Liquid crystal polymer film and laminate
The liquid crystal polymer film with controlled surface roughness and layered structure addresses adhesion issues, providing superior bonding with copper layers and suitability for laminates and electronic components.
Patent Information
- Application Number
- JP2020197562
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-27
AI Technical Summary
Conventional liquid crystal polymer films exhibit poor adhesion, particularly when bonded to copper foil or when bonding liquid crystal polymer films to each other.
A liquid crystal polymer film with surface roughness Rz of 10 nm to 5000 nm, containing a liquid crystal polymer with specific aromatic repeating units and optionally filled with inorganic or organic fillers, and having multiple layers with varying compositions and thicknesses to enhance adhesion.
The film achieves excellent adhesiveness, as evidenced by high peel strength with copper layers, suitable for use in laminates and electronic components.
Smart Images

Figure 0007575249000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to liquid crystal polymer films and laminates. [Background technology]
[0002] In recent years, the frequencies used in communication devices have tended to become very high. In order to suppress transmission loss in the high frequency band, there is a demand for insulating materials used in circuit boards to have low relative dielectric constants and dielectric loss tangents. Conventionally, polyimide has been widely used as an insulating material for circuit boards, but liquid crystal polymers, which have high heat resistance, low water absorption, and small loss in high frequency bands, have been attracting attention.
[0003] As an example of a conventional liquid crystal polymer film, Patent Document 1 describes a liquid crystal polyester film containing at least a liquid crystal polyester, in which when a first orientation degree is an orientation degree in a first direction parallel to the main surface of the liquid crystal polyester film and a second orientation degree is an orientation degree in a second direction parallel to the main surface and perpendicular to the first direction, the ratio of the first orientation degree to the second orientation degree, that is, first orientation degree / second orientation degree, is 0.95 or more and 1.04 or less, and the third orientation degree of the liquid crystal polyester measured by wide-angle X-ray scattering in a direction parallel to the main surface is 60.0% or more.
[0004] Furthermore, as a film having an uneven surface, Patent Document 2 describes an interlayer film for laminated glass in which embossing consisting of fine unevenness is formed on both sides of a thermoplastic resin sheet, the interlayer film for laminated glass being characterized in that the surface roughness of the embossment on at least one side is Ra of 3.5 to 7.0 μm and the Rab / Ra ratio is 15 to 25% in percentage. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-26474 A [Patent Document 2] JP 2000-203900 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a liquid crystal polymer film having excellent adhesion. Another object of the present invention is to provide a laminate using the liquid crystal polymer film. [Means for solving the problem]
[0007] Means for solving the above problems include the following aspects. <1> A liquid crystal polymer film comprising a liquid crystal polymer, at least one surface of which has a surface roughness Rz of 10 nm to 5000 nm. <2> The surface roughness Rz of both surfaces is 10nm to 5000nm. <1> The liquid crystal polymer film according to claim 1. <3> The melting point Tm of the liquid crystal polymer is 280° C. or higher. <1> or <2> The liquid crystal polymer film according to claim 1. <4> The linear expansion coefficient is -20 ppm / K to 50 ppm / K. <1> ~ <3> 13. The liquid crystal polymer film according to claim 12 . <5> The dielectric tangent is 0.01 or less. <1> ~ <4> 13. The liquid crystal polymer film according to claim 12 . <6> Contains fillers, <1> ~ <5> 13. The liquid crystal polymer film according to claim 12 . <7> the number density of the filler is greater inside than on the surface having the surface roughness Rz of 10 nm to 5000 nm; <6> The liquid crystal polymer film according to claim 1. <8> The liquid crystal polymer has a constitutional repeating unit represented by any one of formulas (1) to (3). <1> ~ <7> 13. The liquid crystal polymer film according to claim 12 . Formula (1) -O-Ar 1-CO- Formula (2) -CO-Ar 2 -CO- Formula (3) -X-Ar 3 -Y- In formulas (1) to (3), Ar 1 represents a phenylene group, a naphthylene group, or a biphenylylene group; Ar 2 and Ar 3 each independently represents a phenylene group, a naphthylene group, a biphenylylene group, or a group represented by the following formula (4), X and Y each independently represent an oxygen atom or an imino group, Ar 1 ~Ar 3 Each hydrogen atom in the above group represented by the formula: may be independently substituted with a halogen atom, an alkyl group or an aryl group. Formula (4) -Ar 4 -Z-Ar 5 - In formula (4), Ar 4 and Ar 5 each independently represents a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylene group. <9> A substrate having a layer A and a layer B provided on at least one surface of the layer A, and a surface roughness Rz of the surface of the layer B is 10 nm to 5000 nm. <1> ~ <9> 13. The liquid crystal polymer film according to claim 12 . <10> The optical fiber further includes a layer C, and the optical fiber has the layer B, the layer A, and the layer C in this order, and the surface roughness Rz of the surface of the layer C is 10 nm to 5000 nm. <10> The liquid crystal polymer film according to claim 1. <11> <10> or <11> and a copper layer disposed on the surface of the liquid crystal polymer film on the Layer B side. <12> The thickness of the layer B is greater than the thickness of the copper layer; <12> The laminate according to claim 1. <13> The peel strength between the layer B and the copper layer is 0.5 kN / m or more. <11> or <12> The laminate according to claim 1. <14> <10> a copper layer disposed on the surface of the liquid crystal polymer film facing the layer B; and a copper layer disposed on the surface of the liquid crystal polymer film facing the layer C. <15> The peel strength between layer C and the copper layer disposed on the surface of layer C is 0.5 kN / m or more. <14> The laminate according to claim 1. Effect of the Invention
[0008] According to one embodiment of the present invention, a liquid crystal polymer film having excellent adhesion can be provided. According to another embodiment of the present invention, a laminate using the liquid crystal polymer film can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The contents of the present disclosure will be described in detail below. The following description of the components may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment. In this specification, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower limit and upper limit. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In addition, in the description of groups (atomic groups) in this specification, descriptions that do not indicate whether they are substituted or unsubstituted include those that have no substituents as well as those that have a substituent. For example, an "alkyl group" includes not only an alkyl group that has no substituents (unsubstituted alkyl groups) but also an alkyl group that has a substituent (substituted alkyl groups). In this specification, "(meth)acrylic" is a term used as a concept including both acrylic and methacrylic, and "(meth)acryloyl" is a term used as a concept including both acryloyl and methacryloyl. In addition, the term "step" in this specification includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In addition, in this disclosure, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous. Furthermore, in the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In addition, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) in the present disclosure are molecular weights detected by a gel permeation chromatography (GPC) analyzer using a column of TSKgel SuperHM-H (product name of Tosoh Corporation) in a solvent of PFP (pentafluorophenol) / chloroform = 1 / 2 (mass ratio) and a differential refractometer, and converted using polystyrene as a standard substance.
[0010] (Liquid crystal polymer film) The liquid crystal polymer film according to the present disclosure contains a liquid crystal polymer, and at least one surface has a surface roughness Rz of 10 nm to 5000 nm.
[0011] It has been found that conventional liquid crystal polymer films have poor adhesion, for example, when bonded to copper foil or when bonded to other liquid crystal polymer films. As a result of extensive investigations, the present inventors have found that the above-mentioned structure makes it possible to provide a liquid crystal polymer film having excellent adhesion. Although the detailed mechanism by which the above effects are obtained is unclear, it is speculated as follows. In the liquid crystal polymer film according to the present disclosure, at least one surface has a surface roughness Rz of 10 nm to 5000 nm. The surface smoothness is not too high, and the surface roughness is not too high, and is moderate. This is thought to prevent air bubbles from forming at the adhesive interface, resulting in excellent adhesion to other layers.
