Conductive film, photoelectron device, and method for producing conductive film

A conductive film with two regions of varying transmittance, using a fluorine-containing polymer for patterning, addresses the stability and transparency issues in optoelectronic devices, enhancing device performance and manufacturing efficiency.

JP7574851B2Active Publication Date: 2024-10-29AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022533893
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-30
Filing Date
2021-06-22
Publication Date
2024-10-29
Estimated Expiration
2041-06-22

AI Technical Summary

Technical Problem

Existing conductive films in optoelectronic devices face challenges in achieving both low wiring resistance and high optical transparency, with conventional materials like organic semiconductor materials and PTFE being unstable during deposition, leading to reduced device performance and potential contamination.

Method used

A conductive film with two regions of different light transmittances is created using a fluorine-containing polymer and a conductive material, where the fluorine-containing polymer is deposited as a resin film to pattern the conductive material, ensuring stability and precise patterning without contamination.

Benefits of technology

The solution allows for a conductive film with reduced wiring resistance and high optical transparency, facilitating stable and efficient manufacturing of optoelectronic devices with improved performance and longevity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574851000013
    Figure 0007574851000013
  • Figure 0007574851000014
    Figure 0007574851000014
  • Figure 0007574851000015
    Figure 0007574851000015
Patent Text Reader

Abstract

Provided are: a novel conductive film that has two types of regions with different light transmittance; an optoelectronic element that has such a conductive film; and a conductive film manufacturing method that enables straightforward manufacture of such a conductive film. A conductive film has a first region, and a second region that exhibits a higher light transmittance than the first region, the conductive film having a first film made from a conductive material, and a resin film made from a fluoropolymer. The first film is disposed to overlap at least the first region, from between the first and second regions; the resin film is disposed to overlap the second region; and the fluoropolymer satisfies equations (1) and (2) below. (1) If the temperature is elevated at a temperature elevation rate of 2°C / min under a pressure of 1×10-3Pa, the temperature at which the thermal weight loss rate reaches substantially 100% is 400°C or below. (2) If the temperature is elevated at the temperature elevation rate of 2°C / min under a pressure of 1×10-3Pa, the temperature range from the temperature at which the thermal weight loss rate is 10% to the temperature at which same reaches 90% is 200°C or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive film, an optoelectronic device, and a method for manufacturing the conductive film. [Background technology]

[0002] In various optoelectronic devices, optical transparency, which affects the input and output of optical information, is a very important factor. The primary factor hindering optical transparency is the low optical transparency of the conductive film used as an electrode. In general, to ensure stable operation of optoelectronic devices, it is necessary to keep the wiring resistance of the electrodes below a certain level. Taking a display panel as an example, as the panel size increases, IR drop becomes more likely to occur, causing problems such as voltage distribution within the panel surface, and so measures such as thickening the electrodes to keep the sheet resistance of the electrodes low are required. However, on the other hand, the thicker the electrode, the lower its optical transparency becomes, which becomes a factor hindering the optical transparency of optoelectronic devices, and thus there is a contradictory problem. To address these issues, a conductive film having two regions with different light transmittances is known. In the following description, the region with the relatively low light transmittance may be referred to as the "first region" and the region with the high light transmittance may be referred to as the "second region." Such conductive films are used, for example, in organic electroluminescence elements (hereinafter, organic EL elements) and photoelectric conversion elements.

[0003] A known method for manufacturing such conductive films involves first forming a pattern film from a material that suppresses the formation of a metal film, and then forming a metal film on top of the pattern film by vapor deposition, sputtering, or the like (see, for example, Patent Document 1 and Non-Patent Document 1).

[0004] Specifically, in the method described in Patent Document 1, an organic semiconductor material such as a polycyclic aromatic compound or poly tetrafluoroethylene (PTFE) is proposed as the above-mentioned "material that suppresses the formation of a metal film."

[0005] In addition, in the method described in Non-Patent Document 1, a solution of a fluorine-containing compound is used as the "material for suppressing the formation of a metal film" and a pattern is formed by a printing process.

[0006] According to this method, the metal is deposited while avoiding the pattern film formed beforehand. As a result, a second region with high light transmittance is formed in the region where the pattern film is formed with a material that suppresses the formation of the metal film. Also, a large amount of metal is deposited in the region where the pattern film is not formed, forming a first region with relatively low light transmittance, and a conductive film having each region formed is obtained. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] U.S. Patent No. 10270033 [Non-patent literature]

[0008] [Non-Patent Document 1] Materials Horizons, 2020, 7, 143-148 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the above method has the following problems. First, the organic semiconductor material used in the method described in Patent Document 1 has an insufficient effect of suppressing the formation of a metal film, and there is room for improvement. In addition, the known PTFE described in Patent Document 1 is easily depolymerized or thermally decomposed during deposition, making it difficult to form a stable pattern. Furthermore, if outgassing or partial decomposition products generated by such depolymerization or thermal decomposition remain in the conductive film, there is a risk of reducing the element performance or element life of an electronic device having the conductive film.

[0010] Furthermore, in the method described in Non-Patent Document 1, a solution of a fluorine-containing compound is applied, but the solvent may deteriorate the structure of the printed area and reduce the performance of the element.

[0011] The present invention has been made in view of the above circumstances, and has an object to provide a novel conductive film having two regions with different light transmittances. Another object of the present invention is to provide a photoelectron device having such a conductive film. Another object of the present invention is to provide a method for producing a conductive film that enables such a conductive film to be easily produced. [Means for solving the problem]

[0012] In order to solve the above problems, one aspect of the present invention includes the following aspects.

[0013] [1] A conductive film having a first region and a second region exhibiting a higher light transmittance than the first region, the conductive film comprising a first film made of a conductive material and a resin film made of a fluoropolymer, the first film being disposed so as to overlap at least the first region of the first and second regions, the resin film being disposed so as to overlap the second region, and the fluoropolymer satisfying the following (1) and (2): (1) 1×10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 1×10 Pa, the temperature at which the thermal weight loss rate substantially reaches 100% is 400°C or lower. -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 200°C.

[0014] [2] The conductive film described in [1], comprising a second film made of a conductive material and spanning the first region and the second region, the second film having a higher light transmittance than the first film at a position overlapping with the first region, and the second film contacting the first film in the first region. [3] The conductive film according to [1] or [2], wherein the resin film has a surface energy of 30 mN / m or less. [4] The conductive film according to any one of [1] to [3], wherein the melting point of the fluorine-containing polymer is 300° C. or lower. [5] The conductive film according to any one of [1] to [3], wherein the fluorine-containing polymer is amorphous.

[0015] [6] The conductive film according to any one of [1] to [5], wherein the fluorine-containing polymer has a trifluoromethyl moiety, and the content of the trifluoromethyl moiety in the fluorine-containing polymer is 0.1 mmol / g or more. [7] The conductive film according to any one of [1] to [6], wherein the fluorine-containing polymer has a unit derived from a fluoroolefin. [8] The conductive film according to [7], wherein the fluorine-containing polymer has at least a unit derived from tetrafluoroethylene and a unit derived from perfluoroalkyl vinyl ether. [9] The conductive film according to any one of [1] to [8], wherein the fluorine-containing polymer has an aliphatic ring structure in its main chain.

[0016]

[10] An optoelectronic device having the conductive film according to any one of [1] to [9].

[11] The optoelectronic device according to

[10] , comprising: a substrate; an anode provided on the substrate; a cathode facing the anode; and an active layer disposed between the anode and the cathode, wherein the cathode is the conductive film.

[0017]

[12] A method for producing a conductive film, comprising the steps of: forming a resin film made of a fluorine-containing polymer that satisfies the following (1) and (2) on a substrate by mask deposition; and dry-coating the resin film with a conductive material. -3 When the temperature is increased at a rate of 2°C / min under a pressure of 1×10 Pa, the temperature at which the thermal weight loss rate substantially reaches 100% is 400°C or lower. -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 200°C.

[13] The method for producing a conductive film according to

[12] , further comprising the step of removing the resin film after the dry coating step.

[14] The method for producing a conductive film according to

[12] or

[13] , further comprising the step of forming a film of a conductive material on the surface of the base material prior to the step of forming the resin film. Effect of the Invention

[0018] According to the present invention, it is possible to provide a novel conductive film having two regions with different light transmittances. It is also possible to provide a photoelectron device having such a conductive film. Furthermore, it is also possible to provide a method for manufacturing a conductive film that enables such a conductive film to be easily manufactured. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a plan view of a conductive film 1. As shown in FIG. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is a schematic diagram showing a method for producing the conductive film 1. As shown in FIG. [Figure 4] FIG. 4 is a schematic diagram showing a method for producing the conductive film 1. As shown in FIG. [Diagram 5] FIG. 5 is a schematic diagram showing a method for producing the conductive film 1. As shown in FIG. [Figure 6] FIG. 6 is a schematic diagram illustrating requirements (1) and (2). [Figure 7] FIG. 7 is a schematic diagram showing the conductive film 2 obtained by removing the resin film 15. As shown in FIG. [Figure 8] FIG. 8 is a schematic diagram showing the conductive film 3. As shown in FIG. [Figure 9] FIG. 9 is a cross-sectional view showing a schematic view of an optoelectronic device (organic EL device) 100 according to the second embodiment. [Figure 10] FIG. 10 is a graph showing the results of the example. [Figure 11] FIG. 11 is a graph showing the results of the example. [Figure 12] FIG. 12 is a graph showing the results of the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] In this specification, the term "unit" constituting a polymer means a portion derived from one monomer molecule (i.e., a monomer unit) that exists in the polymer and constitutes the polymer. Hereinafter, a unit derived from an individual monomer may be referred to by the name of the monomer followed by "unit."

[0021] As used herein, the "main chain" of a polymer refers to a carbon atom chain formed by addition polymerization of a monomer having a carbon-carbon unsaturated double bond, and composed of two carbon atoms that constituted the carbon-carbon unsaturated double bond in the monomer.

[0022] The term "reactive functional group" means a group having reactivity that can form a bond when heated or the like by reacting (excluding radical reactions) between molecules of the fluoropolymer or with other components blended together with the fluoropolymer.

[0023] In the present specification, the term "aliphatic ring" refers not only to a carbon ring structure whose ring skeleton is composed only of carbon atoms, but also to a heterocyclic ring structure whose ring skeleton contains an atom other than carbon atoms (heteroatom). Examples of the heteroatom include an oxygen atom, a nitrogen atom, and a sulfur atom.

[0024] [First embodiment] Hereinafter, a conductive film and a method for manufacturing a conductive film according to a first embodiment of the present invention will be described with reference to Fig. 1 to Fig. 8. In all the following drawings, the dimensions and ratios of each component are appropriately changed to make the drawings easier to understand.

[0025] 1 and 2 are explanatory diagrams showing a conductive film 1 of this embodiment. Fig. 1 is a plan view of the conductive film 1, and Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1.

[0026] As shown in FIGS. 1 and 2, the conductive film 1 of this embodiment has a first film 10, a resin film 15, and a second film 20. The conductive film 1 of this embodiment is provided on a substrate 50. The substrate 50 is an object on which the conductive film 1 is formed. The substrate 50 has optical transparency. The second film 20 is provided on the substrate 50, and the first film 10 is provided on the second film 20. The resin film 15 is provided between the first film 10 and the second film 20.

[0027] (1st membrane) The first film 10 is a film made of a conductive material. The conductive material of the first film 10 is not particularly limited as long as it is a material having conductivity, but preferably includes silver (Ag), gold (Au), copper (Cu), aluminum (Al), magnesium (Mg), zinc (Zn), indium (In), tin (Sn), ytterbium (Yb), etc. Specific examples include metals such as silver (Ag), gold (Au), copper (Cu), aluminum (Al), magnesium (Mg), magnesium silver (MgAg), and ytterbium silver (YbAg), and conductive metal oxides such as indium tin oxide (ITO), indium zinc oxide (IZO), and zinc oxide (ZnO).

[0028] The first film 10 has a first region 10A and a second region 10B having a higher light transmittance than the first region 10A. In the conductive film 1 of this embodiment, a thick film portion 11 of the first film (hereinafter simply referred to as the thick film portion 11) is located in the first region 10A, and a thin film portion 12 of the first film (hereinafter simply referred to as the thin film portion 12) is located in the second region 10B. The thick film portion 11 and the thin film portion 12 are integrated to form the first film 10.

[0029] 1, in the conductive film 1, a plurality of second regions 10B, i.e. a plurality of thin film portions 12, are arranged in a matrix, and the remaining portion has a lattice-shaped first region 10A, i.e., a lattice-shaped thick film portion 11. In FIG. 1, the second region 10B is rectangular in plan view, but is not limited thereto and various plan view shapes can be adopted according to the design.

[0030] The lower surface 11a of the thick film portion 11 is in contact with the second film 20. In addition, the side surface 11b of the thick film portion 11 is in contact with the resin film 15. The lower surface 12 a of the thin film portion 12 is in contact with the resin film 15 .

[0031] The thin film portion 12 is thinner than the thick film portion 11. For example, the thickness of the thick film portion 11 is 10 nm to 10000 nm, and the thickness of the thin film portion 12 is 0 nm to 50 nm. The thick film portion 11 formed to a thickness of 50 nm or less has optical transparency. The thick film portion 11 is formed to be thicker than the thin film portion 12 in order to ensure the conductivity of the entire conductive film 1. The thick film portion 11 may or may not be optically transparent as long as it can ensure the required conductivity.

[0032] (2nd membrane) The conductive film of this embodiment may or may not have a second film 20. (An embodiment without a second film will be described later as a conductive film 3.) When the conductive film of this embodiment has the second film 20, the second film 20 is provided on the surface 50a of the substrate 50. The second film 20 is a film made of a conductive material. Examples of the conductive material that is the material of the second film 20 include the same conductive materials that can be used as the material of the first film 10. The conductive material that is the material of the first film 10 and the conductive material that is the material of the second film 20 may be the same or different.

