Laminated structure and its uses

A laminated structure with a cured resin layer on a polypropylene resin composition improves dimensional stability and adhesive strength without a primer, effectively addressing interfacial delamination and strength loss in automobile exterior panels.

JP7575635B2Active Publication Date: 2024-10-29PRIME POLYMER CO LTD +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024111004
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-14
Filing Date
2024-07-10
Publication Date
2024-10-29
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Polypropylene resin compositions used in automobile exterior panels face challenges with high dimensional instability and adhesive strength issues, particularly when bonded to steel, leading to interfacial delamination and decreased strength, despite the need for low linear expansion and high adhesive performance without the use of primers.

Method used

A laminated structure is developed with a cured resin layer containing a curable resin with urethane bonds directly laminated on a molded article made of a polypropylene resin composition, comprising specific ratios of propylene polymers, ethylene/α-olefin copolymers, and inorganic fillers, enhancing dimensional stability and adhesive strength without a primer.

Benefits of technology

The laminated structure achieves high adhesive strength between the molded body and the cured resin layer, maintaining stability even at high temperatures, with a hot shear test strength exceeding 1.5 MPa, addressing the issues of interfacial delamination and strength loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575635000022
    Figure 0007575635000022
  • Figure 0007575635000001
    Figure 0007575635000001
  • Figure 0007575635000002
    Figure 0007575635000002
Patent Text Reader

Abstract

To provide a laminated structure of a polypropylene-based resin composition and a resin curable layer which has a low coefficient of linear expansion and high adhesive strength to a curable resin layer such as an adhesive layer, in a primer-less manner.SOLUTION: There is provided a laminated structure that a resin curable layer (ii) containing a curable resin (E) having a urethane bond is directly laminated on a molding (i) composed of a polypropylene-based resin composition, wherein the polypropylene-based resin composition contains: 5 to 47 pts.mass of a propylene-based polymer (A) having an MFR of 50 to 150 g / 10 min and a decane soluble part amount of 6 to 15 mass%; 20 to 30 pts.mass of a propylene homopolymer (B) having an MFR of 10 to 500 g / 10 min; 23 to 30 pts.mass of an ethylene-α-olefin copolymer (C) which is a random copolymer of ethylene and α-olefin having 4 to 8 carbon atoms, and has a density of 0.850 to 0.880 g / cm3, an MFR of 0.5 to 30 g / 10 min and a melting peak of 110°C or higher; and 30 to 40 pts.mass of an inorganic filler (D).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate structure used, for example, as an automobile exterior member, and the like, which has a layer of a molded article made of a polypropylene-based resin composition. [Background technology]

[0002] In the field of automotive parts, manufacturers are actively promoting the use of resin for exterior panel materials in response to the need to reduce the weight of automobiles. As part of this movement, the outer parts of back doors are also being switched from metal to resin. From the standpoint of design, the use of resin for these exterior panel materials requires dimensional accuracy on a par with that of metal, and the material must have a low linear expansion coefficient. In addition, back door materials need to be bonded to other parts, so they also require high adhesive performance.

[0003] On the other hand, molded articles obtained from resin compositions such as polypropylene are increasingly being used in various fields such as automobile parts and home appliance parts due to their excellent mechanical properties and moldability, as well as their relatively advantageous cost performance compared to other materials. However, polypropylene generally has a relatively large dimensional change (linear expansion coefficient) with respect to temperature. In this situation, various polypropylene-based resin compositions have been proposed in which inorganic fillers such as talc, elastomer components, etc. are blended with polypropylene to improve dimensional stability (see Patent Documents 1 to 8). However, there has been no teaching on a means for improving the adhesive performance when molded articles of these polypropylene-based resin compositions are bonded to other members. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-077396 A [Patent Document 2] Japanese Patent Application Publication No. 5-051498 [Patent Document 3] JP 2000-095919 A [Patent Document 4] JP 2007-91789 A [Patent Document 5] JP 2013-159709 A [Patent Document 6] JP 2014-58614 A [Patent Document 7] JP 2016-84386 A [Patent Document 8] WO2017 / 082358 Summary of the Invention [Problem to be solved by the invention]

[0005] In order to achieve low linear expansion of polypropylene-based molded bodies, it is necessary to increase the amount of secondary materials with low linear expansion coefficients as mentioned above, and to further impart paintability, it is also necessary to increase the rubber content. For these reasons, polypropylene compounds for resin exterior panels have a very high filler and rubber content, but when they are bonded to other components, there is a problem that interfacial peeling is likely to occur at the interface between the secondary materials and the polypropylene compound during adhesion tests, which tends to reduce strength. In addition, since polypropylene itself does not have polar functional groups, flame treatment or plasma treatment is required to create strong chemical bonds with the adhesive, and this treatment is also problematic in that the substrate surface is damaged and the adhesive strength is likely to decrease. To ensure this adhesive strength, a primer is generally used, but the use of a primer increases costs and the number of manufacturing processes. Therefore, there is a need for a composite material that has sufficient adhesive strength without a primer, while maintaining the two properties of high dimensional stability and high adhesive performance and maintaining the low linear expansion coefficient required for exterior panel materials.

[0006] An object of the present invention is to provide a laminated structure of a molded article made of a polypropylene-based resin composition and a cured resin layer, which has a low linear expansion coefficient and a high adhesive strength with a cured resin layer such as an adhesive layer without requiring a primer. [Means for solving the problem]

[0007] As a result of intensive research conducted in light of the above-mentioned circumstances, the present inventors have found that a laminate structure comprising a molded body made of a polypropylene resin composition containing, as an elastomer component, an ethylene-α-olefin copolymer having a very high melting point, and a specific resin cured layer has excellent dimensional stability and also has high adhesive strength between the specific molded body and the specific curable resin even at high temperatures at which adhesion tends to decrease, thereby completing the present invention.

[0008] The present invention relates, for example, to the following: [1] A laminated structure in which a resin cured layer (ii) containing a curable resin (E) having a urethane bond is directly laminated on a molded body (i) made of a polypropylene resin composition, The polypropylene resin composition comprises: 5 to 47 parts by mass of a propylene polymer (A) having a melt flow rate (230°C, 2.16 kg load) of 50 to 150 g / 10 min and a decane soluble content of 6 to 15 mass %, 20 to 30 parts by mass of a propylene homopolymer (B) having a melt flow rate (230°C, 2.16 kg load) of 10 to 500 g / 10 min, A random copolymer of ethylene and an α-olefin having 4 to 8 carbon atoms, with a density of 0.850 to 0.880 g / cm 3 23 to 30 parts by mass of an ethylene-α-olefin copolymer (C) having a melt flow rate (230°C, 2.16 kg load) of 0.5 to 30 g / 10 min and a melting point peak of 110°C or higher, Inorganic filler (D) 30 to 40 parts by mass [The total amount of components (A) to (D) is 100 parts by mass.] A laminated structure comprising: [2] The laminate structure according to [1], characterized in that in a primerless adhesion test, the 90°C hot shear test strength exceeds 1.5 MPa. [3] The laminate structure according to [1] or [2], wherein the propylene-based polymer (A) is a block copolymer of propylene and ethylene, and the intrinsic viscosity [η] of the decane-soluble portion of the copolymer is 2 to 9 dl / g. [4] The laminate structure according to any one of [1] to [3], wherein the inorganic filler (D) is talc and has an aspect ratio of 3 or more and less than 15. [5] The laminate structure according to any one of [1] to [4], wherein the resin cured layer containing the curable resin (E) having a urethane bond is obtained by curing a urethane-based adhesive containing a urethane prepolymer having a polyether skeleton and an aliphatic isocyanate derivative. [6] The laminate structure according to any one of [1] to [5], wherein the molded body (i) is an injection molded body or a press molded body. [7] The laminate structure according to any one of [1] to [6], which is used as an exterior member for an automobile. [8] An automobile exterior member comprising the laminate structure according to any one of [1] to [7]. [9] 5 to 47 parts by mass of a propylene polymer (A) having a melt flow rate (230°C, 2.16 kg load) of 50 to 150 g / 10 min and a decane soluble content of 6 to 15 mass%, 20 to 30 parts by mass of a propylene homopolymer (B) having a melt flow rate (230°C, 2.16 kg load) of 10 to 500 g / 10 min, A random copolymer of ethylene and an α-olefin having 4 to 8 carbon atoms, with a density of 0.850 to 0.880 g / cm 3 23 to 30 parts by mass of an ethylene-α-olefin copolymer (C) having a melt flow rate (230°C, 2.16 kg load) of 0.5 to 30 g / 10 min and a melting point peak of 110°C or higher, Inorganic filler (D) 30 to 40 parts by mass [The total amount of components (A) to (D) is 100 parts by mass.] A step of molding a polypropylene-based resin composition containing the above compound by injection molding or press molding to produce a molded product (i); a step of contacting or applying a curable resin (E) having a urethane bond or a raw material thereof to the molded body (i) and then curing the resin to form a cured resin layer (ii); A method for producing a laminated structure comprising the steps of:

[10] 5 to 47 parts by mass of a propylene-based polymer (A) having a melt flow rate (230°C, 2.16 kg load) of 50 to 150 g / 10 min and a decane-soluble content of 6 to 15 mass%, 20 to 30 parts by mass of a propylene homopolymer (B) having a melt flow rate (230°C, 2.16 kg load) of 10 to 500 g / 10 min, A random copolymer of ethylene and an α-olefin having 4 to 8 carbon atoms, with a density of 0.850 to 0.880 g / cm 3 23 to 30 parts by mass of an ethylene-α-olefin copolymer (C) having a melt flow rate (230°C, 2.16 kg load) of 0.5 to 30 g / 10 min and a melting point peak of 110°C or higher, Inorganic filler (D) 30 to 40 parts by mass [The total amount of components (A) to (D) is 100 parts by mass.] A curable resin composition used to form an adhesive layer to be directly laminated to a molded article made of a polypropylene-based resin composition containing the following: The curable resin composition contains a urethane prepolymer having a polyether skeleton and an aliphatic isocyanate derivative.

[11] Furthermore, the following formula (X):

[0009] [ka] (In the above formula (X), R 37 and R 38 each independently represents a hydrocarbon group. The curable resin composition according to

[10] , comprising an adduct of a compound represented by the formula:

[12] The curable resin composition according to

[10] or

[11] , wherein the aliphatic isocyanate derivative of the curable resin composition includes an isocyanurate of pentamethylene diisocyanate. Effect of the Invention

[0010] According to the present invention, a molded body made of a polypropylene-based resin composition and a cured resin layer are directly laminated together without the use of a primer, and a laminate structure can be provided which has a low linear expansion coefficient and excellent dimensional stability, and which has high adhesive strength between the specific molded body and the specific curable resin without the use of a primer, even at high temperatures at which adhesion is likely to decrease. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram showing a hot shear strength measurement of a laminated structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be specifically described below.

[0013] The laminate structure of the present invention is a laminate structure in which a resin cured layer (ii) containing a curable resin having a urethane bond is directly laminated to a molded body (i) made of a polypropylene-based resin composition. Specifically, for example, it is a laminate structure in which a molded body (i) made of a polypropylene-based resin composition and a layer (ii) of a curable resin formed from a urethane-based adhesive or the like are directly laminated without using a primer.

[0014] [Molded object (i)] The molded article (i) according to the present invention is a molded article made of a polypropylene resin composition. Polypropylene resin composition The polypropylene resin composition according to the present invention contains a propylene polymer (A), a propylene homopolymer (B), an ethylene-α-olefin copolymer (C), and an inorganic filler (D), and may further contain other components as required.

[0015] <Propylene-based polymer (A)> The propylene polymer (A) used in the present invention is a propylene polymer having a melt flow rate (230° C., 2.16 kg load) of 50 to 150 g / 10 min and a decane soluble content of 6 to 15 mass %.

[0016] The propylene polymer (A) substantially contains 6 to 15 mass% of a decane-soluble portion (a1) and 85 to 94 mass% of a decane-insoluble portion (a2). The decane-insoluble portion (a2) is generally a component that is insoluble in n-decane solvent at room temperature (23°C), and is usually equivalent to the propylene homopolymer portion (propylene homopolymer component) in the propylene polymer (A). The decane-soluble portion (a1) is equivalent to a portion other than the propylene homopolymer portion, and is preferably a copolymer portion of propylene and ethylene (ethylene-propylene copolymer component).

[0017] The propylene polymer (A) usually contains 6 to 15 mass% of a decane-soluble portion (a1) and 85 to 94 mass% of a decane-insoluble portion (a2), and preferably contains 7 to 12 mass% of a decane-soluble portion (a1) and 88 to 93 mass% of a decane-insoluble portion (a2) (the sum of the contents of (a1) and (a2) is 100 mass%).

[0018] The propylene polymer (A) is preferably a propylene block copolymer obtained from propylene and ethylene. The intrinsic viscosity [η] of the decane-soluble portion (a1) of the propylene block copolymer is preferably 2 to 9 dl / g, more preferably 3 to 8 dl / g.

