Zn-Al-Mg-Si coated steel sheet
The Zn-Al-Mg-Si plated steel sheet addresses the need for enhanced corrosion resistance at dissimilar joints with aluminum alloy parts by incorporating a ternary eutectic structure and acicular Mg 2Si alloy phase, resulting in improved appearance and joint corrosion resistance.
Patent Information
- Application Number
- JP2024532584
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-05
AI Technical Summary
There is a demand for improved appearance corrosion resistance and corrosion resistance at dissimilar joints in plated steel sheets, particularly when combined with aluminum alloy parts, due to the increasing use of aluminum alloy sheets in automobile bodies to reduce weight, and the need for enhanced corrosion resistance at these joints.
A Zn-Al-Mg-Si plated steel sheet is developed with a specific composition and structure, including a ternary eutectic structure and acicular Mg 2Si alloy phase on the surface, formed using a controlled plating process with a mixed gas wiping technique to enhance corrosion resistance.
The Zn-Al-Mg-Si plated steel sheet exhibits excellent appearance corrosion resistance and improved corrosion resistance at dissimilar joints with aluminum alloy parts, particularly in flat plate and processed parts, through the formation of a dense Si alloy phase on the surface.
Smart Images

Figure 0007574971000003 
Figure 0007574971000001 
Figure 0007574971000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a Zn-Al-Mg-Si plated steel sheet. [Background technology]
[0002] Zinc plating, which suppresses the corrosion of iron through sacrificial corrosion protection, is excellent in rust prevention performance and economy, and is widely used to manufacture steel materials with high corrosion resistance. In particular, hot-dip galvanized steel materials, in which a plating layer is formed by immersing a steel material in molten zinc, have a simpler manufacturing process and a lower product price than electrogalvanized steel materials, and therefore demand is increasing across industries such as automobiles, home appliances, and building materials. However, due to the worsening of air pollution and corrosive environments associated with industrial advancement, and the depletion of zinc resources due to a significant increase in zinc usage, there has been a demand for plated steel materials that are more corrosion resistant than conventional zinc plating and that also require less zinc.
[0003] Patent Document 1 discloses a Zn-Al-Mg plated steel material in which elements such as aluminum (Al) and magnesium (Mg) are added to zinc (Zn) to improve the corrosion resistance of the steel material. Patent Document 2 reports that the addition of silicon (Si) to the Zn-Al-Mg plated layer improves the corrosion resistance of the plated steel material at the flat and end surfaces compared to conventional Zn-Al-Mg plated steel sheets. Patent Document 3 reports that the addition of Si to the plated layer of a Zn-Al-Mg plated steel sheet to concentrate Si at the interface between the plated layer and the base steel sheet gives the plated layer fracture toughness and improves the corrosion resistance after processing. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 4-147955 [Patent Document 2] JP 2005-82834 A [Patent Document 3] Patent Publication No. 2021-508771 Summary of the Invention [Problem to be solved by the invention]
[0005] However, further improvements in the appearance corrosion resistance and joint corrosion resistance of plated steel sheets have been required.In addition, as the use of aluminum alloy sheets and aluminum die castings in automobile bodies has increased in order to drastically reduce the weight of automobiles, corrosion resistance at dissimilar joints between plated steel sheet members and aluminum alloy members has become a new required property, and corrosion resistance at dissimilar joints with aluminum alloy members has been desired.
[0006] In view of the above problems, the present invention aims to provide a Zn-Al-Mg-Si plated steel sheet that is excellent in appearance corrosion resistance and in dissimilar joint corrosion resistance at the contact points between the flat plate portion and the processed portion and an aluminum alloy. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and have come to the following findings. In a Zn-Al-Mg-Si-plated steel sheet, the Mg2Si alloy phase is formed in the surface layer of the plating layer, thereby improving the appearance corrosion resistance and the corrosion resistance of dissimilar joints at the contact area between the flat plate part and the processed part and the aluminum alloy. In addition, when the plated steel sheet is manufactured, the wiping gas (gas used in gas wiping) is a mixed gas of H2 and N2, whereby the Mg2Si alloy phase can be formed in the surface layer of the plating layer.