[0033] The second film 20 is optically transparent. The second film 20 has a higher optical transmittance than the thick film portion 11. The thickness of the second film 20 is preferably 0 nm to 200 nm, more preferably 0 nm to 100 nm, and further preferably 0 nm to 60 nm. Moreover, the second film 20 overlaps in plan view with the thin film portion 12. Therefore, the film thickness of the second film 20 and the total film thickness of the thin film portion 12 may be appropriately adjusted so that the second region 10B has optical transparency.

[0034] It is also possible to use only the second film 20 as a transparent electrode used in various optoelectronic elements such as a light emitting element, a light receiving element, etc. On the other hand, the second film 20 formed thin enough to have optical transparency has high wiring resistance. In contrast, the conductive film 1 of this embodiment is formed by laminating the second film 20 and the first film 10. Therefore, in the position overlapping with the first region 10A, the thick film portion 11 and the second film 20 are laminated to form a thick film. This allows the conductive film 1 to have a low resistance overall while ensuring light transparency in the position overlapping with the second region 10B.

[0035] (Resin film) The resin film 15 is made of a fluorine-containing polymer. The resin film 15 is disposed so as to overlap the second region 10B. The resin film 15 is used to pattern the first region 10A and the second region 10B of the first film 10, as will be described in the manufacturing method of the conductive film later.

[0036] The fluoropolymer, which is the material of the resin film 15, has low absorbance and a low refractive index, and therefore has the advantage of having little light absorption and excellent optical properties over a wide wavelength range including the near-infrared region. Therefore, even if the resin film 15 overlaps with the second region 10B, which has optical transparency, the resin film 15 does not inhibit the optical transparency of the second region 10B.

[0037] The fluorine-containing polymer that is the material of the resin film 15 satisfies the following requirements (1) and (2). (1) 1×10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 1 Pa, the temperature at which the thermal weight loss rate substantially reaches 100% is 400°C or lower. (2) 1×10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 200°C. A fluoropolymer satisfying the requirements (1) and (2) has properties suitable for the production method described below, and therefore, by using a fluoropolymer satisfying the requirements (1) and (2), the conductive film 1 can be suitably produced.

[0038] Hereinafter, the method for producing the conductive film of this embodiment will be described, and then the resin film 15 and the fluorine-containing polymer which is the material of the resin film 15 will be described in order.

[0039] (Method of manufacturing conductive film) 3 to 5 are schematic diagrams showing a method for producing the conductive film 1 described above. First, as shown in Fig. 3, the above-mentioned conductive material is formed on the surface of the substrate 50 to obtain the second film 20. The second film 20 can be formed by a dry coating method such as deposition, sputtering, CVD (chemical vapor deposition), or ALD (atomic layer deposition). The second film 20 corresponds to the "underlayer" of the present invention.

[0040] 4, a fluoropolymer P satisfying the above requirements (1) and (2) is deposited under reduced pressure on the surface 20a of the second film 20 through a mask M. The mask M has openings M2 arranged in a matrix and shielding portions M1 arranged in a lattice pattern. The deposition of the fluorine-containing polymer P is, for example, 1×10 -3 The reaction is carried out by heating the fluoropolymer under a pressure of 100 Pa.

[0041] The fluoropolymer P passes through the openings M2 of the mask M to reach the surface 20a of the second film 20, but is blocked by the blocking portions M1 of the mask M. In this way, a resin film 15 made of the fluoropolymer P is formed. The resin film 15 is arranged in a matrix on the surface 20a. In addition, in the areas where the resin film 15 is not formed, the second film 20 is exposed in a lattice pattern.

[0042] 5, the above-mentioned conductive material 10X is dry-coated on the resin film 15. For the dry coating, vapor deposition, sputtering, ALD (Atomic Layer Deposition), or the like can be used.

[0043] The conductive material 10X does not easily adhere to the surface of the resin film 15 made of a fluorine-containing polymer, but adheres easily to the surface of the second film 20 made of a conductive material. Therefore, by dry-coating the conductive material 10X all over the surface of the substrate 50 from above without using a mask, a relatively thick film of the conductive material 10X is formed on the surface of the second film 20, and a relatively thin film of the conductive material 10X is formed on the surface of the resin film 15.

[0044] As a result, lattice-shaped thick film portions 11 are formed on the surface of the second film 20. Furthermore, matrix-shaped thin film portions 12 are formed corresponding to the positions of the resin film 15. The thick film portions 11 and the thin film portions 12 constitute the first film 10.

[0045] This results in the conductive film 1. The location where the thick film portion 11 is formed is the first region 10A. Moreover, the location where the thin film portion 12 is formed is the second region 10B.

[0046] If thick film portion 11 is to be directly manufactured by mask vapor deposition, it is necessary to use a mask having shielding portions in a matrix. Such a mask requires a holding portion for holding the shielding portion, and therefore thick film portion 11 is not formed in the portion blocked by the holding portion, and the thickness of thick film portion 11 obtained is likely to vary. Alternatively, it is possible to form lattice-shaped thick film portion 11 by vapor deposition in multiple steps using a striped mask, but this makes it difficult to align the mask and the work complicated.

[0047] Furthermore, when the mask material is a metal, if thick film portion 11 is to be manufactured by vapor deposition, the vapor-deposited conductive material 10X may gradually adhere to the metal mask, causing the size of the opening in the mask to change. In this case, it is necessary to either wash away conductive material 10X adhering to the metal mask or replace it with a new mask, which requires complicated work and huge costs.

[0048] On the other hand, in the above-mentioned manufacturing method, as shown in Fig. 5, a resin film 15 made of a fluorine-containing polymer P is formed, and then a conductive material 10X is deposited on the entire surface, thereby obtaining a first film 10 in which thick film portions 11 and thin film portions 12 are naturally patterned. The resin film 15 can be precisely formed by mask deposition. Therefore, according to the above-mentioned manufacturing method for a conductive film, a precisely patterned conductive film can be easily manufactured.

[0049] (Fluorine-containing polymer) Next, the fluorine-containing polymer will be described in detail.

[0050] (Requirement (1)) The fluoropolymer used in the above production method satisfies the requirement (1). (1) 1×10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 1 Pa, the temperature at which the thermal weight loss rate substantially reaches 100% is 400°C or lower.

[0051] In this embodiment, the thermal weight loss rate is a value measured using a vacuum differential thermobalance (VPE-9000, manufactured by Advance Riko Co., Ltd.). -3 The weight loss rate (%) of the fluoropolymer relative to its initial weight (50 mg) is measured when the temperature is raised from room temperature to 500° C. at a rate of 2° C. per minute under a vacuum of 100 Pa. The term "substantially" in requirement (1) means that when the thermal weight loss rate is measured under the above-mentioned conditions, the thermal weight loss is below the lower detection limit in the temperature range of 400°C or less, and no thermal weight loss can be confirmed.

[0052] It can be said that the lower the temperature at which the fluoropolymer of this embodiment satisfies the above requirement (1), the lower the molecular weight (degree of polymerization).

[0053] If a fluoropolymer not satisfying the above requirement (1) is to be vapor-deposited, it will be necessary to heat it to a temperature exceeding 400°C. On the other hand, if it is heated to a temperature range exceeding 400°C, the high temperature may cause the fluoropolymer to depolymerize or pyrolyze. In that case, the products generated by the depolymerization or pyrolysis may increase the internal pressure of the vacuum chamber used for vapor deposition. If the internal pressure of the vacuum chamber increases in this way, the vapor deposition conditions become unstable, and the quality of the obtained vapor-deposited film (resin film) may be unstable. Furthermore, when a fluoropolymer not satisfying the above requirement (1) is heated at a temperature exceeding 400°C, partially depolymerized or thermally decomposed fluoropolymer having a small molecular weight may be mixed into the resin film, which may result in a decrease in the heat resistance of the resin film. Furthermore, when a fluoropolymer not satisfying the above requirement (1) is heated at a temperature exceeding 400°C, the fluoropolymer having unstable terminals produced by depolymerization or thermal decomposition may be mixed into the resin film, possibly impairing the quality of the resin film and the element containing the resin film.

[0054] On the other hand, when the fluoropolymer satisfying the above requirement (1) is used as a material for deposition under vacuum, it can be suitably deposited by heating at a temperature of 400° C. or less, which allows deposition under stable deposition conditions without the risk of the above-mentioned depolymerization or thermal decomposition.

[0055] The fluorine-containing polymer of this embodiment is 1×10 -3 It is preferable that the thermal weight loss rate when heated at a heating rate of 2°C / min under a pressure of 10 Pa reaches substantially 100% at a temperature of 350°C or lower, i.e., the temperature at which the thermal weight loss rate reaches substantially 100% is 350°C or lower.

[0056] (Requirement (2)) The fluoropolymer used in the above production method satisfies the requirement (2). (2) 1×10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 200°C.

[0057] It can be said that the fluoropolymer of this embodiment has a narrower molecular weight distribution as the temperature range satisfying the above requirement (2) is narrower. If an attempt is made to produce a resin film using a fluoropolymer that does not satisfy the above requirement (2), the difference between the molecular weight of the fluoropolymer deposited at the beginning of deposition and the molecular weight of the fluoropolymer deposited at the end of deposition will be large, and the molecular weight of the fluoropolymer will change in the thickness direction of the same resin film, which may cause the physical properties of the resin film to be unstable. Furthermore, when resin films are produced continuously under the same conditions, if a fluoropolymer not satisfying the above requirement (2) is used, the quality of the produced resin films may vary from lot to lot. Furthermore, the low molecular weight substance contained in the fluorine-containing polymer may be generated as outgas during deposition and adhere to the inside of a vacuum chamber, thereby contaminating the vacuum chamber. For example, in the process of producing an optoelectronic device, such a contamination source may cause a reduction in the life span of the device or a short circuit, thereby seriously impairing the quality of the device.

[0058] On the other hand, in the case of a fluoropolymer satisfying the above requirement (2), the difference between the molecular weight of the fluoropolymer deposited at the beginning of deposition and that of the fluoropolymer deposited at the end of deposition is small, and the change in the molecular weight of the fluoropolymer in the thickness direction of the resin film is small. Therefore, the physical properties of the obtained resin film are likely to be stable. Furthermore, when resin films are continuously produced under the same conditions, the quality variation between lots of the produced resin films can be suppressed. Furthermore, since it does not contain low molecular weight substances that cause outgassing, there is no risk of contamination of the deposition chamber. The fluoropolymer of this embodiment preferably satisfies the above requirement (2) in a temperature range of 100°C or less, more preferably 60°C or less.

[0059] Methods for obtaining a fluorine-containing polymer having a narrow molecular weight distribution that satisfies the above requirement (2) include molecular weight adjustment by controlled polymerization such as living radical polymerization, and molecular weight fractionation by sublimation purification, supercritical extraction, and size exclusion chromatography.

[0060] Fig. 6 is a schematic diagram illustrating requirements (1) and (2), and is a graph showing the relationship between the measurement temperature and the thermal weight loss rate. The horizontal axis of Fig. 6 is the measurement temperature (unit: °C), and the vertical axis is the thermal weight loss rate (unit: %). In Fig. 6, the behavior of a fluoropolymer that satisfies requirements (1) and (2) is indicated by the symbol P, and the behavior of a fluoropolymer that does not satisfy requirements (1) and (2) is indicated by the symbol Px.

[0061] In Fig. 6, graph P showing the behavior of the fluoropolymer of this embodiment reaches 100% in terms of thermal weight loss at a temperature (Td100) lower than 400°C. In contrast, graph Px showing the behavior of a fluoropolymer not satisfying requirements (1) and (2) does not reach 100% in terms of thermal weight loss at 400°C. In addition, in FIG. 6, graph P showing the behavior of the fluoropolymer of this embodiment has a value W of Td90-Td10 of 200° C. or less. It is clear from FIG. 6 that the fluoropolymer of this embodiment undergoes a steep thermal weight loss between the temperature Td10 and the temperature Td90.

[0062] The occurrence of depolymerization, thermal decomposition and outgassing during deposition of the fluoropolymer can be evaluated as follows, taking note of the change in the internal pressure of the vacuum chamber.

[0063] (Method for evaluating chamber pressure changes during deposition) 0.1 g of fluoropolymer was charged into the vacuum deposition machine, and the pressure in the chamber was increased to 10 -4 After reducing the pressure to below Pa, a fluorine-containing polymer is deposited to a thickness of 200 nm at a deposition rate of 0.1 nm / sec. During this process, the pressure inside the chamber is monitored and the maximum pressure during deposition is measured. A fluoropolymer having a chamber pressure increase rate of 10 times or less, calculated using the following formula, is less susceptible to depolymerization, thermal decomposition and outgassing, and can be suitably deposited. Chamber pressure increase rate during deposition = Maximum pressure during deposition / Initial pressure before deposition Fluorine-containing polymers with an increase rate of more than 10 times are judged to be unsuitable for deposition because of the large amount of depolymerization, thermal decomposition, and outgassing.

[0064] (Molecular weight fraction) When a fluoropolymer to be used does not satisfy the above requirements (1) and (2), it can be fractionated by molecular weight to obtain the fluoropolymer of the present embodiment which satisfies the above requirements (1) and (2). A fluoropolymer satisfying the above requirements (1) and (2) can be obtained by molecular weight fractionation of a polymer. In the following description, the polymer to be subjected to molecular weight fractionation may be referred to as a "raw polymer."

[0065] Examples of the molecular weight fractionation method include a method in which the molecular weight is fractionated by sublimation purification, supercritical extraction, or size exclusion chromatography to prepare a polymer that satisfies requirements (1) and (2).

