Photosensitive resin composition and cured film thereof
A photosensitive resin composition with a specific polyimide resin structure and molecular weight addresses the issues of high-temperature heating and material limitations, providing low-temperature curing with improved developability and crack resistance.
Patent Information
- Application Number
- JP2021524798
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-03
- Filing Date
- 2020-05-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-05-27
AI Technical Summary
Existing methods for polyimide resins require high-temperature heating, leading to volumetric shrinkage and cracking, and limit material selection due to polymerizable group introduction in side chains, which is not suitable for low-temperature curing applications.
A photosensitive resin composition with a polyimide resin having a specific structure, terminal groups, and molecular weight, allowing for low-temperature curing without heating, and enabling flexibility in material selection.
The composition achieves high transparency, solvent solubility, and excellent developability, effectively suppressing cracking in the cured film while maintaining flexibility in material choice.
Smart Images

Figure 0007574796000001 
Figure 0007574796000002 
Figure 0007574796000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive resin composition and a cured film thereof. [Background technology]
[0002] Polyimide resins with excellent heat resistance and insulation properties are widely used for surface protection films, interlayer insulation films, wiring protection insulation films for circuit boards, etc. of semiconductor elements in electronic devices. From the viewpoint of recent high density and high integration, insulating materials for semiconductor integrated circuits and the like are required to have higher pattern developability than before, as well as various physical properties such as high insulation, improved heat resistance, low temperature curing, crack resistance, and flexibility. The developability is better the greater the difference in solubility between the exposed and unexposed parts, and it is important to widen the difference in solubility between the exposed and unexposed parts in order to improve the developability. In addition, in order to express the desired physical properties, it is also necessary to appropriately select the raw material of the base polymer and design the polymer.
[0003] Since polyimide has low solubility in solvents, a method of introducing a polymerizable group into a polyimide precursor has been proposed as a method for obtaining a photosensitive polyimide. Patent Document 1 proposes a method of introducing a polymerizable group into a side chain of a polyimide precursor. Patent Document 2 proposes a method of introducing a polymerizable group into the terminal of a polyimide precursor.
[0004] On the other hand, a method of introducing a polymerizable group into a solvent-soluble polyimide has been proposed. Since it is possible to introduce polymerizable groups at a high density, a polyimide having a polymerizable group in a side chain has been proposed. Patent Document 3 proposes a method of providing a polymerizable group in a side chain of a polyimide. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-76845 A [Patent Document 2] International Publication No. 2018 / 003725 [Patent Document 3] JP 2000-147761 A Summary of the Invention [Problem to be solved by the invention]
[0006] The methods disclosed in Patent Documents 1 and 2 require heating a polyimide precursor at high temperature for a long period of time to obtain polyimide, which is not suitable for fields requiring low-temperature curing. In addition, when the heating step for obtaining polyimide from a polyimide precursor is included, volume shrinkage of about 50% occurs, which is problematic as it can cause warping or cracking. In the method disclosed in Patent Document 3, it is necessary to introduce a functional group for providing a polymerizable group in the side chain of the polyimide, so the options for raw materials for synthesizing the polyimide are limited. In addition, the method of providing a polymerizable group in the side chain has good curability because the polymerizable group can be introduced at a high density, but has the problem that the cure shrinkage rate is large and cracks are likely to occur.
[0007] In view of the above circumstances, an object of the present invention is to provide a photosensitive resin composition which does not require a heating step, has excellent developability, allows freedom in the selection of polyimide raw materials, and has low cure shrinkage. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by a photosensitive resin composition containing a polyimide resin having a specific structure and a specific terminal structure and having a specific weight-average molecular weight. The present invention relates to the following photosensitive resin composition and a cured film thereof.
[0009] [1] A photosensitive resin composition comprising a polyimide resin (A) having a structure represented by the following general formula (1) and having a weight average molecular weight of 70,000 or less: [ka] [In the general formula (1), R is a tetravalent group having 4 to 10 carbon atoms and having a cyclic structure, a non-cyclic structure, or a cyclic structure and a non-cyclic structure. A is a divalent group having 2 to 39 carbon atoms and having at least one group selected from the group consisting of an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, an aromatic hydrocarbon group, and an organosiloxane group. At least one group selected from the group consisting of -O-, -SO2-, -CO-, -CH2-, -C(CH3)2-, -C2H4O-, and -S- may be present in the main chain of A. n represents the number of repeating units. The terminal of the general formula (1) is either a group represented by the following formula (2) or formula (3) or a hydrogen atom, and at least one of the terminals is a group represented by formula (2) or formula (3)] [ka] [In the general formulas (2) and (3), X and X 2 Each of Y and Y is independently a group having 2 to 15 carbon atoms, and may have at least one group selected from the group consisting of an ester bond and a double bond. 2 are each independently a hydrogen atom or a methyl group. [2] The photosensitive resin composition according to the above [1], wherein the polyimide resin (A) has a weight average molecular weight of 5,000 or more. [3] The photosensitive resin composition according to the above [1] or [2], wherein the polyimide resin (A) has a light transmittance of 50% or more at a wavelength of 200 to 400 nm. [4] Exposure dose at wavelength 365 nm: 1,500 to 2,500 mJ / cm 2 The photosensitive resin composition according to any one of the above [1] to [3], wherein after exposure under the above conditions, the residual film rate of the unexposed area is 40% or less. [5] The photosensitive resin composition according to at least one of the above [1] to [4], wherein A in the general formula (1) contains an aromatic ring as an aromatic hydrocarbon group. [6] The photosensitive resin composition according to any one of the above [1] to [5], wherein A in the general formula (1) includes at least one selected from the group consisting of the structures shown below: [ka] [In the formula, * indicates a bond.] [7] The photosensitive resin composition according to any one of the above [1] to [6], wherein the polyimide resin (A) contains at least one unit composed of 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-indene-5-amine, 4,4'-oxybis[3-(trifluoromethyl)benzeneamine, or 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene. [8] The photosensitive resin composition according to any one of the above [1] to [7], further comprising at least one selected from the group consisting of a photopolymerization initiator, a solvent, and a photopolymerizable compound. [9] The photosensitive resin composition according to the above [8], wherein the photopolymerizable compound is a polyfunctional radically polymerizable monomer.