[0008] That is, the gist and configuration of the present invention are as follows.
[0009] [1] A steel sheet having a base steel sheet and a plating layer formed on at least one surface of the base steel sheet, the plating layer has a composition containing, in mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities, and has a Zn-Al-MgZn2 ternary eutectic structure; In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, needle-shaped Mg2Si alloy phases having a long side length of 0.5 μm or more were observed on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 100,000 pieces / mm 2 A Zn-Al-Mg-Si-plated steel sheet characterized in that the above-mentioned components are present.
[0010] [2] In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the number density of needle-shaped Mg2Si alloy phases with a long side length of 0.5 μm or more present on the Zn-Al-MgZn2 ternary eutectic structure is 1000 pieces / mm 2 The Zn-Al-Mg-Si plated steel sheet according to the above-mentioned [1], which is as follows: Effect of the Invention
[0011] According to the present invention, it is possible to provide a Zn-Al-Mg-Si plated steel sheet that is excellent in appearance corrosion resistance and in dissimilar joint corrosion resistance at the contact points between the flat plate portion and the processed portion and an aluminum alloy. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1(a) is a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of a plating layer with an electron beam at an accelerating voltage of 7.0 kV in one embodiment of the present invention, and FIG. 1(b) to (e) are the Mg distribution, Si distribution, Al distribution, and Zn distribution, respectively, obtained by composition analysis using EDS. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the Zn-Al-Mg-Si-plated steel sheet according to the present invention will be described. Note that the embodiment described below is one example of the present invention, and the configuration of the present invention is not limited to this specific example.
[0014] A Zn-Al-Mg-Si-plated steel sheet according to one embodiment of the present invention comprises a base steel sheet and a plating layer formed on at least one surface of the base steel sheet. The plating layer has a composition, by mass%, of 0.50-3.00% Mg, 0.10-3.00% Al, 0.010-0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities, and a Zn-Al-MgZn2 ternary eutectic structure. Furthermore, in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, needle-shaped Mg2Si alloy phases having a long side length of 0.5 μm or more are present on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 100,000 pieces / mm 2 The present invention is characterized in that:
[0015] The type of the base steel sheet used in the present invention is not particularly limited, and for example, a hot-rolled steel sheet or hot-rolled steel strip that has been pickled and descaled, or a cold-rolled steel sheet or cold-rolled steel strip obtained by cold rolling the hot-rolled steel sheet or hot-rolled steel strip can be used. There is also no particular limit to the thickness of the base steel sheet, but it is preferably 0.7 to 2.0 mm.
[0016] Next, the composition of the Zn-Al-Mg-Si based plating layer in the present invention will be described.
[0017] If the content of Mg in the plating layer is less than 0.50% by mass, the effect of improving the corrosion resistance of dissimilar joints at the contact portion between the flat plate portion and the processed portion and the aluminum alloy is insufficient. Therefore, the content of Mg in the plating layer is set to 0.50% by mass or more, and preferably 1.00% by mass or more. On the other hand, if the content of Mg in the plating layer exceeds 3.00% by mass, a brittle block-like MgZn2 phase is formed, the plating layer becomes brittle, the adhesion decreases, and the workability and the corrosion resistance of the processed portion may deteriorate. Therefore, the content of Mg in the plating layer is set to 3.00% by mass or less, and preferably 2.50% by mass or less.
[0018] If the content of Al in the plating layer is less than 0.10% by mass, the effect of improving the corrosion resistance of dissimilar joints at the contact points between the flat plate portion and the processed portion and the aluminum alloy is insufficient. Therefore, the content of Al in the plating layer is set to 0.10% by mass or more, and preferably 0.50% by mass or more. On the other hand, if the content of Al in the plating layer exceeds 3.00% by mass, swelling from scratches occurring after painting of the plated steel sheet becomes large, and the appearance corrosion resistance deteriorates. Therefore, the content of Al in the plating layer is set to 3.00% by mass or less, and preferably 2.00% by mass or less.
