the parts to be joined can be joined together. Hereinafter, the part formed by sintering the metal particle-containing composition present between the parts to be joined is referred to as the joining layer.
[0027] In addition, since the bonding paste of the present invention contains polyhydric fatty acid (B) and polyamine (C), a bonding layer with fewer defects such as voids (air gaps) is obtained during sintering, so it is presumed that the bonding strength of the bonded parts is high and the decrease in bonding strength is suppressed even after long-term thermal cycles.
[0028] The temperature for sintering the metal particle-containing composition or the bonding paste is not particularly limited, but is generally sintered at 200°C to 350°C. By sintering, dehydration condensation of the polyvalent fatty acid (B) and the polyamine (C) occurs, and in the later stage of the sintering time, polyamide is formed in the bonding layer by dehydration condensation of the polyvalent fatty acid (B) and the polyamine (C). Therefore, even if organic matter remains in the manufactured bonding layer, it is considered that volatilization is suppressed by polymerization, and heat resistance is improved. As a result, it is considered that the decrease in bonding strength due to long-term thermal cycle testing is suppressed.
[0029] <Metal particles (A)> Examples of the metal in the metal particles (A) include gold, silver, copper, nickel, chromium, palladium, rhodium, ruthenium, indium, silicon, aluminum, tungsten, molybdenum, platinum, and alloys thereof. In addition, fine particles coated with a core and a material different from the core material, specifically, for example, silver-coated copper powder, in which the core is copper and the surface is coated with silver, can be mentioned. In addition, powders of metal oxides such as silver oxide, indium oxide, tin oxide, zinc oxide, ruthenium oxide, ITO (tin-doped indium oxide), AZO (aluminum-doped zinc oxide), and GZO (gallium-doped zinc oxide), as well as powders surface-coated with these metal oxides can be mentioned. The type of metal used may be one type, or two or more types may be used in combination.
[0030] The metal particles (A) are preferably selected from copper or silver, since a bonded body having particularly excellent strength can be obtained.Moreover, the metal particles (A) are more preferably silver, since it can be used at a wide range of firing temperatures and in various firing environments, such as under atmospheric pressure, in a nitrogen atmosphere, in a vacuum, or in a reducing atmosphere.
[0031] In the present invention, it is important to use metal particles (A) having a specific average particle size. In this specification, the term "average particle size" means the 50% cumulative particle size distribution particle size (d50) on a volume basis determined by the measurement method described in the Examples. The d50 of the metal particles (A) is 1 to 1000 nm, preferably 180 to 400 nm, and more preferably 200 to 300 nm.
[0032] The metal particles (A) are preferably coated on the surface with an organic component (a). When the metal particles (A) are coated with the organic component (a), it is expected that the storage stability of the metal particle-containing composition and the bonding paste is increased. Examples of the organic component (a) include fatty acids, aliphatic amines, and aliphatic alcohols, and the organic component (a) is preferably a saturated or unsaturated fatty acid, more preferably a saturated or unsaturated fatty acid having 3 to 18 carbon atoms, and even more preferably a saturated or unsaturated fatty acid having 6 to 18 carbon atoms. The organic component (a) may contain one or more types.
[0033] The metal particles (A) may be used alone or in combination. If necessary, metal particles other than the metal particles (A) may be used in combination. In that case, it is preferable to use metal particles having an average particle size of more than 1000 nm in combination.
[0034] <Polyvalent fatty acids (B)> Next, the polyvalent fatty acid (B) will be described. The polyvalent fatty acid (B) refers to a compound having a plurality of carboxy groups in the molecule and having a hydrocarbon as a basic skeleton. The number of carbon atoms in the polyvalent fatty acid (B) is preferably 20 to 80. The number of carbon atoms in the polyvalent fatty acid (B) includes the carboxy carbon in the molecule as the number of carbon atoms in the polyvalent fatty acid (B).
[0035] The polyvalent fatty acid (B) is believed to have the effect of maintaining the metal particle-containing composition in a fluid liquid state during sintering, and is presumed to increase the wettability at the bonding interface with the bonded parts. Therefore, even if voids are generated in the bonding layer, it is believed that the polyvalent fatty acid (B) will flow into the defective parts, making it possible to obtain a bonding layer with few defects and high bonding strength.