[0019] The melt flow rate of the propylene polymer (A) (230° C., 2.16 kg load) is 50 to 150 g / 10 min, preferably 50 to 130 g / 10 min, more preferably 60 to 120 g / 10 min, and particularly preferably 70 to 110 g / 10 min.

[0020] The propylene-based polymer (A) can be produced by a known method. For example, propylene is polymerized using an olefin polymerization catalyst containing a solid titanium catalyst component (I) and an organometallic compound catalyst component (II) described below, and then propylene and ethylene are copolymerized to obtain a propylene-based block copolymer.

[0021] [Solid titanium catalyst component (I)] The solid titanium catalyst component (I) constituting the olefin polymerization catalyst contains, for example, titanium, magnesium, a halogen, and, if necessary, an electron donor. Any known components can be used for this solid titanium catalyst component (I) without any restrictions.

[0022] In the preparation of the solid titanium catalyst component (I), a magnesium compound and a titanium compound are often used.

[0023] Specific examples of magnesium compounds include magnesium halides such as magnesium chloride and magnesium bromide; alkoxy magnesium halides such as methoxy magnesium chloride, ethoxy magnesium chloride, and phenoxy magnesium chloride; alkoxy magnesium such as ethoxy magnesium, isopropoxy magnesium, butoxy magnesium, and 2-ethylhexoxy magnesium; aryloxy magnesium such as phenoxy magnesium; and magnesium carboxylates such as magnesium stearate. The magnesium compounds may be used alone or in combination of two or more. The magnesium compounds may also be complex compounds, complex compounds, or mixtures with other metals.

[0024] Among them, magnesium compounds containing halogen are preferred, and magnesium halides, particularly magnesium chloride, are more preferred.Also preferred are alkoxymagnesiums such as ethoxymagnesium.The magnesium compound may be derived from other substances, for example, a compound obtained by contacting an organomagnesium compound such as a Grignard reagent with a titanium halide, a silicon halide, a halogenated alcohol, or the like.

[0025] The titanium compound may, for example, be a tetravalent titanium compound represented by the following formula:

[0026] Ti(OR) g X 4-g (In the formula, R is a hydrocarbon group, X is a halogen atom, and g is 0≦g≦4.) Specific examples of titanium compounds include titanium tetrahalides such as TiCl4 and TiBr4; alkoxy titanium trihalides such as Ti(OCH3)Cl3, Ti(OC2H5)Cl3, Ti(On-C4H9)Cl3, Ti(OC2H5)Br3, Ti(Oi-C4H9)Br3; alkoxy titanium dihalides such as Ti(OCH3)2Cl2 and Ti(OC2H5)2Cl2; alkoxy titanium monohalides such as Ti(OCH3)3Cl, Ti(On-C4H9)3Cl, Ti(OC2H5)3Br; alkoxy titanium tetrahalides such as Ti(OCH3)4, Ti(OC2H5)4, Ti(OC4H9)4, Ti(O-2-ethylhexyl)4, etc. Titanium compounds may be used alone or in combination of two or more. Among them, titanium tetrahalides are preferred, and titanium tetrachloride is more preferred.

[0027] As the magnesium compound and titanium compound, for example, compounds described in detail in JP-A-57-63310 and JP-A-5-170843 can be used.

[0028] Specific preferred methods for preparing the solid titanium catalyst component (I) used in the present invention include the following methods (P-1) to (P-4). (P-1) A method in which a solid adduct consisting of an electron donor component (1) such as a magnesium compound and an alcohol is contacted in a suspended state with an electron donor component (2) described below and a liquid titanium compound in the presence of an inert hydrocarbon solvent. (P-2) A method in which a solid adduct consisting of a magnesium compound and an electron donor component (1), an electron donor component (2), and a liquid titanium compound are contacted in separate batches. (P-3) A method in which a solid adduct consisting of a magnesium compound and an electron donor component (1), an electron donor component (2), and a liquid titanium compound are contacted in a suspended state in the presence of an inert hydrocarbon solvent, and the contact is carried out in multiple batches. (P-4) A method of contacting a liquid magnesium compound comprising a magnesium compound and an electron donor component (1), a liquid titanium compound, and an electron donor component (2).

[0029] The reaction temperature in preparing the solid titanium catalyst component (I) is preferably from -30 to 150°C, more preferably from -25 to 130°C, and particularly preferably from -25 to 120°C.

[0030] The preparation of the solid titanium catalyst component (I) can be carried out in the presence of a known medium, if necessary. Specific examples of the medium include aromatic hydrocarbons having a slight polarity, such as toluene, and known aliphatic or alicyclic hydrocarbon compounds, such as heptane, octane, decane, and cyclohexane. Among them, aliphatic hydrocarbons are preferred.

[0031] The electron donor component (1) used to form a solid adduct or a liquid magnesium compound is preferably a known compound capable of solubilizing a magnesium compound in a temperature range of about room temperature to 300° C., such as an alcohol, an aldehyde, an amine, a carboxylic acid, or a mixture thereof, etc. Examples of such compounds include those described in JP-A-57-63310 and JP-A-5-170843.

[0032] Specific examples of alcohols capable of solubilizing magnesium compounds include aliphatic alcohols such as methanol, ethanol, propanol, butanol, isobutanol, ethylene glycol, 2-methylpentanol, 2-ethylbutanol, n-heptanol, n-octanol, 2-ethylhexanol, decanol, and dodecanol; alicyclic alcohols such as cyclohexanol and methylcyclohexanol; aromatic alcohols such as benzyl alcohol and methylbenzyl alcohol; and aliphatic alcohols having an alkoxy group such as n-butylcellosolve.

[0033] Specific examples of carboxylic acids include organic carboxylic acids having 7 or more carbon atoms, such as caprylic acid and 2-ethylhexanoic acid. Specific examples of aldehydes include aldehydes having 7 or more carbon atoms, such as capric aldehyde and 2-ethylhexyl aldehyde. Specific examples of amines include amines having 6 or more carbon atoms, such as heptylamine, octylamine, nonylamine, laurylamine, and 2-ethylhexylamine.

[0034] As the electron donor component (1), the above-mentioned alcohols are preferred, and ethanol, propanol, butanol, isobutanol, hexanol, 2-ethylhexanol and decanol are particularly preferred.

[0035] The composition ratio of magnesium to the electron donor component (1) in the resulting solid adduct or liquid magnesium compound varies depending on the type of compound used and cannot be generally defined. However, the amount of the electron donor component (1) per mole of magnesium in the magnesium compound is preferably 2 moles or more, more preferably 2.3 moles or more, and particularly preferably 2.7 moles or more and 5 moles or less.

[0036] Particularly preferred examples of the electron donor that may be used as necessary in the solid titanium catalyst component (I) include aromatic carboxylic acid esters and / or compounds having two or more ether bonds via a plurality of carbon atoms (hereinafter referred to as "electron donor component (2)").

[0037] As the electron donor component (2), known aromatic carboxylic acid esters and polyether compounds that have been preferably used in conventional olefin polymerization catalysts, such as the compounds described in JP-A-5-170843 and JP-A-2001-354714, can be used without limitation.

[0038] Specific examples of aromatic carboxylates include aromatic carboxylate monoesters such as benzoates and toluates, as well as aromatic polyvalent carboxylates such as phthalates. Among these, aromatic polyvalent carboxylates are preferred, and phthalates are more preferred. As the phthalates, alkyl phthalates such as ethyl phthalate, n-butyl phthalate, isobutyl phthalate, hexyl phthalate, and heptyl phthalate are preferred, and diisobutyl phthalate is particularly preferred.

[0039] Specific examples of the polyether compound include compounds represented by the following chemical structural formula (1).

[0040] [ka] In the above formula (1), m is an integer of 1≦m≦10, more preferably an integer of 3≦m≦10; R 11 ~R 36 are each independently a hydrogen atom or a substituent having at least one element selected from carbon, hydrogen, oxygen, fluorine, chlorine, bromine, iodine, nitrogen, sulfur, phosphorus, boron, and silicon. When m is 2 or more, a plurality of R 11 and R 12 may be the same or different. Any R 11 ~R 36 , preferably R 11 and R 12 may combine together to form a ring other than a benzene ring.

[0041] Specific examples of such compounds include mono-substituted dialkoxypropanes such as 2-isopropyl-1,3-dimethoxypropane, 2-s-butyl-1,3-dimethoxypropane, and 2-cumyl-1,3-dimethoxypropane; 2-isopropyl-2-isobutyl-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, and the like. Methoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-diethoxypropane, 2,2-diisobutyl-1,3-dibutoxypropane, 2,2-di-s-butyl-1,3-dimethoxypropane, 2,2-dineopentyl-1,3-dimethoxypropane, 2-isopropyl -2-isopentyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane and other 2-substituted dialkoxypropanes; 2,3-dicyclohexyl-1,4-diethoxybutane, 2,3-dicyclohexyl-1,4-diethoxybutane, 2,3-diisopropyl-1,4-diethoxybutane, 2,4-diphenyl-1,5-dimethoxypentane, 2,5-diphenyl-1,5-dimethoxyhexane, 2,4 2-Diisopropyl-1,5-dimethoxypentane, 2,4-diisobutyl-1,5-dimethoxypentane, 2,4-diisoamyl-1,5-dimethoxypentane, and other dialkoxyalkanes; 2-methyl-2-methoxymethyl-1,3-dimethoxypropane, 2-cyclohexyl-2-ethoxymethyl-1,3-diethoxypropane, 2-cyclohexyl-2-methoxymethyl-1,3-dimethoxypropane, and other trialkoxyalkanes; etc. Polyether compounds may be used singly or in combination of two or more kinds.Among these, 1,3-diethers are preferred, and 2-isopropyl-2-isobutyl-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, and 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane are particularly preferred.

[0042] In the solid titanium catalyst component (I), the halogen / titanium (atomic ratio) (i.e., the number of moles of halogen atoms / the number of moles of titanium atoms) is 2 to 100, preferably 4 to 90, the electron donor component (1) / titanium atom (molar ratio) is 0 to 100, preferably 0 to 10, and the electron donor component (2) / titanium atom (molar ratio) is 0 to 100, preferably 0 to 10. The magnesium / titanium (atomic ratio) (i.e., the number of moles of magnesium atoms / the number of moles of titanium atoms) is 2 to 100, preferably 4 to 50.

[0043] As more detailed preparation conditions for the solid titanium catalyst component (I), the conditions described in, for example, EP585869A1 and JP-A-5-170843 can be suitably used, except for the use of the electron donor component (2). [Organometallic compound catalyst component (II)] The organometallic compound catalyst component (II) is a component containing a metal element selected from Groups 1, 2, and 13 of the periodic table. For example, compounds containing a Group 13 metal (such as organoaluminum compounds), alkyl complexes of Group 1 metals and aluminum, organometallic compounds of Group 2 metals, etc. can be used. Among these, organoaluminum compounds are preferred.

[0044] As the organometallic compound catalyst component (II), specifically, the organometallic compound catalyst components described in known documents such as the above-mentioned EP585869A1 can be suitably used.

[0045] As long as the object of the present invention is not impaired, in addition to the electron donor component (1) and electron donor component (2) explained above, a known electron donor component (3) may be used in combination.

[0046] As the electron donor component (3), an organosilicon compound is preferred. This organosilicon compound is, for example, a compound represented by the following formula.

[0047] R n Si(OR') 4-n (In the formula, R and R' are hydrocarbon groups, and n is an integer where 0 < n < 4.) Specific examples of the organosilicon compound represented by the above formula include diisopropyldimethoxysilane, t-butylmethyldimethoxysilane, t-butylmethyldiethoxysilane, t-amylmethyldiethoxysilane, dicyclohexyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylmethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, t-butyltriethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, cyclohexyltrimethoxysilane, cyclopentyltrimethoxysilane, 2-methylcyclopentyltrimethoxysilane, cyclopentyltriethoxysilane, dicyclopentyldimethoxysilane, dicyclopentyldiethoxysilane, tricyclopentylmethoxysilane, dicyclopentylmethylmethoxysilane, dicyclopentylethylmethoxysilane, cyclopentyldimethylethoxysilane, etc. Among them, vinyltriethoxysilane, diphenyldimethoxysilane, dicyclohexyldimethoxysilane, cyclohexylmethyldimethoxysilane, dicyclopentyldimethoxysilane are preferred.

[0048] Also, the silane compound represented by the following formula described in International Publication No. 2004 / 016662 pamphlet is also a preferred example of the organosilicon compound.

[0049] Si(OR a )3(NR b R c ) In the above formula, R ais a hydrocarbon group having 1 to 6 carbon atoms. For example, it is an unsaturated or saturated aliphatic hydrocarbon group having 1 to 6 carbon atoms, and a hydrocarbon group having 2 to 6 carbon atoms is particularly preferred. Specific examples include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, an n-pentyl group, an iso-pentyl group, a cyclopentyl group, an n-hexyl group, and a cyclohexyl group. Of these, an ethyl group is particularly preferred.

[0050] R b is a hydrocarbon group having 1 to 12 carbon atoms or hydrogen. For example, it is an unsaturated or saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms or hydrogen. Specific examples include a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, an n-pentyl group, an iso-pentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, and an octyl group. Among these, an ethyl group is particularly preferred.