[0019] When the content of Si in the plating layer is 0.010% by mass or more, it forms an Mg2Si alloy phase together with Mg in the plating layer, which contributes to improving the corrosion resistance of the plating layer. This is thought to be due to the following action. That is, since the Mg2Si alloy phase is active, it reacts with water in a corrosive environment and decomposes, and in the plating structure of the Zn-Al-MgZn2 ternary eutectic described below, it sacrificially protects the metal structure containing one or more of the Zn phase, Al phase, and MgZn2 alloy phase. At the same time, the corrosion product of Mg formed forms a protective film and suppresses further progress of corrosion. Therefore, the corrosion resistance of the dissimilar joints at the contact parts with the aluminum alloy of the flat plate part and the processed part is improved. In order to obtain the above effect, the content of Si in the plating layer is 0.010% by mass or more, and preferably 0.050% by mass or more. On the other hand, when the content of Si in the plating layer exceeds 0.20% by mass, a large amount of Mg2Si alloy phase is formed even inside the plating layer. Since the Mg2Si alloy phase is brittle, if a large amount of the Mg2Si alloy phase is formed inside the plating layer, it will induce cracks inside the plating layer in response to external stress. As a result, the plating layer is prone to cracking during forming, and the corrosion resistance of the dissimilar joint at the contact area with the aluminum alloy of the processed part will decrease. Therefore, the Si content in the plating layer is set to 0.20 mass% or less, and preferably 0.15 mass% or less.
[0020] If the Fe content in the coating layer exceeds 0.30 mass%, the growth of the alloy layer formed at the interface between the base steel sheet and the coating layer increases, and workability decreases. Therefore, the Fe content in the coating layer is set to 0.30 mass% or less, and preferably 0.20 mass% or less. On the other hand, the lower limit of the Fe content in the coating layer is not particularly limited, and may be 0.00 mass%.
[0021] The balance of the composition of the plating layer other than the above consists of Zn and unavoidable impurities.
[0022] Next, the structure of the Zn-Al-Mg-Si based coating layer will be described. The coating layer in the present invention has a Zn-Al-MgZn2 ternary eutectic coating structure, and contains a Mg2Si alloy phase in the coating structure. The coating structure may further contain a Zn phase, an Al phase, or a MgZn2 alloy phase.
[0023] The Mg2Si alloy phase in the Zn-Al-Mg-Si-based coating layer contributes to improving corrosion resistance, but if it is present in large quantities even in the interior of the coating layer, stress concentration occurs in the Mg2Si alloy phase when external stress is applied, promoting the generation and growth of cracks and reducing corrosion resistance after processing. Therefore, it is preferable that the Mg2Si alloy phase is located near the surface of the coating layer. To achieve this, it is necessary to control the Si content in the coating bath components and to use a reducing gas as the wiping gas. If such control is insufficient, the Mg2Si alloy phase may be low in the surface of the coating layer, deteriorating corrosion resistance, or may be formed in large quantities even in the interior of the coating layer, reducing corrosion resistance after processing.
[0024] In the present invention, the phrase "the Mg2Si alloy phase is formed in the surface layer of the plating layer" means that an acicular Mg2Si alloy phase having a long side length of 0.5 μm or more is observed on the Zn-Al-MgZn2 ternary eutectic structure in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope. In order to obtain the effect of improving the corrosion resistance of the Mg2Si alloy phase, the number density of the Mg2Si alloy phase formed in the surface layer of the plating layer must be 100,000 pieces / mm 2 More than 150,000 pieces / mm 2 More preferably, it is 200,000 pieces / mm 2 On the other hand, there is no upper limit to the number density of the Mg2Si alloy phase formed in the surface layer of the plating layer, but even if an appropriate wiping gas is used, it is difficult to make the number density of the plating layer produced using the plating bath composition of the present invention 650,000 pieces / mm or more. 2 Since it is difficult to exceed this number density, the number density is usually 650,000 pieces / mm 2 The following is the result.