[0036] The state of the polyvalent fatty acid (B) is not particularly limited, but it is preferably liquid in the normal temperature range of 200° C. to 350° C. in which the metal particle-containing composition of the present invention is usually fired. The polyvalent fatty acid (B) may be solid or liquid at room temperature (25° C.), but is more preferably liquid at room temperature in that it can be uniformly dispersed in the metal particle-containing composition and act effectively.
[0037] The valence of the polyvalent fatty acid (B), ie, the number of carboxy groups, is preferably two or three.
[0038] The polyvalent fatty acid (B) may have a linear structure or a branched and / or cyclic structure, but preferably has a branched and / or cyclic structure. When it has a branched and / or cyclic structure, it is preferable that it has a low crystallinity and is easily liquid with good fluidity. In addition, it is preferable that it has a branched and / or cyclic structure because the flexibility of the polyamide formed from the polyvalent fatty acid (B) and the polyamine (C) is increased, which leads to an improvement in bonding strength and suppression of a decrease.
[0039] When the valence of the polyvalent fatty acid (B) is m, the polyvalent fatty acid (B) preferably has a hydrocarbon group (D) having a valence of m. In the polyvalent fatty acid (B), the skeleton excluding the carboxyl group is more preferably composed only of hydrocarbons having a valence of m.
[0040] It is more preferable for the m-valent hydrocarbon group (D) to have 30 to 60 carbon atoms, since the initial bonding strength and the bonding strength after the cycle test are particularly high.
[0041] Specific examples of polyvalent fatty acids (B) having a linear structure include malonic acid, succinic acid, glutaric acid, adipic acid, maleic acid, fumaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosanediic acid, heneicosanediic acid, docosanediic acid, tetracosanediic acid, triacontanedioic acid, dotriacontanedioic acid, tetracontanedioic acid, pentacontanedioic acid, and hexacontanedioic acid, but are not limited to these.
[0042] Examples of the branched and / or cyclic structures include, but are not limited to, methylmalonic acid, dimer acid, trimer acid, and tetramer acid.
[0043] Among these specific examples, it is more preferable that the polyvalent fatty acid (B) contains a dimer acid and / or a trimer acid.
[0044] Dimer acid, trimer acid, and tetramer acid can be produced by a polymerization reaction of unsaturated fatty acids. For example, they can be produced by a Diels-Alder reaction between oleic acid (carbon number 18) and linoleic acid (carbon number 18) or a radical reaction. The carbon numbers of dimer acid, trimer acid, and tetramer acid are preferably 36, 44, 54, and 72, respectively. In addition, by appropriately changing the carbon number of the unsaturated fatty acid used as a raw material, it is possible to produce polyvalent fatty acids (B) having carbon numbers other than those mentioned above. In this specification, dimers, trimers and tetramers of unsaturated fatty acids having 12 or more carbon atoms are referred to as dimer acid, trimer acid and tetramer acid, respectively.
[0045] The polyvalent fatty acid (B) may be a mixture of compounds having different degrees of polymerization due to the manufacturing process, but it may be used as a mixture of different polymers, or a specific single compound may be used.
[0046] <Polyamine (C)> Next, the polyamine (C) will be described. The polyamine (C) means a compound having a plurality of amino groups (-NH2 groups) in the molecule. The number of carbon atoms in the polyamine (C) is preferably 20 to 80.
[0047] In the polyamine (C), the skeleton (partial structure) excluding the amino group is an organic residue, but is preferably a hydrocarbon group or a group in which the hydrocarbon group is bonded with a linking group that may contain a heteroatom. Examples of such linking groups that contain a heteroatom include -O- group (ether group), -C(=O)- group (carbonyl group), -C(=O)-O- group (also called ester group or oxycarbonyl group), and -C(=O)-NH- group (also called amide group or iminocarbonyl group). In addition, arylene groups such as phenylene group and naphthylene group are also included in the linking group.
[0048] Like the polyvalent fatty acid (B), the polyamine (C) is believed to have the effect of maintaining the metal particle-containing composition in a fluid liquid state during sintering, and is presumed to increase the wettability at the bonding interface with the bonded parts. Therefore, even if voids are generated in the bonding layer, it is believed that the metal particles will flow into the defective parts, making it possible to obtain a bonding layer with few defects and high bonding strength.
[0049] The properties of the polyamine (C) are not particularly limited, but it is preferably liquid in the normal temperature range of 200° C. to 350° C. at which the metal particle-containing composition of the present invention is typically fired. The polyamine (C) may be solid or liquid at room temperature (25° C.), but is more preferably liquid at room temperature in that it can be uniformly dispersed in the metal particle-containing composition and act effectively.