[0051] R c is a hydrocarbon group having 1 to 12 carbon atoms. For example, it is an unsaturated or saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms. Specific examples include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, an n-pentyl group, an iso-pentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, and an octyl group. Among these, an ethyl group is particularly preferable.

[0052] Specific examples of the organosilicon compound represented by the above formula include dimethylaminotriethoxysilane, diethylaminotriethoxysilane, diethylaminotrimethoxysilane, diethylaminotri-n-propoxysilane, di-n-propylaminotriethoxysilane, methyl n-propylaminotriethoxysilane, t-butylaminotriethoxysilane, ethyl n-propylaminotriethoxysilane, ethyl isopropylaminotriethoxysilane, methylethylaminotriethoxysilane, and the like.

[0053] Further, other examples of the organosilicon compound include compounds represented by the following formula:

[0054] RNSi(OR a )3 In the above formula, RN is a cyclic amino group. Specific examples include a perhydroquinolino group, a perhydroisoquinolino group, a 1,2,3,4-tetrahydroquinolino group, a 1,2,3,4-tetrahydroisoquinolino group, and an octamethyleneimino group. a is the same as above.

[0055] Specific examples of organosilicon compounds represented by the above formula include (perhydroquinolino)triethoxysilane, (perhydroisoquinolino)triethoxysilane, (1,2,3,4-tetrahydroquinolino)triethoxysilane, (1,2,3,4-tetrahydroisoquinolino)triethoxysilane, octamethyleneiminotriethoxysilane, and the like.

[0056] The organosilicon compounds described above may be used in combination of two or more kinds.

[0057] [polymerization] The propylene-ethylene block copolymer, which is a preferred embodiment of the propylene polymer (A), can be produced by polymerizing propylene in the presence of the above-mentioned olefin polymerization catalyst and then copolymerizing propylene and ethylene, or by polymerizing propylene in the presence of a prepolymerization catalyst obtained by prepolymerization and then copolymerizing propylene and ethylene.

[0058] The prepolymerization is carried out by prepolymerizing an olefin in an amount of usually 0.1 to 1000 g, preferably 0.3 to 500 g, and particularly preferably 1 to 200 g per 1 g of the olefin polymerization catalyst. In the prepolymerization, a catalyst having a higher concentration than the catalyst concentration in the system in the main polymerization can be used.

[0059] The concentration of the solid titanium catalyst component (I) in the prepolymerization is usually 0.001 to 200 millimoles, preferably 0.01 to 50 millimoles, more preferably 0.1 to 20 millimoles, calculated as titanium atom per liter of the liquid medium.

[0060] The amount of the organometallic compound catalyst component (II) in the prepolymerization may be such that usually 0.1 to 1000 g, preferably 0.3 to 500 g, of polymer is produced per gram of the solid titanium catalyst component (I), and is usually 0.1 to 300 mol, preferably 0.5 to 100 mol, more preferably 1 to 50 mol per mol of titanium atom in the solid titanium catalyst component (I).

[0061] In the preliminary polymerization, the above-mentioned electron donor component can be used as necessary. In this case, the amount of the component is usually 0.1 to 50 mol, preferably 0.5 to 30 mol, more preferably 1 to 10 mol per mol of titanium atom in the solid titanium catalyst component (I).

[0062] The prepolymerization can be carried out under mild conditions by adding an olefin and the above-mentioned catalyst components to an inert hydrocarbon medium. When an inert hydrocarbon medium is used, the prepolymerization is preferably carried out in a batch manner.

[0063] Specific examples of the inert hydrocarbon medium include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, methylcyclopentane, cyclohexane, cycloheptane, methylcycloheptane, and cyclooctane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride and chlorobenzene; and mixtures thereof. Among these, aliphatic hydrocarbons are preferred.

[0064] The prepolymerization can be carried out using the olefin itself as a solvent, or in the substantial absence of a solvent. In this case, it is preferable to carry out the prepolymerization continuously.

[0065] The olefin used in the prepolymerization may be the same as or different from the olefin used in the main polymerization described below. As the olefin, propylene is particularly preferred.

[0066] The temperature during the prepolymerization is usually from -20 to 100°C, preferably from -20 to 80°C, and more preferably from 0 to 40°C.

[0067] Next, the main polymerization, which is carried out after or without going through preliminary polymerization, will be described.

[0068] This polymerization is divided into a step for producing a propylene homopolymer component and a step for producing a propylene-ethylene copolymer component.

[0069] The main polymerization (and preliminary polymerization) can be carried out by any of liquid phase polymerization methods such as bulk polymerization, solution polymerization, and suspension polymerization, or gas phase polymerization methods. As a process for producing a propylene homopolymer component, liquid phase polymerization methods such as bulk polymerization and suspension polymerization, or gas phase polymerization methods are preferred. As a process for producing a propylene-ethylene copolymer component, liquid phase polymerization methods such as bulk polymerization and suspension polymerization, or gas phase polymerization methods are preferred, and gas phase polymerization methods are more preferred.

[0070] When the main polymerization is carried out in the form of a slurry polymerization reaction, the reaction solvent may be the inert hydrocarbon used in the above-mentioned preliminary polymerization, or an olefin which is liquid at the reaction temperature and pressure.

[0071] In the main polymerization, the solid titanium catalyst component (I) is used in an amount of usually 0.0001-0.5 millimoles, preferably 0.005-0.1 millimoles, calculated as titanium atoms per 1 liter of polymerization volume. The organometallic compound catalyst component (II) is used in an amount of usually 1-2000 moles, preferably 5-500 moles, per mole of titanium atoms in the prepolymerized catalyst component in the polymerization system. When an electron donor component is used, it is used in an amount of usually 0.001-50 moles, preferably 0.01-30 moles, more preferably 0.05-20 moles, per mole of the organometallic compound catalyst component (II).

[0072] If this polymerization is carried out in the presence of hydrogen, the molecular weight of the resulting polymer can be adjusted (reduced), and a polymer with a high melt flow rate (MFR) can be obtained. The amount of hydrogen required to adjust the molecular weight varies depending on the type of manufacturing process used, the polymerization temperature, and the pressure, so it can be adjusted appropriately.

[0073] In the process for producing the propylene homopolymer component, the MFR can be adjusted by adjusting the polymerization temperature and the amount of hydrogen. Also, in the process for producing the propylene-ethylene copolymer component, the intrinsic viscosity can be adjusted by adjusting the polymerization temperature, pressure, and the amount of hydrogen.

[0074] In this polymerization, the polymerization temperature of the olefin is usually 0 to 200° C., preferably 30 to 100° C., and more preferably 50 to 90° C. The pressure (gauge pressure) is usually normal pressure to 100 kgf / cm. 2 (9.8MPa), preferably 2 to 50kgf / cm 2 (0.20~4.9MPa).

[0075] In the production of the propylene-ethylene block copolymer, which is a preferred embodiment of the propylene polymer (A), the polymerization can be carried out by any of batch, semi-continuous, and continuous methods. Furthermore, the reactor shape can be either tubular or tank type. Furthermore, the polymerization can be carried out in two or more stages by changing the reaction conditions. In this case, the tubular type and tank type can be combined.

[0076] In order to obtain a propylene-ethylene copolymer portion in a propylene-ethylene block copolymer, which is a preferred embodiment of the propylene-based polymer (A), the ethylene / (ethylene+propylene) gas ratio is controlled in the polymerization step 2 described below. The ethylene / (ethylene+propylene) gas ratio is usually 5 to 80 mol%, preferably 10 to 70 mol%, and more preferably 15 to 60 mol%.

[0077] As mentioned above, the decane-insoluble portion (a2) of the propylene-ethylene block copolymer is mainly composed of a propylene homopolymer component. On the other hand, the decane-soluble portion (a1) is mainly composed of an ethylene-propylene copolymer component, which is a rubber-like component. For example, a propylene-ethylene block copolymer, which is a preferred embodiment of the propylene-based polymer (A), can be obtained by continuously carrying out the following two polymerization steps 1 and 2. (Polymerization step 1) A process for polymerizing propylene in the presence of a solid titanium catalyst component to produce a propylene homopolymer component (propylene homopolymer production process). (Polymerization step 2) A process for producing an ethylene-propylene copolymer component by copolymerizing propylene and ethylene in the presence of a solid titanium catalyst component (copolymer rubber production process).

[0078] In particular, it is more preferable to carry out the polymerization step 1 in the first stage and the polymerization step 2 in the second stage. Each of the polymerization steps 1 and 2 can be carried out using two or more polymerization tanks. The content of the decane-soluble part (a1) can be adjusted by the polymerization time (residence time) of the polymerization step 1 and the polymerization step 2. The polymerization step 1 in the first stage can be carried out in two or more polymerization tanks connected in series. In this case, the ratio of propylene to hydrogen in each tank can be different for each polymerization tank.

[0079] The propylene-based polymer (A) used in the present invention may contain one or more types of biomass-derived monomers. The same type of monomer constituting the polymer may be only biomass-derived monomers, or may contain both biomass-derived monomers and fossil fuel-derived monomers. The biomass-derived monomer is a monomer made from any renewable natural raw material, such as fungi, yeast, algae, and bacteria, or from animal or plant origin, and its residue, and contains carbon as the raw material. 14 C isotope 10 -12 The biomass-derived monomer is contained in a ratio of about 100 (pMC) as measured in accordance with ASTM D 6866. The biomass-derived monomer can be obtained by a conventionally known method. It is preferable from the viewpoint of reducing the environmental load that the propylene-based polymer (A) used in the present invention contains a biomass-derived monomer. If the polymer production conditions such as the polymerization catalyst and polymerization temperature are the same, even if the raw material olefin contains a biomass-derived olefin, 14 C isotope 10 -12 Other than the proportion of propylene in the polymer, the molecular structure is the same as that of propylene polymers made from fossil fuel-derived monomers, and therefore the performance is said to be the same.

[0080] The propylene polymer (A) according to the present invention may contain propylene derived from chemical recycling. The propylene constituting the polymer may be only propylene derived from chemical recycling, or may contain propylene derived from chemical recycling and propylene derived from fossil fuel and / or propylene derived from biomass. The propylene derived from chemical recycling is obtained by a conventionally known method. It is preferable that the propylene polymer (A) according to the present invention contains propylene derived from chemical recycling from the viewpoint of reducing the environmental load (mainly reducing waste). Even if the raw material monomer contains a monomer derived from chemical recycling, the monomer derived from chemical recycling is a monomer obtained by depolymerizing or pyrolyzing a polymer such as waste plastic back to a monomer unit such as propylene, and a monomer produced using the monomer as a raw material. Therefore, if the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are the same, the molecular structure is the same as that of a propylene homopolymer made of a monomer derived from a fossil fuel. Therefore, the performance is said to be the same.

[0081] <Propylene homopolymer (B)> The propylene homopolymer (B) used in the present invention is a propylene homopolymer having a melt flow rate (230° C., 2.16 kg load) of 10 to 500 g / 10 min.

[0082] The propylene homopolymer (B) may be a polymer obtained by polymerizing substantially only propylene. For example, a homopolymer obtained by polymerizing only propylene, or a crystalline polymer obtained by copolymerizing propylene with 6 mol % or less, preferably 3 mol % or less, of another α-olefin may be used. Among them, a homopolymer obtained by polymerizing only propylene is preferred.

[0083] The propylene homopolymer (B) can be produced by polymerizing a monomer mainly composed of propylene by a known method. For example, it can be obtained by polymerizing a monomer mainly composed of propylene in the presence of an olefin polymerization catalyst containing the solid titanium catalyst component (I) and the organometallic compound catalyst component (II) described above, or a combined catalyst of titanium trichloride and an alkylaluminum compound, usually called a Ziegler-Natta type catalyst. The polymerization reaction may be carried out in a continuous manner or a batch manner. For example, it can be suitably produced by carrying out only the polymerization step 1 described above.

[0084] In the polymerization reaction, the polymerization temperature is usually 0 to 200° C., preferably 30 to 100° C., and more preferably 50 to 90° C. The pressure (gauge pressure) is usually normal pressure to 100 kgf / cm. 2 (9.8MPa), preferably 2 to 50kgf / cm 2 (0.20~4.9MPa).

[0085] The melt flow rate of the propylene homopolymer (B) (230° C., 2.16 kg load) is from 10 to 500 g / 10 min, preferably from 10 to 300 g / 10 min, and more preferably from 20 to 250 g / 10 min.

[0086] The propylene homopolymer (B) may be one type of polymer, or two or more types of propylene homopolymers may be arbitrarily combined within the range that satisfies the above melt flow rate as a whole.