[0066] (sublimation purification) Sublimation purification is a technique in which the target compound is separated and recovered as a solid (or liquid) by utilizing the precipitation (or condensation) temperature difference of the compounds contained in the gaseous target compound after heating the target compound (raw polymer) under reduced pressure to sublimate or evaporate a part or all of the target compound. This type of sublimation purification can be performed using a sublimation purification device that has a feed section for feeding the target compound and a collection section for separating the target compound in the gaseous state according to the precipitation (or condensation) temperature and collecting it as a solid (or liquid), and that can maintain a high degree of vacuum.

[0067] The structure of the sublimation purification apparatus is not particularly limited, but for example, a so-called Mill-type sublimation purification apparatus consisting of a glass cooling tube, a flask-shaped glass container surrounding the cooling tube, and a vacuum exhaust device for reducing the pressure inside the glass container can be used. Also, as the sublimation purification apparatus, a glass tube-type sublimation purification apparatus including a cylindrical glass sublimation tube, a heating device for accommodating the sublimation tube inside and heating the sublimation tube, and a high vacuum exhaust device for reducing the pressure inside the sublimation tube can be used.

[0068] Hereinafter, sublimation purification of a fluoropolymer and a method for fractionating the molecular weight by sublimation purification will be described using a glass tube type sublimation purification apparatus as an example. Note that, although the case of collecting the fluoropolymer as a solid will be described as an example here, the case of collecting the fluoropolymer as a liquid can be similarly described.

[0069] In the sublimation purification of fluoropolymers, the raw polymer is charged into the sublimation tube, and the pressure is reduced to, for example, 1×10 -3 After increasing the degree of vacuum in the sublimation tube to 0.1 Pa or less, the feed section is heated using a heating device, whereby the fluorine-containing polymer contained in the raw polymer is sublimated or evaporated. In the sublimation tube, the region on the side of the feed section that is exhausted by the high vacuum exhaust device corresponds to the "collection section." The collection section is set at a temperature lower than the heating temperature of the feed section. The fluoropolymer sublimated or evaporated from the raw material polymer in the feed section precipitates and solidifies on the wall surface of the collection section, and is collected.

[0070] The collection temperature of the collection section corresponds to the temperature at which the fluoropolymer sublimes from a gas to a solid (precipitates), and corresponds to the molecular weight of the fluoropolymer. By providing a plurality of collection sections with different collection temperatures in the sublimation tube, the raw polymer can be fractionated into fluoropolymers with different molecular weights. Specifically, for example, when the feed section is heated to A°C and the collection section is heated to B°C and C°C from the side closer to the feed section (A>B>C), the collection section set at B°C collects a fluoropolymer in a molecular weight range that is in a gaseous state at A°C and a solid state at B°C. Similarly, the collection section set at C° C. collects a fluoropolymer in a molecular weight range which is gaseous at B° C. and solid at C° C. That is, the collection section set at C° C. collects, among the fluoropolymers contained in the raw material polymer, a fluoropolymer in the collection temperature range B° C.-C° C. which is gaseous at B° C. and solid at C° C.

[0071] The above-mentioned requirement (2) can be satisfied by controlling the collection temperature range as described above, for example, by collecting in a collection section having a collection temperature range of 200° C. The collected fluoropolymer is checked to see whether it satisfies requirement (2), and if it does not, the temperature conditions of the collection section are controlled to narrow the collection temperature range.

[0072] In the collection section, the lower the set temperature of the fluoropolymer collected, the lower the concentration of fluoropolymers collected. -3 The temperature at which the thermal weight loss rate under a pressure of 100 Pa reaches 100% is low, that is, the molecular weight of the fluoropolymer is small. The collection temperature range is preferably 200° C. or less, more preferably 100° C. or less, and even more preferably 60° C. or less. The smaller the collection temperature range, the less the fluctuation in the deposition conditions becomes, and the more likely it is that the quality of the resin film will be stable.

[0073] As long as the molecular weight fractionated fluoropolymer satisfies the requirements (1) and (2), a plurality of fluoropolymers having different collection temperature ranges may be mixed.

[0074] (Supercritical extraction) Supercritical extraction is a technique for obtaining an extract by utilizing the high solubility and diffusivity of a supercritical fluid. For example, supercritical CO2 is used as the supercritical fluid, and a relatively low molecular weight fluorine-containing polymer is dissolved in the supercritical CO2 to obtain an extract.

[0075] Furthermore, by using a fluorine-containing solvent as an additive (entrainer) for the supercritical fluid, the solubility of the fluorine-containing polymer in the supercritical fluid can be increased. The fluorine-containing solvent used as the entrainer is not particularly limited. For example, the fluorinophilic parameter P F A fluorine-containing solvent in which is 1 or more is preferred.

[0076] (Fluorophilic parameter P F ) 30 μL of the fluorine-containing solvent is dropped into a two-phase system of 3 g of toluene and 3 g of perfluoromethylcyclohexane, mixed thoroughly, and allowed to stand overnight, and then the fluorine-containing solvent contained in the toluene and the fluorine-containing solvent contained in the perfluoromethylcyclohexane are measured by gas chromatography. The concentration (unit: mL / L) of the fluorine-containing solvent in the toluene is expressed as M P The concentration of the fluorine-containing solvent in the perfluoromethylcyclohexane (unit: mL / L) is M F When the above formula is used, the fluorine-philic parameter P is calculated by the following formula (A). F Let us assume that. P F =M F / M P …(A)

[0077] Examples of the fluorine-containing solvent used as an entrainer include the following compounds.

[0078] 1,1,1,2,2,3,3,4,4,5,5,6,6-Tridecafluorohexane (AC-2000, manufactured by AGC) (P F =12) 1,1,1,2,2,3,3,4,4,5,5,6,6-Tridecafluorooctane (AC-6000, manufactured by AGC) (P F =5.6) Cytop CT-SOLV100E (AGC) (P F =8.2) Cytop CT-SOLV180 (AGC) (P F =∞) HFE7300 (manufactured by 3M) (P F =8.2) 1,1,1,2,2,3,4,5,5,5-Decafluoropentane (Vertre XF, manufactured by Chemours) (P F =3.7) 1H,1H,2H,2H-Perfluorooctanol (P F =1.1) 1,1,2,2-Tetrafluoroethyl-2,2,2-trifluoroethyl ether (AE-3000, manufactured by AGC) (PF =0.6) HCFC-225ca / HCFC-225cb(45 / 55)(P F =0.3) Perfluorobenzene (P F =0.3) Hexafluoro-2-propanol (P F =0.24) 1H,1H,7H-Perfluoroheptanol (P F =0.23) 1H,1H,5H-Perfluoropentanol (P F =0.1)

[0079] The extraction process can be carried out, for example, using supercritical CO2 under conditions of an extraction pressure of 7.4 MPa or higher and an extraction temperature of 31°C or higher. The extraction pressure is preferably 30 MPa or more, more preferably 50 MPa or more, and even more preferably 70 MPa or more. There is no particular limit to the upper limit of the extraction pressure, but it is preferably 100 MPa or less. The upper limit and lower limit of the extraction pressure can be combined in any way. The extraction temperature is preferably 40° C. or higher, and more preferably 80° C. or higher. The extraction temperature is preferably 300° C. or lower, more preferably 200° C. or lower, and even more preferably 100° C. or lower. The upper and lower limit values ​​of the extraction temperature can be combined in any manner. Within the above range, the desired molecular weight fractionation of the fluoropolymer can be carried out efficiently.

[0080] Molecular weight fractionation is also useful for the purpose of removing residual foreign matter such as initiators, chain transfer agents, solvents, by-products, etc., used in the polymerization process of the fluoropolymer. Since such residual foreign matter is generated as outgas during deposition and adheres to the inside of the vacuum chamber, which may contaminate the vacuum chamber, it is more preferable to carry out sublimation purification or supercritical extraction even when requirements (1) and (2) are met.

[0081] As long as the molecular weight fractionated fluoropolymer satisfies the requirements (1) and (2), a plurality of fluoropolymers extracted under different conditions may be mixed.

[0082] (Fluorine-containing polymer structure) The fluorine-containing polymer used in the conductive film and the method for producing a conductive film of this embodiment is not particularly limited in terms of the units constituting the polymer, so long as it is a fluorine-containing polymer that satisfies the above requirements (1) and (2).

[0083] The fluorine atom content of the fluorine-containing polymer is preferably 20% by mass or more, more preferably 40% by mass or more, further preferably 60% by mass or more, and particularly preferably 70% by mass or more. The higher the fluorine atom content, the lower the surface energy of the resulting resin film 15, and the more difficult it is for the conductive material 10X to adhere to the surface of the resin film 15. Therefore, when a fluorine-containing polymer having the above fluorine atom content is used, it is easy to pattern the thick film portion 11 and the thin film portion 12.

[0084] The fluorine atom content (mass %) is calculated by the following formula. (Fluorine atom content) = [19 x NF / MA] x 100 NF: the sum of the values ​​obtained by multiplying the total atomic weight of fluorine atoms constituting each type of unit constituting a fluorine-containing polymer by the molar ratio of that unit to all units. MA: the sum of the values ​​obtained by multiplying the total atomic weight of all atoms constituting the unit by the molar ratio of the unit to all units for each type of unit constituting the fluorine-containing polymer.

[0085] The above NF and MA are 1 H-NMR, 19 The NF and MA can be calculated from the molar ratio and terminal amount of the structural units of the fluoropolymer obtained by F-NMR, elemental analysis, and IR. In addition, the NF and MA can also be calculated from the charged amounts of the monomers and initiator used in the production of the fluoropolymer.

[0086] The fluorine-containing polymer preferably contains a trifluoromethyl moiety. The "trifluoromethyl moiety" refers to CF3-. The trifluoromethyl moiety includes not only a trifluoromethyl group, but also a part of a substituent such as CF3- contained in a pentafluoroethyl group.

[0087] The content of the trifluoromethyl moiety is preferably 0.1 mmol / g or more, more preferably 0.3 mmol / g or more, and even more preferably 0.6 mmol / g or more. The higher the content of the trifluoromethyl moiety, the lower the surface energy of the resin film 15. This makes it difficult for the conductive material 10X to adhere to the surface of the resin film 15 in the dry coating process shown in FIG. 5, and makes it easier to pattern the thick film portion 11 and the thin film portion 12.

[0088] The content (mmol / g) of trifluoromethyl moieties can be calculated by the following formula. (Trifluoromethyl moiety content) = [NCF3 / MA] x 1000 NCF3: the sum of values ​​obtained by multiplying the number of moles of trifluoromethyl moieties constituting the units by the molar ratio of the units to all units for each type of unit constituting the fluorinated polymer. MA: the sum of the values ​​obtained by multiplying the total atomic weight of all atoms constituting the unit by the molar ratio of the unit to all units for each type of unit constituting the fluorine-containing polymer. The above NCF3 and MA are 1 H-NMR, 19 NCF3 and MA can be calculated from the molar ratio and terminal amount of the structural units of the fluoropolymer obtained by F-NMR, elemental analysis, and IR. NCF3 and MA can also be calculated from the amounts of monomers and initiators used in the production of the fluoropolymer.

[0089] As the fluorine-containing polymer, the following polymer (1) and polymer (2) are preferred. Polymer (1): A fluorine-containing polymer having no aliphatic ring in the main chain and having a fluoroolefin unit. Polymer (2): A fluorine-containing polymer having an aliphatic ring in the main chain. In the present invention, as the fluorine-containing polymer, either one of the polymers (1) and (2) may be used alone, or the polymers (1) and (2) may be used in combination.

[0090] <Polymer (1)> The polymer (1) may be a homopolymer of a fluoroolefin, a copolymer of two or more kinds of fluoroolefins, or a copolymer of a fluoroolefin and another monomer copolymerizable with the fluoroolefin.

[0091] Examples of fluoroolefins include perfluoroolefins such as tetrafluoroethylene (TFE) and hexafluoropropene (HFP), and perfluoro(alkyl vinyl ethers) such as perfluoro(methyl vinyl ether) (PMVE), perfluoro(ethyl vinyl ether) (PEVE), and perfluoro(propyl vinyl ether) (PPVE). In addition, (perfluoroalkyl vinyl ether) can also be expressed as perfluoro(alkoxyethylene).

[0092] Further, the fluoroolefin may include fluoroolefins having hydrogen atoms or chlorine atoms, such as chlorotrifluoroethylene (CTFE), trifluoroethylene (TrFE), vinylidene fluoride (VdF), 1,2-difluoroethylene, and 1-fluoroethylene.

[0093] Examples of other monomers copolymerizable with fluoroolefins include olefins such as ethylene and propylene, aromatic vinyl compounds such as vinyl ethers, vinyl esters and styrene, allyl compounds such as allyl ethers, acryloyl compounds, and methacryloyl compounds. Also usable are fluorine-containing monomers having a perfluoroalkyl group or a perfluoropolyether group, such as vinyl ethers, vinyl esters, aromatic vinyl compounds, allyl compounds, acryloyl compounds and methacryloyl compounds.

[0094] In particular, the polymer (1) preferably has a perfluoro(alkyl vinyl ether) unit. More specifically, the fluorine-containing polymer preferably has a PPVE unit.

[0095] The crystallinity of polymer (1) changes as the content of the PPVE unit changes. Specifically, as the content of the PPVE unit in the fluoropolymer increases, the crystallinity of the fluoropolymer decreases.

[0096] The content of the PPVE unit is preferably 2 mol% or more, more preferably 4 mol% or more, and even more preferably 6 mol% or more, based on the total number of moles of all monomer units constituting the fluoropolymer. The content within the above range is preferable because the crystallinity of the obtained resin film is lower, the conductive material 10X is less likely to adhere to the surface of the resin film 15, and the thick film portion 11 and the thin film portion 12 are easily patterned.