[0050] The number of amino groups (-NH2) in the polyamine (C) is preferably 2 or 3. The polyamine (C) preferably contains a diamine and / or a triamine.
[0051] The polyamine (C) may have a linear structure or a branched and / or cyclic structure, but preferably has a branched and / or cyclic structure, which is preferable because it has low crystallinity and tends to be a liquid with good fluidity.
[0052] When the number of amino groups (-NH2) in the polyamine (C) is n, the polyamine (C) preferably has an n-valent hydrocarbon group (E). In the polyamine (C), the skeleton excluding the amino groups (-NH2) is more preferably composed of only n-valent hydrocarbons. When the carbon number of the n-valent hydrocarbon group (E) is 30 to 60, it is more preferable in that the initial bonding strength and the bonding strength after the cycle test are particularly high.
[0053] Among the polyamines (C), examples of polyamines having a linear structure include ethylenediamine, 1,3-propanediamine, 1,4-butanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,9-nonanediamine, and 1,12-diaminododecane, and examples of polyamines having a branched and / or cyclic structure include metaxylenediamine, isophoronediamine, norbornanediamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, and piperazine. In addition, dimer diamine, trimer triamine, and tetramer tetraamine are also included in the polyamines (C). Among these specific examples, it is more preferable that the polyamine (C) contains dimer diamine and / or trimer triamine.
[0054] The dimer diamine has a structure in which the carboxy group of the dimer acid is converted to an amino group, the trimer triamine has a structure in which the carboxy group of the trimer acid is converted to an amino group, and the tetramer tetramine has a structure in which the carboxy group of the tetramer acid is converted to an amino group. The dimer diamine, trimer triamine, and tetramer tetramine preferably have 36, 54, and 72 carbon atoms, respectively.
[0055] The combination of the polyvalent fatty acid (B) and the polyamine (C) is not limited, but a combination in which the polyvalent fatty acid (B) contains a dimer acid and / or a trimer acid, and the polyamine (C) contains a dimer diamine and / or a trimer triamine is more preferable.
[0056] In the metal particle-containing composition of the present invention, the blending amount of the polyvalent fatty acid (B) is preferably 0.05 parts by mass to 1 part by mass, more preferably 0.1 parts by mass to 0.5 parts by mass, relative to 100 parts by mass of the metal particles (A). The blending amount of the polyamine (C) is preferably 0.05 parts by mass to 1 part by mass, more preferably 0.1 parts by mass to 0.5 parts by mass, relative to 100 parts by mass of the metal particles (A). If the blending amount is within this range, it is expected that the fluidity during sintering will increase, which is preferable in that a bonded body having excellent initial and long-term cycle resistance is easily obtained.
[0057] The blending ratio of the polyhydric fatty acid (B) and the polyamine (C) is not limited, but in terms of facilitating the formation of polyamide, the mass ratio of polyhydric fatty acid (B) / polyamine (C) is preferably 0.1 / 0.9 to 0.9 / 0.1, and more preferably 0.3 / 0.7 to 0.7 / 0.3.
[0058] <Dispersion medium (F)> The bonding paste of the present invention contains a dispersion medium (F). The dispersion medium (F) serves to disperse the metal particles (A), the polyvalent fatty acid (B), and the polyamine (C). The dispersion medium (F) may be any medium capable of dispersing the metal particles (A), polyvalent fatty acid (B), and polyamine (C). Specific examples include terpineol, dihydroterpineol, dihydroterpinyl acetate, Tersolve MTPH (manufactured by Nippon Terpene Co., Ltd.), Texanol (2,2,4-trimethylpentane-1,3-diol monoisobutyrate), carbitol, carbitol acetate, butyl carbitol, isophorone, γ-butyrolactone, dipropylene glycol monomethyl ether, dipropylene glycol methyl-n-propyl ether, 3-methoxy-3-methylbutyl acetate, ethylene glycol, hexanoic acid, propylene glycol diacetate, dipropylene glycol methyl ether acetate, 1,3-butylene glycol, and isoparaffin-based solvents contained in hydrocarbon solvents, but are not limited thereto.
[0059] Among these dispersion media (F), terpineol, dihydroterpineol, tersolve MTPH, texanol, carbitol, carbitol acetate, butyl carbitol, isophorone, γ-butyl lactone, dipropylene glycol monomethyl ether, and isoparaffin-based solvents are more preferably used. These dispersion media (F) can be used alone or in combination.