[0025] In the present invention, the phrase "the Mg2Si alloy phase is formed inside the plating layer" means that, in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, needle-shaped Mg2Si alloy phases with a long side length of 0.5 μm or more are observed on the Zn-Al-MgZn2 ternary eutectic structure. 2 When the thickness is less than 1000 mm, the corrosion resistance after processing is favorable. Therefore, the number density of the Mg2Si alloy phase formed inside the plating layer is 1000 pieces / mm 2 It is preferable that the number of pieces is 750 pieces / mm or less. 2 More preferably, it is 500 pieces / mm or less. 2 More preferably, it is 0 particles / mm 2 It is most preferable that:
[0026] 1(a) to (e) show backscattered electron images (5000x) and EDS analysis results observed when the surface of the plating layer of the Zn-Al-Mg-Si-plated steel sheet produced in one embodiment of the present invention was irradiated with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope. FIG. 1(a) is a backscattered electron image of the Zn-Al-Mg-Si-plated layer, and (b) to (e) are Mg distribution, Si distribution, Al distribution, and Zn distribution, respectively, analyzed by EDS. As shown in FIG. 1(a) to (e), the Mg2Si alloy phase has a needle-like shape where the compositions of Mg and Si overlap, and it can be seen that it is in the Zn-Al-MgZn2 ternary eutectic structure.
[0027] [Manufacturing method of Zn-Al-Mg-Si plated steel sheet] Next, a method for producing a Zn-Al-Mg-Si-plated steel sheet according to one embodiment of the present invention will be described. The method for producing a Zn-Al-Mg-Si-plated steel sheet according to one embodiment of the present invention includes the steps of immersing a base steel sheet in a plating bath containing, in mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities, to perform a plating treatment on the base steel sheet, and the step of gas wiping the base steel sheet after the plating treatment to adjust the adhesion amount of the plating layer formed on the base steel sheet. The gas wiping is characterized in that it is performed by spraying a mixed gas consisting of H2 and N2 onto the base steel sheet. The cooling method of the plated steel sheet after gas wiping is not particularly limited, and various methods such as air cooling, air-water cooling, and water cooling can be applied.
[0028] In the method for producing a Zn-Al-Mg-Si plated steel sheet according to the present invention, the base steel sheet to be plated is the same as that described above for the base steel sheet.
[0029] When the annealing heat treatment is performed on the base steel sheet before the plating treatment, if the H2 concentration in the furnace atmosphere during annealing is 1 volume % or more, the oxides on the surface of the base steel sheet can be suitably reduced. Therefore, the H2 concentration in the furnace atmosphere during annealing is preferably 1 volume % or more. On the other hand, if the H2 concentration in the furnace atmosphere during annealing is 10 volume % or less, the manufacturing cost can be suitably suppressed. Therefore, the H2 concentration in the furnace atmosphere during annealing is preferably 10 volume % or less. In addition, the furnace atmosphere during annealing is preferably a mixed gas containing H2 and the balance consisting of N2. The temperature of the annealing heat treatment is not particularly limited, but is preferably 600 to 850°C. In addition, the time of the annealing heat treatment is not particularly limited, but is preferably 10 to 60 seconds.
[0030] The plating bath used in the production of the Zn-Al-Mg-Si plated steel sheet according to the present invention has a composition containing, in mass%, 0.50-3.00% Mg, 0.10-3.00% Al, 0.010-0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities. The explanation of each component in the plating bath is the same as the explanation of each component of the plating layer described above. The composition of the plating bath and the composition of the applied plating layer are equivalent.