[0012] In the liquid crystal polymer film according to the present disclosure, from the viewpoint of adhesion, the surface roughness Rz of at least one surface is 10 nm to 5000 nm, preferably 20 nm to 1000 nm, and more preferably 50 nm to 500 nm.
[0013] In the liquid crystal polymer film according to the present disclosure, from the viewpoint of adhesion, the surface roughness Rz of both surfaces is preferably 10 nm to 5000 nm, more preferably 20 nm to 1000 nm, and further preferably 50 nm to 500 nm.
[0014] In this disclosure, "surface roughness Rz" refers to the sum of the maximum peak height and the maximum valley depth observed on a roughness curve over a reference length, expressed in nanometers. In the present disclosure, the surface roughness Rz of the surface of the liquid crystal polymer film is measured by the following method. A non-contact surface / layer cross-sectional shape measurement system, VertScan (manufactured by Ryoka Systems), is used to measure an area 465.48 μm long and 620.64 μm wide, and a roughness curve and the average line of the roughness curve are created for the surface of the object to be measured (liquid crystal polymer film). A portion corresponding to the reference length is extracted from the roughness curve. The surface roughness Rz of the object to be measured is measured by calculating the sum of the maximum peak height (i.e., the height from the average line to the peak) and the maximum valley depth (i.e., the height from the average line to the valley bottom) observed in the extracted roughness curve.
[0015] Methods for forming a liquid crystal polymer film having a surface roughness Rz of 10 nm to 5000 nm include, for example, a method of generating Benard cells during film formation, a method of using a solution containing a filler and a liquid crystal polymer, a method of phase separation of a material mixed with a liquid crystal polymer during film formation, a method of forming a skin on the surface during the film formation process and using the difference in the amount of shrinkage with the inside (reticulation), a method of performing a replica process using a mold with an uneven surface during solution film formation, and a method of roughening the film after film formation by surface treatment such as sputtering.
[0016] From the viewpoint of adhesion, the dielectric tangent of the liquid crystal polymer film according to the present disclosure is preferably 0.02 or less, more preferably 0.01 or less, even more preferably 0.005 or less, and particularly preferably greater than 0 and 0.003 or less.
[0017] The dielectric loss tangent in the present disclosure is measured by the following method. The dielectric loss tangent is measured at a frequency of 10 GHz by the resonance perturbation method. A 10 GHz cavity resonator (Kanto Electronics Application Development Co., Ltd. CP531) is connected to a network analyzer (Agilent Technology "E8363B"), and a film sample (width: 2.0 mm x length: 80 mm) is inserted into the cavity resonator. The dielectric loss tangent of the film is measured from the change in resonance frequency before and after insertion for 96 hours in an environment with a temperature of 25°C and a humidity of 60%.
[0018] From the viewpoint of adhesion, the linear expansion coefficient of the liquid crystal polymer film according to the present disclosure is preferably from -20 ppm / K to 50 ppm / K, more preferably from -10 ppm / K to 40 ppm / K, even more preferably from 0 ppm / K to 35 ppm / K, particularly preferably from 10 ppm / K to 30 ppm / K, and particularly more preferably from 15 ppm / K to 25 ppm / K.
[0019] In the present disclosure, the linear expansion coefficient is measured by the following method. Using a thermomechanical analyzer (TMA), a tensile load of 1 g is applied to both ends of a film that is 5 mm wide and 20 mm long, and the film is heated from 25°C to 200°C at a rate of 5°C / min, then cooled to 30°C at a rate of 20°C / min, and heated again at a rate of 5°C / min. The linear expansion coefficient is calculated from the slope of the TMA curve between 30°C and 150°C.
[0020] The liquid crystal polymer film according to the present disclosure comprises a liquid crystal polymer.
[0021] In the present disclosure, the type of liquid crystal polymer is not particularly limited, and any known liquid crystal polymer can be used. The liquid crystal polymer may be a thermotropic liquid crystal polymer that exhibits liquid crystallinity in a molten state, or a lyotropic liquid crystal polymer that exhibits liquid crystallinity in a solution state. In the case of a thermotropic liquid crystal, it is preferable that the liquid crystal polymer melts at a temperature of 450° C. or less. Examples of the liquid crystal polymer include liquid crystal polyester, liquid crystal polyester amide in which an amide bond is introduced into a liquid crystal polyester, liquid crystal polyester ether in which an ether bond is introduced into a liquid crystal polyester, and liquid crystal polyester in which a carbonate bond is introduced into a liquid crystal polyester. Examples include styrene carbonate. From the viewpoint of liquid crystallinity, the liquid crystal polymer is preferably a polymer having an aromatic ring, and more preferably an aromatic polyester or an aromatic polyester amide. Furthermore, the liquid crystal polymer may be a polymer in which an imide bond, a carbodiimide bond, or a bond derived from an isocyanate such as an isocyanurate bond is further introduced into an aromatic polyester or an aromatic polyester amide. The liquid crystal polymer is preferably a wholly aromatic liquid crystal polymer made using only aromatic compounds as raw material monomers.
[0022] Examples of liquid crystal polymers include, for example: 1) (i) A compound obtained by polycondensation of an aromatic hydroxycarboxylic acid, (ii) an aromatic dicarboxylic acid, and (iii) at least one compound selected from the group consisting of an aromatic diol, an aromatic hydroxyamine, and an aromatic diamine. 2) Those obtained by polycondensation of multiple types of aromatic hydroxycarboxylic acids. 3) (i) a polycondensation product of an aromatic dicarboxylic acid and (ii) at least one compound selected from the group consisting of an aromatic diol, an aromatic hydroxyamine, and an aromatic diamine. 4) (i) Polyester such as polyethylene terephthalate and (ii) aromatic hydroxycarboxylic acid are polycondensed. Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, aromatic hydroxyamine and aromatic diamine may each independently be replaced in whole or in part by a polycondensable derivative thereof.
[0023] Examples of polymerizable derivatives of compounds having a carboxy group, such as aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids, include those in which the carboxy group has been converted to an alkoxycarbonyl group or an aryloxycarbonyl group (esters), those in which the carboxy group has been converted to a haloformyl group (acid halides), and those in which the carboxy group has been converted to an acyloxycarbonyl group (acid anhydrides). Examples of polymerizable derivatives of compounds having a hydroxy group, such as aromatic hydroxycarboxylic acids, aromatic diols and aromatic hydroxyamines, include those obtained by acylation of a hydroxy group into an acyloxy group (acylated products). Examples of polymerizable derivatives of compounds having an amino group, such as aromatic hydroxyamines and aromatic diamines, include those obtained by acylation of the amino group to an acylamino group (acylated product).