[0087] The propylene homopolymer (B) used in the present invention may contain biomass-derived propylene. The propylene constituting the polymer may be only biomass-derived propylene, or may contain both biomass-derived propylene and fossil fuel-derived propylene. Biomass-derived propylene is a monomer made from any renewable natural raw material, such as fungi, yeast, algae, and bacteria, or from plants or animals, and its residues, and contains propylene as carbon. 14 C isotope 10 -12The biomass-derived propylene is contained in a ratio of about 100 (pMC) as measured in accordance with ASTM D 6866. Biomass-derived propylene can be obtained by a conventionally known method. It is preferable from the viewpoint of reducing the environmental load that the propylene homopolymer (B) used in the present invention contains a biomass-derived monomer. If the polymer production conditions such as the polymerization catalyst and polymerization temperature are the same, even if the raw material propylene contains biomass-derived propylene, 14 C isotope 10 -12 Other than the proportion of propylene in the polymer, its molecular structure is the same as that of propylene homopolymers made from fossil fuel-derived propylene, and therefore its performance is said to be the same.

[0088] The propylene homopolymer (B) used in the present invention may contain propylene derived from chemical recycling as a monomer, similar to the above-mentioned propylene-based polymer (A). That is, the propylene constituting the polymer may be only propylene derived from chemical recycling, or may contain propylene derived from chemical recycling and propylene derived from fossil fuels and / or propylene derived from biomass.

[0089] <Ethylene-α-olefin copolymer (C)> The ethylene-α-olefin copolymer (C) used in the present invention is a random copolymer of ethylene and an α-olefin having 4 to 8 carbon atoms, and has a density of 0.850 to 0.880 g / cm. 3 It is an ethylene-α-olefin copolymer having a melt flow rate (230°C, 2.16 kg load) of 0.5 to 30 g / 10 minutes and a melting point peak of 110°C or higher. This ethylene-α-olefin copolymer (C) is expected to contribute to improving the dimensional stability (reducing the linear expansion coefficient) of the molded product (i) and a laminated structure containing it through a synergistic effect with other components, and also contribute to improving other physical properties, resulting in the molded product achieving a high level of balance in physical properties.

[0090] As the α-olefin having 4 to 8 carbon atoms constituting the ethylene-α-olefin copolymer (C), 1-butene, 1-hexene, and 1-octene are preferred. The α-olefins may be used alone or in combination of two or more. As the ethylene-α-olefin copolymer (C), ethylene-octene copolymers and ethylene-butene copolymers are particularly preferred.

[0091] The melt flow rate of the ethylene / α-olefin copolymer (C) (230° C., 2.16 kg load) is from 0.5 to 30 g / 10 minutes, preferably from 1 to 25 g / 10 minutes, and more preferably from 2 to 20 g / 10 minutes.

[0092] If the melt flow rate (230°C, 2.16 kg load) of the ethylene-α-olefin copolymer (C) is 0.5 g / 10 min or more, the polypropylene resin composition is less likely to have a reduced fluidity or poor dispersion during kneading, and the physical properties such as impact resistance and the surface appearance of the molded product are less likely to deteriorate. If the melt flow rate (230°C, 2.16 kg load) is 30 g / 10 min or less, the molded product (i) and the laminate structure having the same tend to have sufficient impact resistance.

[0093] The density of the ethylene-α-olefin copolymer (C) is 0.850 to 0.880 g / cm 3 and preferably 0.855 to 0.875 g / cm 3 It is.

[0094] The melting peak of the ethylene-α-olefin copolymer (C) is 110°C or higher, preferably 110 to 130°C. The melting peak means a value determined by a differential scanning calorimeter (DSC). Specifically, the temperature at the maximum peak position when an endothermic curve is determined by a differential scanning calorimeter (DSC) can be determined as the melting peak (Tm). When the melting peak of the ethylene-α-olefin copolymer (C) satisfies the above-mentioned high temperature range, the laminate structure of the present invention in which the molded product (i) made of a polypropylene resin composition containing the copolymer and the cured resin layer (ii) are laminated has excellent adhesive strength.

[0095] <Inorganic filler (D)> The inorganic filler (D) used in the present invention may be a known inorganic filler, and is not particularly limited, but examples thereof include talc, calcium carbonate, natural mica, synthetic mica, wollastonite, montmorillonite, etc. The inorganic filler (D) may be used alone or in combination of two or more. Among them, talc is preferred. By using such an inorganic filler (D), the mechanical properties of the molded body (i) and the laminated structure having the same are improved.

[0096] The inorganic filler (D) may be dispersed in the resin composition, and is not particularly limited, but its average particle size is, for example, 1 μm to 20 μm, preferably more than 3.0 μm and 10.0 μm or less, preferably 3.0 μm to 8.0 μm, and more preferably 3.0 μm to 7.0 μm. This average particle size is a value measured by a laser diffraction method. Specifically, it is a particle size at an integrated value of 50% in the particle size distribution obtained by a particle size distribution meter such as a laser diffraction scattering type particle size distribution meter, and examples of the measuring device include MT3300EXII manufactured by Microtrac and LA-920 type manufactured by Horiba, Ltd.

[0097] The aspect ratio of the inorganic filler (D) is not particularly limited, but is usually 3 or more and less than 15, preferably 4 to 13, and more preferably 5 to 11. In general, the aspect ratio is a value that represents the ratio of the major axis and thickness of the filler, or the ratio of the major side and minor side. If this aspect ratio is 3 or more, the rigidity and dimensional stability of the molded body tend not to decrease. If it is less than 15, the balance of mechanical properties tends not to decrease, and furthermore, the impact strength tends not to decrease. Specifically, this aspect ratio is a value obtained by taking a photograph using an electron microscope, measuring the major axis and thickness of the powder, calculating the average value, and calculating the ratio of the average particle size / average thickness.

[0098] The inorganic filler (D) contributes to improving the dimensional stability (reducing the linear expansion coefficient) of the molded body (i) and the laminated structure having the same, and also contributes to improving mechanical properties such as rigidity and impact strength. When the inorganic filler (D) has the above-mentioned average particle size (and aspect ratio), it is preferable because it is easy to achieve a high level of balance of physical properties, particularly excellent dimensional stability, rigidity, and impact strength, due to the synergistic effect with other components.

[0099] As the inorganic filler (D), inorganic fillers in any shape, such as granular, plate-like, rod-like, fibrous, whisker-like, etc., can be used. In addition, inorganic fillers commercially available as fillers for polymers can also be used. Furthermore, in addition to the general powder and roving shapes, chopped strand, compressed solid, pellet (granulated) and granular shapes, which are easy to handle, can also be used. Among these, powder, compressed solid and granular shapes are preferred.

[0100] The inorganic filler (D) may be a mixture of two or more forms of inorganic filler.

[0101] The method of producing the inorganic filler (D) is not particularly limited, and it can be produced by various known methods. When talc is used as the inorganic filler (D), for example, talc having a specific average particle size and aspect ratio can be produced by pulverization or granulation. Specifically, for example, there is a method of pulverizing raw talc with an impact pulverizer or a micron mill type pulverizer, and then further pulverizing with a jet mill and classifying and adjusting with a cyclone or a micron separator. The aspect ratio and average particle size of talc can be appropriately adjusted by the pulverizing device and pulverization time, and talc with a controlled shape can be obtained by classifying as necessary.

[0102] As the inorganic filler (D), a filler obtained by crushing raw stone may be used directly, or at least a part of the filler may be surface-treated. For the surface treatment, various surface treatment agents such as organic titanate coupling agents, organic silane coupling agents, unsaturated carboxylic acids or modified polyolefins grafted with their anhydrides, fatty acids, fatty acid metal salts, fatty acid esters, etc. may be used. The surface treatment agents may be used alone or in combination of two or more.

[0103] The polypropylene resin composition according to the present invention may contain other additives such as nucleating agents, heat stabilizers, antistatic agents, weather stabilizers, light stabilizers, antioxidants, antioxidants, fatty acid metal salts, softeners, dispersants, fillers, colorants, lubricants, pigments, etc., as necessary, within the scope of the present invention. The additives may be mixed in any order, and may be mixed simultaneously, or a multi-stage mixing method may be used in which some components are mixed and then other components are mixed.

[0104] <Polypropylene resin composition> The polypropylene resin composition according to the present invention contains 5 to 47 parts by mass of a propylene polymer (A), 20 to 30 parts by mass of a propylene homopolymer (B), 23 to 30 parts by mass of an ethylene-α-olefin copolymer (C), and 30 to 40 parts by mass of an inorganic filler (D) (wherein the total amount of components (A) to (D) is 100 parts by mass).

[0105] The polypropylene resin composition according to the present invention preferably contains 7 to 35 parts by mass of a propylene polymer (A), 20 to 30 parts by mass of a propylene homopolymer (B), 23 to 28 parts by mass of an ethylene-α-olefin copolymer (C), and 32 to 40 parts by mass of an inorganic filler (D) (wherein the total amount of the components (A) to (D) is 100 parts by mass).

[0106] More preferably, the polypropylene resin composition according to the present invention contains 8 to 28 parts by mass of a propylene polymer (A), 23 to 30 parts by mass of a propylene homopolymer (B), 24 to 28 parts by mass of an ethylene-α-olefin copolymer (C), and 33 to 38 parts by mass of an inorganic filler (D) (wherein the total amount of the components (A) to (D) is 100 parts by mass).

[0107] The polypropylene resin composition according to the present invention particularly preferably contains 10 to 22 parts by mass of a propylene polymer (A), 25 to 30 parts by mass of a propylene homopolymer (B), 24 to 27 parts by mass of an ethylene-α-olefin copolymer (C), and 34 to 37 parts by mass of an inorganic filler (D) (wherein the total amount of components (A) to (D) is 100 parts by mass).

[0108] The polypropylene resin composition according to the present invention can be produced by blending the above-mentioned components (A) to (D) and optional components such as additives as required. The components may be blended sequentially in any order, or may be mixed simultaneously. A multi-stage mixing method may be adopted in which some components are mixed and then other components are mixed. Specifically, for example, the polypropylene resin composition can be produced by first blending the components (A) to (C), which are resin components (organic compound components) in the polypropylene resin composition, and then adding and blending component (D) and optional components such as additives as required.

[0109] Examples of the method for blending the components include a method in which the components are mixed or melt-kneaded simultaneously or sequentially using a mixing device such as a Banbury mixer, a single-screw extruder, a twin-screw extruder, or a high-speed twin-screw extruder.

[0110] The polypropylene resin composition according to the present invention has a melt flow rate (230°C, 2.16 kg load) of usually 23 g / 10 min or more, preferably more than 23 g / 10 min and 50 g / 10 min or less. By setting the melt flow rate within this range, the moldability is improved and deterioration of the coating appearance after injection molding can be suppressed.

[0111] <Molded object (i)> The molded article (i) according to the present invention is a molded article obtained from the polypropylene resin composition according to the present invention described above. The molded article (i) can be obtained by appropriately molding the polypropylene resin composition according to the present invention. The molding method of the polypropylene resin composition is not particularly limited, and various methods known as molding methods for resin compositions can be used. As the molding method of the molded article (i), injection molding and press molding are particularly preferred. The molded article (i) obtained from the polypropylene resin composition according to the present invention has small dimensional change due to temperature change and excellent dimensional stability, and the laminate structure having the molded article (i) also has small dimensional change due to temperature change and excellent dimensional stability.

[0112] [Cured resin layer (ii)] The cured resin layer (ii) according to the present invention is a layer of a cured resin containing a curable resin (E) having a urethane bond.

[0113] The curable resin (E) used in the present invention is a curable resin having a urethane bond. As such a curable resin (E), a known curable resin having a urethane bond can be used without limitation, specifically, polyurethane resin and the like can be mentioned. The curable resin (E) having a urethane bond may contain a urea bond, a biuret bond, and the like in addition to the urethane bond. In the production of the resin cured layer (ii) containing the curable resin (E) having a urethane bond, a curing agent may be used as necessary.

[0114] The polyurethane resin used as the curable resin (E) having a urethane bond may be a known polyurethane resin, such as a polymer obtained by reacting a polyfunctional isocyanate or a derivative thereof with a polyol or a derivative thereof and / or a polyester or a derivative thereof.

[0115] Examples of polyfunctional isocyanates or derivatives thereof that are raw materials for polyurethane resins include polyfunctional isocyanates such as tolylene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), isophorone diisocyanate, and norbornane diisocyanate, as well as their block derivatives or isocyanurate derivatives, etc. These can be used alone or in combination of two or more.

[0116] Examples of polyols or derivatives thereof that are raw materials for polyurethane resins include polypropylene glycols, polyethylene glycol-polypropylene glycol block copolymers, and polypropylene glycols with amine terminals, each having a molecular weight of 500 to 100,000. These may be used alone or in combination of two or more.

[0117] Examples of polyesters or derivatives thereof that are raw materials for polyurethane resins include polyethylene terephthalate, polyethylene isophthalate, polybutylene terephthalate, and polybutylene isophthalate, as well as reaction products of these polyesters with polyethylene glycol or polypropylene glycol, etc. These may be used alone or in combination of two or more.

[0118] To obtain a polyurethane resin from a polyfunctional isocyanate and a polyol and / or polyester, for example, the two can be mixed and stirred in an equimolar ratio or an excess of the polyfunctional isocyanate. In this case, a polymerization accelerator such as an amine compound may be added.