[0031] The coating weight of the plating layer in the plating process is set at 15g / m from the viewpoint of corrosion resistance. 2 It is preferable that the thickness is 30 g / m or more. 2 On the other hand, the coating weight of the plating layer is preferably 100 g / m or more. 2 If the coating weight of the plating layer is less than 100 g / m, the manufacturing cost can be suppressed favorably. 2 It is preferable that the temperature of the plating bath during plating is 430 to 540°C. If the temperature of the plating bath is less than 430°C, the fluidity of the plating bath may decrease, which may hinder uniform plating coverage. Therefore, the temperature of the plating bath is preferably 430°C or higher. On the other hand, if the temperature of the plating bath exceeds 540°C, there is a risk of an increase in oxides on the surface of the plating bath due to oxidation of Mg in the plating bath, and erosion of the refractory material in the plating bath by Al and Mg. Therefore, the temperature of the plating bath is preferably 540°C or lower, more preferably 530°C or lower.
[0032] In order to form the Mg2Si alloy phase in the surface layer of the coating layer and not to form a large amount inside the coating layer, it is important that the wiping gas has reducing properties. Therefore, the gas wiping of the present invention is performed by spraying a mixed gas consisting of H2 and N2 onto the substrate steel sheet. Conventionally, in the production of hot-dip galvanized steel sheets, air or N2 gas has been used as the wiping gas from the viewpoint of economy. The present inventors have found that, particularly in the production of the Si-containing Zn-Al-Mg-Si-coated steel sheets of the present invention, the surface layer of the coating is oxidized by O2 contained in the wiping gas, and as a result, the desired corrosion resistance may not be obtained. As a result of intensive studies to improve the corrosion resistance of the coating, the present inventors have found that the lower the H2 concentration of the wiping gas, the more difficult it is to suppress the generation of oxides on the surface of the substrate steel sheet, and as a result, the oxides generated on the surface of the substrate steel sheet hinder the formation of the Mg2Si alloy phase in the surface layer of the coating layer and promote its formation inside the coating layer.
[0033] When the H2 concentration of the wiping gas is 1% by volume or more, the Mg2Si alloy phase is preferably formed in the surface layer of the plating layer, and the effect of contributing to the improvement of corrosion resistance is preferably obtained. Therefore, the H2 concentration of the wiping gas is preferably 1% by volume or more. Furthermore, when the H2 concentration of the wiping gas is 5% by volume or more, the generation of oxides on the surface of the base steel sheet is preferably suppressed, the Mg2Si alloy phase is formed in the surface layer of the plating layer, and the formation inside the plating layer is preferably suppressed. On the other hand, when the H2 concentration of the wiping gas is 10% by volume or less, the manufacturing cost can be preferably suppressed. Therefore, the H2 concentration of the wiping gas is preferably 10% by volume or less. The atmosphere during wiping is preferably air.
[0034] Regarding steps and conditions not described in the present invention, conventional methods can be used. EXAMPLES
[0035] Using an ultra-low carbon cold-rolled steel sheet with a thickness of 0.8 mm as the base steel sheet, all the Zn-Al-Mg-Si plated steel sheets to be used as samples were manufactured using hot-dip plating equipment. Each sample was plated using variously changed plating bath compositions, and the temperature of the plating bath was set to 450°C, 30°C higher than the solidification start temperature estimated from the Zn-Al-Mg-Si quaternary equilibrium phase diagram. The base steel sheet was heated in an H2 (5% by volume) + N2 atmosphere, and the temperature of the base steel sheet when immersed in the plating bath was set to the same temperature as the plating bath temperature, and hot-dip plating was performed in the plating bath for 1 second. Thereafter, the thickness of the plating layer was reduced to 7 μm (50 g / m) by adjusting the flow rate of the wiping gas. 2 The plating bath composition, the wiping gas composition, and the plating layer composition are shown in Table 1. Note that the wiping was performed in an air atmosphere.