[10] The photosensitive resin composition according to any one of the above [1] to [9], further comprising a sensitizer.
[11] The photosensitive resin composition according to any one of the above [1] to
[10] , which is used for forming an insulating film.
[12] A cured film obtained by curing the photosensitive resin composition according to any one of the above [1] to
[11] .
[13] The cured film according to the above
[12] , having a film thickness of 10 to 85 μm. Effect of the Invention
[0010] According to the present invention, it is possible to obtain a photosensitive resin composition that does not require a heating step, has high transparency and excellent solvent solubility, and therefore has excellent developability, and has a degree of freedom in selecting polyimide raw materials. The resin composition has low cure shrinkage, and therefore the occurrence of cracks in the obtained cured film can be effectively suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] A detailed description will be given of an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment"). The following present embodiment is an example for explaining the present invention, and does not limit the contents of the present invention. The present invention can be carried out by appropriately modifying it within the scope of its gist. In this specification, the provisions that are considered to be preferable can be adopted arbitrarily, and it can be said that a combination of preferable provisions is more preferable. In this specification, the description "XX to YY" means "XX or more and YY or less."
[0012] In this specification, "(meth)acrylate" means both "acrylate" and "methacrylate". The same applies to other similar terms (such as "(meth)acrylic acid" and "(meth)acryloyl group").
[0013] [Polyimide resin (A)] The polyimide resin (A) of this embodiment has a structure represented by the following general formula (1) and has a weight average molecular weight of 70,000 or less. [ka] [In the general formula (1), R is a tetravalent group having 4 to 10 carbon atoms and having a cyclic structure, a non-cyclic structure, or a cyclic structure and a non-cyclic structure. A is a divalent group having 2 to 39 carbon atoms and having at least one group selected from the group consisting of an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, an aromatic hydrocarbon group, and an organosiloxane group. At least one group selected from the group consisting of -O-, -SO2-, -CO-, -CH2-, -C(CH3)2-, -C2H4O-, and -S- may be present in the main chain of A. n represents the number of repeating units. The terminal of the general formula (1) is either a group represented by the following formula (2) or formula (3) or a hydrogen atom, and at least one of the terminals is a group represented by formula (2) or formula (3)]
[0014] [ka] [In the general formulas (2) and (3), X and X 2Each of Y and Y is independently a group having 2 to 15 carbon atoms, and may have at least one group selected from the group consisting of an ester bond and a double bond. 2 are each independently a hydrogen atom or a methyl group.
[0015] It is preferable that R in the above formula (1) has at least a cyclic structure, and examples of the cyclic structure include tetravalent groups formed by removing four hydrogen atoms from cyclohexane, cyclopentane, cyclobutane, bicyclopentane, and stereoisomers thereof. More specifically, examples of the tetravalent group include groups represented by the following structural formula: [ka] [In the formula, * indicates a bond.]
[0016] Among the above, a tetravalent group formed by removing four hydrogen atoms from cyclohexane is more preferable.
[0017] In formula (1), A is a divalent group having 2 to 39 carbon atoms and at least one group selected from the group consisting of an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, an aromatic hydrocarbon group, and an organosiloxane group. The main chain of A may be interrupted by at least one group selected from the group consisting of -O-, -SO2-, -CO-, -CH2-, -C(CH3)2-, -C2H4O-, and -S-.
[0018] More specifically, A includes divalent groups formed by removing two hydrogen atoms from compounds such as cyclohexane, dicyclohexylmethane, dimethylcyclohexane, isophorone, norbornane, and alkyl and halogen-substituted derivatives thereof; benzene, naphthalene, biphenyl, diphenylmethane, diphenyl ether, diphenyl sulfone, benzophenone, and alkyl and halogen-substituted derivatives thereof; and organo(poly)siloxane. A preferably has a cyclic structure, and preferably has an alicyclic hydrocarbon group and / or an aromatic ring. A preferably has an aromatic ring as an aromatic hydrocarbon group. More specifically, preferred examples include divalent groups having 6 to 27 carbon atoms represented by the following structural formula. [ka] [In the formula, * indicates a bond.]
[0019] It is more preferable that the group corresponding to A exemplified above includes at least one selected from the group consisting of the structures shown below. [ka] [In the formula, * indicates a bond.]
[0020] n, which indicates the number of repeating units of the structural unit represented by formula (1), is preferably 5 to 250, more preferably 10 to 200, and further preferably 15 to 150. When n is 15 or more, a cured film having desired mechanical properties can be obtained. When n is 250 or less, sufficient solvent solubility can be ensured.
[0021] The polyimide resin (A) of the present embodiment has either a group represented by the above general formula (2) or general formula (3) or a hydrogen atom at its terminal, and at least one of the terminals is a group represented by general formula (2) or general formula (3). One terminal of the polyimide resin (A) may have a structure represented by general formula (2) or general formula (3), or both terminals may have a structure represented by general formula (2) or general formula (3). X or X in general formula (2) or general formula (3) 2 The group represented by the following formula (1) has 2 to 15 carbon atoms and may have at least one group selected from the group consisting of an ester bond and a double bond. 2 is a hydrogen atom or a methyl group.
[0022] More specifically, the structure represented by the above general formula (2) or general formula (3) corresponds to a structure obtained by reacting the terminal diamine of the polyimide resin (A) with a functional group-containing compound. Such a functional group-containing compound may be a compound having an isocyanate group or an epoxy group and a (meth)acrylic group. Such a compound may be 2-isocyanatoethyl methacrylate, 2-isocyanatoethyl acrylate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate, glycidyl methacrylate, glycidyl acrylate, allyl glycidyl ether, etc. The structure represented by the general formula (2) or general formula (3) may have a structure in which the compound reacts with the amine terminal.
