Polyolefin-based extruded resin foam with excellent foamability in which an antiviral phosphate compound is exposed on the surface of the skin layer, and laminate using said polyolefin-based extruded resin foam

Exposing phosphate compounds like zirconium phosphate or hydroxyapatite with silver ions on the skin layer of extruded polyolefin resin foams addresses the challenge of maintaining foaming and surface quality while ensuring robust antiviral activity and resistance to resin deterioration, enhancing the efficacy of antiviral resin foams.

JP7575285B2Active Publication Date: 2024-10-29FURUKAWA ELECTRIC CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021016769
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-04
Publication Date
2024-10-29
Estimated Expiration
2041-02-04

AI Technical Summary

Technical Problem

Existing extruded polyolefin resin foams with antiviral agents face challenges in maintaining excellent foaming properties and surface quality while preventing resin deterioration, especially when exposed to high expansion ratios, and there is a lack of effective antiviral activity on the skin layer.

Method used

The use of a phosphate compound with antiviral properties, such as zirconium phosphate or a hydroxyapatite composition containing silver or silver ions, is exposed on the surface of the skin layer of the extruded polyolefin resin foam, along with optional surfactants and antioxidants, to maintain foaming properties and enhance antiviral efficacy.

Benefits of technology

The solution provides extruded polyolefin resin foams with excellent foaming properties and surface quality, effective antiviral activity across various expansion ratios, and resistance to oxidative deterioration, ensuring high antiviral efficacy and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575285000001
    Figure 0007575285000001
  • Figure 0007575285000002
    Figure 0007575285000002
  • Figure 0007575285000003
    Figure 0007575285000003
Patent Text Reader

Abstract

To provide an antiviral polyolefin-based extrusion resin foam excellent in surface quality of a foam material without damaging foam formation, and few in oxidation degradation, and a laminate using the same.SOLUTION: A polyolefin-based extrusion resin foam excellent in foam formation includes 0.8-5.0 pts.mass of a phosphate-based compound carried with silver, a silver compound, or a silver ion as an antiviral agent with respect to 100 pts.mass of a polyolefin resin. At least one side surface of the polyolefin-based extrusion resin foam is a skin layer, and the antiviral agent is exposed on the surface of the skin layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyolefin-based extruded resin foam having an antiviral phosphate compound on the surface of a skin layer, which has excellent foamability and surface quality and is free from resin deterioration, and a laminate using the polyolefin-based extruded resin foam.Furthermore, the present invention relates to a polyolefin-based extruded resin foam that has a sufficient antiviral effect not only in the case of a high expansion ratio but also in the case of a low expansion ratio extruded resin foam, does not inhibit foamability, and is capable of preventing oxidative deterioration of the resin. [Background technology]

[0002] Unlike bacteria, viruses do not have cell membranes or ribosomes, and are composed of a protein membrane called an envelope and either DNA or RNA. However, because they are particles with a membrane called an envelope or a shell called a capsid, they cannot replicate themselves by performing their own energy metabolism, as bacteria can.

[0003] Therefore, viruses grow by parasitizing animals, plants, or bacteria. Viruses can be classified into membrane-bound viruses, which have a membrane called an envelope, and membrane-less viruses, and the effects of antiviral agents on viruses can be considered as follows, due to the structural differences between bacteria and viruses as described above.

[0004] In the case of enveloped viruses, the envelope is often made of fat or other materials, so organic surfactants may be effective, but in the case of non-membrane viruses, organic surfactants may not necessarily be effective.

[0005] Specific examples of organic surfactants having antiviral properties include linear alkydobenzenesulfonic acid, alkyl glycosides, alkylamine oxides, benzalkonium chloride, benzethonium chloride, dialkyldimethylammonium chloride, polyoxyalkyl ethers, etc. In addition, organic antiviral agents such as organic surfactants have problems with thermal stability.

[0006] On the other hand, in the case of heavy metal antiviral agents, the following mechanisms are thought to be responsible: For example, the inhibitory effects of heavy metals such as Ag and Cu as antiviral agents are thought to be 1) inhibition of membrane fusion between cells and viruses, in which heavy metal complexes and heavy metal ions bind to the envelope and inhibit membrane fusion with cells, thereby inhibiting binding to the host, and 2) inhibition of replication system enzymes, in other words, heavy metal complexes and heavy metal ions inhibit replication system enzymes.

[0007] Furthermore, Ag ions and Cu ions generate singlet oxygen, which has higher energy than normal triplet oxygen, i.e., they generate so-called active oxygen. The singlet oxygen generated here reacts with water to generate hydroxyl radicals (·OH), which are thought to have an antiviral effect.

[0008] Since antibacterial agents and antiviral agents are closely related, for reference, the inhibitory effects of antibacterial agents are described in Non-Patent Document 1. In summary, Non-Patent Document 1 describes that the mechanism of action of antibacterial agents may include inhibition of cell wall synthesis, inhibition of cell wall synthesis, inhibition of protein synthesis associated with inhibition of translation and transcription of genetic material, inhibition of nucleic acid synthesis, etc.

[0009] Specifically, Non-Patent Document 1 describes that, first, inhibition of cell wall synthesis causes the cell to collapse, as the cell wall plays a role in maintaining the cell's shape and internal osmotic pressure, and that inhibition of cell wall synthesis leads to the collapse of the cell; second, inhibition of cell membrane function causes dysfunction of the cell membrane, which has selective permeability and functions to transport components inside the cell and regulate the components inside the cell, but inhibition of cell membrane function causes macromolecules and ions inside the cell to leak out, resulting in cell damage and cell death.

[0010] Next, Non-Patent Document 1 states that, thirdly, there is the inhibition of protein synthesis accompanying the inhibition of the translation and transcription of genetic material; when an antibacterial agent adheres to bacterial ribosomes, proteins that do not have translation or transcription functions are synthesized, or the ribosomes are destroyed, making protein synthesis impossible and preventing cell growth; and, fourthly, there is the inhibition of nucleic acid synthesis; when an antibacterial agent binds to DNA to form a complex, it blocks the inhibition of mRNA formation and inhibits bacterial growth.

[0011] As mentioned above, viruses can be classified into those that are enveloped in a membrane containing lipids, called an envelope, and those that do not. In the case of membrane-bound viruses, the envelope is mostly composed of lipids, so they can be easily destroyed by treatment with organic antiviral agents such as ethanol, organic solvents, and soap.

[0012] For this reason, while enveloped viruses are generally easy to inactivate, non-enveloped capsid viruses are said to be highly resistant to the above-mentioned treatment agents, and it is believed that antiviral agents different from organic antiviral agents are necessary.

[0013] In the present invention, although it is possible to use an organic antiviral agent, the study will focus on a polyolefin-based extruded resin foam with an exposed skin layer having antiviral properties, and a laminate of the polyolefin-based extruded resin foam, which mainly uses an inorganic antiviral agent using a metal ion.

[0014] Patent Document 1 discloses an invention relating to expandable resin particles containing an inorganic antibacterial agent having an average particle size of 0.1 to 2.0 μm. Patent Document 1 also describes an antibacterial synthetic resin foam molded product obtained by pre-expanding the antibacterial expandable microparticles and then subjecting them to secondary expansion molding.

[0015] Furthermore, the molded article of Patent Document 1 has the same antibacterial properties even on the sliced ​​surface after secondary processing of the skin layer and the inside of the foam layer. It is described that the expandable microparticles contain 0.01 to 5.0 parts by mass of a metal ion-based antibacterial agent and 0.01 to 2.0 parts by weight of hardened oil per 100 parts by mass of the expandable microparticles, the metal ions are supported on zirconium phosphate, and it is further described that the expandable microparticles preferably contain a fatty acid ester.

[0016] Patent Document 2 describes a foamed sheet having at least one surface coated with an organic specific compound selected from the group consisting of palmityl diethanolamine, stearyl diethanolamine, glycerin monolaurate, and glycerin monocaprate in an amount of 0.002 to 0.05 (g / m 2 ) is laminated on an antibacterial thermoplastic resin foam sheet.

[0017] In addition, the film laminated on the foamed sheet in Patent Document 2 is laminated after foaming, and the foamed sheet has an expansion ratio of 2 times, a foam thickness of 1 mm, and the laminated film is a thin material with a thickness of about 30 to 40 μm, and is a biaxially oriented multilayer film.

[0018] Patent Document 3 relates to an antiviral agent, a resin composition, and an antiviral product, and describes an antiviral agent containing an inorganic solid acid having an acid site concentration of more than 0.005 mol / g, the inorganic solid acid containing silver, copper, or any one of these compounds in addition to an inorganic phosphate compound, an inorganic silicic acid compound, or an inorganic oxide, and a resin composition containing this antiviral agent. Furthermore, Patent Document 3 describes that the acid strength (pKa) of the acid site in the inorganic solid acid is preferably 3.3 or less.

[0019] Furthermore, in Patent Document 3, the antiviral agent is sprayed or painted onto textile products such as clothing, bedding, and masks, filters used in air purifiers and air conditioners, interior products such as curtains, carpets, and furniture, and automobile interior materials, or is spread onto the surface layers of building materials such as wallpaper and flooring materials, thereby imparting the effect of reducing viral activity.

[0020] Patent Document 4 describes an antimicrobial member in which a cured binder containing an antimicrobial component is fixed to a substrate surface, and the cured binder is formed on the substrate surface, and the substrate surface has a gloss level according to JIS Z8741 of 45% or more and less than 100%.

[0021] Furthermore, Patent Document 4 describes inorganic antimicrobial agents such as silver, copper, zinc, platinum, zinc compounds, silver compounds, copper compounds, metal oxide catalysts carrying metals or metal oxides, zeolites ion-exchanged with metal ions, and copper complexes.

[0022] Patent Document 4 describes an antimicrobial member in which the organic antimicrobial agent is at least one selected from the group consisting of antimicrobial resins, sulfonic acid surfactants, copper alkoxides, and bis-type quaternary ammonium salts, and Patent Document 4 describes that the binder cured material includes a binder cured material composed of an organic binder, an inorganic binder, and an organic-inorganic hybrid binder.