[0060] The bonding paste of the present invention contains the polyhydric fatty acid (B) and the polyamine (C) and is therefore capable of forming a bonding interface having good adhesion to the bonded parts even after a part or all of the dispersion medium (F) has volatilized.
[0061] The bonding paste of the present invention has excellent fluidity even when the metal particles (A) are contained at a high concentration, that is, when the content ratio of the dispersion medium (F) is small, by using a combination of metal particles (A), polyvalent fatty acid (B), and polyamine (C), and therefore has excellent printability on the bonded parts. In addition, the bonding paste of the present invention does not have a risk of the compatibility of the components decreasing, resulting in non-uniformity, or loss of fluidity, compared to the case where a polyamide resin is added. As a result, it is possible to obtain a stronger bonded body with fewer defects.
[0062] In the bonding paste, the mass ratio of the metal particles (A) to the sum of the masses of the metal particles (A), the polyvalent fatty acid (B), the polyamine (C), and the dispersion medium (F) is preferably 80% by mass to 95% by mass, and more preferably 85% by mass to 94% by mass. By including the above range, good printability of the bonding paste can be ensured. Furthermore, by including the above range, the residual of the dispersion medium (F) in the bonded body can be suppressed, and voids originating from the dispersion medium (F) are unlikely to occur, so that good bonding strength can be expressed.
[0063] <Other ingredients> The bonding paste of the present invention may further contain other components such as additives, etc. Examples of the other components include a sintering accelerator, a binder resin, and a dispersant such as a low molecular weight dispersant or a resin type dispersant. The dispersant that may be contained in the bonding paste of the present invention is preferably a low molecular weight dispersant having a molecular weight of 150 to 600, and more preferably an unsaturated fatty acid having 18 to 22 carbon atoms or an unsaturated fatty acid amide having 18 to 22 carbon atoms. The unsaturated fatty acid is a monovalent fatty acid having an unsaturated bond, and specific examples thereof include oleic acid, elaidic acid, linoleic acid, linolenic acid, ricinoleic acid, and erucic acid. The unsaturated fatty acid amide is a monovalent fatty acid amide having an unsaturated bond, and specific examples thereof include oleamide (oleic acid amide) and erucic acid amide. By containing these dispersants, the metal particles (A) in the bonding paste are more uniformly loosened, and a strong bonded body with less unevenness in voids can be obtained, which is preferable. The amount of the low molecular weight dispersant is not limited, but in order to achieve both good dispersion of the metal particles (A) and densification of the bonding layer, the amount is preferably 0.1 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, and even more preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the metal particles (A).
[0064] Examples of a device for preparing a bonding paste from the metal particles (A), the compound (B) and the dispersion medium (C) include a disperser, a three-roll mill, a bead mill, an ultrasonic disperser, and a planetary stirrer.
[0065] <zygote> The bonding paste of the present invention can bond a first bonded part and a second bonded part to obtain a bonded body. In detail, the bonded body of the present invention is a bonded body in which a first bonded part and a second bonded part are bonded via a bonding layer, and the bonded body can be produced by a production method including a step of applying a bonding paste containing metal particles (A) having an average particle size of 1 nm to 1000 nm, a polyvalent fatty acid (B), a polyamine (C), and a dispersion medium (F) to the first bonded part, placing the second bonded part on the bonding paste, and sintering the applied paste. The method of applying the bonding paste to the bonded portion is not particularly limited as long as it can be applied uniformly to the member. For example, various printing methods such as screen printing, flexographic printing, offset printing, gravure printing, metal mask printing, gravure offset printing, and the like, and a discharge method using a dispenser, etc. are included. Since the bonding paste of the present invention has excellent fluidity even when it contains metal particles at a high concentration, it is particularly preferable to use it in combination with metal mask printing.
[0066] When placing the second part to be joined on the first part to be joined coated with the joining paste of the present invention, the second part to be joined can be placed under pressure. The pressure is appropriately set depending on the viscosity of the joining paste and the drying state of the paste, and is preferably 0.1 to 40 MPa, more preferably 0.3 to 30 MPa.
