Cemented lens, optical system including same, optical device, and method for manufacturing cemented lens

The cemented lens design with an exposed adhesive layer and low refractive index layer addresses optical defects by ensuring complete film curing and reducing reflection, maintaining performance and functionality.

JP7575256B2Active Publication Date: 2024-10-29TAMRON CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020202240
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-04
Publication Date
2024-10-29
Estimated Expiration
2040-12-04

AI Technical Summary

Technical Problem

Cemented lenses experience optical defects due to low-temperature curing of light-shielding films, which lead to solvent infiltration, dye elution, insufficient adhesion, and moisture condensation, causing deterioration in optical performance.

Method used

A cemented lens design where the adhesive layer is exposed between light-shielding films, allowing low-temperature curing of the films without solvent infiltration, ensuring complete curing and preventing moisture condensation, and incorporating a low refractive index layer to reduce reflection.

Benefits of technology

Prevents optical defects by maintaining optical performance and functionality, resisting cleaning and environmental changes, and reducing reflection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575256000006
    Figure 0007575256000006
  • Figure 0007575256000007
    Figure 0007575256000007
  • Figure 0007575256000008
    Figure 0007575256000008
Patent Text Reader

Abstract

To provide a technique for preventing occurrence of optical defects of a cemented lens caused by a light shield film.SOLUTION: A cemented lens (50) according to an aspect of the present invention comprises a first optical element (10) provided with a first light shield film (12) and a second optical element (20) provided with a second light shield film (22) that are cemented together by a bonding layer (30). The bonding layer (30) is exposed from between the first light shield film (12) and the second light shield film (22).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cemented lens used in an imaging device such as a camera, an optical system including the cemented lens, an optical instrument, and a method for manufacturing the cemented lens. [Background technology]

[0002] In order to correct chromatic aberration, a cemented lens in which a plurality of glass lenses with different refractive indices are bonded together by an organic adhesive is widely used in imaging devices such as cameras. In addition, in order to reduce internal reflections that cause ghosts and flares, lenses used in imaging devices have a black, opaque light-shielding layer (ink coating film) formed on a non-optically effective area (edge ​​portion). In cemented lenses, a black coating film is also formed on the edge portion for the same purpose. For example, in the cemented lens disclosed in Patent Document 1, a solvent-free epoxy resin mixed with carbon black is applied to the outer peripheral end of the adhesive that is sandwiched and spread between a convex lens and a concave lens. In addition, Patent Document 2 discloses a cemented lens in which a first optical element and a second optical element are bonded together by a third optical element containing a resin, and the surface of the third optical element that is not in contact with the first and second optical elements is covered with a light-shielding film. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-108642 A [Patent Document 2] JP 2020-24331 A Summary of the Invention [Problem to be solved by the invention]

[0004] Generally, a light-shielding film (ink coating) needs to be thermally cured at high temperatures after application. On the other hand, in the case of cemented lenses, the bonding interface is prone to peeling due to the difference in linear expansion coefficient between the glass lens and the layer of bonding adhesive. For this reason, the light-shielding film applied to cemented lenses is thermally cured at a lower temperature than when the light-shielding film of a single lens is thermally cured. However, curing the light-shielding film at low temperatures has the following problems compared to curing at high temperatures:

[0005] First, low-temperature curing does not allow the solvent contained in the light-shielding film to evaporate sufficiently, which can cause the solvent to seep into the layer of adhesive that the light-shielding film is in contact with, resulting in deterioration (discoloration) and significant deterioration of the optical performance and functions of the cemented lens.

[0006] In addition, the light-shielding film is more difficult to harden in low-temperature curing than in high-temperature treatment. Therefore, when a cemented lens on which a light-shielding film is formed is washed with a cleaning solution such as isopropyl alcohol, the dye contained in the light-shielding film dissolves in the cleaning solution, causing a deterioration in the performance of the light-shielding film. In addition, since the hardening does not proceed as easily as in high-temperature treatment, the adhesion to the cemented lens is not sufficient, and the light-shielding film may peel off during ultrasonic cleaning or the like.

[0007] Furthermore, in a high-temperature, high-humidity environment, moisture absorbed in the layer of the resin-containing adhesive is released from the end not in contact with the lens. However, the light-shielding film formed on the end inhibits the release of moisture, and the moisture becomes supersaturated at the end, causing condensation to form at the interface between the layer of the adhesive and the lens, whitening the interface and degrading the optical performance.

[0008] One aspect of the present invention has been made in view of the above problems, and has an object to provide a technique for preventing optical defects in a cemented lens caused by a light-shielding film. [Means for solving the problem]

[0009] In order to solve the above-mentioned problems, a cemented lens according to one embodiment of the present invention is a cemented lens including: a first optical element having a first light-shielding film formed in a non-optically effective region of a substrate; a second optical element having a second light-shielding film formed in the non-optically effective region of the substrate; and an adhesive layer bonding the optically effective regions of the first optical element and the second optical element together, wherein the adhesive layer is exposed between the first light-shielding film and the second light-shielding film.

[0010] In order to solve the above-mentioned problems, an optical system according to one aspect of the present invention includes the above-mentioned cemented lens.

[0011] In order to achieve the above object, an optical device according to one aspect of the present invention includes the cemented lens and a light receiving element that receives light focused by the cemented lens.

[0012] According to the above-described configuration, it is possible to provide a technique for preventing the occurrence of optical defects in the cemented lens caused by the light-shielding film.

[0013] In order to solve the above-described problems, a manufacturing method for a cemented lens according to one aspect of the present invention includes a bonding step of bonding together, via an adhesive layer, optically effective areas of a first optical element having a non-optically effective area of ​​a substrate, a first light-shielding film formed on a non-optically effective area of ​​a substrate, and a second optical element having a non-optically effective area of ​​a substrate, a second light-shielding film formed on a non-optically effective area of ​​the substrate.

[0014] According to the above-described configuration, it is possible to provide a technique for preventing the occurrence of optical defects in the cemented lens caused by the light-shielding film. Effect of the Invention

[0015] According to one aspect of the present invention, it is possible to provide a technique for preventing the occurrence of optical defects in a cemented lens caused by a light-shielding film. [Brief description of the drawings]

[0016] [Figure 1] 1 is a cross-sectional view showing a configuration of a cemented lens according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view showing a configuration of a first optical element of the cemented lens shown in FIG. [Diagram 3] 2 is a cross-sectional view showing a configuration of a second optical element of the cemented lens shown in FIG. [Figure 4] FIG. 2 is a partial enlarged view of the area indicated by A in FIG. [Diagram 5] 1 is a cross-sectional view showing the configuration of a zoom lens as an optical system according to an embodiment of the present invention. [Figure 6] 1 is a diagram showing a configuration of an imaging apparatus as an optical device according to an embodiment of the present invention; [Figure 7] FIG. 3 is a partially enlarged view showing a modification of the embodiment shown in FIG. [Figure 8] FIG. 11 is a cross-sectional view showing a configuration of a cemented lens according to another embodiment of the present invention. [Figure 9] 9 is a cross-sectional view showing a configuration of a first optical element of the cemented lens shown in FIG. [Figure 10] 9 is a cross-sectional view showing a configuration of a second optical element of the cemented lens shown in FIG. [Figure 11] 9 is a cross-sectional view showing the configuration of a low refractive index layer of the cemented lens shown in FIG. [Figure 12] 9 is a graph showing the reflection reducing effect of the cemented lens shown in FIG. 1 and the cemented lens shown in FIG. 8. [Figure 13] FIG. 13 is a diagram illustrating a comparative configuration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] [Embodiment 1] Hereinafter, one embodiment of the present invention will be described with reference to FIGS.

[0018] 1.Cemented Lens 1 is a cross-sectional view of the cemented lens 50 of this embodiment. The cemented lens 50 can be applied to various optical elements constituting various optical systems such as an imaging optical system, a projection optical system, and the like, such as lenses, prisms (color separation prisms, color synthesis prisms, etc.), polarizing beam splitters (PBS), and cut filters (for infrared rays, ultraviolet rays, etc.), and there is no limitation on the type of optical elements.

[0019] The cemented lens 50 is formed by bonding a first optical element 10 and a second optical element 20 together with an adhesive layer 30 interposed therebetween.