[0023] Patent Document 5 describes the provision of an antibacterial zeolite that is unlikely to cause discoloration over time even when contained in a resin or the like, and an antibacterial zeolite containing the antibacterial zeolite, and further describes an antibacterial zeolite in which some or all of the ion-exchangeable ions in the zeolite are replaced with hydrogen ions and silver ions, and an antibacterial resin composition containing 0.05 to 80 mass % of the antibacterial zeolite.

[0024] Furthermore, Patent Document 5 describes an antibacterial zeolite in which the ion-exchangeable metal ions of zeolite are replaced with antibacterial metal ions such as silver, copper, and zinc, and an antibacterial composition containing the same, in which the zeolite contains silver ions and ammonium ions to solve the problem of discoloration over time that is a characteristic of antibacterial zeolite.

[0025] Patent Document 6 discloses a virus inactivation sheet capable of inactivating attached viruses, which is characterized by comprising a sheet body and monovalent copper compound microparticles and / or iodide microparticles held by the sheet body.

[0026] Patent Document 6 describes a virus inactivation sheet in which the monovalent copper compound microparticles are at least one selected from the group consisting of chlorides, acetates, sulfides, iodides, bromides, peroxides, oxides, and thiocyanides, and further describes a virus inactivation sheet in which the iodide microparticles contain a large number of iodide particles.

[0027] The inactivation sheet of Patent Document 6 describes that the monovalent copper compound microparticles and / or iodide microparticles are held on the sheet body via a group of other inorganic microparticles that are fixed to the sheet body by chemical bonds with silane monomers and / or polymers of silane monomers.

[0028] An antiviral agent was kneaded into the resin foam to impart antiviral properties, but because a non-foamed layer known as the skin layer exists on the surface of the foam, the antiviral agent particles are present in the non-foamed layer on the surface of the foaming agent and are therefore difficult to expose, making it impossible to obtain a sufficient antiviral effect.

[0029] Furthermore, in the case of Patent Document 1, the invention requires a binder to apply and fix an antibacterial agent to expandable resin particles as a raw material, and furthermore, the antibacterial expandable microparticles are pre-expanded and then secondary foamed to produce an antibacterial synthetic resin foam molded body, so the molded body of Patent Document 1 is a secondary molded body made from antibacterial expandable microparticles as a raw material and does not have a skin layer. Therefore, it is not a continuously molded extruded foam having a skin layer in which an antiviral agent is directly kneaded into a base resin as in the present invention. It is based on a technical idea different from that of the present application, which is directed to an antiviral agent exposed on the surface of the skin layer of a foam.

[0030] Patent Document 2 discloses an antibacterial thermoplastic resin foam sheet laminated with a film, but the foam itself is not endowed with antibacterial or antiviral properties. The antiviral agent, resin composition, and antiviral product of Patent Document 3 do not impart antiviral activity to the surface of the skin layer of a resin foam.

[0031] Patent Document 4 discloses organic antiviral agents, inorganic antiviral agents, hybrid antiviral agents, and ion-exchanged zeolites as antiviral agents, but these do not impart antiviral properties to the skin layer of a resin foam. Patent Document 5 discloses a composition containing antibacterial zeolite that contains antibacterial metal ions such as silver, copper, and zinc, and Patent Document 6 describes a virus inactivation sheet that contains monovalent copper compound particles or iodide particles, but none of these impart antiviral properties to the surface of the skin layer of a resin foam. [Prior art documents] [Patent documents]

[0032] [Patent Document 1] Japanese Patent Application Publication No. 11-335481 [Patent Document 2] JP 2015-48391 A [Patent Document 3] International Publication No. 2017 / 150063 [Patent Document 4] JP 2020-083779 A [Patent Document 5] International Publication No. 2007 / 037195 [Patent Document 6] International Publication No. 2011 / 040048 [Non-patent literature]

[0033] [Non-Patent Document 1] Yasuhiro Iwasawa, "Interface Handbook," NTS Publishing, September 2001 Summary of the Invention [Problem to be solved by the invention]

[0034] As described above, there has been no sheet-shaped polyolefin-based extruded resin foam containing a heavy metal as an antiviral agent produced by extrusion foaming up to now that is excellent in both antiviral effect and foamability and does not deteriorate the resin. The present invention has been made in consideration of such facts, and aims to provide a polyolefin-based extruded resin foam in which a phosphate-based compound having antiviral properties, excellent foamability and surface quality, and little effect on resin deterioration is exposed on the surface of the skin layer, and a laminate using the polyolefin-based extruded resin foam. In the present invention, excellent foamability means both that a desired expansion ratio is obtained without foaming inhibition and that the surface properties of the obtained foamed product are excellent. As specific characteristics, the two are specified separately.

[0035] In the present invention, in addition to the antiviral agent of the present invention, a surfactant, an antioxidant, and the like can be contained in predetermined amounts as necessary. However, it is an object of the present invention to reduce the amount of a surfactant added even when it is used, and further to use no antioxidant as much as possible, or to use only a trace amount of an antioxidant, if any.

[0036] The skin layer of the polyolefin extruded resin foam of the present invention can be laminated with another polyolefin extruded resin foam so that the thickness of the extruded resin foam can be adjusted according to the product application. In addition, since the present invention utilizes the surface exposure effect of the antiviral agent in the skin layer, it can be suitably used not only in the case of a low expansion ratio of 10 times or less, but also in the case of an extruded resin foam with a high expansion ratio of more than 10 times, such as 20 to 40 times, and the higher the expansion ratio, the more improved the antiviral effect tends to be. [Means for solving the problem]

[0037] The polyolefin extruded resin foam of the present invention is a polyolefin extruded resin foam containing, as an antiviral agent, silver or a silver compound or a phosphate-based compound carrying silver ions in the range of 0.8 to 5.0 parts by mass relative to 100 parts by mass of polyolefin resin, and is characterized in that at least one surface of the polyolefin extruded resin foam is a skin layer, and the antiviral agent is exposed on the surface of the skin layer. The content of the antiviral agent is preferably 1.0 to 4.0 parts by mass in total relative to 100 parts by mass of the polyolefin extruded resin. The resin foam of the present invention is a polyolefin extruded resin foam with excellent foamability and surface quality and little effect on resin deterioration.

[0038] The phosphate-based antiviral agent contained in the polyolefin-based extruded resin foam desirably contains at least one of zirconium phosphate carrying silver or a silver compound by ion exchange, and a phosphate compound having a hydroxyapatite composition containing calcium / zinc carrying silver or silver ions by ion exchange.

[0039] The base resin of the polyolefin-based extruded resin foam may be low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, very low-density polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-methyl acrylate copolymer, or ethylene-ethyl acrylate copolymer. The polyolefin-based extruded resin foam may be characterized by being made of at least one of these or a mixture of two or more of these blended together.

[0040] The extruded polyolefin resin foam may contain 0.5 to 2.0 parts by mass of a surfactant in addition to the antiviral agent. By adding a surfactant to the extruded polyolefin resin foam, the dispersibility of the antiviral agent is improved, and the activity value, which is an index of antiviral properties, is improved. Thus, a surfactant may be added, but since at least sufficient antiviral properties can be obtained even with a composition containing only the antiviral agent, a surfactant may not be added. The preferred range of the surfactant is 0.8 to 2.0 parts by mass.

[0041] The polyolefin-based extruded resin foam preferably does not contain an antioxidant, but may contain 0.05 to 1.0 parts by mass of an antioxidant in addition to the antiviral agent. The content of the antioxidant is preferably 0.1 to 0.8 parts by mass, taking into account the influence of foaming inhibition, etc.

[0042] It is desirable that the laminate is formed by laminating another polyolefin-based extruded resin foam to the surface of the polyolefin-based extruded resin foam, and that at least one skin layer is exposed to the surface of the laminate.

[0043] The extruded polyolefin resin foam preferably contains, as an antiviral agent, at least one of zirconium phosphate having silver or a silver compound supported by ion exchange; or a phosphate compound having a hydroxyapatite composition containing calcium / zinc having silver or silver ions supported by ion exchange, in an amount in the range of 0.8 to 5.0 parts by mass per 100 parts by mass of polyolefin resin, and at least one skin layer of the extruded polyolefin resin foam has a thickness of 100 μm or less, and the extruded polyolefin resin foam has excellent foaming properties in which the antiviral agent is exposed on the surface of the skin layer.

[0044] In the present invention, since the object is to expose the antiviral agent on the skin layer of the extruded polyolefin resin foam, the antiviral agent used in the present invention is mainly composed of an inorganic antiviral agent, but the antiviral agent used may be an organic antiviral agent or a hybrid antiviral agent containing both organic and inorganic systems.

[0045] (Base resin for polyolefin-based extruded resin foam) Examples of the base resin for the polyolefin-based extruded resin foam in the present invention include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, very low-density polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-methyl acrylate copolymer, and ethylene-ethyl acrylate copolymer, and these can be used alone or as a mixture of two or more types blended together.

[0046] (Antiviral Agents) The antiviral agent in the present invention includes inorganic antiviral agents and organic antiviral agents. Inorganic antiviral agents are preferred from the viewpoint of thermal stability. Inorganic antiviral agents do not decompose even when exposed to high temperatures during kneading and molding when obtaining a polyolefin-based extruded resin foam, and can impart sufficient antiviral properties to the foam. The antiviral agent of the present invention uses a silver-containing phosphate-based antiviral agent as a silver-based inorganic antiviral agent that does not contain copper, in order to suppress the promotion of resin deterioration without inhibiting the foamability of the resin. This is because heavy metals, particularly copper, have the effect of promoting thermal deterioration of polyolefin resins.

[0047] In particular, as a phosphate-based antiviral agent, an antiviral agent in which either a metal-based antiviral agent is supported on a phosphate-based compound, such as zirconium phosphate supported by silver or a silver compound through ion exchange, or a phosphate compound having a hydroxyapatite composition containing calcium / zinc supported by silver or silver ions, is used.