[0036] [Table 1] TIFF0007574971000002.tif233119
[0037] Each sample of the obtained Zn-Al-Mg-Si plated steel sheet was sheared to a size of 10 x 20 mm. The presence or absence of a Zn-Al-MgZn2 ternary eutectic structure was confirmed by observing the plating layer of the sheared sample from the surface direction of the plated steel sheet using a scanning electron microscope. If a structure consisting of three phases, Zn phase, Al phase, and MgZn2 alloy phase, was found when the composition analysis was performed by EDS during observation, and if the Zn phase, Al phase, and MgZn2 alloy phase were confirmed when the same surface was analyzed by XRD, then the Zn-Al-MgZn2 ternary eutectic structure was present and "present" was recorded in Table 1. If a structure consisting of three phases, Zn phase, Al phase, and MgZn2 alloy phase, was not found when the composition analysis was performed by EDS during observation, and if any of the Zn phase, Al phase, and MgZn2 alloy phase was not confirmed when the same surface was analyzed by XRD, then the Zn-Al-MgZn2 crystalline structure was not present and "absent" was recorded in Table 1.
[0038] The plating layer of the sample after shearing was observed from the surface direction of the plated steel sheet using a scanning electron microscope to observe the state of the Mg2Si alloy phase present in the surface layer and inside of the plating layer, and the number density was evaluated. The number density of the Mg2Si alloy phase present in the surface layer of the plating layer was evaluated from a backscattered electron image (5000x) observed when irradiated with an electron beam at an accelerating voltage of 7.0 kV. The number density of the Mg2Si alloy phase present in the inside of the plating layer was evaluated from a backscattered electron image (5000x) observed when irradiated with an electron beam at an accelerating voltage of 15.0 kV.
[0039] [Appearance and corrosion resistance] Next, to evaluate the appearance and corrosion resistance of the resulting Zn-Al-Mg-Si plated steel sheets after painting, each sample was sheared to a size of 70 x 80 mm, then phosphated under the same conditions, and electrocoated (the thickness of the coating was constant at 15 μm). The coated surface was cut with a blade in a cross shape, and then a corrosion test was performed. At this time, the depth of the blade was set to reach the surface of the base steel. After 90 cycles of corrosion testing according to SAE J2334 (2016), the blister width from the cross-shaped cut scratch on the coated surface was measured, and the maximum blister width was used for evaluation. If the blister width was less than 3 mm, it was marked as "◎", if it was 3 mm or more but less than 5 mm, it was marked as "○", if it was 5 mm or more but less than 7 mm, it was marked as "△", and if it was 7 mm or more, it was marked as "×". If it was marked as "◎" or "○", it was marked as "pass", and if it was marked as "△" or "×", it was marked as "fail".
[0040] [Corrosion resistance of dissimilar plate joints] Next, in order to evaluate the corrosion resistance of the flat dissimilar joints of the Zn-Al-Mg-Si-plated steel sheets, each sample was sheared to a size of 80 x 80 mm, and then bolted to an Al alloy (A6061, Al-0.6Si-1Mg-based) sheared to a size of 40 x 40 mm to prepare a flat dissimilar joint sample of the Zn-Al-Mg-Si-plated steel sheet and the Al alloy. At this time, the joint surface was covered with a resin tape. Then, a corrosion test according to SAE J2334 (2016) was performed on the above dissimilar joint samples. The corrosion amount of the Al alloy after 20 cycles of the corrosion test was evaluated. The amount of Al corrosion was calculated by immersing the flat dissimilar joint samples in a 60 mass% nitric acid aqueous solution at room temperature to remove the corrosion products mainly composed of aluminum, and calculating the difference between the weight before the test and the weight after the corrosion products were removed, in accordance with ISO8407:2021. If the corrosion amount was 5 g / m 2 If less than 5g / m, mark with "◎" 2 More than 10g / m 2 If less than 10g / m, mark as "○" 2 More than 15g / m 2 If it is less than 15g / m, it is marked as "△". 2 In the above cases, it is indicated as "X" in Table 1. The evaluation of ◎ or ◯ was considered to be a pass, and the evaluation of △ or × was considered to be a fail.