[0020] (1) First Optical Element 10 The first optical element 10 includes a substrate 11 and a first light-shielding film 12. The first optical element 10 may include layers other than those described above.

[0021] <Base material 11> The substrate 11 may be made of glass or plastic, and is not particularly limited to a material as long as it is made of an optical material. The substrate 11 may be a concave meniscus lens, but is not limited to this.

[0022] The substrate 11 has optically effective regions 11a and 11b through which the effective light beam that contributes to imaging passes, and a non-optically effective region 11c outside the optically effective regions 11a and 11b. Here, the optically effective regions 11a and 11b refer to the region where the maximum diameter of the optical path when the effective light beam passes through the optical surface of the substrate 11 intersects with the optical surface. In FIG. 1, the optically effective region 11a is provided on the convex side, and the optically effective region 11b is provided on the concave side. The non-optically effective region 11c corresponds to a region generally called an edge surface or edge portion. Note that the shapes, ranges, etc. of the optically effective regions 11a and 11b and the non-optically effective region 11c shown in FIG. 1 are merely examples, and the shapes, ranges, etc. of the optically effective region and the non-optically effective region change as appropriate depending on the optical characteristics of the cemented lens 50 and its specific shape, etc.

[0023] <First light-shielding film 12> The first light-shielding film 12 is formed in the optically ineffective region 11c of the base material 11. The first light-shielding film 12 is a layer that is opaque to incident light. The first light-shielding film 12 may have any configuration as long as it is an opaque film to incident light. For example, the first light-shielding film 12 may be a light-absorbing film containing a substance that absorbs incident light and converts it into energy (hereinafter, referred to as a light-absorbing substance). Specifically, when the wavelength region of light used by the cemented lens 50 is a visible light region to near-infrared region of about 400 nm to 800 nm, a substance having a high absorption rate of light with wavelengths in the visible light region and near-infrared region, such as carbon, black pigment, and black dye, can be used as the light-absorbing substance. A coating liquid is prepared by dissolving or dispersing these light-absorbing substances together with a binder component (resin component) such as epoxy resin in a solvent, and the coating liquid is applied to the surface of the optically ineffective region 11c to form a coating film, and then the first light-shielding film 12 can be formed by undergoing a process such as drying. In addition, a commercially available internal reflection preventing paint used for applying so-called black coating to the inside of a lens or a lens barrel can be used as the coating liquid, and the coating film can also be used as the first light-shielding film 12.

[0024] The average absorption coefficient β of the first light-shielding film 12 is 1.0×10 4 m -1 From the viewpoint of further improving the effect of preventing internal reflection, the absorption coefficient β is preferably 1.0×10 5 m -1 More preferably, it is equal to or greater than this.

[0025] The difference between the refractive index of the first light-shielding film 12 and that of the base material 11 is preferably small. Specifically, since the refractive index of the base material 11 is generally about 1.4 to 2.1, the refractive index of the first light-shielding film 12 is preferably 1.4 to 1.8. Here, the refractive index of the first light-shielding film 12 is determined by the refractive index and the blending ratio of each component (light absorbing material and binder component) constituting the first light-shielding film 12. When the ratio of the binder component of the first light-shielding film 12 is high, the refractive index and the light absorption coefficient of the first light-shielding film 12 are reduced, but the strength is improved. On the other hand, when the ratio of the binder component of the first light-shielding film 12 is low, the refractive index and the light absorption coefficient of the first light-shielding film 12 are high, but the strength is reduced.

[0026] (2) Second Optical Element 20 The second optical element 20 includes a base material 21 and a second light-shielding film 22 .

[0027] <Base material 21> The base material 21 may be made of glass or plastic, and is not particularly limited as long as it is made of an optical material. A biconvex lens may be used for the base material 21, but is not limited thereto.

[0028] The substrate 21 has optically effective regions 21a and 21b through which the effective light beam that contributes to image formation passes, and a non-optically effective region 21c outside the optically effective regions 21a and 21b. Here, the optically effective regions 21a and 21b refer to the region where the maximum diameter of the optical path when the effective light beam passes through the optical surface of the substrate 21 intersects with the optical surface. In FIG. 1, the optically effective region 21a is provided on the side of the first optical element 10, and the optically effective region 21b is provided on the opposite side. The non-optically effective region 21c corresponds to a region generally called an edge surface or edge portion. Note that the shapes, ranges, etc. of the optically effective regions 21a and 21b and the non-optically effective region 21c shown in FIG. 1 are merely examples, and the shapes, ranges, etc. of the optically effective region and the non-optically effective region change appropriately depending on the optical characteristics of the cemented lens 50 and its specific shape, etc.

[0029] <Second light-shielding film 22> The second light-shielding film 22 is formed in the optically ineffective region 21c of the base material 21. The second light-shielding film 22 may have the same configuration as the first light-shielding film 12, or may be a light-shielding film made of a material different from that of the first light-shielding film 12, among the film materials applicable to the first light-shielding film 12 described above.

[0030] (3) Adhesive layer 30 The adhesive layer 30 is formed of a bonding adhesive used to bond the optically effective area 11b of the first optical element 10 and the optically effective area 21a of the second optical element 20 together. The adhesive layer 30 is exposed between the first light-shielding film 12 and the second light-shielding film 22. In other words, the adhesive layer 30 has an end face that is not in contact with either the first optical element 10 or the second optical element 20. That is, this end face is not covered by either the first light-shielding film 12 or the second light-shielding film 22, and is not covered by any other light-shielding film. The adhesive layer 30 is sandwiched and stretched between the first optical element 10 and the second optical element 20, and is therefore exposed between the first light-shielding film 12 and the second light-shielding film 22. More specifically, as shown in FIG. 4, the adhesive layer 30 is exposed on a surface 12a of the first light-shielding film 12 and a surface 22a of the second light-shielding film 22.

[0031] The adhesive layer 30 is a layer of hardened adhesive used for bonding glass lenses. In addition to being optically transparent, the adhesive is required to have high adhesive strength and a fast hardening speed, and acrylic, epoxy, and polyene / polythiol hardening adhesives are suitable for use. A hardening initiator is added to these adhesives, and they can be hardened by heat or ultraviolet light.

[0032] A method for bonding the first optical element and the second optical element 20 via the adhesive layer 30 (bonding process) may be, for example, to coat an adhesive that will become the adhesive layer 30 on either surface of the first optical element 10 or the second optical element 20, and then bonding the optical elements 10, 20 together.

[0033] The optically effective areas 11a, 11b of the substrate 11 of the first optical element 10 and the optically effective areas 21a, 21b of the substrate 21 of the second optical element 20 are interfaces with materials having different refractive indices, and are refracting surfaces. If the difference in refractive index between the materials in contact with each other at these interfaces is large, light will be reflected, and therefore an anti-reflection film (not shown) that reduces the refractive index difference is provided as necessary. The anti-reflection film will be described later.

[0034] 3. Zoom lens (optical system) Next, a zoom lens, which is one aspect of an optical system including the cemented lens of this embodiment, will be described with reference to Fig. 5. Fig. 5 is a cross-sectional view of a zoom lens 500.

[0035] The zoom lens 500 has a plurality of lens groups, one or more of which are equipped with the above-mentioned cemented lens 50. As shown in Fig. 5, the zoom lens 500 includes, from the object side, a first lens group G1 having a first lens L1, a second lens group G2 having second to fourth lenses L2 to L4, and a third lens group G3 having fifth to eighth lenses L5 to L8. In this zoom lens 500, the second lens L2 corresponds to the above-mentioned first optical element 10, and the third lens L3 corresponds to the above-mentioned second optical element 20 in the second lens group G2 equipped with the cemented lens 50.

[0036] In this embodiment, a zoom lens is given as an example of an optical system, but the optical system is not limited to this. Also, the optical system includes one cemented lens of this embodiment, but may include multiple cemented lenses. For example, the optical system may be a single focal length lens including the cemented lens of this embodiment.

[0037] 4. Imaging devices (optical equipment) Next, an example will be shown in which a zoom lens 500 including the cemented lens 50 of this embodiment is applied to an imaging device, which is one form of optical equipment. Fig. 6 is a diagram showing an example of an imaging device 600 including the zoom lens 500 of this embodiment.