[0023] The polyimide resin (A) must have a weight average molecular weight of 70,000 or less. If the weight average molecular weight exceeds 70,000, the solvent solubility of the resin composition decreases, making it unsuitable for forming a cured film. The weight average molecular weight is preferably 60,000 or less, more preferably 50,000 or less, even more preferably 45,000 or less, even more preferably 40,000 or less, even more preferably 35,000 or less, even more preferably 30,000 or less, and particularly preferably less than 30,000. Since a cured film having desired mechanical properties can be obtained, it is preferable that the weight average molecular weight of the polyimide resin (A) is 5,000 or more. The weight average molecular weight of the polyimide resin (A) is more preferably 10,000 or more, even more preferably 13,000 or more, and even more preferably 15,000 or more. By having the weight average molecular weight of the polyimide resin (A) in the above range, a resin composition having a low residual film rate in the unexposed area and excellent developability can be obtained.
[0024] The polyimide resin (A) can be obtained by reacting a diamine component, which will be described in detail below, with a tetracarboxylic acid component.
[0025] <Diamine component> The diamine component may include diamine, diisocyanate, diaminodisilane, etc., and is preferably diamine. The diamine content in the diamine component used as a raw material is preferably 50 mol % or more, and may be 100 mol %.
[0026] The diamine may be either an aliphatic diamine or an aromatic diamine, or a mixture of these. In the present invention, the term "aromatic diamine" refers to a diamine in which an amino group is directly bonded to an aromatic ring, and may contain an aliphatic group, an alicyclic group, or other substituents as part of its structure. The term "aliphatic diamine" refers to a diamine in which an amino group is directly bonded to an aliphatic group or an alicyclic group, and may contain an aromatic group, or other substituents as part of its structure.
[0027] In general, when an aliphatic diamine is used as a raw material for polyimide resin, the intermediate product polyamic acid and aliphatic diamine form a strong complex, making it difficult to obtain a high molecular weight polyimide. Therefore, it is necessary to use a solvent that has a relatively high solubility for the complex, such as cresol. When cyclohexanetetracarboxylic acid, cyclobutanetetracarboxylic acid, or a derivative thereof is used as a tetracarboxylic acid component, a complex is formed in which the bond between the polyamic acid and the aliphatic diamine is relatively weak, so that the polyimide can be easily made high molecular weight. It is preferable to select a diamine having a fluorine substituent as a raw material, since the resulting polyimide resin has excellent transparency.
[0028] Any aliphatic diamine can be used as the above-mentioned aliphatic diamine. Examples of the aliphatic diamine include 4,4'-diaminodicyclohexylmethane, ethylenediamine, hexamethylenediamine, polyethylene glycol bis(3-aminopropyl)ether, polypropylene glycol bis(3-aminopropyl)ether, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, m-xylylenediamine, p-xylylenediamine, isophoronediamine, norbornanediamine, and siloxanediamines.
[0029] Examples of the aromatic diamine include 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, m-phenylenediamine, p-phenylenediamine, diaminobenzophenone, 2,6-diaminonaphthalene, 1,5-diaminonaphthalene, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 4,4'-oxybis[3-(trifluoromethyl)benzeneamine], 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine, and 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene.
[0030] It is preferable that the diamine contains at least 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 4,4'-oxybis[3-(trifluoromethyl)benzeneamine], 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine or 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene. By containing at least one of them as a diamine component, the photosensitive resin composition containing the obtained polyimide resin (A) has high light transmittance at a specific wavelength and high solvent solubility. Therefore, the photosensitive resin composition has excellent curability in the exposed area, low residual film rate in the unexposed area, and excellent developability. It is sufficient to contain any of the above as a diamine component, and the excellent effect is maintained even when used in combination with other diamines. The polyimide resin (A) of the present embodiment preferably contains at least one unit composed of 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine, 4,4'-oxybis[3-(trifluoromethyl)benzeneamine], or 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene.
[0031] <Tetracarboxylic acid component> Any tetracarboxylic acid component can be used. Examples of the tetracarboxylic acid component include cyclohexane tetracarboxylic acid, cyclohexane tetracarboxylic acid esters, cyclohexane tetracarboxylic acid dianhydride, cyclobutane tetracarboxylic acid, cyclobutane tetracarboxylic acid esters, cyclobutane tetracarboxylic acid dianhydride, cyclopentane tetracarboxylic acid, cyclopentane tetracarboxylic acid esters, cyclopentane tetracarboxylic acid dianhydride, and bicyclopentane tetracarboxylic acid dianhydride. Among these, cyclohexane tetracarboxylic acid dianhydride, cyclobutane tetracarboxylic acid dianhydride, and cyclopentane tetracarboxylic acid dianhydride are more preferred. Among the above, cyclohexane tetracarboxylic acid dianhydride is even more preferred. The above-mentioned various tetracarboxylic acid components include positional isomers.
[0032] More preferred specific examples of the tetracarboxylic acid component include 1,2,4,5-cyclohexanetetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride, 1,2,4,5-cyclohexanetetracarboxylic acid methyl ester, 1,2,3,4-butanetetracarboxylic acid, 1,2,3,4-butanetetracarboxylic acid dianhydride, 1,2,3,4-butanetetracarboxylic acid methyl ester, 1,2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cyclobutanetetracarboxylic acid dianhydride, 1,2,3,4-cyclobutanetetracarboxylic acid methyl ester, and 1,2,4,5-cyclopentanetetracarboxylic acid. , 1,2,4,5-cyclopentane tetracarboxylic acid dianhydride, 1,2,4,5-cyclopentane tetracarboxylic acid methyl ester, 3-carboxymethyl-1,2,4-cyclopentane tricarboxylic acid, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic acid, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic acid methyl ester, dicyclohexyl tetracarboxylic acid, dicyclohexyl tetracarboxylic acid dianhydride, and dicyclohexyl tetracarboxylic acid methyl ester. Among these, 1,2,4,5-cyclohexanetetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, and 1,2,4,5-cyclohexanetetracarboxylic acid methyl ester are particularly preferred because they are advantageous in that they can be easily increased in molecular weight when producing a polyimide resin and a flexible film can be easily obtained.
