Alkaline earth aluminate phosphor, light emitting device, and method for manufacturing alkaline earth aluminate phosphor
The formulation and heat treatment of alkaline earth aluminate phosphors with controlled molar ratios enhance luminescence intensity, allowing emission in the near-infrared range for medical and plant growth applications.
Patent Information
- Application Number
- JP2020145823
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-31
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2040-08-31
AI Technical Summary
Existing light emitting devices using alkaline earth aluminate phosphors lack sufficient luminescence intensity and are limited in their ability to emit light in the near-infrared wavelength range necessary for applications like medical imaging and plant growth promotion.
A specific composition of alkaline earth aluminate phosphors is formulated with controlled molar ratios of elements such as alkaline earth metals, Al, Cr, and optional Group 13 elements, along with co-activating elements, and heat-treated in a reducing atmosphere to enhance luminescence intensity and emission in the 720-900 nm range.
The resulting phosphors exhibit improved luminescence intensity and emission in the near-infrared range, enabling effective medical imaging and plant growth applications by absorbing excitation light and emitting light that easily penetrates living tissues and affects plant photoreceptors.
Smart Images

Figure 0007575658000002 
Figure 0007575658000003 
Figure 0007575658000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to alkaline earth aluminate phosphors, light emitting devices, and methods for making alkaline earth aluminate phosphors. [Background technology]
[0002] Various light emitting devices have been developed that combine an excitation light source such as a light emitting diode (LED) or a laser diode (LD) with a phosphor and emit light such as white or warm white light based on the principle of light mixing. These light emitting devices are used in a wide range of fields such as lighting, in-vehicle use, medical use, and backlighting for liquid crystal display devices.
[0003] In such light emitting devices, various kinds of phosphors are used depending on the purpose. For example, Non-Patent Document 1 (Ruixia Zhong et al. "Red phosphrescence in Sr4Al 14 O 25 :Cr 3+ ,EU 3+ ,Dy 3+ "through persistent energy transfer" APPLIED PHYSICS LETTERS 88.201916 (2006) describes Sr4Al 14 O 25 :Cr 3+ ,EU 3+ ,Dy 3+ Alkaline earth aluminate phosphors represented by the formula: [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Ruixia Zhong et al. “Red phosphrescence in Sr4Al14O25:Cr3+,Eu3+,Dy3+ through persistent energy transfer” APPLIED PHYSICS LETTERS 88.201916(2006) Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present disclosure is to provide an alkaline earth aluminate phosphor having improved luminous intensity, a light emitting device, and a method for producing the alkaline earth aluminate phosphor. [Means for solving the problem]
[0006] The first aspect is a composition comprising at least one element A selected from the group consisting of alkaline earth metal elements, Al, Cr, and, as necessary, at least one element M selected from the group consisting of Group 13 elements excluding Al. 1 and optionally at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm. 2 The molar ratio of the element A is in the range of 1.0 to 4.0, and the Al and the element M 1 the molar ratio of the total of the elements M is in the range of 4.0 to 14.0, the molar ratio of the Cr is in the range of 0.004 to 0.8, 2 The molar ratio of the Cr and the element M is within a range of 0 to 0.4. 2 The total molar ratio of Al and the element M is within a range of 0.004 to 0.8. 1 The molar ratio of the element M when the sum of the elements is 1 1 The molar ratio of is 0.7 or less, and the phosphor has an emission peak wavelength within the range of 720 nm to 900 nm.
[0007] A second aspect is a light emitting device comprising the alkaline earth aluminate phosphor and a light source that irradiates the alkaline earth aluminate phosphor.
[0008] The third aspect is a compound including a first compound containing at least one element A selected from the group consisting of alkaline earth metal elements, a second compound containing Al, and a third compound containing Cr, and optionally containing at least one element M selected from the group consisting of Group 13 elements excluding Al. 1 and optionally at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm. 2 At least one compound selected from the group consisting of the first compound, the second compound, and the third compound is an oxide, the molar ratio of the element A in 1 mole of the composition is within a range of 1.0 to 4.0, and the Al and the element M 1 the molar ratio of the total of the elements M is in the range of 4.0 to 14.0, the molar ratio of the Cr is in the range of 0.004 to 0.8, 2 The molar ratio of Al to the element M is within a range of 0 to 0.4. 1 The molar ratio of the element M when the sum of the elements is 1 1 the molar ratio of the first compound, the second compound, and the third compound to be 0.7 or less, and optionally including a fourth compound and a fifth compound; and a heat-treating the raw material mixture at a temperature in the range of 1000° C. or more and 1500° C. or less in a reducing atmosphere to obtain an alkaline earth aluminate phosphor. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide an alkaline earth aluminate phosphor having improved luminous intensity, a light emitting device using the same, and a method for producing the alkaline earth aluminate phosphor. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram showing the emission spectrum of the alkaline earth aluminate phosphor of Example 1 and the emission spectrum of a compound having the alkaline earth aluminate composition of Comparative Example 1. [Diagram 2] FIG. 2 is a diagram showing the excitation spectrum of the alkaline earth aluminate phosphor according to Example 1. As shown in FIG. [Diagram 3] FIG. 3 is a diagram showing the emission spectra of the alkaline earth aluminate phosphors according to Examples 4, 5 and 6, and the emission spectrum of a compound having the alkaline earth aluminate composition according to Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The alkaline earth aluminate phosphor, light emitting device, and method for producing the alkaline earth aluminate phosphor according to the present invention will be described below. However, the following embodiments are merely examples for embodying the technical idea of the present invention, and the present invention is not limited to the following alkaline earth aluminate phosphor, light emitting device, and method for producing the alkaline earth aluminate phosphor. The relationship between the color name and the chromaticity coordinate, the relationship between the wavelength range of light and the color name of monochromatic light, and the like conform to JIS Z8110. In this specification, in the formula representing the composition of the phosphor, a plurality of elements separated by a comma (,) indicate that at least one of these elements is contained in the composition, and two or more elements may be contained in combination. In this specification, in the formula representing the composition of the phosphor, the elements before the colon (:) represent the elements constituting the host crystal and their molar ratio, and the elements after the colon (:) represent the activating element. In this specification, the "molar ratio" represents the ratio of each element in 1 mole of the chemical composition of the compound or phosphor, unless otherwise specified.