[0038] As shown in FIG. 6, the imaging device 600 is composed of a lens barrel 601 that houses the zoom lens 500, and a camera body 602 that includes a solid-state imaging element 603 (light receiving element). The zoom lens 500 performs magnification change and the like by driving a mechanical mechanism (not shown). The solid-state imaging element 603 can be, for example, a photoelectric conversion element such as a CCD (Charge Coupled Device) or a CMOS (Complementary Metal Oxide Semiconductor). In the imaging device 600, light incident from the object side of the zoom lens 500 is finally imaged on the imaging surface of the solid-state imaging element 603. The solid-state imaging element 603 then photoelectrically converts the received light and outputs it as an electrical signal. This output signal is arithmetically processed by a signal processing circuit (not shown), and a digital image corresponding to the object image is generated. The digital image can be recorded on a recording medium such as an HDD (Hard Disk Drive), a memory card, an optical disk, or a magnetic tape. Specific examples of the imaging device 600 include, but are not limited to, a video camera, a digital still camera, a single-lens reflex camera, and a mirrorless single-lens camera.

[0039] 5. Effects of this embodiment According to the cemented lens 50 of this embodiment, it is possible to realize a cemented lens that prevents the occurrence of optical defects in the cemented lens caused by the light-shielding film.

[0040] Specifically, in the cemented lens 50, the adhesive layer 30 is not covered by either the first light-shielding film 12 or the second light-shielding film 22. That is, before the adhesive layer 30 is formed, the first light-shielding film 12 and the second light-shielding film 22 (hereinafter, may be simply described as light-shielding film) are formed on each optical element. That is, when the light-shielding film (the first light-shielding film 12 and the second light-shielding film 22) is formed in the non-optically effective areas 11c, 21c, it is not necessary to thermally cure the light-shielding film (the first light-shielding film 12 and the second light-shielding film 22) at a low temperature in consideration of the adhesive layer 30, and the light-shielding film (the first light-shielding film 12 and the second light-shielding film 22) can be thermally cured at a high temperature. Therefore, the solvent of the first light-shielding film 12 and the second light-shielding film 22 can be sufficiently volatilized. As a result, the solvent does not infiltrate into the adhesive layer 30 formed between the optical elements 10, 20. Therefore, the adhesive layer does not change in quality (discoloration) as may occur due to infiltration, and the optical performance and function are not deteriorated.

[0041] In addition, since the first light-shielding film 12 and the second light-shielding film 22 can be sufficiently cured, even if the cemented lens 50 is washed with a cleaning liquid such as isopropyl alcohol, the dye contained in the first light-shielding film 12 and the second light-shielding film 22 is not eluted into the cleaning liquid, and the performance of the first light-shielding film 12 and the second light-shielding film 22 does not deteriorate. In addition, since the first light-shielding film 12 and the second light-shielding film 22 can be sufficiently cured, the adhesion between the first light-shielding film 12 and the second light-shielding film 22 and the substrates 11 and 21 of the optical element can be ensured. Therefore, the first light-shielding film 12 and the second light-shielding film 22 do not peel off from the substrates 11 and 21 due to ultrasonic cleaning or the like.

[0042] In addition, since the adhesive layer 30 is exposed between the first light-shielding film 12 and the second light-shielding film 22, moisture absorbed in the adhesive layer 30 can be released in a high-temperature and high-humidity environment, etc. This makes it possible to avoid a situation in which moisture becomes supersaturated in the adhesive layer 30, causing condensation to form at the interfaces between the adhesive layer 30 and the first optical element 10 and the second optical element 20, resulting in whitening, and good optical performance can be achieved.

[0043] Furthermore, in the cemented lens 50 of this embodiment, the adhesive layer 30 is exposed on a surface 12a (FIG. 4) of the first light-shielding film 12 formed in the non-optically effective region 11c of the base 11 of the first optical element 10, and on a surface 22a (FIG. 4) of the second light-shielding film 22 formed in the non-optically effective region 21c of the base 21 of the second optical element 20. This makes it possible to realize a state in which the adhesive layer 30 is exposed over a relatively wide area, thereby enabling the aforementioned moisture release to be performed efficiently.

[0044] Furthermore, in the cemented lens 50 of this embodiment, an antireflection film (not shown) may be formed on the optically effective area 11a of the base material 11 of the first optical element 10. This antireflection film may be made of the same transparent material as the underlayer 13a of the second embodiment described below.

[0045] Furthermore, in the cemented lens 50 of this embodiment, an antireflection film (not shown) may also be formed on the optically effective area 21b of the base material 21 of the second optical element 20. This antireflection film may be made of the same transparent material as the underlayer 23b of the second embodiment described below.

[0046] An antireflection film (not shown) may also be formed on the optically effective region 11b of the substrate 11 of the first optical element 10 and the optically effective region 21a of the substrate 21 of the second optical element 20, but is not necessary if the refractive index of the bonding resin of the adhesive layer 30 is close to that of the substrates 11 and 21. When an antireflection film is also provided on the optically effective region 11b and the optically effective region 21a, an antireflection film made of the same transparent material as the underlayers 13a and 23b of the second embodiment described later can be formed.

[0047] [Modification 2] In the above-described embodiment, the adhesive layer 30 is exposed on the surface 12a of the first light-shielding film 12 and on the surface 22a of the second light-shielding film 22 (FIG. 4). However, this is not limiting, and it is sufficient that the adhesive layer 30 is exposed between the first light-shielding film 12 and the second light-shielding film 22. For example, a modified configuration shown in FIG. 7 may be used.

[0048] 7 differs from the embodiment in Fig. 4 in that the adhesive layer 30 is not exposed on the surface 12a of the first light-shielding film 12 and on the surface 22a of the second light-shielding film 22. Even in the embodiment in Fig. 7, the adhesive layer 30 has an exposed portion that is not covered by the light-shielding film, and therefore it is possible to achieve the same effect as the adhesive layer 30 in the first embodiment and to realize a cemented lens that prevents optical defects in the cemented lens caused by the light-shielding film.

[0049] The embodiment of the adhesive layer 30 shown in Fig. 7 and the embodiment of the adhesive layer 30 shown in Fig. 4 are determined, for example, by the difference in the amount of adhesive applied that constitutes the adhesive layer 30. In addition, the embodiment shown in Fig. 7 is achieved by including a step of wiping off the parts of the adhesive layer 30 exposed on the surface 12a and the surface 22a after the adhesive layer 30 is exposed on the surface 12a of the first light-shielding film 12 and the surface 22a of the second light-shielding film 22 as shown in Fig. 4.

[0050] [Embodiment 2] Other embodiments of the present invention will be described below. For ease of explanation, the same reference numerals are given to members having the same functions as those described in the above embodiment, and the description thereof will not be repeated.

[0051] 1.Cemented Lens 8 is a cross-sectional view of a cemented lens 50A of the present embodiment. The cemented lens 50A differs in that the layer configurations laminated on the respective substrates 11, 21 of the first optical element 10A and the second optical element 20A are different from the layer configurations laminated on the respective substrates 11, 21 of the cemented lens 50 of the above-described first embodiment. Furthermore, the cemented lens 50A of the present embodiment differs from the cemented lens 50 of the above-described first embodiment in that the cemented lens 50A is covered with a low refractive index layer 40.

[0052] (1) First Optical Element 10A 9 is a cross-sectional view of a first optical element 10A. The first optical element 10A of this embodiment differs from the first optical element 10 of embodiment 1 in that an undercoat layer 13a is formed in the optically effective region 11a of the substrate 11. Note that, in the case where an antireflection film is formed in the optically effective region 11a of the substrate 11 of the first optical element 10 of embodiment 1 described above, an undercoat layer 13a is formed in place of the antireflection film in the first optical element 10A of this embodiment.

[0053] An underlayer 13b as a bonding surface antireflection coating may be formed in the optically effective area 11b of the substrate 11. As the bonding surface antireflection coating, a transparent material used for the underlayer 13a described below can be used.

[0054] <Base layer 13a> The underlayer 13a functions as an anti-reflection film. The layer structure and materials of the underlayer 13a will be described below.

[0055] (a) Layer composition The underlayer 13a may be a single-layer film or a multi-layer film in which one or more thin films (hereinafter, sub-layers) made of transparent materials each having a refractive index of 1.35 to 2.5 are laminated. Here, the sub-layer refers to a single physical thin film that constitutes the underlayer 13a. For example, the underlayer 13a may be configured by laminating at least one or more sub-layers, and each sub-layer may function as an optical interference layer, thereby making it possible to extremely reduce the reflectance of the anti-reflection film.