[0048] If the content of the antiviral agent is too low, the antiviral properties are weak, and if it is too high, the generation of bubbles during foaming becomes unstable, which may make it difficult to obtain a foam with a high expansion ratio or cause the foam to be easily burned at its ends. If the content of the antiviral agent is high, the antiviral agent is more likely to aggregate and the cost increases. The content of the antiviral agent is preferably 0.8 to 5.0 parts by mass relative to 100 parts by mass of the polyolefin resin. Within this range, it is easy to achieve both antiviral properties and good foams. It is more preferably 1.0 to 4.0 parts by mass.

[0049] (silver or silver compound ion-exchanged zirconium phosphate) Supports in which compounds carrying silver, copper, zinc, or the like are used as antiviral agents include various inorganic solid acids. Particularly representative ones include those using zirconium phosphate, those using phosphate ceramics, those carrying the compound on glass, and those using magnesium aluminosilicate or clay minerals.

[0050] In the present invention, the content of zirconium phosphate carrying silver or a silver compound is set to 0.8 to 5.0 parts by mass. The reason for this is that a predetermined antiviral effect can be obtained even with a content of 5.0 parts by mass, and if the content is 5.0 parts by mass or more, the generation of bubbles becomes unstable and at the same time, the dispersibility decreases, and the product cost of the resin foam increases. Considering the balance of these properties, the upper limit of the content of zirconium phosphate is preferably 5.0 parts by mass. Furthermore, although an antiviral effect is observed when the content is less than 0.8 parts by mass, the antiviral effect is weak, so it is preferable that the content is 0.8 parts by mass or more. Therefore, in order to obtain a stable antiviral effect and further consider the cost balance, the content of zirconium phosphate is preferably 1.0 to 4.0 parts by mass.

[0051] As an inorganic solid acid, a material containing at least one of silver, copper, and their compounds in addition to zirconium phosphate as an inorganic oxide can be used as an antiviral agent. Specifically, it is possible to use hexagonal zirconium phosphate, which is an inorganic ion exchanger, which supports silver ions by ion exchange.

[0052] Zirconium-centered oxygen octahedra and phosphorus-centered oxygen tetrahedra are linked three-dimensionally with oxygen sharing, and silver ions exist in the cavities of the framework. Here, for example, to obtain zirconium phosphate carrying silver, first, a zirconium oxychloride aqueous solution of a predetermined concentration is added to a phosphoric acid aqueous solution of a predetermined concentration, and the mixture is aged at 100°C for 12 hours, and then the resulting precipitate is washed with water and dried to recover zirconium phosphate.

[0053] Next, this zirconium phosphate precipitate was stirred in an aqueous silver nitrate solution at 100° C. for 2 hours. The precipitate obtained was then filtered, washed with water, dried and crushed to obtain an α-type zirconium phosphate powder containing a predetermined amount of white silver. In addition to silver nitrate, aqueous solutions of silver sulfate, silver perchlorate, silver acetate, diamine nitrate, diamine sulfate, etc. can be used.

[0054] In the present invention, as a zirconium phosphate-based antibacterial agent carrying silver or a silver compound, Toa Gosei's Novaron IV1000 was used. The average particle size of Novaron IV1000 is 1 to 2 μm, and the weight of Ag carried on the zirconium phosphate is about 10% by weight of the weight of the zirconium phosphate.

[0055] (A phosphate compound containing calcium and zinc carrying silver or silver ions) Similarly, instead of zirconium phosphate, a compound in which silver or silver ions are supported on a phosphate compound in which calcium and zinc are combined may be used as the antiviral agent. The composition of this antiviral agent is a phosphate compound in which calcium and zinc are combined, and has a hydroxyapatite composition represented by the following formula (1). (1)Ag-CaαZnβAlγ(PO4)δ(OH)2

[0056] The phosphate compound having a hydroxyapatite composition carrying Ag is produced as follows. First, a crude reaction is carried out to synthesize a phosphate compound having a calcium and zinc complex using calcium hydroxide, zinc oxide, aluminum hydroxide, and phosphoric acid as raw materials. Next, silver nitrate is added and a mechanochemical reaction is carried out using a ball mill to carry out silver ions at the acid sites of the phosphate compound, after which the product is washed and filtered, and pulverized to obtain a fine powder of a specified size.

[0057] The amount of Ag supported by this material is 10% by weight of the phosphate compound. The average particle size of this material can be 1 μm or less. Here, the content of the phosphate compound complexed with calcium and zinc as an antiviral agent relative to 100 parts by mass of the base resin is 0.8 to 5.0 parts by mass, and preferably 1.0 to 4.0 parts by mass. The reasons for specifying these numerical values ​​are the same as those for zirconium phosphate.

[0058] (Surfactant) The extruded polyolefin resin foam of the present invention may contain a surfactant together with the base resin and the antiviral agent. In the present invention, the surfactant is allowed to be contained in an amount of 0.5 to 2.0 parts by mass. The preferable range of the surfactant is 0.8 to 2.0 parts by mass.

[0059] Here, by including a surfactant in the resin, it is possible to impart hydrophilicity to the surface of the hydrophobic resin, as compared with the case of the resin alone. In addition, the surfactant is expected to have the effect of improving the dispersibility of the antiviral agent.

[0060] Here, the reason for adding a surfactant to the base resin is as follows. The surface of the resin foam, which is the base material according to this embodiment, is generally hydrophobic. If it remains hydrophobic, regardless of the type of genome or the presence or absence of an envelope, the antiviral agent will not easily come into contact with and adhere to the surface of the virus. Therefore, by changing the surface property of the resin foam constituting the antiviral / antibacterial layer from hydrophobic to hydrophilic, the virus will be more likely to be adsorbed to the antiviral layer. The surfactant used may be anionic, cationic, or nonionic. In the present invention, calcium stearate can be used as the anionic surfactant, and Rikemal S-100, a glycerin fatty acid ester type from Riken Vitamin, can be used as the nonionic surfactant. In addition, Rheomix HT flakes manufactured by Lion Corporation can also be used as the cationic surfactant.

[0061] (Crosslinking agent) The crosslinking agent adjusts the viscosity of the resin in the molten state during foaming to ensure a stable foaming state. Examples of organic peroxides used as crosslinking agents include dicumyl peroxide, 2,5-dimethyl-2,5-di-(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(t-butylperoxy)hexyne-3, α,α'-bis(t-butylperoxydiisopropyl)benzene, t-butylperoxycumene, 4,4'-di(t-butylperoxy)valeric acid n-butyl ester, 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-butylperoxy)cyclohexane, and di-t-butyl peroxide.

[0062] If the amount of organic peroxide is small, the strength of the cell membrane is small and it is difficult to form closed cells during foaming, and if the amount of organic peroxide is large, the growth of the cell membrane is inhibited and only a foam with a low expansion ratio can be obtained. In the present invention, an organic peroxide is used as a crosslinking agent, and the amount of the organic peroxide used as a foaming agent is usually 0.3 to 2.0 parts by mass, preferably 0.5 to 1.5 parts by mass, per 100 parts by mass of polyolefin resin, but since it is closely related to the content of the foaming agent, the amount of the crosslinking agent may be determined in consideration of the content of the foaming agent. As the crosslinking agent, for example, dicumyl peroxide can be suitably used.

[0063] (foaming agent) In the present invention, the foaming agent may be an inorganic foaming agent, but it is preferable to use an organic pyrolytic foaming agent that decomposes when heated to generate gas.

[0064] Examples of such foaming agents that can be used include azodicarbonamide (ADCA), oxybisbenzenesulfonylhydrazide (OBSH), N,N'-dinitrosopentamethylenetetramine (DPT), p-toluenesulfonylhydrazide, benzenesulfonylhydrazide, diazoaminobenzene, N,N'-dimethyl-N,N'-dinitroterephthalamide, azobisisobutyronitrile, etc. These can be used alone or in combination of two or more.

[0065] In particular, when at least one selected from the group consisting of azodicarbonimide, N,N'-dinitrosopentamethylenetetramine, and oxybisbenzenesulfonylhydrazide is used in a predetermined amount, a foam with a high expansion ratio can be easily obtained. The amount of the foaming agent is preferably in the range of 5 to 40 parts by mass relative to 100 parts by mass of the polyolefin resin, and the amount of the foaming agent added may be determined in consideration of the resin material and the expansion ratio, and the amount of the foaming agent added is more preferably in the range of 10 to 40 parts by mass. In particular, azodicarbonamide (ADCA) is particularly preferably used as the foaming agent.

[0066] (Antioxidants, stabilizers, weatherproofing agents) The polyolefin-based extruded resin foam of the present invention is preferably not using an antioxidant or, if used, in a small amount, since the antioxidant has a tendency to inhibit foaming of the resin foam, but may contain a small amount of an antioxidant, light stabilizer, weathering agent, etc., as necessary. In particular, when the antiviral agent to be blended is an antiviral agent containing a metal compound, there is a possibility of oxidative deterioration and foaming inhibition of the extruded foam resin, which is the base material, so it is preferable to use an antiviral agent that is less likely to cause oxidative deterioration and foaming inhibition. The extruded resin foam of the present invention is an extruded resin foam containing an antiviral agent that is less likely to cause oxidative deterioration and foaming inhibition, and does not necessarily need to use an antioxidant, but may be used in a small amount.

[0067] Adding an antioxidant can prevent the base resin constituting the foam from being oxidized and deteriorated. Antioxidants include phenol-based antioxidants, phosphite-based antioxidants, blended antioxidants that are a blend of phenol-based antioxidants and phosphite-based antioxidants, and thioether-based antioxidants.

[0068] Examples of antioxidants that satisfy the above requirements include hindered phenol-based antioxidants and hindered amine-based compounds. The above antioxidants have effects as stabilizers or weather resistance agents in addition to their effects as antioxidants. For example, in the present invention, specifically, Irganox 1010 manufactured by BASF is used as tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane.

[0069] The content of the antioxidant is preferably 0.05 to 1.0 parts by mass relative to 100 parts by mass of the polyolefin resin. If the content of the antioxidant is too high, crosslinking of the base resin is inhibited and the viscosity is reduced, so that the bubble diameter becomes large, which may lead to gas escape and a reduction in the expansion ratio. Therefore, it is preferable not to add the antioxidant in an amount exceeding 1.0 part by mass.