[0033] The tetracarboxylic acid component may contain other tetracarboxylic acids or derivatives thereof as long as the flexibility and thermocompression bondability of the finally obtained cured film, for example, the film, is not impaired. Examples of these other tetracarboxylic acids or derivatives thereof include pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, 2,2-bis(2,3-dicarboxyphenyl)propane, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(2,3-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane, bis(3,4-dicarboxyphenyl)sulfone, biphenyl, At least one selected from the group consisting of bis(3,4-dicarboxyphenyl)ether, bis(2,3-dicarboxyphenyl)ether, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2',3,3'-benzophenonetetracarboxylic acid, 4,4-(p-phenylenedioxy)diphthalic acid, 4,4-(m-phenylenedioxy)diphthalic acid, ethylenetetracarboxylic acid, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)methane, and derivatives thereof can be mentioned.
[0034] <Preparation method of polyimide resin> The polyimide resin (A) contained in the photosensitive resin composition of the present embodiment can be obtained by the following steps (1) and (2): Step (1): A tetracarboxylic acid component and a diamine component are reacted to obtain a polyimide resin having amino groups at the terminals. Step (2): The polyimide resin having an amino group at its terminal obtained in the above step (1) is reacted with the above functional group-containing compound (a compound having an isocyanate group or an epoxy group, and a (meth)acrylic group).
[0035] <Process (1)> The above-mentioned tetracarboxylic acid is reacted with a diamine component to obtain a polyimide resin having amino groups at its terminals. The organic solvent used when reacting the tetracarboxylic acid component with the diamine component is not particularly limited, but is preferably at least one selected from the group consisting of cyclic ethers, cyclic ketones, cyclic esters, amides, and ureas. Specific examples of suitable solvents are not particularly limited, but include at least one selected from the group consisting of aprotic polar organic solvents such as γ-butyrolactone, N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethylsulfoxide, hexamethylphosphoramide, cyclopentanone, cyclohexanone, 1,3-dioxolane, 1,4-dioxane, tetramethylurea, and tetrahydrofuran. Among these, it is more preferable to use at least one selected from the group consisting of γ-butyrolactone, N,N-dimethylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone.
[0036] An imidization catalyst can be used when reacting the tetracarboxylic acid component with the diamine component in step (1). The imidization catalyst is preferably a tertiary amine compound, and specifically, at least one selected from the group consisting of trimethylamine, triethylamine (TEA), tripropylamine, tributylamine, triethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, triethylenediamine, N-methylpyrrolidine, N-ethylpyrrolidine, N-methylpiperidine, N-ethylpiperidine, imidazole, pyridine, quinoline, and isoquinoline can be used.
[0037] The reaction temperature in step (1) is usually in the range of 160 to 200°C, preferably in the range of 170 to 190°C, and more preferably in the range of 180 to 190°C. If the temperature is 160°C or higher, imidization and high molecular weight can be sufficiently promoted. If the temperature is 200°C or lower, the solution viscosity can be appropriately maintained, and problems such as the resin being burned onto the wall of the reaction vessel can be avoided. In some cases, an azeotropic dehydrating agent such as toluene or xylene may be used. The reaction pressure is usually normal pressure, but the reaction can be carried out under pressure as necessary. The reaction temperature is preferably maintained for at least 1 hour, more preferably 3 hours or more. If the reaction temperature is maintained for 1 hour or more, imidization and high molecular weight can be sufficiently promoted. There is no particular upper limit to the reaction time, but the reaction is usually carried out within the range of 3 to 10 hours.
[0038] In step (1), it is preferable to react "A moles" of the tetracarboxylic acid component with "B moles" of the diamine component in the range of 0.80≦A / B≦0.99, and more preferably in the range of 0.85≦A / B≦0.95. By making A / B≦0.99, it is possible to make the terminals of the polyimide have an excess of diamine, and it is possible to obtain a polyimide resin having an amino group at the terminal, and a polyimide resin having a molecular weight with sufficient solvent solubility is obtained. If 0.80≦A / B, it is possible to obtain a polyimide resin having a molecular weight that exhibits sufficient flexibility. The closer A / B is to 1.0, the higher the molecular weight of the resulting polyimide resin will be. By appropriately adjusting A / B, it is possible to obtain a polyimide resin with the desired molecular weight.
[0039] <Process (2)> Step (2) is a step of modifying the terminals of the polyimide resin obtained in the above step (1). Specifically, as described above, polyimide is reacted with the above functional group-containing compound (a compound having an isocyanate group or an epoxy group and a (meth)acrylic group) to obtain a polyimide resin having a (meth)acrylic group at its terminal.
[0040] The functional group-containing compound that modifies the terminal of the polyimide resin is a compound having an isocyanate group or an epoxy group and a (meth)acrylic group, and specific examples thereof include 2-isocyanatoethyl methacrylate, 2-isocyanatoethyl acrylate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate, glycidyl methacrylate, and allyl glycidyl ether. These functional group-containing compounds may be used alone or in combination of two or more. The functional group-containing compound is preferably used in a molar ratio of 0.1 to 30 times the solid content in the solution containing the polyimide resin having a (meth)acrylic group at the terminal.