[0119] The resin cured layer (ii) according to the present invention may be produced by applying a composition such as an adhesive or paint containing the raw material of the polyurethane resin described above onto the molded body (i) and curing it, or by applying it onto another member to be bonded to the molded body (i) and curing it. In addition, a laminate consisting of the molded body (i), the resin cured layer (ii), and another member may be produced by applying a composition containing the raw material of the polyurethane resin described above onto the molded body (i), bonding the other member to be bonded to the molded body (i) before the composition cures, and curing it, or by applying it onto a member other than the molded body (i), bonding the molded body (i) to the composition before the composition cures, and curing it.

[0120] The resin cured layer (ii) according to the present invention may be obtained, for example, by forming a layer made of a composition obtained by mixing a first agent containing a curable resin (E) having a urethane bond and a second agent containing a curing agent, and curing the layer; by forming a layer made of a moisture-curable composition containing a curable resin (E) having a urethane bond, and curing the layer; or by forming a layer containing a curable resin (E) having a urethane bond, which is a thermosetting resin, and curing the layer by heating.

[0121] The resin cured layer (ii) according to the present invention is preferably a cured adhesive containing a polyurethane resin or an adhesive forming a urethane bond. Examples of the adhesive include a room temperature two-liquid curing adhesive, a one-liquid moisture curing adhesive, and a heat curing adhesive. The resin cured layer obtained by curing such an adhesive contains a curable resin having a urethane bond.

[0122] As the adhesive containing polyurethane resin or the adhesive that forms a urethane bond, any known adhesive can be used, but two-component or one-component moisture-curing adhesive, or water-based or water-based emulsion adhesive is preferred. Specific examples include two-component or one-component moisture-curing adhesives or water-based or water-based emulsion adhesives containing polyurethane resin such as urethane resin-based, acrylic resin-based, urethane-acrylic resin-based, or epoxy resin-based adhesives, or urethane resin-based, acrylic resin-based, urethane-acrylic resin-based, or epoxy resin-based adhesives that form urethane bonds after application.

[0123] The adhesive can use a combination of a base agent (a composition containing an isocyanate compound) and a curing agent (a composition containing an active hydrogen-containing compound such as polyol). Examples of such base agents include isocyanate-based and polyisocyanate-based agents, and examples of curing agents include polyol-based and polyamine-based agents. The curing agent may be latent-treated and then blended into the adhesive, but it is usually mixed with the adhesive in a specific ratio just before application. As the base agent, isocyanate-based and polyisocyanate-based agents are preferred. As the adhesive, commercially available polyurethane-based adhesives can also be used.

[0124] Among such adhesives, an adhesive containing a urethane prepolymer and an isocyanate derivative is preferred, and a urethane-based adhesive containing a polyether-skeleton urethane prepolymer and an aliphatic isocyanate derivative is more preferred. That is, it is preferred that the resin cured layer containing the curable resin (E) having a urethane bond is obtained by curing a urethane-based adhesive containing a polyether-skeleton urethane prepolymer and an aliphatic isocyanate derivative.

[0125] ·Urethane prepolymer The urethane prepolymer can be obtained by reacting a polyisocyanate compound having two or more isocyanate groups in one molecule with an active hydrogen compound having two or more active hydrogens in one molecule that react with isocyanate groups.

[0126] Examples of polyisocyanate compounds used in the preparation of urethane prepolymers include aliphatic polyisocyanates such as hexamethylene diisocyanate, 1,5-pentamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine methyl ester diisocyanate; and 1,4-cyclohexane diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, hydrogenated tolylene diisocyanate, norbornene diisocyanate, hydrogenated m-xylylene diisocyanate, and hydrogenated p-xylylene diisocyanate. Examples of the polyisocyanates include alicyclic polyisocyanates, p-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 3,3'-dimethyldiphenyl-4,4'-diisocyanate, 4,4'-diphenylmethane diisocyanate, naphthalene diisocyanate, m-xylylene diisocyanate, and aromatic diisocyanates such as tolidine diisocyanate, and the above polyisocyanates modified with carbodiimide or isocyanurate, which can be used alone or in combination of two or more. Among these, aromatic isocyanates are more preferably used from the viewpoint of excellent adhesion and curability.

[0127] The active hydrogen compound used in the preparation of the urethane prepolymer may be a polyol compound having two or more alcoholic hydroxyl groups in one molecule, such as polyether polyol, polyester polyol, or other polyols, which may be used alone or in combination of two or more. It is preferable to use polyether polyol. The urethane prepolymer obtained by using polyether polyol as the active hydrogen compound has a polyether skeleton, and the obtained adhesive has excellent adhesion performance with the molded body (i). As these polyol compounds, those having a number average molecular weight of 100 to 50,000, particularly 300 to 10,000 are preferred.

[0128] Specific examples of polyether polyols, which are active hydrogen compounds that can be suitably used in preparing urethane prepolymers, include polyoxyethylene glycol, polyoxypropylene glycol, polyoxyethyleneoxypropylene glycol, polyoxytetramethylene glycol, polyoxyhexamethylene glycol, and the like, as well as low molecular weight active hydrogen compounds having two or more active hydrogens, for example, random copolymers obtained by ring-opening polymerization of propylene oxide and / or ethylene oxide in the presence of one or more of the following: diols, such as bisphenol A, ethylene glycol, propylene glycol, butylene glycol, and 1,6-hexanediol; triols, such as glycerin, trimethylolpropane, and 1,2,6-hexanetriol; and amines, such as ammonia, methylamine, ethylamine, propylamine, and butylamine.

[0129] The urethane prepolymer can be obtained by reacting a polyol compound with a polyisocyanate compound, heating as necessary, in a ratio of more than 1 mole of isocyanate group contained in the polyisocyanate compound to 1 mole of hydroxyl group contained in the polyol compound, that is, a chemical equivalent ratio (NCO / OH) of more than 1. Such a urethane prepolymer usually has isocyanate groups at both ends of the molecule. As the urethane prepolymer, a urethane prepolymer obtained by reacting a polyol compound with a polyisocyanate compound in a ratio of 1.5 to 20 in chemical equivalent ratio (NCO / OH) of the hydroxyl group contained in the polyol compound and the isocyanate group contained in the polyisocyanate compound and being liquid at 23°C is more preferable in terms of workability, physical properties of the cured product, etc. In addition, as the urethane prepolymer, a urethane prepolymer obtained by reacting a polyether polyol with an aromatic polyisocyanate compound is preferable from the viewpoint of excellent adhesion and curability.

[0130] ·Isocyanate derivatives As the isocyanate derivative, any isocyanate derivative that acts as a base agent can be used without any particular limitation. For example, isocyanates, diisocyanates, polyisocyanates, and derivatives thereof can be used, and specifically, the above-mentioned polyfunctional isocyanate or its derivatives can be used.

[0131] The isocyanate derivative is preferably a compound having an isocyanurate structure and an isocyanate group. When a compound having an isocyanurate structure and an isocyanate group, particularly an aliphatic isocyanate derivative, is used as the isocyanate derivative, it is preferable because the adhesive strength with the molded body (i) is high.

[0132] The isocyanurate structure is a structure represented by the following formula (B1): The aliphatic isocyanate derivative can have at least one of the isocyanurate structures per molecule, and one preferred embodiment has one of the isocyanurate structures.

[0133] [ka] The above-mentioned isocyanate derivative can have at least one isocyanate group per molecule, preferably has a plurality of isocyanate groups, and more preferably has three or more isocyanate groups per molecule.

[0134] In the isocyanate derivative, the isocyanurate structure and the isocyanate group can be bonded directly or via a linking group, and one preferred embodiment is bonded via a linking group.

[0135] In the isocyanate derivative, the isocyanurate structure and the isocyanate group can be bonded directly or via a linking group, and one preferred embodiment is bonded via a linking group.

[0136] The linking group may be, for example, a hydrocarbon group that may have a heteroatom. The hydrocarbon group is preferably composed of only carbon atoms and hydrogen atoms. The hydrocarbon group is not particularly limited, but specifically includes, for example, an aliphatic hydrocarbon group, an aromatic hydrocarbon group, and a combination thereof. Among them, an aliphatic hydrocarbon group is preferred.

[0137] The aliphatic hydrocarbon group may be linear, branched, cyclic, or a combination thereof. Specific examples of the aliphatic hydrocarbon group include linear or branched aliphatic hydrocarbon groups. From the viewpoint of achieving superior effects of the present invention, the aliphatic hydrocarbon group is preferably a linear aliphatic hydrocarbon group. From the viewpoint of achieving superior effects of the present invention, the aliphatic hydrocarbon group preferably has a carbon number of 1 to 20, more preferably 3 to 10, and even more preferably 4 to 5. From the viewpoint of achieving superior effects of the present invention, the aliphatic hydrocarbon group is preferably a methylene group, an ethylene group, a propylene group, a trimethylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, or a decylene group, more preferably a butylene group or a pentylene group, and even more preferably a pentylene group.

[0138] The heteroatom that the hydrocarbon group may have is not particularly limited, and specific examples include, for example, an oxygen atom, a nitrogen atom, a sulfur atom, a halogen atom (such as a fluorine atom, a chlorine atom, a bromine atom, etc.) The above heteroatom may be bonded to another heteroatom, a carbon atom, or a hydrogen atom to form a functional group.

[0139] From the viewpoint of obtaining superior effects of the present invention, the isocyanate derivative is preferably a compound represented by the following formula (B2).

[0140] [ka] In formula (B2), R 141 , R 142, R 143 R each independently represents a hydrocarbon group which may have a heteroatom. 141 The hydrocarbon group which may have a hetero atom such as aryl, aryloxy ...

[0141] From the viewpoint of achieving superior effects of the present invention, the isocyanate derivative preferably contains an isocyanurate of an aliphatic polyisocyanate described below, more preferably contains an isocyanurate of pentamethylene diisocyanate (a compound represented by the following formula (B2-1)) and / or an isocyanurate of hexamethylene diisocyanate (a compound represented by the following formula (B2-2)), and even more preferably contains an isocyanurate of pentamethylene diisocyanate.

[0142] [ka] The isocyanate derivative may be, for example, a polyisocyanate compound. The polyisocyanate compound is not particularly limited as long as it is a compound in which a plurality of isocyanate groups are bonded to the linking group. Among them, aliphatic polyisocyanates (compounds in which a plurality of isocyanate groups are bonded to the aliphatic hydrocarbon group) are preferred.

[0143] Examples of the isocyanate derivative include aliphatic diisocyanates such as pentamethylene diisocyanate (PDI) and hexamethylene diisocyanate (HDI). The polyisocyanate compound that can constitute the isocyanate compound (B) may be one type or a combination of two or more types.

[0144] The isocyanate derivative is preferably the compound represented by the above formula (B2-1), because it is more effective in providing the effects of the present invention (initial adhesion and adhesion durability) and has a low viscosity and is therefore easily added to the composition.

[0145] From the viewpoint of achieving superior effects of the present invention (particularly adhesion durability), the content of the isocyanate derivative is preferably 0.10 to 10.0 mass %, and more preferably 0.50 to 5.0 mass %, based on the total amount of the composition of the present invention.

[0146] Additions The adhesive containing a polyurethane resin or the adhesive forming a urethane bond is a compound represented by the following formula (X) (wherein R 37 and R 38 Each of the groups independently represents a hydrocarbon group.) may contain an adduct of a phenol compound. This adduct can function as an adhesion promoter in an adhesive containing a polyurethane resin or an adhesive that forms a urethane bond.

[0147] [ka] In formula (X), R 37 and R 38 each independently represents a hydrocarbon group.

[0148] R 37 and R 38 The hydrocarbon group as is not particularly limited. The above-mentioned hydrocarbon group may have a heteroatom. One of the preferred embodiments is one that is composed of only carbon atoms and hydrogen atoms. The above-mentioned hydrocarbon group is not particularly limited, and specific examples thereof include an aliphatic hydrocarbon group, an aromatic hydrocarbon group, and a combination thereof. Among them, an aliphatic hydrocarbon group is preferred.

[0149] The aliphatic hydrocarbon group may be linear, branched, cyclic, or a combination thereof. Specific examples of the aliphatic hydrocarbon group include linear or branched aliphatic hydrocarbon groups. From the viewpoint of achieving superior effects of the present invention, the aliphatic hydrocarbon group is preferably a linear aliphatic hydrocarbon group. From the viewpoint of achieving superior effects of the present invention, the aliphatic hydrocarbon group preferably has a carbon number of 1 to 20, more preferably 1 to 10. From the viewpoint of achieving superior effects of the present invention, the aliphatic hydrocarbon group is preferably a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, or a decyl group, more preferably a methyl group.

[0150] Examples of the aromatic hydrocarbon group include an aryl group, a naphthyl group, etc. Examples of the aryl group include aryl groups having 6 to 18 carbon atoms, such as a phenyl group, a tolyl group, and a xylyl group.

[0151] The heteroatom that the hydrocarbon group may have is not particularly limited, and specific examples include, for example, an oxygen atom, a nitrogen atom, a sulfur atom, a halogen atom (such as a fluorine atom, a chlorine atom, a bromine atom, etc.) The above heteroatom may be bonded to another heteroatom, a carbon atom, or a hydrogen atom to form a functional group.