[0067] The sintering conditions for bonding the laminate in which the second bonded portion is placed on the first bonded portion may be appropriately changed, and may be, for example, conditions of 200 to 350°C under atmospheric pressure, in a nitrogen atmosphere, in a vacuum, or in a reducing atmosphere. Examples of the sintering device include a hot air oven, an infrared oven, a reflow oven, a microwave oven, a hot plate, and a light sintering device. These devices may be used alone or in combination as appropriate. Pressure may also be applied during sintering. The pressure is appropriately set depending on the viscosity of the bonding paste and the drying state of the paste, and is preferably 0.1 to 40 MPa, and more preferably 0.3 to 30 MPa.
[0068] Before the firing step, a preliminary drying step can be appropriately performed in order to remove organic components from the bonding coating film. For example, the pre-drying step can be performed under conditions in the range of 60 to 220°C using a device similar to the firing device.
[0069] A preferred method for joining two parts to be joined is to apply the joining paste of the present invention to a first part to be joined, place a second part to be joined on it, and heat it up to about 300° C. at a heating rate of about 2° C. / min to perform sintering. After the temperature rise is completed, it is preferable to maintain the temperature higher than the temperature at the end of the temperature rise for about 10 minutes to 2 hours.
[0070] The type of the parts to be joined is not particularly limited, and examples thereof include metal materials, semiconductor materials, plastic materials, ceramic materials, etc. Also included are electronic elements.
[0071] Examples of the metal include copper, gold, and aluminum. Examples of semiconductor materials include silicon, germanium, gallium arsenide, gallium phosphide, cadmium sulfide, silicon nitride, graphite, yttrium oxide, magnesium oxide, silicon carbide, gallium nitride, and gallium oxide. Examples of the plastic material include polyimide, polyethylene, polypropylene, polyethylene terephthalate, polycarbonate, and polyethylene naphthalate. Examples of the ceramic material include glass and silicon. Examples of electronic elements include semiconductor elements, LED elements, and power device elements.
[0072] The first and second joined parts may be of different types or may not be the same type. The surfaces of the joined parts may be subjected to a corona treatment, a plating treatment, or the like in order to increase the joining strength at the joined portion.
[0073] There is no limit to the thickness of the bonding layer formed when bonding parts to be bonded with the metal particle-containing composition or bonding paste of the present invention, but it is preferably 3 μm to 500 μm, more preferably 10 μm to 200 μm, and even more preferably 20 μm to 100 μm. EXAMPLES
[0074] The present invention will be described in detail below using examples and comparative examples, but the technical scope of the present invention is not limited thereto. In the examples, unless otherwise specified, "parts" means "parts by mass", "%" means "% by mass", and the numerical values in the tables mean "parts" unless otherwise specified.
[0075] <Production of metal particles> (Production example 1) Metal particles A1 Under a nitrogen atmosphere, 200 parts of toluene and 22.3 parts of silver hexanoate were mixed while stirring at 25°C to obtain a 0.5M solution, and then 1.6 parts of diethylaminoethanol and 0.28 parts of oleic acid were added as a dispersant and dissolved. Then, 73.1 parts of a 20% aqueous solution of succinic acid dihydrazide (hereinafter, SUDH) was added dropwise as a reducing agent, and the liquid color changed from light yellow to dark brown. The temperature was raised to 40°C to promote the reaction. After standing and separating, the aqueous phase was removed to remove excess reducing agent and impurities, and distilled water was added to the toluene layer several times, washing and separation were repeated, and then the process of adding toluene, centrifuging, and removing the supernatant was repeated twice. The precipitate was dried to obtain metal particles A1 in which silver particles were coated with hexanoic acid and oleic acid. The particle size of metal particles A1 was determined by the method described below, and d50 was 210 nm.
[0076] (Production example 2) Metal particles A2 Metal particles A2 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 1.8 parts and the amount of oleic acid was 0.31 parts. The d50 was 185 nm. (Production example 3) Metal particles A3 Metal particles A3 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 1.2 parts and the amount of oleic acid was 0.18 parts. The d50 was 290 nm. (Production example 4) Metal particles A4 Metal particles A4 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 1.0 part and the amount of oleic acid was 0.14 part. The d50 was 390 nm. (Production example 5) Metal particles A5 Metal particles A5 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 2.1 parts and the amount of oleic acid was 0.71 parts. The d50 was 85 nm. (Production example 6) Metal particles A6 Metal particles A6 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 0.6 parts and the amount of oleic acid was 0.070 parts. The d50 was 1100 nm. Among the metal particles produced by the above method, metal particles A1 to A5 correspond to metal particles (A), and metal particle A6 corresponds to metal particles other than metal particles (A).
