Room temperature curable organopolysiloxane composition and article, hydrolyzable organosilane compound and method for producing same

A hydrolyzable organosilane compound with cyclopentanone as a leaving group addresses health and environmental concerns in room-temperature-curable organopolysiloxane compositions, offering rapid curing and improved safety with equivalent performance to conventional compositions.

JP7574861B2Active Publication Date: 2024-10-29SHIN ETSU CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022565054
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-26
Filing Date
2021-08-16
Publication Date
2024-10-29
Estimated Expiration
2041-08-16

AI Technical Summary

Technical Problem

Existing room-temperature-curable organopolysiloxane compositions using hydrolyzable organosilane compounds as curing agents face health hazards such as carcinogenicity and reproductive toxicity, as well as environmental hazards like toxicity to aquatic organisms, and often require environmentally hazardous tin catalysts, while also having inferior curing properties compared to oxime-free types.

Method used

The use of a hydrolyzable organosilane compound with a cyclic ketone compound like cyclopentanone as a leaving group, which is less harmful to humans and the environment, and can be cured using titanium, guanidine, or bismuth catalysts, achieving equivalent or better curing properties than conventional compositions.

Benefits of technology

The composition provides a cured silicone rubber product with excellent adhesive properties, rapid curing, and improved safety and environmental friendliness, suitable for various applications including adhesives, sealants, and coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574861000001
    Figure 0007574861000001
  • Figure 0007574861000002
    Figure 0007574861000002
  • Figure 0007574861000003
    Figure 0007574861000003
Patent Text Reader

Abstract

The present invention provides: a room temperature curable organopolysiloxane composition which has curability equivalent to the curability of conventional dealcoholization type or deoximation type room temperature curable organopolysiloxane compositions even if various catalysts are used therefor, while reducing harmful effects on human bodies and burden on the environment, and which enables the achievement of a cured product that has good rubber properties, adhesiveness and durability if cured; various articles which comprise this composition or a cured product that is obtained by curing this composition; a novel hydrolyzable organosilane compound which is useful as a curing agent for this composition; and a method for producing this novel hydrolyzable organosilane compound. A room temperature curable organopolysiloxane composition which contains, as a curing agent, a hydrolyzable organosilane compound that is represented by general formula (2) and releases / discharges a cyclic ketone compound as a leaving group and / or a partial hydrolysis-condensation product of the hydrolyzable organosilane compound. (In the formula, R2 represents a monovalent hydrocarbon group having from 1 to 10 carbon atoms; n represents a number from 1 to 8; and m represents 3 or 4.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a room-temperature curable organopolysiloxane composition of the condensation curing type which crosslinks (cures) through a hydrolysis / condensation reaction caused by moisture (water) in the atmosphere at room temperature (23°C±15°C), in particular a room-temperature curable organopolysiloxane composition in which the elimination compound released from the crosslinking agent (curing agent) by the hydrolysis reaction during curing is a cyclic ketone compound such as cyclobutanone or cyclopentanone, which cures well through a condensation reaction and gives a silicone rubber cured product (elastomeric organopolysiloxane cured product) with excellent adhesiveness, and a method for producing the same. Things The present invention relates to various articles having the above-mentioned structure, as well as to a novel hydrolyzable organosilane compound which releases cyclopentanone as a leaving group upon hydrolysis, and a method for producing the same. [Background technology]

[0002] Room temperature curable organopolysiloxane compositions that cure at room temperature to become silicone rubber have been known for some time and have been widely used in the industrial world. Known mechanisms for curing at room temperature include a mechanism for curing by hydrosilylation addition reaction, a mechanism for radical curing by ultraviolet light, and a mechanism for curing by condensation reaction between a hydrolyzable group bonded to a silicon atom and a hydroxyl group. Among these, room temperature curable organopolysiloxane compositions that cure by condensation reaction have the advantage that they can be easily cured at room temperature and are less likely to be inhibited by impurities that occur in hydrosilylation addition reactions, etc. Therefore, cured products (silicone rubber cured products) obtained by curing room temperature curable organopolysiloxane compositions that cure by condensation reaction are widely used in the fields of automobiles such as on-board gaskets and sealants, architecture such as building sealants, and electrical and electronic parts.

[0003] Room temperature curable organopolysiloxane compositions that cure by condensation reactions contain a hydrolyzable organosilane compound having a hydrolyzable group in the molecule as a curing agent (crosslinking agent), and examples of curing agents that are already widely used include deoxime-type hydrolyzable organosilane compounds that release oxime compounds such as 2-butanone oxime upon curing, and dealcohol-type hydrolyzable organosilane compounds that release alcohol compounds such as methanol. The rubber-like cured products obtained by curing compositions containing these curing agents have high heat resistance, chemical resistance, and weather resistance derived from silicone (siloxane structure). On the other hand, oxime compounds such as 2-butanone oxime that are generated when a deoxime-type curing agent is cured are suspected to be carcinogenic and are undesirable, and methanol and the like that are generated when a dealcohol-type curing agent is cured are toxic to the human body and designated as a deleterious substance, making them undesirable from the viewpoint of human health. Furthermore, in some cases, these compositions use tin catalysts as curing catalysts, which are subject to stronger regulations as environmentally hazardous substances, and are undesirable from the viewpoint of ensuring the safety of workers and protecting the environment in recent years, and there is a demand for them to be replaced by hydrolyzable organosilane compounds (curing agents) that have a safer leaving group (leaving compound).

[0004] Furthermore, the curing agent (crosslinking agent) used in the alcohol-free type room-temperature-curable organopolysiloxane composition is less reactive than the curing agent used in the oxime-free type room-temperature-curable organopolysiloxane composition, and therefore has the disadvantage of being inferior in curability to the oxime-free type. From the standpoint of environmental protection and minimizing health hazards, there is a particular desire for products that not only have improved performance but also are more environmentally friendly and safer, and there is an increasing demand for room-temperature-curable organopolysiloxane compositions that have excellent performance and contain highly safe compounds that are eliminated.

[0005] JP2018-515634A proposes a condensation-curing organosiloxane composition containing a silane compound as a crosslinking agent that eliminates and releases an α-hydroxycarboxylic acid ester compound, typically ethyl lactate, as an alternative to dealcohol-removing and oxime-removing curing agents. In this system, the leaving group, ethyl lactate, is a highly safe compound, but the use of a tin catalyst is essential. Tin catalysts have been pointed out as being harmful to aquatic organisms, and the use of tin catalysts is undesirable from the perspective of environmental protection.

[0006] Japanese Patent Publication No. 51-39673 proposes a condensation-curing organopolysiloxane composition that releases a ketone compound, typically acetone. Compared to 2-butanone oxime or methanol, acetone is a compound that is less harmful to the human body, and the composition provides a silicone rubber cured product that cures faster and has better durability than conventional curing methods. However, acetone has a low flash point of -20°C and is highly volatile, which limits the environment in which it can be used.

[0007] Cyclopentanone is a compound with low toxicity and high biodegradability, and has a relatively high flash point of 35° C. for an organic solvent. As a silane coupling agent having cyclopentanone as a leaving group, there are synthesis examples of tris(1-cyclopenten-1-yloxy)methylsilane having a methyl group as a substituent in Journal of Organometallic Chemistry (1984), 273(1) (Non-Patent Document 1) and Journal of Organometallic Chemistry (1985), 281(2-3) (Non-Patent Document 2), but there is no example of its use as a crosslinking agent for a room temperature curable organopolysiloxane composition. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 2018-515634 [Patent Document 2] Special Publication No. 51-39673 [Non-patent literature]

[0009] [Non-Patent Document 1] Journal of Organometallic Chemistry (1984), 273(1) [Non-Patent Document 2] Journal of Organometallic Chemistry (1985), 281(2-3) Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention has been made in view of the above circumstances, and provides a room-temperature-curable organopolysiloxane composition which has no reported health hazards, such as carcinogenicity or reproductive toxicity to the human body, or environmental hazards, such as toxicity to aquatic organisms, and which uses as a curing agent a hydrolyzable organosilane compound having a leaving group (leaving compound) that is a cyclic ketone compound, such as cyclobutanone or cyclopentanone, which has a relatively high flash point, and which has curability equivalent to that of conventional dealcohol- or oxime-type room-temperature-curable organopolysiloxane compositions even when various catalysts are used, while at the same time reducing harmful effects to the human body and environmental load, and which can give a silicone rubber cured product having good rubber properties, adhesion, and durability after curing, and a composition which uses this composition Things The present invention aims to provide a novel hydrolyzable organosilane compound which is useful for various articles having the above-mentioned properties, as well as a curing agent for the above-mentioned composition, and a method for producing the same. [Means for solving the problem]

[0011] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, it has been discovered that when an organosilicon compound (hydrolyzable organosilane compound) having vinyl or phenyl groups as a substituent or having four functional groups, which is represented by the following general formula (4) and which releases cyclopentanone upon hydrolysis and has low toxicity to the human body, is used as a crosslinking agent for a room-temperature-curable organopolysiloxane composition, it is possible to obtain a room-temperature-curable organopolysiloxane composition which is excellent in safety and exhibits rubber physical properties and rapid curing properties equal to or superior to those of conventional curing types (dealcohol-free type and oxime-free type). [ka] (In the formula, R 6 is a vinyl group or a phenyl group, and m is 3 or 4. The present inventors have further found that a room-temperature-curable organopolysiloxane composition containing as a curing agent (crosslinking agent) a hydrolyzable organosilane compound which leaves and releases a cyclic ketone compound such as cyclobutanone or cyclopentanone as a leaving group (leaving compound), and / or a partial hydrolysis condensate thereof, as represented by the following general formula (2), solves the above-mentioned problems of toxicity and safety to the human body and the environment, and have further found that even when an organic compound containing titanium, guanidine, or the like is added as a curing catalyst to this composition, the composition exhibits curability and cured product performance equivalent to those when a tin catalyst is added, which has led to the completion of the present invention. [ka] (In the formula, R 2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, n is an integer from 1 to 8, and m is 3 or 4.