[0041] [Corrosion resistance of processed and dissimilar joints] Next, the corrosion resistance of the processed and dissimilar joints of the Zn-Al-Mg-Si-plated steel sheets was evaluated. Each sample was sheared to a size of 70 × 120 mm, and mechanically joined at two points to the Al alloy sheared to a size of 40 × 90 mm by mechanical clinching (5 mmφ) to give a processed part, and a processed dissimilar joint sample of the Zn-Al-Mg-Si-plated steel sheet and the Al alloy was prepared. In this case, the other than the joint surface was treated with phosphate under the same conditions, and then electrocoated (the thickness of the coating was constant at 15 μm) and covered. Then, a corrosion test according to SAE J2334 (2016) was performed on the above processed dissimilar joint samples. The amount of corrosion of the Al alloy after 20 cycles of the corrosion test was evaluated. The amount of Al corrosion was calculated by immersing the processed dissimilar joint sample in a 60 mass% nitric acid aqueous solution at room temperature to remove the aluminum-based corrosion products, and calculating the difference between the weight before the test and the weight after the corrosion products were removed, in accordance with ISO8407:2021. Corrosion rate is 5g / m 2 If less than 5g / m, mark with "◎" 2 More than 10g / m 2 If less than 10g / m, mark as "○" 2 More than 15g / m 2 If it is less than 15g / m, it is marked as "△". 2 In the above cases, it is indicated as "X" in Table 1. The evaluation of ◎ or ◯ was considered to be a pass, and the evaluation of △ or × was considered to be a fail.
[0042] As shown in Table 1, the plating composition specified in the present invention had a number density of Mg2Si alloy phase of 100,000 / mm2 when observed at an accelerating voltage of 7.0 kV. 2 The above-mentioned inventive examples were excellent in corrosion resistance of appearance, corrosion resistance of dissimilar joints of flat plate parts, and corrosion resistance of dissimilar joints of processed plate parts. In other words, it was found that the presence of a large amount of Mg2Si alloy phase in the surface layer of the plating layer has an advantageous effect on the corrosion resistance of appearance, corrosion resistance of dissimilar joints of flat plate parts, and corrosion resistance of dissimilar joints of processed plate parts. In particular, when observed at an accelerating voltage of 15.0 kV, the number density of the Mg2Si alloy phase was 500 / mm 2In contrast, the comparative examples outside the scope of the present invention were inferior to the examples of the present invention in any of the corrosion resistance of the appearance, the corrosion resistance of the flat portion dissimilar joint, and the corrosion resistance of the processed portion dissimilar joint. [Industrial Applicability]
[0043] According to the present invention, it is possible to provide a Zn-Al-Mg-Si plated steel sheet that is excellent in appearance corrosion resistance and in dissimilar joint corrosion resistance at the contact area between the flat plate portion and the processed portion and an aluminum alloy.
Claims
1. A steel sheet having a base steel sheet and a plating layer formed on at least one surface of the base steel sheet, The plating layer has a composition, in mass%, of Mg: 0.50 to 3.00%, Al: 0.10 to 3.00%, Si: 0.010 to 0.20%, and Fe: 0.30% or less, with the balance being Zn and unavoidable impurities; and Zn-Al-MgZn. 2 A ternary eutectic structure; In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, the Zn-Al-MgZn 2 On the ternary eutectic structure, needle-like Mg with a long side length of 0.5 μm or more is 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 The Zn-Al-Mg-Si plated steel sheet is characterized in that the above-mentioned components are present.
2. In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn-Al-MgZn 2 Needle-like Mg with a long side length of 0.5 μm or more that exists on the ternary eutectic structure 2 The number density of the Si alloy phase is 1000 pieces / mm 2 The Zn-Al-Mg-Si plated steel sheet according to claim 1, wherein:
Citation Information
Patent Citations
Plated steel
WO2018139619A1
Plated steel
WO2018139620A1
Production of hot-dip zn-mg-al coated steel sheet
JP1992147955A
Highly corrosion-resistant hot-dip plating steel sheet and manufacturing method therefor
JP2005082834A
Zinc alloy plated steel material with excellent corrosion resistance after processing and its manufacturing method
JP2021508771A