[0077] [Particle size measurement] Isopropyl alcohol was added to each metal particle (A) and dispersed in an ultrasonic disperser to obtain a 0.5% by mass dispersion. The particle size of the metal particles (A) in the dispersion was measured using Nanotrac UPA-EX150 (manufactured by Nikkiso Co., Ltd.) to determine the average particle size (d50).
[0078] [Fatty acids, amines and other components] The fatty acids, amines, and other materials used in the examples and comparative examples are as follows. The number of carbon atoms, material name, and properties at 25°C are shown in parentheses. Among the following, Pripol and Priamine were used, manufactured by Croda Japan Co., Ltd., oleic acid amide was used, manufactured by Tokyo Chemical Industry Co., Ltd., and other materials were used, manufactured by Sigma-Aldrich. The fatty acids B1 to B3, B5, and B6 correspond to polyvalent fatty acids (B), and the amines C1 to C3 correspond to polyamines (C). The fatty acid B4 and fatty acid amide G1 correspond to dispersants that may be added to the present invention.
[0079] Fatty acid B1: Pripol 1009 (a hydrogenated dimer acid with 36 carbon atoms, consisting of two carboxyl groups and a divalent hydrocarbon group with a branched and cyclic structure. A liquid polyvalent fatty acid) Fatty acid B2: Pripol 1040 (a trimer acid with 54 carbon atoms, consisting of three carboxyl groups and a trivalent hydrocarbon group with a branched and cyclic structure. A liquid polyvalent fatty acid) Fatty acid B3: Straight-chain dibasic acid (22 carbon atoms, docosane diacid, consisting of two carboxyl groups and a divalent hydrocarbon with a straight-chain structure. A solid polyvalent fatty acid) Fatty acid B4: Oleic acid (a monovalent straight-chain fatty acid with 18 carbon atoms. A liquid monounsaturated fatty acid) Fatty acid B5: Malonic acid (a straight-chain dibasic acid with 3 carbon atoms. A solid polyvalent fatty acid) Fatty acid B6: Pripol 1004 (a hydrogenated dimer acid with 44 carbon atoms, consisting of two carboxyl groups and a divalent hydrocarbon group with a branched and cyclic structure. A liquid polyvalent fatty acid) Amine C1: Priamine 1071 [a mixture of a dimer diamine having 36 carbon atoms (a liquid polyamine consisting of two amino groups and a divalent hydrocarbon group having a branched and cyclic structure) and a trimer triamine having 54 carbon atoms (a liquid polyamine consisting of three amino groups and a trivalent hydrocarbon group having a branched and cyclic structure)] Amine C2: Priamine 1075 (a dimer diamine having 36 carbon atoms, consisting of two amino groups and a divalent hydrocarbon group having a branched and cyclic structure. A liquid polyamine) Amine C3: 1,12-diaminododecane (a solid polyamine with 12 carbon atoms, two amino groups, and a divalent hydrocarbon group with a linear structure) Amine C4: Oleylamine (a monovalent linear monoamine with 18 carbon atoms. Liquid) Fatty acid amide G1: Oleic acid amide (solid monounsaturated fatty acid amide)
[0080] (Production Example 7) Polyamide containing phenolic hydroxyl groups (Polyamide P1) Polyamide P1 was synthesized as follows with reference to JP 2017-137375 A. A four-neck flask equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, an inlet tube, and a thermometer was charged with 202.9 g of Pripol 1009 (0.35 mol in terms of dibasic acid), 25.7 g (0.14 mol) of 5-hydroxyisophthalic acid, 35.1 g (0.21 mol) of terephthalic acid, 313.9 g (0.59 mol in terms of diamine) of Priamine 1074 (manufactured by Croda Japan Co., Ltd.) as a polyamine compound having a carbon number of 36, and 100 g of water, and stirred until the temperature of the heat generation became constant. When the temperature stabilized, the temperature was raised to 110 ° C., and after confirming the outflow of water, the temperature was raised to 120 ° C. after 30 minutes, and the dehydration reaction was continued while raising the temperature by 10 ° C. every 30 minutes. When the temperature reached 230° C., the reaction was continued at that temperature for 3 hours, and then the mixture was held under a vacuum of about 2 kPa for 1 hour and then allowed to cool to obtain polyamide P1 having a weight average molecular weight of 9,800 and containing phenolic hydroxyl groups.
