Resin composition
A resin composition of polyimide and siloxane-containing polycarbonate resins addresses warping and thermal expansion issues in flexible substrates, achieving a cured product with improved thermal stability and compatibility.
Patent Information
- Application Number
- JP2019136416
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-07-24
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2039-07-24
AI Technical Summary
Polyimide and polycarbonate resins used in flexible substrates have low thermal expansion coefficients but are prone to warping, while polysiloxane resins suppress warping but have high thermal expansion and low compatibility.
A resin composition comprising a polyimide resin and a siloxane-containing polycarbonate resin, with specific molecular weight ranges and ratios, to achieve a cured product with low thermal expansion and suppressed warping.
The composition results in a cured product with a low coefficient of thermal expansion and reduced warpage, enhancing compatibility and performance in flexible substrates.
Smart Images

Figure 0007575865000001 
Figure 0007575865000002 
Figure 0007575865000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition containing a polyimide resin, and further to a cured product, a resin sheet, a multilayer flexible substrate, and a semiconductor device obtained by using the resin composition. [Background technology]
[0002] In recent years, there has been an increasing demand for thinner, lighter, and more densely packed semiconductor components. To meet this demand, the use of flexible boards as substrates for semiconductor components has been attracting attention. Flexible boards can be made thinner and lighter than rigid boards. Furthermore, flexible boards are flexible and deformable, so they can be folded for mounting.
[0003] Flexible substrates are generally manufactured by preparing a three-layer film consisting of a polyimide film, a copper foil, and an adhesive, or a two-layer film consisting of a polyimide film and a conductor layer, and etching the conductor layer according to a subtractive method to form a circuit. Conventionally, three-layer films have been widely used because they can be produced relatively inexpensively. However, in circuit boards having high-density wiring, two-layer films are sometimes used to solve problems with the heat resistance and electrical insulation of the adhesive. However, two-layer films have problems with cost and productivity. Therefore, in order to solve this problem, Patent Documents 1 to 3 disclose insulating materials for multilayer flexible substrates. Patent Documents 4 and 5 also describe polyimide resins. Patent Document 6 also describes siloxane-containing polycarbonate resins. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2006-37083 A [Patent Document 2] JP 2016-41797 A [Patent Document 3] Patent No. 6387181 [Patent Document 4] Patent No. 6240798 [Patent Document 5] Patent No. 6240799 [Patent Document 6] Patent No. 6343680 Summary of the Invention [Problem to be solved by the invention]
[0005] Generally, polyimide resins and polycarbonate resins used for flexible substrates have a low thermal expansion coefficient but are prone to large warping, whereas polysiloxane resins are known to suppress warping but have a high thermal expansion coefficient and low compatibility.
[0006] An object of the present invention is to provide a resin composition and the like which can give a cured product having a low coefficient of thermal expansion and suppressed warping. [Means for solving the problem]
[0007] Means for Solving the Problems of the Invention The present inventors conducted intensive research to achieve the objects of the present invention and unexpectedly found that by using a resin composition containing (A) a polyimide resin and (B) a siloxane-containing polycarbonate resin, a cured product having a low thermal expansion coefficient and suppressed warping can be obtained, thereby completing the present invention.
[0008] That is, the present invention includes the following. [1] A resin composition comprising (A) a polyimide resin and (B) a siloxane-containing polycarbonate resin. [2] The resin composition according to the above [1], wherein the weight average molecular weight of the (A) component is 1,000 or more and 100,000 or less. [3] The resin composition according to the above [1] or [2], wherein the component (B) is a polycarbonate-polysiloxane copolymer containing a polycarbonate block having a polycarbonate structure and a polysiloxane block having a polysiloxane structure. [4] The resin composition according to the above [3], wherein the polysiloxane structure is a polydialkylsiloxane structure. [5] The resin composition according to the above [3] or [4], wherein the polycarbonate structure is an aromatic polycarbonate structure. [6] The resin composition according to any one of the above [3] to [5], wherein the content of the polysiloxane structure in the component (B) is 1% by mass or more and 30% by mass or less, when the component (B) is taken as 100% by mass. [7] The resin composition according to any one of the above [1] to [6], wherein the viscosity average molecular weight of component (B) is 13,000 or more and 25,000 or less. [8] The resin composition according to any one of the above [1] to [7], wherein a mass ratio of the component (A) to the component (B) (component (A) / component (B)) is 1 or more and 5 or less. [9] The resin composition according to any one of the above [1] to [8], further comprising (C) an inorganic filler.
[10] The resin composition according to the above [9], wherein the component (C) is silica.
[11] The resin composition according to [9] or
[10] above, wherein the content of the (C) component is 30% by mass or more and 60% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass.
[12] The resin composition according to any one of the above [1] to
[11] , further comprising (D) an epoxy resin and (E) a curing agent.
[13] The resin composition according to the above
[12] , wherein the component (E) contains an active ester-based curing agent.
[14] The resin composition according to any one of the above [1] to
[13] , which is for forming an insulating layer of a multilayer flexible substrate.
[15] A cured product of the resin composition according to any one of [1] to
[14] above.
[16] A resin sheet comprising a support and a resin composition layer formed on the support from the resin composition according to any one of [1] to
[14] above.
[17] A multilayer flexible substrate comprising an insulating layer formed by curing the resin composition according to any one of the above [1] to
[14] .
[18] A semiconductor device comprising the multilayer flexible substrate described in
[17] above. Effect of the Invention
[0009] According to the resin composition of the present invention, it is possible to obtain a cured product having a low coefficient of thermal expansion and suppressed warping. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0011] <Resin composition> The resin composition of the present invention contains (A) a polyimide resin and (B) a siloxane-containing polycarbonate resin. By using such a resin composition, a cured product having a low thermal expansion coefficient and suppressed warping can be obtained. In addition, the compatibility of each component can be excellent.
[0012] The resin composition of the present invention may further contain optional components in addition to the (A) polyimide resin and the (B) siloxane-containing polycarbonate resin. Examples of the optional components include (C) inorganic filler, (D) epoxy resin, (E) curing agent, (F) curing accelerator, (G) other additives, and (H) organic solvent. Each component contained in the resin composition will be described in detail below.
[0013] <(A) Polyimide resin> The resin composition of the present invention includes a polyimide resin (A). The polyimide resin (A) is a resin having an imide bond in a repeating unit. The polyimide resin (A) may generally include a resin obtained by an imidization reaction between a diamine compound and a tetracarboxylic acid anhydride. The polyimide resin (A) also includes modified polyimide resins such as siloxane-modified polyimide resins.
[0014] The polyimide resin (A) is not particularly limited, but may be, for example, a polyimide resin represented by the formula (1):
[0015] [ka]
[0016] [where, X 1 represents a tetravalent group obtained by removing two -CO-O-CO- from a tetracarboxylic dianhydride, and may be, for example, an organic group having 2 to 100 (preferably 2 to 50) skeletal atoms selected from carbon atoms, oxygen atoms, nitrogen atoms, and sulfur atoms. X 2 represents a divalent group obtained by removing two -NH2 from a diamine compound, and may be, for example, an organic group having 2 to 100 (preferably 2 to 50) skeletal atoms selected from carbon atoms, oxygen atoms, nitrogen atoms, and sulfur atoms. n represents an integer of 2 or more.]. X in formula (1) may include a structure represented by the following formula. 1 and X 2 The organic group is not particularly limited as long as it is within the range of a chemically stable structure, and may be a structure appropriately selected by a person skilled in the art, for example, a structure of a known polyimide resin. When the (A) polyimide resin contains a structure represented by formula (1), it preferably contains 80 mass % or more of the structure represented by formula (1), more preferably contains 85 mass % or more, even more preferably contains 90 mass % or more, and particularly preferably contains 95 mass % or more.