[0097] Furthermore, the content of the PPVE unit is preferably 15 mol% or less, more preferably 12 mol% or less, and even more preferably 10 mol% or less, based on the total number of moles of all monomer units constituting the fluoropolymer. If it exceeds the above range, the softening temperature of the obtained resin film decreases, and there is a risk that the shape of the film made of the fluoropolymer cannot be maintained at the process temperature in the production of the element or under the conditions of use of the element.

[0098] When the polymer (1) is a copolymer, the proportion of the fluoroolefin unit is preferably 20 mol % or more, more preferably 40 mol % or more, and even more preferably 80 mol % or more.

[0099] As the polymer (1), a synthesized product or a commercially available product may be used.

[0100] Examples of the polymer (1) include the following polymers. Polytetrafluoroethylene (PTFE) Tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer (PFA) Tetrafluoroethylene / hexafluoropropylene copolymer (FEP) Tetrafluoroethylene / perfluoro(alkyl vinyl ether) / hexafluoropropylene copolymer (EPA) Ethylene / Tetrafluoroethylene Copolymer (ETFE) Polyvinylidene fluoride (PVDF) Polyvinyl fluoride (PVF) Polychlorotrifluoroethylene (PCTFE) Ethylene / chlorotrifluoroethylene copolymer (ECTFE)

[0101] Among these, a polymer in which all hydrogen atoms bonded to carbon atoms are substituted with fluorine is preferred because it is easy to pattern the thick film portion 11 and the thin film portion 12. That is, Polytetrafluoroethylene (PTFE), Tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer (PFA), Tetrafluoroethylene / hexafluoropropylene copolymer (FEP), Tetrafluoroethylene / perfluoro(alkyl vinyl ether) / hexafluoropropylene copolymers (EPA) are preferred.

[0102] The above-mentioned "tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer (PFA)" may be a polymer having at least tetrafluoroethylene units and perfluoro(alkyl vinyl ether) units, and further having other perfluoromonomer units.

[0103] The polymer (1) can be produced by a known method. As the polymer (1), a synthesized product or a commercially available product may be used.

[0104] <Polymer (2)> The polymer (2) is a fluorine-containing polymer having an aliphatic ring in the main chain.

[0105] The term "fluoropolymer having an aliphatic ring in the main chain" means that the fluoropolymer has a unit having an aliphatic ring structure, and at least one of the carbon atoms constituting the aliphatic ring is a carbon atom constituting the main chain. The aliphatic ring may be a ring having a heteroatom such as an oxygen atom.

[0106] The "main chain" of a polymer refers to the chain of carbon atoms derived from the two carbon atoms that constitute the polymerizable double bond in the case of a monoene polymer. In the case of a cyclopolymerizable diene cyclopolymer, it refers to a chain of carbon atoms derived from four carbon atoms constituting two polymerizable double bonds. Furthermore, in a copolymer of a monoene and a cyclopolymerizable diene, it refers to a chain of carbon atoms derived from the above two carbon atoms of the monoene and the above four carbon atoms of the diene.

[0107] When the monoene has a polymerizable double bond between one carbon atom constituting the ring structure of the aliphatic ring and an exocyclic carbon atom, the main chain of the polymer having the aliphatic ring in the main chain has one carbon atom constituting the ring structure that previously constituted the polymerizable double bond of the monoene. When the monoene has a polymerizable double bond between two adjacent carbon atoms constituting the ring structure of the aliphatic ring, the main chain of the polymer having the aliphatic ring in the main chain has two carbon atoms constituting the ring structure that previously constituted the polymerizable double bond of the monoene. In the case of the above-mentioned cyclopolymerizable diene, the main chain of the polymer having an aliphatic ring in the main chain has four carbon atoms which constituted the two polymerizable double bonds of the diene, and two to four of the four carbon atoms constitute the ring skeleton of the aliphatic ring.

[0108] The number of atoms constituting the ring skeleton of the aliphatic ring in the polymer (2) is preferably 4 to 7, and more preferably 5 to 6. That is, the aliphatic ring is preferably a 4- to 7-membered ring, and more preferably a 5- or 6-membered ring. When the aliphatic ring has a heteroatom as an atom constituting the ring, examples of the heteroatom include an oxygen atom and a nitrogen atom, and an oxygen atom is preferred. The number of heteroatoms constituting the ring is preferably 1 to 3, and more preferably 1 or 2.

[0109] The aliphatic ring may or may not have a substituent. The term "optionally having a substituent" means that a substituent may be bonded to an atom constituting the ring skeleton of the aliphatic ring.

[0110] The hydrogen atoms bonded to the carbon atoms constituting the aliphatic ring of the polymer (2) are preferably substituted with fluorine atoms. In addition, when the aliphatic ring has a substituent, and when the substituent has a hydrogen atom bonded to a carbon atom, the hydrogen atom is preferably substituted with a fluorine atom. Examples of the substituent having a fluorine atom include a perfluoroalkyl group, a perfluoroalkoxy group, and =CF2. The aliphatic ring in the polymer (2) is preferably a perfluoroaliphatic ring (an aliphatic ring in which all of the hydrogen atoms bonded to carbon atoms, including substituents, are substituted with fluorine atoms).

[0111] Examples of the polymer (2) include the following polymers (21) and (22). Polymer (21): a fluorine-containing polymer having a unit derived from a cyclic fluorine-containing monoene. Polymer (22): A fluorine-containing polymer having units formed by cyclopolymerization of a fluorine-containing diene capable of cyclopolymerization (hereinafter also simply referred to as "fluorine-containing diene").

[0112] Polymer (21): The term "fluorine-containing cyclic monoene" means a fluorine-containing monomer having one polymerizable double bond between carbon atoms constituting an aliphatic ring, and a fluorine-containing monomer having one polymerizable double bond between a carbon atom constituting an aliphatic ring and a carbon atom outside the aliphatic ring.

[0113] As the fluorine-containing cyclic monoene, the following compounds (1) and (2) are preferred. [ka] [where, X 1 , X 2 , X 3 , X 4 , Y 1 and Y 2are each independently a fluorine atom, a perfluoroalkyl group which may contain an ethereal oxygen atom (-O-), or a perfluoroalkoxy group which may contain an ethereal oxygen atom. 3 and X 4 may be bonded to each other to form a ring.

[0114] X 1 , X 2 , X 3 , X 4 , Y 1 and Y 2 The perfluoroalkyl group in the formula (I) preferably has 1 to 7 carbon atoms, and more preferably has 1 to 4 carbon atoms. The perfluoroalkyl group is preferably linear or branched, and more preferably linear. Specific examples of the perfluoroalkyl group include a trifluoromethyl group, a pentafluoroethyl group, and a heptafluoropropyl group, and the trifluoromethyl group is particularly preferred.

[0115] X 1 , X 2 , X 3 , X 4 , Y 1 and Y 2 The perfluoroalkoxy group in the above formula includes the above perfluoroalkyl group to which an oxygen atom (-O-) is bonded, and a trifluoromethoxy group is particularly preferred.

[0116] In formula (1), X 1 is preferably a fluorine atom. X 2 is preferably a fluorine atom, a trifluoromethyl group, or a perfluoroalkoxy group having 1 to 4 carbon atoms, and particularly preferably a fluorine atom or a trifluoromethoxy group. X 3 and X 4 are each independently preferably a fluorine atom or a perfluoroalkyl group having 1 to 4 carbon atoms, and particularly preferably a fluorine atom or a trifluoromethyl group. X 3 and X 4may be bonded to each other to form a ring. The number of atoms constituting the ring skeleton of the ring is preferably 4 to 7, and particularly preferably 5 to 6.

[0117] Preferred specific examples of the compound (1) include the compounds (1-1) to (1-5). [ka]

[0118] In formula (2), Y 1 and Y 2 are each independently preferably a fluorine atom, a perfluoroalkyl group having 1 to 4 carbon atoms, or a perfluoroalkoxy group having 1 to 4 carbon atoms, and particularly preferably a fluorine atom or a trifluoromethyl group.

[0119] Preferred specific examples of the compound (2) include the compounds (2-1) and (2-2). [ka]

[0120] The polymer (21) may be a homopolymer of the above-mentioned fluorine-containing cyclic monoene, or a copolymer of the above-mentioned fluorine-containing cyclic monoene and another monomer copolymerizable therewith. However, the proportion of units derived from fluorinated cyclic monoenes to all units in the polymer (21) is preferably at least 20 mol %, more preferably at least 40 mol %, and even more preferably 100 mol %.

[0121] Examples of other monomers copolymerizable with the fluorine-containing cyclic monoenes include fluorine-containing dienes, monomers having a reactive functional group in the side chain, tetrafluoroethylene, chlorotrifluoroethylene, perfluoroalkyl vinyl ethers, and the like.

[0122] Examples of the fluorine-containing diene include those mentioned in the description of the polymer (22) described below. Examples of the monomer having a reactive functional group in the side chain include a monomer having a polymerizable double bond and a reactive functional group. Examples of the polymerizable double bond include CF2=CF-, CF2=CH-, CH2=CF-, CFH=CF-, CFH=CH-, CF2=C-, CF=CF-, etc. The polymer obtained by copolymerization of a fluorinated cyclic monoene and a fluorinated diene is referred to as polymer (21).

[0123] Polymer (22): The "fluorine-containing diene" is a fluorine-containing monomer having two polymerizable double bonds and a fluorine atom, which can undergo cyclic polymerization. As the polymerizable double bond, a vinyl group, an allyl group, an acryloyl group, or a methacryloyl group is preferable. As the fluorine-containing diene, the following compound (3) is preferable. CF2=CF-Q-CF=CF2 (3)

[0124] In formula (3), Q is a perfluoroalkylene group having 1 to 5 carbon atoms, preferably 1 to 3 carbon atoms, which may contain an ether oxygen atom and may have a branch, in which some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Examples of the halogen atoms other than fluorine atoms include chlorine atoms and bromine atoms.

[0125] Q is preferably a perfluoroalkylene group containing an etheric oxygen atom.In this case, the etheric oxygen atom in the perfluoroalkylene group may be present at one end of the perfluoroalkylene group, may be present at both ends of the perfluoroalkylene group, or may be present between the carbon atoms of the perfluoroalkylene group.From the viewpoint of cyclic polymerization, it is preferable that an etheric oxygen atom is present at one end of the perfluoroalkylene group.

[0126] Specific examples of compound (3) include the following compounds. CF2=CFFOCF2CF=CF2, CF2 = CFOCF(CF3)CF = CF2, CF2=CFFOCF2CF2CF=CF2, CF2 = CFOCF2CF(CF3)CF = CF2, CF2 = CFOCF(CF3)CF2CF = CF2, CF2=CFOCFClCF2CF=CF2, CF2=CFOCCl2CF2CF=CF2, CF2 = CFOCF2OCF = CF2, CF2 = CFOC(CF3)2OCF = CF2, CF2 = CFOCF2CF(OCF3)CF = CF2, CF2=CFCF2CF=CF2, CF2=CFCF2CF2CF=CF2, CF2=CFCF2OCF2CF=CF2.

[0127] Examples of units formed by cyclopolymerization of compound (3) include the following units (3-1) to (3-4).

[0128] [ka]

[0129] The polymer (22) may be a homopolymer of a fluorinated diene, or a copolymer of a fluorinated diene and another monomer copolymerizable therewith.

[0130] Examples of other monomers copolymerizable with the fluorine-containing diene include monomers having a reactive functional group in the side chain, tetrafluoroethylene, chlorotrifluoroethylene, perfluoro(methyl vinyl ether), and the like.

[0131] A specific example of the polymer (22) is a polymer represented by the following formula (3-1-1) obtained by cyclopolymerization of CF2=CFOCF2CF2CF=CF2 (perfluoro(3-butenyl vinyl ether)). In the following, perfluoro(3-butenyl vinyl ether) will be referred to as "BVE."

[0132] [ka]

[0133] In the formula (3-1-1), p is an integer of 5 to 1,000. p is preferably an integer of 10 to 800, particularly preferably an integer of 10 to 500.

[0134] As the polymer (2), a synthesized product or a commercially available product may be used. Specific examples of the polymer (2) that may be preferred include BVE cyclized polymer (manufactured by AGC: Cytop (registered trademark)), tetrafluoroethylene / perfluoro(4-methoxy-1,3-dioxole) copolymer (manufactured by Solvay: Hyflon (registered trademark) AD), tetrafluoroethylene / perfluoro(2,2-dimethyl-1,3-dioxole) copolymer (manufactured by Dupont: Teflon (registered trademark) AF), and perfluoro(4-methyl-2-methylene-1,3-dioxolane) polymer (MMD polymer).

[0135] In the present invention, as the fluorine-containing polymer, either one of the polymers (1) and (2) may be used alone, or the polymers (1) and (2) may be used in combination.

[0136] (Terminal Structure of Fluorine-Containing Polymer) The fluorine-containing polymer is usually polymerized by radical polymerization of each of the above-mentioned monomers using a radical polymerization initiator. In this case, the fluorine-containing polymer at the end of the polymerization is considered to have a structure at the end of the molecular chain (main chain) to which a fragment of the radical polymerization initiator used in the polymerization is added. In addition, when a chain transfer agent is used in the polymerization, the structure at the end of the molecular chain (main chain) may have a structure to which a fragment of the chain transfer agent is added.

[0137] The above-mentioned terminal structure of the fluoropolymer may be converted to another structure. For example, by heat-treating the above-mentioned fluoropolymer at the end of the polymerization at 250° C. or more, the terminal structure of the main chain becomes —C(═O)—F, and the fluoropolymer becomes an acid fluoride.