[0152] From the viewpoint of obtaining superior effects of the present invention, the compound represented by the above formula (X) is preferably camphene. Camphene is a compound represented by the following formula (X1).

[0153] [ka] In the present invention, the other compound forming the adduct is a phenol compound. The phenol compound is not particularly limited as long as it is a compound having a hydroxy group bonded to a benzene ring.

[0154] The phenolic compound may have one or more phenolic hydroxy groups (hydroxy groups directly bonded to a benzene ring) in one molecule, and preferably has one. Examples of the phenolic compound include compounds represented by the following formula (Y).

[0155] [ka] In formula (Y), R 39 represents a substituent; n2 represents 0 or 1 to 4.

[0156] R in formula (Y) 39 Examples of the substituent as the substituent include a hydrocarbon group and a hydroxy group.

[0157] n2 represents 0 or 1 to 4, and is preferably 0 from the viewpoint of obtaining superior effects of the present invention.

[0158] The phenol compound is preferably phenol from the viewpoint of obtaining superior effects of the present invention.

[0159] From the viewpoint of achieving superior effects of the present invention and less odor, the adduct is preferably a reaction product of one molecule of the compound represented by the formula (X) and one molecule of the phenol compound.

[0160] From the viewpoint of achieving superior effects of the present invention, the adduct preferably has a phenolic hydroxy group or a phenoxy group (either of which may further have the above-mentioned substituent on the benzene ring) due to the phenol compound.

[0161] The adduct may contain at least the reaction product, and may further contain reaction by-products and unreacted substances in addition to the reaction product.

[0162] Examples of the adduct include compounds represented by the following formulas (Z1) to (Z3).

[0163] [ka] In formula (Z1), R 40 and R 41 each independently represents a hydrocarbon group; R 42 represents a substituent; n3 represents 0 or 1 to 4.

[0164] In formula (Z1), R 40 and R 41 The hydrocarbon group as R in formula (X) 37 and R 38 R is the same as the hydrocarbon group. 42 The substituent as R in formula (Y) 39 n3 represents 0 or an integer of 1 to 4, and preferably 0.

[0165] [ka] In formula (Z2), R 43 and R 44 each independently represents a hydrocarbon group; R 45 represents a substituent; n4 represents 0 or an integer of 1 to 4.

[0166] In formula (Z2), R 43 and R 44 The hydrocarbon group as R in formula (X) 37 and R 38 R is the same as the hydrocarbon group. 45 The substituent as R in formula (Y) 39 n4 represents 0 or an integer of 1 to 4, and preferably 0.

[0167] [ka] In formula (Z3), R 51 and R 52 each independently represents a hydrocarbon group; R 53 represents a substituent; n5 represents 0 or an integer of 1 to 4.

[0168] In formula (Z3), R51 and R 52 The hydrocarbon group as R in formula (X) 37 and R 38 The same applies to the hydrocarbon group as above.

[0169] R 53 The substituent as R in formula (Y) 39 The substituents are the same as those in the above formula (I).

[0170] n5 represents 0 or 1 to 4, with 0 being preferred.

[0171] From the viewpoint of achieving superior effects of the present invention and less odor, the adduct preferably contains at least one compound selected from the group consisting of compounds represented by the following formulas (Z1-1), (Z1-2), (Z2-1), (Z2-2) and (Z3-1).

[0172] [ka]

[0173] [ka]

[0174] [ka] The method for producing the adduct is not particularly limited as long as it is a method of reacting the compound represented by the formula (X) with the phenol compound. The amount of the compound represented by the formula (X) and the phenol compound used in the reaction is not particularly limited. The amount of the compound represented by the formula (X) and the phenol compound used when reacting the compound represented by the formula (X) with the phenol compound (molar ratio; compound represented by (X):phenol compound) can be, for example, 1:0.5 to 2, preferably 1:0.8 to 1.2, and more preferably 1:1. The compound represented by the formula (X) and the phenol compound can be reacted in the presence of a catalyst. An example of the catalyst is boron trifluoride ether complex. The compound represented by the formula (X) and the phenol compound may be reacted in a solvent. Examples of the solvent include aromatic hydrocarbons such as benzene and toluene; aliphatic hydrocarbons such as cyclohexane; and halogenated hydrocarbons such as carbon tetrachloride.

[0175] The reaction temperature when reacting the compound represented by the above formula (X) with the above phenol compound can be, for example, 0 to 100°C.

[0176] From the viewpoint of achieving superior effects of the present invention, the content of the above-mentioned additive is preferably 0.05 to 10 mass %, and more preferably 0.1 to 1.0 mass %, based on the total amount of the composition (adhesive) that forms the curable resin (E) of the present invention.

[0177] From the viewpoint of obtaining superior effects of the present invention, the mass ratio of the content of the isocyanate derivative to the content of the adduct (mass ratio of isocyanate derivative:adduct) is preferably 0.1:1 to 50:1, and more preferably 10:1 to 2:1. In the case of a two-liquid type, it can be appropriately selected whether the above-mentioned additive is added to the base agent or to the curing agent.

[0178] The adhesive containing polyurethane resin or the adhesive forming a urethane bond may contain other components other than the above-mentioned components. In the case of a two-liquid type, whether the other components are added to the main agent or the curing agent can be appropriately selected. Examples of such other components include fillers (e.g., carbon black, calcium carbonate), catalysts (curing catalysts), plasticizers, antiaging agents, antioxidants, silane coupling agents, pigments (dyes), adhesion promoters, terpene compounds such as terpineol, thixotropy agents, ultraviolet absorbers, flame retardants, surfactants (including leveling agents), dispersants, dehydrating agents, antistatic agents, and various other additives. The fillers may be surface-treated with at least one treating agent selected from the group consisting of fatty acids, resin acids, urethane compounds, and fatty acid esters. In addition, in the case of a two-liquid type adhesive, whether the above-mentioned optional components are added to the main agent or the curing agent can be appropriately selected.

[0179] The resin cured layer (ii) may be a layer containing the curable resin (E) having the above-mentioned urethane bond, and the method for forming the layer is not limited. Preferably, the layer is formed by curing an adhesive containing a polyurethane resin or an adhesive that forms a urethane bond.

[0180] From the viewpoint of utilizing renewable resources and reducing CO2 emissions, the curable resin (E) having a urethane bond and the resin cured layer (ii) containing the same are preferably manufactured using at least a part of a biomass-derived raw material. That is, in the present invention, it is preferable to use one or more kinds of biomass-derived raw materials as raw materials used in forming the curable resin (E) having a urethane bond or the resin cured layer (ii) containing the same, such as an adhesive containing a polyurethane resin or a component constituting an adhesive forming a urethane bond. Here, biomass refers to "renewable, biologically derived organic resources excluding fossil resources", and biomass-derived raw materials refer to raw materials containing components derived from organic matter produced by organisms through photosynthesis from water and carbon dioxide using solar energy. Whether a raw material is biomass-derived can also be determined by the proportion of biomass-derived carbon determined by the 14C method specified in ASTM D6866.

[0181] As the biomass-derived raw material, for example, a raw material having a biomass content of 50% or more as measured by ASTM D6866 Method B, a raw material having a plant content (proportion of plant-derived components) of 50% or more, a commercially available raw material that is clearly stated to be derived from natural raw materials other than fossil resources, etc. can be used without particular limitation.

[0182] [Laminated structure] The laminate structure of the present invention is obtained by directly laminating a cured resin layer (ii) containing a curable resin (E) having a urethane bond onto a molded article (i) made of the above-mentioned polypropylene resin composition.

[0183] The polypropylene resin composition according to the present invention has excellent adhesion to the resin-cured layer (ii) containing the curable resin (E) having a urethane bond, and although the molded body (i) and the resin-cured layer (ii) are laminated directly without a primer, they are firmly bonded to each other, and the laminate structure maintains a high level of adhesion even at high temperatures at which the adhesion usually decreases.

[0184] In the present invention, the manufacturing method and shape of the molded body (i), the resin cured layer (ii), and the laminated structure of the present invention in which these are laminated are not limited. The laminated structure of the present invention may be a laminated structure consisting of only the molded body (i) and the resin cured layer (ii), or may be a laminated structure in which layers other than the molded body (i) and the resin cured layer (ii) are further laminated, for example, a laminated structure in which the molded body (i), the resin cured layer (ii), and other members are laminated in this order. The laminated structure in which the molded body (i), the resin cured layer (ii), and another member are laminated can be produced, for example, by a method of applying a curable composition that forms the resin cured layer (ii) on the molded body (i), laminating the other member before the composition cures, and curing the composition to form the resin cured layer (ii) between the molded body (i) and the other member, or a method of applying a curable composition that forms the resin cured layer (ii) on the other member, laminating the molded body (i) before the composition cures, and curing the composition to form the resin cured layer (ii) between the molded body (i) and the other member.

[0185] When the resin cured layer (ii) is a cured adhesive containing a polyurethane resin or an adhesive that forms a urethane bond, the resin cured layer (ii) may be produced by applying the adhesive onto the molded body (i) and curing it, or may be produced by applying the adhesive onto the molded body (i) and curing it in a state where it is laminated with another member, or may be produced by applying the adhesive onto another member to be laminated with the molded body (i) and curing it in a state where it is laminated with the molded body (i). In addition, in the production of a laminated structure in which the molded body (i), the resin cured layer (ii), and another member are laminated, a release film or the like on which an adhesive has been applied is attached to the molded body (i), the release film is peeled off to form an adhesive layer on the molded body (i), the other member is laminated, and the adhesive layer is cured to produce the resin cured layer (ii), or a release film or the like on which an adhesive has been applied is attached to the other member, the release film is peeled off to form an adhesive layer on the other member, the molded body (i) is laminated, and the adhesive layer is cured to produce the resin cured layer (ii). In producing such a cured resin layer (ii), it is preferable that the adhesive is in contact with the molded body (i) during curing, and it is more preferable that the adhesive is applied onto the molded body (i) and cured.

[0186] Also preferably, the method for producing the laminate structure of the present invention includes the steps of: molding the polypropylene resin composition described above by injection molding or press molding to produce a molded body (i); and a step of contacting or applying a curable resin (E) having a urethane bond or a raw material thereof to the molded body (i) and then curing the resin to form a cured resin layer (ii).

[0187] More preferably, the method includes the steps of: molding the polypropylene resin composition by injection molding or press molding to produce a molded article (i); and a step of applying a urethane-based adhesive containing a urethane prepolymer having a polyether skeleton and an aliphatic isocyanate derivative to the molded body (i) and then curing the adhesive to form a cured resin layer (ii).

[0188] Specifically, for example, the above-mentioned polypropylene resin composition is molded by injection molding or press molding to obtain a molded body (i), and then, if necessary, a surface treatment such as a frame treatment or a plasma treatment is applied to the surface of the molded body (i), and then the molded body is cured by directly applying a curable resin (E) having a urethane bond or an adhesive or the like which is a raw material of the molded body (i) to form a resin cured layer (ii). The curing conditions can be selected according to the type of the curable resin (E) or its raw material used, the presence or absence and the type of the curing agent, and the like. For example, the molded body can be cured at a temperature of 20°C or higher and lower than 100°C, preferably 40°C or higher and lower than 80°C.

[0189] The laminated structure of the present invention may have a layer of other member other than the molded body (i) and the resin cured layer (ii). A preferred embodiment of the laminated structure of the present invention is a laminated structure in which the molded body (i), the resin cured layer (ii), and the layer of the other member are laminated in this order. In such a laminated structure, it is preferable that the molded body (i) and the layer of the other member are bonded via the resin cured layer (ii).

[0190] The other member constituting the layer of the other member is not particularly limited and may be any member, for example, resin members such as ABS resin, PVC sheet, polyolefin sheet, and polyolefin sheet with a foam layer, glass, cloth, fabric, metal (iron (mild steel), cationic electrodeposited steel plate, aluminum, etc.), wood, paper, etc., and composite materials thereof. In manufacturing a laminated structure having a layer of these other members, for example, a method can be adopted in which the curable resin (E) having a urethane bond constituting the resin cured layer (ii) or an adhesive as a raw material thereof is directly applied to the surface of the molded body (i), the other member is brought into contact with the applied surface, and then the other member is laminated, followed by room temperature curing, heating, pressing, etc. to bond them.

[0191] Such a laminated structure of the present invention has excellent dimensional stability, and the molded body (i) and the resin-cured layer (ii) are firmly bonded without the aid of a primer even at high temperatures where adhesion is likely to decrease. For example, the laminated structure maintains high adhesion strength even at high temperatures of about 90°C, which is considered to be the most difficult to achieve strength in conventional adhesion tests, and shows sufficient adhesion strength in a hot shear test at 90°C. Specifically, in a hot shear strength test (tensile speed 50 mm / min) at 90°C according to JIS K6850:1999, the laminated structure shows excellent adhesion strength in which the interlaminar shear strength between the molded body (i) and the resin-cured layer (ii) is usually 1.2 MPa or more, preferably more than 1.5 MPa, more preferably more than 2.0 MPa, and even more preferably 2.5 MPa or more.