[0041] The reaction temperature in step (2) is preferably in the range of 30 to 100° C., and the reaction time is preferably 1 to 5 hours. When reacting the amino group terminal of the polyimide resin with the isocyanate group or epoxy group of the functional group-containing compound, the reaction may be performed as is, or may be performed in the presence of a catalyst as necessary. Examples of the catalyst include amine compounds such as triethylamine, and organic phosphorus compounds such as triphenylphosphine, which may be used alone or in combination of two or more. A polymerization inhibitor may be used to suppress side reactions during the reaction. Examples of the polymerization inhibitor include hydroquinone, hydroquinone monomethyl ether, and methylhydroquinone, which may be used alone or in combination of two or more.
[0042] The polyimide resin (A) contained in the photosensitive resin composition of this embodiment preferably has a light transmittance at a wavelength of 200 to 400 nm of 50% or more, more preferably 55% or more, even more preferably 60% or more, and still more preferably 70% or more.
[0043] The polyimide resin (A) contained in the photosensitive resin composition of the present embodiment has high light transmittance at the above wavelength and excellent solvent solubility. Therefore, the photopolymerization initiator that can be contained in the composition acts effectively, so that a cured film can be obtained efficiently. In addition, by using the polyimide resin (A) having a specific structure and a specific terminal structure and a specific molecular weight, when a cured film is formed from the composition described below, the residual film rate of the unexposed part is low, the film has excellent developability, and the occurrence of cracks can be effectively suppressed.
[0044] [Photosensitive polyimide resin composition] The photosensitive polyimide resin composition in this embodiment contains a polyimide resin (A) having the structure of the above general formula (1) and the terminal structure represented by general formula (2). In addition to the polyimide resin (A), it is preferable to contain at least one selected from the group consisting of a photopolymerization initiator, a solvent, and a photopolymerizable compound. It is also preferable to further contain a sensitizer.
[0045] Examples of the solvent include N-methyl-2-pyrrolidone, N-acetyl-2-pyrrolidone, N-benzyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphortriamide, N-acetyl-ε-caprolactam, dimethylimidazolidinone, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, γ-butyrolactone, etc. These solvents may be used alone or in combination of two or more. By using an appropriate solvent, the photosensitive resin composition of the present embodiment can be used in a solution (varnish) state, which is convenient for forming a film.
[0046] As the photopolymerizable compound, a polyfunctional radically polymerizable monomer, for example, a di- or higher functional (meth)acrylic monomer, can be used. Examples of (meth)acrylic monomers include tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethacrylate, polypropylene glycol diacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, tris-(2-acryloxyethyl)isocyanurate, ditrimethylolpropane tetraacrylate, dipentaerythritol hexaacrylate, etc. These photopolymerizable compounds may be used alone or in combination of two or more. The flexibility and heat resistance of the polyimide resin composition can be controlled by the structure of the photopolymerizable compound to be mixed. These photopolymerizable compounds are preferably mixed in a ratio of 5 to 500 parts by mass based on the solid content in the solution containing the polyimide resin having a (meth)acrylic group at its end.
[0047] The photopolymerization initiator is not particularly limited and known ones can be used. For example, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-methyl-1- Examples include (4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0048] These photopolymerization initiators may be used alone or in combination of two or more kinds. The photopolymerization initiator is preferably mixed in an amount of 0.1 to 10 parts by mass relative to the solid content in the solution containing the polyimide resin (A) having a (meth)acrylic group at its end.
[0049] The sensitizer is not particularly limited, and known sensitizers can be used. For example, an amino group-containing sensitizer can be mentioned, and a compound having an amino group and a phenyl group in the same molecule can be preferably exemplified. More specifically, benzophenone compounds such as 4,4'-dimethylaminobenzophenone, 4,4'-diethylaminobenzophenone, 2-aminobenzophenone, 4-aminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, and 3,4-diaminobenzophenone; 2-(p-dimethylaminophenyl)benzoxazole, 2-(p-diethylaminophenyl)benzoxazole, 2-(p-dimethylaminophenyl)benzo[4,5]benzoxazole, 2-(p-dimethylaminophenyl)benzo[6,7]benzoxazole, and 2,5-bis(p-diethylaminophenyl)-1,3,4-oxadiazole. p-Dialkylaminophenyl group-containing compounds such as 2-(p-dimethylaminophenyl)benzothiazole, 2-(p-diethylaminophenyl)benzothiazole, 2-(p-dimethylaminophenyl)benzimidazole, 2-(p-diethylaminophenyl)benzimidazole, 2,5-bis(p-diethylaminophenyl)-1,3,4-thiadiazole, (p-dimethylaminophenyl)pyridine, (p-diethylaminophenyl)pyridine, (p-dimethylaminophenyl)quinoline, (p-diethylaminophenyl)quinoline, (p-dimethylaminophenyl)pyrimidine, and (p-diethylaminophenyl)pyrimidine can be mentioned. These sensitizers may be used alone or in combination of two or more kinds. The sensitizer is preferably mixed in an amount of 0.001 to 10 parts by mass relative to the solid content in the solution containing the polyimide resin (A) having a (meth)acrylic group at its terminal.
[0050] The photosensitive resin composition of the present embodiment is not particularly limited, but can be prepared as follows. A photosensitive polyimide composition is obtained by mixing, as necessary, at least one selected from the group consisting of a solvent, a photopolymerization initiator, a photopolymerizable compound, and a sensitizer with polyimide resin (A) having a structure represented by general formula (1) and generally having a terminal structure represented by (2) or (3). The photosensitive resin composition of the present embodiment is particularly suitable for use in forming an insulating film.
[0051] [Cured film] In order to obtain the cured film of this embodiment, a solution containing the polyimide resin (A) having the above structural characteristics is applied onto a substrate. The method for applying the composition onto the substrate is not particularly limited, and specific examples thereof include an inkjet method, a spin coating method, a casting method, a microgravure method, a gravure coating method, a bar coating method, a roll coating method, a wire bar coating method, a dip coating method, a spray coating method, a screen printing method, a flexographic printing method, and a die coating method.