[0056] Whether the underlayer 13a is a single-layer film or a multi-layer film, the optical design of each layer (design of the refractive index and optical film thickness) can be performed by a matrix method in the same manner as in the design of a normal antireflection film. By increasing the number of sub-layers constituting the underlayer 13a, an antireflection film with higher antireflection performance can be obtained.

[0057] (b) Transparent material The transparent material constituting each sub-layer of the underlayer 13a may be at least one of a transparent inorganic material having a refractive index of 1.35 to 2.5, an organosilane, and an organic resin.

[0058] Transparent inorganic materials include, for example, inorganic oxides and inorganic fluorides.

[0059] Examples of inorganic oxides include Al2O3, ZrO2+Al2O3, SiO, MgO, La2O3+Al2O3, Y2O3, In2O3+SnO2, La2Ti2O7, SnO2, Ta2O5, HfO2, ZrO2, CeO2, WO3, ZrO2+TiO2, Ta2O5, Ta2O5+ZrO2, Ta2O5+TiO2, Ti3O5, Ti4O7, and TiPr6O. 11 +TiO2, TiO, TiO2, Nb2O5, TiO2+La2O3, Pr6O 11 +TiO2, SiO2, SiO x N y , CeO2, etc.

[0060] Examples of inorganic fluorides include MgF2, AlF3, Na2SiF6, H2SiF6, NaF, CaF2, Na3AlF6, and YF3.

[0061] Furthermore, as the transparent inorganic material, in addition to the above inorganic oxides and inorganic fluorides, SiN, SiC, ZnS, etc. can also be used.

[0062] Next, as the organosilane, for example, straight silicones such as dimethyl silicone, methylphenyl silicone, and methylhydrogen silicone can be mentioned. In addition to these straight silicones, various modified silicones may be used as the organosilane. As the modified silicone, for example, modified silicones modified with functional groups at one end, both ends, or side chains such as polyether modified silicone, epoxy modified silicone, amino modified silicone, carboxy modified silicone, mercapto modified silicone, carbino modified silicone, methacryl modified silicone, and long chain alkyl modified silicone can be used. Furthermore, it is also possible to use a product obtained by appropriately combining these straight silicones and / or modified silicones and reacting them to polymerize them.

[0063] Examples of the organic resin include epoxy resin, fluororesin, silicone resin, polyethylene resin, polypropylene resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl acetate resin, acrylic resin, polyamide resin, polyacetal resin, polycarbonate resin, modified polyphenylene ether resin, polybutylene terephthalate resin, polyethylene terephthalate resin, cyclic polyolefin resin, liquid crystal polymer, and the like, or monomer compounds thereof.

[0064] However, when the underlayer 13a is a multilayer film, the sub-layer disposed on the outermost surface of the underlayer is preferably any one of inorganic oxides, inorganic fluorides, organosilanes, and organic resins. By making the outermost layer of the underlayer 13a a layer made of any one of these materials, adhesion between the first light-shielding film 12 and the low refractive index layer 40 described later is improved when the first light-shielding film 12 and the low refractive index layer 40 are laminated on the surface of the underlayer 13a.

[0065] (c) Film thickness In order to obtain an antireflection coating with a wider bandwidth and lower reflection, it is preferable that the optical thickness of each sublayer is 150 nm or less. If the optical thickness of each sublayer exceeds 150 nm, the design will have many unnecessary ripples, and it is not preferable because the average reflectance of the antireflection coating cannot be kept low.

[0066] (d) Film formation method When forming the underlayer 13a (each sub-layer), it is preferable to adopt a vacuum film formation method or a wet film formation method. As the vacuum film formation method, either a physical vapor deposition method or a chemical vapor deposition method can be suitably used. As the physical vapor deposition method, a vacuum vapor deposition method, a sputtering method, an ion plating method, and an ion beam vapor deposition method can be mentioned. As the chemical vapor deposition method, a CVD method (including a plasma CVD method) and an atomic layer deposition method (ALD method) can be mentioned. Among these, in particular, a vacuum vapor deposition method, a sputtering method, and a CVD method can be suitably adopted. As the wet film formation method, for example, a dip coating method, a spin coating method, a spray coating method, a roll coating method, a screen printing method, and the like can be mentioned. By adopting these methods, it is possible to precisely form the underlayer 13a (or a sub-layer) having a physical thickness in the range of 1 nm to 150 nm.

[0067] <First light-shielding film 12> The first light-shielding film 12 is formed in the non-optically effective region 11c of the substrate 11, similarly to the first light-shielding film 12 of the first embodiment. In this embodiment, the above-mentioned underlayer 13b formed in the optically effective region 11b of the substrate 11 is also formed slightly in the non-optically effective region 11c (FIG. 9). Therefore, the first light-shielding film 12 is provided on the surface of the underlayer 13b formed slightly in the non-optically effective region 11c of the substrate 11 and on the surface of the substrate 11. The light-shielding film 12 may also be formed slightly on the surface of the underlayer 13a.

[0068] (2) Second Optical Element 20A 10 is a cross-sectional view of the second optical element 20A. The second optical element 20A of this embodiment differs from the second optical element 20 of the first embodiment in that an underlayer 23b is formed in the optically effective region 21b of the substrate 21. Note that, in the case where an antireflection film is formed in the optically effective region 21b of the substrate 21 of the second optical element 20 of the first embodiment described above, an underlayer 23b is formed in the second optical element 20A of this embodiment instead of the antireflection film.

[0069] <Base layer 23b> The underlayer 23b functions as an anti-reflection film, similar to the underlayer 13a. Details of the underlayer 23b are the same as those of the underlayer 13a described above. The underlayer 23b may be made of the same material as the underlayer 13a, or may be made of a different material.

[0070] In the second optical element 20A of this embodiment, an underlayer 23a may be formed in the optically effective region 21a of the substrate 21. This underlayer 23a is a bonding surface antireflection coating similar to the underlayer 13b provided in the optically effective region 11b of the substrate 11. However, when the refractive index of the substrate 21 is close to the refractive index of the adhesive used in the adhesive layer 30 and the reflectance at the interface therebetween is sufficiently small, the underlayer 23a is not necessary.

[0071] <Second light-shielding film 22> The second light-shielding film 22 is formed in the optically ineffective region 21c of the base material 21, similarly to the second light-shielding film 22 in the first embodiment. The light-shielding film 22 may be formed slightly on the surfaces of the base layer 23a and the base layer 23b.

[0072] (3) Adhesive layer 30 8, the cemented lens 50 of this embodiment is formed by bonding the above-mentioned first optical element 10A and second optical element 20A together via an adhesive layer 30. In this embodiment, as in the first embodiment, the adhesive layer 30 is exposed between the first light-shielding film 12 and the second light-shielding film 22.

[0073] (4) Low refractive index layer 40 The low refractive index layer 40 covers the entire surface of the structure in which the above-mentioned first optical element 10A and second optical element 20A are bonded by the adhesive layer 30. That is, as shown in Fig. 8, the low refractive index layer 40 covers the surface of the base layer 13a, the surface of the first light-shielding film 12, the exposed surface of the adhesive layer 30, the surface of the second light-shielding film 22, and the surface of the base layer 23b.

[0074] The low refractive index layer 40 is a layer with a refractive index of 1.15 to 1.35, and functions as an antireflection film that suppresses the reflection of incident light by optical interference. Therefore, by laminating the low refractive index layer 40 with the underlayers 13a and 23b formed in the optically effective regions of the substrates 11 and 21, the reflectance of the antireflection film can be kept low even when light in a wide wavelength range is incident. In addition, by laminating the low refractive index layer 40 with the first light-shielding film 12 and the second light-shielding film 22, the reflectance of the antireflection film can be kept low.

[0075] The low refractive index layer 40 may be, for example, a layer in which low refractive index materials having voids in the particles, such as hollow silica particles or porous silica (nanoporous silica), are bound by a binder, or a layer made of a material having a refractive index within the above range, such as a group consisting of SiO2, MgF2, and Al2O3. In this embodiment, it is particularly preferable that the low refractive index layer 40 is a hollow silica layer in which hollow silica particles 401 are bound to each other by a binder 402 (binding material), as illustrated in FIG. 11. Hereinafter, the configuration of the low refractive index layer 40 will be specifically described assuming that the low refractive index layer 40 is a hollow silica layer.