[0024] From the viewpoint of liquid crystallinity, the liquid crystal polymer preferably has a constitutional repeating unit represented by any one of the following formulas (1) to (3) (hereinafter, the constitutional repeating unit represented by formula (1) etc. may be referred to as repeating unit (1) etc.), more preferably has a constitutional repeating unit represented by the following formula (1), and particularly preferably has a constitutional repeating unit represented by the following formula (1), a constitutional repeating unit represented by the following formula (2), and a constitutional repeating unit represented by the following formula (2). Formula (1) -O-Ar 1 -CO- Formula (2) -CO-Ar 2 -CO- Formula (3) -X-Ar 3 -Y- In formulas (1) to (3), Ar 1 represents a phenylene group, a naphthylene group, or a biphenylylene group; Ar 2 and Ar 3 each independently represents a phenylene group, a naphthylene group, a biphenylylene group, or a group represented by the following formula (4), X and Y each independently represent an oxygen atom or an imino group, Ar 1 ~Ar 3 Each hydrogen atom in the above group represented by the formula: may be independently substituted with a halogen atom, an alkyl group or an aryl group. Formula (4) -Ar 4 -Z-Ar 5 - In formula (4), Ar 4 and Ar 5 each independently represents a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylene group.
[0025] The halogen atom includes a fluorine atom, a chlorine atom, a bromine atom and an iodine atom. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-hexyl group, a 2-ethylhexyl group, an n-octyl group, and an n-decyl group, and the number of carbon atoms is preferably 1 to 10. Examples of the aryl group include a phenyl group, an o-tolyl group, a m-tolyl group, a p-tolyl group, a 1-naphthyl group, and a 2-naphthyl group, and the number of carbon atoms is preferably 6 to 20. When the hydrogen atoms are replaced with these groups, the number of them is Ar 1 , Ar 2 Or Ar 3 The number of each of the above groups represented by the following formula (I) is preferably 2 or less, and more preferably 1.
[0026] Examples of the alkylene group include a methylene group, a 1,1-ethanediyl group, a 1-methyl-1,1-ethanediyl group, a 1,1-butanediyl group, and a 2-ethyl-1,1-hexanediyl group, and the number of carbon atoms is preferably 1 to 10.
[0027] The repeating unit (1) is a constituent repeating unit derived from a specific aromatic hydroxycarboxylic acid. The repeating unit (1) is Ar 1 is a p-phenylene group (constituent repeating unit derived from p-hydroxybenzoic acid), and Ar 1 is preferably a 2,6-naphthylene group (a repeating unit derived from 6-hydroxy-2-naphthoic acid) or a 4,4'-biphenylylene group (a repeating unit derived from 4'-hydroxy-4-biphenylcarboxylic acid).
[0028] The repeating unit (2) is a constituent repeating unit derived from a specific aromatic dicarboxylic acid. Repeating unit (2) is Ar 2 is a p-phenylene group (constituent repeating unit derived from terephthalic acid), Ar 2 is an m-phenylene group (a repeating unit derived from isophthalic acid), Ar 2 is a 2,6-naphthylene group (a repeating unit derived from 2,6-naphthalenedicarboxylic acid), or Ar 2 is a diphenylether-4,4'-diyl group (constituent repeating unit derived from diphenylether-4,4'-dicarboxylic acid).
[0029] The repeating unit (3) is a constituent repeating unit derived from a specific aromatic diol, aromatic hydroxylamine or aromatic diamine. Repeating unit (3) is Ar 3 is a p-phenylene group (constituent repeating units derived from hydroquinone, p-aminophenol or p-phenylenediamine), Ar 3is an m-phenylene group (a repeating unit derived from isophthalic acid), or Ar 3 is a 4,4'-biphenylylene group (a repeating unit derived from 4,4'-dihydroxybiphenyl, 4-amino-4'-hydroxybiphenyl or 4,4'-diaminobiphenyl).
[0030] The content of the repeating unit (1) is preferably 30 mol % or more, more preferably 30 mol % to 80 mol %, even more preferably 30 mol % to 60 mol %, and particularly preferably 30 mol % to 40 mol %, based on the total amount of all constituent repeating units (the mass of each constituent repeating unit constituting the liquid crystal polymer is divided by the formula weight of that repeating unit to determine the substance amount equivalent (mol) of each repeating unit, and the total value). The content of the repeating unit (2) is preferably 35 mol % or less, more preferably 10 mol % to 35 mol %, even more preferably 20 mol % to 35 mol %, and particularly preferably 30 mol % to 35 mol %, based on the total amount of all constituent repeating units. The content of the repeating unit (3) is preferably 35 mol % or less, more preferably 10 mol % to 35 mol %, still more preferably 20 mol % to 35 mol %, and particularly preferably 30 mol % to 35 mol %, based on the total amount of all constituent repeating units. The greater the content of the repeating unit (1), the more likely it is that the heat resistance, strength and rigidity will improve. However, if the content is too high, the solubility in solvents will tend to decrease.
[0031] The ratio of the content of the repeating unit (2) to the content of the repeating unit (3), expressed as [content of the repeating unit (2)] / [content of the repeating unit (3)] (mol / mol), is preferably 0.9 / 1 to 1 / 0.9, more preferably 0.95 / 1 to 1 / 0.95, and even more preferably 0.98 / 1 to 1 / 0.98.
[0032] The liquid crystal polymer may have two or more kinds of repeating units (1) to (3) independently. The liquid crystal polymer may have a constituent repeating unit other than the repeating units (1) to (3), but the content of such a repeating unit is preferably 10 mol % or less, more preferably 5 mol % or less, based on the total amount of all repeating units.
[0033] The liquid crystal polymer preferably has, as the repeating unit (3), at least one of X and Y being an imino group, i.e., at least one of a constituent repeating unit derived from a specific aromatic hydroxylamine and a constituent repeating unit derived from an aromatic diamine, since this has excellent solubility in a solvent, and more preferably has, as the repeating unit (3), only those in which at least one of X and Y is an imino group.
[0034] The liquid crystal polymer is preferably produced by melt-polymerizing the raw material monomers corresponding to the repeating units constituting the polymer. The melt-polymerization may be carried out in the presence of a catalyst, and examples of the catalyst include metal compounds such as magnesium acetate, stannous acetate, tetrabutyl titanate, lead acetate, sodium acetate, potassium acetate, and antimony trioxide, and nitrogen-containing heterocyclic compounds such as 4-(dimethylamino)pyridine and 1-methylimidazole, and nitrogen-containing heterocyclic compounds are preferably used. The melt-polymerization may be further carried out as necessary by solid-phase polymerization.
[0035] The liquid crystal polymer has a flow initiation temperature of preferably 250° C. or higher, more preferably 250° C. or higher and 350° C. or lower, and further preferably 260° C. or higher and 330° C. or lower. When the flow initiation temperature of the liquid crystal polymer is within the above range, the liquid crystal polymer has excellent solubility, heat resistance, strength and rigidity, and the viscosity of the solution is appropriate.
[0036] The flow initiation temperature is also called the flow temperature or flow temperature, and is measured using a capillary rheometer at 9.8 MPa (100 kg / cm 2When a liquid crystal polymer is melted and extruded from a nozzle with an inner diameter of 1 mm and a length of 10 mm while heating at a rate of 4°C / min under a load of 100 g / mol / L, the temperature at which the polymer shows a viscosity of 4,800 Pa s (48,000 poise) is reached, and this temperature is an indication of the molecular weight of the liquid crystal polymer (see "Liquid Crystal Polymer - Synthesis, Molding, Applications" edited by Koide Naoyuki, CMC Corporation, June 5, 1987, p. 95).