[0012] That is, the present invention relates to the following room temperature curable organopolysiloxane composition, Things Various items owned (contact The present invention provides a method for producing hydrolyzable organosilane compounds and their preparation, as well as adhesives, sealing materials, potting agents, coating agents, etc. [1] (A) 100 parts by mass of an organopolysiloxane having a viscosity of 20 to 1,000,000 mPa s at 23°C and represented by the following general formula (1): HO-(SiR 1 2O) a -H (1) (In the formula, R 1 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and each R 1 may be the same or different groups; a is an integer of 50 or more; and (B) a hydrolyzable organosilane compound represented by the following general formula (2) and / or a partial hydrolysis condensate thereof: 1 to 40 parts by mass [ka] (In the formula, R 2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, n is an integer from 1 to 8, and m is 3 or 4. A room temperature curable organopolysiloxane composition comprising: [2] The room-temperature-curable organopolysiloxane composition according to [1], wherein the hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof of component (B) is one that releases a cyclic ketone compound upon hydrolysis. [3] The room-temperature-curable organopolysiloxane composition according to [2], wherein the cyclic ketone compound that is eliminated is cyclobutanone or cyclopentanone. [4] The room-temperature-curable organopolysiloxane composition according to any one of [1] to [3], wherein the hydrolyzable organosilane compound of component (B) is a hydrolyzable organosilane compound represented by the following general formula (4): [ka] (In the formula, R 6 is a vinyl group or a phenyl group, and m is 3 or 4. [5] The room-temperature-curable organopolysiloxane composition according to any one of [1] to [4], further comprising 0.01 to 10 parts by mass of a curing catalyst (C) per 100 parts by mass of the component (A). [6] The room-temperature-curable organopolysiloxane composition according to [5], wherein the curing catalyst (C) is at least one selected from the group consisting of tin catalysts, titanium catalysts, strong organic base catalysts, and organobismuth catalysts. [7] The room-temperature-curable organopolysiloxane composition according to any one of [1] to [6], which does not contain a tin catalyst. [8] The room-temperature-curable organopolysiloxane composition according to any one of [1] to [7], further comprising (D) 0.01 to 10 parts by mass of a silane coupling agent represented by the following general formula (3) and / or a partial hydrolysis condensate thereof, per 100 parts by mass of the component (A): R 3 R 4 b Six 3-b (3) (In the formula, R 3 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms and at least one functional group (excluding a guanidyl group) containing one or more heteroatoms selected from a nitrogen atom, a sulfur atom, and an oxygen atom. 4 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and X is a hydrolyzable group. b is 0, 1, or 2. [9] The room-temperature-curable organopolysiloxane composition according to any one of [1] to [8], further comprising 1 to 500 parts by mass of an inorganic filler (E) per 100 parts by mass of the component (A).

[10] The room-temperature-curable organopolysiloxane composition according to [9], wherein component (E) is one or more inorganic fillers selected from calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide. [ 11 ] An adhesive comprising the room-temperature-curable organopolysiloxane composition according to any one of [1] to

[10] . [ 12 ] A sealant comprising the room-temperature-curable organopolysiloxane composition according to any one of [1] to

[10] . [ 13 ] A potting agent comprising the room-temperature-curable organopolysiloxane composition according to any one of [1] to

[10] . [ 14 ] A coating agent comprising the room-temperature-curable organopolysiloxane composition according to any one of [1] to

[10] . [ 15 ] A hydrolyzable organosilane compound represented by the following general formula (4): [ka] (In the formula, R 6 is a vinyl group or a phenyl group, and m is 3 or 4. [ 16 ] It is hydrolyzed to release cyclopentanone. 15 2. The hydrolyzable organosilane compound according to claim 1 . [ 17 ] The following reaction formula [I] [ka] (In the formula, R 6 , m is as defined above.) The method includes reacting a chlorosilane compound represented by the formula: 15 ] or [ 16 2. A method for producing a hydrolyzable organosilane compound according to claim 1, [ 18 ] The amount of cyclopentanone added is 0.95 to 3.0 moles per mole of chlorine atoms in the chlorosilane compound. 17 2. A method for producing a hydrolyzable organosilane compound according to claim 1, [ 19 ] The catalytic substance is copper chloride, copper iodide, copper bromide, silver chloride, silver iodide or silver bromide. 17 ] or [ 18 2. A method for producing a hydrolyzable organosilane compound according to claim 1, [ 20 ] The amount of the catalyst substance added is 0.001 to 0.5 moles per mole of the chlorosilane compound. 17 ]~[ 19 13. A method for producing a hydrolyzable organosilane compound according to any one of claims 1 to 12. [ 21 ] The basic substance is trimethylamine, triethylamine, tripropylamine, tributylamine, urea, diazabicycloundecene, or diazabicyclononene. 17 ]~[ 20 13. A method for producing a hydrolyzable organosilane compound according to any one of claims 1 to 12. [ 22 ] The amount of the basic substance added is 0.95 to 2.5 moles per mole of chlorine atoms in the chlorosilane compound. 17 ]~[ 21 13. A method for producing a hydrolyzable organosilane compound according to any one of claims 1 to 12. Effect of the Invention

[0013] The room-temperature-curable organopolysiloxane composition of the present invention generates compounds (elimination compounds) from the curing agent (crosslinking agent) by hydrolysis and condensation reactions during curing, which are highly safe cyclic ketone compounds such as cyclobutanone and cyclopentanone, and gives a silicone rubber cured product (elastomeric organopolysiloxane cured product) that has excellent curability and adhesiveness after curing and good durability, and therefore can be suitably used as various adhesives, sealing materials, potting agents, coating agents, etc., with consideration given to human health and safety. Furthermore, the room-temperature-curable organopolysiloxane composition of the present invention shows the same curability and cured product performance when an organic compound containing titanium, bismuth, guanidine, etc. is added as a curing catalyst as when a tin catalyst is added, and therefore can be suitably used as various adhesives, sealing materials, potting agents, coating agents, etc., with consideration given to environmental protection (load reduction). Furthermore, the hydrolyzable organosilane compound of the present invention releases a safer compound as a leaving group (leaving compound), and particularly when used as a crosslinking agent for a room-temperature-curable organopolysiloxane composition, the composition has excellent curing properties, cures quickly when exposed to air, and exhibits excellent physical properties. Therefore, compositions containing this hydrolyzable organosilane compound can be effectively used in construction applications, automotive applications, and electrical and electronic adhesive applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described in detail below. In the present invention, the viscosity is a value measured by a rotational viscometer in accordance with the method specified in JIS Z 8803. Unless otherwise specified, "room temperature" refers to a state of a temperature of 23°C ± 15°C and a humidity of 50% RH ± 5% RH.

[0015] [Component (A): Organopolysiloxane] The component (A) used in the room-temperature-curable organopolysiloxane composition of the present invention is an organopolysiloxane represented by the following general formula (1) and having a viscosity at 23° C. of 20 to 1,000,000 mPa·s. HO-(SiR 1 2O) a -H (1) (In the formula, R 1 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and each R 1 may be the same or different groups. a is an integer of 50 or more.

[0016] Component (A) is a linear diorganopolysiloxane having a main chain consisting of repeating diorganosiloxane units as shown in formula (1), both ends of the molecular chain being blocked with hydroxyl groups (silanol groups) bonded to silicon atoms, and having a viscosity at 23°C of 20 to 1,000,000 mPa s. It functions as the main agent (base polymer) of the room-temperature-curable organopolysiloxane composition of the present invention.

[0017] In the above formula (1), R 1 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly 1 to 6 carbon atoms, and examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, octyl, 2-ethylhexyl, nonyl, and decyl groups, cycloalkyl groups such as cyclohexyl groups, alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and hexenyl groups, aryl groups such as phenyl and tolyl groups, and aralkyl groups such as benzyl and phenylethyl groups. Alternatively, examples of the groups include those in which the hydrogen atoms of these hydrocarbon groups are partially substituted with halogen atoms such as chlorine, fluorine, and bromine, such as a trifluoropropyl group. 1 The unsubstituted or substituted monovalent hydrocarbon group of R is preferably one that does not contain an aliphatic unsaturated bond, and specifically, an alkyl group such as a methyl group, or an aryl group such as a phenyl group is more preferred, with a methyl group being particularly preferred. 1 may be the same group or different groups.