[0076] (a) Hollow silica particles 401 First, the hollow silica particles 401 will be described. In the present invention, the hollow silica particles 401 refer to primary particles of silica having a core-shell structure (balloon structure) with a hollow portion in a shell made of silica. The primary particles refer to particles of silica that are not aggregated with other particles. Specifically, as shown in FIG. 11, the hollow silica particles 401 refer to silica particles composed of a shell portion 401a made of silica and a hollow portion 401b completely surrounded by the shell portion 401a. By adopting the hollow silica particles 401 having the core-shell structure as the main material for the layer-constituting material of the low refractive index layer 40, the refractive index of the low refractive index layer 40 can be reduced below the refractive index (1.48) of silica itself. In addition, compared with the porous silica layer composed of the aggregate of the porous silica having many pores in the silica particles, the present embodiment uses hollow silica in which the hollow portion 401b is completely surrounded by the shell portion 401a, so that a film having high strength and excellent durability can be obtained. Furthermore, since no liquid or the like penetrates into the hollow silica particle 401, even when a film is formed by a wet film formation method, there is no risk of the hollow portion 401b inside the silica being filled with a resin material or the like, and the porosity of the material itself can be maintained, thereby preventing an increase in the refractive index.

[0077] Average particle size D of hollow silica particles 401 50 The average particle diameter D of the hollow silica particles 401 is preferably 5 nm or more and 100 nm or less. 50 When the average particle diameter D of the hollow silica particles 401 is less than 5 nm, it becomes difficult to provide the voids 403 other than the hollows 401b of the hollow silica particles 401 in the low refractive index layer 40. 50 If the average particle diameter D of the hollow silica particles 401 exceeds 100 nm, light scattering (haze) may occur, which is not preferable. 50 If it exceeds 100 nm, it becomes extremely difficult to precisely control the physical film thickness of the low refractive index layer 40 to an order of several nm.

[0078] (b) Binder 402 Next, the binder 402 will be described. As shown in Fig. 11, the low refractive index layer 40 is formed as a layer by binding hollow silica particles 401 to each other with the binder 402. In this case, it is preferable that the outer surfaces of the hollow silica particles 401 are covered with the binder 402, and the hollow silica particles 401 are bound to each other by the binder 402 that covers the outer surfaces of the hollow silica particles 401.

[0079] As the binder 402, a resin material or a metal alkoxide can be adopted. Examples of the resin material include epoxy resin, fluororesin, silicone resin, polyethylene resin, polypropylene resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl acetate resin, acrylic resin, polyamide resin, polyacetal resin, polycarbonate resin, modified polyphenylene ether resin, polybutylene terephthalate resin, polyethylene terephthalate resin, cyclic polyolefin resin, liquid crystal polymer, and the like, or monomer compounds thereof. These resin materials are preferably ultraviolet curable, room temperature curable, or thermosetting compounds, and are particularly preferably ultraviolet curable or room temperature curable compounds. As a specific layer formation method, for example, these materials are mixed with hollow silica particles 401, a polymerization initiator or a crosslinking agent is added as necessary, and the coating liquid is prepared by diluting it to an appropriate concentration with a solvent, and a wet method such as a dip coating method, a spin coating method, a spray method, a roll coating method, or a screen printing method can be adopted. By these methods, the coating liquid is applied to the surfaces of the layers (undercoat layer 13a, first light-shielding film 12, second light-shielding film 22, adhesive layer 30, undercoat layer 23b) on which the low refractive index layer 40 is to be laminated to an appropriate thickness, and then the layers are polymerized and cross-linked by ultraviolet irradiation or heat treatment, and the solvent is volatilized, thereby forming the low refractive index layer 40.

[0080] In addition, the material is preferably a material in which a sol is formed by dissolving or suspending a metal alkoxide in a solvent, and a gel is generated by hydrolysis and polymerization, and for example, a material in which silica gel is generated by hydrolysis and polymerization, such as alkoxysilane or silsesquioxane, is preferably used. These materials and hollow silica particles 401 are dissolved or suspended in a solvent to prepare a sol-gel agent, and the sol-gel agent is applied to the surfaces of the layers (underlying layer 13a, first light-shielding film 12, second light-shielding film 22, adhesive layer 30, and underlying layer 23b) on which the low refractive index layer 40 is laminated by spray coating, spin coating, dip coating, flow coating, bar coating, or the like, and a gel containing hollow silica particles 401 is formed by hydrolysis, and the solvent is volatilized, and the low refractive index layer 40 can be formed.

[0081] The solvent may be evaporated by natural drying at room temperature, or by heating and drying using a dryer, a hot plate, an electric furnace, or the like. The drying conditions are temperature and time that do not affect the lens and can evaporate the organic solvent in the low refractive index layer 40 to a certain extent. When the adhesive layer 30 is cured to bond the first optical element 10 and the optical element 20 constituting the cemented lens 50 through the adhesive layer 30, stress due to curing shrinkage remains inside the resin of the adhesive layer 30, and the stress in the resin may be released due to the effect of heat during drying, causing surface deformation. Therefore, it is preferable to dry at room temperature or the like, which is 100°C or less, more preferably 80°C or less, and even more preferably 40°C or less.

[0082] (c) Gap 403 In this embodiment, it is preferable that voids 403 are provided between silica particles 401 bonded to each other in the low refractive index layer 40 as shown in Fig. 11. By providing, in the low refractive index layer 40, hollows 401b present inside the hollow silica particles 401 and voids 403 surrounded by a binder 402 between the hollow silica particles 401, the porosity in the low refractive index layer 40 can be increased and the refractive index of the low refractive index layer 40 can be made lower than the refractive index of silica itself, resulting in a layer with higher antireflection performance. Moreover, as in this embodiment, even if the voids 403 are not filled with a binder or the like, the hollow silica particles 401 are bonded together via the binder 402 that covers the outer surface of the hollow silica particles 401, thereby improving the adhesion between the hollow silica particles 401 and the layers (underlayer 13a, first light-shielding film 12, second light-shielding film 22, adhesive layer 30, underlayer 23b) that stack the low refractive index layer 40. Moreover, since the hollow silica particles 401 themselves are surrounded by the outer shell 401a made of silica, the low refractive index layer 40 can be made into a layer with excellent scratch resistance and durability even if the outer surface of the low refractive index layer 40 is not covered with a resin or the like.

[0083] (d) Volume ratio of hollow silica particles 401 and binder 402 Here, the volume occupied by the hollow silica particles 401 and the binder 402 in the low refractive index layer 40 is preferably 30 volume % or more and 99 volume % or less. The volume occupied by the hollow silica particles 401 here means the total volume of the hollow silica spheres including the outer shell 401a of the hollow silica particles 401 and the hollow portion 401b surrounded by the hollow portion 401b in the low refractive index layer 40. If the volume occupied by the hollow silica particles 401 and the binder 402 in the low refractive index layer 40 is less than 30 volume %, this is not preferable because the durability and scratch resistance of the low refractive index layer 40 are reduced. On the other hand, if the volume occupied by the hollow silica particles 401 in the low refractive index layer 40 exceeds 99 volume %, the volume of the void portion 403 in the low refractive index layer becomes small, and the refractive index of the low refractive index layer 40 does not reach the desired characteristics. From this viewpoint, it is more preferable that the volume occupied by the hollow silica particles 401 in the low refractive index layer 40 is 90 volume % or less.

[0084] (e) Refractive index The refractive index of the low refractive index layer 40 is required to be 1.15 or more and 1.35 or less, as described above. If the refractive index of the low refractive index layer 40 is less than 1.15, in the case of the low refractive index layer 40 made of a hollow silica layer, the porosity in the layer becomes too high, which is undesirable as it reduces the durability of the low refractive index layer 40. From this viewpoint, it is more preferable that the refractive index of the low refractive index layer 40 is 1.17 or more. On the other hand, if the refractive index of the low refractive index layer 40 exceeds 1.35, it is undesirable as the reflectance at the design central wavelength becomes high. Therefore, from this viewpoint, it is preferable that the refractive index of the low refractive index layer 40 is lower within the above range, more preferably 1.32 or less, and even more preferably 1.30 or less.