[0037] The liquid crystal polymer preferably has a melting point Tm of 280° C. or higher, more preferably 290° C. or higher and 350° C. or lower, and further preferably 300° C. or higher and 330° C. or lower. When the melting point Tm of the liquid crystal polymer is within the above range, the liquid crystal polymer has excellent solubility, heat resistance, strength and rigidity, and has an appropriate viscosity of the solution.
[0038] The liquid crystal polymer preferably has a weight average molecular weight of 1,000,000 or less, more preferably 3,000 to 300,000, even more preferably 5,000 to 100,000, and particularly preferably 5,000 to 30,000. When the weight average molecular weight of the liquid crystal polymer is within the above range, the film after heat treatment has excellent thermal conductivity in the thickness direction, heat resistance, strength, and rigidity.
[0039] Moreover, the liquid crystal polymer is preferably a solvent-soluble polymer (hereinafter, also referred to as a "soluble polymer"). Specifically, the soluble polymer in the present disclosure is a polymer that dissolves in an amount of 0.1 g or more at 25° C. in 100 g of at least one solvent selected from the group consisting of N-methylpyrrolidone, N-ethylpyrrolidone, dichloromethane, dichloroethane, chloroform, N,N-dimethylacetamide, γ-butyrolactone, dimethylformamide, ethylene glycol monobutyl ether, and ethylene glycol monoethyl ether.
[0040] The liquid crystal polymer film according to the present disclosure may contain only one type of liquid crystal polymer, or may contain two or more types of liquid crystal polymers. From the viewpoints of the dielectric tangent of the liquid crystal polymer film and adhesion to the metal foil, the content of the liquid crystal polymer is preferably 20% by mass to 99% by mass, more preferably 30% by mass to 98% by mass, even more preferably 40% by mass to 97% by mass, and particularly preferably 50% by mass to 95% by mass, relative to the total mass of the liquid crystal polymer film.
[0041] The liquid crystal polymer film according to the present disclosure preferably contains a filler.
[0042] -Filler- The filler may be particulate or fibrous, and may be an inorganic filler or an organic filler.
[0043] In the liquid crystal polymer film according to the present disclosure, the number density of the filler is preferably greater in the interior than on the surface from the viewpoint of adhesion.
[0044] As the inorganic filler, a known inorganic filler can be used. Examples of the inorganic filler material include BN, Al2O3, AlN, TiO2, SiO2, barium titanate, strontium titanate, aluminum hydroxide, calcium carbonate, and materials containing two or more of these. Among these, as the inorganic filler, from the viewpoints of thermal expansion coefficient and adhesion to the metal foil, metal oxide particles or fibers are preferred, silica particles, titania particles, or glass fibers are more preferred, and silica particles or glass fibers are particularly preferred. From the viewpoints of thermal expansion coefficient and adhesion to the metal foil, the average particle size of the inorganic filler is preferably 5 nm to 20 μm, more preferably 10 nm to 10 μm, further preferably 20 nm to 1 μm, and particularly preferably 25 nm to 500 nm. In the case where the particles or fibers are flat, the average particle size indicates the length in the short side direction.
[0045] As the organic filler, a known organic filler can be used. Examples of the organic filler material include polyethylene, polystyrene, urea-formalin filler, polyester, cellulose, acrylic resin, fluororesin, hardened epoxy resin, crosslinked benzoguanamine resin, crosslinked acrylic resin, and materials containing two or more of these. The organic filler may be in the form of fibers such as nanofibers, or may be in the form of hollow resin particles. Among these, from the viewpoints of thermal expansion coefficient and adhesion to the metal foil, the organic filler is preferably fluororesin particles, or nanofibers of polyester-based resin or cellulose-based resin, and more preferably polytetrafluoroethylene particles. From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the average particle size of the organic filler is preferably 5 nm to 20 μm, more preferably 10 nm to 1 μm, further preferably 20 nm to 500 nm, and particularly preferably 25 nm to 90 nm.
[0046] The liquid crystal polymer film according to the present disclosure may have a single layer structure or a multilayer structure. When the film has a single layer structure, a preferable embodiment is one in which the composition changes from the inside to the surface, and the elastic modulus changes.
[0047] The liquid crystal polymer film according to the present disclosure preferably has a layer A and a layer B provided on at least one surface of the layer A. The surface roughness Rz of the surface of the layer B is preferably 10 nm to 5000 nm, more preferably 20 nm to 1000 nm, and further preferably 50 nm to 500 nm.
[0048] From the viewpoint of adhesion, Layer B is preferably a surface layer (outermost layer).
[0049] <Layer A> Layer A preferably contains a liquid crystal polymer. Layer A may contain only one type of liquid crystal polymer, or may contain two or more types of liquid crystal polymer. From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the content of the liquid crystal polymer in Layer A is preferably 20 volume % to 100 volume %, more preferably 20 volume % to 90 volume %, even more preferably 30 volume % to 80 volume %, and particularly preferably 40 volume % to 70 volume %, relative to the total volume of Layer A.
[0050] Layer A may contain a filler. When Layer A contains a filler, Layer A may contain only one type of filler, or may contain two or more types of fillers.
[0051] From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the content of the filler in Layer A is preferably 5 volume % to 80 volume %, more preferably 10 volume % to 70 volume %, even more preferably 20 volume % to 70 volume %, and particularly preferably 30 volume % to 60 volume %, relative to the total volume of Layer A.
[0052] The layer A may contain additives other than the liquid crystal polymer and the filler. As the other additives, known additives can be used, specifically, for example, a leveling agent, a defoaming agent, an antioxidant, an ultraviolet absorbing agent, a flame retardant, a colorant, etc.
[0053] Furthermore, the layer A may contain, as other additives, resins other than the liquid crystal polymer. Examples of resins other than liquid crystal polymers include thermoplastic resins other than liquid crystal polyesters, such as polypropylene, polyamide, polyesters other than liquid crystal polyesters, polyphenylene sulfide, polyether ketone, polycarbonate, polyether sulfone, polyphenylene ether and modified products thereof, and polyether imide; elastomers such as copolymers of glycidyl methacrylate and polyethylene; and thermosetting resins such as phenol resins, epoxy resins, polyimide resins, and cyanate resins.
[0054] The total content of other additives in Layer A is preferably 25 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, based on 100 parts by mass of the liquid crystal polymer.
[0055] The average thickness of Layer A is not particularly limited, but from the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, it is preferably 5 μm to 90 μm, more preferably 10 μm to 70 μm, and particularly preferably 15 μm to 50 μm.
[0056] The method for measuring the average thickness of each layer in the liquid crystal polymer film according to the present disclosure is as follows. The liquid crystal polymer film is cut with a microtome, and the cross section is observed with an optical microscope to evaluate the thickness of each layer. Cross-sectional samples are cut out in three or more places, and the thickness is measured at three or more points on each cross section, and the average value of these is taken as the average thickness.
[0057] From the viewpoint of adhesion, the dielectric tangent of Layer A is preferably 0.02 or less, more preferably 0.01 or less, further preferably 0.005 or less, and particularly preferably more than 0 and 0.003 or less.
[0058] <Layer B> Layer B preferably comprises a liquid crystal polymer. A preferred embodiment of the liquid crystal polymer used in Layer B is the same as that used in Layer A, except as described below. The liquid crystal polymer contained in Layer B may be the same as the liquid crystal polymer contained in Layer A or may be different.