[0138] Moreover, by treating the acid fluoride with methanol, the structure of the terminal of the main chain becomes a methyl ester group. The methyl ester group can be converted from the highly reactive acid fluoride by a simple methanol treatment. Therefore, it is preferable because the stability of the obtained fluorine-containing polymer can be easily improved.

[0139] Furthermore, by subjecting the acid fluoride to a fluorination treatment, the structure of the terminal of the main chain becomes a trifluoromethyl group. As an example of the fluorination treatment, the treatment method described in paragraph 0040 of JP-A-11-152310 can be mentioned. The trifluoromethyl group is preferable because it has high heat resistance and the heat resistance of the obtained fluorine-containing polymer is easily improved. In addition, when the terminal is a trifluoromethyl group, the surface energy of the obtained resin film is low, the conductive material 10X is difficult to adhere to the surface of the resin film 15, and the thick film portion 11 and the thin film portion 12 are easily patterned, which is preferable.

[0140] Furthermore, it is preferable that the fluorine-containing polymer has a terminal structure of a main chain of a methyl ester group or a trifluoromethyl group, since the intermolecular interaction at the terminal of the main chain is small and deposition is facilitated. The above-mentioned structure of the main chain terminal can be confirmed by infrared spectroscopy.

[0141] (Crystallization of Fluorine-Containing Polymer) The fluorine-containing polymer of the present embodiment is preferably low in crystallinity or amorphous. When the crystallinity is high, the grain boundaries (interfaces) become the starting points for nucleation during deposition of the conductive film, increasing the adhesion probability of the conductive film. In other words, the lower the crystallinity or the more amorphous the polymer is, the easier it is to pattern the thick film portion 11 and the thin film portion 12, which is preferable.

[0142] One index for judging the crystallinity of a fluoropolymer is the melting point. For example, when the above-mentioned polymer (1) has PPVE units, as the content of the PPVE units increases, the crystallinity of the fluoropolymer decreases and at the same time the melting point decreases. In addition, since the aliphatic ring structure of the polymer (2) easily breaks down the crystallinity, the polymer (2) has low crystallinity or is amorphous. If the polymer (2) is amorphous, no melting point is observed.

[0143] In this embodiment, the melting point is a value measured using a differential scanning calorimeter (for example, DSC 204 F1 Phoenix manufactured by NETZSCH). Specifically, 9 mg of the fluoropolymer is placed in a sample container, and the heat capacity is measured when the temperature is raised from -70°C to 350°C at 10°C per minute, and the melting point is determined from the obtained melting peak.

[0144] The melting point of the fluoropolymer used in the present embodiment is preferably not more than 300° C., more preferably not more than 270° C., and even more preferably not more than 240° C. There is no particular lower limit to the melting point, but from the viewpoint of maintaining the shape of the film made of the fluoropolymer, it is preferably not less than 100° C. It is also preferable that the fluoropolymer is amorphous, in which case the melting point cannot be observed by the above-mentioned method.

[0145] (Molecular Weight of Fluorine-Containing Polymer) Highly crystalline fluorine-containing polymers have low solubility in solvents, making it difficult to measure the molecular weight. However, amorphous fluorine-containing polymers have high solubility in fluorine-containing solvents, making it possible to measure the molecular weight by gel permeation chromatography (GPC) or other methods.

[0146] The weight average molecular weight (hereinafter referred to as "Mw") of the fluorine-containing polymer is preferably from 1,000 to 20,000, more preferably from 1,500 to 15,000, and even more preferably from 2,000 to 10,000.

[0147] If the weight average molecular weight is less than 1000, the softening temperature of the fluororesin will be low, and the shape of the film made of the fluoropolymer may not be maintained at the process temperature in the device fabrication or under the conditions of use of the device. If the weight average molecular weight is more than 20,000, the main chain of the fluorine-containing polymer is cleaved during deposition, the molecular weight of the fluorine-containing polymer is reduced, the strength of the layer formed is insufficient, and defects due to decomposition products are generated, making it difficult to obtain a smooth surface. In addition, it is assumed that molecules or ions unintentionally mixed in due to the cleavage of the main chain may affect the conductivity of the conductive film. In addition, there is a risk of shortening the life of an element having the conductive film of this embodiment (for example, the light emission life of an organic EL element). Therefore, when the Mw of the fluoropolymer is within the range of 1,000 to 20,000, the main chain of the fluoropolymer will not be cleaved, and a layer having sufficient strength and a smooth surface can be formed.

[0148] The weight average molecular weight of the fluoropolymer is a value measured using gel permeation chromatography (GPC). First, a PMMA standard sample with a known molecular weight is measured using GPC, and a calibration curve is created from the peak top elution time and molecular weight. Next, the fluoropolymer is measured, and Mw and Mn are obtained from the calibration curve. A mixed solvent of 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane / hexafluoroisopropyl alcohol (volume ratio 85 / 15) is used as the mobile phase solvent.

[0149] The term "molecular weight distribution" refers to the ratio of Mw to the number average molecular weight (hereinafter referred to as "Mn"), that is, Mw / Mn. From the viewpoint of the stability of the quality of the layer formed, the molecular weight distribution (Mw / Mn) of the fluoropolymer is preferably small, and is preferably 2 or less. The molecular weight distribution of the fluoropolymer is more preferably 1.5 or less, and further preferably 1.2 or less. The theoretical lower limit of the molecular weight distribution is 1. The narrower the molecular weight distribution of the fluorine-containing polymer, the less the fluctuation in deposition conditions becomes, and the more easily a homogeneous phase-separated structure is formed in the film thickness direction.

[0150] Methods for obtaining a fluorine-containing polymer having a narrow molecular weight distribution include molecular weight adjustment by controlled polymerization such as living radical polymerization, and molecular weight fractionation by sublimation purification, supercritical extraction, and size exclusion chromatography.

[0151] In this specification, the weight average molecular weight and molecular weight distribution are values ​​measured by gel permeation chromatography (GPC).

[0152] (Surface energy of resin film) The resin film 15 made of the above-mentioned fluorine-containing polymer preferably has a surface energy of 30 mN / m or less, more preferably 25 mN / m or less, and even more preferably 20 mN / m or less. When the resin film 15 has such a surface energy, the conductive material 10X is less likely to adhere to the surface of the resin film 15 when the conductive material 10X is dry-coated, making patterning easier.

[0153] The surface energy of the resin film 15 can be adjusted by changing the fluorine atom content or the trifluoromethyl moiety content of the fluorine-containing polymer used. Increasing the fluorine atom content or the trifluoromethyl moiety content of the fluorine-containing polymer reduces the surface energy of the resin film 15.

[0154] The conductive film having the above-mentioned structure is a novel conductive film having two regions with different light transmittances. Moreover, according to the above-described method for manufacturing a conductive film, such a conductive film can be easily manufactured.

[0155] In this embodiment, the thin film portion 12 is present in the second region 10B of the conductive film 1, but the thin film portion 12 may be absent. In the present embodiment, the resin film 15 is present in the second region 10B of the conductive film 1, but a step of removing the resin film may be included after the dry coating step shown in Fig. 5. By removing the resin film 15, the resin film 15 and the thin film portion 12 can be removed at the same time.

[0156] Fig. 7 is a schematic diagram showing the conductive film 2 obtained by removing the resin film 15, and corresponds to Fig. 2. As shown in Fig. 7, the conductive film 2 has a first film 13 and a second film 20. In the first region 13A of the conductive film 2, a lattice-shaped thick film portion 11 and the second film 20 overlap. In addition, in the second region 13B of the conductive film 2, the second film 20 is present. In the conductive film 2 configured as above, the light transmittance of the second region 13B is higher than the light transmittance of the second region 10B of the conductive film 1 described above, and the contrast between the first region 13A and the second region 13B is high.

[0157] Examples of methods for removing the resin film 15 include a method in which the fluorine-containing polymer is dissolved or peeled off using a fluorine-containing solvent, and a method in which the resin film 15 is removed by dry etching.

[0158] The fluorine-containing solvent used is one that dissolves the resin film 15 but does not substantially dissolve other materials constituting the substrate on which the conductive film 1 is formed. Therefore, the fluorine-containing polymer can be removed without impairing the quality of the organic optoelectronic device. The fluorine-containing solvent used for removing the fluorine-containing polymer has, for example, the above-mentioned fluorinophilic parameter P F A fluorine-containing solvent in which is 1 or more is preferred.

[0159] Furthermore, in this embodiment, the second film 20 is provided, but the second film 20 may be omitted.

[0160] FIG. 8 is an explanatory diagram of a modified example of this embodiment, and corresponds to FIG. 8 includes a first film 10 and a resin film 15. The first film 10 is provided on a base material 50. The resin film 15 is provided between the first film 10 and the base material 50.

[0161] The bottom surface 11a of the thick film portion 11 of the first film 10 is in contact with the base material 50. In addition, the side surface 11b of the thick film portion 11 is in contact with the resin film 15. The lower surface 12 a of the thin film portion 12 of the first film 10 is in contact with the resin film 15 .

[0162] Such a conductive film 3 can be produced in the same manner as the above-mentioned conductive film producing method, except that the step shown in FIG. 3 is not included and the fluorine-containing polymer P is directly vapor-deposited onto the surface 50a of the substrate 50. Furthermore, after the conductive film 3 is produced by the dry coating process shown in FIG. 5, a process of removing the above-mentioned resin film 15 may be included.

[0163] [Second embodiment] The second embodiment of the present invention is an optoelectronic device having the conductive film according to the first embodiment of the present invention described above. As such a photoelectric element, an organic EL element is preferable, which comprises a substrate, an anode provided on the substrate, a cathode facing the anode, and an active layer disposed between the anode and the cathode, wherein the cathode is the conductive film according to the first embodiment of the present invention.

[0164] 9 is a cross-sectional view showing an organic EL element (optoelectronic element according to a second embodiment of the present invention) 100. The organic EL element 100 has a laminated structure of a substrate 110, an anode 111, a partition wall 112, a functional layer 113, and a cathode 115. The functional layer 113 includes a light-emitting layer. The organic EL element 100 of this embodiment employs a top emission system in which light generated in the functional layer 113 is emitted to the outside via the cathode 115.

[0165] (substrate) The substrate 110 may or may not have optical transparency. The substrate 110 may be made of inorganic materials such as glass, quartz glass, silicon nitride, etc., or organic polymers (resins) such as polyimide resin, acrylic resin, polycarbonate resin, etc. Furthermore, as long as the insulating properties of the surface are ensured, a metal material may also be used as the substrate 110. The substrate 110 also includes various wirings and driving elements (not shown) that are electrically connected to the organic EL elements.

[0166] (anode) The anode 111 is formed on the substrate 110, and supplies holes to the functional layer 113. In addition, the anode 111 has light reflectivity that reflects light emitted from a light-emitting layer included in the functional layer 113.

[0167] The anode 111 is made of a conductive material. The conductive material may be a conductive metal oxide such as ITO or IZO. In order to impart light reflectivity to the anode 111, a reflective film made of a metal may be provided on the substrate 110 side of the anode 111 or on the functional layer 113 side of the anode 111. In other words, the anode 111 may have a laminated structure of a layer made of a conductive metal oxide and a reflective film made of a metal. The anode 111 may be made of a metal such as silver.

[0168] The thickness of the anode 111 is not particularly limited, but is preferably 30 to 300 nm, and is, for example, 100 nm.

[0169] (bulkhead) The partitions 112 are formed, for example, in a lattice shape, and overlap the periphery of the anode 111. In the openings of the partitions 112, functional layers 113 are formed to separate the organic EL elements 100. The partition wall 112 is made of a resin material such as polyimide.

[0170] (Functional layer) The functional layer 113 is formed to overlap the anode 111. The functional layer 113 has a light-emitting layer. In the light-emitting layer, holes injected from the anode 111 and electrons injected from the cathode 115 recombine to emit photons and emit light. The emission wavelength at that time is determined by the material from which the light-emitting layer is formed. The light-emitting layer corresponds to the "active layer" in the present invention.

[0171] The light-emitting layer can be formed using a material known as a material for the light-emitting layer of an organic EL element. The materials for forming the light-emitting layer may be used alone or in combination of two or more kinds, and are appropriately selected according to the desired emission wavelength.

[0172] The functional layer 113 may have a hole injection layer and a hole transport layer between the light emitting layer and the anode 111 . The hole injection layer has the function of facilitating the injection of holes from the anode to the hole transport layer. The hole transport layer has a function of efficiently transporting holes injected from the anode 111 toward the light emitting layer.

[0173] Furthermore, the functional layer 113 may have an electron transport layer and an electron injection layer between the light emitting layer and the cathode 115 . The electron transport layer has a function of efficiently transporting electrons injected from the cathode 115 toward the light emitting layer. The electron injection layer has the function of facilitating the injection of electrons from the cathode 115 to the electron transport layer.

[0174] (cathode) The cathode 115 is formed on the entire surface so as to cover the partition wall 112 and the functional layer 113. The cathode 115 has a function of injecting electrons into the functional layer.

[0175] In the optoelectronic device of this embodiment, the conductive film of the present invention described above is adopted as the cathode 115. The cathode 115 has a first film 116, a resin film 117, and a second film 118.

[0176] The second film 118 is formed to cover the partition walls 112 and the functional layer 113. The configuration and material of the second film 118 may be the same as those shown for the second film 20 of the first embodiment.

[0177] The resin film 117 overlaps the functional layer 113 in plan view and is formed on an upper surface 118a of the second film 118. The resin film 117 may have the same structure and material as the resin film 15 of the first embodiment.

[0178] The first film 116 is formed to overlap with the partition wall 112 in a plan view. The configuration and material of the first film 116 may be the same as those shown for the first film 10 of the first embodiment.