[0012] A light-emitting device using a phosphor is required to emit the most suitable light depending on the visual target. For example, in the medical field, it may be required to easily obtain information inside a living body. In a living body, light absorbers include water, hemoglobin, melanin, etc. For example, hemoglobin has a high absorption rate of light in the visible light region with a wavelength of less than 650 nm, and it is difficult for light in the visible light region to penetrate into a living body with a light-emitting device that emits light in the visible light region, making it difficult to obtain information inside the living body. Therefore, a light-emitting device that emits light in the near-infrared wavelength range of 650 nm to 1000 nm, which is called the "biological window" through which light easily penetrates inside a living body, may be required. For example, if it is possible to measure the increase or decrease in the oxygen concentration in blood inside a living body by the increase or decrease in the absorption of light by hemoglobin that binds with oxygen, it will be possible to easily obtain information inside the living body by irradiating light from a light-emitting device.
[0013] In addition, in the midst of environmental changes such as climate change, it is desirable to provide a stable supply of vegetables and other plants and to increase plant production efficiency. Plant factories, which allow artificial management, are capable of steadily supplying safe vegetables to the market and are expected to be the next-generation industry. In such plant factories, light-emitting devices that irradiate light that can promote plant growth are required. Plant responses to light are divided into photosynthesis and photomorphogenesis. Photosynthesis is a reaction that uses light energy to decompose water, generate oxygen, and fix carbon dioxide into organic matter, and is a reaction necessary for plant growth. Photomorphogenesis is a morphological reaction that uses light as a signal to perform seed germination, differentiation (germination formation, leaf formation, etc.), movement (stoma opening and closing, chloroplast movement), light refraction, etc. It has been found that light in the wavelength range of 690 nm to 800 nm affects the photoreceptors of plants in photomorphogenesis reactions. For this reason, light-emitting devices used in plant factories and the like may be required to be capable of emitting light in a wavelength range that affects plant photoreceptors (chlorophyll a, chlorophyll b, carotenoids, phytochromes, cryptochromes, phototropins) and promotes plant growth. Regarding the alkaline earth aluminate phosphors described above, when they are combined with an excitation light source such as a light emitting diode (LED) or a laser diode (LD) to form a light emitting device, there is still room for improvement in the light emitting properties as a phosphor so that the device can become a light source suitable for these applications.
[0014] Alkaline Earth Aluminate Phosphors The alkaline earth aluminate phosphor according to the first embodiment includes at least one element A selected from the group consisting of alkaline earth metal elements, Al, and Cr, and, as necessary, at least one element M selected from the group consisting of Group 13 elements excluding Al. 1 and optionally at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm. 2 The molar ratio of the element A is in the range of 1.0 to 4.0, and the Al and the element M 1 the molar ratio of the total of the elements M is in the range of 4.0 to 14.0, the molar ratio of the Cr is in the range of 0.004 to 0.8, 2 The molar ratio of the Cr and the element M is within a range of 0 to 0.4. 2 The total molar ratio of Al and the element M is within a range of 0.004 to 0.8. 1 The molar ratio of the element M when the sum of the elements is 1 1 The alkaline earth aluminate phosphor has a composition in which the molar ratio of is 0.70 or less, and has an emission peak wavelength in the range of 720 nm to 900 nm. The alkaline earth aluminate phosphor can absorb excitation light and emit light having an emission peak wavelength in the range of 720 nm to 900 nm, emit light having an emission peak wavelength in the near-infrared wavelength range called the "biological window," and emit light that affects the photoreceptors of plants. In this specification, the near-infrared wavelength range refers to the wavelength range of 700 nm to 2500 nm.
[0015] The alkaline earth aluminate phosphor consists of elements A, Al, Cr, and optionally element M. 1 and element M, which is included as necessary. 2It is preferable that the composition has the following formula (I): A x (Al 1-y M 1 y ) z O x+3 / 2z :Cr v ,M 2 w (I) (In formula (I), A is at least one element selected from the group consisting of alkaline earth metal elements, M 1 is at least one element selected from the group consisting of Group 13 elements excluding Al, and M 2 is at least one element selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er, and Tm, and v, w, x, y, and z satisfy 0.004≦v≦0.8, 0≦w≦0.4, 0.004≦v+w≦0.8, 1.0≦4.0, 0≦y≦0.7, and 4.0≦z≦14.0.
[0016] By firing the alkaline earth aluminate phosphor having the above-mentioned composition in a reducing atmosphere, the activator Cr has a valence of three and easily enters the host crystal of the alkaline earth aluminate phosphor, so that the phosphor absorbs excitation light and emits light having an emission peak wavelength in the range of 720 nm or more and 900 nm or less.