[0018] In the above formula (1), the difunctional diorganosiloxane unit (SiR 1 2O 2 / 2a, which indicates the number of repetitions (or degree of polymerization) of the formula (a), is an integer of 50 or more, preferably an integer of 50 to 2,000, more preferably an integer of 100 to 1,500, and particularly preferably an integer of 200 to 1,200. In the present invention, the degree of polymerization (or molecular weight) can be determined, for example, as the polystyrene-equivalent number average degree of polymerization (or number average molecular weight) in gel permeation chromatography (GPC) analysis using toluene, tetrahydrofuran (THF) or the like as a developing solvent.

[0019] The organopolysiloxane of component (A) has a viscosity at 23°C of 20 to 1,000,000 mPa·s, preferably 100 to 300,000 mPa·s, more preferably 1,000 to 200,000 mPa·s, and particularly preferably 10,000 to 100,000 mPa·s. If the viscosity of the organopolysiloxane is less than the lower limit (20 mPa·s), a large amount of component (C) described below is required, which is economically disadvantageous. On the other hand, if the viscosity of the organopolysiloxane exceeds the upper limit (1,000,000 mPa·s), workability decreases, which is not preferable.

[0020] The organopolysiloxane of the component (A) may use either a single type, or a combination of two or more types.

[0021] [Component (B): Hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof] The component (B) used in the room-temperature-curable organopolysiloxane composition of the present invention is a hydrolyzable organosilane compound represented by the following general formula (2) and / or a partial hydrolysis condensate thereof, which is used as a crosslinking agent (curing agent) and is characterized in that it releases a cyclic ketone compound such as cyclobutanone or cyclopentanone as a leaving group (leaving substance) upon hydrolysis. In the present invention, the term "partial hydrolysis condensate" refers to an organosiloxane oligomer having 3 or more, preferably 4 or more, residual hydrolyzable groups in the molecule, which is produced by partial hydrolysis and condensation of the hydrolyzable organosilane compound. [ka] (In the formula, R 2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, n is an integer from 1 to 8, and m is 3 or 4.

[0022] In the above general formula (2), R 2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 10 carbon atoms; 2 Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, octyl, 2-ethylhexyl, nonyl, and decyl, alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and hexenyl, aryl groups such as phenyl and tolyl, and aralkyl groups such as benzyl and phenylethyl. Among these, methyl, ethyl, vinyl, and phenyl groups are preferred, and methyl, vinyl, and phenyl groups are particularly preferred.

[0023] In the above general formula (2), n is an integer of 1 to 8, preferably an integer of 2 to 6, more preferably an integer of 2 to 4, and even more preferably 2 or 3. When n is 0, a cyclic structure is not formed. When n is an integer of 9 or more, the molecular weight of the hydrolyzable organosilane becomes large, making purification by distillation difficult and increasing the amount added to ensure storage stability, which is disadvantageous in terms of cost.

[0024] As mentioned above, m is 3 or 4. If this number is less than 3 (i.e., if m is 0, 1 or 2), rubber curing by a crosslinking reaction does not occur, making the compound unsuitable as a crosslinking agent for room-temperature-curable organopolysiloxane compositions.

[0025] In addition, the leaving group (leaving compound) generated by hydrolysis of the hydrolyzable organosilane compound represented by the above general formula (2) is a cyclic ketone compound such as cyclopropanone, cyclobutanone, cyclopentanone, cyclohexanone, cycloheptanone, cyclooctanone, cyclononanone, cyclodecanone, etc., preferably cyclobutanone and cyclopentanone, more preferably cyclopentanone. There are no reports of cyclobutanone and cyclopentanone being harmful to human health, such as carcinogenicity or reproductive toxicity, or environmentally harmful, such as toxicity to aquatic organisms. In addition, cyclopentanone is mass-produced industrially, is easily available, and is highly cost-competitive, so it is also advantageous for producing the hydrolyzable organosilane compound of the component (B), as described below.

[0026] The hydrolyzable organosilane compound of component (B) can be produced, for example, by reacting a chlorosilane compound corresponding to the hydrolyzable organosilane compound represented by general formula (2) with a cyclic ketone compound in the presence of a catalyst and a basic substance (e.g., dehydrochlorination reaction). The reaction formula is, for example, represented by the following formula [1].

[0027] [ka] (In the formula, R 2 , n, and m are as defined above.)

[0028] Examples of the chlorosilane compound include the following. [ka]

[0029] Examples of the cyclic ketone compound include the following. [ka]

[0030] The amount of the cyclic ketone compound to be reacted with the chlorosilane compound is preferably 0.95 to 3.0 mol, more preferably 0.99 to 2.5 mol, and even more preferably 1.0 to 2.0 mol, per mol of chlorine atoms in the chlorosilane compound. If the amount of the cyclic ketone compound is too small, the reaction may not be completed, whereas if the amount of the cyclic ketone compound is too large, purification may take a long time, resulting in an increase in production time.

[0031] The catalyst used in the reaction includes monovalent or divalent metallic copper compounds, such as, but not limited to, copper chloride, copper bromide, copper iodide, copper sulfate, copper nitrate, copper carbonate, basic copper carbonate, copper formate, copper acetate, and copper butyrate. The amount of catalyst (metallic copper compound) added is preferably 0.001 to 0.5 mol, more preferably 0.002 to 0.2 mol, and even more preferably 0.003 to 0.1 mol, per mol of the chlorosilane compound. If the amount of catalyst added is too small, the reaction may not be completed, whereas if the amount of catalyst added is too large, it is disadvantageous in terms of cost.

[0032] The basic substance used in the reaction may be a basic substance having low nucleophilicity, such as trimethylamine, triethylamine, tripropylamine, tributylamine, urea, diazabicycloundecene, diazabicyclononene, etc. Among these, trimethylamine, triethylamine, and tributylamine are preferred, and triethylamine is particularly preferred. The amount of the basic substance added is preferably 0.95 to 2.5 mol, more preferably 0.99 to 2.0 mol, and even more preferably 1.0 to 1.5 mol, per mol of chlorine atoms in the chlorosilane compound. If the amount of the basic substance added is small, the reaction may not be completed, whereas if the amount of the basic substance added is too large, it is economically disadvantageous.

[0033] A commonly used solvent may be used in the production of the hydrolyzable organosilane compound of component (B). Examples of the solvent include organic solvents such as aromatic hydrocarbons, such as toluene, xylene, and benzene; aliphatic hydrocarbons, such as pentane, hexane, heptane, nonane, octane, and decane; ethers, such as dimethyl ether, methyl ethyl ether, tetrahydrofuran, and dioxane; halogenated hydrocarbons, such as perchloroethane, perchloroethylene, trichloroethane, chloroform, and carbon tetrachloride; amides, such as dimethylformamide; and esters, such as ethyl acetate, methyl acetate, and butyl acetate. The amount of the solvent used is not particularly limited, but is usually in the range of 10 to 500 parts by mass, preferably 30 to 400 parts by mass, and more preferably 50 to 300 parts by mass, per 100 parts by mass of the cyclic ketone compound used.

[0034] The reaction conditions of the chlorosilane compound and the cyclic ketone compound are usually 0 to 120°C, preferably 0 to 100°C, at which the chlorosilane compound is dropped into the cyclic ketone compound, and the reaction is carried out at 50 to 120°C, preferably 60 to 100°C, for 1 to 48 hours, more preferably 3 to 30 hours. If the reaction temperature is too low, the reaction may not be completed, and if the reaction temperature is too high, the product may become significantly colored. If the reaction time is too short, the reaction may not be completed, and if the reaction time is too long, the reaction time is disadvantageous to productivity. After the reaction is complete, the product can be purified by distillation under reduced pressure. The degree of reduction is preferably 1×10 -5 ~3,000 Pa, more preferably 1×10 -5 The pressure during the purification is preferably 100 to 250° C., and more preferably 120 to 230° C. If the pressure during the purification (degree of reduction in pressure) is too high, distillation may become difficult. If the temperature during the purification is too low, purification by distillation may become difficult, and if it is too high, coloration or decomposition of the reaction product may occur.

[0035] Specific examples of the hydrolyzable organosilane compound of component (B) include those represented by the following formula: In this case, Me represents a methyl group. [ka]

[0036] As the component (B), in terms of rapid curing properties, it is particularly preferred that the component (B) is a novel organosilicon compound (hydrolyzable organosilane compound) that eliminates cyclopentanone as a leaving group (eliminating compound) generated by hydrolysis, as represented by the following general formula (4): [ka] (wherein m is the same as above, and R 6 is a vinyl or phenyl group.)

[0037] Here, in the above general formula (1), R 6 is a vinyl group or a phenyl group, with a vinyl group being particularly preferred. As mentioned above, m is 3 or 4. If this number is less than 3 (i.e., if m is 0, 1 or 2), rubber curing by a crosslinking reaction does not occur, and the compound is unsuitable as a crosslinking agent for a condensation-curable room-temperature-curable organopolysiloxane composition.