[0179] That is, a first region of the cathode 115 overlaps with the partition wall 112, and a second region of the cathode 115 overlaps with the functional layer 113 including the light-emitting layer.

[0180] (Microcavity structure) In the organic EL element 100 of this embodiment, the anode 111 and the cathode 115 form an optical resonance structure (microcavity) that resonates light between the anode 111 and the cathode 115, i.e., between the upper surface of the reflective film of the anode 111 and the lower surface of the second film 118. Between the anode 111 and the cathode 115, light generated in the light-emitting layer is repeatedly reflected, and light with a wavelength that matches the optical path length between the anode 111 and the cathode 115 resonates and is amplified. On the other hand, light with a wavelength that does not match the optical path length between the anode 111 and the cathode 115 is attenuated. The "optical path length" here is calculated using the wavelength of the desired light emitted outside the element and the refractive index of each layer at the wavelength of the desired light.

[0181] The optical path length between the anode 111 and the cathode 115 is set to, for example, an integer multiple of the central wavelength of the light L generated in the light-emitting layer included in the functional layer 113. In this case, the light L emitted from the light-emitting layer is amplified as it approaches the central wavelength and is attenuated as it departs from the central wavelength, before being emitted to the outside of the organic EL element 100. In this way, the light L emitted from the organic EL element 100 has a narrow half-width of the emission spectrum and improved color purity.

[0182] In the organic EL element 100 having such a configuration, since the cathode 115 is the conductive film of the present invention, the wiring resistance of the cathode 115 can be reduced while maintaining high light extraction efficiency in the second region, and good driving can be achieved.

[0183] In the above embodiment, an organic EL element has been described as an example of an optoelectronic element, but the optoelectronic element to which the conductive film of the present invention is applied is not limited to an organic EL element.

[0184] The optoelectronic device of the present invention may be, for example, a semiconductor laser. A known configuration can be adopted for the semiconductor laser. By adopting the above-mentioned conductive film for the cathode of the semiconductor laser, the resistance of the cathode is reduced, resulting in a semiconductor laser with improved output.

[0185] The optoelectronic device of the present invention may be, for example, a light-receiving element such as a photosensor, a solar cell, etc. The photosensor and the solar cell may have a known configuration in which holes and electrons generated in an active layer (light-receiving layer) according to the intensity of light received by the active layer are transferred to a cathode and an anode via a semiconductor layer. By employing the above-mentioned conductive film in the electrodes (anode, cathode) of the photosensor and solar cell, the photosensor has improved detection performance, and the solar cell has improved power generation efficiency.

[0186] Furthermore, the conductive film and optoelectronic device of the present invention have high transmittance as a whole device, and are therefore useful in applications such as transparent displays, etc. In under-display cameras, under-display sensors, etc., it is necessary to increase the transmittance of the display above the camera and sensor, and the conductive film of the present invention is extremely useful.

[0187] Furthermore, the conductive film of the present invention can also be used as patterned electrodes and wiring in addition to optoelectronic devices.

[0188] Although the preferred embodiment of the present invention has been described above with reference to the accompanying drawings, the present invention is not limited to the above embodiment. The shapes and combinations of the components shown in the above embodiment are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention. EXAMPLES

[0189] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.

[0190] <Evaluation method> In this embodiment, evaluation was performed by the following methods.

[0191] [Measurement of thermal weight loss rate of fluoropolymer under vacuum] The measurement was performed using a vacuum differential thermobalance (Advance Riko Co., Ltd.: VPE-9000). 50 mg of fluoropolymer was placed in a cell with an inner diameter of 7 mm, and the temperature was measured at 1 × 10 -3 The weight loss rate (%) of the fluoropolymer relative to the initial weight (50 mg) was measured when the temperature was raised from room temperature to 500° C. at a rate of 2° C. per minute under a vacuum of 100 Pa. This measurement determines the temperature at which the weight loss rate reaches 100% (T d100 ), and the temperature at which the weight loss rate becomes 10% (T d10 ) and the temperature at which the weight loss rate reaches 90% (T d90 ) was sought.

[0192] [Melt point measurement] Measurement was performed using a differential scanning calorimeter (NETZSCH: DSC 204 F1 Phoenix). 9 mg of the fluoropolymer was placed in a sample container, and the heat capacity was measured while the temperature was raised from -70°C to 350°C at 10°C per minute, and the melting point was calculated from the obtained melting peak.

[0193] [Measurement of surface energy of resin film] (Preparation of samples for contact angle measurement) A fluorine-containing polymer was deposited on a 25 mm square silicon substrate at a deposition rate of 0.1 nm / sec to form a 100 nm thick resin film, thereby obtaining a measurement sample.

[0194] (Surface energy evaluation) Using a contact angle meter (DSA25 manufactured by KRUSS), 2 μL droplets of water and n-hexadecane were dropped onto the resin film surface of the horizontally placed measurement sample, and the contact angle was measured. Using the contact angle thus obtained and the following formula (A), the surface energy γ S The variance term γ S d and the surface energy of the resin film γ S The polar term γ S p The surface energy γ of the resin film is calculated using the obtained value and the following formula (B). S was calculated.

[0195] Gamma L (cosθ+1) / (2(γ L d ) 1 / 2 )=(γ S p ) 1 / 2 ×(γ L p ) 1 / 2 / (γ L d ) 1 / 2 +(γ S d ) 1 / 2 …(A) Gamma L : Surface energy of water or n-hexadecane Gamma L d: Dispersion term of surface energy of water or n-hexadecane Gamma L p : Polar term of surface energy of water or n-hexadecane θ: Contact angle of water or n-hexadecane

[0196] Gamma S =γ S d +γ S p …(B) Gamma S : Surface energy of resin film Gamma S d : Dispersion term of surface energy of resin film Gamma S p : Polar term of the surface energy of the resin film

[0197] The dispersion term, polar term, and surface energy of water and n-hexadecane were given in the values ​​shown in Table 1 below. [Table 1]

[0198] (Measurement of CF3 concentration) The content (mmol / g) of trifluoromethyl moieties was calculated from the following formula. (Trifluoromethyl moiety content) = [NCF3 / MA] x 1000 NCF3: the sum of values ​​obtained by multiplying the number of moles of trifluoromethyl moieties constituting the units by the molar ratio of the units to all units for each type of unit constituting the fluorine-containing polymer. MA: the sum of the values ​​obtained by multiplying the total atomic weight of all atoms constituting the unit by the molar ratio of the unit to all units for each type of unit constituting the fluorine-containing polymer. The number of moles of the trifluoromethyl moiety, the total atomic weights of all atoms constituting the unit, the molar ratio, etc. used in the above formula were calculated using the molar ratios and terminal amounts of the constituent units of the fluorine-containing polymer obtained by NMR analysis and IR analysis of the fluorine-containing polymer.

[0199] (Measurement of fluorine atom content) The fluorine atom content (mass %) was calculated by the following formula. (Fluorine atom content) = [19 x NF / MA] x 100 NF: the sum of the values ​​obtained by multiplying the total atomic weight of fluorine atoms constituting each type of unit constituting a fluorine-containing polymer by the molar ratio of that unit to all units. MA: the sum of the values ​​obtained by multiplying the total atomic weight of all atoms constituting the unit by the molar ratio of the unit to all units for each type of unit constituting the fluorine-containing polymer. The atomic weight of the fluorine atom, the total atomic weight of all atoms constituting the unit, the molar ratio, etc. used in the above formula were calculated using the molar ratio and terminal amount of the constituent units of the fluorine-containing polymer obtained by NMR analysis and IR analysis of the fluorine-containing polymer.

[0200] <Synthesis of Fluorine-Containing Polymer> The fluorine-containing polymers used for the evaluation were synthesized as follows.

[0201] [Synthesis Example 1] 30 g of perfluoro(3-butenyl vinyl ether) (BVE), 30 g of 1,1,1,2,2,3,3,4,4,5,5,6,6-tridecafluorohexane (1H-PFH), 0.5 g of methanol, and 0.44 g of diisopropyl peroxydicarbonate (IPP) were weighed and charged into a 50 ml glass reactor. After the inside of the reactor was replaced with high purity nitrogen gas, the reactor was heated to 40°C and polymerization was carried out for 24 hours. The solvent was removed from the resulting solution under conditions of 666 Pa (absolute pressure) and 50° C., yielding 28 g of a polymer.

[0202] Next, the obtained polymer was heated in an oven at 300° C., and then treated by the method described in paragraph

[0040] of JP-A-11-152310 to replace the unstable terminal groups with —CF3 groups using fluorine gas, thereby obtaining a fluorine-containing polymer A.

[0203] The obtained fluoropolymer A was charged into the raw material charging section of the above-mentioned glass tube type sublimation purification apparatus, and the inside of the collection section was filled with 3.0×10 -3 The pressure was reduced to 100 Pa. Then, the raw material supply section was gradually heated to 330°C to sublimate the fluoropolymer A. In the sublimation purification apparatus, the collection section was heated at set temperatures of 310°C, 280°C, 250°C, and 200°C from the side closer to the supply section.

[0204] Of these, the substances precipitated in the collection sections at set temperatures of 200° C., 250° C., 280° C. and 310° C. were recovered to obtain 2 g of purified fluoropolymer A1.

[0205] [Synthesis Example 2] A polymer produced in the same manner as in Synthesis Example 1 was heated in an oven at 300°C, immersed in methanol, and heated in an oven at 75°C for 20 hours to replace the terminal groups with methyl ester groups, thereby obtaining a fluorinated polymer B. Fluorine-containing polymer B was sublimated in the same manner as in Synthesis Example 1. Substances precipitated in collection sections set at temperatures of 200° C., 250° C. and 280° C. were recovered to obtain 2 g of purified fluorine-containing polymer B1.

[0206] [Synthesis Example 3] A 1006 mL stainless steel autoclave was charged with 152.9 g of perfluoro(propyl vinyl ether) (PPVE), 805 g of AC2000 (AGC), 2.40 g of methanol, and 1.15 g of azobisisobutyronitrile (AIBN), and the contents were frozen and degassed with liquid nitrogen.

[0207] After the autoclave was heated to 70°C, 56.3 g of tetrafluoroethylene (TFE) was introduced into the autoclave to initiate polymerization. As the polymerization proceeded, the pressure inside the autoclave decreased, so TFE was continuously fed and polymerization was continued while maintaining the temperature and pressure of the autoclave constant. Five hours after the start of polymerization, the autoclave was cooled to terminate the polymerization, and the gas inside the system was discharged to obtain a reaction solution.

[0208] The reaction solution was mixed with 800 g of methanol to precipitate the polymer dissolved in the reaction solution, and then the layers were separated and the lower layer in which the polymer was dispersed was collected. The resulting polymer dispersion was dried with hot air at 80°C for 16 hours, and then vacuum dried at 100°C for 16 hours to obtain a polymer. The composition of the obtained polymer was PPVE units:TFE units=14:86 (mol %).

[0209] The obtained polymer was then heated in an oven at 330° C., immersed in methanol and heated in an oven at 75° C. for 40 hours to substitute the terminal groups with methyl ester groups, thereby obtaining a fluorine-containing polymer C. The fluoropolymer C was sublimated in the same manner as in Synthesis Example 1. The substance precipitated in a collection section set at a temperature of 280° C. was recovered to obtain 4 g of a purified fluoropolymer C1.

[0210] [Synthesis Example 4] A polymer was obtained in the same manner as in Synthesis Example 3, except that 78.9 g of PPVE, 767 g of AC2000, 4.23 g of methanol, 1.27 g of AIBN, and 48.4 g of TFE were used. The composition of the obtained polymer was PPVE units:TFE units=9:91 (mol %).

[0211] Then, in the same manner as in Synthesis Example 3, the terminal groups of the polymer were substituted with methyl ester groups to obtain a fluorine-containing polymer D. Fluorine-containing polymer D was sublimated in the same manner as in Synthesis Example 1. The substances precipitated in the collection sections set at temperatures of 250° C. and 280° C. were recovered to obtain 4 g of purified fluorine-containing polymer D1.

[0212] [Synthesis Example 5] A polymer was obtained in the same manner as in Synthesis Example 3, except that 57.9 g of PPVE, 4.13 g of methanol, and 1.24 g of AIBN were used. The composition of the obtained polymer was PPVE units:TFE units=6:94 (mol %).

[0213] Then, the terminal groups of the polymer were substituted with methyl ester groups in the same manner as in Synthesis Example 4 to obtain a fluoropolymer E. Fluorine-containing polymer E was sublimated in the same manner as in Synthesis Example 1. Substances precipitated in collection sections set at temperatures of 200° C., 250° C. and 280° C. were recovered to obtain 5 g of purified fluorine-containing polymer E1.

[0214] [Synthesis Example 6] A jacketed polymerization tank (made of stainless steel) having an internal volume of 1.351 L was degassed, and 649 g of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (AE-3000, manufactured by AGC Corporation), 152 g of perfluoropropyl vinyl ether (PPVE), 109 g of tetrafluoroethylene (TFE), and 15.5 g of methanol were weighed and charged into the polymerization tank. The temperature of the polymerization tank was maintained at 60° C., and 18.9 mL of a 0.79 mass % solution of t-butyl peroxypivalate (PBPV) (solvent: AE-3000) was charged to initiate polymerization.

[0215] During the polymerization, the polymerization pressure decreased with the progress of the polymerization, so TFE was continuously introduced into the polymerization tank so that the polymerization pressure was kept almost constant. The polymerization pressure was maintained at 1.04±0.04 MPaG (gauge pressure). When the amount of TFE introduced reached 121 g, the polymerization was terminated to obtain a polymer. The composition of the obtained polymer was PPVE units:TFE units=4:96 (mol %).