[0017] The diamine compound for preparing the (A) polyimide resin is not particularly limited, but examples thereof include aliphatic diamine compounds and aromatic diamine compounds.
[0018] Examples of the aliphatic diamine compound include linear aliphatic diamine compounds such as 1,2-ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane, 1,6-hexamethylenediamine, 1,5-diaminopentane, and 1,10-diaminodecane; branched aliphatic diamine compounds such as 1,2-diamino-2-methylpropane, 2,3-diamino-2,3-butane, and 2-methyl-1,5-diaminopentane; alicyclic diamine compounds such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,4-diaminocyclohexane, and 4,4'-methylenebis(cyclohexylamine); and dimer acid diamines (hereinafter also referred to as "dimer diamines").
[0019] The dimer acid type diamine means a diamine compound obtained by replacing two terminal carboxyl groups (-COOH) of a dimer acid with an aminomethyl group (-CH2-NH2) or an amino group (-NH2). Dimer acid is a known compound obtained by dimerizing an unsaturated fatty acid (preferably one having 11 to 22 carbon atoms, particularly preferably one having 18 carbon atoms), and its industrial production process is almost standardized in the industry. Dimer acid is easily obtained, especially those containing dimer acid having 36 carbon atoms as the main component obtained by dimerizing unsaturated fatty acid having 18 carbon atoms such as oleic acid and linoleic acid, which are inexpensive and easily available. In addition, dimer acid may contain any amount of monomer acid, trimer acid, other polymerized fatty acid, etc., depending on the production method, degree of purification, etc. In addition, although double bonds remain after the polymerization reaction of unsaturated fatty acid, in this specification, hydrogenated products in which the degree of unsaturation is reduced by further hydrogenation reaction are also included in dimer acid. Dimer acid type diamines are commercially available, and examples thereof include PRIAMINE 1073, PRIAMINE 1074, and PRIAMINE 1075 manufactured by Croda Japan, and Versamine 551 and Versamine 552 manufactured by Cognis Japan.
[0020] Examples of the aromatic diamine compound include a phenylenediamine compound, a naphthalenediamine compound, and a dianiline compound.
[0021] The phenylenediamine compound means a compound consisting of a benzene ring having two amino groups, and the benzene ring may further have any of 1 to 3 substituents. The substituents on the benzene ring are not particularly limited, and examples thereof include a halogen atom, an alkyl group, an alkoxy group, an alkylcarbonyl group, an alkoxycarbonyl group, an alkylcarbonyloxy group, an aryl group, an aryloxy group, an arylcarbonyl group, an aryloxycarbonyl group, an arylcarbonyloxy group, an aralkyl group, and combinations thereof.
[0022] Examples of the "halogen atom" include a fluorine atom, a chlorine atom, and a bromine atom. The "alkyl group" refers to a linear, branched, or cyclic monovalent aliphatic saturated hydrocarbon group. The "alkyl group" is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. Examples of the "alkyl group" include a methyl group, an ethyl group, a propyl group, an isopropyl group, a cyclopentyl group, and a cyclohexyl group. The "alkoxy group" refers to a monovalent group (alkyl-O-) formed by an alkyl group bonding to an oxygen atom. The "alkoxy group" is preferably an alkoxy group having 1 to 6 carbon atoms, and more preferably an alkoxy group having 1 to 3 carbon atoms. Examples of the "alkoxy group" include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a cyclopentoxy group, and a cyclohexyloxy group. The "alkylcarbonyl group" refers to a monovalent group (alkyl-CO-) formed by an alkyl group bonding to a carbonyl. The "alkylcarbonyl group" is preferably an alkylcarbonyl group having 2 to 7 carbon atoms, more preferably an alkylcarbonyl group having 2 to 4 carbon atoms. Examples of the "alkylcarbonyl group" include an acetyl group, a propanoyl group, a butanoyl group, and a 2-methylpropanoyl group. The "alkoxycarbonyl group" refers to a monovalent group (alkyl-O-CO-) formed by an alkoxy group bonding to a carbonyl. The "alkoxycarbonyl group" is preferably an alkoxycarbonyl group having 2 to 7 carbon atoms, more preferably an alkoxycarbonyl group having 2 to 4 carbon atoms. Examples of the "alkoxycarbonyl group" include a methoxycarbonyl group, an ethoxycarbonyl group, and a propoxycarbonyl group. The "alkylcarbonyloxy group" refers to a monovalent group (alkyl-CO-O-) formed by an alkylcarbonyl group bonding to an oxygen atom. The "alkylcarbonyloxy group" is preferably an alkylcarbonyloxy group having 2 to 7 carbon atoms, more preferably an alkylcarbonyloxy group having 2 to 4 carbon atoms. Examples of the "alkylcarbonyloxy group" include an acetyloxy group, a propanoyloxy group, and a butanoyloxy group. The "aryl group" refers to a monovalent aromatic hydrocarbon group.The "aryl group" is preferably an aryl group having 6 to 14 carbon atoms, more preferably an aryl group having 6 to 10 carbon atoms. Examples of the "aryl group" include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group, and is preferably a phenyl group. The "aryloxy group" refers to a monovalent group (aryl-O-) formed by an aryl group bonding to an oxygen atom. The "aryloxy group" is preferably an aryloxy group having 6 to 14 carbon atoms, more preferably an aryloxy group having 6 to 10 carbon atoms. Examples of the "aryloxy group" include a phenoxy group, a 1-naphthoxy group, and a 2-naphthoxy group. The "arylcarbonyl group" refers to a monovalent group (aryl-CO-) formed by an aryl group bonding to a carbonyl. The "arylcarbonyl group" is preferably an arylcarbonyl group having 7 to 15 carbon atoms, more preferably an arylcarbonyl group having 7 to 11 carbon atoms. Examples of the "arylcarbonyl group" include a benzoyl group, a 1-naphthoyl group, and a 2-naphthoyl group. The "aryloxycarbonyl group" refers to a monovalent group (aryl-O-CO-) formed by bonding an aryloxy group to a carbonyl. The "aryloxycarbonyl group" is preferably an aryloxycarbonyl group having 7 to 15 carbon atoms, and more preferably an aryloxycarbonyl group having 7 to 11 carbon atoms. Examples of the "aryloxycarbonyl group" include a phenoxycarbonyl group, a 1-naphthoxycarbonyl group, and a 2-naphthoxycarbonyl group. The "arylcarbonyloxy group" refers to a monovalent group (aryl-CO-O-) formed by bonding an arylcarbonyl group to an oxygen atom. The "arylcarbonyloxy group" is preferably an arylcarbonyloxy group having 7 to 15 carbon atoms, and more preferably an arylcarbonyloxy group having 7 to 11 carbon atoms. Examples of the "arylcarbonyloxy group" include a benzoyloxy group, a 1-naphthoyloxy group, and a 2-naphthoyloxy group. The "aralkyl group" refers to an alkyl group substituted with one or more aryl groups. The "aralkyl group" is preferably an aralkyl group having 7 to 15 carbon atoms, and more preferably an aralkyl group having 7 to 11 carbon atoms.Examples of the "aralkyl group" include a benzyl group, a phenethyl group, and a 2-naphthylmethyl group.
[0023] Specific examples of the phenylenediamine compound include 1,4-phenylenediamine, 1,2-phenylenediamine, 1,3-phenylenediamine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobiphenyl, and 2,4,5,6-tetrafluoro-1,3-phenylenediamine.
[0024] The naphthalene diamine compound means a compound consisting of a naphthalene ring having two amino groups, and the naphthalene ring may have 1 to 3 substituents. The substituents of the naphthalene ring are not particularly limited, but may be the same as those exemplified as the substituents of the benzene ring in the phenylenediamine compound. Specific examples of the naphthalene diamine compound include 1,5-diaminonaphthalene, 1,8-diaminonaphthalene, 2,6-diaminonaphthalene, and 2,3-diaminonaphthalene.