[0017] The element A is at least one element selected from the group consisting of alkaline earth metal elements, and may contain two or more elements. The element A may be at least one element selected from the group consisting of Ca, Sr, and Ba. The element A may contain two or more elements selected from the group consisting of alkaline earth metal elements. The element A may be Sr, or may be Sr and Ca. The element A is at least two elements A selected from the group consisting of alkaline earth metal elements. a and element A b If it contains element A a and element A b The molar ratio of element A a and element A b When the total molar ratio of element A is 10,a and element A b Molar ratio (A a / A b The molar ratio x of element A in the composition of the alkaline earth aluminate phosphor is in the range of 1.0 to 4.0, and the ratio of Al to element M in 1 mole of the alkaline earth aluminate composition is 1 When the total molar ratio of is 14, it is preferably 4.
[0018] When element A includes two or more elements selected from the group consisting of alkaline earth metal elements, the alkaline earth aluminate phosphor may have a composition represented by the following formula (I-1). (A a 1-u A b u ) x (Al 1-y M 1 y ) z O x+3 / 2z :Cr v ,M 2 w (I-1) (In formula (I-1), A a is an element selected from the group consisting of alkaline earth metal elements, b A a An element selected from the group consisting of alkaline earth metal elements excluding M 1 is at least one element selected from the group consisting of Group 13 elements excluding Al, and M 2 is at least one element selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er, and Tm, and u, v, w, x, y, and z are within the range of 0.1≦u≦0.9, 0.004≦v≦0.8, 0≦w≦0.4, 0.004≦v+w≦0.8, 1.0 ≦x ≦4.0, 0≦y≦0.7, 4.0≦z≦14.0.)
[0019] The Al contained in the composition of the alkaline earth aluminate phosphor, together with the element A and oxygen (O), constitutes a crystal skeleton that becomes the host crystal of the alkaline earth aluminate phosphor. In addition to Al, the composition of the alkaline earth aluminate phosphor contains at least one element M selected from the group consisting of elements of Group 13 except Al. 1 Even when it contains Al and element M 1 When the molar ratio z of the total of element M and element M is within the range of 4.0 to 14.0 (4.0≦z≦14.0), the crystal skeleton of the host crystal of the alkaline earth aluminate phosphor is formed. 1 In the case where it contains Al and element M 1 When the sum of the molar ratios of Al and M is 1, it is preferable that Al is contained in an amount of 0.3 moles or more. 1 When the total molar ratio of these is 1, if the content of Al is 0.3 moles or more, a stable crystal structure can be maintained.
[0020] The element M in the composition of alkaline earth aluminate phosphors 1 When the element M is contained, it is preferably at least one element selected from the group consisting of the Group 13 elements excluding Al. 1 is preferably at least one selected from the group consisting of B, Ga, In, and Tl, more preferably at least one selected from the group consisting of B, Ga, and In, and may be at least one selected from the group consisting of B and Ga, or may be Ga. The element M contained in the composition of the alkaline earth aluminate phosphor 1 is the Al and element M in the composition. 1 Element M when the sum of 1 The molar ratio y is preferably in the range of 0 or more and 0.7 or less (0≦y≦0.7), may be in the range of 0.1 or more and 0.7 or less (0.1≦y≦0.7), or may be in the range of 0.2 or more and 0.6 or less (0.2≦y≦0.6).
[0021] The element M in the composition of alkaline earth aluminate phosphors 1 Contains Al and element M in the composition 1 Element M when the sum of1 When the molar ratio y is within the range of 0.1 to 0.7 (0.1≦y≦0.7), the emission wavelength and shape can be changed without significantly decreasing the luminous efficiency.
[0022] The alkaline earth aluminate phosphor has a composition in which the element A is at least one element selected from the group consisting of Ca, Sr, and Ba, and the element M 1 The element A may be at least one element selected from the group consisting of Ba, Ga and In. The alkaline earth aluminate phosphor may have a composition in which the element A is Sr and the element M is 1 may be Ga.
[0023] The alkaline earth aluminate phosphor contains Cr, which is an activator element, and the molar ratio v of Cr in 1 mole of the composition of the alkaline earth aluminate phosphor is preferably in the range of 0.004 to 0.8 (0.004≦v≦0.8), may be in the range of 0.005 to 0.7 (0.005≦v≦0.7), may be in the range of 0.008 to 0.6 (0.008≦v≦0.6), or may be in the range of 0.010 to 0.5 (0.010≦v≦0.5). When the alkaline earth aluminate phosphor contains Cr, which is an activator element, and the molar ratio of Cr in 1 mole of the composition of the alkaline earth aluminate phosphor is in the range of 0.004 to 0.8, a phosphor that emits light having an emission peak wavelength in the range of 720 nm to 900 nm can be obtained.
[0024] The alkaline earth aluminate phosphor contains, in addition to Cr, at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er, and Tm as a coactivator element. 2 The alkaline earth aluminate phosphor may contain the element M 2 If it contains element M 2 Characteristic luminescence is obtained due to the inclusion of element M. 2When the alkaline earth metal aluminate phosphor contains Cr, the phosphor may have a peak emission wavelength in a different wavelength range from that of an alkaline earth metal aluminate phosphor containing only Cr. 2 and may contain element M 2 The molar ratio of Cr to element M is in the range of 0 to 0.4 (0≦w≦0.4) and may be in the range of 0.1 to 0.3 (0.1≦w≦0.3). 2 The total molar ratio of the above is within the range of 0.004 or more and 0.8 or less.