[0070] Next, we will look at the effect of antioxidants on the foaming process. In the foaming process, the balance between the crosslinking reaction caused by peroxides and the gas generation caused by the decomposition of the foaming agent is important, and antioxidants have an effect on this process. The crosslinking reaction begins when peroxides decompose due to heat, generating radicals that attack the polyethylene molecular chains and pull out hydrogen molecules. In contrast, antioxidants are added to suppress the deterioration of resins. Resin deterioration is also caused by a radical chain reaction involving resin and oxygen, and antioxidants trap these radicals and inactivate them, preventing deterioration.

[0071] Therefore, if a large amount of antioxidant is contained in the resin, the radicals derived from the peroxide generated to cause the crosslinking reaction are inactivated by the antioxidant. Therefore, the crosslinking reaction as intended is inhibited. As a result, the degree of crosslinking required to realize a normal foaming process, that is, the effect of adjusting the viscosity of the polyethylene resin by crosslinking, is inhibited, and the foaming process proceeds without obtaining an appropriate resin viscosity, resulting in the problem that a stable foam with the desired expansion ratio cannot be obtained.

[0072] Therefore, when an antioxidant is added, the upper limit of the content within the range that does not inhibit crosslinking is preferably 0.8 parts by mass or less. Since the antioxidant is effective even in a small amount, it is sufficient to include 0.05 parts by mass or more, but if the amount is less than this, the antioxidant's effect is insufficient, so the antioxidant needs to be included in an amount of at least 0.05 parts by mass or more, but it is preferable to appropriately adjust the amount within the above range depending on the type of antioxidant and the use of the polyolefin foam. The antioxidant may be an antioxidant that has metal inactivation ability.

[0073] (Addition of flame retardants and other additives to resin foams) The resin foam of the present invention may further contain other additives such as flame retardants, lubricants, pigments, dyes, plasticizers, fillers, metal deactivators, and antistatic agents, depending on the purpose, as long as they do not inhibit foaming. For example, adding a flame retardant to the resin foam can impart flame retardancy, and adding an inorganic pigment or the like can impart design and design properties. Known commercially available additives can be used as these additives.

[0074] Examples of the flame retardant include metal hydroxides, phosphorus-based flame retardant stabilizers, halogen-based flame retardants, etc. In order to improve flame retardancy, resins such as ethylene-based copolymers such as ethylene-vinyl acetate copolymers and ethyl acrylate copolymers may be included. Although detailed descriptions of the metal hydroxides, phosphorus-based flame retardant stabilizers, and halogen-based flame retardants are omitted, known flame retardants can be appropriately used in combination.

[0075] In addition, the polyolefin-based extruded resin foam of the present invention may contain oil components and various additives to improve processability. Examples of such additives include paraffin, modified polyethylene wax, stearates, hydroxystearates, vinylidene fluoride-hexafluoropropylene copolymers, and organic modified siloxanes. The polyolefin-based extruded resin foam of the present invention may contain various pigments, dyes, and carbon black. Furthermore, titanium oxide may be contained. Titanium oxide contributes to improving antiviral properties and weather resistance. There are no particular restrictions on the amount of additives such as flame retardants added to the resin foam as long as they do not affect antiviral properties or foamability, but considering the effects on other mechanical properties of the foam, it is preferable to add as little as possible as long as the purpose of adding them is achieved.

[0076] (Method of manufacturing resin foam containing antiviral agent) The resin foam of the present invention can be obtained by adding a foaming agent and a crosslinking agent to a polyolefin resin, and extruding and foaming under predetermined conditions to obtain a resin foam having closed cells with a high expansion ratio. A crosslinking assistant may be added as necessary. In the present invention, in order to obtain a resin foam having antiviral properties, it is necessary to add a predetermined amount of a predetermined antiviral agent or surfactant to the base resin as necessary, and change the contents of the foaming agent, crosslinking agent, etc. according to the expansion ratio of the extruded polyolefin resin foam.

[0077] For example, when the base resin is a low-density polyolefin, the foaming agent and crosslinking agent contents are 11 parts by mass and 0.9 parts by mass, respectively, for 100 parts by mass of the base resin when the expansion ratio is 20 times, and 16 parts by mass and 0.8 parts by mass, respectively, for 100 parts by mass of the base resin when the expansion ratio is 40 times. The polyolefin-based extruded resin foam of the present invention has an average cell diameter, excluding the skin layer, of 200 μm to 1500 μm, preferably 400 μm to 800 μm. The thickness of the skin layer varies depending on the expansion ratio, but is, for example, about 5 μm to 200 μm.

[0078] In the present invention, a masterbatch may be used to produce an extruded polyolefin resin foam containing an antiviral agent, or pellets obtained by compounding a base resin and an antiviral agent may be used, or a direct blending method in which the antiviral agent is directly blended may be used; however, production by the masterbatch method or compound method is preferable because a stable dispersed state is more likely to be obtained during product molding.

[0079] To make a masterbatch, the antiviral agent is mixed with a resin and a surfactant, antioxidant, etc., which will be described later, and then kneaded and granulated at a high concentration into the polyolefin resin in a twin-screw or single-screw kneading extruder.The masterbatch is usually transported forward by a screw, where it is plasticized, homogenized, pressurized, and made uniform.

[0080] The molten resin containing the antiviral agent homogenized in the kneading extruder is extruded through a die of the extrusion head into strands, which are then cut to obtain masterbatches. In this case, for example, if the number of parts of the antiviral agent blended is 20 parts per 100 parts of polyolefin resin, a masterbatch can be produced containing 20 parts of antiviral agent particles. In this case, it is necessary to manage the concentration of the masterbatch very carefully.

[0081] In the compound method, additives such as antiviral agents, resins, and surfactants may be added as necessary. Phosphate-based compounds are stable as a result of thermal analysis, so antioxidants are not necessarily required, but in some cases, antioxidants can be added in small amounts to the resin within a specified range. After mixing these additives with the resin, the mixture is kneaded and extruded to prepare a pellet-shaped compound as a preform. This compound is used to manufacture a resin foam by extruding and foaming.

[0082] In the polyolefin-based extruded resin foam of the present invention, additives such as an antiviral agent and a surfactant may be added to the base resin depending on the purpose. These additives can be melt-kneaded with the base resin and extruded, and crosslinked and foamed at the same time during extrusion.

[0083] In this method, a resin composition obtained by compounding a polyolefin resin with additives such as an antiviral agent, a surfactant, and an antioxidant, as well as an organic decomposition type foaming agent and a crosslinking agent, is kneaded in a kneading machine such as a pressure kneader or a two-roll mixer, and extruded into a foaming base sheet of desired thickness and width in an extruder. The resulting mixture is then introduced into a heating furnace at about 200 to 230°C for foaming.

[0084] Here, as the antiviral agent, it is preferable to use an inorganic compound containing heavy metals in some form, such as zirconium phosphate ion-exchanged with silver or a silver compound, or a phosphate compound in which calcium and zinc carrying silver or silver ions are combined. Of course, organic antiviral agents can also be used as necessary. Here, zeolite carrying silver or copper by ion exchange promotes foaming and resin deterioration as described below, so although there is no problem with its antiviral properties, its use is undesirable.

[0085] (Formation of cell structure in resin foam and distribution of antiviral particles in the skin layer) The surface of the extruded sheet-shaped resin foam has a predetermined bubble diameter depending on the type of base resin and the expansion ratio. A non-foamed layer called a skin layer is formed near the surface of the sheet-shaped resin foam. A foamed bubble structure is observed in the rest of the sheet. The size of the bubbles near the center and near the surface in the thickness direction of the sheet is generally slightly larger near the center than near the surface.

[0086] Here, let us consider the distribution of the antiviral agent inside the foam of the present invention. In this case, since the antiviral agent is three-dimensionally dispersed approximately evenly in the thickness direction and the planar direction before foaming, the manifestation of the antiviral effect of the antiviral agent is premised on contact with the virus, and therefore only the antiviral agent exposed on the surface of the resin foam can manifest the antiviral effect. The base resin before foaming is in a bulk state, but during foaming, the bubble walls receive the pressure of the gas in the bubbles from both sides, and each bubble wall becomes thinner as the bubbles grow, and the growth of the bubbles stops at a predetermined bubble diameter where the pressure in the bubbles and the deformation resistance of the resin are balanced, thereby forming a predetermined bubble structure.

[0087] In contrast, in the skin layer, crosslinking proceeds faster than in the internal foam layer during the heating step in the crosslinking and foaming process of the foam, so foaming is inhibited and foaming does not occur or occurs only slightly. Even if foaming occurs inside the skin layer, the gas foamed inside the skin layer escapes to the surface of the skin layer due to the pressure of the gas foamed in the foam layer, and re-fuses, resulting in a layer that does not have bubbles formed on the surface of the extruded resin foam.

[0088] Here, the skin layer is thinned by biaxially stretching the skin layer in a state where the skin layer is constrained by the foam layer at the interface between the skin layer and the foam layer and is subjected to a pressing force toward the surface of the skin layer. At this time, the antiviral agent particles move in the thickness direction as the spacing between the antiviral agent particles increases in the surface direction and the skin layer is thinned. At this time, since the skin layer is close to the foaming temperature and the resin has a certain level of viscosity, the antiviral agent particles move relatively toward the surface direction of the skin layer while maintaining a state in which they are not easily dropped off.

[0089] In this case, even if the particles do not actually move in the thickness direction, the antiviral agent particles appear to move toward the surface due to the thinning of the skin layer, and furthermore, because the interfacial free energy of the surface of the skin layer is lower than that of the interior of the skin layer, it is understood that the antiviral agent particles actually tend to move toward the surface of the skin layer. Furthermore, even if the viscosity of the resin is high during the foaming process and the antiviral agent particles move close to the surface, they hardly fall off due to the viscosity of the polyethylene resin that constitutes the resin film.