[0025] The dianiline compound means a compound containing two aniline structures in the molecule, and each of the two benzene rings in the two aniline structures may further have 1 to 3 optional substituents. The substituents here are not particularly limited, but may be the same as those exemplified as the substituents of the benzene ring in the phenylenediamine compound. The two aniline structures in the dianiline compound may be bonded via a direct bond and / or one or two divalent linking groups having 1 to 100 (preferably 1 to 50, more preferably 1 to 20) skeletal atoms selected from carbon, oxygen, sulfur, and nitrogen atoms. The dianiline compound also includes one in which the two aniline structures are bonded at two positions.
[0026] Examples of the "divalent linking group" in the dianiline compound include, for example, -NHCO-, -OCO-, -O-, -S-, -CO-, -SO2-, -SO-, -NH-, -(alkylene group)-, -(haloalkylene group)-, -CH=CH-, -Ph-, -Ph-Ph-, -Ph-O-Ph-, -Ph-S-Ph-, -Ph-CO-Ph-, -Ph-SO2-Ph-, -Ph-SO-Ph-, -Ph-NH-Ph-, -Ph-(alkylene group)-Ph-, -(alkylene group)-Ph-(alkylene group)-, -Ph-(haloalkylene group)-Ph-, -(haloalkylene group)-Ph-(haloalkylene group)-, -O-Ph-O-, -O-Ph-Ph-O-, -O-Ph-O-Ph-O-, -O-Ph-CO-Ph-O-, -O-Ph-SO2-Ph-O-, -O-Ph-(alkylene group)-Ph-O-, -O-(alkylene group)-Ph-(alkylene group)-O-, -O-Ph-(haloalkylene group)-Ph-O-, -O-(haloalkylene group)-Ph-(haloalkylene group)-O-,
[0027] [ka]
[0028] (In the formula, * indicates a binding site.) etc.
[0029] "Ph" represents a 1,4-phenylene group, a 1,3-phenylene group, or a 1,2-phenylene group. "Alkylene group" refers to a linear, branched, or cyclic divalent aliphatic saturated hydrocarbon group. "Alkylene group" is preferably an alkylene group having 1 to 6 carbon atoms, more preferably an alkylene group having 1 to 3 carbon atoms. Examples of the "alkylene group" include, but are not limited to, -CH2-, -CH2-CH2-, -CH(CH3)-, -CH2-CH2-CH2-, -CH2-CH(CH3)-, -CH(CH3)-CH2-, -C(CH3)2-, -CH2-CH2-CH2-CH2-, -CH2-CH2-CH(CH3)-, -CH2-CH(CH3)-CH2-, -CH(CH3)-CH2-CH2-, -CH2-C(CH3)2-, -C(CH3)2-CH2-, -CH2-CH2-CH2- Examples of the haloalkylene group include CH2-CH2-, -CH2-CH2-CH2-CH(CH3)-, -CH2-CH2-CH(CH3)-CH2-, -CH2-CH(CH3)-CH2-CH2-, -CH(CH3)-CH2-CH2-CH2-, -CH2-CH2-C(CH3)2-, -CH2-C(CH3)2-CH2-, -C(CH3)2-CH2-CH2-, -C(CH2CH3)2-, 1,1-cyclohexylene, and 3,3,5-trimethyl-1,1-cyclohexylene. The haloalkylene group is preferably a haloalkylene group having 1 to 6 carbon atoms, and more preferably a haloalkylene group having 1 to 3 carbon atoms. Examples of the "haloalkylene group" include the above-mentioned alkylene groups in which all of the hydrogen atoms have been replaced with fluorine atoms.
[0030] Specific examples of the dianiline compound include 4,4'-diamino-2,2'-ditrifluoromethyl-1,1'-biphenyl, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, 4-aminophenyl 4-aminobenzoate, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis (4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis(4-aminophenyl)propane, 4,4'-(hexafluoroisopropylidene)dianiline, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, α,α-bis[4-(4-aminophenoxy)phenyl]-1,3-diisopropylbenzene , α,α-bis[4-(4-aminophenoxy)phenyl]-1,4-diisopropylbenzene, 4,4'-(9-fluorenylidene)dianiline, 2,2-bis(3-methyl-4-aminophenyl)propane, 2,2-bis(3-methyl-4-aminophenyl)benzene, 4,4'-diamino-3,3'-dimethyl-1,1'-biphenyl, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 9,9'-bis(3-methyl-4- Examples of such an aminobenzoic acid include 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindan, and 5-amino-1,1'-biphenyl-2-yl 4-aminobenzoate. Preferred are 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindan, and 5-amino-1,1'-biphenyl-2-yl 4-aminobenzoate.
[0031] The diamine compound may be a commercially available product or may be synthesized by a known method. The diamine compound may be used alone or in combination of two or more kinds.
[0032] The tetracarboxylic acid anhydride for preparing the (A) polyimide resin is not particularly limited, and examples thereof include aromatic tetracarboxylic acid dianhydrides and aliphatic tetracarboxylic acid dianhydrides.
[0033] Examples of aromatic tetracarboxylic dianhydrides include benzenetetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, anthracenetetracarboxylic dianhydride, diphthalic dianhydride, and the like, with diphthalic dianhydride being preferred.
[0034] Benzenetetracarboxylic dianhydride means a dianhydride of benzene having four carboxy groups, and further, the benzene ring here may have 1 to 3 optional substituents. Here, the substituent is not particularly limited, but may be the same as those exemplified as the substituent of the benzene ring in the phenylenediamine compound. Specific examples of the benzenetetracarboxylic dianhydride include pyromellitic dianhydride and 1,2,3,4-benzenetetracarboxylic dianhydride.
[0035] Naphthalenetetracarboxylic dianhydride means a dianhydride of naphthalene having four carboxy groups, and further, the naphthalene ring here may have 1 to 3 optional substituents. Here, the substituent is not particularly limited, but may be the same as those exemplified as the substituent of the benzene ring in the phenylenediamine compound. Specific examples of naphthalenetetracarboxylic dianhydride include 1,4,5,8-naphthalenetetracarboxylic dianhydride and 2,3,6,7-naphthalenetetracarboxylic dianhydride.
[0036] Anthracene tetracarboxylic dianhydride means a dianhydride of anthracene having four carboxy groups, and further, the anthracene ring here may have 1 to 3 substituents. Here, the substituent is not particularly limited, but may be the same as those exemplified as the substituent of the benzene ring in the phenylenediamine compound. There is no particular limit. Specific examples of anthracene tetracarboxylic dianhydride include 2,3,6,7-anthracene tetracarboxylic dianhydride.
[0037] Diphthalic dianhydride means a compound containing two phthalic anhydride structures in the molecule, and further, each of the two benzene rings in the two phthalic anhydride structures may have 1 to 3 optional substituents. Here, the substituents are not particularly limited, but may be the same as those exemplified as the substituents of the benzene ring in the phenylenediamine compound. The two phthalic anhydrides in the diphthalic dianhydride may be bonded directly or via a divalent linking group having 1 to 100 (preferably 1 to 50, more preferably 1 to 20) skeletal atoms selected from carbon, oxygen, sulfur, and nitrogen atoms.
[0038] Examples of the "divalent linking group" in the diphthalic dianhydride include the same as the "divalent linking group" in the dianiline compound.
[0039] Specific examples of diphthalic dianhydride include 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,2',3,3'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 2,3,3',4'-diphenyl sulfone tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenoxyphenyl)sulfone dianhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethynylidene-4,4'-diphthalic Acid dianhydride, 2,2-propylidene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenyl)benzene dianhydride 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)bisphthalic dianhydride, and the like.