[0038] The hydrolyzable organosilane compound of the present invention can be produced, for example, by reacting a chlorosilane compound with cyclopentanone in the presence of a catalyst and a basic substance (for example, dehydrochlorination reaction). This reaction formula is represented, for example, by the following formula [I].

[0039] [ka] (In the formula, R 6 , m is as defined above.)

[0040] Examples of the chlorosilane compound include the following. [ka]

[0041] The amount of cyclopentanone added to react with the chlorosilane compound is preferably 0.95 to 3.0 mol, more preferably 0.99 to 2.5 mol, and even more preferably 1.0 to 2.0 mol, per mol of chlorine atoms in the chlorosilane compound. If the amount of cyclopentanone added is small, the reaction may not be completed, whereas if the amount of cyclopentanone added is too large, purification takes a long time, increasing the production time.

[0042] The basic substance used in the reaction may be a basic substance having low nucleophilicity, such as trimethylamine, triethylamine, tripropylamine, tributylamine, urea, diazabicycloundecene, diazabicyclononene, etc. Among these, trimethylamine, triethylamine, and tributylamine are preferred, and triethylamine is particularly preferred. The amount of the basic substance added is preferably 0.95 to 2.5 mol, more preferably 0.99 to 2.0 mol, and even more preferably 1.0 to 1.5 mol, per mol of chlorine atoms in the chlorosilane compound. If the amount of the basic substance added is small, the reaction may not be completed, whereas if the amount of the basic substance added is too large, it is economically disadvantageous.

[0043] Examples of catalysts used in the reaction include monovalent or divalent metallic copper compounds and metallic silver compounds, such as copper chloride, copper bromide, copper iodide, copper sulfate, copper nitrate, copper carbonate, basic copper carbonate, copper formate, copper acetate, copper butyrate, silver chloride, silver iodide, silver sulfate, silver nitrate, silver carbonate, basic silver carbonate, silver formate, silver acetate, and silver butyrate, but are not limited to these. The amount of catalyst (metallic copper compound, metallic silver compound) added is preferably 0.001 to 0.5 mol, more preferably 0.002 to 0.2 mol, and even more preferably 0.003 to 0.1 mol, per mol of the chlorosilane compound. If the amount of catalyst added is too small, the reaction may not be completed, whereas if the amount of catalyst added is too large, it is disadvantageous in terms of cost.

[0044] In producing the hydrolyzable organosilane compound of the present invention, a commonly used solvent may be used, and examples of such organic solvents include aromatic hydrocarbons such as toluene, xylene, benzene, etc.; aliphatic hydrocarbons such as pentane, hexane, heptane, nonane, octane, decane, etc.; ethers such as dimethyl ether, methyl ethyl ether, tetrahydrofuran, dioxane, etc.; halogenated hydrocarbons such as perchloroethane, perchloroethylene, trichloroethane, chloroform, carbon tetrachloride, etc.; amides such as dimethylformamide, etc.; and esters such as ethyl acetate, methyl acetate, butyl acetate, etc. The amount of the solvent used is not particularly limited, but is usually in the range of 10 to 500 parts by mass, preferably 30 to 400 parts by mass, and more preferably 50 to 300 parts by mass, per 100 parts by mass of cyclopentanone used.

[0045] The reaction conditions of the chlorosilane compound and cyclopentanone are usually 0 to 130°C, preferably 20 to 120°C, at which the chlorosilane compound is dropped into cyclopentanone, and the reaction is carried out at 50 to 140°C, preferably 60 to 130°C, for 0.5 to 48 hours, preferably 1 to 30 hours. If the reaction temperature is too low, the reaction may not be completed, and if the reaction temperature is too high, the product may become significantly colored. If the reaction time is too short, the reaction may not be completed, and if the reaction time is too long, the reaction may be disadvantageous to productivity. After the reaction is complete, the product can be purified by distillation under reduced pressure. The degree of reduction is preferably 1×10 -5 ~3,000 Pa, more preferably 1×10 -5 The pressure during the purification is preferably 100 to 250° C., and more preferably 120 to 230° C. If the pressure during the purification (degree of reduction in pressure) is too high, distillation may become difficult. If the temperature during the purification is too low, purification by distillation may become difficult, and if it is too high, coloration or decomposition of the reaction product may occur.

[0046] Specific examples of the hydrolyzable organosilane compound of the present invention include those represented by the following formula: [ka]

[0047] If an organosilicon compound (hydrolyzable organosilane compound) that leaves cyclopentanone as the leaving group (leaving compound) generated by such hydrolysis is used as a crosslinking agent (curing agent) for a room temperature curable organopolysiloxane composition, it is possible to obtain a cured product that has particularly fast curing properties and excellent rubber physical properties. Cyclopentanone is a compound that is less harmful to the human body and the environment and has excellent biodegradability compared to methanol and 2-butanone oxime.

[0048] The novel hydrolyzable organosilane compound of the present invention has cyclopentanone as the leaving group (leaving compound) generated by hydrolysis, and is particularly suitable for use as a crosslinking agent for room temperature curable organopolysiloxane compositions.

[0049] When such a hydrolyzable organosilane compound is used as a crosslinking agent for a room temperature curable organopolysiloxane composition, it is possible to impart higher safety and rapid curing properties. By using a hydrolyzable organosilane compound that releases cyclopentanone, which is a safer leaving group (leaving compound) generated by hydrolysis, as a crosslinking agent (curing agent), a condensation-curable, room-temperature-curable organosiloxane composition that gives a cured product with excellent rubber physical properties and has fast curing properties can be obtained.

[0050] The component (B) may use one type alone, or two or more types in combination. The amount of component (B) is 1 to 40 parts by mass, preferably 3 to 30 parts by mass, and more preferably 5 to 20 parts by mass, per 100 parts by mass of component (A). If the amount of component (B) is less than the lower limit of 1 part by mass, the shelf life may deteriorate when stored in a sealed container. If the amount of component (B) is more than the upper limit of 40 parts by mass, the curability of the room-temperature-curable organopolysiloxane composition may decrease significantly, and the adhesiveness may also deteriorate. The hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof, component (B), is clearly distinguished from the silane coupling agent and / or partial hydrolysis condensate thereof, component (D), which is an optional component described later, in that it does not have in its molecule a monovalent hydrocarbon group having at least one functional group containing one or more atoms selected from a nitrogen atom, a sulfur atom, and an oxygen atom.

[0051] [(C) component curing catalyst] The room-temperature-curable organopolysiloxane composition of the present invention may optionally contain a curing catalyst (C) as an optional component, as required. As the curing catalyst (C), any metallic or non-metallic condensation catalyst that has conventionally been used as a curing accelerator for room-temperature-curable organopolysiloxane compositions may be used. For example, dibutyltin methoxide, dibutyltin diacetate, dibutyltin dioctate, dibutyltin dilaurate, dioctyltin dilaurate, dioctyltin dioctate, dimethyltin dimethoxide, dimethyltin diacetate, and other organic tin compounds (tin catalysts), tetrapropyl titanate, tetrabutyl titanate, tetra-2-ethylhexyl titanate, dimethoxytitanium diacetylacetonate, titanium diisopropoxybis(ethylacetoacetate), and other organic titanium compounds (titanium catalysts), triethylamine, hexylamine, tetramethylguanidine, γ-tetramethylguanidylpropyltrimethoxysilane, and other amine compounds and salts thereof (organic strong base catalysts), bismuth tris(2-ethylhexanoate), bismuth tris(neodecanoate), and other organic bismuth compounds and mixtures thereof (organic bismuth catalysts), and the like can be mentioned. At least one of these, that is, one type can be used alone, or two or more types can be used in combination. In the present invention, among the above catalysts, when any of the titanium catalyst, the organic strong base catalyst, and the organic bismuth catalyst is blended, the same curability and cured product performance are exhibited as when a tin catalyst is blended. Therefore, from the viewpoint of environmental protection, it is preferable to blend a titanium catalyst, an organic strong base catalyst, or an organic bismuth catalyst without blending a tin catalyst.

[0052] When component (C) is blended, the blending amount is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 8 parts by mass, and even more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of component (A). If the blending amount of component (E) is less than the lower limit of 0.01 parts by mass, the catalytic effect may not be obtained, whereas if the blending amount exceeds the upper limit of 10 parts by mass, the storage stability of the composition may be deteriorated.

[0053] [Component (D): Silane coupling agent and / or partial hydrolysis condensate thereof] The room-temperature-curable organopolysiloxane composition of the present invention may contain, as an optional component, a silane coupling agent (D) and / or a partial hydrolysis condensate thereof, as necessary. Component (D) is a silane coupling agent represented by the following general formula (3) (i.e., a hydrolyzable organosilane compound or carbon functional silane having a functional group-containing monovalent hydrocarbon group) and / or a partial hydrolysis condensate thereof, and is a component for imparting good adhesion to the cured product of the room-temperature-curable organopolysiloxane composition of the present invention. R 3 R 4 b Six 3-b (3) (In the formula, R 3 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms and at least one functional group (excluding a guanidyl group) containing one or more heteroatoms selected from a nitrogen atom, a sulfur atom, and an oxygen atom. 4 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and X is a hydrolyzable group. b is 0, 1, or 2.