[0090] This means that the antiviral agent particles kneaded into the base resin before foaming have a larger effect of increasing the probability distribution density of the number of antiviral agent particles on the surface of the skin layer when the skin layer is formed than the probability density inside the skin layer. Therefore, the present invention can be suitably used not only in the case of a low expansion ratio of 10 times or less, but also in the case of a high expansion ratio of 20 to 40 times more than 10 times. In addition, the pressing force pressing the skin layer toward the surface and the driving force for biaxially stretching the skin layer during the foaming process are such that the spacing between particles becomes somewhat larger when the expansion ratio is higher, but the effect of increasing the surface density in the thickness direction on the skin layer surface inside the skin layer becomes larger when the expansion ratio is higher.

[0091] Regarding the skin layer thickness during the foaming process, the skin layer tends to become thinner as the foaming ratio increases. When the foaming ratio is 10 or less, the skin layer is more than 100 μm thick, but when the foaming ratio is between 10 and 40, the skin layer is usually 5 μm to 100 μm thick, and the skin layer tends to become thinner at an accelerated rate as the foaming ratio increases. Here, the reason why the skin layer becomes thinner as the expansion ratio increases is thought to be that as the expansion ratio increases, the relative thickness of the foamed layer to the skin layer when viewed in the plate thickness direction increases, while the thickness of the skin layer formed by gas escape from the bubbles becomes relatively thinner, and this is combined with the thinning effect of the skin layer due to the biaxial stretching effect on the surface of the foam during expansion.

[0092] Thus, for a material using Novalon, the foam was cut in the thickness direction, and the numerical distribution of the antiviral agent particles in the skin layer on the surface of the foam was observed under a scanning electron microscope. The results confirmed that the number of antiviral agent particles near the surface of the skin layer was greater than that near the surface of the foam skin layer when comparing the area other than the area near the surface of the skin layer.

[0093] As described above, it was confirmed that the probability density of the presence of antiviral agent particles increases when the skin layer of the foam is thinned and microscopically stretched during foaming. Here, because the above results are the relationship between the foaming behavior of the resin foam and dispersed antiviral agent particles, it is thought that a similar relationship would hold unless the size of the antiviral agent particles changes drastically.

[0094] (Foam Rolling) In a typical mass production process, the extruded resin foam is then rolled with one or more rolls while applying tension to the product in order to adjust the surface condition and dimensions. This causes the bubbles to change from a roughly isotropic state to a slightly flattened shape in the rolling direction. During this process, the foam also stretches in its entire length. The rolling rate is usually set in the range of 5% to 15%.

[0095] Looking at the changes in bubble structure due to roll rolling and the effects on the skin layer, when bubbles are flattened by roll rolling, it is thought that the flattening occurs because the extension angles of the bubble walls at the triple and quadruple junctions, which are the boundaries between the bubble walls, undergo plastic deformation and change in shape due to stress concentration caused by shear strain during roll rolling. However, if the rolling is light in order to smooth the surface, much of the rolling amount elastically recovers immediately after rolling, so there is no significant effect on the surface properties of the skin layer or the shape of the bubbles.

[0096] Regarding the state of the skin layer after rolling, the skin layer near the surface becomes slightly thinner by passing through the rolls, but the foamed layer recovers elastically after passing through the rolls, so it only flattens and expands very slightly, and there is almost no effect on the thickness of the skin layer or the shape of the bubbles. Also, taking into account the elastic recovery after rolling, the degree of thinning of the skin layer becomes smaller than the set value of the rolling ratio of the rolls. Effect of the Invention

[0097] The present invention makes it possible to provide a polyolefin-based extruded resin foam in which silver or a silver compound or a phosphate-based compound carrying silver ions is exposed on the surface of a skin layer as an antiviral agent having antiviral properties that are excellent in surface quality of the foamed material and cause almost no oxidative deterioration of the resin without inhibiting foamability, and a laminate using the polyolefin-based extruded resin foam. In the present invention, in addition to the antiviral agent of the present invention, a surfactant, an antioxidant, etc. can be contained in predetermined amounts as necessary.

[0098] A laminate can be obtained by laminating another polyolefin-based extruded resin foam on the surface of the polyolefin-based extruded resin foam, and at least one skin layer can be exposed on the surface of the laminate. In addition, since the present invention utilizes the exposure effect of the antiviral agent on the skin layer surface, it can be suitably used not only in the case of a low expansion ratio of 10 times or less, but also in the case of an extruded resin foam with a high expansion ratio of more than 10 times, such as 20 to 40 times, but in consideration of the exposure effect on the skin layer surface, the thickness of the skin layer is preferably 100 μm or less, and more preferably 70 μm or less. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS EXAMPLES

[0099] In the present invention, not only the antiviral properties of the oil foam containing the antiviral agent were evaluated, but also the long-term stability of the resin against oxidative degradation was evaluated in addition to the foamability, since the antiviral agent contains heavy metal ions or heavy metal compounds, and there is a concern of foaming inhibition and oxidative degradation of the base resin. The antiviral properties were evaluated based on the activity value in accordance with ISO21702, the foamability was evaluated based on the expansion ratio and the expansion ratio and surface properties of the foam, and the long-term stability of the resin against oxidative degradation was evaluated by a thermal analysis test on a material of a specified composition when the content of the antiviral agent was 5 parts by mass. Details of the test method will be described later.

[0100] The present invention will be described in further detail below with reference to examples. (Example) The base resin was a polyolefin resin, and the material was 100% by weight of low-density polyethylene (LDPE in the table). The antiviral agents were zirconium phosphate ion-exchanged with silver or silver compounds; phosphate compounds containing calcium and zinc ion-exchanged with silver or silver compounds; and zeolite supported with silver and copper by ion exchange. The antiviral and foaming properties of ten test materials each having the composition shown in Tables 1 to 3, including combinations with surfactants, were evaluated as Test Examples 1 to 3. The expansion ratio and surface properties were evaluated. The resin was also evaluated against oxidation degradation, but because long-term stability against oxidation degradation requires time to test, DSC analysis was performed on materials of a given composition and used to evaluate the results. Details of each test material will be described later.

[0101] Furthermore, in Test Example 4, a titanium oxide-based antiviral agent, which is a visible light-activated photocatalyst, was used as the antiviral agent, and evaluation was performed on the five types of test materials shown in Table 4 in the same manner as in Test Examples 1 to 3.

[0102] Test Example 5 was a test conducted to evaluate the effects of the type of base resin, the effect of the expansion ratio, and the effect of the antioxidant. In Test Example 5, the effects of differences in base resin were evaluated using a mixed resin of low-density polyethylene and high-density polyethylene, polypropylene resin, and ethylene-vinyl acetate copolymer (EVA) as the base resin.

[0103] Next, in Test Example 5, in order to see the effect on antiviral properties when the expansion ratio is changed to change the skin layer thickness, the base resin was low-density polyethylene, the content of the antiviral agent was constant, and resin foams with expansion ratios changed in four stages between 15 and 40 times, 15 times, 20 times, 30 times, and 40 times, and five types of materials with an expansion ratio of 10 times were prepared. Here, the amounts of crosslinking agent and foaming agent added to each test material were adjusted according to the expansion ratio as follows. Specifically, when the expansion ratio was 15 times, 0.9 parts of crosslinking agent and 8.0 parts of foaming agent were added, when the expansion ratio was 20 times, 0.9 parts by mass of crosslinking agent and 11 parts by mass of foaming agent were added, and when the expansion ratio was 30 times, 0.8 parts by mass and 16 parts by mass of crosslinking agent were added. When the expansion ratio was 40 times, 0.7 parts by mass of crosslinking agent and 22 parts by mass of foaming agent were added to produce a resin foam with an adjusted expansion ratio. When the expansion ratio was 10 times, 0.9 parts by mass of the crosslinking agent and 5.0 parts by mass of the foaming agent were added. Next, in order to examine the effect of the antioxidant, resin foams were prepared with compositions containing 0.8 parts by mass and 1.2 parts by mass of the antioxidant.

[0104] Here, the following organic decomposition type foaming agent and crosslinking agent were mixed with the base resin, kneaded with a pressure kneader, and pelletized to obtain pellets of a foamable resin composition. The pellets were fed from the hopper of a single-screw extruder, melt-kneaded in the extruder, and extruded through a die of a predetermined width to obtain a smooth foaming base sheet with a thickness of 4 mm. In this case, low-density polyethylene (LDPE) was used as the base resin except for the test to evaluate the effect of the resin composition in Test Example 5, and in all cases, F120N manufactured by Ube Maruzen Polyethylene Co., Ltd. was used as the low-density polyethylene.

[0105] Next, this foaming base sheet was extruded at 120 to 150 ° C., and then passed through a heating furnace at 220 ° C. to 240 ° C. to foam at an expansion ratio corresponding to each test material, to obtain a sheet-like foam. To obtain this sheet-like foam, 0.8 parts by mass of Percumyl D dicumyl peroxide (trade name) manufactured by Nippon Oil & Fats Co., Ltd. was used as a crosslinking agent, and 16 parts by mass of Vinihol AC # LQ (azodicarbonamide (ADCA)) manufactured by Eiwa Kasei Co., Ltd. was used as a foaming agent as an organic decomposition type foaming agent. Here, this sheet-like extruded resin foam was obtained, and a test piece was cut out from the surface of the skin layer of this foam, and subjected to tests for evaluation of the expansion ratio, surface properties, and oxidation deterioration for evaluation of antiviral properties and foaming properties. In addition, in the present invention, in order to correctly evaluate the influence on the surface properties of the foam as described later, it was decided not to perform rolling.

[0106] (Test Example 1) (zirconium phosphate carrying silver or a silver compound by ion exchange) Polyolefin foams were prepared using 100% by weight of low-density polyethylene as the base resin, and containing 1.0 parts by mass, 2.0 parts by mass, 3.5 parts by mass, and 5.0 parts by mass of Toa Gosei's Novalon IV1000, an antiviral agent consisting of zirconium phosphate ion-exchanged with silver or a silver compound, expanded 30 times, per 100 parts by mass of the base resin. These were designated Test Materials 1 to 4, respectively.

[0107] A polyolefin-based extruded resin foam was prepared using only low-density polyethylene as the base resin, and the antiviral agent was 30 times expanded, containing 3.5 parts by mass of Toa Gosei's Novalon IV1000, which consists of zirconium phosphate ion-exchanged with silver or a silver compound, per 100 parts by mass of the base resin, and further containing 0.8 parts by mass of Riken Vitamin's glycerin fatty acid ester-based Rikemal S-100 as a surfactant, and each was designated test material 5.