[0040] Specific examples of the aliphatic tetracarboxylic dianhydride include 1,2,3,4-cyclobutane tetracarboxylic dianhydride, cyclopentane tetracarboxylic dianhydride, cyclohexane-1,2,3,4-tetracarboxylic dianhydride, cyclohexane-1,2,4,5-tetracarboxylic dianhydride, 3,3',4,4'-bicyclohexyl tetracarboxylic dianhydride, carbonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, methylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,2-ethylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, thio-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, and sulfonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride.
[0041] The tetracarboxylic dianhydride may be a commercially available product, or may be synthesized by a known method or a method similar thereto. The tetracarboxylic dianhydride may be used alone or in combination of two or more kinds.
[0042] The content of structures derived from aromatic tetracarboxylic dianhydrides relative to all structures derived from tetracarboxylic dianhydrides constituting the (A) polyimide resin is preferably 10 mol % or more, more preferably 30 mol % or more, even more preferably 50 mol % or more, still more preferably 70 mol % or more, still more preferably 90 mol % or more, and particularly preferably 100 mol %.
[0043] The weight average molecular weight of the (A) polyimide resin is not particularly limited, but is preferably at least 1,000, more preferably at least 5,000, even more preferably at least 8,000, and particularly preferably at least 10,000. The upper limit of the weight average molecular weight of the (A) polyimide resin is not particularly limited, but is preferably not more than 100,000, more preferably not more than 80,000, particularly preferably not more than 60,000, and particularly preferably not more than 50,000.
[0044] The content of the polyimide resin (A) in the resin composition is not particularly limited, but is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more, when the nonvolatile components in the resin composition are taken as 100% by mass. The upper limit of the content of the polyimide resin (A) is not particularly limited, but is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less, and particularly preferably 20% by mass or less, when the nonvolatile components in the resin composition are taken as 100% by mass.
[0045] <(B) Siloxane-containing polycarbonate resin> The resin composition of the present invention contains (B) a siloxane-containing polycarbonate resin. (B) Siloxane-containing polycarbonate resin means a polymer having a polysiloxane structure (preferably a polydiorganosiloxane structure) in the main chain or side chain and a carbonate bond (-O-CO-O-) in the repeating unit of the main chain, and the main chain may have a branched structure. (B) Siloxane-containing polycarbonate resin may be, for example, a polycarbonate-polysiloxane copolymer containing a polycarbonate block having a polycarbonate structure obtained by polycarbonating a dihydroxy compound, and a polysiloxane block having a polysiloxane structure (preferably a polydiorganosiloxane structure).
[0046] The dihydroxy compound for obtaining the polycarbonate block may be any dihydroxy compound generally used for obtaining a polycarbonate resin, and among them, aromatic diols are preferred. In other words, the polycarbonate structure in the polycarbonate block is preferably an aromatic polycarbonate structure. Examples of aromatic diols include bisphenol compounds and bisnaphthol compounds.
[0047] The bisphenol compound means a compound containing two phenol structures in the molecule, and each of the two benzene rings in the two phenol structures may further have 1 to 3 optional substituents. The substituents here are not particularly limited, but may be the same as those exemplified as the substituents of the benzene ring in the phenylenediamine compound. The two phenol structures in the bisphenol compound may be bonded via a direct bond and / or a divalent linking group having 1 to 100 (preferably 1 to 50, more preferably 1 to 20) skeletal atoms selected from carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms.
[0048] Examples of the "divalent linking group" in the bisphenol compound include the same as the "divalent linking group" in the dianiline compound.
[0049] Specific examples of bisphenol compounds include 4,4'-dihydroxybiphenyl, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxy-3,3'-biphenyl)propane, 2,2-bis(4-hydroxy-3-isopropylphenyl)propane, 2,2-bis(3 -tert-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 1,1-bis(3-cyclohexyl-4-hydroxyphenyl)cyclohexane, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, (p-hydroxy-3-methylphenyl)fluorene, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, 4,4'-dihydroxy-3 ,3'-dimethyldiphenyl sulfide, 2,2'-diphenyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfide, 1,3-bis{2-(4-hydroxyphenyl)-2-propyl}benzene, 1,4-bis{2-(4-hydroxyphenyl)-2-propyl}benzene, 1,4-bis(4-hydroxyphenyl)cyclohexane, 1,3-bis(4-hydroxyphenyl)cyclohexane, and the like.
[0050] The bisnaphthol compound means a compound containing two naphthol structures in the molecule, and each of the two naphthalene rings in the two naphthol structures may further have 1 to 3 optional substituents. The substituents here are not particularly limited, but may be the same as those exemplified as the substituents of the benzene ring in the phenylenediamine compound. The two naphthol structures in the bisnaphthol compound may be bonded via a direct bond and / or a divalent linking group having 1 to 100 (preferably 1 to 50, more preferably 1 to 20) skeletal atoms selected from carbon, oxygen, sulfur, and nitrogen atoms.
[0051] Examples of the "divalent linking group" in the bisnaphthol compound include the same as the "divalent linking group" in the dianiline compound.
[0052] Specific examples of the bisnaphthol compound include bis(2-hydroxy-1-naphthyl)methane, 2,2-bis(2-hydroxy-1-naphthyl)propane, and 9,9-bis(6-hydroxy-2-naphthyl)fluorene.
[0053] When the main chain of the (B) siloxane-containing polycarbonate resin has a branched structure, for example, a dihydroxy compound may be converted into a polycarbonate ester together with a branching agent. Examples of the branching agent include trifunctional or higher functional hydroxy compounds, and trifunctional or higher functional aromatic hydroxy compounds are preferred.
[0054] Examples of aromatic hydroxy compounds with three or more functional groups include phloroglucine, phloroglucide, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)-2-heptene, 2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, and 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol.
[0055] The polydiorganosiloxane structure is not particularly limited, but examples thereof include polydialkylsiloxane structures such as a polydimethylsiloxane structure; polydiarylsiloxane structures such as a polydiphenylsiloxane structure; polyalkylarylsiloxane structures such as a polymethylphenylsiloxane structure; polydialkyl-diarylsiloxane structures such as a polydimethyl-diphenylsiloxane structure; polydialkyl-alkylarylsiloxane structures such as a polydimethyl-methylphenylsiloxane structure; and polydiaryl-alkylarylsiloxane structures such as a polydiphenyl-methylphenylsiloxane structure. Of these, a polydialkylsiloxane structure is preferred, and a polydimethylsiloxane structure is particularly preferred.
[0056] The polydiorganosiloxane structure may be, for example, a modified polydiorganosiloxane structure in which a functional group has been introduced into part of the side chain, such as an amino-modified polydiorganosiloxane structure, an epoxy-modified polydiorganosiloxane structure, a carboxy-modified polydiorganosiloxane structure, an acrylic-modified polydiorganosiloxane structure, a methacrylic-modified polydiorganosiloxane structure, a mercapto-modified polydiorganosiloxane structure, or a phenol-modified polydiorganosiloxane structure, but is preferably a non-modified polydiorganosiloxane structure.
[0057] The polysiloxane structure may be contained in the (B) siloxane-containing polycarbonate resin in an amount of preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on 100% by mass of the (B) siloxane-containing polycarbonate resin. The upper limit of the content may be, for example, 30% by mass or less, 25% by mass or less, 20% by mass or less, 15% by mass or less, 10% by mass or less, etc.
[0058] (B) The siloxane-containing polycarbonate resin is preferably a polycarbonate-polysiloxane copolymer in which polysiloxane domains having an average size of 5 to 18 nm are present in a polycarbonate matrix. The average size of the polysiloxane domains is more preferably 5 to 15 nm, even more preferably 5 to 12 nm, and particularly preferably 8 to 12 nm. As a method for evaluating and measuring the average size of the polysiloxane domains, for example, the method described in Japanese Patent No. 6343680 can be used.