[0216] Next, the obtained polymer was heated in an oven at 330° C., and the terminal groups of the polymer were then substituted with —CF 3 groups in the same manner as in Synthesis Example 1 to obtain a fluorine-containing polymer F. 20 g of the fluoropolymer F was used and sublimated in the same manner as in Synthesis Example 1. The substances precipitated in collection sections set at temperatures of 250° C. and 280° C. were recovered to obtain 2 g of purified fluoropolymer F1.

[0217] Furthermore, 20 g of the obtained fluoropolymer F was placed in a pressure vessel of a supercritical extraction apparatus and subjected to supercritical extraction with carbon dioxide. After 0.2 g was extracted at an extraction temperature of 40°C, extraction pressure of 30 MPa, and carbon dioxide flow rate of 30 ml / min (condition 1), the extraction temperature was increased to 80°C and extraction pressure to 60 MPa, and AC-2000 (AGC) was used as an entrainer at a ratio of 10 volume% to carbon dioxide (condition 2), to obtain 1.4 g of extract. The extract obtained by the supercritical extraction was named fluoropolymer F2.

[0218] [Synthesis Example 7] The terminal groups of the polymer produced in the same manner as in Synthesis Example 6 were substituted with methyl ester groups under the same conditions as in Synthesis Example 3 to obtain a fluoropolymer G. Fluoropolymer G was sublimated in the same manner as in Synthesis Example 1. The substance precipitated in a collector set at a temperature of 250° C. was recovered to obtain 4 g of purified fluoropolymer G1.

[0219] [Synthesis Example 8] A polymer was obtained in the same manner as in Synthesis Example 6, except that 701 g of AE-3000, 57 g of PPVE, 108 g of TFE, 35.7 g of methanol, and 18.9 mL of a 0.53 mass % solution of PBPV (solvent: AE-3000) were used. The composition of the obtained fluoropolymer was PPVE units:TFE units=2:98 (mol %).

[0220] Then, the terminal groups of the polymer were substituted with -CF3 groups in the same manner as in Synthesis Example 1 to obtain a fluorine-containing polymer H. Fluorine-containing polymer H was sublimated in the same manner as in Synthesis Example 1. The substance precipitated in a collector set at a temperature of 280° C. was recovered to obtain 4 g of purified fluorine-containing polymer H1.

[0221] [Synthesis Example 9] The terminal groups of the polymer produced in the same manner as in Synthesis Example 8 were substituted with methyl ester groups under the same conditions as in Synthesis Example 3 to obtain a fluorine-containing polymer I. Fluorine-containing polymer I was sublimated in the same manner as in Synthesis Example 1. Substances precipitated in collection sections set at temperatures of 250° C. and 280° C. were recovered to obtain 4 g of purified fluorine-containing polymer I1.

[0222] [Commercially available fluorine-containing polymers] As commercially available fluorine-containing polymers, the following materials were used for evaluation. Fluon PTFE L173JE (AGC): Tetrafluoroethylene polymer Fluon PFA P-63 (AGC): Tetrafluoroethylene / perfluoropropyl vinyl ether copolymer TEFLON AF 1600 (DuPont): Tetrafluoroethylene / perfluoro(2,2-dimethyl-1,3-dioxole) copolymer Kynar 301F (Arkema): vinylidene fluoride polymer Kynar 720 (Arkema): vinylidene fluoride polymer

[0223] Furthermore, 50 g of TEFLON AF 1600 was weighed out and sublimated in the same manner as in Synthesis Example 1, and the substances precipitated in collection sections set at temperatures of 250° C. and 280° C. were recovered to obtain 2 g of purified fluoropolymer J1.

[0224] <Evaluation> The obtained fluoropolymer was subjected to the following evaluations 1 to 4.

[0225] [Evaluation 1: Change in chamber pressure during deposition] 0.1 g of fluoropolymer was charged into the vacuum deposition apparatus, and the pressure in the chamber was increased to 10 -4 After reducing the pressure to below 1 Pa, a fluoropolymer film was formed at a deposition rate of 0.1 nm / sec to a thickness of 200 nm. The pressure in the chamber was monitored during this process, and the maximum pressure during deposition was measured. The measured value was used to calculate the pressure increase rate according to the following formula. [Chamber pressure increase rate during deposition] = [Maximum pressure during deposition] / [Initial pressure before deposition]

[0226] Fluorine-containing polymers whose chamber pressure increase rate was 2 times or less were evaluated as "good," and fluorine-containing polymers whose chamber pressure increase rate was more than 2 times were evaluated as "poor." As for the fluoropolymers that were evaluated as defective in this evaluation, the evaluation of the conductive film that follows was abandoned due to concerns about contamination of the chamber.

[0227] [Evaluation 2: Conductive film patterning evaluation 1] (Preparation of samples for transmittance measurement) A quartz substrate measuring 25 mm×25 mm×0.525 mm was used. A fluorine-containing polymer was deposited by vapor deposition using a metal mask having a rectangular opening of 21 mm×5 mm in the center of the quartz substrate when viewed from above, to prepare a quartz substrate having a resin film. The deposition of the fluoropolymer was carried out at a deposition rate of 0.1 nm / sec until the thickness reached 10 nm as measured by a film thickness meter attached to the deposition apparatus.

[0228] Next, Ag was evaporated onto the entire surface of the resin film on the quartz substrate without using a mask, to prepare a conductive film sample for measuring transmittance. The deposition of Ag was carried out at a deposition rate of 0.05 nm / sec until the thickness of Ag reached 15 nm as measured by a film thickness gauge attached to the deposition apparatus.

[0229] (Transmittance measurement) The transmittance of the prepared conductive film sample was measured using a spectrophotometer (Shimadzu Corporation, model number: UV-3600 Plus). From the results, it was determined that the higher the transmittance, the better the patterning property (the easier the patterning).

[0230] [Examples 1-11] Resin films were formed using the above-mentioned fluoropolymers A1 to J1, and the above-mentioned evaluations 1 and 2 were carried out.

[0231] [Example 12] Evaluation was carried out in the same manner as in Example 1, except that a resin film was formed using Fluon PTFE L173JE as the fluoropolymer. Since the temperature inside the chamber rose significantly during deposition in evaluation 1, no other evaluations were performed.

[0232] [Example 13] Evaluation was carried out in the same manner as in Example 1, except that a resin film was formed using Fluon PFA P-63 as the fluorine-containing polymer. Since the temperature inside the chamber rose significantly during deposition in evaluation 1, no other evaluations were performed.

[0233] [Example 14] Evaluation was carried out in the same manner as in Example 1, except that the resin film was formed using TEFLON AF 1600 as the fluoropolymer. Since the temperature inside the chamber rose significantly during deposition in evaluation 1, no other evaluations were performed.

[0234] [Example 15] Evaluation was carried out in the same manner as in Example 1, except that the resin film was formed using Kynar 301F as the fluorine-containing polymer. Since the temperature inside the chamber rose significantly during deposition in evaluation 1, no other evaluations were performed.

[0235] [Example 16] Evaluation was carried out in the same manner as in Example 1, except that a resin film was formed using Kynar 720 as the fluorine-containing polymer. Since the temperature inside the chamber rose significantly during deposition in evaluation 1, no other evaluations were performed.

[0236] [Example 17] Except for forming a resin film using the following 3-(4-biphenyl)-4-phenyl-5-tert-butylphenyl-1,2,4-triazole (hereinafter, TAZ) instead of the fluorine-containing polymer, evaluation was performed in the same manner as in Example 1. TAZ is a polycyclic organic semiconductor used in Prior Patent Document 1 (U.S. Pat. No. 10,270,033). [ka]

[0237] [Example 18] Evaluation was performed in the same manner as in Example 1, except that the resin film was formed using the following N-(diphenyl-4-yl)-9,9-dimethyl-N-(4-(9-phenyl-9H-carbazoyl-3yl)phenyl)-9H-fluoren-2-amine (hereinafter, HT211) instead of the fluorine-containing polymer. [ka]

[0238] [Reference example 1] An Ag film was formed to a thickness of 15 nm on a quartz substrate, and evaluation 2 was performed. The thickness of the Ag film in Reference Example 1 is the same as that of the metal film formed in Evaluation 2 of Examples 1 to 18 at a position not overlapping with the resin film.

[0239] [Reference example 2] An Ag film was formed to a thickness of 2 nm on a quartz substrate, and evaluation 2 was performed.

[0240] Of the above Examples 1 to 18, Examples 1 to 11 correspond to working examples, and Examples 12 to 18 correspond to comparative examples. The evaluation results are shown in Tables 2 and 3. Table 2 is a summary of the physical properties of the resin film material, and Table 3 is a summary of the evaluation results. In the tables, "-" indicates that no data is available.

[0241] [Table 2]

[0242] [Table 3]

[0243] The results of evaluation 2 are shown in FIG.

[0244] As a result of the evaluation, it was found that in Examples 1 to 11, there was no increase in the pressure inside the chamber during deposition, and no depolymerization, thermal decomposition, or outgassing was observed. It is also found that in Examples 1 to 11, the light transmittance of the second region in the prepared samples is greater than the light transmittance of Reference Example 1. Therefore, it is found that in Examples 1 to 11, patterning of the first region and the second region is achieved. Moreover, it was confirmed that Examples 1 to 11 have high transmittance, particularly in the long wavelength region including the near infrared region, and are extremely useful in under-display sensor applications equipped with an optical authentication sensor that uses near infrared rays. In particular, Examples 1 to 5 had higher light transmittance than Reference Example 2 (Ag 2 nm) in the wavelength range of 450 nm or more, and Examples 1, 3, and 4 had higher light transmittance than Reference Example 2 over the entire measured wavelength range.

[0245] In contrast, in Examples 12 to 16, an increase in the pressure inside the chamber during deposition was observed, and it was found that depolymerization, thermal decomposition, and outgassing occurred during deposition, making these methods essentially unsuitable for producing the conductive film of this embodiment. In addition, in Examples 17 and 18, the light transmittance of the second region in the prepared sample can be evaluated as being larger than that of Reference Example 1, but it was found that the light transmittance was lower than that of Examples 1 to 11. That is, it was found that the resin films formed in Examples 17 and 18 are more likely to have a metal film formed on the upper surface than the resin films formed in Examples 1 to 11, and that patterning with a large contrast between the first region and the second region is difficult. In particular, it was found that the transmittance in the long wavelength region including the near infrared region was low, and the patterning ability was significantly inferior to that of the conductive film of this embodiment.

[0246] [Evaluation 3: Conductive film patterning evaluation 2] (Preparation of samples for transmittance measurement) A quartz substrate measuring 25 mm×25 mm×0.525 mm was used. Ag was evaporated onto the entire surface of the quartz substrate without using a mask to form a second film. The deposition of Ag was carried out at a deposition rate of 0.05 nm / sec until the thickness of the Ag film reached 10 nm as measured by a film thickness gauge attached to the deposition apparatus.

[0247] Next, a fluorine-containing polymer was deposited on the quartz substrate with the above-mentioned Ag deposited over the entire surface thereof using a metal mask having a rectangular opening of 21 mm x 5 mm in the center of the substrate when viewed from above, to produce a quartz substrate with a resin film. The deposition of the fluoropolymer was carried out at a deposition rate of 0.1 nm / sec until the thickness reached 50 nm as measured by a film thickness meter attached to the deposition apparatus.

[0248] Next, Ag or Mg was deposited on the entire surface of the quartz substrate having the Ag-vapor-deposited film and the resin film without using a mask, to prepare a conductive film sample for measuring transmittance. The deposition of Ag or Mg was carried out at a deposition rate of 0.05 nm / sec until the thickness reached 15 nm as measured by a film thickness meter attached to the deposition apparatus.

[0249] (Transmittance measurement) The transmittance of the prepared conductive film sample was measured using a spectrophotometer (Shimadzu Corporation, model number: UV-3600 Plus). From the results, it was determined that the higher the transmittance, the better the patterning property.

[0250] [Example 19] A resin film was formed using the above-mentioned fluoropolymer D1, and the above-mentioned evaluation 3 was carried out. [Example 20] Evaluation was performed in the same manner as in Example 19, except that the resin film was formed using TAZ instead of the fluoropolymer.

[0251] [Reference example 3] An Ag film was formed on a quartz substrate to a thickness of 10 nm, and then an Ag or Mg film was formed to a thickness of 15 nm, and evaluation 3 was performed. The thickness of the Ag film and the Mg film in Reference Example 3 is the same as that of the metal film formed in Evaluation 3 of Examples 19 and 20 at a position not overlapping with the resin film.

[0252] Example 19 corresponds to an embodiment, and Example 20 corresponds to a comparative example. The evaluation results are shown in Table 4.

[0253] [Table 4]

[0254] The results of evaluation 3 are shown in FIG.

[0255] It can be seen that the light transmittance of the second region in the prepared sample in Example 19 is higher than that in Reference Example 3. Therefore, it was found that the first region and the second region were patterned in Example 19. In addition, it was confirmed that Example 19 has high transmittance in the long wavelength region including the near infrared region, and is useful for under-display sensor applications equipped with an optical authentication sensor using near infrared rays.

[0256] In contrast, in Example 20, it was found that the light transmittance of the second region in the prepared sample was equal to or lower than the light transmittance of Reference Example 1. That is, it was found that the resin film formed in Example 20 was more likely to have a metal film formed on its upper surface than the resin film formed in Example 19, making it difficult to pattern the first region and the second region.

[0257] [Evaluation 4: Conductive film patterning evaluation 3] (Preparation of conductive film sample 1: for measuring total light transmittance) (Process 1) Ag was evaporated onto the entire surface of a 25 mm×25 mm×0.525 mm quartz substrate without using a mask to form a second film. The deposition of Ag was carried out at a deposition rate of 0.05 nm / sec until the thickness of Ag reached 30 nm as measured by a film thickness gauge attached to the deposition apparatus.