[0059] The content of the liquid crystal polymer in Layer B is preferably greater than the content of the liquid crystal polymer in Layer A from the viewpoints of the thermal expansion coefficient and the adhesion to the metal foil. From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the content of the liquid crystal polymer in Layer B is preferably 50 volume% to 100 volume%, more preferably 80 volume% to 100 volume%, even more preferably 90 volume% to 100 volume%, and particularly preferably 95 volume% to 100 volume%, relative to the total volume of Layer B.
[0060] Layer B preferably contains a filler. When Layer B contains a filler, Layer B may contain only one type of filler, or may contain two or more types of fillers.
[0061] From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the content of the filler in Layer B is preferably 5 volume % to 80 volume %, more preferably 10 volume % to 70 volume %, even more preferably 20 volume % to 70 volume %, and particularly preferably 30 volume % to 60 volume %, relative to the total volume of Layer B.
[0062] Layer B may contain other additives in addition to the liquid crystal polymer and the filler. The preferred embodiments of the other additives used in the layer B are the same as the preferred embodiments of the other additives used in the layer A.
[0063] The average thickness of Layer B is preferably smaller than the average thickness of Layer A from the viewpoints of the thermal expansion coefficient and adhesion to the metal foil. Average thickness T of layer A A and the average thickness T of layer B B The ratio of T A / T B From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the value of is preferably greater than 1, more preferably 2 to 100, further preferably 2.5 to 20, and particularly preferably 3 to 10. From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the average thickness of Layer B is preferably 0.1 μm to 20 μm, more preferably 0.5 μm to 15 μm, even more preferably 1 μm to 10 μm, and particularly preferably 3 μm to 8 μm.
[0064] From the viewpoint of adhesion, the dielectric tangent of Layer B is preferably 0.02 or less, more preferably 0.01 or less, further preferably 0.005 or less, and particularly preferably more than 0 and 0.003 or less.
[0065] From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the liquid crystal polymer film according to the present disclosure preferably further comprises a layer C in addition to the layer A and the layer B, and more preferably comprises the layer B, the layer A, and the layer C in this order. The surface roughness Rz of the surface of the layer C is preferably 10 nm to 5000 nm, more preferably 20 nm to 1000 nm, and even more preferably 50 nm to 500 nm.
[0066] <Layer C> Layer C is preferably a surface layer (outermost layer). From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the layer C preferably contains a liquid crystal polymer. A preferred embodiment of the liquid crystal polymer used in the layer C is the same as that of the liquid crystal polymer used in the layer A, except as described below. The liquid crystal polymer contained in layer C may be the same as or different from the liquid crystal polymer contained in layer A or layer B, but is preferably the same as the liquid crystal polymer contained in layers A and B.
[0067] The content of the liquid crystal polymer in Layer C is preferably greater than the content of the liquid crystal polymer in Layer A from the viewpoints of the thermal expansion coefficient and the adhesion to the metal foil. From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the content of the liquid crystal polymer in Layer C is preferably 50 volume% to 100 volume%, more preferably 80 volume% to 100 volume%, even more preferably 90 volume% to 100 volume%, and particularly preferably 95 volume% to 100 volume%, relative to the total volume of Layer C.
[0068] The layer C may contain a filler. Preferred embodiments of the filler used in Layer C are the same as those of the filler used in Layer A, except as described below.
[0069] The filler content in Layer C is preferably smaller than the filler content in Layer A from the viewpoints of the thermal expansion coefficient and adhesion to the metal foil. From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the content of the filler in Layer C is preferably either zero or more than 0 volume % and not more than 20 volume % relative to the total volume of Layer C, more preferably zero or more than 0 volume % and not more than 10 volume % relative to the total volume of Layer C, even more preferably zero or more than 0 volume % and not more than 5 volume % relative to the total volume of Layer C, and particularly preferably zero or no filler.
[0070] The layer C may contain additives other than the liquid crystal polymer and the filler. The preferred embodiments of the other additives used in the layer C are the same as the preferred embodiments of the other additives used in the layer A.
[0071] The average thickness of Layer C is preferably smaller than the average thickness of Layer A from the viewpoints of the thermal expansion coefficient and adhesion to the metal foil. Average thickness T of layer A A and the average thickness T of layer C C T A / T C From the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the value of is preferably greater than 1, more preferably 2 to 100, further preferably 2.5 to 20, and particularly preferably 3 to 10. Also, the average thickness T of layer C C and the average thickness T of layer B B T C / T B From the viewpoints of the thermal expansion coefficient and the adhesion to the metal foil, the value of is preferably from 0.2 to 5, more preferably from 0.5 to 2, and particularly preferably from 0.8 to 1.2. Furthermore, from the viewpoints of the thermal expansion coefficient and adhesion to the metal foil, the average thickness of Layer C is preferably 0.1 μm to 20 μm, more preferably 0.5 μm to 15 μm, even more preferably 1 μm to 10 μm, and particularly preferably 3 μm to 8 μm.
[0072] From the viewpoint of adhesion, the dielectric tangent of Layer C is preferably 0.02 or less, more preferably 0.01 or less, further preferably 0.005 or less, and particularly preferably more than 0 and 0.003 or less.
[0073] The average thickness of the liquid crystal polymer film according to the present disclosure is preferably 6 μm to 500 μm, more preferably 6 μm to 100 μm, and particularly preferably 12 μm to 100 μm, from the viewpoints of strength and electrical properties (characteristic impedance) when laminated with copper foil.
[0074] The average thickness of the liquid crystal polymer film is determined by measuring any five points using an adhesive film thickness meter, for example, an electronic micrometer (product name "KG3001A" manufactured by Anritsu Corporation), and averaging these values.
[0075] <Film manufacturing method> (Film forming) The method for producing the liquid crystal polymer film according to the present disclosure is not particularly limited, and known methods can be referred to. The method for producing the liquid crystal polymer film according to the present disclosure is preferably, for example, a casting method, a coating method, an extrusion method, etc. Among them, the casting method is particularly preferred for producing a relatively thin film, and the co-extrusion method is particularly preferred for producing a thick film. In addition, when the liquid crystal polymer film according to the present disclosure has a multi-layer structure, for example, a co-casting method, a multi-layer coating method, a co-extrusion method, etc. are preferably used. Among them, the co-casting method is particularly preferred. When a multilayer structure in a liquid crystal polymer film is produced by the co-casting method or the multi-layer coating method, it is preferable to carry out the co-casting method or the multi-layer coating method using a composition for forming layer A, a composition for forming layer B, a composition for forming layer C, etc., in which the components of each layer, such as a liquid crystal polymer, are dissolved or dispersed in a solvent.
[0076] Examples of the solvent include halogenated hydrocarbons such as dichloromethane, chloroform, 1,1-dichloroethane, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, 1-chlorobutane, chlorobenzene, and o-dichlorobenzene; halogenated phenols such as p-chlorophenol, pentachlorophenol, and pentafluorophenol; ethers such as diethyl ether, tetrahydrofuran, and 1,4-dioxane; ketones such as acetone and cyclohexanone; esters such as ethyl acetate and γ-butyrolactone; and ethylene carbonate. Examples of the organic solvent include carbonates such as propylene carbonate and propylene carbonate; amines such as triethylamine; nitrogen-containing heterocyclic aromatic compounds such as pyridine; nitriles such as acetonitrile and succinonitrile; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and urea compounds such as tetramethylurea; nitro compounds such as nitromethane and nitrobenzene; sulfur compounds such as dimethyl sulfoxide and sulfolane; and phosphorus compounds such as hexamethylphosphoramide and tri-n-butylphosphoric acid, and two or more of these may be used.