[0059] The viscosity average molecular weight of the (B) siloxane-containing polycarbonate resin is not particularly limited, but is preferably 13,000 or more, more preferably 14,000 or more, even more preferably 15,000 or more, and particularly preferably 16,000 or more. The upper limit of the viscosity average molecular weight of the (B) siloxane-containing polycarbonate resin is not particularly limited, but is preferably 25,000 or less, more preferably 23,000 or less, even more preferably 22,000 or less, and particularly preferably 21,000 or less. The method for measuring and calculating the viscosity average molecular weight may be, for example, the method described in Japanese Patent No. 6343680.
[0060] (B) The siloxane-containing polycarbonate resin is, for example, a polycarbonate resin represented by the formula (2):
[0061] [ka]
[0062] [In the formula, R 1each independently represents a halogen atom, an alkyl group, an alkoxy group, an alkylcarbonyl group, an alkoxycarbonyl group, an alkylcarbonyloxy group, an aryl group, an aryloxy group, an arylcarbonyl group, an aryloxycarbonyl group, an arylcarbonyloxy group, an aralkyl group, or a combination thereof. Each Y independently represents a direct bond, or a divalent linking group having 1 to 100 (preferably 1 to 50, more preferably 1 to 20) skeletal atoms selected from carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms. Each a independently represents an integer of 0 to 3. s represents an integer of 1 or more.] and a polycarbonate block represented by formula (3):
[0063] [ka]
[0064] [In the formula, R 2 R each independently represents a halogen atom, an alkyl group, an alkoxy group, an alkylcarbonyl group, an alkoxycarbonyl group, an alkylcarbonyloxy group, an aryl group, an aryloxy group, an arylcarbonyl group, an aryloxycarbonyl group, an arylcarbonyloxy group, an aralkyl group, or a combination thereof. 3 each independently represents a hydrogen atom, an alkyl group, or an aryl group. each Z independently represents an alkylene group. each b independently represents an integer of 0 to 3. u represents an integer of 4 to 150. t represents an integer of 1 or more.] and a polysiloxane block represented by the following formula (1):
[0065] When the (B) siloxane-containing polycarbonate resin is a polycarbonate-polysiloxane copolymer containing a polycarbonate block represented by formula (2) and a polysiloxane block represented by formula (3), the (B) component preferably contains 80 mass % or more of the polycarbonate block represented by formula (2) and the polysiloxane block represented by formula (3) in total, more preferably 85 mass % or more, even more preferably 90 mass % or more, and particularly preferably 95 mass % or more.
[0066] In the above formula (2), examples of the "divalent linking group" represented by Y include the same as the "divalent linking group" in the dianiline compound. Each Y is preferably a direct bond or an alkylene group, more preferably an alkylene group. a is preferably 0 or 1, and particularly preferably 0.
[0067] In the above formula (3), R 3 are each independently preferably an alkyl group or an aryl group, more preferably an alkyl group, and particularly preferably a methyl group. b is preferably 0 or 1, and particularly preferably 0. u is preferably an integer of 4 to 120, more preferably an integer of 30 to 120, still more preferably an integer of 30 to 100, and particularly preferably an integer of 30 to 60.
[0068] The content of the (B) siloxane-containing polycarbonate resin in the resin composition is not particularly limited, but is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, and particularly preferably 7% by mass or more, when the non-volatile components in the resin composition are 100% by mass. The upper limit of the content of the (B) siloxane-containing polycarbonate resin is not particularly limited, but is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less, when the non-volatile components in the resin composition are 100% by mass.
[0069] The mass ratio of the polyimide resin (A) to the siloxane-containing polycarbonate resin (B) (component (A) / component (B)) is not particularly limited, but is preferably 0.1 or more, more preferably 0.5 or more, even more preferably 1 or more, and particularly preferably 1.5 or more. The upper limit of the mass ratio is preferably 20 or less, preferably 10 or less, preferably 5 or less, and preferably 3 or less.
[0070] <(C) Inorganic filler> The resin composition of the present invention may contain an inorganic filler (C) as an optional component. The inorganic filler (C) is contained in the resin composition in the form of particles.
[0071] (C) An inorganic compound is used as the material of the inorganic filler. (C) Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferable as the silica. The (C) inorganic filler may be used alone or in combination of two or more kinds in any ratio.
[0072] (C) Commercially available inorganic fillers include, for example, "UFP-30" manufactured by Denka Chemical Industry Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumitomo Metal Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd.; "UFP-30" manufactured by Denka Company; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; and "DAW-03" and "FB-105FD" manufactured by Denka Company, Ltd.
[0073] The average particle size of the (C) inorganic filler is not particularly limited, but is preferably 40 μm or less, more preferably 10 μm or less, even more preferably 5 μm or less, even more preferably 3 μm or less, and particularly preferably 1 μm or less. The lower limit of the average particle size of the (C) inorganic filler is not particularly limited, but is preferably 0.005 μm or more, more preferably 0.01 μm or more, even more preferably 0.05 μm or more, even more preferably 0.1 μm or more, even more preferably 0.3 μm or more, and particularly preferably 0.4 μm or more. The average particle size of the (C) inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering type particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0074] The specific surface area of the (C) inorganic filler is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m2 / g or more, more preferably 1m 2 / g or more, particularly preferably 5m 2 The upper limit of the specific surface area of the inorganic filler (C) is not particularly limited, but is preferably 50 m 2 / g or less, more preferably 30m 2 / g or less, more preferably 20m 2 / g or less, particularly preferably 15m 2 The specific surface area of the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.
[0075] The inorganic filler (C) is preferably surface-treated with an appropriate surface treatment agent, which can enhance the moisture resistance and dispersibility of the inorganic filler (C). Examples of the surface treatment agent include vinyl-based silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane; epoxy-based silane coupling agents such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane; styryl-based silane coupling agents such as p-styryltrimethoxysilane; methacryl-based silane coupling agents such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-methacryloxypropyltriethoxysilane; acrylic-based silane coupling agents such as 3-acryloxypropyltrimethoxysilane; N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, and N-2-(aminoethyl)-3-aminopropyltriethoxysilane; Amino-based silane coupling agents such as trimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-8-aminooctyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane; isocyanurate-based silane coupling agents such as tris-(trimethoxysilylpropyl)isocyanurate; ureido-based silane coupling agents such as 3-ureidopropyltrialkoxysilane; mercapto-based silane coupling agents such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; isocyanate-based silane coupling agents such as 3-isocyanatepropyltriethoxysilane; acid anhydride-based silane coupling agents such as 3-trimethoxysilylpropylsuccinic anhydride; and other silane coupling agents;Examples of the non-silane coupling alkoxysilane compounds include methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, 1,6-bis(trimethoxysilyl)hexane, and trifluoropropyltrimethoxysilane. Among these, amino-based silane coupling agents are preferred. The surface treatment agent may be used alone or in combination of two or more in any ratio.;
[0076] Commercially available surface treatment agents include, for example, "KBM-1003" and "KBE-1003" (vinyl-based silane coupling agents) manufactured by Shin-Etsu Chemical Co., Ltd.; "KBM-303", "KBM-402", "KBM-403", "KBE-402", and "KBE-403" (epoxy-based silane coupling agents); "KBM-1403" (styryl-based silane coupling agents); "KBM-502", "KBM-503", "KBE-502", and "KBE-503" (methacrylic-based silane coupling agents); "KBM-5103" (acrylic-based silane coupling agents); "KBM-602", "KBM-603", "KBM-903", "KBE-903", "KBE-9103P", "KBM-573", and "KBM-575" (amino-based silane coupling agents); Examples include "KBM-9659" (isocyanurate-based silane coupling agent); "KBE-585" (ureido-based silane coupling agent); "KBM-802", "KBM-803" (mercapto-based silane coupling agent); "KBE-9007N" (isocyanate-based silane coupling agent); "X-12-967C" (acid anhydride-based silane coupling agent); "KBM-13", "KBM-22", "KBM-103", "KBE-13", "KBE-22", "KBE-103", "KBM-3033", "KBE-3033", "KBM-3063", "KBE-3063", "KBE-3083", "KBM-3103C", "KBM-3066", and "KBM-7103" (non-silane coupling alkoxysilane compound).