[0052] When applying onto a substrate, it is preferable to adjust the solid content concentration of the solution containing the polyimide resin (A) of this embodiment to be in the range of 5 to 50 mass %. As the solvent used for application, an aprotic polar solvent is preferable from the viewpoint of solubility. Specifically, N-methyl-2-pyrrolidone, N-acetyl-2-pyrrolidone, N-benzyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphortriamide, N-acetyl-ε-caprolactam, dimethylimidazolidinone, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, γ-butyrolactone, etc. can be mentioned as suitable examples. These solvents may be used alone or in combination of two or more. In order to further improve the application property, solvents such as toluene, xylene, diethyl ketone, methoxybenzene, cyclopentanone, etc. may be mixed within a range that does not adversely affect the solubility of the polymer.
[0053] Examples of the substrate include glass, silicon wafers, metal foils, and plastic films. Among the metal foils, silicon wafers and copper foils are particularly preferred.
[0054] The photosensitive resin composition of the present embodiment applied onto the substrate is irradiated with light (usually ultraviolet light) through a photomask having a predetermined pattern. After irradiation, the unexposed areas are dissolved and removed with a developer to obtain a desired relief pattern. The cumulative amount of UV radiation is 500 to 8,000 mJ / cm 2 It is preferable that:
[0055] In the resin pattern forming method using the photosensitive resin composition of this embodiment, it is preferable to use an organic solvent as the developer. The developer is not particularly limited as long as it dissolves the photosensitive resin composition of this embodiment. Specifically, N-methyl-2-pyrrolidone, N-acetyl-2-pyrrolidone, N-benzyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphortriamide, N-acetyl-ε-caprolactam, dimethylimidazolidinone, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, γ-butyrolactone, and the like are preferred examples. These developers may be used alone or in combination of two or more.
[0056] The relief pattern formed by development is then washed with a rinse solution to remove the developing solvent. Suitable examples of the rinse solution include methanol, ethanol, isopropyl alcohol, water, and the like, which are well miscible with the developing solution. The relief pattern obtained by the above-mentioned treatment is heated at a temperature selected from the range of 80 to 250° C. to dry the solvent, and a cured film obtained by curing the photosensitive resin composition of the present embodiment can be obtained. According to the present embodiment, a resin composition having excellent developability, i.e., an exposed portion is sufficiently cured and an unexposed portion is sufficiently removed, is used, so that the resulting relief pattern can have high resolution.
[0057] Specifically, the cured film obtained by curing the photosensitive resin composition according to this embodiment has an exposure dose of 1,500 to 2,500 mJ / cm at a wavelength of 365 nm. 2 The residual film ratio of the unexposed portion after exposure under the above conditions is preferably 45% or less, more preferably 40% or less, even more preferably 30% or less, and even more preferably 10% or less. The exposure light source is not particularly limited, but for example, a high-pressure mercury lamp can be used, and exposure is performed at 365 nm to achieve the above exposure amount. In this specification, the term "unexposed portion remaining film ratio" refers to a value calculated from the following definition. The details of the measurement method will be described in detail in the Examples. Unexposed area remaining film ratio (%) = [mass of unexposed area after development / mass of unexposed area before development] x 100
[0058] The cured film obtained by curing the photosensitive resin composition according to this embodiment has a residual film rate in exposed areas of preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more. In this specification, the term "exposed area remaining film ratio" refers to a value calculated from the following definition. The details of the measurement method will be described in detail in the Examples. Residual film rate of exposed area (%) = [mass of exposed area after development / mass of exposed area before development] x 100
[0059] The thickness of the cured film obtained by this embodiment is preferably 10 to 85 μm. When the thickness is within the above range, it can be used as an excellent insulating film. As the thickness increases (i.e., the amount of the photosensitive resin composition applied to the substrate increases), problems often occur, particularly with respect to the solvent solubility of the polyimide resin. However, according to the present invention, by using a polyimide resin having a specific structure and a specific terminal structure and a specific molecular weight range, it is possible to achieve both excellent solvent solubility and transparency even in such a situation. Therefore, the cured film of the present embodiment can be suitably used, for example, in insulating film applications where application of high voltage is expected. The cured film obtained from the photosensitive resin composition of the present embodiment, which contains the polyimide resin (A) having a specific structure and a specific terminal structure and a specific molecular weight, can effectively suppress the occurrence of cracks and has excellent physical properties.
[0060] [Application] The photosensitive resin composition and cured film of the present embodiment can be used in various applications, such as a surface protection film for semiconductor elements in electronic devices, an interlayer insulating film, and a wiring protection insulating film for circuit boards, and can be particularly suitably used in the above applications involving high density and high integration. EXAMPLES
[0061] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way. The evaluation methods employed in the present examples and comparative examples are as follows.