[0054] In the above formula (3), R 3is a monovalent hydrocarbon group having 1 to 20 carbon atoms and having at least one functional group containing one or more heteroatoms selected from a nitrogen atom, a sulfur atom, and an oxygen atom (for example, an unsubstituted or substituted amino group, an unsubstituted or substituted imino group, an amido group, a ureido group, a mercapto group, an epoxy group, a (meth)acryloxy group, etc., but excluding a guanidyl group), and specifically, a β-(2,3-epoxycyclohexyl)ethyl group, a β-(3,4-epoxycyclohexyl)ethyl group, a γ-glycidoxypropyl group, a γ-methacryloxypropyl group, Examples of monovalent hydrocarbon groups containing at least one heteroatom selected from a nitrogen atom, a sulfur atom, and an oxygen atom, preferably having 3 to 20 carbon atoms, more preferably having 3 to 14 carbon atoms, include a γ-acryloxypropyl group, a N-β-(aminoethyl)-γ-aminopropyl group [also known as a N-2-(aminoethyl)-3-aminopropyl group], a γ-aminopropyl group, a N-phenyl-γ-aminopropyl group, a γ-ureidopropyl group, a γ-mercaptopropyl group, and a γ-isocyanatopropyl group. 5 As the alkyl group, a γ-glycidoxypropyl group, a γ-aminopropyl group, and an N-β-(aminoethyl)-γ-aminopropyl group are particularly preferred.

[0055] In addition, in the above formula (3), R 4 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, octyl, 2-ethylhexyl, nonyl, and decyl groups, cycloalkyl groups such as cyclohexyl groups, alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and hexenyl groups, aryl groups such as phenyl and tolyl groups, and aralkyl groups such as benzyl and phenylethyl groups. Alternatively, examples include groups in which the hydrogen atoms of these hydrocarbon groups are partially substituted with halogen atoms such as chlorine, fluorine, and bromine, such as trifluoropropyl groups. Among these, methyl, ethyl, propyl, and isopropyl groups are preferred. In addition, R 4 may be the same group or different groups.

[0056] In the above formula (3), examples of the hydrolyzable group X include ketoxime groups, alkoxy groups, alkoxyalkoxy groups, acyloxy groups, and alkenyloxy groups.Specific examples include ketoxime groups having 3 to 8 carbon atoms, such as dimethylketoxime groups, diethylketoxime groups, methylethylketoxime groups, and methylisobutylketoxime groups; alkoxy groups having 1 to 4 carbon atoms, preferably 1 or 2 carbon atoms, such as methoxy groups, ethoxy groups, propoxy groups, isopropoxy groups, butoxy groups, isobutoxy groups, sec-butoxy groups, and tert-butoxy groups; alkoxyalkoxy groups having 2 to 4 carbon atoms, such as methoxymethoxy groups and methoxyethoxy groups; acyloxy groups having 2 to 4 carbon atoms, such as acetoxy groups and propionoxy groups; and alkenyloxy groups having 2 to 4 carbon atoms, such as vinyloxy groups, allyloxy groups, propenoxy groups, and isopropenoxy groups.Preferably, X is a methoxy group. The hydrolyzable groups X may be the same or different.

[0057] Specific examples of the silane coupling agent represented by formula (3) of the component (D) include aminosilanes such as γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-2-(aminoethylamino)propyltrimethoxysilane [also known as N-2-(aminoethyl)-3-aminopropyltrimethoxysilane], epoxysilanes such as γ-glycidoxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, (meth)acrylic silanes such as γ-(meth)acryloxypropyltrimethoxysilane, γ-(meth)acryloxypropyltriethoxysilane, mercaptosilanes such as γ-mercaptopropyltrimethoxysilane, and isocyanate silanes such as γ-isocyanatepropyltrimethoxysilane.

[0058] The silane coupling agent and / or partial hydrolysis condensate thereof as the component (D) may use one type alone, or two or more types may be used in combination.

[0059] When component (D) is blended, the blending amount is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 8 parts by mass, per 100 parts by mass of component (A). If the blending amount is less than 0.01 part by mass, the cured product may not exhibit sufficient adhesive performance, whereas if the blending amount exceeds 10 parts by mass, the rubber strength after curing may decrease, or the curability may decrease.

[0060] [Component (E): Inorganic filler] The room-temperature-curable organopolysiloxane composition of the present invention may optionally contain an inorganic filler (E) as an optional component. The inorganic filler (E) is a reinforcing or non-reinforcing filler that imparts rubber properties to the room-temperature-curable organopolysiloxane composition of the present invention. Examples of inorganic fillers of component (E) include dry silica such as calcined silica, fused silica, crushed silica, and fumed silica (fumed silica), wet silica such as precipitated silica and sol-gel silica, and silica-based fillers such as crystalline silica (fine powder quartz), diatomaceous earth, carbon black, talc, bentonite, calcium carbonate, zinc carbonate, and magnesium carbonate, calcium oxide, zinc oxide, magnesium oxide, and aluminum hydroxide, which are surface-treated or untreated, and among these, calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide are preferred, and calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide, which are surface-treated or untreated, are more preferred.In this case, it is preferred that these inorganic fillers have a low moisture content. There are no particular limitations on the type, amount, treatment method, etc. of the surface treatment agent (hydrophobic treatment agent). Representative examples of the surface treatment agent that can be used include organosilicon compounds such as chlorosilanes, alkoxysilanes, and organosilazanes, fatty acids, paraffins, silane coupling agents, and titanium coupling agents. The inorganic filler of component (E) may use one type alone, or two or more types in combination.

[0061] When the (E) component is blended, the blending amount is preferably 1 to 500 parts by mass, more preferably 20 to 500 parts by mass, even more preferably 20 to 300 parts by mass, and particularly preferably 50 to 300 parts by mass, relative to 100 parts by mass of the (A) component. If the blending amount is less than 1 part by mass, sufficient rubber strength cannot be obtained, and the blending amount may be unsuitable for the intended use, whereas if the blending amount exceeds 500 parts by mass, the ejection property from the cartridge may deteriorate, storage stability may decrease, and the mechanical properties of the resulting rubber may also decrease.

[0062] [Other ingredients] In addition, in the room temperature curable organopolysiloxane composition of the present invention, other than the above-mentioned components, generally known additives may be used within the scope that does not impair the purpose of the present invention.Additives include polyether as a thixotropy improver, silicone oil (non-functional organopolysiloxane) as a plasticizer, isoparaffin, etc., and if necessary, colorants such as pigments, dyes, and fluorescent whitening agents, bioactive additives such as antifungal agents, antibacterial agents, and marine organism repellents, surface modifiers such as phenyl silicone oil, fluorosilicone oil, and organic liquids that are incompatible with silicone as bleeding oils, solvent volatile oils, and solvents such as low-boiling point isoparaffins can also be added.

[0063] The room temperature curable organopolysiloxane composition of the present invention can be obtained by uniformly mixing the above-mentioned components and the above-mentioned various additives in predetermined amounts in a dry atmosphere. The room temperature curable organopolysiloxane composition of the present invention cures by leaving it at room temperature, and the molding method, curing conditions, etc. can be known methods and conditions according to the type of composition.

[0064] The room temperature curable organopolysiloxane composition of the present invention, particularly the one-component composition, is stored in the absence of moisture, i.e., in a sealed container that is protected from moisture, and is readily cured at room temperature (23° C.±15° C.) by exposure to moisture in the air at the time of use.

[0065] In the room temperature curable organopolysiloxane composition of the present invention, the compound generated from the crosslinking agent by the hydrolysis reaction during curing is a cyclic ketone compound such as cyclopentanone, which is highly safe, and is therefore considered to be safe for the human body and the environment. Furthermore, cyclopentanone has a flash point of 35°C, which is higher than that of a dealcohol type that releases an alcohol compound such as methanol during curing of the composition, and is therefore highly safe. Such a room temperature curable organopolysiloxane composition of the present invention exhibits good curability by using various existing catalysts, and the cured product (silicone rubber) is also excellent in adhesion. In addition, it is possible to provide a composition that takes environmental load into consideration by using a catalyst other than tin.

[0066] Therefore, the room-temperature-curable organopolysiloxane composition of the present invention is useful as an adhesive, a sealing material, a potting agent, a coating agent, etc. The method for using the room-temperature-curable organopolysiloxane composition of the present invention as an adhesive, a sealing material, a potting agent, or a coating agent may follow a conventionally known method.

[0067] Examples of target articles include automobile parts, automobile oil seals, electrical and electronic parts, building structures, and civil engineering structures. EXAMPLES

[0068] The present invention will be described in more detail below with reference to synthesis examples, examples, and comparative examples, as well as synthesis examples, composition examples, and composition comparative examples, but the present invention is not limited to the following examples and synthesis examples. The viscosity is a value measured at 23°C using a rotational viscometer according to the method specified in JIS Z 8803. Note that Me represents a methyl group.