[0192] The laminated structure of the present invention can be suitably used as automobile interior materials such as door trims, instrument panels, ceilings, console boxes, pillars, glove boxes, etc.; automobile exterior parts such as bumpers, side guards, air spoilers, side protectors, fenders, door panels, tailgates, etc.; industrial parts such as home appliance parts and building materials, and can be particularly suitably used as automobile exterior parts such as tailgates. EXAMPLES

[0193] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0194] The physical properties were measured and evaluated by the following methods. [Melt flow rate (MFR) (g / 10 min)] The measurements were performed in accordance with ISO 1133, with a test load of 2.16 kg and a test temperature of 230°C. [Decane solubles (D sol ) and insoluble matter (D insol )] Add approximately 3 g (10 -4The mass was measured to the nearest g. This mass was expressed as x2(g) in the formula below. 500 ml of n-decane, 500 ml of n-decane, and a small amount of a heat stabilizer soluble in n-decane were added, and the temperature was raised to 150°C over 2 hours while stirring with a stirrer under a nitrogen atmosphere to dissolve the sample. The sample was then held at 150°C for 2 hours and then slowly cooled to 23°C over 8 hours. The resulting liquid containing the precipitate was filtered under reduced pressure using a 25G-4 standard glass filter manufactured by Iwata Glass Co., Ltd. 100 ml of the filtrate was collected and dried under reduced pressure to obtain a portion of the decane-soluble components, and the mass of this was calculated by multiplying the mass by 100 ml. -4 The mass was measured to the nearest g (this mass was expressed as x1 (g) in the formula below). Using this measurement, the amount of decane solubles (D sol ) and insoluble matter (D insol ) was determined by the following formula: D sol (mass%)=100×(500×x1) / (100×x2) D insol (mass%)=100-D sol

[0195] [Melting point peak] An endothermic curve is obtained by differential scanning calorimetry (DSC), and the temperature at the maximum peak position is determined as the melting point peak (Tm). The measuring machine used was Pyris 1 manufactured by PerkinElmer Co. The sample was packed in an aluminum pan, held at 30°C for 1 minute, then heated to 160°C at 500°C / min, held at 160°C for 5 minutes, cooled to -30°C at 10°C / min, and then heated from -30°C to 160°C at 10°C / min to obtain an endothermic curve from which the melting point peak (Tm) was determined. [Average particle size of inorganic filler] In accordance with JIS R1620 and JIS R1622, the particle size value at a cumulative amount of 50% by mass read from a particle size cumulative curve measured by a laser diffraction method was taken as the average particle size. [Aspect ratio of inorganic filler] Photographs were taken using an electron microscope, the powder's long diameter (particle size) and thickness were measured, the average values ​​were calculated, and the aspect ratio was calculated from the ratio of average particle size / average thickness. [Flexural modulus (MPa)] Measured according to ASTM D790 under the following conditions. Temperature: 23℃ Test piece: 127mm (length) x 12.7mm (width) x 6.35mm (thickness) Bending speed: 30mm / min Span: 100cm

[0196] [IZOD impact strength (J / m)] The IZOD impact strength was measured according to ASTM D256 under the following conditions: Test piece: 63.5mm (length) x 12.7mm (width) x 3.2mm (thickness) with notch Test temperature: -30℃ [Linear expansion coefficient (10 -5 / ℃)] The evaluation was performed according to ASTM D 696 using the TMA method (measurement range: -30 to 80°C). [Primerless interlayer adhesion test (90℃ hot shear test)] In accordance with JIS K6850:1999, a tensile testing machine was used to fix the resin plate side of an adhesive shear test specimen, which had a resin plate and a glass plate as adherends, as shown in the schematic diagram of Figure 1, and the glass side was attached to a fixing jig. The shear strength was measured at 90°C and a tensile speed of 50 mm / min, and the average of four measured values ​​was calculated as the hot shear test strength (MPa).

[0197] [Production Example 1] Preparation of propylene-ethylene block copolymer (A-1) (1) Preparation of solid titanium catalyst component 95.2 g of anhydrous magnesium chloride, 442 mL of decane, and 390.6 g of 2-ethylhexyl alcohol were reacted by heating at 130°C for 2 hours to obtain a homogeneous solution, to which 21.3 g of phthalic anhydride was added, and the mixture was stirred and mixed at 130°C for 1 hour to dissolve the phthalic anhydride.

[0198] After cooling this homogeneous solution to room temperature, 75 mL of the homogeneous solution was added dropwise over one hour to 200 mL of titanium tetrachloride kept at -20° C. After the addition was completed, the temperature of this mixture was raised to 110° C. over four hours, and when it reached 110° C., 5.22 g of diisobutyl phthalate (DIBP) was added and the mixture was kept at the same temperature with stirring for two hours.

[0199] After the reaction had finished for 2 hours, the solid portion was collected by hot filtration, resuspended in 275 mL of titanium tetrachloride, and then heated again for 2 hours at 110° C. After the reaction had finished, the solid portion was collected again by hot filtration, and thoroughly washed with decane and hexane at 110° C. until no free titanium compounds were detected in the solution.

[0200] The detection of the free titanium compounds was confirmed by the following method. 10 mL of the supernatant of the above solid catalyst component was collected with a syringe and placed in a 100 mL sidearm Schlenk tube that had been previously substituted with nitrogen. Next, the solvent hexane was dried with a nitrogen stream, and then vacuum dried for 30 minutes. 40 mL of ion-exchanged water and 10 mL of (1+1) sulfuric acid were added and stirred for 30 minutes. This aqueous solution was transferred to a 100 mL measuring flask through a filter paper, followed by the addition of 1 mL of concentrated H3PO4 solution as a masking agent for iron (II) ions and 5 mL of 3% hydrogen peroxide solution as a titanium coloring reagent, and the measuring flask was then filled up to 100 mL with ion-exchanged water, shaken, and 20 minutes later, the absorbance at 420 nm was observed using UV, and the free titanium was washed and removed until this absorption was no longer observed.

[0201] The solid titanium catalyst component prepared as above was stored as a decane slurry, and a portion of this was dried in order to examine the catalyst composition. The composition of the solid titanium catalyst component thus obtained was 2.3 mass% titanium, 61 mass% chlorine, 19 mass% magnesium, and 12.5 mass% DIBP. (2) Preparation of prepolymerization catalyst 100g of the solid titanium catalyst component, 131mL of triethylaluminum, 37.3ml of diethylaminotriethoxysilane, and 14.3L of heptane were charged into a 20L autoclave equipped with a stirrer, and 1000g of propylene was charged while maintaining the internal temperature at 15-20°C, and the reaction was carried out for 120 minutes while stirring. After the polymerization was completed, the solid components were allowed to settle, and the supernatant was removed and washed with heptane twice. The obtained prepolymerization catalyst was resuspended in purified heptane, and the concentration was adjusted with heptane so that the solid catalyst component concentration was 1.0g / L, to obtain a prepolymerization catalyst slurry. (3) Main Polymerization To a jacketed circulation type tubular polymerization reactor having an internal volume of 58 L, propylene was continuously fed at 43 kg / h, hydrogen at 256 NL / h, the prepolymerization catalyst slurry produced in (2) above at 0.49 g / h as a solid titanium catalyst component, triethylaluminum at 4.5 mL / h, and diethylaminotriethoxysilane at 1.8 mL / h, and polymerization was carried out in a liquid-filled state in which no gas phase was present. The temperature of the tubular polymerization reactor was 70°C, and the pressure was 3.57 MPa / G. The obtained slurry was transferred to a 100 L vessel polymerization reactor equipped with a stirrer, and further polymerization was carried out. Propylene was supplied to the polymerization reactor at 45 kg / hour, and hydrogen was supplied to the polymerization reactor so that the hydrogen concentration in the gas phase was 8.8 mol%, and polymerization was carried out at a polymerization temperature of 68°C and a pressure of 3.36 MPa / G.

[0202] The obtained slurry was then transferred to a 2.4 L liquid transfer tube, and the slurry was gasified and subjected to gas-solid separation. The polypropylene homopolymer powder was then sent to a 480 L gas-phase polymerization reactor, where ethylene / propylene block copolymerization was carried out. Propylene, ethylene, and hydrogen were continuously supplied so that the gas composition in the gas-phase polymerization reactor was ethylene / (ethylene+propylene)=0.20 (molar ratio) and hydrogen / ethylene=0.0031 (molar ratio), and polymerization was carried out at a polymerization temperature of 70°C and a pressure of 1.40 MPa / G.

[0203] The resulting propylene-based block copolymer was then vacuum-dried at 80° C. The MFR (230° C., 2.16 kg load) of the thus obtained propylene-ethylene block copolymer (A-1) was 80 g / 10 min, the amount of the decane-soluble portion (propylene-ethylene copolymer component) was 7 mass%, the amount of the decane-insoluble portion (propylene homopolymer component) was 93 mass%, and the intrinsic viscosity [η] of the decane-soluble portion was 7.5 dl / g.

[0204] [Production Example 2] Preparation of propylene homopolymer (B-1) A solid titanium catalyst component was obtained in the same manner as in Production Example 1(1) Preparation of a solid titanium catalyst component. (2) Preparation of prepolymerization catalyst 100 g of the solid titanium catalyst component, 39.3 mL of triethylaluminum, and 100 L of heptane were charged into a 200 L autoclave equipped with a stirrer, and 600 g of propylene was added while maintaining the internal temperature at 15 to 20°C. The mixture was reacted for 60 minutes with stirring to obtain a prepolymerization catalyst slurry. (3) Main Polymerization To a 58 L jacketed circulation tubular polymerization reactor, 43 kg / hr of propylene, 177 NL / hr of hydrogen, 0.58 g / hr of the prepolymerization catalyst slurry produced in (2) as a solid titanium catalyst component, 3.1 ml / hr of triethylaluminum, and 3.3 ml / hr of dicyclopentyldimethoxysilane were continuously fed, and polymerization was carried out in a liquid-filled state with no gas phase present. The temperature of the tubular polymerization reactor was 70° C., and the pressure was 3.53 MPa / G. The obtained slurry was transferred to a 100 L vessel polymerization reactor equipped with a stirrer, and further polymerization was carried out. Propylene was supplied to the polymerization reactor at 45 kg / hour, and hydrogen was supplied to the polymerization reactor so that the hydrogen concentration in the gas phase was 3.2 mol%, and polymerization was carried out at a polymerization temperature of 70°C and a pressure of 3.28 MPa / G. The resulting propylene homopolymer was then vacuum dried at 80° C. The MFR (230° C., 2.16 kg load) of the propylene homopolymer (B-1) thus obtained was 30 g / 10 min.

[0205] [Production Example 3] Preparation of propylene homopolymer (B-2) First, a prepolymerized catalyst slurry was obtained in the same manner as in Production Example 1 (1) Preparation of a solid titanium catalyst component and (2) Production of a prepolymerized catalyst. (3) Main Polymerization To a 1000 L vessel polymerization reactor equipped with a stirrer, 131 kg / hour of propylene, 0.70 g / hour of the prepolymerization catalyst slurry as a transition metal catalyst component, 19.6 mL / hour of triethylaluminum, and 4.2 mL / hour of diethylaminotriethoxysilane were continuously supplied, and hydrogen was supplied so that the hydrogen concentration in the gas phase became 5.3 mol%, and polymerization was performed at a polymerization temperature of 75°C and a pressure of 3.5 MPa / G.

[0206] The obtained slurry was transferred to a 500 L vessel polymerization reactor equipped with a stirrer, and further polymerization was carried out. Propylene was supplied to the polymerization reactor at 30 kg / hr, and hydrogen was supplied to the polymerization reactor so that the hydrogen concentration in the gas phase was 3.9 mol%, and polymerization was carried out at a polymerization temperature of 74.5°C and a pressure of 3.4 MPa / G.

[0207] The obtained slurry was then transferred to a 500 L vessel polymerization reactor equipped with a stirrer, and polymerization was further carried out. Propylene was supplied to the polymerization reactor at 20 kg / hr, and hydrogen was supplied to the polymerization reactor so that the hydrogen concentration in the gas phase was 3.4 mol%, and polymerization was carried out at a polymerization temperature of 73°C and a pressure of 3.4 MPa / G. The resulting slurry was then deactivated, vaporized, and then gas-solid separated. The resulting propylene homopolymer was vacuum dried at 80° C. The MFR (230° C., 2.16 kg load) of the thus obtained propylene homopolymer (B-2) was 210 g / 10 min.

[0208] [Ethylene-α-olefin copolymer] The ethylene-α-olefin copolymer (C-1) was TAFMER (registered trademark) A4050S (ethylene content = 80 mol%, 1-butene content = 20 mol%, MFR (230°C, 2.16 kg load) = 7 g / 10 min, density = 0.862 g / cm) manufactured by Mitsui Chemicals. 3 , melting point peak = less than 50°C) was used.

[0209] The ethylene-α-olefin copolymer (C-2) was TAFMER (registered trademark) A1050S (ethylene content = 80 mol%, 1-butene content = 20 mol%, MFR (230°C, 2.16 kg load) = 2 g / 10 min, density = 0.862 g / cm) manufactured by Mitsui Chemicals. 3 , melting point peak = less than 50°C) was used.