[0062] (1) Weight average molecular weight and number average molecular weight The weight average molecular weight (Mw) and number average molecular weight (Mn) were determined by GPC analysis using the following apparatus and conditions: Equipment: Viscotek TDAmax (Malvern Panalytical Ltd.) Column: A6000M × 2 (Malvern Panalytical Ltd.) Eluent: dimethylformamide with 20 mM lithium bromide Flow rate: 1.0ml / min Column temperature: 40℃ Detector: RI (Refractive Index Detector), RALS (Light Scattering Detector), LALS (Light Scattering Detector)
[0063] (2) Residual film rate in unexposed areas (%) In the following examples and comparative examples, a varnish containing a photosensitive resin composition containing a polyimide resin is prepared. The varnish obtained in each example and comparative example was applied to a silicon wafer using a spin coater, and then heated at 100°C for 60 minutes to remove the solvent. The mass of the varnish at this point (the point at which the solvent was removed under the above conditions) was taken as the pre-development mass of the unexposed area. After immersing in γ-butyrolactone as a developer for 5 minutes, the wafer was washed using methanol as a rinse solution, and the solvent was removed under air circulation until there was no change in mass. The mass of the film remaining on the silicon wafer after the solvent removal was taken as the post-development mass of the unexposed area, and the unexposed area remaining film ratio was calculated by the following formula. Unexposed area remaining film ratio (%) = [mass of unexposed area after development / mass of unexposed area before development] x 100
[0064] (3) Residual film rate in exposed area (%) In the following examples and comparative examples, a varnish containing a photosensitive resin composition containing a polyimide resin is prepared. The varnish obtained in each example and comparative example was applied to a silicon wafer using a spin coater, and then heated at 100°C for 60 minutes to remove the solvent. The mass of the varnish at this point (the point at which the solvent was removed under the above conditions) was taken as the pre-development mass of the exposed area. After UV irradiation and immersion in γ-butyrolactone developer for 5 minutes, the wafer was washed using methanol as a rinse solution, and the solvent was removed under air flow until no mass change occurred. The mass of the film remaining on the silicon wafer after the solvent removal was taken as the post-development mass of the exposed area, and the remaining film ratio was calculated by the following formula. Residual film rate of exposed area (%) = [mass of exposed area after development / mass of exposed area before development] x 100
[0065] The equipment and conditions used for the development of (2) and (3) above are as follows. Ultraviolet irradiation device: ECS-1511U (manufactured by iGraphics Co., Ltd.) Light source: High pressure mercury lamp Illuminance: 670~700mW / cm 2 Accumulated light output: 2,400mJ / cm 2 Developer: γ-butyrolactone Development time: 5 minutes Rinse solution: Methanol Silicon wafer: 4-inch silicon wafer (Advantec Co., Ltd.)
[0066] Synthesis Example 1 In a 500 ml five-neck flask equipped with a nitrogen inlet tube, a stirrer, a thermometer, and a condenser, 97.279 g (0.28 mol) of 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene (hereinafter, BiS-AP), 32.141 g (0.12 mol) of 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine (hereinafter, TMDA), 18.754 g (0.19 mol) of triethylamine (hereinafter, TEA), 0.083 g (0.74 mmol) of triethylenediamine (hereinafter, TEDA), and 259.7 g of γ-butyrolactone (hereinafter, GBL) were added under nitrogen introduction, and the mixture was heated to 70°C with stirring. 82.943 g (0.37 mol) of 1,2,4,5-cyclohexanetetracarboxylic dianhydride (hereinafter, HPMDA) was added thereto and reacted at 180° C. for 5 hours. The mixture was diluted with 536.8 g of N,N-dimethylacetamide (hereinafter, DMAc) to obtain 995 g of polyimide varnish with a solid content concentration of 20 mass%. As a result of measurement by GPC, the weight average molecular weight of the polyimide obtained in this synthesis example was 15,800.
[0067] Synthesis Example 2 Except for changing the amount of BiS-AP to 93.921 g (0.27 mol), the amount of TMDA to 31.126 g (0.12 mol), the amount of TEA to 18.72 g (0.19 mol), the amount of TEDA to 0.083 g (0.74 mmol), the amount of GBL to 254.8 g, and the amount of DMAc to 524.3 g, 973 g of polyimide varnish was obtained in the same manner as in Synthesis Example 1. As a result of GPC measurement, the weight average molecular weight of the polyimide obtained in this Synthesis Example was 27,000.
[0068] Synthesis Example 3 Except for changing the amount of BiS-AP to 92.462 g (0.27 mol), the amount of TMDA to 30.642 g (0.12 mol), the amount of TEA to 18.72 g (0.19 mol), the amount of TEDA to 0.083 g (0.74 mmol), the amount of GBL to 252.4 g, and the amount of DMAc to 519.3 g, 964 g of polyimide varnish was obtained in the same manner as in Synthesis Example 1. As a result of GPC measurement, the weight average molecular weight of the polyimide obtained in this Synthesis Example was 33,200.
[0069] Synthesis Example 4 The same procedure as in Synthesis Example 1 was repeated to obtain 959 g of polyimide varnish, except that the amount of BiS-AP was 91.513 g (0.27 mol), the amount of TMDA was 30.327 g (0.11 mol), the amount of TEA was 18.72 g (0.19 mol), the amount of TEDA was 0.083 g (0.74 mmol), the amount of GBL was 250.9 g, and the amount of DMAc was 516.1 g. As a result of GPC measurement, the weight average molecular weight of the polyimide obtained in this Synthesis Example was 42,800.
[0070] Synthesis Example 5 Except for changing the amount of BiS-AP to 90.401 g (0.26 mol), the amount of TMDA to 29.959 g (0.11 mol), the amount of TEA to 18.72 g (0.19 mol), the amount of TEDA to 0.083 g (0.74 mmol), the amount of GBL to 249.0 g, and the amount of DMAc to 512.3 g, 952 g of polyimide varnish was obtained in the same manner as in Synthesis Example 1. As a result of GPC measurement, the weight average molecular weight of the polyimide obtained in this Synthesis Example was 75,600.
[0071] Synthesis Example 6 Except for changing the amount of BiS-AP to 0.00g (0.00mol), the amount of TMDA to 103.720g (0.39mol), the amount of TEA to 1.871g (0.018mol), the amount of TEDA to 0.0g (0.00mmol), the amount of GBL to 228.3g, and the amount of DMAc to 464.1g, 865g of polyimide varnish was obtained in the same manner as in Synthesis Example 1. As a result of GPC measurement, the weight average molecular weight of the polyimide obtained in this Synthesis Example was 14,000.
[0072] Synthesis Example 7 The amount of BiS-AP was 0.00g (0.00mol), the amount of TMDA was 0.00g (0.00mol), 130.950g (0.39mol) of 4,4'-oxybis[3-(trifluoromethyl)benzeneamine] (hereinafter, 6FODA) was added as an aromatic diamine, the amount of TEA was 1.871g (0.018mol), the amount of TEDA was 0.0g (0.00mmol), the amount of GBL was 261.6g, and the amount of DMAc was 539.7g. Except for this, 1002g of polyimide varnish was obtained in the same manner as in Synthesis Example 1. As a result of GPC measurement, the weight average molecular weight of the polyimide obtained in this Synthesis Example was 23,100.