[0077] As the solvent, since it is less corrosive and easy to handle, a solvent mainly composed of an aprotic compound, particularly an aprotic compound having no halogen atom, is preferred, and the ratio of the aprotic compound to the entire solvent is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. In addition, as the aprotic compound, since it is easy to dissolve the liquid crystal polymer, it is preferred to use amides such as N,N-dimethylformamide, N,N-dimethylacetamide, tetramethylurea, and N-methylpyrrolidone, or esters such as γ-butyrolactone, and N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone are more preferred.
[0078] In addition, the solvent is preferably a solvent mainly composed of a compound having a dipole moment of 3 to 5, since it is easy to dissolve the liquid crystal polymer. The proportion of the compounds 3 to 5 is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. As the aprotic compound, a compound having a dipole moment of 3 to 5 is preferably used.
[0079] Furthermore, as the solvent, a solvent mainly composed of a compound having a boiling point of 220° C. or lower at 1 atmospheric pressure is preferred because it is easy to remove, and the proportion of the compound having a boiling point of 220° C. or lower at 1 atmospheric pressure in the entire solvent is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. As the aprotic compound, it is preferable to use a compound having a boiling point of 220° C. or lower at 1 atmospheric pressure.
[0080] In the method for producing a liquid crystal polymer film according to the present disclosure, a support may be used when the film is produced by the co-casting method, multi-layer coating method, co-extrusion method, or the like. Examples of the support include a metal drum, a metal band, a glass plate, a resin film, and a metal foil. Among these, a metal drum, a metal band, and a resin film are preferred. Examples of resin films include polyimide (PI) films, and examples of commercially available products include U-Pirex S and U-Pirex R manufactured by Ube Industries, Ltd., Kapton manufactured by DuPont-Toray Co., Ltd., and IF30, IF70, and LV300 manufactured by SKC Kolon PI. The support may have a surface treatment layer formed on its surface so that it can be easily peeled off. The surface treatment layer may be made of hard chrome plating, fluororesin, or the like. The average thickness of the resin film support is not particularly limited, but is preferably from 25 to 75 μm, and more preferably from 50 to 75 μm.
[0081] The method for removing at least a part of the solvent from the cast or coated film-like composition (cast film or coating film) is not particularly limited, and a known drying method can be used.
[0082] As described above, methods for forming a liquid crystal polymer film having a surface roughness Rz of 10 nm to 5000 nm include a method of generating Benard cells during film formation, a method of using a solution containing a filler and a liquid crystal polymer, a method of phase-separating a material mixed with a liquid crystal polymer during film formation, a method of forming a skin on the surface during film formation and using the difference in shrinkage between the inside and the inside (reticulation), a method of performing a replica process using a mold with a surface unevenness during solution film formation, and a method of roughening the film after film formation by surface treatment such as sputtering. In the method of generating Benard cells during film formation, it is preferable to use a liquid crystal polymer solution that has low viscosity on the air interface side and high surface energy. In the method of phase separation, it is also effective to adjust the drying speed or drying temperature to pass the film at a film surface temperature and solid content concentration that are phase-separable, and to apply drying air that has the effect of inducing phase separation, such as high humidity air. In addition, when using reticulation, it is preferable to apply strong drying air immediately after casting the liquid crystal polymer solution on the support to form a skin on the surface.
[0083] (Stretching) The liquid crystal polymer film according to the present disclosure can be appropriately combined with stretching in terms of controlling molecular orientation and adjusting the thermal expansion coefficient and mechanical properties. The stretching method is not particularly limited, and known methods can be referred to. It may be performed in a state containing a solvent or in a dry film state. Stretching in a state containing a solvent may be performed by gripping the film and stretching it, or it may be performed by utilizing autogenous shrinkage due to drying without stretching it. Stretching is particularly effective for the purpose of improving the breaking elongation and breaking strength when the brittleness of the film is reduced by adding an inorganic filler or the like.
[0084] <Application> The liquid crystal polymer film according to the present disclosure can be used for various applications, and among them, it can be suitably used as a film for electronic components such as a printed wiring board, and can be even more suitably used for a flexible printed circuit board. Moreover, the liquid crystal polymer film according to the present disclosure can be suitably used as a liquid crystal polymer film for metal bonding.
[0085] (Laminate) The laminate according to the present disclosure may be any laminate in which the liquid crystal polymer film according to the present disclosure is laminated. The laminate according to the present disclosure preferably has the liquid crystal polymer film according to the present disclosure and a metal layer disposed on the surface of the liquid crystal polymer film on the Layer B side, and more preferably the metal layer is a copper layer.
[0086] In addition, the laminate according to the present disclosure preferably comprises a liquid crystal polymer film according to the present disclosure having a layer B, a layer A, and a layer C in this order, a metal layer disposed on the surface of the liquid crystal polymer film facing the layer B, and a metal layer disposed on the surface of the liquid crystal polymer film facing the layer C, and it is more preferable that both of the metal layers are copper layers.
[0087] In addition, the metal layer disposed on the surface on the layer B side and the metal layer disposed on the surface on the layer C side may be metal layers of the same material, thickness and shape, or metal layers of different material, thickness and shape. From the viewpoint of characteristic impedance adjustment, the metal layer disposed on the surface on the layer B side and the metal layer disposed on the surface on the layer C side may be metal layers of different material and thickness, and a metal layer may be laminated on only one of the layers B and C. Furthermore, from the viewpoint of adjusting the characteristic impedance, a preferred embodiment is one in which a metal layer is laminated on one side of layer B or layer C, and another film (preferably another liquid crystal polymer film) is laminated on the other side.
[0088] The peel strength between Layer B and the copper layer is preferably 0.5 kN / m or more, more preferably 0.7 kN / m or more, even more preferably 0.7 kN / m to 2.0 kN / m, and particularly preferably 0.9 kN / m to 1.5 kN / m. Furthermore, the peel strength between the layer C and the copper layer is preferably 0.5 kN / m or more, more preferably 0.7 kN / m or more, even more preferably 0.7 kN / m to 2.0 kN / m, and particularly preferably 0.9 kN / m to 1.5 kN / m.
[0089] In the present disclosure, the peel strength between Layer B or Layer C of the liquid crystal polymer film and a metal layer (eg, a copper layer) is measured by the following method. A 1.0 cm wide peel test piece is prepared from a laminate of a liquid crystal polymer film and a metal layer, and the liquid crystal polymer film is fixed to a flat plate with double-sided adhesive tape. The strength (kN / m) is measured when the metal layer is peeled from the liquid crystal polymer film at a speed of 50 mm / min using the 180° method in accordance with JIS C 5016 (1994).
[0090] The metal layer is preferably a copper layer. The copper layer is preferably a rolled copper foil formed by a rolling method or an electrolytic copper foil formed by an electrolytic method, and more preferably a rolled copper foil from the viewpoint of flex resistance.
[0091] The average thickness of the metal layer, preferably the copper layer, is not particularly limited, but is preferably 2 μm to 20 μm, more preferably 3 μm to 18 μm, and even more preferably 5 μm to 12 μm. The copper foil may be a carrier-attached copper foil formed on a support (carrier) in a peelable manner. As the carrier, a known carrier can be used. The average thickness of the carrier is not particularly limited, but is preferably 10 μm to 100 μm, and more preferably 18 μm to 50 μm.