[0210] As the ethylene-α-olefin copolymer (C-3), ENGAGE® 11547, a polyolefin elastomer manufactured by Dow Chemical Company (MFR (230°C, 2.16 kg load) = 9 g / 10 min, density = 0.866 g / cm 3 , melting point peak = 120°C) was used. [Inorganic filler] As the inorganic filler (D-1), talc having the following properties was used. (D-1): Talc, average particle size (laser diffraction method) = 6.0 μm, aspect ratio (SEM measurement) = 7.0

[0211] [Production Examples 4 to 6] Preparation of Main Agents (E1-1) to (E1-3) The components in Table 1 below were mixed using a stirrer in the compositions (parts by mass) shown in the table to prepare main components (E1-1) to (E1-3) of two-component curing adhesives.

[0212] [Table 1] Details of each component in Table 1 above are as follows. (Details of main ingredient) Polymer 1: A urethane prepolymer synthesized from: 700 g of polyoxypropylene diol (average molecular weight 2000), 300 g of polyoxypropylene triol (average molecular weight 3000), and 499 g of 4,4'-diisocyanate phenylmethane (molecular weight 250) were mixed (NCO / OH=2.0 at this time), and 500 g of diisononyl phthalate was added. The mixture was stirred at 80°C for 12 hours in a nitrogen stream to react, synthesizing a urethane prepolymer (polymer 1) containing 2.10% isocyanate groups. Polymer 2: Modified silicone resin whose main chain is polyoxypropylene and has a methyldimethoxysilyl group as a hydrolyzable silyl group at the end. Kaneka MS Polymer S203 (Kaneka Corporation) Epoxy resin 1: Adeka Resin EP-4100 (manufactured by Adeka Corporation) Epoxy resin 2: Adeka Resin EP-4006 (manufactured by Adeka Corporation) Compound 1: Isocyanurate of hexamethylene diisocyanate (Takenate D-170HN, manufactured by Mitsui Chemicals, Inc.) Compound 2: A mixture of isocyanurate and allophanate forms of pentamethylene diisocyanate (STABIO D-376N (low viscosity type), manufactured by Mitsui Chemicals) (Biomass-derived compounds: Plant content (ASTM D6866-04): 67%) Compound 3: Ketimine-type latent hardener Epicure H-30 (manufactured by Mitsubishi Chemical Corporation) Compound 4: an adduct of camphene and phenol (manufactured by Yasuhara Chemical Co., Ltd.). The adduct used as compound 4 is a commercially available product, and contains at least one compound selected from the group consisting of a compound represented by the following formula (Z1-1), a compound represented by the formula (Z1-2), a compound represented by the formula (Z2-1), a compound represented by the formula (Z2-2), and a compound represented by the formula (Z3-1). (Biomass-derived compound: biomass degree (ASTM D6866 Method B): 55%)

[0213] [ka]

[0214] [ka] Carbon black: #200MP (manufactured by Shinnikka Carbon Co., Ltd.) Calcium carbonate 1: Super S (manufactured by Maruo Calcium Co., Ltd.) Calcium carbonate 2: Calfine 200 (manufactured by Maruo Calcium Co., Ltd.) Plasticizer 1: Diisononyl phthalate (JPlus) Plasticizer 2: ShellsolTM (Japan Chemtech Co., Ltd.) Catalyst 1: Dimorpholinodiethyl ether (San-Apro) Catalyst 2: Tin-based catalyst Neostan U-303 (manufactured by Nitto Kasei Co., Ltd.)

[0215] [Production Examples 7 and 8] Preparation of Curing Agents (E2-1) and (E2-2) The components in Table 2 below were mixed using a stirrer in the compositions (parts by mass) shown in the table to prepare hardeners (E2-1) and (E2-2) for the two-component hardening adhesive.

[0216] [Table 2] Details of each component in Table 2 above are as follows. (Details of hardener components) Compound 5: Trifunctional polypropylene polyol (Exenol 1030, Asahi Glass Co., Ltd.) Compound 6: Polybutadiene diol (Poly bd R-45HT, Idemitsu Kosan Co., Ltd., hydroxyl value: 0.8 mol / kg) Compound 7: Terpineol (manufactured by Yasuhara Chemical Co., Ltd.) (Biomass-derived compound: Biomass ratio (ASTM D6866 Method B): 95% or more) Compound 8: 3-glycidoxypropyltrimethoxysilane SilaAce S-510 (Chisso Corporation) Compound 9: X-12-972F (aminosilane oligomer) (manufactured by Shin-Etsu Chemical Co., Ltd.) Calcium carbonate 2: Calfine 200 (manufactured by Maruo Calcium Co., Ltd.) Catalyst 1: Dimorpholinodiethyl ether (San-Apro) Catalyst 3: Amine catalyst TEDA-L33E (manufactured by Tosoh Corporation)

[0217] [Examples 1 to 3, Comparative Examples 1 to 3] - Preparation of molded test specimens and surface treatment The propylene polymer (A), propylene homopolymer (B), ethylene-α-olefin copolymer (C) and inorganic filler (D) were mixed in the types and amounts shown in Table 3 and extruded using a twin-screw extruder (TEX (registered trademark) 30α, manufactured by The Japan Steel Works, Ltd.) at a cylinder temperature of 180°C, a screw rotation of 750 rpm and an extrusion rate of 60 kg / h to obtain polypropylene resin compositions. The melt flow rates (230°C, 2.16 kg load) of the obtained polypropylene resin compositions are shown in Table 3.

[0218] Each of the obtained polypropylene resin compositions was injection molded using a mold cavity having a length of 350 mm, a width of 100 mm, and a thickness of 3 mm at a resin temperature of 210°C and a mold temperature of 40°C to obtain a flat plate, which was then cut into a shape of 100 mm x 50 mm x 3 mm to obtain a molded test piece (flat plate) for producing a laminate structure.

[0219] In addition, molded specimens for measurement having the above-mentioned shapes were obtained by injection molding and cutting at the same resin temperature and mold temperature. The flexural modulus, IZOD impact strength, and linear expansion coefficient were measured using each of the obtained molded specimens by the above-mentioned test methods. The results are shown in Table 3.

[0220] The flat plate obtained above was cut into a shape of 100 mm x 25 mm x 3 mm to obtain a test piece. The surface of the obtained test piece was subjected to a surface treatment (flame treatment). For the surface treatment, a flame treatment device (FTS 201 manufactured by Arcogas) was used. The flame treatment device can adjust the flow rate of the combustion gas and air.

[0221] For the surface treatment, the air flow rate was fixed at 100 L / min, the combustion gas (propane gas) flow rate was adjusted to 3.7 L / min, the distance between the plate and the flame irradiation head was set to 40 mm, and the treatment speed was set to 800 mm / sec to produce a surface with a surface free energy of 42 dynes / cm (mN / m) (surface treatment state: low treatment). Similarly, a surface with a surface free energy of 52 dynes / cm (mN / m) was produced with a distance of 30 mm and 800 mm / sec (surface treatment state: medium treatment), and a surface with a surface free energy of 64 dynes / cm (mN / m) was produced with a distance of 10 mm and 800 mm / sec (surface treatment state: high treatment).

[0222] Preparation of adhesive The types of base agent and curing agent shown in Table 3 were used, and 100 g of the base agent and 10 g of the curing agent were mixed together immediately before application of the adhesive to obtain an adhesive. The adhesives (E-1) and (E-3) are urethane adhesives, and the adhesive layer obtained by using them is cured to form a resin cured layer containing a curable resin having a urethane bond. The adhesive (E-2) is a non-urethane adhesive, and the adhesive layer obtained by using it is cured to form a resin cured layer containing a curable resin having a non-urethane bond. - Fabrication and evaluation of laminated structures An adhesive layer made of the adhesive obtained above was formed on each of the surface-treated test pieces obtained above so as to have an adhesive area of ​​25 mm (width) x 10 mm (length) and a thickness of 5 mm. Glass (7.5 x 25 x 5 mm thick) was selected and used as the opposing member through the adhesive layer, and cured at room temperature to obtain a laminated structure test piece in which a molded body made of a polypropylene resin composition, a cured resin layer obtained from the adhesive, and glass were laminated.

[0223] After aging for 3 days at room temperature, the back side of the resin substrate side of each laminated structure test piece obtained was subjected to the same surface treatment as described above, and a cationic electroplated steel plate with a thickness of 1 mm was attached using an adhesive (WS-242 manufactured by Sika Hamatite Co., Ltd.), and after further aging for 3 days at room temperature, a hot shear strength test was performed at 90°C (tensile speed: 50 mm / min) using a tensile tester in accordance with JIS K6850:1999, with the glass fixed as shown in the schematic diagram of Figure 1. The results are shown in Table 3.

[0224] [Table 3] As is clear from the results shown in Table 3, the laminate structures of Examples 1 to 3, which have a molded layer made of a polypropylene resin composition containing an ethylene-α-olefin copolymer having a high melting point peak of 110°C or higher, and a cured resin layer made of a curable resin (cured product of the adhesive) having a urethane bond, have excellent mechanical properties, and despite being laminate structures formed without the use of a primer (primerless), the layers are firmly bonded together, and the laminate structures have high adhesive strength even under high temperature conditions of 90°C. Industrial Applicability

[0225] The laminate structure of the present invention can be suitably used for automobile interior materials such as door trims, instrument panels, ceilings, console boxes, pillars, glove boxes, etc.; automobile exterior members such as bumpers, side guards, air spoilers, side protectors, fenders, door panels, back doors, etc.; home appliance parts, industrial parts such as building materials, etc.

Claims

1. A laminated structure in which a resin cured layer (ii) containing a curable resin (E) having a urethane bond is directly laminated on a molded article (i) made of a polypropylene-based resin composition, The polypropylene resin composition comprises: 5 to 47 parts by mass of a propylene polymer (A) having a melt flow rate (230° C., 2.16 kg load) of 50 to 150 g / 10 min and a decane soluble content of 6 to 15 mass %, 20 to 30 parts by mass of a propylene homopolymer (B) having a melt flow rate (230° C., 2.16 kg load) of 10 to 500 g / 10 min, A random copolymer of ethylene and an α-olefin having 4 to 8 carbon atoms, with a density of 0.850 to 0.880 g / cm 3 23 to 30 parts by mass of an ethylene / α-olefin copolymer (C) having a melt flow rate (230° C., 2.16 kg load) of 0.5 to 30 g / 10 min and a melting point peak of 110° C. or higher, Inorganic filler (D) 30 to 40 parts by mass [The total amount of components (A) to (D) is 100 parts by mass.] Contains The resin cured layer (ii) The adhesive (I) is a cured adhesive that contains a polyurethane resin or forms a urethane bond, The adhesive (I) comprises an adduct of camphene and phenol, The adduct contains at least one compound selected from the group consisting of a compound represented by the following formula (Z1-1), a compound represented by the formula (Z1-2), a compound represented by the formula (Z2-1), a compound represented by the formula (Z2-2), and a compound represented by the formula (Z3-1): 【Chemistry 1】

2. An automobile exterior member comprising the laminate structure according to claim 1.

3. 5 to 47 parts by mass of a propylene polymer (A) having a melt flow rate (230° C., 2.16 kg load) of 50 to 150 g / 10 min and a decane soluble content of 6 to 15 mass %, 20 to 30 parts by mass of a propylene homopolymer (B) having a melt flow rate (230° C., 2.16 kg load) of 10 to 500 g / 10 min, A random copolymer of ethylene and an α-olefin having 4 to 8 carbon atoms, with a density of 0.850 to 0.880 g / cm 3 23 to 30 parts by mass of an ethylene / α-olefin copolymer (C) having a melt flow rate (230° C., 2.16 kg load) of 0.5 to 30 g / 10 min and a melting point peak of 110° C. or higher, Inorganic filler (D) 30 to 40 parts by mass [The total amount of components (A) to (D) is 100 parts by mass.] A step of molding a polypropylene-based resin composition containing the above compound by injection molding or press molding to produce a molded product (i); a step of contacting or applying an adhesive (I) containing a polyurethane resin or an adhesive that forms a urethane bond to the molded body (i) and then curing the adhesive to form a resin cured layer (ii); Including, The adhesive (I) comprises an adduct of camphene and phenol, The method for producing a laminate structure, wherein the adduct contains at least one compound selected from the group consisting of a compound represented by the following formula (Z1-1), a compound represented by the formula (Z1-2), a compound represented by the formula (Z2-1), a compound represented by the formula (Z2-2), and a compound represented by the formula (Z3-1): 【Chemistry 2】

Citation Information

Patent Citations

  • Thermoplastic resin composition and its injection-molded article

    JP1993051498A

  • Resin composition for molding automobile side molding and automobile side molding

    JP2000095919A

  • Polypropylene-based resin composition excellent in coating appearance and molded article

    JP2007091789A

  • Propylene-based resin composition and molded article thereof

    JP2010077396A

  • Polypropylene-based resin composition for exterior member of automobile and exterior member of automobile

    JP2013159709A