[0025] In the emission spectrum of the alkaline earth aluminate phosphor, the half-width of the emission peak wavelength in the range of 720 nm to 900 nm is preferably 80 nm or more, may be 90 nm or more, may be 150 nm or less, or may be 120 nm or less. When the alkaline earth aluminate phosphor emits light having an emission peak wavelength in the range of 720 nm to 900 nm, for example, information on the increase or decrease in the oxygen concentration in blood in a living body can be obtained by the increase or decrease in the absorption of light by hemoglobin that binds with oxygen. In a living body, light is absorbed and scattered, and in order to measure subtle changes in the propagation behavior of light in blood in a living body, it is preferable that the half-width of the emission peak in the range of 720 nm to 900 nm emitted from the light emitting device is wide. In addition, it is preferable that the color of an object when irradiated with light (hereinafter also referred to as "color rendering") has an emission spectrum in a wide range, and a wide half-width can emit light with excellent color rendering. For example, in a plant factory, even when emitting light in a wavelength range that affects plant growth, it may be required to emit light that does not disrupt the spectral balance of light so that workers can work easily. In the emission spectrum of an alkaline earth aluminate phosphor, if the half-width of an emission peak within the range of 720 nm to 900 nm is 80 nm or more and 150 nm or less, color rendering can be improved. The half-width refers to the full width at half maximum of the emission peak in the emission spectrum, and refers to the wavelength width of the emission peak that shows 50% of the maximum value of the emission peak in the emission spectrum.
[0026] Light-emitting device The light emitting device includes an alkaline earth aluminate phosphor and a light source for irradiating the alkaline earth aluminate phosphor. The aluminate phosphor according to one embodiment of the present invention can be used as a member constituting a wavelength conversion member together with a light-transmitting material.
[0027] The light emitting device preferably includes a light emitting element such as an LED or LD as a light source, and a wavelength conversion member containing an alkaline earth aluminate phosphor that emits light when irradiated with light from the light emitting element.
[0028] The light emitting element may be, for example, an LED chip or an LD chip, which is a semiconductor light emitting element using a nitride semiconductor. The light-emitting element preferably has an emission peak wavelength in the range of 380 nm or more and 500 nm or less, more preferably has an emission peak wavelength in the range of 390 nm or more and 495 nm or less, even more preferably has an emission peak wavelength in the range of 400 nm or more and 490 nm or less, and particularly preferably has an emission peak wavelength in the range of 420 nm or more and 490 nm or less.
[0029] The wavelength converting member includes an alkaline earth aluminate phosphor and a light-transmitting material.
[0030] In addition to the alkaline earth aluminate phosphor and the light-transmitting material, a phosphor other than the alkaline earth aluminate phosphor may be included.
[0031] The first phosphor may be an alkaline earth aluminate phosphor, and the second phosphor may have a different emission peak wavelength from the first phosphor. The second phosphor may be one type of phosphor used alone, or two or more types of phosphors may be used in combination. The second phosphor may be, for example, a phosphor having a composition represented by the following formula: M 1 10 (PO4)6Cl2:Eu(i) (In formula (i), M 1 is at least one element selected from the group consisting of Ca, Sr and Ba. M 2 MgAl 10 O 17 :Mn,Eu (ii) (In formula (ii), M 2 is at least one element selected from the group consisting of Ba and Sr. M 3 8MgSi4O 16 Cl2:Eu(iii) (In formula (iii), M 3 is at least one element selected from the group consisting of Ca, Sr and Ba. Sr4Al 14 O 25 :Eu (iv) M 4 3M 5 5O 12 :Ce (v) (In formula (v), M 4 is at least one element selected from the group consisting of Y and Gd, and M 5 is at least one element selected from the group consisting of Al and Ga.) Lu3M 6 5O 12 :Ce (vi) (In formula (vi), M 6 is at least one element selected from the group consisting of Al and Ga.) Si 6-z Al z O z N 8-z :Eu (vii) (In formula (vii), z satisfies 0 < z ≦ 4.2.) M 7 AlSiN3:Eu (viii) (In formula (viii), M 7 is at least one element selected from the group consisting of Sr and Ca.)
[0032] The light-transmitting material includes at least one selected from the group consisting of resin, glass, and inorganic substances. The resin is preferably at least one selected from the group consisting of epoxy resin, silicone resin, phenol resin, and polyimide resin. The inorganic substance includes at least one selected from the group consisting of aluminum oxide and aluminum nitride. The wavelength conversion member may contain a filler, a colorant, and a light diffusing material as needed in addition to the phosphor and the light-transmitting material. Examples of the filler include silicon oxide, barium titanate, titanium oxide, aluminum oxide, and the like.
[0033] Method for producing alkaline earth aluminate The method for producing an alkaline earth aluminate phosphor according to the third embodiment includes a method for producing an alkaline earth aluminate phosphor comprising: a first compound including at least one element A selected from the group consisting of alkaline earth metals; a second compound including Al; and a third compound including Cr, and, as necessary, at least one element M selected from the group consisting of Group 13 elements excluding Al. 1 and optionally at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm. 2 and a fifth compound including the compound, wherein at least one compound selected from the group consisting of the first compound, the second compound, and the third compound is an oxide, the molar ratio of the element A in 1 mole of the composition is within a range of 1.0 to 4.0, and the Al and the element M 1 the molar ratio of the total of the elements M is in the range of 4.0 to 14.0, the molar ratio of the Cr is in the range of 0.004 to 0.8, 2 The molar ratio of the Cr and the element M is within the range of 0 to 0.4. 2 The total molar ratio of Al and the element M is within a range of 0.004 to 0.8. 1 The molar ratio of the element M when the sum of the elements is 1 1 preparing a raw material mixture containing the first compound, the second compound, and the third compound, and optionally containing the fourth compound and optionally the fifth compound, so that a molar ratio of the first compound, the second compound, and the third compound is 0.7 or less; and heat-treating the raw material mixture in a reducing atmosphere at a temperature in the range of 1000° C. or more and 1500° C. or less to obtain an alkaline earth aluminate phosphor.