[0069] [Synthesis Example 1] Synthesis of hydrolyzable organosilane compound 1 In a 5,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, a reflux condenser and a dropping funnel, 834g (9.9mol) of cyclopentanone, 825g (8.2mol) of triethylamine, 5g (0.05mol) of copper(I) chloride and 1,500ml of hexane were charged, and 400g (2.47mol) of vinyltrichlorosilane was dropped over about 2 hours at 40-60℃. After stirring for 12 hours at 80℃, the generated triethylamine hydrochloride was removed by filtration, and hexane was distilled from the filtrate at 100℃ and normal pressure, and then distilled at 180℃ and 300Pa to obtain hydrolyzable organosilane compound 1 (yield 532g, 69%). This reaction formula is represented by the following formula [2]. [ka]

[0070] [Synthesis Example 2] Synthesis of hydrolyzable organosilane compound 2 Cyclopentanone 834g (9.9mol), triethylamine 825g (8.2mol), copper(I) chloride 5g (0.05mol), and hexane 1,500ml were charged into a 5,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, a reflux condenser, and a dropping funnel, and methyltrichlorosilane 368g (2.47mol) was added dropwise over about 2 hours at 40-60°C. After stirring at 80°C for 12 hours, the generated triethylamine hydrochloride was removed by filtration, and hexane was distilled from the filtrate at 100°C and normal pressure, and then the mixture was distilled at 170°C and 300Pa to obtain hydrolyzable organosilane compound 2 (yield 519g, 71%). This reaction formula is represented by the following formula [3]. [ka]

[0071] [Synthesis Example 3] Synthesis of hydrolyzable organosilane compound 3 Cyclopentanone 834g (9.9mol), triethylamine 825g (8.2mol), copper(I) chloride 5g (0.05mol), and hexane 1,500ml were charged into a 5,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, a reflux condenser, and a dropping funnel, and phenyltrichlorosilane 522g (2.47mol) was added dropwise over about 2 hours at 40-60°C. After stirring at 80°C for 12 hours, the generated triethylamine hydrochloride was removed by filtration, and hexane was distilled from the filtrate at 100°C and normal pressure, and then distilled at 200°C and 300Pa to obtain hydrolyzable organosilane compound 3 (yield 568g, 65%). This reaction formula is represented by the following formula [4]. [ka]

[0072] [Example 1] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R 1 = methyl group, a = about 620) to 100 parts by mass of (E-1) heavy calcium carbonate whose surface is treated with paraffin (product name; MC Coat P-20, Maruo Calcium Co., Ltd.), 10 parts by mass of (E-2) fumed silica whose surface is treated with dimethyldichlorosilane (product name; MU-215, Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then (B-1) 8 parts by mass of the hydrolyzable organosilane compound 1 was added and thoroughly mixed. Finally, (D-1) γ-aminopropyltrimethoxysilane (product name; KBM-903, Shin-Etsu Chemical Co., Ltd.) was added to 1 part by mass, and (C-1) dioctyltin dilaurate was added to 0.1 parts by mass, and thoroughly mixed under reduced pressure to obtain composition 1.

[0073] [Example 2] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R1 = methyl group, a = approximately 620), 100 parts by mass of (E-1) heavy calcium carbonate the surface of which has been treated with a paraffin-based material (product name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) and 10 parts by mass of (E-2) fumed silica the surface of which has been treated with dimethyldichlorosilane (product name: MU-215, manufactured by Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then 8 parts by mass of (B-1) the hydrolyzable organosilane compound 1 was added and thoroughly mixed. Finally, 1 part by mass of (D-2) γ-glycidoxypropyltrimethoxysilane (product name: KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) and 4 parts by mass of (C-2) titanium diisopropoxybis(ethylacetoacetate) (product name: Orgatix TC750, manufactured by Matsumoto Fine Chemical Co., Ltd.) were added and thoroughly mixed under reduced pressure to obtain composition 2.

[0074] [Example 3] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R 1 = methyl group, a = about 620) to 100 parts by mass of (E-1) heavy calcium carbonate whose surface is treated with paraffin (product name; MC Coat P-20, Maruo Calcium Co., Ltd.), 10 parts by mass of (E-2) fumed silica whose surface is treated with dimethyldichlorosilane (product name; MU-215, Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then (B-1) 8 parts by mass of the hydrolyzable organosilane compound 1 was added and thoroughly mixed. Finally, (D-3) 1 part by mass of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (product name; KBM-603, Shin-Etsu Chemical Co., Ltd.) and (C-3) 0.6 parts by mass of γ-tetramethylguanidylpropyltrimethoxysilane were added and thoroughly mixed under reduced pressure to obtain composition 3.

[0075] [Example 4] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R 1 = methyl group, a = approximately 620), 100 parts by mass of (E-1) heavy calcium carbonate the surface of which has been treated with a paraffin-based material (product name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) and 10 parts by mass of (E-2) fumed silica the surface of which has been treated with dimethyldichlorosilane (product name: MU-215, manufactured by Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then 8 parts by mass of (B-1) the hydrolyzable organosilane compound 1 was added and thoroughly mixed. Finally, 1 part by mass of (D-1) γ-aminopropyltrimethoxysilane (product name: KBM-903, manufactured by Shin-Etsu Chemical Co., Ltd.) and 1 part by mass of (C-4) an organic bismuth catalyst mainly composed of bismuth tris(2-ethylhexanoate) (product name: Neostan U-600, manufactured by Nitto Kasei Co., Ltd.) were added and thoroughly mixed under reduced pressure to obtain composition 4.

[0076] [Example 5] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R 1 = methyl group, a = about 620) to 100 parts by mass of (E-1) heavy calcium carbonate whose surface is treated with paraffin (product name; MC Coat P-20, Maruo Calcium Co., Ltd.), 10 parts by mass of (E-2) fumed silica whose surface is treated with dimethyldichlorosilane (product name; MU-215, Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then 8 parts by mass of (B-2) the hydrolyzable organosilane compound 2 were added and thoroughly mixed. Finally, 1 part by mass of (D-3) N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (product name; KBM-603, Shin-Etsu Chemical Co., Ltd.) and 0.6 parts by mass of (C-3) γ-tetramethylguanidylpropyltrimethoxysilane were added and thoroughly mixed under reduced pressure to obtain composition 5.

[0077] [Example 6] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R 1 = methyl group, a = about 620) to 100 parts by mass of (E-1) heavy calcium carbonate whose surface is treated with paraffin (product name; MC Coat P-20, Maruo Calcium Co., Ltd.), 10 parts by mass of (E-2) fumed silica whose surface is treated with dimethyldichlorosilane (product name; MU-215, Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then (B-3) 8 parts by mass of the hydrolyzable organosilane compound 3 was added and thoroughly mixed. Finally, (D-3) 1 part by mass of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (product name; KBM-603, Shin-Etsu Chemical Co., Ltd.) and (C-3) 0.6 parts by mass of γ-tetramethylguanidylpropyltrimethoxysilane were added and thoroughly mixed under reduced pressure to obtain composition 6.

[0078] [Comparative Example 1] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R 1 = methyl group, a = about 620) to 100 parts by mass of (E-1) heavy calcium carbonate whose surface is treated with paraffin (product name; MC Coat P-20, Maruo Calcium Co., Ltd.), 100 parts by mass of (E-2) fumed silica whose surface is treated with dimethyldichlorosilane (product name; MU-215, Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then 10 parts by mass of (B') methyl trismethylethylketoximesilane were added and thoroughly mixed. Finally, 1 part by mass of (D-1) γ-aminopropyltrimethoxysilane (product name; KBM-903, Shin-Etsu Chemical Co., Ltd.) and 0.1 parts by mass of (C-1) dioctyltin dilaurate were added and thoroughly mixed under reduced pressure to obtain composition 7.

[0079] [Comparative Example 2] (A') a linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both molecular chain terminals capped with methyldimethoxy groups (in the general formula (1) above, R 1 = methyl group, a = about 620) to 100 parts by mass of (E-1) heavy calcium carbonate whose surface is treated with paraffin (product name; MC Coat P-20, Maruo Calcium Co., Ltd.), 10 parts by mass of (E-2) fumed silica whose surface is treated with dimethyldichlorosilane (product name; MU-215, Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then 10 parts by mass of (B'') methyltrimethoxysilane were added and thoroughly mixed. Finally, 1 part by mass of (D-2) γ-glycidoxypropyltrimethoxysilane (product name; KBM-403, Shin-Etsu Chemical Co., Ltd.) and 4 parts by mass of (C-2) titanium diisopropoxybis(ethylacetoacetate) (product name; Orgatics TC750, Matsumoto Fine Chemical Co., Ltd.) were added and thoroughly mixed under reduced pressure to obtain composition 8.