[0092] The thickness of layer B is preferably greater than the thickness of the metal layer (eg, copper layer).
[0093] The metal layer in the laminate according to the present disclosure may be a metal layer having a circuit pattern. It is also preferable to process the metal layer in the laminate according to the present disclosure into a desired circuit pattern by, for example, etching, to form a flexible printed circuit board. The etching method is not particularly limited, and any known etching method can be used. EXAMPLES
[0094] The present disclosure will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the present disclosure is not limited to the specific examples shown below.
[0095] <<Measurement method>> [Dissipation factor] The dielectric loss tangent was measured at a frequency of 10 GHz by the resonance perturbation method. A 10 GHz cavity resonator (Kanto Electronics Application Development Co., Ltd. CP531) was connected to a network analyzer (Agilent Technology "E8363B"), and a film sample (width: 2.0 mm x length: 80 mm) was inserted into the cavity resonator. The dielectric loss tangent of the liquid crystal polymer film was measured from the change in resonance frequency before and after insertion for 96 hours in an environment with a temperature of 25°C and a humidity of 60%.
[0096] [Surface roughness Rz] A non-contact surface / layer cross-sectional shape measurement system, VertScan (manufactured by Ryoka Systems Co., Ltd.), was used to measure an area 465.48 μm long and 620.64 μm wide, and a roughness curve and the average line of the roughness curve were created for the surface of the object to be measured (liquid crystal polymer film). A portion corresponding to the reference length was extracted from the roughness curve. The surface roughness Rz of the object to be measured was measured by calculating the sum of the maximum peak height (i.e., the height from the average line to the peak) and the maximum valley depth (i.e., the height from the average line to the valley bottom) observed in the extracted roughness curve.
[0097] [Peel strength] A 10 mm wide peel test piece was prepared from a double-sided copper-clad laminate of liquid crystal polymer film and copper foil, one of the copper foils was fixed to a flat plate with double-sided adhesive tape, and the adhesive surfaces of the liquid crystal polymer films were peeled off at a speed of 50 mm / min using the 180° method in accordance with JIS C 5016 (1994), and the strength (kN / m) was measured.
[0098] <<Production Example>> <Liquid crystal polymer> LC-A: Liquid crystal polymer prepared according to the following manufacturing method
[0099] -Production of LC-A- Into a reactor equipped with a stirrer, a torque meter, a nitrogen gas inlet tube, a thermometer, and a reflux condenser, 940.9 g (5.0 mol) of 6-hydroxy-2-naphthoic acid, 377.9 g (2.5 mol) of 4-hydroxyacetaminophen, 415.3 g (2.5 mol) of isophthalic acid, and 867.8 g (8.4 mol) of acetic anhydride were placed, and the gas in the reactor was replaced with nitrogen gas. After that, the mixture was heated from room temperature (23°C) to 140°C over 60 minutes while stirring under a nitrogen gas stream, and refluxed at 140°C for 3 hours. Next, while distilling off by-product acetic acid and unreacted acetic anhydride, the temperature was raised from 150°C to 300°C over 5 hours, and after holding at 300°C for 30 minutes, the contents were removed from the reactor and cooled to room temperature. The obtained solid was pulverized with a pulverizer to obtain a powdered liquid crystal polyester (B1). The flow-start temperature of this liquid crystal polyester (B1) was 193.3°C.
[0100] The liquid crystal polyester (B1) obtained above was heated from room temperature to 160°C over 2 hours and 20 minutes in a nitrogen atmosphere, then heated from 160°C to 180°C over 3 hours and 20 minutes, and held at 180°C for 5 hours to perform solid-phase polymerization, then cooled and pulverized in a pulverizer to obtain a powdered liquid crystal polyester (B2). The flow-start temperature of this liquid crystal polyester (B2) was 220°C.
[0101] The liquid crystal polyester (B2) obtained above was heated in a nitrogen atmosphere from room temperature (23°C) to 180°C over 1 hour 25 minutes, then heated from 180°C to 255°C over 6 hours 40 minutes, and held at 255°C for 5 hours to perform solid-phase polymerization, and then cooled to obtain a powdered liquid crystal polyester (B) (LC-A). The flow-start temperature of the liquid crystal polyester (B) was 302°C. The melting point of this liquid crystal polyester (B) was measured using a differential scanning calorimeter, and was found to be 311°C.
[0102] <Filler> A-1: Spiny silica sol (average particle size 36 nm) produced according to the following manufacturing method
[0103] -How to make confetti-like silica sol- Water was added to 102.4 g of silica sol (Catalysts and Chemical Industries Co., Ltd.: Cataloid SI-40, average particle size 21.2 nm, SiO2 concentration 40.7% by mass) to make 4,170 g (SiO2 concentration 1% by mass), and a 5% by mass aqueous sodium hydroxide solution was added to adjust the pH of the silica sol to 11. Next, the temperature of the silica sol was raised to 80°C and maintained at 80°C for 30 minutes to obtain a core particle dispersion liquid (liquid A).
[0104] 575 g of water glass (manufactured by AGC Si-Tech Co., Ltd.: JIS No. 3 water glass, SiO2 concentration 24% by mass) was diluted with 2,185 g of water to prepare 2,760 g of an aqueous alkali silicate solution (liquid B). 2,450 g of an aqueous electrolyte solution was prepared by adding 2,352 g of water to 98.0 g of ammonium sulfate (manufactured by Mitsubishi Chemical Co., Ltd.) as an electrolyte. Then, the entire amount of the aqueous alkali silicate solution (liquid B) and the aqueous electrolyte solution were each added at 80°C over one hour to the entire amount of the core particle dispersion liquid (liquid A) maintained at a temperature of 80°C, thereby causing particle growth. Next, after aging at 80°C for 1 hour, the core particle dispersion liquid in which particles had grown was washed with an ultrafiltration membrane until the pH reached 10.8. Next, the dispersion was concentrated to a SiO2 concentration of 20 mass%, and the solvent was replaced with N-methylpyrrolidone to obtain a spinous silica sol.
[0105] <Film forming> The methods shown in Table 1 were selected from the following multilayer coating and co-casting methods.
[0106] [Multilayer Coating] -Preparation of polymer solution- The liquid crystal polymer was added to N-methylpyrrolidone and stirred for 4 hours at 140° C. under a nitrogen atmosphere to obtain a liquid crystal polymer solution. The liquid crystal polymer and additives were added in the volume ratios shown in Table 1, and the solid content concentration was 10 mass % for the solution for Layer A and 5 mass % for the solution for Layer B. Subsequently, the mixture was first passed through a sintered fiber metal filter having a nominal pore size of 5 μm, and then passed through a sintered fiber filter also having a nominal pore size of 5 μm to obtain each polymer solution.
[0107] -Film production- The obtained polymer solutions for Layer A and Layer B were fed to a slot die coater equipped with a slide coater, and applied to the treated surface of a copper foil (12μm, CF-T4X-SV-12, manufactured by Fukuda Metal Foil and Powder Co., Ltd.) so that the Layer A side of the two-layer structure (Layer B / Layer A) was in contact. The solvent was removed from the casting film by drying at 140°C for 30 minutes, and a liquid crystal polymer film (laminate) having a copper layer was obtained. The surface roughness Rz of the surface opposite to the copper layer of the obtained laminate was measured. The surface roughness Rz was the value shown in Table 1.