[0034] Preparation of raw material mixture raw material The raw materials for producing the alkaline earth aluminate phosphor include a first compound containing element A, a second compound containing Al, and a third compound containing Cr. The first compound, the second compound, and the third compound may be nitrides, hydrides, fluorides, oxides, carbonates, chlorides, and hydrates thereof. At least one compound selected from the group consisting of the first compound, the second compound, and the third compound may be an oxide, and two or more of the compounds may be oxides. The second compound and the third compound may be oxides. Specific examples of the first compound include Ca3N2, CaH2, CaF2, CaO, CaCO3, CaCl2, SrH2, Sr3N2, Sr2N, SrN, SrF2, SrO, SrCO3, SrCl2, Ba3N2, BaF2, BaO, BaCO3, and BaCl2. Specific examples of the second compound include AlN, AlF3, Al2O3, and AlCl3. Specific examples of the third compound include CrN, CrF3, Cr2O3, Cr2(CO3)3, and CrCl3·6H2O. When the element A is at least one element selected from the group consisting of Ca, Sr, and Ba, the first compound is preferably at least one compound selected from the group consisting of a compound containing Ca, a compound containing Sr, and a compound containing Ba. When the element A is Sr, the first compound is preferably a compound containing Sr.
[0035] element M 1 The fourth compound contains the element M 1 Examples of the fourth compound include nitrides, hydrides, fluorides, bromides, oxides, carbonates, chlorides, and hydrates thereof, including the element M. The fourth compound may be an oxide. The fourth compound is preferably a solid, and specific examples thereof include BN, B2O3, BCl3, GaN, GaBr3, Ga2O3, InBr3, In2O3, InCl3, Tl2O3, and TlF3. 1 When the element M is at least one selected from the group consisting of B, Ga, and In, the fourth compound is preferably at least one compound selected from the group consisting of a compound containing B, a compound containing Ga, and a compound containing In. 1When is Ga, the fourth compound is preferably a compound containing Ga.
[0036] element M 2 The fifth compound containing the element M 2 The fifth compound may be an oxide. The fifth compound is preferably a solid, and specific examples of the fifth compound include MnO2, Eu2O3, EuCl3·6H2O, CeCl3·7H2O, CeO2, TbCl3·6H2O, Tb4O7, PrCl3·7H2O, PrF3, Pr6O 11 , NdCl3·6H2O, Nd2O3, SmCl3·6H2O, SmF3, Sm2O3, YbF3, Yb2O3, Ho2O3, ErCl3·6H2O, Er2O3, ErF3, TmCl3·6H2O, TmF3, and Tm2O3.
[0037] raw material mixture Each compound as a raw material is weighed out so that the molar ratio of each element in 1 mole of the composition is a specific value, and then the weighed compounds as raw materials are mixed in a mixer in a wet or dry manner to obtain a raw material mixture. As the mixer, a ball mill that is commonly used industrially, as well as a vibration mill, a roll mill, a jet mill, etc. can be used.
[0038] Each compound to be used as a raw material contains the elements A, Al, and Cr, and the element M which may be contained as necessary. 1 and element M 2 It is preferable to prepare a raw material mixture containing each compound weighed so as to have a composition represented by the above formula (I). a and element A b In the case where the compound contains the element A, the element A is measured so as to have a composition represented by the formula (I-1). a Compounds containing element A b It is preferred to provide a raw material mixture that includes a compound containing the compound, and other compounds.
[0039] Flux The raw material mixture may contain a flux. By including the flux in the raw material mixture, the reaction between the raw materials is promoted, and furthermore, the solid-phase reaction proceeds more uniformly, so that a phosphor having a large particle size and excellent luminescence characteristics can be obtained. When the temperature of the heat treatment for obtaining the phosphor is about the same as the temperature at which the liquid phase of the compound used as the flux is generated, the flux promotes the reaction between the raw materials. As the flux, a halide containing at least one element selected from the group consisting of rare earth metal elements, alkaline earth metal elements, and alkali metal elements can be used. As the flux, among the halides, a fluoride can be used. When the element contained in the flux is the same element as at least a part of the elements constituting the alkaline earth aluminate phosphor, the flux can be added as a part of the raw materials of the alkaline earth aluminate phosphor having the desired composition so that the composition of the alkaline earth aluminate phosphor becomes the desired composition, or the flux can be added by further adding after mixing the raw materials so as to obtain the desired composition.
[0040] A step of obtaining an alkaline earth aluminate phosphor by heat treatment. The raw material mixture can be placed in a crucible or boat made of a material such as graphite or other carbon, boron nitride (BN), alumina (Al2O3), tungsten (W), or molybdenum (Mo), and then heat-treated in a furnace.
[0041] Heat treatment atmosphere The heat treatment is carried out in a reducing atmosphere. The reducing atmosphere may be a hydrogen-nitrogen atmosphere containing hydrogen gas and nitrogen gas having reducing properties. The hydrogen-nitrogen atmosphere may contain nitrogen gas at preferably 70% by volume or more, 80% by volume or more, or 90% by volume or more. The hydrogen-nitrogen atmosphere may contain hydrogen gas at 1% by volume or more, 2% by volume or more, 3% by volume or more, or 10% by volume or less.