[0258] (Process 2) Next, a fluorine-containing polymer was deposited on the above-mentioned substrate on which the Ag was deposited over the entire surface using a metal mask having a rectangular opening of 21 mm x 5 mm in the center of the substrate when viewed from above, to produce a quartz substrate with a resin film. The deposition of the fluoropolymer was carried out at a deposition rate of 0.1 nm / sec until the thickness reached 50 nm as measured by a film thickness meter attached to the deposition apparatus.

[0259] (Step 3) Next, Ag was deposited on the entire surface of the resin film of the quartz substrate having the resin film prepared in step 2 without using a mask to prepare a conductive film sample for measuring total light transmittance. In the prepared conductive film sample, the region where the resin film is not formed corresponds to the "first region" in the present invention, and the region where the resin film is formed corresponds to the "second region" in the present invention. The deposition of Ag was carried out at a deposition rate of 0.05 nm / sec until the thickness reached 70 nm as measured by a film thickness gauge attached to the deposition apparatus.

[0260] (Preparation of conductive film sample 2: for film thickness measurement) A conductive film sample for film thickness measurement was prepared in the same manner as in preparation of conductive film sample 1, except that a 25 mm×25 mm silicon substrate was used instead of the quartz substrate. In addition, a reference sample 1 was prepared by carrying out step 1 on a silicon substrate and forming only the second film, and a reference sample 2 was prepared by carrying out steps 1 and 2 on a silicon substrate and forming the second film and a resin film.

[0261] (Total light transmittance measurement) For the conductive film sample for measuring the total light transmittance, the total light transmittance of the second region was measured using a haze meter (manufactured by Suga Test Instruments, model number: HZ-V3, measuring light: D65 light).

[0262] (film thickness measurement) In a first region of the conductive film sample for film thickness measurement, a scratch was made from the surface of the first film to the silicon substrate, and the film thickness from the surface of the first film to the surface of the silicon substrate (total film thickness in the first region) was measured. Similarly, in a second region of the conductive film sample for film thickness measurement, a scratch was made from the surface of the first film to the silicon substrate, and the film thickness from the surface of the first film to the surface of the silicon substrate (total film thickness in the second region) was measured. Similarly, in reference sample 1, a scratch was made from the surface of the second film to the silicon substrate, and the film thickness from the surface of the second film to the surface of the silicon substrate (the film thickness of the second film of reference sample 1) was measured. Similarly, in the second region of reference sample 2, a scratch was made from the surface of the resin film to the silicon substrate, and the film thickness from the surface of the resin film to the surface of the silicon substrate (the total film thickness of the second film and the resin film of reference sample 2) was measured. The film thickness was measured using a stylus-type surface measurement device (Dektak XT, manufactured by Bruker AXS).

[0263] The film thickness a of the first film in the first region and the film thickness b of the first film in the second region were calculated based on the following formula. Thickness of the first film in the first region a (nm) = Total film thickness in the first region (nm) - film thickness of the second film on the reference sample 1 (nm) The thickness of the first film in the second region, b (nm) = Total film thickness in the second region (nm) - Total film thickness of the second film and the resin film of the reference sample 2 (nm)

[0264] (Patterning evaluation) The feasibility of patterning using the resin film was evaluated according to the following criteria: A and B were evaluated as good, and C and D were evaluated as poor. A: Film thickness b is 0% or more and 10% or less of film thickness a. B: Film thickness b is more than 10% and less than 50% of film thickness a C: Film thickness b is more than 50% and less than 90% of film thickness a D: Film thickness b is more than 90% and less than 100% of film thickness a

[0265] [Example 21] A resin film was formed using the above-mentioned fluoropolymer A1, and the above-mentioned evaluation 4 was carried out.

[0266] [Reference example 4] On a quartz substrate, a Ag film was formed to a thickness of 30 nm, and then a Ag film was formed to a thickness of 70 nm. The total light transmittance of the obtained sample was measured. The thickness of the Ag film in Reference Example 4 is the same as that of the metal film formed in the first region of the conductive film sample prepared in Example 21.

[0267] Example 21 corresponds to an embodiment. As a result of the evaluation, the total light transmittance of the second region of Example 21 was 27%. In Example 21, the film thickness a of the first film in the first region was 68 nm, and the film thickness b of the first film in the second region was 0 nm, and the patterning ability was evaluated as A. Moreover, the total light transmittance of Reference Example 4 was 0.6%.

[0268] From the measurement results of the total light transmittance of the second region of the conductive film sample of Example 21 and the sample of Reference Example 4, it was found that in the conductive film sample of Example 21, the second region had higher light transmittance than the first region. Moreover, from the results of the film thickness measurement of Example 21, it was confirmed that in the conductive film sample of Example 21, the formation of the first film in the second region was suppressed. These results show that the conductive film sample of Example 21 had the first and second regions well patterned.

[0269] [Evaluation 5: Confirmation of conductive film patterning shape] (Preparation of conductive film: for microscopic observation) A 25 mm × 25 mm × 0.525 mm quartz substrate was used. A fluorine-containing polymer was deposited on the quartz substrate using a metal mask with circular openings, each 30 μm in diameter, arranged at a pitch of 60 μm in the X-axis and Y-axis directions on a flat surface, to produce a quartz substrate with a resin film. The deposition of the fluoropolymer was carried out at a deposition rate of 0.1 nm / sec until the thickness reached 30 nm as measured by a film thickness meter attached to the deposition apparatus. Next, Ag, which will become the first film, was deposited on the entire surface of the resin film on the quartz substrate without using a mask, to prepare a conductive film sample for confirming the patterning shape. The deposition of Ag was carried out at a deposition rate of 0.5 nm / sec until the thickness reached 70 nm as measured by a film thickness gauge attached to the deposition apparatus.

[0270] (Microscope observation and pattern size measurement) The conductive film sample for confirming the patterning shape was observed using a digital microscope (Keyence Corporation, model number: VHX-2000). The diameter of region B was also measured.

[0271] [Example 22] A resin film was formed using the above-mentioned fluoropolymer A1, and the above-mentioned evaluation 5 was carried out. [Example 23] A resin film was formed using the above-mentioned fluoropolymer C1, and the above-mentioned evaluation 5 was carried out. [Example 24] A resin film was formed using the above-mentioned fluoropolymer D1, and the above-mentioned evaluation 5 was carried out. [Reference example 5] The diameter of the openings of the metal mask used in the deposition of the fluoropolymer in Evaluation 5 was measured in the same manner as in the pattern size measurement in Evaluation 5. The measured value was 27 μm.

[0272] The microscope image and the measurement results of the diameter of region B (unit: μm) are shown in Table 5. As shown in Table 5, the conductive film obtained using the fluorine-containing polymer has region B that reflects the design of the metal mask, and forms a conductive film with a fine patterning process of several tens of μm. [Table 5]

[0273] [Evaluation 6: Evaluation of sheet resistance of conductive film] (Preparation of conductive film: for measuring sheet resistance) (Process 1) Mg:Ag was evaporated onto the entire surface of a 75mm x 75mm quartz substrate without using a mask to form a second film with a thickness of 15nm. The evaporation was adjusted so that the volume ratio of Mg to Ag was 1:10. The total evaporation rate of Mg and Ag was 0.1nm / sec. (Process 2) Next, a fluoropolymer was deposited on the quartz substrate, on which the above Mg:Ag was deposited over the entire surface, using a metal mask with circular openings of 150 μm in diameter arranged at a pitch of 250 μm in the X-axis and Y-axis directions on a plane, to prepare a quartz substrate with a resin film. The deposition of the fluoropolymer was continued at a deposition rate of 0.1 nm / sec until the thickness reached 50 nm as measured by a film thickness gauge attached to the deposition apparatus. (Step 3) Next, Mg:Ag was evaporated onto the entire surface of the resin film on the quartz substrate having the resin film prepared in step 2 without using a mask to form the first film, producing a conductive film sample for measuring sheet resistance. The evaporation was adjusted so that the volume ratio of Mg to Ag was 1:10, and continued until the film thickness measured by the film thickness meter attached to the evaporation device reached 15 nm. The total evaporation rate of Mg and Ag was 0.1 nm / sec.

[0274] (Preparation of conductive films with different first film thicknesses) Conductive film samples for measuring sheet resistance were prepared in the same manner as in steps 1 to 3 above, in which the film thicknesses of the first film in step 3 were 45 nm and 75 nm. (Sheet resistance measurement) The sheet resistance of the prepared conductive film sample for sheet resistance measurement was measured using a low-resistance resistivity meter (Loresta, manufactured by Nitto Seiko Analytech Co., Ltd.) The four-point probe of the Loresta was pressed against the upper surface of the conductive film sample to measure the sheet resistance.

[0275] [Example 25] A resin film was formed using the above-mentioned fluoropolymer D1, and the above-mentioned Evaluation 6 was carried out. [Reference example 6] Mg:Ag was evaporated onto the entire surface of a 75 mm x 75 mm quartz substrate without using a mask to form a second film with a thickness of 15 nm. The evaporation was adjusted so that the volume ratio of Mg to Ag was 1:10. The total evaporation rate of Mg and Ag was 0.1 nm / sec. The sheet resistance measurement for evaluation 6 was carried out without forming the resin film and the first film.

[0276] Example 25 corresponds to an embodiment. The results of measuring the sheet resistance are shown in FIG. As a result of the evaluation, the sheet resistance of Example 25 was lower than that of Reference Example 6, which did not have the first film. It was also confirmed that the sheet resistance was reduced as the thickness of the first film increased to 15 nm, 45 nm, and 75 nm.

[0277] From the above results, it was confirmed that the present invention is useful. The entire contents of the specification, claims, abstract and drawings of Japanese Patent Application No. 2020-112962, filed on June 30, 2020, are hereby incorporated by reference as the disclosure of the specification of the present invention. [Explanation of symbols]

[0278] Reference Signs List 1, 2, 3, 11, 12...conductive film, 10, 13, 116...first film, 10A, 13A...first region, 10B, 13B...second region, 10X...conductive material, 15, 117...resin film, 20, 118...second film, 20a, 50a...surface, 50...base material, 110...substrate, 111...anode, 115...cathode, P...fluorine-containing polymer, M...mask

Claims

1. A conductive film having a first region and a second region exhibiting a higher light transmittance than the first region, A first film made of a conductive material; A resin film made of a fluorine-containing polymer; the first film is disposed so as to overlap at least the first region of the first region and the second region; the resin film is disposed so as to overlap the second region, The fluorine-containing polymer is a conductive film that satisfies the following (1) and (2). (1) 1 x 10 -3 When the temperature is increased at a rate of 2° C. / min under a pressure of 100 Pa, the temperature at which the thermal weight loss rate reaches substantially 100% is 400° C. or lower. (2) 1 x 10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 200°C.

2. a second film made of a conductive material and spanning the first region and the second region; the second film has a higher light transmittance than the first film at a position overlapping the first region; The conductive film according to claim 1 , wherein the second film is in contact with the first film in the first region.

3. The conductive film according to claim 1 or 2, wherein the resin film has a surface energy of 30 mN / m or less.

4. The conductive film according to claim 1 , wherein the melting point of the fluorine-containing polymer is 300° C. or lower.

5. The conductive film according to claim 1 , wherein the fluorine-containing polymer is amorphous.

6. The fluorine-containing polymer has a trifluoromethyl moiety, The conductive film according to claim 1 , wherein the content of the trifluoromethyl moiety in the fluorine-containing polymer is 0.1 mmol / g or more.

7. The conductive film according to claim 1 , wherein the fluorine-containing polymer has a unit derived from a fluoroolefin.

8. The conductive film according to claim 7 , wherein the fluorine-containing polymer has at least a unit derived from tetrafluoroethylene and a unit derived from a perfluoroalkyl vinyl ether.

9. The conductive film according to claim 1 , wherein the fluorine-containing polymer has an aliphatic ring structure in a main chain.

10. An optoelectronic device comprising the conductive film according to claim 1 .

11. A substrate; an anode provided on the substrate; a cathode facing the anode; an active layer disposed between the anode and the cathode; The optoelectronic device according to claim 10 , wherein the cathode is the conductive film.

12. A step of depositing a fluoropolymer that satisfies the following (1) and (2) on a substrate using a mask to form a resin film made of the fluoropolymer: and dry-coating the resin film with a conductive material. (1) 1 x 10 -3 When the temperature is increased at a rate of 2° C. / min under a pressure of 100 Pa, the temperature at which the thermal weight loss rate reaches substantially 100% is 400° C. or lower. (2) 1 x 10 -3 When the temperature is increased at a rate of 2°C / min under a pressure of 10 Pa, the temperature range from the temperature at which the thermal weight loss rate becomes 10% to the temperature at which it becomes 90% is within 200°C.

13. The method for producing a conductive film according to claim 12 , further comprising the step of removing the resin film after the dry coating step.

14. The method for producing a conductive film according to claim 12 or 13, further comprising the step of forming a film of a conductive material on the surface of the base material prior to the step of forming the resin film.

Citation Information

Patent Citations

  • Fluorine-based surface treating agent and article treated with the same

    JP2015010209A

  • Surfaces containing patterned coatings and methods of patterning coatings on devices

    JP2018533183A

  • Method for patterning a coating on a surface and device including a patterned coating

    US10270033B2

  • Liquid repellent compound, liquid repellent polymer, curable composition, coating composition, article having cured film, article having pattern with lyophilic region and liquid repellent region, and method for producing same

    WO2013089204A1

  • Organic electroluminescence element

    WO2018110244A1