[0077] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a predetermined range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably 0.2% to 3% by mass, and even more preferably 0.3% to 2% by mass.
[0078] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition or the melt viscosity in the form of a sheet, it is more preferable that the melt viscosity is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:
[0079] (C) The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.
[0080] When the resin composition contains an inorganic filler (C), the content of the inorganic filler (C) in the resin composition is not particularly limited, but is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 40% by mass or more, when the non-volatile components in the resin composition are 100% by mass. The upper limit of the content of the inorganic filler (C) is not particularly limited, but is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 60% by mass or less, and particularly preferably 50% by mass or less, when the non-volatile components in the resin composition are 100% by mass.
[0081] <(D) Epoxy resin> The resin composition of the present invention may contain an optional component (D) epoxy resin. (D) Epoxy resin means a resin having an epoxy group.
[0082] Examples of the (D) epoxy resin include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, cresol novolac type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, isocyanurate type epoxy resin, and the like. Among them, cyclohexane type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, and bisphenol AF type epoxy resins are particularly preferred. (D) The epoxy resins may be used alone or in combination of two or more.
[0083] The resin composition preferably contains, as the (D) epoxy resin, an epoxy resin having two or more epoxy groups in one molecule. The proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the non-volatile components of the (D) epoxy resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.
[0084] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition of the present invention may contain only a liquid epoxy resin or only a solid epoxy resin as the epoxy resin, but it is preferable that the resin composition contains a combination of a liquid epoxy resin and a solid epoxy resin.
[0085] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0086] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, and epoxy resin having a butadiene structure are preferred, and among these, cyclohexane type epoxy resin is particularly preferred.
[0087] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", and "604" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol type epoxy resin) manufactured by ADEKA Corporation; and "EP-3950L" manufactured by ADEKA Corporation. Examples of such epoxy resins include "EP-3980S" (glycidylamine type epoxy resin); "EP-4088S" (dicyclopentadiene type epoxy resin) manufactured by ADEKA; "ZX1059" (mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase Chemtex; "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel; "PB-3600" manufactured by Daicel, "JP-100" and "JP-200" (epoxy resin having a butadiene structure) manufactured by Nippon Steel & Sumitomo Metal Chemical; and "ZX1658" and "ZX1658GS" (cyclohexane type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical. These may be used alone or in combination of two or more types.
[0088] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.
[0089] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and among these, naphthol type epoxy resin, biphenyl type epoxy resin, and bisphenol AF type epoxy resin are particularly preferred.
[0090] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", and "HP-7200H" (dicyclopentadiene type epoxy resin) manufactured by DIC Corporation; EXA-7311, EXA-7311-G3, EXA-7311-G4, EXA-7311-G4S, HP6000 (naphthylene ether type epoxy resin); EPPN-502H (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; NC7000L (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; NC3000H, NC3000, NC3000L, NC3000FH, NC3100 (biphenyl type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN485" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YL6121", "YL7890", "YX4000HK" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd. Examples of such epoxy resins include "YX7700" (xylene structure-containing novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation, "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals Co., Ltd., "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Corporation, "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Corporation, "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical Corporation, and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Corporation. These may be used alone or in combination of two or more types.
[0091] When a liquid epoxy resin and a solid epoxy resin are used in combination as the (D) epoxy resin, the mass ratio thereof (liquid epoxy resin:solid epoxy resin) is preferably in the range of 100:1 to 1:100, more preferably in the range of 20:1 to 1:50, and even more preferably in the range of 1:1 to 1:30.
[0092] The epoxy equivalent of the (D) epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 70 g / eq. to 2,000 g / eq., even more preferably 90 g / eq. to 1,000 g / eq., and even more preferably 100 g / eq. to 400 g / eq. The epoxy equivalent is the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.
[0093] The weight average molecular weight (Mw) of the epoxy resin (D) is preferably from 100 to 5,000, more preferably from 250 to 3,000, and further preferably from 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.
[0094] When the resin composition contains the epoxy resin (D), the content of the epoxy resin (D) in the resin composition is not particularly limited, but is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more, when the non-volatile components in the resin composition are taken as 100% by mass. The upper limit of the content of the epoxy resin (D) is not particularly limited, but is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 25% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass.
[0095] <(E) Hardener> When the resin composition of the present invention contains an epoxy resin (D), it may contain a curing agent (E) having a function of curing the epoxy resin (D).
[0096] The (E) curing agent is not particularly limited, but examples thereof include phenol-based curing agents, naphthol-based curing agents, acid anhydride-based curing agents, active ester-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, and carbodiimide-based curing agents. The curing agents may be used alone or in combination of two or more. It is particularly preferable that the (E) curing agent contains an active ester-based curing agent.
[0097] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferred. Also, from the viewpoint of adhesion to the adherend, a nitrogen-containing phenol-based curing agent or a nitrogen-containing naphthol-based curing agent is preferred, and a triazine skeleton-containing phenol-based curing agent or a triazine skeleton-containing naphthol-based curing agent is more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, a triazine skeleton-containing phenol novolac resin is preferred. Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", "TD2090", and "TD-2090-60M" manufactured by DIC Corporation.
[0098] Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule, and a curing agent having two or more acid anhydride groups in one molecule is preferable. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, and the like. Examples of acid anhydrides include polymeric acid anhydrides such as anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and styrene-maleic acid resins, which are copolymers of styrene and maleic acid. Commercially available acid anhydride hardeners include "HNA-100" and "MH-700" manufactured by New Japan Chemical Co., Ltd.
[0099] The active ester curing agent is not particularly limited, but generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.
[0100] Specifically, active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing an acetylated product of phenol novolac, and active ester compounds containing a benzoylated product of phenol novolac are preferred, and among these, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentalene-phenylene.
[0101] Commercially available active ester curing agents include "EXB9451", "EXB9460", "EXB9460S", "HPC-8000", "HPC-8000H", "HPC-8000-65T", "HPC-8000H-65TM", "EXB-8000L", "EXB-8000L-65M", and "EXB-8000L-65TM" (manufactured by DIC Corporation) as active ester compounds containing a dicyclopentadiene-type diphenol structure; and "EXB -9416-70BK", "EXB-8150-65T", "EXB-8100L-65T", "EXB-8150L-65T" (manufactured by DIC Corporation); as an active ester type curing agent which is an acetylated product of phenol novolac, "DC808" (manufactured by Mitsubishi Chemical Corporation); as active ester type curing agents which are benzoylated products of phenol novolac, "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), "YLH1048" (manufactured by Mitsubishi Chemical Corporation); and the like.
[0102] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0103] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.
[0104] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.
[0105] When the resin composition contains a curing agent (E), the ratio of the amount of the epoxy resin (D) to the curing agent (E) is preferably 1:0.2 to 1:2, more preferably 1:0.3 to 1:1.5, and even more preferably 1:0.4 to 1:1.4, in terms of the ratio of [the number of epoxy groups in the epoxy resin (D)] to [the number of reactive groups in the curing agent (E)]. Here, the reactive groups of the curing agent (E) vary depending on the type of curing agent, for example, aromatic hydroxyl groups for phenol-based curing agents and naphthol-based curing agents, and active ester groups for active ester-based curing agents.