[0042] Heat Treatment Temperature The heat treatment temperature is within the range of 1000° C. to 1500° C., preferably within the range of 1100° C. to 1450° C., and more preferably within the range of 1200° C. to 1400° C. If the heat treatment temperature is 1000° C. to 1500° C., decomposition due to heat is suppressed, and a phosphor having a desired composition and a stable crystal structure can be obtained.
[0043] The heat treatment may be performed in two or more stages. For example, when performing a two-stage heat treatment, the first heat treatment may be performed at a temperature of 1000°C or higher and 1500°C or lower, and the second heat treatment may be performed at a temperature of 1200°C or higher and 1400°C or lower. When the first heat treatment temperature is 1000°C or higher and 1500°C or lower, it is easy to obtain a heat-treated product having a desired composition. When the second heat treatment temperature is 1200°C or higher and 1400°C or lower, it is possible to obtain a phosphor having a stable crystal structure.
[0044] In the heat treatment, a holding time may be set at a predetermined temperature. For example, between the first heat treatment and the second heat treatment, a holding time may be set at a temperature of about room temperature, 20°C or more and 28°C or less. The holding time may be, for example, 0.5 hours to 48 hours, 1 hour to 40 hours, or 2 hours to 30 hours. By setting the holding time to 0.5 hours to 48 hours, crystal growth can be promoted.
[0045] The pressure of the heat treatment atmosphere may be standard atmospheric pressure (0.101 MPa), or may be 0.101 MPa or more, and is preferably performed in a pressurized atmosphere of 0.11 MPa to 200 MPa. The heat-treated product obtained by heat treatment is more likely to have a decomposed crystal structure as the heat treatment temperature increases, but by using a pressurized atmosphere, the decomposition of the crystal structure is suppressed and the decrease in luminescence intensity can be suppressed. The pressure of the heat treatment atmosphere is, in terms of gauge pressure, more preferably 0.11 MPa to 100 MPa, even more preferably 0.5 MPa to 10 MPa, and from the viewpoint of ease of production, even more preferably 1.0 MPa or less.
[0046] The heat treatment time can be appropriately selected depending on the heat treatment temperature and the pressure of the atmosphere during the heat treatment, and is preferably 0.5 hours or more and 20 hours or less. Even when two or more stages of heat treatment are performed, it is preferable that the heat treatment time for each step is 0.5 hours or more and 20 hours or less. When the heat treatment time is 0.5 hours or more and 20 hours or less, decomposition of the heat-treated product obtained is suppressed, and a phosphor having a stable crystal structure and a desired emission intensity can be obtained. In addition, the production cost can be reduced and the manufacturing time can be relatively short. The heat treatment time is more preferably 1 hour or more and 10 hours or less, and even more preferably 1.5 hours or more and 9 hours or less.
[0047] The heat-treated product obtained by the heat treatment may be subjected to post-treatment such as pulverization, dispersion, solid-liquid separation, drying, etc. Solid-liquid separation can be carried out by an industrially commonly used method such as filtration, suction filtration, pressure filtration, centrifugation, decantation, etc. Drying can be carried out by an industrially commonly used device such as a vacuum dryer, a hot air heating dryer, a conical dryer, a rotary evaporator, etc. EXAMPLES
[0048] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0049] Example 1 The raw materials were weighed out so that the amounts of SrCO3, Al2O3, and Cr2O3 were 8.86g, 10.71g, and 0.14g, respectively. The composition of each raw material was Sr4Al 14 O 25 :Cr 0.12 Each raw material was weighed so that the total weight of the raw materials was 1000g. The raw materials were mixed for 10 minutes using an agate mortar and an agate pestle to obtain a raw material mixture. The obtained raw material mixture was heat-treated for 8 hours at 1300°C, standard atmospheric pressure (0.101 MPa), in a hydrogen-nitrogen atmosphere containing hydrogen gas and nitrogen gas (hydrogen: 3% by volume, nitrogen: 97% by volume). After the heat treatment, the obtained heat-treated product was pulverized to obtain the alkaline earth aluminate phosphor of Example 1.
[0050] Example 2 The raw materials were weighed out so that CaCO3 was 6.01g, Al2O3 was 10.71g, and Cr2O3 was 0.15g. The composition of the mixture was Ca4Al 14 O 25 :Cr 0.12 An alkaline earth aluminate phosphor of Example 2 was obtained in the same manner as in Example 1, except that the raw materials were used so as to satisfy the following formula:
[0051] Example 3 The raw materials were weighed out so that the amounts were 4.43g SrCO3, 3.01g CaCO3, 10.71g Al2O3, and 0.14g Cr2O3. The composition of each raw material was (Sr 0.5 Ca 0.5 )4Al 14 O 25 :Cr 0.12 An alkaline earth aluminate phosphor of Example 3 was obtained in the same manner as in Example 1, except that the raw materials were weighed so as to satisfy the following formula and the heat treatment temperature was set to 1250°C.
[0052] Example 4 The raw materials were weighed out so that the amounts were 8.86g of SrCO3, 7.66g of Al2O3, 5.64g of Ga2O3, and 0.14g of Cr2O3. Each raw material had the following composition: Sr4Al 10 GaO 25 :Cr 0.12 The alkaline earth aluminate phosphor of Example 4 was obtained in the same manner as in Example 1, except that the raw materials were weighed and used so as to satisfy the following formula: and the heat treatment temperature was set to 1250° C. 1 The element M when the total molar ratio of (Ga) is 1 1 The molar ratios of Al and element M in the alkaline earth aluminate phosphors and compounds having the alkaline earth aluminate compositions of Examples 1 to 3, Examples 5 and 6 described below, and Comparative Examples 1 and 2 are shown in Table 1. 1 The element M when the total molar ratio of (Ga) is 1 1 The molar ratio of (Ga) is also shown in Table 1.