[0085] (f) Film thickness The physical thickness of the low refractive index layer 40 is preferably within a range of 80 nm to 240 nm. If the physical thickness of the low refractive index layer 40 is less than 80 nm or exceeds 240 nm, it is difficult to set the phase change to an appropriate value for light with wavelengths in the visible light region and near infrared region, and the antireflection performance of the low refractive index layer 40 may be deteriorated, which is not preferable.

[0086] 2. Effects of the Present Embodiment According to the configuration of this embodiment, in addition to the effects achieved by the configuration of the above-mentioned first embodiment, it is possible to reduce reflection of light incident on the surface of the adhesive layer 30 exposed between the first light-shielding film 12 and the second light-shielding film 22 by forming a low refractive index layer 40 on the adhesive layer 30. This reduction in reflection will be described with reference to FIG.

[0087] Fig. 12 shows the reflectance of light when the cemented lens 50A of this embodiment and the cemented lens 50 of embodiment 1 (Fig. 1) are used and light is incident on the surface of the adhesive layer 30 exposed between the first light-shielding film 12 and the second light-shielding film 22. In Fig. 12, the reflectance data of the cemented lens 50 of embodiment 1 is shown by a solid line, and the reflectance data of the cemented lens 50A of embodiment 2 is shown by a dashed line.

[0088] As shown in FIG. 12, it can be seen that the cemented lens 50A of the present embodiment effectively reduces the reflectance of light when light is incident on the surface of the adhesive layer 30 that is exposed between the first light-shielding film 12 and the second light-shielding film 22.

[0089] The low refractive index layer 40 provides the above-mentioned effect as long as it covers at least the adhesive layer 30. However, by forming the low refractive index layer 40 not only on the adhesive layer 30 but also on the underlayers 13a and 23b, the first light-shielding film 12, and the second light-shielding film 22, the reflectance of the antireflection film can be kept low even when light in a wide wavelength range is incident.

[0090] The cemented lens 50A of the present embodiment may include layers other than the above-mentioned layers. For example, a functional layer may be provided on the surface of the low refractive index layer 40. The functional layer is a transparent, very thin film that does not optically affect the anti-reflection performance of the low refractive index layer 40 and refers to a layer having various functions. Examples of such functional layers include layers having various functions such as improving the hardness, scratch resistance, heat resistance, weather resistance, solvent resistance, water repellency, oil repellency, anti-fogging properties, hydrophilicity, anti-fouling properties, and electrical conductivity of the surface of the low refractive index layer 40.

[0091] As another layer, an adhesion layer may be provided between the first light-shielding film 12 and the low refractive index layer 40 and between the first light-shielding film 12 and the second light-shielding film 22 and the low refractive index layer 40 in order to improve adhesion therebetween.

[0092] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0093] 〔summary〕 In order to solve the above-mentioned problems, a cemented lens 50, 50', 50A according to one embodiment of the present invention is a cemented lens 50, 50', 50A including a first optical element 10 having a first light-shielding film 12 formed on a non-optically effective region 11c of a substrate 11, a second optical element 20 having a second light-shielding film 22 formed on a non-optically effective region 12c of a substrate 12, and an adhesive layer 30 that bonds the optically effective regions of the first optical element 10 and the second optical element 20 together, and the adhesive layer 30 is exposed between the first light-shielding film and the second light-shielding film.

[0094] According to the above-described configuration, it is possible to provide a technique for preventing the occurrence of optical defects in the cemented lens caused by the light-shielding film.

[0095] Specifically, the adhesive layer 30 is exposed between the first light-shielding film 12 and the second light-shielding film 22, and has a portion (exposed portion) that is not covered by either the first light-shielding film 12 or the second light-shielding film 22. That is, before the adhesive layer 30 is formed, the first light-shielding film 12 and the second light-shielding film 22 (hereinafter, may be simply described as light-shielding film) are formed on each optical element. That is, when the light-shielding film (the first light-shielding film 12 and the second light-shielding film 22) is formed in the non-optically effective areas 11c, 21c, it is not necessary to thermally cure the light-shielding film (the first light-shielding film 12 and the second light-shielding film 22) at a low temperature in consideration of the adhesive layer 30, and the light-shielding film (the first light-shielding film 12 and the second light-shielding film 22) can be thermally cured at a high temperature. Therefore, the solvent of the first light-shielding film 12 and the second light-shielding film 22 can be sufficiently volatilized. This prevents the solvent from seeping into the adhesive layer 30 formed between the optical elements 10 and 20. Therefore, no deterioration (discoloration) of the adhesive layer that may occur due to seepage does occur, and no deterioration of the optical performance and function occurs.

[0096] In addition, since the first light-shielding film 12 and the second light-shielding film 22 can be sufficiently cured, even if the cemented lens 50 is washed with a cleaning liquid such as isopropyl alcohol, the dye contained in the first light-shielding film 12 and the second light-shielding film 22 is not eluted into the cleaning liquid, and the performance of the first light-shielding film 12 and the second light-shielding film 22 does not deteriorate. In addition, since the first light-shielding film 12 and the second light-shielding film 22 can be sufficiently cured, the adhesion between the first light-shielding film 12 and the second light-shielding film 22 and the substrates 11 and 21 of the optical element can be ensured. Therefore, the first light-shielding film 12 and the second light-shielding film 22 do not peel off from the substrates 11 and 21 due to ultrasonic cleaning or the like.

[0097] In addition, since the adhesive layer 30 is exposed between the first light-shielding film 12 and the second light-shielding film 22, moisture absorbed in the adhesive layer 30 can be released in a high-temperature and high-humidity environment, etc. This makes it possible to avoid a situation in which moisture becomes supersaturated in the adhesive layer 30, causing condensation to form at the interfaces between the adhesive layer 30 and the first optical element 10 and the second optical element 20, resulting in whitening, and good optical performance can be achieved.

[0098] In addition, in the cemented lenses 50, 50', and 50A, the adhesive layer is exposed on a surface of the first light-shielding film formed in the non-optically effective area of ​​the first optical element, and on a surface of the second light-shielding film formed in the non-optically effective area of ​​the second optical element.

[0099] According to the above-mentioned configuration, the adhesive layer extends onto the surface of the light-shielding film, and a relatively wide exposed state can be realized. This allows the adhesive layer 30 to be exposed over a relatively wide area, which allows the aforementioned moisture release to be performed efficiently.

[0100] In addition, in the cemented lens 50A, at least one selected from the group consisting of (i) the optically effective areas (optically effective areas 11a, 21b) of the cemented lens, (ii) the first light-shielding film 12 and the second light-shielding film 22, and (iii) the exposed portion of the adhesive layer 30 is covered with a low-refractive index layer 40 having a refractive index of 1.15 to 1.35.

[0101] According to the above-mentioned configuration, the low refractive index layer 40 functions as an anti-reflection film that suppresses reflection of incident light by optical interference, and therefore the light transmittance of the cemented lens can be improved, thereby realizing the cemented lens 50A having high optical performance.

[0102] In addition, a portion of the light incident on the first light-shielding film 12 and the second light-shielding film 22 may be reflected and become harmful light, but by covering the light-shielding films 12, 22 with the low refractive index layer 40, reflection can be prevented.

[0103] Furthermore, light incident on the exposed portion of the adhesive layer 30 may be reflected and become harmful light, but by covering this portion with the low refractive index layer 40, reflection can be prevented.

[0104] In the cemented lens 50A, the low refractive index layer 40 is selected from the group consisting of SiO2, MgF2, and Al2O3.

[0105] According to the above-mentioned configuration, the low refractive index layer 40 can be firmly adhered to the layer below it.

[0106] In the cemented lens 50A, the low refractive index layer 40 is a layer in which hollow silica particles 401, each having a balloon structure with a shell portion made of silica and a hollow portion surrounded by the shell portion, are bound by a binder 402, and in which voids exist other than the hollow portions of the hollow silica particles, and the average particle size of the hollow silica particles is 5 nm or more and 100 nm or less.

[0107] According to the above-mentioned configuration, by adopting hollow silica particles having a hollow portion as the main component of the low refractive index layer, the refractive index of the low refractive index layer 40 can be reduced below the refractive index (1.48) of silica itself.

[0108] Furthermore, by forming a layer in which hollow silica particles 401, the periphery of which is completely surrounded by an outer shell, are bound by binder 402, it is possible to firmly adhere low refractive index layer 40 to the layer below. This contributes to realizing an anti-reflection film (low refractive index layer 40) with excellent scratch resistance and durability.