[0108] Test material 6 was prepared by changing test material 5 to a material containing 3.5 parts by mass of Novalon IV1000 as an antiviral agent and 0.8 parts by mass of Rikemal S-100 as a surfactant instead of Rikemal S-100. Test material 7 was prepared to contain 2.0 parts by mass of Rikemal S-100 as a surfactant.

[0109] Furthermore, a small amount of 0.6 parts by mass of Novaron was added as an antiviral agent to prepare test material 8, and 3.5 parts by mass of Novaron was added as an antiviral agent and 0.3 parts by mass of Rikemal S-100 as a surfactant was added to prepare test material 9. Furthermore, a material containing 3.0 parts by mass of Rikemal S-100 as a surfactant, exceeding the upper limit of 2.0 parts by mass for the surfactant content, was prepared and designated test material 10.

[0110] (Test Example 2) (A phosphate compound consisting of hydroxyapatite containing silver or calcium and zinc carrying silver ions) Using low-density polyethylene as the base resin, polyolefin foams were prepared containing 1.0 parts by mass, 2.0 parts by mass, 3.5 parts by mass, and 5.0 parts by mass of a phosphate compound made of hydroxyapatite composition containing calcium and zinc with silver or a silver compound supported by ion exchange, per 100 parts by mass of the base resin, expanded 30 times. These were designated test materials 11 to 14, respectively.

[0111] Test materials 15 and 16 were prepared by using 100 parts by weight of low-density polyethylene as the base resin, and the antiviral agent was expanded 30 times to a polyolefin foam containing 3.5 parts by mass of a phosphate compound consisting of a hydroxyapatite composition containing calcium and zinc supported by silver or silver compound ion exchange, per 100 parts by mass of the base resin, and further containing 0.8 parts by mass each of Rikemal S-100 and calcium stearate as surfactants. Test material 17 was prepared by using 2.0 parts by mass of calcium stearate as a surfactant.

[0112] Furthermore, a small amount of 0.6 parts by mass of a phosphate compound consisting of a hydroxyapatite composition containing calcium and zinc supported by silver or silver compound ion exchange was added as an antiviral agent to prepare test material 18, and 3.5 parts by mass of the above phosphate compound was added as an antiviral agent to prepare test material 19, in which 0.3 parts by mass of calcium stearate was added as a surfactant. A material containing 3.0 parts by mass of calcium stearate as a surfactant, exceeding the upper limit of 2.0 parts by mass for the surfactant content, was prepared as test material 20 from test material 13.

[0113] (Test Example 3) (Ion-exchanged zeolite containing silver and copper) For each test material in Test Example 3, the antiviral agent was changed from Toagosei's Novalon IV1000, which consists of zirconium phosphate ion-exchanged with silver or a silver compound, to Sinanen's AC100D, which consists of ion-exchanged zeolite containing silver and copper, but the combination of the content ratio of the antiviral agent and surfactant for each test material was the same as in Test Example 1.

[0114] Polyolefin foams were prepared using low-density polyethylene as the base resin and expanded 30 times to contain 1.0 part by mass, 2.0 parts by mass, 3.5 parts by mass, and 5.0 parts by mass of ion-exchanged zeolite containing silver and copper per 100 parts by mass of the base resin. These were designated Test Materials 21 to 24, respectively.

[0115] Using low-density polyethylene as the base resin, polyolefin-based extruded resin foams were prepared using an antiviral agent expanded 30 times, containing 3.5 parts by mass of ion-exchanged zeolite containing silver and copper per 100 parts by mass of the base resin, and further containing 0.8 parts by mass each of Riken Vitamin's glycerin fatty acid ester-based Rikemal S-100 and calcium stearate as surfactants, and these were designated test materials 25 and 26. Test material 27 was a material containing 2.0 parts by mass of Rikemal S-100 as the surfactant.

[0116] Furthermore, a small amount of 0.6 parts by mass of ion-exchanged zeolite containing silver and copper was added as an antiviral agent to prepare test material 28, and 3.5 parts by mass of the above-mentioned ion-exchanged zeolite containing silver and copper was added as an antiviral agent to prepare test material 29. A material containing 3.0 parts by mass of calcium stearate as a surfactant, exceeding the upper limit of 2 parts by mass for the surfactant content, was prepared as test material 30 from test material 23.

[0117] (Test Example 4) (Antiviral agent based on titanium oxide using visible light responsive photocatalyst) In addition, using only low-density polyethylene as the base resin, 1.0 parts by mass, 2.0 parts by mass, 3.5 parts by mass, and 5.0 parts by mass of Wilan, an antiviral agent manufactured by Naka Kogyo Co., Ltd., which is a titanium oxide-based antiviral agent using a visible light responsive photocatalyst, were added as another antiviral agent per 100 parts by mass of the base resin, and materials were created by foaming this 30 times, and these were designated test materials 31 to 34. A further material was added to which 3.5 parts by mass of Wilan was added, and 1.0 part by mass of Rheomix HT Flake, manufactured by Lion Corporation, as a cationic surfactant was added to obtain test material 35, and this material was evaluated in the same manner as the test materials containing other antivirals.

[0118] (Test Example 5) (Evaluation of the impact of base resin type, foaming ratio, and antioxidant on antiviral properties) For the test material of Test Example 4, 100% by weight of low-density polyethylene was used as the base resin in Test Examples 1 to 3, but a mixed resin foam was made by mixing 80% by weight of low-density polyethylene and 20% by weight of high-density polyethylene and foaming it 30 times, and a material similar to Test Material 3 was prepared containing 3.5 parts by weight of Novalon IV1000 by Toa Gosei per 100 parts by weight of the base resin, and this was designated Test Material 36. For Test Material 36, F120N manufactured by Ube Maruzen Polyethylene Co., Ltd. was used as the low-density polyethylene, and HD1300 manufactured by Japan Polyolefins Co., Ltd. was used as the high-density polyethylene.

[0119] Test material 37 is an example where the base resin of the resin foam was changed from low-density polyethylene to polypropylene. Since polypropylene is difficult to crosslink by chemical crosslinking, a sheet was extruded by the electron beam crosslinking method using two electron beam crosslinking devices, and the sheet was crosslinked by electron beam crosslinking from above and below under specified conditions, and then expanded 30 times. The composition of the antiviral agent in this test material is the same as that of test material 3. Prime Polymer's Prime Polypro E702MG was used as the polypropylene. Test material 38 is an example where the base resin was an ethylene-vinyl acetate copolymer. The ethylene-vinyl acetate copolymer used was VF218G manufactured by Ube Maruzen Polyethylene Co., Ltd., and the test material was manufactured in the same manner as the low-density polyethylene of test material 3.

[0120] Next, test materials 39 and 40 are foamed by changing the foaming ratio from 30 times to 15 times and 20 times for a material containing 3.5 parts by mass of Novalon as an antiviral agent with the same composition as test material 3, and test material 41 is the same material as test material 3, but the numbers in the table are renumbered consecutively. Test material 42 is foamed by changing the foaming ratio from 30 times to 40 times for a material with the same antiviral agent composition as test material 3. Test material 43 is foamed 10 times for a material with the same composition as test material 3. Test materials 44 and 45 are foamed bodies to which 0.8 parts by mass and 1.2 parts by mass of Irganox 1010 were added as an antioxidant to see the effect of the antioxidant.

[0121] (Anti-viral test method) The antiviral test was basically performed in accordance with ISO21702. The test used influenza virus (H3N2, A / hongkong / 6 / 86) and MDCK cells (canine kidney tubular epithelial derived cells) as host cells, and was performed under the following conditions: sensitization temperature 25°C, sensitization time 24 hours. SCDLP medium was used as the washout solution, and the infectivity was measured using the plaque method.

[0122] The specific test procedure was as follows: three samples measuring 40 mm x 40 mm x 4 mm thick were cut out from each test material of each Example, and each was individually attached to the bottom of a separate petri dish. Next, 400 μL of virus was inoculated onto each sample, and then a PET film (4 cm x 4 cm) was placed over the sample. After the sensitization time had elapsed, 10 mL of washout solution was added and the samples were washed out by pipetting. Finally, the infectivity value V after 24 hours in the washout solution was measured. 24 Based on this, the percentage R (%) of the amount of virus that had decreased after 24 hours relative to the initial harvested amount V0 and the activity value Mv after 24 hours were calculated.

[0123] Specifically, assuming that the percentage of virus reduction after 24 hours is R (%) and the antiviral activity value is Mv, both can be calculated by the following formula using the initial infectivity immediately after inoculation and the infectivity titer 24 hours after inoculation. The percentage of the virus reduction amount after 24 hours relative to the initial virus amount R (%) was calculated using the following formula (1): (1)R = (V0 - V 24 ) / V0 The activity value of an antiviral agent can be calculated by the following formula (2). (2) Mv = log(V0) - log(V 24 )

[0124] Where, V0: initial infectivity immediately after inoculation, V 24 In the present invention, for convenience, the infectivity after 24 hours is expressed as a logarithmic value of the infectivity after 24 hours, which is referred to as the logarithmic value of the virus infectivity (Log(PFU)), and is described together with the activity value (originally logarithmic titer). By describing it in this manner, the sum of the logarithmic expression of the infectivity after 24 hours and the activity value is always the logarithmic value of the initial infectivity, making it easier to confirm the relationship between the activity value and the infectivity. Here, the measured value of the initial infectivity is 1.70×10 6 The logarithmic titer of the initial infectivity was 6.23.

[0125] (Method of evaluating foaming property) In order to ensure the soundness of the foamed products used in the test during extrusion foaming, the foamability was evaluated by evaluating both the stability of the foaming ratio of each test material and the surface properties of the foamed products. The foaming ratio of each test material was measured by cutting out test pieces for measuring the foaming ratio from five points, the four corners and the center of the product after extrusion foaming, and measuring the foaming ratio of the cut test pieces as follows. The average value of the five points was taken as the foaming ratio. The materials used in the foaming evaluation were not rolled in order to eliminate the effect of roll rolling on the foaming ratio.