[0053] Example 5 The raw materials were weighed out so that the amounts were 8.86g of SrCO3, 5.36g of Al2O3, 9.86g of Ga2O3, and 0.14g of Cr2O3. The composition of each raw material was Sr4Al7Ga7O 25 :Cr 0.12 An alkaline earth aluminate phosphor of Example 5 was obtained in the same manner as in Example 1, except that the raw materials were weighed so as to satisfy the following formula and the heat treatment temperature was set to 1200°C.
[0054] Example 6 The raw materials were weighed out so that the amounts were 8.86g of SrCO3, 4.60g of Al2O3, 11.27g of Ga2O3, and 0.14g of Cr2O3. The composition of each raw material was Sr4Al6Ga8O 25 :Cr 0.12 An alkaline earth aluminate phosphor of Example 6 was obtained in the same manner as in Example 1, except that the raw materials were weighed so as to satisfy the following formula and the heat treatment temperature was set to 1200°C.
[0055] Comparative Example 1 A compound having the composition of the alkaline earth aluminate of Comparative Example 1 was obtained in the same manner as in Example 1, except that the heat treatment was carried out in an air atmosphere (oxygen: about 20 volume %, nitrogen: about 78 volume %).
[0056] Comparative Example 2 The raw materials were weighed out so that the amounts were 8.86g of SrCO3, 3.07g of Al2O3, 14.09g of Ga2O3, and 0.14g of Cr2O3. Each raw material had the following composition: Sr4Al4Ga 10 O 25 :Cr 0.12 A compound having the composition of the alkaline earth aluminate of Comparative Example 2 was obtained in the same manner as in Example 1, except that the raw materials were weighed and used so as to satisfy the following formula: and the heat treatment temperature was 1200°C.
[0057] Measurement of emission spectrum The emission spectrum of each alkaline earth aluminate phosphor of the Examples and the compound having the composition of each alkaline earth aluminate of the Comparative Examples was measured using a quantum efficiency measurement system (QE-2000, manufactured by Otsuka Electronics Co., Ltd.). The emission peak wavelength of the excitation light used in the quantum efficiency measurement system was 450 nm. From each obtained emission spectrum, the emission peak wavelength (nm) and the half width (nm) at the emission peak in the range of 720 nm to 900 nm were obtained. The results are shown in Table 1. In addition, the emission intensity at the emission peak wavelength of Example 2 was set to 100%, and the relative emission intensity (%) at the emission peak wavelength of the alkaline earth aluminate phosphor of the Examples and the compound having the composition of each alkaline earth aluminate of the Comparative Examples was measured. The results are shown in Table 1. FIG. 1 shows the emission spectrum of the alkaline earth aluminate phosphor of Example 1 and the emission spectrum of the compound having the composition of alkaline earth aluminate of Comparative Example 1. FIG. 3 shows the emission spectra of the alkaline earth aluminate phosphors according to Examples 4, 5 and 6, and the emission spectrum of a compound having the alkaline earth aluminate composition according to Comparative Example 2.
[0058] Measurement of excitation spectrum The excitation spectrum of the alkaline earth aluminate phosphor according to Example 1 was measured in the range of 350 nm to 700 nm at an emission wavelength of 791 nm at 25° C.±5° C. (room temperature) using a spectrofluorophotometer (F-4500, manufactured by Hitachi High-Technologies Corporation). FIG. 2 shows the excitation spectrum of the alkaline earth aluminate phosphor according to Example 1.
[0059] [Table 1]
[0060] The alkaline earth aluminate phosphors according to Examples 1 to 6 have a peak emission wavelength in the range of 720 nm to 900 nm in the emission spectrum, and show a broad emission peak with a half-width of 80 nm or more. From this result, it is clear that the alkaline earth aluminate phosphors according to Examples 1 to 6 can emit light having a peak emission wavelength in the near-infrared wavelength range called the "biological window," and can emit light that has an effect on the photoreceptors of plants.
[0061] As shown in FIGS. 1 and 3, each of the alkaline earth aluminate phosphors according to Examples 1 and 4 to 6 had an emission peak wavelength in the range of 720 nm or more and 900 nm or less, and had a wide half-value width of 80 nm or more.
[0062] 2, in the excitation spectrum of the wavelength range of 350 nm to 700 nm, the alkaline earth aluminate phosphor of Example 1 has high relative intensities in the wavelength range of 400 nm to 450 nm and in the wavelength range of 550 nm to 580 nm. This result shows that by selecting the emission peak wavelength of the excitation light source, the alkaline earth aluminate phosphor can efficiently emit light having an emission peak wavelength in the range of 720 nm to 900 nm.
[0063] The compounds having the alkaline earth aluminate compositions according to Comparative Examples 1 and 2 hardly emitted light even when irradiated with light having an emission peak wavelength of 450 nm. [Industrial Applicability]
[0064] The alkaline earth aluminate phosphor of the present disclosure can be used in light-emitting devices used in lighting devices, backlights for liquid crystal display devices, etc. Furthermore, the alkaline earth aluminate phosphor of one embodiment of the present invention can also be used in light-emitting devices for medical lighting to obtain information within a living body, and light-emitting devices for plant cultivation that affect the photoreceptors of plants.