[0109] In the cemented lens 50A, the low refractive index layer 40 is a layer formed using the hollow silica particles 401 and a resin material or metal alkoxide as a component of the binder 402.

[0110] According to the above-mentioned configuration, it is possible to form a low refractive index layer without performing heat treatment, which makes it possible to prevent thermal expansion and deformation of the base materials of the first and second optical elements and realize a good cemented lens 50A.

[0111] The optically effective areas (optically effective areas 11a, 21b) of the cemented lenses are provided with underlayers 13a, 23b each having one or more thin films made of a transparent material having a refractive index of 1.35 to 2.5 laminated thereon, and the low refractive index layer is laminated on the underlayer.

[0112] According to the above-mentioned configuration, since the base layers 13a and 23b are provided, the anti-reflection performance can be improved compared to a configuration in which no base layer is provided and the low refractive index layer is provided, and the generation of harmful light (stray light) that causes ghosts and flares can be suppressed.

[0113] In the cemented lens 50A, the underlayers 13a and 23b are films formed by a vacuum deposition method, a sputtering method, or an ALD method.

[0114] According to the above-described configuration, it is possible to provide a cemented lens in which the underlayers 13a and 23b are formed with high accuracy.

[0115] In order to solve the above problem, an optical system (zoom lens 500) according to one aspect of the present invention includes the cemented lens 50 described above.

[0116] According to the above-described configuration, since the cemented lens is provided which suppresses deterioration of optical performance and has resistance to cleaning processes and environmental changes, it is possible to provide an optical system (zoom lens 500) with excellent optical performance.

[0117] In order to solve the above-mentioned problems, an optical device (imaging device 600) according to one embodiment of the present invention includes the cemented lenses 50, 50', 50A, and a light receiving element (solid-state imaging element 603) that receives light collected by the cemented lens.

[0118] According to the above configuration, it is possible to use light focused by the cemented lens that is resistant to deterioration of optical performance and is resistant to cleaning processes and environmental changes, thereby realizing an optical device (imaging device 600) with excellent optical performance.

[0119] In order to solve the above-described problems, a manufacturing method for a cemented lens according to one aspect of the present invention includes a bonding step of bonding together, via an adhesive layer, optically effective areas of a first optical element having a non-optically effective area of ​​a substrate, a first light-shielding film formed on a non-optically effective area of ​​a substrate, and a second optical element having a non-optically effective area of ​​a substrate, a second light-shielding film formed on a non-optically effective area of ​​the substrate.

[0120] According to the above-described configuration, like the cemented lens according to one aspect of the present invention, it is possible to provide a technique for preventing the occurrence of optical defects in the cemented lens caused by the light-shielding film. EXAMPLES

[0121] Example 1 An embodiment of the present invention will now be described.

[0122] The cemented lens 50 shown in Fig. 1 was produced. The substrate 11 was made of S-NBM51 manufactured by Ohara Co., Ltd., which has a refractive index (hereinafter referred to as nd) at d line (wavelength 587.56 nm) of 1.613. The substrate 21 was made of S-FPL51 manufactured by Ohara Co., Ltd., which has an nd of 1.497.

[0123] Next, a dielectric multilayer film consisting of an Al2O3 layer, a ZrO2+TiO2 layer, and an MgF2 layer was formed as an anti-reflection film on the optically effective region 11a of the substrate 11. The thickness of each layer is shown in Table 1. A dielectric multilayer film consisting of an Al2O3 layer, a ZrO2+TiO2 layer, and an MgF2 layer was also formed as an anti-reflection film on the optically effective region 21b of the substrate 21. The thickness of each layer is shown in Table 1. A dielectric multilayer film consisting of an SiO2 layer and an Al2O3 layer was also formed as an anti-reflection film on the optically effective region 11b of the substrate 11. The thickness of each layer is shown in Table 2. On the other hand, no particular film was formed on the optically effective region 21a of the substrate 21. This is because the refractive index of the substrate 21 is close to the refractive index of the adhesive used for bonding, and the reflectance at the interface is sufficiently small. Each anti-reflection film was formed by a vacuum deposition method.

[0124] Furthermore, a light-shielding coating material GT-7II manufactured by Canon Chemical Industry Co., Ltd. was applied to the end surface of the substrate 11 in a thickness of 5 to 10 μm on the non-optically effective region 11c of the substrate 11, and dried and cured at 200° C. for 1 hour to form a first light-shielding film 12 (ink coating film). In this manner, a first optical element 10 was obtained.

[0125] Similarly, a light-shielding coating material GT-7II manufactured by Canon Chemical Co., Ltd. was applied to the end surface of the substrate 21 in a thickness of 5 to 10 μm on the non-optically effective region 21c of the substrate 21, and dried and cured at 200° C. for 1 hour to form a second light-shielding film 22 (ink coating film). In this manner, a second optical element 20 was obtained.

[0126] Next, the surface of the first optical element 10 on the optical effective area 11b side and the surface of the second optical element 20 on the optical effective area 21a side were bonded with an adhesive layer 30 to produce a cemented lens 50. Specifically, in a state where the optical effective area 11a of the substrate 11 was placed facing downward, an adhesive was applied to the optical effective area 11b, and while the adhesive was sandwiched and pressed between the optical effective area 11b of the substrate 11 and the optical effective area 21a of the substrate 21, the substrate 21 was placed in an appropriate position using an optical axis adjustment device, and the adhesive layer 30 was cured by irradiating with UV light. For the adhesive layer 30, a polyene polythiol adhesive OP-1080L (manufactured by Denka Co., Ltd.) was used. The refractive index of OP-1080L after UV curing, that is, the refractive index of the adhesive layer 30, was 1.52. The thickness of the adhesive layer 30 was about 10 μm. In the above manner, a cemented lens 50 in the form shown in FIG. 1 was produced, and this was designated as Example 1. [Table 1] [Table 2]

[0127] Example 2 The cemented lens 50A shown in Fig. 8 was produced. S-NBM51 manufactured by Ohara Inc., having a refractive index (hereinafter referred to as nd) at d line (wavelength 587.56 nm) of 1.613, was used as the substrate 11. S-FPL51 manufactured by Ohara Inc., having an nd of 1.497, was used as the substrate 21.

[0128] Next, a dielectric multilayer film consisting of an Al2O3 layer, a ZrO2+TiO2 layer, and a SiO2 layer was formed as the underlayer 13a on the optically effective region 11a of the substrate 11. The thickness of each layer is shown in Table 3. A dielectric multilayer film consisting of an Al2O3 layer, a ZrO2+TiO2 layer, and a SiO2 layer was also formed as the underlayer 23b on the optically effective region 21b of the substrate 21. The thickness of each layer is shown in Table 3. A dielectric multilayer film consisting of a SiO2 layer and an Al2O3 layer was also formed as the underlayer 13b on the optically effective region 11b of the substrate 11. The thickness of each layer is shown in Table 4. On the other hand, no particular film was formed on the optically effective region 21a of the substrate 21. This is because the refractive index of the substrate 21 is close to the refractive index of the adhesive used for bonding, and the reflectance at the interface is sufficiently small. Each underlayer and anti-reflection film was formed by vacuum deposition.

[0129] A light-shielding paint GT-7II manufactured by Canon Chemical Co., Ltd. was applied to the non-optically effective region 11c of the substrate 11 to a thickness of 5 to 10 μm on the substrate end surface, and dried and cured at 200° C. for 1 hour to form a first light-shielding film 12 (ink coating film). Similarly, a light-shielding paint GT-7II manufactured by Canon Chemical Co., Ltd. was applied to the non-optically effective region 21c of the substrate 21 to a thickness of 5 to 10 μm on the substrate end surface, and dried and cured at 200° C. for 1 hour to form a second light-shielding film 22 (ink coating film).