[0080] [Comparative Example 3] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R 1 = methyl group, a = about 620) to 100 parts by mass of (E-1) heavy calcium carbonate whose surface is treated with paraffin (product name; MC Coat P-20, Maruo Calcium Co., Ltd.), 100 parts by mass of (E-2) fumed silica whose surface is treated with dimethyldichlorosilane (product name; MU-215, Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then 10 parts by mass of (B'') methyltrimethoxysilane were added and thoroughly mixed. Finally, 1 part by mass of (D-1) γ-aminopropyltrimethoxysilane (product name; KBM-903, Shin-Etsu Chemical Co., Ltd.) and 1 part by mass of (C-4) organic bismuth catalyst whose main component is bismuth tris(2-ethylhexanoate) (product name; Neostan U-600, Nitto Kasei Co., Ltd.) were added and thoroughly mixed under reduced pressure to obtain composition 9.

[0081] [Comparative Example 4] (A) A linear dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain of which are blocked with silanol groups (hydroxyl groups bonded to silicon atoms) (in the above general formula (1), R 1 = methyl group, a = about 620) to 100 parts by mass of (E-1) heavy calcium carbonate whose surface is treated with paraffin (product name; MC Coat P-20, Maruo Calcium Co., Ltd.), 10 parts by mass of (E-2) fumed silica whose surface is treated with dimethyldichlorosilane (product name; MU-215, Shin-Etsu Chemical Co., Ltd.) were added and thoroughly mixed, and then 8 parts by mass of (B''') vinyltrisisopropoxysilane were added and thoroughly mixed. Finally, 1 part by mass of (D-3) N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (product name; KBM-603, Shin-Etsu Chemical Co., Ltd.) and 0.6 parts by mass of (C-3) γ-tetramethylguanidylpropyltrimethoxysilane were added and thoroughly mixed under reduced pressure to obtain composition 10.

[0082] [Test Method] The following evaluations were carried out for each of the compositions (room-temperature-curable organopolysiloxane compositions) prepared in the above Examples 1 to 6 and Comparative Examples 1 to 4. The evaluation results are shown in Table 1 below, together with the blending amounts of Examples 1 to 6 and Comparative Examples 1 to 4.

[0083] (Initial evaluation) As an initial evaluation, the following tack-free time, curing speed, rubber properties, and adhesion were evaluated using each of the compositions immediately after preparation. Tuck Free Time Using each of the compositions prepared in the above Examples and Comparative Examples, the tack-free time (touch-dry time) was measured according to the method prescribed in JIS A 5758.

[0084] curing speed The hardening rate test method was to fill each composition prepared in the above Examples and Comparative Examples into a glass petri dish with an inner diameter of 10 mm, and after one day (24 hours) at 23°C and 50% RH, the hardened thickness (depth) was measured from the part exposed to air by inserting a probe.

[0085] Rubber properties Each composition prepared in the above Examples and Comparative Examples was poured into a 2 mm mold and cured at 23°C and 50% RH for 7 days to obtain a rubber sheet with a thickness of 2 mm. The rubber physical properties (type A durometer hardness, tensile strength, and elongation at break) were measured in accordance with JIS K 6249.

[0086] Adhesiveness Each composition prepared in the above Examples and Comparative Examples was cured by aging for 7 days at 23°C and 50% RH between two aluminum plates with a width of 25 mm and a length of 100 mm. The adhesive area between the upper and lower aluminum plates was 2.5 cm 2 A 1 mm thick layer of the cured silicone rubber was formed to prepare shear adhesion test specimens. The shear adhesive strength and cohesive failure rate for each test specimen were measured according to the method specified in JIS K 6249.

[0087] (Heat and humidity resistance evaluation) To confirm the moisture and heat resistance performance, the obtained cured silicone rubber sheet and shear adhesion test specimen were exposed to an environment of 85°C and 85% RH and allowed to deteriorate for 1,000 hours, and then tests (rubber properties, adhesion) similar to those performed at the initial stage of production (initial evaluation) were conducted to confirm the moisture and heat resistance.

[0088] (Heat resistance evaluation) To confirm heat resistance, the obtained cured silicone rubber sheet and shear adhesion test specimen were exposed to a dry environment at 150°C and allowed to deteriorate for 1,000 hours, and then tests (rubber properties, adhesion) similar to those performed at the initial stage of production (initial evaluation) were conducted to confirm heat resistance.

[0089] [Table 1]

[0090] [Table 2]

[0091] From the above results, it was shown that the room temperature curable organopolysiloxane composition of the present invention has good curability (tack-free time, curing speed), rubber properties, and adhesion in the initial evaluation, regardless of whether a tin catalyst, a titanium catalyst, an organic strong base catalyst, or an organic bismuth catalyst is used, and also has good properties in the moist heat resistance test and the heat resistance test. The properties of the room temperature curable organopolysiloxane composition of the present invention are not inferior to the commonly used oxime-free, alcohol-free, and acetone-free compositions. Furthermore, as shown in Example 4, the room temperature curable organopolysiloxane composition of the present invention shows good properties even when an organic bismuth catalyst is used, but the alcohol-free composition of Comparative Example 3 using an organic bismuth catalyst did not cure. From these results, it can be seen that the hydrolyzable organosilane compound used in the room temperature curable organopolysiloxane composition of the present invention has better endblocking ability and curing ability than the alcohol-free curing agent. The compound released during curing from the compositions of the examples is cyclopentanone, which is a highly safe compound with no reported health hazards such as carcinogenicity and reproductive toxicity to the human body, or environmental hazards such as toxicity to aquatic organisms. On the other hand, the compounds released during curing from the compositions of the comparative examples are all labeled with health hazards in SDS (Safety Data Sheets) and the like, and are 2-butanone oxime, which may be carcinogenic and is toxic to aquatic organisms, methanol, which is designated as a deleterious substance and is highly harmful to the human body, and acetone, which causes damage to organs through repeated exposure. Also, since methanol and acetone have lower flash points and boiling points than cyclopentanone, it can be seen that the room temperature curable organopolysiloxane composition of the present invention is superior in terms of human health and environmental protection.

[0092] From the above results, it was confirmed that the room-temperature-curable organopolysiloxane composition of the present invention releases safer compounds during curing, has good curing properties even when various catalysts are used, and the cured product has good physical properties, adhesiveness, and durability (moisture heat resistance, heat resistance), making it suitable for use in a variety of applications (adhesives, sealing materials, potting agents, coating agents, etc.).

[0093] The synthesis examples of the novel hydrolyzable organosilane compounds of the present invention are shown below. The synthesized compounds are 1 Identification was performed by 1 H-NMR, and synthesis was confirmed.

[0094] [Synthesis Example 1] Synthesis of hydrolyzable organosilane compound 4 Cyclopentanone 834g (9.9mol), triethylamine 825g (8.2mol), copper(I) chloride 5g (0.05mol), and hexane 1,500ml were charged into a 5,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, a reflux condenser, and a dropping funnel, and vinyltrichlorosilane 400g (2.47mol) was added dropwise over about 2 hours at 40-60°C. After stirring at 80°C for 12 hours, the generated triethylamine hydrochloride was removed by filtration, and hexane was distilled from the filtrate at 100°C and normal pressure, and then the mixture was distilled at 180°C and 300Pa to obtain hydrolyzable organosilane compound 4 (yield 532g, 69%). This reaction formula is represented by the following formula [II]. 1 H-NMR(400MHz,CDCl3)δ6.11(-CH=C H 2,m,2H),δ6.02(-C H =CH2,m,1H), δ4.43(-OC(CH2)=C H- ,s,3H),δ2.20(-OC-C H 2-,t,6H),δ2.15(-OC=CH- CH 2-,m,6H) δ2.15(-OC-CH2- CH 2-,m,6H) [ka]

[0095] [Synthesis Example 2] Synthesis of hydrolyzable organosilane compound 5 Cyclopentanone 834g (9.9mol), triethylamine 825g (8.2mol), copper(I) chloride 5g (0.05mol), and hexane 1,500ml were charged into a 5,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, a reflux condenser, and a dropping funnel, and phenyltrichlorosilane 522g (2.47mol) was dropped over about 2 hours in the range of 40-60°C. After stirring at 80°C for 12 hours, the generated triethylamine hydrochloride was removed by filtration, and hexane was distilled from the filtrate at 100°C and normal pressure, and then distilled at 200°C and 300Pa to obtain hydrolyzable organosilane compound 5 (yield 568g, yield 65%). This reaction formula is represented by the following formula [III]. 1 H-NMR(400MHz, CDCl3)δ6.64(Si-C6 H 5,m,5H), δ4.40(-OC(CH2)=C H- ,s,3H),δ2.20(-OC-C H 2-,t,6H),δ2.15(-OC=CH- CH 2-,m,6H) δ2.13(-OC-CH2- CH 2-,m,6H) [ka]

[0096] [Synthesis Example 3] Synthesis of hydrolyzable organosilane compound 6 A 5,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, a reflux condenser and a dropping funnel was charged with 758g (9.0mol) of cyclopentanone, 727g (7.2mol) of triethylamine, 5g (0.05mol) of copper(I) chloride and 1200ml of hexane, and 255g (1.5mol) of tetrachlorosilane was dropped over about 2 hours at 40℃ to 60℃. After stirring for 12 hours at 80℃, the generated triethylamine hydrochloride was removed by filtration, and the hexane was distilled from the filtrate at 100℃ and normal pressure, and then the hydrolyzable organosilane compound 6 was obtained by distillation at 210℃ and 300Pa (yield 302g, 56%). This reaction formula is represented by the following formula [IV]. 1 H-NMR(400MHz,CDCl3)δ4.45(-OC(CH2)=C H- ,s,4H),δ2.22(-OC-C H 2-,t,8H), δ2.15(-OC=CH- CH 2-,m,8H) δ2.15(-OC-CH2- CH 2-,m,8H) [ka]

[0097] [Composition Example 1] A linear dimethylpolysiloxane (R 1 A composition was prepared by adding 100 parts by mass of a dimethylpolysiloxane corresponding to (a = methyl group, a = approximately 620), 7 parts by mass of hydrolyzable organosilane compound 4, and 0.5 parts by mass of γ-tetramethylguanidylpropyltrimethoxysilane, and mixing them until they became uniform while blocking out moisture.