[0081] (Production Example 8) Polyamide containing phenolic hydroxyl groups (Polyamide P2) In Production Example 7, 202.9 g of Pripol 1009 (0.35 mol in terms of dibasic acid) was replaced with 243.1 g of Pripol 1004 (0.35 mol in terms of dibasic acid), and the same procedure was followed to obtain polyamide P2 containing phenolic hydroxyl groups and having a weight average molecular weight of 11,700.
[0082] [Dispersion medium (F)] The following materials were used as the dispersion medium (F). The manufacturer's name and supplementary information are given in parentheses. Dispersion medium F1: Dihydroterpineol (manufactured by Nippon Terpene Chemical Co., Ltd.) Dispersion medium F2: Isobornylcyclohexanol (manufactured by Nippon Terpene Chemical Co., Ltd.) Dispersion medium F3: Isopar L (manufactured by Ando Parachemie Co., Ltd.) Dispersion medium F4: Texanol (Tokyo Chemical Industry Co., Ltd., reagent)
[0083] <Production of bonding paste> [Example 1] Metal particles A1 (92 parts), dihydroterpineol (8 parts), fatty acid B1 (0.15 parts), and amine C2 (0.15 parts) were mixed using a planetary stirrer to prepare a bonding paste. Then, a bonded body was produced and evaluated by the method described below. The results are shown in Table 1.
[0084] [Examples 2 to 39], [Comparative Examples 1 to 8] A bonding paste and a bonded body were obtained and then evaluated in the same manner as in Example 1, except that the types and amounts of materials were changed according to the compositions shown in Table 1. The results are shown in Table 1.
[0085] <Evaluation of bonding paste> [Preparation of junction] Each joining paste was printed once on the plated surface of the joining part 1 described below under the printing conditions described below, and then the plated surface of the joining part 2 (chip) described below was placed facing the joining paste surface and heated under the sintering conditions described below to obtain each joining body. <Joined part 1> Gold-plated copper substrate: 20 x 20 x 3 mm <Joined part 2> Gold-plated SiC chip: 5×5×0.3mm <Printing conditions (metal mask printing)> Metal mask: 4mm square opening, 50μm thickness (manufactured by Celia Corporation) Metal squeegee: 40mm x 250mm, thickness 1mm (manufactured by Celia Corporation) <Sintering conditions> The unsintered bonded body was placed in a hot air oven, and the temperature was raised from 25°C to 300°C at 2°C / min. After reaching 300°C, it was held at 300°C for 2 hours. [Evaluation criteria (printability)] ○: Printing was possible on the bonded part 1. ×: Printing on the bonded portion 1 was not possible.
[0086] [Bonding strength (initial, after thermal cycle test) The bond strength (die shear strength) of the obtained bonded body was measured using the following measuring device and test conditions. Note that an asterisk (*) in Table 1 indicates that this evaluation was not performed because printing was not possible. Measurement equipment: Universal bond tester (Daisi Japan Co., Ltd., 4000 series) <Test conditions> Measurement height: 100μm Measurement speed: 500μm / s
[0087] Specifically, the bonded body was fixed at the site of the part to be bonded 1, and the bond was pushed from the interface between the part to be bonded 1 and the bonding layer toward the part to be bonded 2 at a height of 100 μm at a speed of 500 μm / s to determine the bonding strength at which the bond was destroyed. The bonding strength (initial strength) immediately after the bonded body was produced and the bonding strength after the cycle test described below were measured and evaluated based on the evaluation criteria below. The higher the adhesive strength value, the better, and a value of 15 MPa or more is within the practical range. The higher the evaluation criterion value, the better, and an evaluation criterion value of 2 or less indicates poor bonding.
[0088] 6: 40MPa or more 5: 30MPa or more but less than 40MPa 4: 20MPa or more but less than 30MPa 3: 15MPa or more but less than 20MPa 2: 5MPa or more and less than 15MPa 1: Less than 5MPa
[0089] <Cold-heat cycle test> The bonded body was stored for 500 cycles, with one cycle being held at -40°C for 30 minutes, then at 25°C for 15 minutes, and finally at 150°C for 30 minutes. After that, the bond strength was evaluated using the same procedures and criteria as in the bond strength evaluation method described above. Furthermore, a similar evaluation was performed after 1000 cycles as a long-term durability test.