[0130] Next, the optically effective area 11b of the substrate 11 and the optically effective area 21a of the substrate 21 were bonded with the adhesive layer 30 to produce the cemented lens 50. Specifically, the optically effective area 11a of the substrate 11 was placed facing downward, and adhesive was applied to the optically effective area 11b. The adhesive was then sandwiched between the optically effective area 11b of the substrate 11 and the optically effective area 21a of the substrate 21, while the substrate 21 was placed in an appropriate position using an optical axis adjustment device, and the adhesive layer 30 was cured by irradiating with UV light, after which the excess adhesive protruding from the edge portion was wiped off and removed. For the adhesive layer 30, a polyene polythiol adhesive OP-1080L (manufactured by Denka Co., Ltd.) was used. The refractive index of OP-1080L after UV curing, i.e., the refractive index of the adhesive layer 30, was 1.52. The thickness of the adhesive layer 30 was about 10 μm.

[0131] Furthermore, the surfaces of the underlayer 13a and the underlayer 23b of the cemented lens 50A were subjected to RIE treatment (reactive ion etching treatment) using oxygen to improve the wettability of the surfaces of the underlayer 13a and the underlayer 23b, and then the low refractive index layer 40 was formed on the surfaces of the underlayer 13a and the underlayer 23b. In forming the low refractive index layer 40, a coating liquid was prepared by stirring, dissolving, and preparing hollow silica particles having a particle size of about 60 nm and acrylic resin as a binder component in a solvent mainly composed of propylene glycol monomethyl ether and propylene glycol, and the coating liquid was simultaneously formed on the underlayer 13a and the underlayer 23b by a dip coating method. Thereafter, the formed coating film was left for 2 hours in a clean room atmosphere at room temperature of 23°C. As a result, a low refractive index layer 40 was obtained in which hollow silica particles were bound by acrylic resin (binder). In the above manner, a cemented lens having a form shown in FIG. 8 was fabricated as Example 2. [Table 3] [Table 4]

[0132] Comparative Example As a comparative example, a cemented lens 1000 shown in FIG. 13 was produced. In the cemented lens 1000, a light-shielding film was not formed on each of the base materials 1011 and 1021, while an antireflection film (not shown) was formed on the optically effective areas 1011a, 1011b, and 1021b of the base materials 1011 and 1012, and then the base materials 1011 and 1021 were bonded together via an adhesive layer 1030. A polyene / polythiol adhesive OP-1080L (manufactured by Denka Co., Ltd.) was used for the adhesive layer 1030. The refractive index of OP-1080L after UV curing, i.e., the refractive index of the adhesive layer 1030, was 1.52. The thickness of the adhesive layer 1030 was about 10 μm.

[0133] Next, a light-shielding paint GT-7II manufactured by Canon Chemical Industry Co., Ltd. was applied to the non-optically effective area of ​​the bonded structure to a thickness of 3 to 5 μm on the end face of the substrate, and left to dry and harden at room temperature of 23°C for 24 hours to form a light-shielding film 1050 for comparison.

[0134] 〔evaluation〕 1. Evaluation method The produced cemented lenses were evaluated according to the following method.

[0135] (1) High temperature test The cemented lenses produced in the examples and comparative examples were each placed in a thermostatic chamber at 80° C. for 240 hours, after which the occurrence of infiltration of the ink-containing components of the light-shielding film into the adhesive layer 30 (1030) was visually observed. Evaluation was made according to the following criteria. ○: No discoloration was observed in the adhesive layer. ×: Discoloration (yellow) was observed in the adhesive layer.

[0136] (2) Wipe test A wiping test was carried out on the cemented lens 50 of Example 1 and the cemented lens 1000 of the comparative example.

[0137] The wiping test involved wiping the surface of the light-shielding film of the cemented lens with a nonwoven fabric soaked in isopropyl alcohol (polyester wiper, AS ONE Corporation) under a load of 50 g, and then visually inspecting the wiper surface to evaluate the elution of the black coating film. ○: No discoloration was observed on the wiper after wiping. ×: After wiping, the wiper turned black or yellow.

[0138] (3) High humidity and high temperature test The cemented lenses produced in the examples and comparative examples were each placed in a thermo-hygrostat at 60°C and 90% RH for 240 hours, then removed to an environment at 23°C and 50% RH, and the occurrence of whitening in the periphery of the cemented lenses was visually observed after removal. Evaluation was based on the following criteria. ◯: No whitening was observed on the outer periphery of the cemented lens. ×: Whitening was observed on the outer periphery of the cemented lens.

[0139] 2. Evaluation results The cemented lenses produced in the examples and comparative examples were evaluated in the above items (1) to (3), and the results are shown in Table 5 below. [Table 5]

[0140] From the above results, it was confirmed that the cemented lens according to one embodiment of the present invention suppresses deterioration of optical performance due to deterioration of the adhesive layer, and has resistance to cleaning processes and environmental changes.

[0141] In the first and second embodiments, an example of a cemented lens formed by bonding two optical elements together has been described, but the present invention is not limited to this. The present invention can also be applied to a cemented lens formed by bonding three or more optical elements (lenses). [Explanation of symbols]

[0142] 10, 10A First Optical Element 11, 21 Base material 11a, 11b Optical effective area 11c, 21c Non-optical effective area 12 First light-shielding film 12a, 22a surface 13a,13b,23a,23b Base layer 20, 20A Second Optical Element 22 Second light-shielding film 30 Adhesive layer 40 Low refractive index layer 50, 50´, 50A cemented lenses 401 Hollow Silica Particles 401a Outer shell 401b Hollow part 402 Binder 403 Cavity 500 Zoom lens (optical system) 600 Imaging devices (optical equipment) 603 Solid-state imaging element (photodetector)

Claims

1. a first optical element having a first light-shielding film formed on a non-optically effective region of a substrate; a second optical element having a second light-shielding film formed on a non-optically effective region of a substrate; an adhesive layer bonding optically effective areas of the first optical element and the second optical element to each other, the first light-shielding film is formed only in the non-optically effective area of ​​the first optical element, the second light-shielding film is formed only in the non-optically effective area of ​​the second optical element, The non-optically effective area is an edge surface, the adhesive layer is exposed between the first light-shielding film and the second light-shielding film, the adhesive layer is exposed on a surface of the first light-shielding film and a surface of the second light-shielding film; Cemented lens.

2. At least one selected from the group consisting of (i) an optically effective area of ​​the cemented lens, (ii) the first light-shielding film and the second light-shielding film, and (iii) the exposed portion of the adhesive layer is covered with a low refractive index layer having a refractive index of 1.15 to 1.

35. The cemented lens according to claim 1 .

3. The low refractive index layer is made of SiO 2 , MgF 2 , and Al 2 O 3 Selected from the group consisting of: The cemented lens according to claim 2 .

4. the low refractive index layer is a layer in which hollow silica particles, each having a balloon structure including a shell portion made of silica and a hollow portion surrounded by the shell portion, are bound together by a binder, and in which voids exist other than the hollow portions of the hollow silica particles; The average particle size of the hollow silica particles is 5 nm or more and 100 nm or less. The cemented lens according to claim 2 or 3.

5. the low refractive index layer is a layer formed using the hollow silica particles and a resin material or a metal alkoxide as a component of the binder; The cemented lens according to claim 4 .

6. a base layer formed by laminating one or more thin films made of a transparent material having a refractive index of 1.35 to 2.5 in an optically effective area of ​​the cemented lens; The low refractive index layer is laminated on the underlayer. The cemented lens according to claim 2 .

7. The underlayer is a film produced by a vacuum deposition method, a sputtering method, or an ALD method. The cemented lens according to claim 6 .

8. A cemented lens according to any one of claims 1 to 7, optical system.

9. The cemented lens according to claim 1 ; a light receiving element that receives the light collected by the cemented lens; Equipped with optical equipment.

10. a bonding step of bonding together optically effective regions of a first optical element having a first light-shielding film formed on a non-optically effective region of a substrate and a second optical element having a second light-shielding film formed on a non-optically effective region of the substrate via an adhesive layer; the first light-shielding film is formed only in the non-optically effective area of ​​the first optical element, the second light-shielding film is formed only in the non-optically effective area of ​​the second optical element, The non-optically effective area is an edge surface, In the bonding step, the adhesive layer is exposed on a surface of the first light-shielding film and a surface of the second light-shielding film. A method for manufacturing a cemented lens.

Citation Information

Patent Citations

  • Compound lens

    JP1999064607A

  • Optical element and optical system having the same

    JP2010117472A

  • Composite optical element and imaging optical system

    JP2012252307A

  • Cemented lens

    JP2015108642A

  • Cemented lens, optical system having the same, optical device, and method of fabricating cemented lens

    JP2020024331A