[0106] The reactive group equivalent of the (E) curing agent is preferably 50 g / eq. to 3,000 g / eq., more preferably 100 g / eq. to 1,000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The reactive group equivalent is the mass of the curing agent per equivalent of reactive group.
[0107] When the (E) curing agent contains an active ester curing agent, its content is not particularly limited, but is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 40% by mass or more, when the total amount of the (E) curing agent is 100% by mass.
[0108] When the resin composition contains a (E) curing agent, the content of the (E) curing agent in the resin composition is not particularly limited, but is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and particularly preferably 5% by mass or more, when the non-volatile components in the resin composition are 100% by mass. The upper limit of the content of the (E) curing agent is not particularly limited, but is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less, when the non-volatile components in the resin composition are 100% by mass.
[0109] <(F) Curing accelerator> When the resin composition of the present invention contains the epoxy resin (D), it may contain, as an optional component, a curing accelerator (F) that has the function of accelerating the curing of the epoxy resin (D).
[0110] (F) The curing accelerator is not particularly limited, but examples thereof include phosphorus-based curing accelerators, urea-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. Among these, phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are preferred, and amine-based curing accelerators are particularly preferred. The curing accelerator may be used alone or in combination of two or more types.
[0111] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutyl phosphonium bromide, tetrabutyl phosphonium chloride, tetrabutyl phosphonium acetate, tetrabutyl phosphonium decanoate, tetrabutyl phosphonium laurate, bis(tetrabutyl phosphonium)pyromellitate, tetrabutyl phosphonium hydrogen hexahydrophthalate, tetrabutyl phosphonium cresol novolac trimer salt, and di-tert-butylmethyl phosphonium tetraphenylborate; methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide, propyl triphenyl phosphonium bromide, butyl triphenyl phosphonium bromide, benzyl triphenyl phosphonium chloride, tetraphenyl phosphonium bromide, p-tolyl triphenyl phosphonium tetra-p-tolyl borate, and tetraphenyl phosphonium tetraphenyl borate. aromatic phosphonium salts such as tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of aromatic phosphines include tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.
[0112] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as butylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].
[0113] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine (DMAP), benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine being preferred.
[0114] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct imidazole compounds such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins.
[0115] As the imidazole-based curing accelerator, a commercially available product may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0116] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.
[0117] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0118] When the resin composition contains a (F) curing accelerator, the content of the (F) curing accelerator in the resin composition is not particularly limited, but is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more, when the non-volatile components in the resin composition are 100% by mass. The upper limit of the content of the (F) curing accelerator is not particularly limited, but is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and particularly preferably 0.3% by mass or less, when the non-volatile components in the resin composition are 100% by mass.
[0119] <(G) Other Additives> The resin composition of the present invention may further contain any additive as a non-volatile component. Examples of such additives include organic fillers such as rubber particles, polyamide fine particles, and silicone particles; thermoplastic resins such as polycarbonate resins, phenoxy resins, polyvinyl acetal resins, polyolefin resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polyetheretherketone resins, and polyester resins other than the component (B); organic metal compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; bentone. , thickeners such as montmorillonite; defoamers such as silicone defoamers, acrylic defoamers, fluorine defoamers, and vinyl resin defoamers; ultraviolet absorbers such as benzotriazole ultraviolet absorbers; adhesion improvers such as urea silane; adhesion imparters such as triazole adhesion imparters, tetrazole adhesion imparters, and triazine adhesion imparters; antioxidants such as hindered phenol antioxidants and hindered amine antioxidants; fluorescent brighteners such as stilbene derivatives; surfactants such as fluorine surfactants and silicone surfactants; flame retardants other than non-reactive phosphazene compounds such as phosphorus flame retardants (e.g., phosphoric acid ester compounds, phosphazene compounds, phosphinic acid compounds, and red phosphorus), nitrogen flame retardants (e.g., melamine sulfate), halogen flame retardants, and inorganic flame retardants (e.g., antimony trioxide). The additives may be used alone or in combination of two or more in any ratio. (G) The content of other additives can be appropriately set by those skilled in the art.
[0120] <(H) Organic Solvent> The resin composition of the present invention may further contain an arbitrary organic solvent as a volatile component in addition to the non-volatile components described above. As the (H) organic solvent, a known one may be appropriately used, and the type is not particularly limited. As the (H) organic solvent, for example, ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, etc.; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, etc.; alcohol-based solvents such as methanol, ethanol, propanol, butanol, ethylene glycol, etc.; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, methyl methoxypropionate, etc. Examples of the organic solvent include ether ester solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent (H) may be used alone or in combination of two or more in any ratio.
[0121] <Method of producing resin composition> The resin composition of the present invention can be produced, for example, by adding (A) polyimide resin (previously imidized), (B) siloxane-containing polycarbonate resin (previously carbonated), if necessary (C) inorganic filler, if necessary (D) epoxy resin, if necessary (E) curing agent, if necessary (F) curing accelerator, if necessary (G) other additives, if necessary, and if necessary (H) organic solvent in any order and / or all at once and mixing them in any reaction vessel. In addition, the temperature can be appropriately set during the process of adding and mixing each component, and heating and / or cooling may be performed temporarily or throughout. In addition, stirring or shaking may be performed during the process of adding and mixing each component. In addition, the resin composition may be stirred using a stirring device such as a mixer during or after adding and mixing to disperse uniformly.
[0122] <Characteristics of resin composition> The resin composition of the present invention contains (A) a polyimide resin and (B) a siloxane-containing polycarbonate resin, and therefore can provide a cured product with a low coefficient of thermal expansion and reduced warping. In addition, the compatibility of each component can be excellent.
[0123] The cured product of the resin composition of the present invention has a low coefficient of thermal expansion, and therefore, for example, the linear thermal expansion coefficient (ppm) of the cured product obtained by curing the resin composition under curing conditions of 190°C for 90 minutes from 25°C to 150°C at a heating rate of 5°C / min can be preferably less than 80 ppm, more preferably less than 70 ppm, even more preferably less than 65 ppm, still more preferably less than 62 ppm, and particularly preferably less than 60 ppm.
[0124] Since warping is suppressed in the cured product of the resin composition of the present invention, for example, when a cured product having a width of 160 mm and a length of 120 mm obtained by curing the resin composition under curing conditions of 190°C for 90 minutes is fixed at three points and the warping at the remaining point is measured, the amount of warping can be preferably less than 30 mm, more preferably less than 25 mm, even more preferably less than 20 mm, and particularly preferably less than 17 mm.
[0125] Since the resin composition of the present invention can have excellent compatibility, for example, even if the resin composition is stored in a refrigerator at 5°C for 3 days and then observed under an optical microscope, preferably no separated matter is observed.
[0126] <Applications of resin composition> The resin composition of the present invention can be used in a wide range of applications, such as insulating materials for printed wiring boards and multilayer flexible substrates, solder resists, underfill materials, die bonding materials, semiconductor encapsulants, hole filling resins, component embedding resins, etc. Printed wiring boards, multilayer flexible substrates, etc. can be produced using sheet-like laminate materials such as resin sheets and prepregs, for example.
[0127] <Resin sheet> The resin sheet of the present invention includes a support and a resin composition layer formed from the resin composition of the present invention provided on the support.
[0128] The thickness of the resin composition layer is preferably 200 μm or less, more preferably 150 μm or less, further preferably 100 μm or less, and particularly preferably 70 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 1 μm or more, 1.5 μm or more, 2 μm or more, etc.
[0129] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0130] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0131] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0132] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.
[0133] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0134] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.
[0135] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.
[0136] The resin sheet can be produced by applying the resin composition as is, or a resin varnish prepared by dissolving the resin composition in an organic solvent, onto a support using a die coater or the like, and then drying to form a resin composition layer.