[0108] [Co-casting 1 (solution casting)] -Preparation of polymer solution- The liquid crystal polymer was added to N-methylpyrrolidone and stirred for 4 hours at 140°C under a nitrogen atmosphere to obtain a liquid crystal polymer solution. The liquid crystal polymer and additives were added at the volume ratios shown in Table 1, and the solid content concentration was 23 mass% for the solution for layer A (core layer), and 20 mass% for the solution for layer B (surface layer). Subsequently, the mixture was first passed through a sintered fiber metal filter having a nominal pore size of 10 μm, and then through a sintered fiber filter also having a pore size of 10 μm to obtain a polymer solution.
[0109] -Film production- The obtained polymer solutions for layer A and layer B were sent to a casting die equipped with a feed block adjusted for co-casting, and cast onto the treated surface of a copper foil (12 μm, CF-T4X-SV-12, manufactured by Fukuda Metal Foil and Powder Co., Ltd.) so that the layer A side was in contact with the treated surface. The solvent was removed from the cast film by drying at 140° C. for 30 minutes, and a liquid crystal polymer film (laminate) having a copper layer was obtained. The surface roughness Rz of the surface opposite to the copper layer of the obtained laminate was measured. The surface roughness Rz was the value shown in Table 1.
[0110] [Co-casting 2 (solution casting)] In the preparation of the film of co-casting 1, the casting film was pressed against an embossing roll (diameter 350 mm, roll surface was blasted to form 0.5 μm high unevenness) equipped with a backup roll when the residual solvent amount in the casting film was 50 mass %. The same procedure as co-casting 1 was carried out to obtain a liquid crystal polymer film (laminate) having a copper layer. The surface roughness Rz of the surface opposite to the copper layer of the obtained laminate was measured. The surface roughness Rz was the value shown in Table 1.
[0111] <Preparation of double-sided copper-clad laminate 1> (Copper-clad laminate precursor process) A pair of liquid crystal polymer films (laminates) having the above-mentioned copper layer were prepared, placed so that the liquid crystal polymer films were in contact with each other, and laminated for 1 minute using a laminator (Nikko Materials Co., Ltd.'s "Vacuum Laminator V-130") at 140°C and a lamination pressure of 0.4 MPa to obtain a copper foil laminate precursor.
[0112] (Main thermocompression bonding process) The obtained copper-clad laminate precursor was subjected to thermocompression bonding for 10 minutes under conditions of 300° C. and 4.5 MPa using a thermocompression bonding machine (Toyo Seiki Seisakusho, “MP-SNL”) to produce a double-sided copper-clad laminate.
[0113] <Preparation of double-sided copper-clad laminate 2> A separately prepared copper foil (CF-T4X-SV-12 12μm, manufactured by Fukuda Metal Foil and Powder Co., Ltd.) was placed on the liquid crystal polymer film (laminate) having the copper layer so that the treated side of the copper foil was in contact with the liquid crystal polymer film, and a lamination process was performed for 1 minute using a laminator ("Vacuum Laminator V-130" manufactured by Nikko Materials Co., Ltd.) at 140°C and a lamination pressure of 0.4MPa. Subsequently, a double-sided copper-clad laminate was produced by thermocompression bonding the obtained copper-clad laminate precursor at 300°C and 4.5MPa for 10 minutes using a thermocompression bonding machine ("MP-SNL" manufactured by Toyo Seiki Seisakusho Co., Ltd.). The produced double-sided copper-clad laminate had excellent adhesion between layers and was free of air bubbles or other inclusions.
[0114] The double-sided copper-clad laminate prepared in the above "Preparation of double-sided copper-clad laminate 1" was used to evaluate the peel strength. The higher the peel strength, the better the adhesion. The evaluation results are shown in Table 1.
[0115] [Table 1]
[0116] As shown in Table 1, in Examples 1 to 3, since the liquid crystal polymer was included and at least one surface had a surface roughness Rz of 10 nm to 5000 nm, it was found that the peel strength was large and the adhesion was excellent.
[0117] On the other hand, in Comparative Example 1, since the surface roughness Rz was 5 nm, it was found that the peel strength was small and the adhesion was poor.
Claims
1. A film having a layer A and a layer B provided on at least one surface of the layer A, The layer A and the layer B each contain a liquid crystal polymer, the surface roughness Rz of the surface of the layer B is 10 nm to 5000 nm; A liquid crystal polymer film having an average thickness of 6 μm to 100 μm.
2. 2. The liquid crystal polymer film according to claim 1, wherein the surface roughness Rz of both surfaces is from 10 nm to 5000 nm.
3. 3. The liquid crystal polymer film according to claim 1, wherein the liquid crystal polymer has a melting point Tm of 280° C. or higher.
4. 4. The liquid crystal polymer film according to claim 1, having a linear expansion coefficient of -20 ppm / K to 50 ppm / K.
5. 5. The liquid crystal polymer film according to claim 1, having a dielectric loss tangent of 0.01 or less.
6. The liquid crystal polymer film according to any one of claims 1 to 5, further comprising a filler.
7. 7. The liquid crystal polymer film according to claim 6, wherein the number density of the filler is greater inside than on the surface having the surface roughness Rz of 10 nm to 5000 nm.
8. 8. The liquid crystal polymer film according to claim 1, wherein the liquid crystal polymer has a constitutional repeating unit represented by any one of formulas (1) to (3). Formula (1) -O-Ar 1 -CO- Formula (2) -CO-Ar 2 -CO- Formula (3) -X-Ar 3 -Y- In formulas (1) to (3), Ar 1 represents a phenylene group, a naphthylene group, or a biphenylylene group; Ar 2 and Ar 3 each independently represents a phenylene group, a naphthylene group, a biphenylylene group, or a group represented by the following formula (4), each of X and Y independently represents an oxygen atom or an imino group, Ar 1 ~Ar 3 Each hydrogen atom in the group represented by the formula: may be independently substituted with a halogen atom, an alkyl group or an aryl group. Formula (4) -Ar 4 -Z-Ar 5 -[[]]END]] In formula (4), Ar 4 and Ar 5 each independently represents a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylene group.
9. Further comprising a layer C, The layer B, the layer A, and the layer C in this order, The liquid crystal polymer film according to any one of claims 1 to 8, wherein the surface roughness Rz of the surface of the layer C is 10 nm to 5000 nm.
10. A liquid crystal polymer film according to any one of claims 1 to 9, a copper layer disposed on the liquid crystal polymer film on the side of the layer B; A laminate having the following structure:
11. The laminate of claim 10 , wherein the thickness of the layer B is greater than the thickness of the copper layer.
12. 12. The laminate according to claim 10 or 11, wherein a peel strength between the layer B and the copper layer is 0.5 kN / m or more.
13. A laminate comprising the liquid crystal polymer film according to claim 9, a copper layer disposed on the surface of the liquid crystal polymer film on the layer B side, and a copper layer disposed on the surface of the liquid crystal polymer film on the layer C side.
14. The laminate according to claim 13, wherein a peel strength between the layer C and the copper layer disposed on the surface on the layer C side is 0.5 kN / m or more.
Citation Information
Patent Citations
Film of heat-sealable co-extruded liquid crystal polymer
JP1993226796A
Liquid crystal polymer film and its laminate
JP1998034742A
Interlayer for laminated glass
JP2000203900A
Liquid crystal polyester film, liquid composition containing liquid crystal polyester and method for manufacturing liquid crystal polyester film