[0098] Composition Example 2 A linear dimethylpolysiloxane (R 1A composition was prepared by adding 100 parts by mass of a dimethylpolysiloxane corresponding to (a = methyl group, a = approximately 620), 7 parts by mass of hydrolyzable organosilane compound 5, and 0.5 parts by mass of γ-tetramethylguanidylpropyltrimethoxysilane, and mixing them until they became uniform while blocking out moisture.

[0099] Composition Example 3 A linear dimethylpolysiloxane (R 1 A composition was prepared by adding 100 parts by mass of a dimethylpolysiloxane corresponding to (a = methyl group, a = approximately 620), 7 parts by mass of hydrolyzable organosilane compound 6, and 0.5 parts by mass of γ-tetramethylguanidylpropyltrimethoxysilane, and mixing them until they became uniform while blocking out moisture.

[0100] [Comparative Composition Example 1] A linear dimethylpolysiloxane (R 1 A composition was prepared by adding 100 parts by mass of dimethylpolysiloxane (corresponding to a = methyl group, a = approximately 620), 7 parts by mass of vinyl trisketoximesilane, and 0.1 parts by mass of dioctyltin dilaurate, and mixing them in a moisture-proof state until they became uniform.

[0101] [Comparative Composition Example 2] A linear dimethylpolysiloxane (R 1 A composition was prepared by adding 100 parts by mass of dimethylpolysiloxane (corresponding to a = methyl group, a = approximately 620), 7 parts by mass of vinyltrimethoxysilane, and 0.1 parts by mass of dioctyltin dilaurate, and mixing them in a moisture-proof state until they became uniform.

[0102] The compositions prepared in the above Composition Examples and Comparative Composition Examples were poured into a 2 mm mold and cured for 7 days at 23°C and 50% RH to obtain a 2 mm thick rubber sheet. The tack-free time (touch-dry time) was measured according to the method specified in JIS A 5758, and the rubber properties (hardness, elongation at break, tensile strength) of the 2 mm thick sheet were measured according to JIS K 6249. The results are shown in Table 3 below.

[0103] [Table 3]

[0104] It was found that the hydrolyzable organosilane compound of the present invention exhibits high curability even when a basic catalyst is used, and the tack-free time is very short compared to conventional crosslinking agents. In addition, the physical properties after curing were also satisfactory. On the other hand, in the composition examples 1 and 2, the use of a highly toxic tin catalyst was essential, and the tack-free time was long and the curing property was poor. In the compositions of the composition examples 1 to 3, the gas released during curing is cyclopentanone, a highly safe compound, and is also advantageous in terms of safety compared to the composition of the composition example 1 that releases 2-butanone oxime, which is suspected to be carcinogenic, and the composition of the composition example 2 that releases methanol, which is a deleterious substance.

Claims

1. (A) 100 parts by mass of an organopolysiloxane having a viscosity of 20 to 1,000,000 mPa·s at 23° C. and represented by the following general formula (1): HO-(SiR 1 2 O) a -+ (1) (In the formula, R 1 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and each R 1 may be the same or different groups; a is an integer of 50 or more; and (B) a hydrolyzable organosilane compound represented by the following general formula (2) and / or a partial hydrolysis condensate thereof: 1 to 40 parts by mass 【Chemistry 1】 (In the formula, R 2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, n is an integer from 1 to 8, and m is 3 or 4. A room temperature curable organopolysiloxane composition comprising:

2. 2. The room-temperature-curable organopolysiloxane composition according to claim 1, wherein the hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof, component (B), is one which releases a cyclic ketone compound upon hydrolysis.

3. 3. The room temperature curable organopolysiloxane composition according to claim 2, wherein the cyclic ketone compound which is eliminated is cyclobutanone or cyclopentanone.

4. 4. The room-temperature-curable organopolysiloxane composition according to claim 1, wherein the hydrolyzable organosilane compound of component (B) is a hydrolyzable organosilane compound represented by the following general formula (4): 【Chemistry 2】 (In the formula, R 6 is a vinyl group or a phenyl group, and m is 3 or 4.

5. 5. The room-temperature-curable organopolysiloxane composition according to any one of claims 1 to 4, further comprising 0.01 to 10 parts by mass of a curing catalyst (C) per 100 parts by mass of component (A).

6. 6. The room-temperature-curable organopolysiloxane composition according to claim 5, wherein the curing catalyst (C) is at least one catalyst selected from the group consisting of tin catalysts, titanium catalysts, strong organic base catalysts, and organobismuth catalysts.

7. 7. The room-temperature-curable organopolysiloxane composition according to any one of claims 1 to 6, which does not contain a tin catalyst.

8. The room-temperature-curable organopolysiloxane composition according to any one of claims 1 to 7, further comprising (D) 0.01 to 10 parts by mass of a silane coupling agent represented by the following general formula (3) and / or a partial hydrolysis condensate thereof, per 100 parts by mass of component (A): R 3 R 4 b SiX 3-b (3) (In the formula, R 3 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms and at least one functional group (excluding guanidyl groups) containing one or more heteroatoms selected from a nitrogen atom, a sulfur atom, and an oxygen atom. 4 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and X is a hydrolyzable group. b is 0, 1, or 2.

9. 9. The room-temperature-curable organopolysiloxane composition according to any one of claims 1 to 8, further comprising 1 to 500 parts by mass of an inorganic filler (E) per 100 parts by mass of component (A).

10. 10. The room temperature curable organopolysiloxane composition according to claim 9, wherein component (E) is one or more inorganic fillers selected from the group consisting of calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide.

11. An adhesive comprising the room temperature curable organopolysiloxane composition according to any one of claims 1 to 10.

12. A sealant comprising the room temperature curable organopolysiloxane composition according to any one of claims 1 to 10.

13. A potting agent comprising the room temperature curable organopolysiloxane composition according to any one of claims 1 to 10.

14. A coating agent comprising the room temperature curable organopolysiloxane composition according to any one of claims 1 to 10.

15. A hydrolyzable organosilane compound represented by the following general formula (4): 【Chemistry 3】 (In the formula, R 6 is a vinyl group or a phenyl group, and m is 3 or 4.

16. The hydrolyzable organosilane compound according to claim 15, which eliminates cyclopentanone by hydrolysis.

17. The following reaction formula [I] 【Chemistry 4】 (In the formula, R 6 , m is as defined above.) 17. The method for producing a hydrolyzable organosilane compound according to claim 15 or 16, comprising a step of reacting a chlorosilane compound represented by the following formula (I) with cyclopentanone in the presence of a basic substance and a catalyst.

18. 18. The method for producing a hydrolyzable organosilane compound according to claim 17, wherein the amount of cyclopentanone added is 0.95 to 3.0 moles per mole of chlorine atoms in the chlorosilane compound.

19. 19. The method for producing a hydrolyzable organosilane compound according to claim 17 or 18, wherein the catalytic substance is copper chloride, copper iodide, copper bromide, silver chloride, silver iodide or silver bromide.

20. The method for producing a hydrolyzable organosilane compound according to any one of claims 17 to 19, wherein the amount of the catalyst substance added is 0.001 to 0.5 moles per mole of the chlorosilane compound.

21. 21. The method for producing a hydrolyzable organosilane compound according to any one of claims 17 to 20, wherein the basic substance is trimethylamine, triethylamine, tripropylamine, tributylamine, urea, diazabicycloundecene, or diazabicyclononene.

22. 22. The method for producing a hydrolyzable organosilane compound according to any one of claims 17 to 21, wherein the amount of the basic substance added is 0.95 to 2.5 moles per mole of chlorine atoms in the chlorosilane compound.

Citation Information

Patent Citations

  • Shinkina 5 9 beeta 2 chikan 22 tetorahidorofurufuriruu 6 77 benzomorufuan oyobi sonosanfukaenno seizohoho

    JP1976039673A

  • Method for producing room temperature-curable organopolysiloxane composition, sealant, and article

    JP2015113377A

  • Hardening silicone composition

    JP2018515634A

  • Room temperature curing organopolysiloxane composition and production method thereof, and long life coolant sealant for automobile

    JP2019073670A

  • Curable silicone rubber compounds

    JP2020517771A