[0073] Synthesis Example 8 The amount of BiS-AP was 0.00g (0.00mol), the amount of TMDA was 31.13g (0.12mol), 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene (hereinafter, BiS-AM) was 93.92g (0.27mol) as an aromatic diamine, the amount of TEA was 21.248g (0.21mol), the amount of TEDA was 0.094g (0.83mmol), the amount of GBL was 254.6g, and the amount of DMAc was 525.4g, but the same procedure as in Synthesis Example 1 was used to obtain 975g of polyimide varnish. As a result of GPC measurement, the weight average molecular weight of the polyimide obtained in this Synthesis Example was 28,100.
[0074] The average molecular weights of the polyimide resins obtained in Synthesis Examples 1 to 8 above are summarized in Table 1.
[0075] [Table 1]
[0076] Example 1 160g of the polyimide varnish obtained in Synthesis Example 1, 4.95g of 2-isocyanatoethyl acrylate (manufactured by Showa Denko K.K., Karenz AOI), and 0.05g of paramethoxyphenol (hereinafter, MEHQ) were added and reacted at 50°C for 5 hours. Thereafter, the reaction liquid was dropped into water to precipitate polyimide, and the polyimide was dried overnight at 70°C to obtain polyimide resin (A). 3g of this polyimide resin (A) was dissolved in 10g of GBL, and 0.75g of trimethylolpropane triacrylate (TMP-TA), 0.045g of 1-hydroxycyclohexyl phenyl ketone (manufactured by BASF, IRGACURE184), and 0.105g of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (manufactured by BASF, IRGACURE819) were added and stirred until dissolved to obtain a photosensitive resin composition (photosensitive resin varnish). This photosensitive resin composition was applied onto a silicon wafer and dried at 100°C for 60 minutes. The wafer was then immersed in GBL for 5 minutes, rinsed with methanol, and the solvent was removed under airflow until there was no change in mass, and the unexposed remaining film ratio was calculated. The unexposed remaining film ratio at this time was 0%. The photosensitive resin composition was also applied onto a silicon wafer and dried at 100°C for 60 minutes, and then measured using an Aimini Grandage (ECS-1511U) manufactured by AiGraphics Co., Ltd., a high-pressure mercury lamp was used as the light source, and an exposure dose of 1,500 to 2,500 mJ / cm at an exposure wavelength of 365 nm was measured. 2 The film was exposed to light under the conditions of 100% to form a cured film, then immersed in GBL for 5 minutes, rinsed with methanol, and the solvent was removed under air circulation until there was no change in mass, and the exposed area residual film ratio was calculated. The exposed area residual film ratio at this time was 100%. The results are shown in Table 2.
[0077] Examples 2 to 9 and Comparative Example 1 A photosensitive resin composition was prepared in the same manner as in Example 1 above, except for the formulation shown in the table below, and its properties were evaluated. The results are also shown in Table 2.
[0078] [Table 2]
[0079] It is found that the cured film containing the photosensitive resin composition according to this embodiment has excellent developability compared to Comparative Example 1. It was also confirmed that the cured film containing the photosensitive resin composition according to this embodiment does not crack.
Claims
1. A photosensitive resin composition comprising a polyimide resin (A) having a structure represented by the following general formula (1) and having a weight average molecular weight of 70,000 or less: 【Chemistry 1】 In general formula (1), R is a tetravalent group having 4 to 10 carbon atoms and having a cyclic structure, a non-cyclic structure, or a cyclic structure and a non-cyclic structure. A is at least one group selected from the group consisting of the structures shown below. 【Chemistry 2】 [In the formula, * indicates a bond.] n represents the number of repeating units. The terminals of the general formula (1) are either a group represented by the following formula (2) or formula (3) or a hydrogen atom, and at least one of the terminals is a group represented by the following formula (2) or formula (3). 【Chemistry 3】 [In the general formulas (2) and (3), X and X 2 are each independently a group having 2 to 15 carbon atoms, and may have at least one group selected from the group consisting of an ester bond and a double bond. 2 are each independently a hydrogen atom or a methyl group.
2. 2. The photosensitive resin composition according to claim 1, wherein the polyimide resin (A) has a weight average molecular weight of 5,000 or more.
3. 3. The photosensitive resin composition according to claim 1, wherein the polyimide resin (A) has a light transmittance of 50% or more in the wavelength range of 200 to 400 nm.
4. Exposure dose at wavelength 365 nm: 1,500 to 2,500 mJ / cm 2 The photosensitive resin composition according to any one of claims 1 to 3, wherein a residual film rate of an unexposed portion after exposure under the above conditions is 40% or less.
5. The photosensitive resin composition according to any one of claims 1 to 4, further comprising at least one selected from the group consisting of a photopolymerization initiator, a solvent, and a photopolymerizable compound.
6. The photosensitive resin composition according to claim 5 , wherein the photopolymerizable compound is a polyfunctional radically polymerizable monomer.
7. The photosensitive resin composition according to any one of claims 1 to 6, further comprising a sensitizer.
8. The photosensitive resin composition according to any one of claims 1 to 7, which is used for forming an insulating film.
9. A cured film obtained by curing the photosensitive resin composition described in any one of claims 1 to 8.
10. The cured film according to claim 9, having a film thickness of 10 to 85 μm.
Citation Information
Patent Citations
Photosensitive polyimide composition and pattern forming method by using same
JP2000147761A
Photosensitive resin composition and application thereof
JP2011180571A
Photosensitive resin composition
JP2013076845A
New polyimide composition
JP2017513959A
Photosensitive polyimide composition