[0126] The expansion ratio is an apparent expansion ratio generally used for resin foams. This apparent magnification is determined by the following procedure. First, a test piece measuring 10 cm x 10 cm is cut out from the sheet before foaming, and its weight (W1 [g]) is measured. After that, the thickness of the test piece is measured at each of the four corners and at the center (the measuring machine conforms to the JIS K 6767 method). The apparent density is calculated using the average value (T [cm]) of the five points according to the following formula (3). Apparent specific gravity = 10 × 10 × T / W1 (3) The same measurement was also carried out after foaming, and the specific gravity of the sheet before and after foaming was calculated. (Expansion ratio)=(specific gravity of composition before foaming) / (specific gravity of foamed composition) The value calculated by the above formula is defined as the expansion ratio.

[0127] As a result, the foaming ratio was rated as A for 31.5 to 28.5 times, 30±1.5 times, within ±5% of the target value of 30 times, B for less than 28.5 to 27.0 times, -5% to -10% of the target value, and C for less than 27.0 times, -10% of the target value. Here, the surface properties of each test material were evaluated as follows: ◎ for no discoloration or wrinkles on the surface of the foamed material, △ for slight unevenness of 2 to 3 mm, and × for both unevenness of 2 to 3 mm and wrinkles on the surface.

[0128] (Evaluation of long-term durability of extruded resin foam) In order to predict the long-term durability of the resin used in the test, since it was expected that there would be differences in the long-term stability of the resin between zirconium phosphate, zeolite, and titanium oxide (photocatalytic type), DSC thermal analysis tests were performed in an air atmosphere for the specified composition using these materials as antiviral agents.Thermal analysis was performed by heating from room temperature to a specified temperature at a heating rate of 10°C / min, and the heat generation start temperature was confirmed.

[0129] Test materials in which 5.0 parts by mass each of zirconium phosphate, zeolite, and titanium oxide-based antiviral agents were added to the base resin LDPE were used. Test materials 4, 24, and 34 were gradually heated from room temperature in an air atmosphere, and the oxidative degradation behavior of each material was compared by DSC analysis.

[0130] (Test Results) Tables 1 to 4 show the antiviral test results and foaming property evaluation results for each test material of Test Examples 1 to 4 in the skin layer of a resin foam when the type of antiviral and the amount and type of surfactant added were changed. Table 5 shows the test results for Test Example 5, which evaluated the composition of the base resin, the foaming ratio, and the antiviral property and foaming property of the antioxidant. As the results of the antiviral test, three types of results were obtained and listed: the logarithm of the infectivity value of the virus after 24 hours, the amount of virus reduced relative to the initial amount collected, and the activity value.

[0131] [Table 1]

[0132] [Table 2]

[0133] [Table 3]

[0134] [Table 4]

[0135] [Table 5]

[0136] Table 1 shows the test results when the content of zirconium phosphate obtained by ion-exchange of silver or a silver compound was changed in the range of 1.0 to 5.0 parts by mass and added alone to the antiviral agent corresponding to Test Example 1, when 0.5 to 2.0 parts by mass of a surfactant was added, when an under-addition and over-addition of the surfactant was added, and when only the antiviral agent was added at 0.6 parts by mass or under-addition. Table 2 shows the test results when the content of a phosphate compound consisting of a hydroxyapatite composition containing calcium and zinc with silver or silver ions supported by ion exchange was changed in the range of 1.0 to 5.0 parts by mass and added alone to the antiviral agent corresponding to Test Example 2, when 0.5 to 2.0 parts by mass of a surfactant was added, when an under-addition and over-addition of the surfactant was added, and when only the antiviral agent was added at 0.6 parts by mass or under-addition. Table 3 shows the results of similar tests using ion-exchanged zeolite containing silver and copper, and Table 4 shows the results of similar tests using an antiviral agent based on titanium oxide as a visible light responsive photocatalyst.

[0137] (Antiviral evaluation results for each test material) In Test Examples 1 to 4 in Tables 1 to 4, for any of the antiviral agents, the virus amount in the test material tends to decrease within a specified range as the content of the antiviral agent increases when the antiviral agent is in the range of 1.0 to 5.0 parts by mass, but the antiviral effect is greatest when the content of the antiviral agent is in the vicinity of 3.5 parts by mass, and the effect saturates when the amount of the antiviral agent exceeds 3.5 parts by mass. Furthermore, it can be seen from the reduction in the virus amount and activity value that by adding a surfactant within a specified range when the amount of the antiviral agent is 3.5 parts by mass, the virus reduction effect becomes slightly greater even if the content of the antiviral agent is the same.

[0138] Here, in the results of Test Examples 1 to 4, when the content of the antiviral agent is in the range of 1.0 part by mass to 5.0 parts by mass, the amount of virus reduced from the initial intake is 95% or more, and the activity value exceeds 1.40, regardless of the type of antiviral agent. Also, when the content exceeds 2 parts by mass, the amount of virus reduced from the initial intake is 99% or more, and the activity value exceeds 2.0, indicating that when the content of the antiviral agent is 2 parts by mass or more, stable antiviral properties are exhibited.

[0139] Furthermore, the antiviral effect was greatest at 3.5 parts by mass of the antiviral agent, and even if the amount of the antiviral agent was increased from 3.5 parts to 5.0 parts by mass, no reduction in the amount of virus or increase in activity was observed. The reason for this is unclear, but it is thought to be due to factors such as uneven dispersion even when the amount of the antiviral agent is increased.

[0140] Therefore, the upper limit of the content of the antiviral agent is set to 5.0 parts by mass. In the case of the test material to which 0.6 parts by mass of the antiviral agent, which is 1.0 part by mass or less, was added, the activity value was below 1.3, and although the antiviral effect was recognized, the activity value was low and the antiviral effect was insufficient, and the activity value never exceeded 1.3. Therefore, in order to obtain a sufficient antiviral effect, it is considered that the content range of the antiviral agent needs to satisfy 0.8 to 5.0 parts by mass, and preferably needs to satisfy 1.0 to 5.0 parts by mass.

[0141] To see the effect of the surfactant, an explanation will be given based on Table 1. In comparing Test Material 9, 5, 7, and 10, which use Test Material 3 as the base and have a constant antiviral agent content of 3.5 parts by mass and change the surfactant to 0.3, 0.8, 2.0, or 3.0 parts by mass, Test Material 9, which added 0.3 parts by mass of the surfactant, had a low surfactant content and therefore no surfactant effect was obtained, while Test Material 10, which added 3.0 parts by mass, showed a tendency that even when the amount was increased up to 3.0 parts by mass, the virus suppression effect was equivalent to when 2.0 parts by mass of the antiviral agent was added, and did not change much.

[0142] Therefore, even if the surfactant content is increased up to 3.0 parts by mass, the effect is saturated and the cost becomes high, so the upper limit is set to 2.0 parts by mass, and the lower limit is set to 0.5 parts by mass or more as a result of the above. In addition, when test material 5 and test material 6, in which the same amount of 0.8 parts by mass of Rikemal S-100 and calcium stearate were added as surfactants, were compared, the two were almost equivalent. Therefore, the content of the surfactant is set to 0.5 to 2.0 parts by mass, and the preferable range is 0.8 to 2.0 parts by mass.

[0143] Here, the surfactants have been explained based on the test examples in Table 1, but the differences between Table 2 and Table 1 are that the antiviral agent was changed to another phosphate compound, and that the surfactant with a different surfactant content was changed from Rikemal S-100 to calcium stearate in Table 2. Table 3 differs only in that the antiviral agent was changed from zirconium phosphate to ion-exchanged zeolite containing silver and copper. In Table 4, for the antiviral agent using a titanium oxide-based visible light responsive photocatalyst, the effect of the surfactant was confirmed at only one level, using 1.0 part by mass of Rheomix HT Flake as a cationic surfactant.

[0144] Although there were slight differences in the antiviral effect between the materials, similar effects were confirmed for each material, including the phosphate compounds carrying silver or silver ions, ion-exchanged zeolites containing silver and copper, and the titanium oxide-based antiviral agent using a visible light responsive photocatalyst, in Tables 2 and 3. Additionally, the effects of the surfactants in Tables 2 to 4 were almost the same as those of the test materials in Table 1.

[0145] (Evaluation results of foaming properties of each test material) The results of evaluating the foaming property, foaming ratio, and surface properties of the foam for each test example are shown in Tables 1 to 4. In the case of a phosphate compound consisting of zirconium phosphate with ion-exchanged silver or silver compound as the antiviral agent, and hydroxyapatite containing calcium and zinc with silver or silver ions supported by ion-exchange, the foaming ratio was within ±5% of the target value of 30 times (28.5 to 31.5 times), and the foaming property of all materials satisfied the A rank. In addition, there was no discoloration on the surface of the foam, wrinkles on the surface of the foam, or unevenness of about 2 to 3 mm on the surface of the foam, and there were no problems with the surface quality.

[0146] In contrast, in the case of titanium oxide-based antiviral agents using ion-exchanged zeolite containing silver and copper and visible light responsive photocatalysts shown in Tables 3 and 4, the foaming properties were evaluated as Rank B, where the foaming ratio was less than 28.5 to 27.0 times, or Rank C, where the foaming ratio was less than 27.0 times, and it was considered that the foaming properties were inhibited. In addition, as a result of checking the surface properties of these materials on the foam surface, irregularities of about 2 to 3 mm and wrinkles on the surface were confirmed on the foam surface. Note that the material containing only 0.6 parts by mass of zeolite as an antiviral agent had a low zeolite content, so it behaved in the same way as other antiviral agents and had little effect on foaming properties.

[0147] Furthermore, for test materials 3, 13, 23, and 33, which contained 3.5 parts of each of the antivirals in Tables 1 to 4, observation of the cut surfaces of the foams revealed that test materials 3 and 13, which used a phosphate-based antiviral agent and had no foaming problems, had a uniform bubble structure, whereas the antiviral agents using zeolite or visible light responsive photocatalysts had a non-uniform bubble structure and there were areas where the bubble diameter had not expanded to a stable state, causing foaming inhibition. This was thought to have led to a decrease in the expansion ratio and non-uniform surface properties of the foam.