[0090] The bonding pastes of the comparative examples could not be printed when they contained a high concentration of metal particles (Comparative Examples 1, 5, and 7). By reducing the concentration of metal particles, printing became possible, but the bonding strength of the resulting bonded body was extremely low, and when a sample that had been destroyed after a die shear test was observed, it was found that the bond was destroyed at the interface between the gold-plated SiC chip and the bonding layer. On the other hand, it was confirmed that the bonding paste of the examples has excellent printability even when it contains metal particles at a high concentration, the bonding strength of the obtained bonded body is very high, and the decrease in bonding strength is suppressed even after a thermal cycle test. In addition, in Examples 1 to 39, when the samples after the evaluation of bonding strength were immersed in toluene to extract and concentrate the remaining organic matter, and the IR was measured, a peak attributed to an amide bond was detected in each sample, and it was confirmed that polyamide formed in the bonded body by condensation of polyvalent fatty acid (B) and polyamine (C) was generated.
[0091] [Table 1-1]
[0092] [Table 1-2]
[0093] [Table 1-3]
Claims
1. The present invention comprises metal particles (A) having an average particle size of 1 nm to 1000 nm, a polyvalent fatty acid (B), and a polyamine (C), A metal particle-containing composition comprising 0.05 to 0.98 parts by mass of the polyvalent fatty acid (B) and 0.05 to 0.98 parts by mass of the polyamine (C) relative to 100 parts by mass of the metal particles (A).
2. 2. The metal particle-containing composition according to claim 1, wherein the polyvalent fatty acid (B) has 20 to 80 carbon atoms, and the polyamine (C) has 20 to 80 carbon atoms.
3. 3. The metal particle-containing composition according to claim 1, wherein the polyvalent fatty acid (B) includes a divalent and / or trivalent fatty acid.
4. 4. The metal particle-containing composition according to claim 1, wherein the polyamine (C) includes a diamine and / or a triamine.
5. 5. The metal particle-containing composition according to claim 1, wherein the polyvalent fatty acid (B) and / or the polyamine (C) have a branched and / or cyclic structure.
6. The metal particle-containing composition according to any one of claims 1 to 5, characterized in that, when the valence of the polyvalent fatty acid (B) is m and the valence of the polyamine (C) is n, the polyvalent fatty acid (B) has a hydrocarbon group (D) having an m valence, or the polyamine (C) has a hydrocarbon group (E) having an n valence.
7. 7. The metal particle-containing composition according to claim 6, wherein the m-valent hydrocarbon group (D) and / or the n-valent hydrocarbon group (E) have 30 to 60 carbon atoms.
8. 8. The metal particle-containing composition according to claim 1, further comprising 0.1 to 0.5 parts by mass of the polyvalent fatty acid (B) per 100 parts by mass of the metal particles (A).
9. 9. The metal particle-containing composition according to claim 1, comprising 0.1 to 0.5 parts by mass of polyamine (C) per 100 parts by mass of metal particles (A).
10. 10. The metal particle-containing composition according to claim 1, wherein the metal particles (A) have an average particle size of 180 nm to 400 nm.
11. 11. The metal particle-containing composition according to claim 1, wherein the metal particles (A) have an average particle size of 200 nm to 300 nm.
12. A bonding paste comprising the metal particle-containing composition according to any one of claims 1 to 11 and a dispersion medium (F).
13. The ratio of the mass of the metal particles (A) to the sum of the masses of the metal particles (A), the polyvalent fatty acid (B), the polyamine (C), and the dispersion medium (F) is 80% by mass to 95% by mass. The bonding paste according to claim 12.
14. A bonded body in which a first bonded part and a second bonded part are bonded via a bonding layer, the bonding layer being a layer formed from the bonding paste according to claim 12 or 13.
15. A method for producing a bonded body in which a first bonded part and a second bonded part are bonded via a bonding layer, the method comprising the steps of: applying a bonding paste to the first bonded part, the bonding paste containing metal particles (A) having an average particle size of 1 nm to 1000 nm, a polyvalent fatty acid (B), a polyamine (C), and a dispersion medium (F), placing the second bonded part on the bonding paste, and sintering the bonded part.
Citation Information
Patent Citations
Metal nanoparticle paste, and pattern forming method
JP2009097074A
Joining material and joining method using the same
JP2011080147A
Bonding material and bonding method using the same
JP2011240406A
Binding agent and article bound by binding agent