Claims
1. At least one element A selected from the group consisting of alkaline earth metal elements, Al, Cr, and at least one element M selected from the group consisting of Group 13 elements excluding Al as required. 1 and optionally at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm. 2 wherein the element A, the Al, the Cr, and the elements M 1 and M 2 which are included as necessary are represented by the following formula (I), and the alkaline earth aluminate phosphor has an emission peak wavelength in the range of 720 nm to 900 nm. A x (Al 1-y M 1 y) z O x + 3 / 2z: Cr v ,M 2 w (I) (In the formula (I), v, w, x, y, and z satisfy 0.004≦v≦0.8, 0≦w≦0.4, 0.004≦v+w≦0.8, x=4.0, 0≦y≦0.7, and 4.0≦z≦14.0.)
2. The alkaline earth aluminate phosphor according to claim 1, wherein when the element A contains two or more elements selected from the group consisting of alkaline earth metal elements, the alkaline earth aluminate phosphor has a composition represented by the following formula (I-1): (A a 1-u A b u ) x (Al 1-y M 1 y ) z O x+3 / 2z :Cr v , M 2 w (I-1) (In formula (I-1), A a is one element selected from the group consisting of alkaline earth metal elements, A b is one element selected from the group consisting of alkaline earth metal elements excluding A a , M 1 is at least one element selected from the group consisting of Group 13 elements excluding Al, M 2 is at least one element selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm, and u, v, w, x, y and z satisfy 0.1≦u≦0.9, 0.004≦v≦0.8, 0≦w≦0.4, 0.004≦v+w≦0.8, x=4.0, 0≦y≦0.7, 4.0≦z≦14.0.)
3. The element A is at least one element selected from the group consisting of Ca, Sr and Ba, and the element M 1 3. The alkaline earth aluminate phosphor according to claim 1, wherein is at least one element selected from the group consisting of B, Ga and In.
4. The element A is Sr, and the element M 1 3. The alkaline earth aluminate phosphor of claim 1, wherein is Ga.
5. 5. The alkaline earth aluminate phosphor according to claim 1, having an emission spectrum with an emission peak wavelength in the range of 720 nm or more and 900 nm or less and a half-value width of 80 nm or more.
6. The alkaline earth aluminate phosphor according to claim 1, wherein in formula (I) or formula (I-1), z=14.
0.
7. A light emitting device comprising: the alkaline earth aluminate phosphor according to claim 1 ; and a light source for irradiating the alkaline earth aluminate phosphor.
8. A first compound including at least one element A selected from the group consisting of alkaline earth metals, a second compound including Al, and a third compound including Cr, and optionally including at least one element M selected from the group consisting of Group 13 elements excluding Al. 1 and optionally at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm. 2 and a fifth compound comprising: preparing a raw material mixture so that the element A, Al, Cr, and the elements M 1 and M 2 contained as necessary have a composition represented by the following formula (I); and heat-treating the raw material mixture in a reducing atmosphere at a temperature in the range of 1000° C. to 1500° C. to obtain an alkaline earth aluminate phosphor. A x (Al 1-y M 1 y) z O x + 3 / 2z: Cr v ,M 2 w (I) (In the formula (I), v, w, x, y, and z satisfy 0.004≦v≦0.8, 0≦w≦0.4, 0.004≦v+w≦0.8, x=4.0, 0≦y≦0.7, and 4.0≦z≦14.0.)
9. The method for producing an alkaline earth aluminate phosphor described in claim 8, wherein, in the step of preparing the raw material mixture, when the element A contains two or more elements selected from the group consisting of alkaline earth metal elements, the raw material mixture is prepared so as to have a composition represented by the following formula (I-1): (A a 1-u A b u ) x (Al 1-y M 1 y ) z O x+3 / 2z :Cr v , M 2 w (I-1) (In formula (I-1), A a is one element selected from the group consisting of alkaline earth metal elements, A b is one element selected from the group consisting of alkaline earth metal elements excluding A a , M 1 is at least one element selected from the group consisting of Group 13 elements excluding Al, M 2 is at least one element selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm, and u, v, w, x, y and z satisfy 0.1≦u≦0.9, 0.004≦v≦0.8, 0≦w≦0.4, 0.004≦v+w≦0.8, x=4.0, 0≦y≦0.7, 4.0≦z≦14.0.)
10. The element A is at least one element selected from the group consisting of Ca, Sr and Ba, and the element M 1 10. The method for producing an alkaline earth aluminate phosphor according to claim 8, wherein is at least one element selected from the group consisting of B, Ga and In.
11. The element A is Sr, and the element M is included as necessary. 1 The method for producing an alkaline earth aluminate phosphor according to claim 8 or 9, wherein is Ga.
12. 12. The method for producing an alkaline earth aluminate phosphor according to claim 8, wherein at least one selected from the group consisting of the fourth compound and the fifth compound is an oxide.
13. The method for producing an alkaline earth aluminate phosphor according to claim 8 , wherein the temperature of the heat treatment is within a range of 1100° C. or more and 1450° C. or less.
14. 14. The method for producing an alkaline earth aluminate phosphor according to claim 8, wherein the reducing atmosphere contains nitrogen gas and hydrogen gas, and the hydrogen gas content is 1 volume % or more.
15. The method for producing an alkaline earth aluminate phosphor according to claim 8, wherein z=14.0 in formula (I) or formula (I-1).
Citation Information
Patent Citations
Infrared LED
WO2015177327A1
Light emitting device and fluorescent body
WO2018143198A1
Light emitting device and phosphor
WO2018207703A1