[0148] From the above results, it was confirmed that the phosphate-based antiviral agent of the present invention containing silver or a silver compound or silver ions as a heavy metal not only has antiviral properties compared to other antiviral agents containing other heavy metals, but also is not inhibited by the antiviral agent during the foaming process and is excellent in foaming properties and surface properties of the foam.

[0149] (Evaluation results of resin deterioration by thermal analysis of test material) In addition, DSC analysis was performed to evaluate each antiviral agent in terms of its long-term stability against resin degradation, with the results being as follows: When each material was heated from room temperature in an air atmosphere at a constant rate (10°C / min), an endothermic peak thought to be the melting peak of polyethylene crystals was observed between 100 and 130°C (the peak was in a broad endothermic peak around 125°C), and when the temperature was then increased at the same constant rate, the DSC curves for the zeolite-based and titanium oxide-based antiviral agents gradually began to rise and heat was generated, whereas the DSC curve for the zirconium phosphate compound showed almost no rise in the temperature range above 130°C and was stable.

[0150] As a result, in the case of zeolite-based and titanium oxide-based antiviral agents, signs of oxidative deterioration were observed when the test temperature exceeded 130°C. From this, when comparing the case of the zirconium phosphate compound antiviral agent with the case of the zeolite-based and titanium oxide-based antiviral agents, the case of zirconium phosphate contains Ag as a heavy metal ion, but the case of the zeolite-based antiviral agent contains Cu in addition to Ag, which accelerates deterioration, and in the case of the titanium oxide-based antiviral agent, the difference in photocatalytic function and material structure is also considered to be one of the factors that accelerates the deterioration of the resin. From the above thermal analysis results, it was confirmed that the phosphate-based antiviral agent also has superior long-term stability of the resin.

[0151] (Anti-viral properties evaluation based on differences in base resin) Test materials 36, 37, 38, and 41 in Table 5 show the evaluation results of the antiviral properties of test materials foamed at the same expansion ratio and with a constant antiviral agent content of 3.5 parts by mass when the base resin was changed from low-density polyethylene to a mixed resin of low-density polyethylene and high-density polyethylene, polypropylene resin, and ethylene-vinyl acetate copolymer (EVA), as well as when the base resin was low-density polyethylene as the standard. Although there were some differences in the antiviral properties due to the differences in the base resin, the activity value exceeded 2.5 for all resins, indicating sufficient antiviral properties. The foamability of all of these test materials was good, there was no foaming inhibition, and the surface properties of the foams were all good.

[0152] (Anti-viral properties evaluation results when foaming ratio is changed) As can be seen from the results of test materials 39 to 43 in Table 5, the behavior of the reduction in virus quantity and change in activity value for test materials 39, 40, and 41 (test material 3), which are resin foams with expansion ratios of 15, 20, and 30 times using the same base resin material as in Test Example 3, and test material 42, which is a resin foam with an expansion ratio of 40 times, showed a tendency for the activity value to increase as the expansion ratio increased, and the activity value also increased from 2.40 to 2.82 as the expansion ratio increased from 15 to 40 times. Here, when the expansion ratio was 40 times, the activity value was particularly large at 2.82, which is thought to be because the skin layer became extremely thin at 5 μm, which is less than 10 μm, and the surface effect of the antiviral agent particles became significantly larger. In contrast, when the expansion ratio of test material 43 was 10 times, the activity value was 2.12, which was a lower value than when the expansion ratio was 15 times or more, and although the antiviral effect was recognized, the antiviral effect was lower than when the expansion ratio was 15 times or more. From this result, it was thought that the difference in the antiviral effect due to the expansion ratio was due to the difference in the surface effect of the antiviral agent particles on the skin layer surface, and it was confirmed that the skin layer thickness is preferably 100 μm or less. In addition, all of these test materials with different expansion ratios had no problems with the stability of the expansion ratio and surface properties in the foaming test, and no foaming inhibition occurred.

[0153] In the present invention, a metal-based antiviral agent supported on an inorganic substance is used as the antiviral agent. Therefore, the resin foams described in Test Materials 44 and 45, in which the material of Test Material 3 was further supplemented with 0.8 and 1.2 parts by mass of BASF antioxidant Irganox 1010 as an antioxidant to prevent oxidative deterioration of the resin, were used to evaluate the influence of the antioxidant on the antiviral effect and the influence on the foaming behavior of the base resin.

[0154] As a result of the evaluation of test materials 44 and 45, in test material 44, which contains 0.8 parts by mass of antioxidant, it was confirmed that the antioxidant had no significant effect on the activity value, and the desired antiviral effect was obtained, and furthermore, foaming inhibition did not occur and the surface properties of the foam were excellent. However, in test material 45, which contains more than 1.0 parts by mass of antioxidant, although the antiviral effect was not a problem, foaming inhibition occurred, foaming properties were reduced, and the surface properties were not good. Therefore, the content of the antioxidant needs to be 1.0 parts by mass or less. As shown in the comparative examples in Table 5, if the content of the antioxidant is 1.0 parts by mass or less, it is considered that there is no problem even if the antioxidant is added.

[0155] As described above, in the present invention, it has been confirmed that a material can be obtained in which the extruded polyolefin resin foam contains as an antiviral agent 0.8 to 5.0 parts by mass of a silver or silver-based compound, or a phosphate-based compound carrying silver ions, or which further contains these antiviral agents and 0.5 to 2.0 parts by mass of a surfactant, and the antiviral agent is exposed on the surface of the skin layer of the resin foam, thereby not only exhibiting excellent antiviral properties, but also exhibiting excellent foaming properties and resistance to oxidative deterioration of the resin.

[0156] More specifically, this is thought to be because the skin layer is formed while being subjected to a pressing force from the gas inside the bubbles when the melt viscosity of the resin is high, so that almost no antiviral agent particles fall off during the growth of the skin layer, and the increase in the probability distribution density of the number of antiviral agent particles near the bubble wall surface due to thinning of the bubble walls becomes dominant.

[0157] The antiviral effect of the surfactant is thought to be promoted by the overlapping effect of improving the dispersibility of the antiviral agent by the surfactant, as well as the effect of increasing the adsorption to the virus due to the improved wettability caused by the improved hydrophilicity of the air bubble surface. Furthermore, when different types of surfactants were used to confirm the effect of the type of surfactant, there was almost no difference due to the type of surfactant.

[0158] Furthermore, since the present invention uses an antiviral agent based on silver or a silver-based compound, or a phosphate compound carrying silver ions, it is not necessarily necessary to add an antioxidant. However, when the effect of including an antioxidant in a specified range of 1.0 part by mass or less was confirmed, it was found that adding an antioxidant in this range did not affect foamability.

[0159] In addition, when a material of the same composition containing 3.5 parts by mass of zirconium phosphate as an antiviral agent was foamed in the range of 10 to 40 times, a difference in the antiviral effect was observed depending on the skin layer thickness, and it was confirmed that the activity value was high and the antiviral property was high when the skin layer thickness was 100 μm or less compared to when the skin layer thickness was thicker than 100 μm. Therefore, it is considered that the skin layer thickness is preferably 5 to 100 μm, and more preferably 5 to 70 μm or less.

[0160] Although the antiviral effects of antiviral agents and surfactants in resin foams have been described in the above embodiments of the present invention, the technical scope of the present invention is not limited to the above-described embodiments. It is clear that a person skilled in the art can come up with various modified or revised examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present invention.

Claims

1. A polyolefin-based extruded resin foam having excellent foamability, comprising, as an antiviral agent, silver or a silver compound, or a phosphate-based compound carrying silver ions, in an amount in the range of 0.8 to 5.0 parts by mass per 100 parts by mass of polyolefin resin, at least one surface of the polyolefin-based extruded resin foam is a skin layer, and the antiviral agent is exposed on the surface of the skin layer.

2. 2. The polyolefin-based extruded resin foam according to claim 1, characterized in that the antiviral agent contained in the polyolefin-based extruded resin foam contains at least one of: zirconium phosphate carrying silver or a silver compound by ion exchange; and a phosphate compound having a hydroxyapatite composition containing calcium-zinc carrying silver or silver ions by ion exchange.

3. The polyolefin extruded resin foam according to claim 1 or 2, characterized in that the base resin of the polyolefin extruded resin foam is at least any one of low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, very low-density polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-methyl acrylate copolymer, and ethylene-ethyl acrylate copolymer, or a mixture of two or more of these blended together.

4. The extruded polyolefin resin foam according to any one of claims 1 to 3, characterized in that, in addition to the antiviral agent, the extruded polyolefin resin foam contains 0.5 to 2.0 parts by mass of a surfactant.

5. The extruded polyolefin resin foam according to any one of claims 1 to 4, characterized in that, in addition to the antiviral agent, the extruded polyolefin resin foam contains 0.05 to 1.0 part by mass of an antioxidant.

6. A laminate according to any one of claims 1 to 5, characterized in that the laminate is a laminate in which another polyolefin-based extruded resin foam is attached to the surface of the polyolefin-based extruded resin foam, and at least one skin layer is exposed to the surface of the laminate.

7. A polyolefin-based extruded resin foam having excellent foaming properties, comprising at least one of: zirconium phosphate carrying silver or a silver compound by ion exchange as an antiviral agent; and a phosphate compound having a hydroxyapatite composition containing calcium-zinc carrying silver or silver ions by ion exchange, in an amount in the range of 0.8 to 5.0 parts by mass per 100 parts by mass of polyolefin resin, wherein at least one skin layer of the polyolefin-based extruded resin foam has a thickness of 100 μm or less, and the antiviral agent is exposed on the surface of the skin layer.

Citation Information

Patent Citations

  • Antimicrobial thermoplastic resin foam

    JP1995173318A

  • Fine particle-containing resin molding

    JP1998182844A

  • Food taking board

    JP1999056653A

  • Expandable resin particle having photocatalytic function and foam thereof

    JP1999293025A

  • Antibacterial foaming resin particle and molded product made of the same

    JP1999335481A