[0137] Examples of organic solvents that can be used when applying the resin composition onto a support include the same organic solvents as those described above as components of the resin composition. The organic solvents may be used alone or in combination of two or more.
[0138] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the organic solvent in the resin composition layer becomes 10 mass% or less, preferably 5 mass% or less. Although it varies depending on the boiling point of the organic solvent in the resin composition or resin varnish, for example, when a resin composition or resin varnish containing 30 mass% to 60 mass% of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0139] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0140] <Laminated sheet> The laminate sheet is a sheet produced by laminating and curing a plurality of resin composition layers. The laminate sheet includes a plurality of insulating layers as cured products of the resin composition layers. Usually, the number of resin composition layers laminated to produce the laminate sheet corresponds to the number of insulating layers contained in the laminate sheet. The specific number of insulating layers per laminate sheet is usually 2 or more, preferably 3 or more, particularly preferably 5 or more, and preferably 20 or less, more preferably 15 or less, particularly preferably 10 or less.
[0141] The laminate sheet is a sheet that is folded so that one side of the laminate sheet faces the other when used. The minimum bending radius of the laminate sheet is not particularly limited, but is preferably 0.1 mm or more, more preferably 0.2 mm or more, and even more preferably 0.3 mm or more, and is preferably 5 mm or less, more preferably 4 mm or less, and particularly preferably 3 mm or less.
[0142] Each insulating layer included in the laminated sheet may have a hole formed therein, which can function as a via hole or a through hole in the multi-layer flexible substrate.
[0143] The laminate sheet may further include an optional element in addition to the insulating layer. For example, the laminate sheet may include a conductor layer as an optional element. The conductor layer is usually partially formed on the surface of the insulating layer or between the insulating layers. This conductor layer usually functions as wiring in the multilayer flexible substrate.
[0144] The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor material may be a single metal or an alloy. Examples of the alloy include alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among them, from the viewpoints of versatility of conductor layer formation, cost, ease of patterning, etc., single metals such as chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper; and alloys such as nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy; are preferred. Among them, single metals such as chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper; and nickel-chromium alloy; are more preferred, and single metal copper is even more preferred.
[0145] The conductor layer may be a single-layer structure or a multi-layer structure including two or more single metal layers or alloy layers made of different kinds of metals or alloys. When the conductor layer is a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0146] The conductor layer may be patterned to function as wiring.
[0147] The thickness of the conductor layer depends on the design of the multilayer flexible board, but is preferably 3 μm to 35 μm, more preferably 5 μm to 30 μm, further preferably 10 μm to 20 μm, and particularly preferably 15 μm to 20 μm.
[0148] The thickness of the laminate sheet is preferably 100 μm or more, more preferably 150 μm or more, particularly preferably 200 μm or more, and is preferably 2,000 μm or less, more preferably 1,000 μm or less, particularly preferably 500 μm or less.
[0149] <Method of manufacturing laminated sheet> The laminated sheet can be manufactured by a manufacturing method including the steps of (a) preparing a resin sheet, and (b) laminating and curing a plurality of resin composition layers using the resin sheet. The order of laminating and curing the resin composition layers is arbitrary as long as a desired laminated sheet is obtained. Depending on the components contained in the resin composition, for example, after laminating all of the plurality of resin composition layers, the laminated plurality of resin composition layers may be cured all at once. In addition, for example, each time a certain resin composition layer is laminated on another resin composition layer, the laminated resin composition layer may be cured.
[0150] A preferred embodiment of step (b) will be described below. In the embodiment described below, for the purpose of distinction, the resin composition layers are appropriately numbered and shown as "first resin composition layer" and "second resin composition layer", and the insulating layers obtained by curing these resin composition layers are also numbered and shown as "first insulating layer" and "second insulating layer" in the same manner as the resin composition layers.
[0151] In a preferred embodiment, step (b) comprises: (II) curing the first resin composition layer to form a first insulating layer; (VI) laminating a second resin composition layer on the first insulating layer; (VII) curing the second resin composition layer to form a second insulating layer; Step (b) may further include, as necessary: (I) laminating a first resin composition layer onto a sheet supporting substrate; (III) drilling holes in the first insulating layer; (IV) subjecting the first insulating layer to a roughening treatment; (V) forming a conductor layer on the first insulating layer Each step will be described below.
[0152] Step (I) is a step of laminating a first resin composition layer onto a sheet supporting substrate prior to step (II). The sheet supporting substrate is a peelable member, and for example, a plate-, sheet- or film-shaped member is used.
[0153] The lamination of the sheet support substrate and the first resin composition layer may be performed by a vacuum lamination method. In the vacuum lamination method, the heat-pressure bonding temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the heat-pressure bonding pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the heat-pressure bonding time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.
[0154] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0155] When a resin sheet is used, the lamination of the sheet support substrate and the first resin composition layer can be performed, for example, by pressing the resin sheet from the support side and thermocompressing the first resin composition layer of the resin sheet to the sheet support substrate. Examples of the member for thermocompressing the resin sheet to the sheet support substrate (hereinafter, also referred to as "thermocompression member") include a heated metal plate (SUS mirror plate, etc.) or a metal roll (SUS roll), etc. It is preferable to press the thermocompression member through an elastic material such as heat-resistant rubber so that the first resin composition layer sufficiently follows the surface irregularities of the sheet support substrate, rather than directly pressing the resin sheet with the thermocompression member.
[0156] After lamination, the first resin composition layer may be smoothed by pressing, for example, with a heat-pressure bonding member under normal pressure (atmospheric pressure). For example, when a resin sheet is used, the first resin composition layer of the resin sheet can be smoothed by pressing the resin sheet from the support side with a heat-pressure bonding member. The pressing conditions for the smoothing treatment can be the same as the heat-pressure bonding conditions for the lamination. The smoothing treatment can be performed with a commercially available laminator. The lamination and the smoothing treatment may be performed continuously using the commercially available vacuum laminator.
[0157] Step (II) is a step of curing the first resin composition layer to form a first insulating layer. The curing conditions of the first resin composition layer are not particularly limited, and the conditions adopted when forming an insulating layer of a printed wiring board can be applied arbitrarily. The first resin composition layer can be cured by drying, but when it contains a thermosetting resin such as an epoxy resin, it can be cured by drying and then thermally curing.
[0158] Usually, when an epoxy resin is contained, specific heat curing conditions vary depending on the type of resin composition. For example, the curing temperature is preferably 120°C to 240°C, more preferably 150°C to 220°C, and even more preferably 170°C to 210°C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 110 minutes, and even more preferably 20 minutes to 100 minutes.
[0159] When the first resin composition layer contains an epoxy resin, the first resin composition layer may be preheated at a temperature lower than the curing temperature before being thermally cured. For example, the first resin composition layer may be preheated for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes) at a temperature of 50°C or more and less than 120°C (preferably 60°C or more and 115°C or less, and more preferably 70°C or more and 110°C or less) before being thermally cured.
[0160] Step (III) is a step of drilling holes in the first insulating layer. This step (III) allows holes such as via holes and through holes to be formed in the first insulating layer. The holes may be drilled using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition. The dimensions and shape of the holes may be appropriately set depending on the design of the multilayer flexible substrate.
[0161] Step (IV) is a step of performing a roughening treatment on the first insulating layer. Usually, in this step (IV), smears are also removed. Therefore, the roughening treatment is sometimes called a desmear treatment. An example of the roughening treatment is a method in which a swelling treatment using a swelling liquid, a roughening treatment using an oxidizing agent, and a neutralization treatment using a neutralizing liquid are performed in this order.
[0162] The swelling liquid is not particularly limited, and examples thereof include alkaline aqueous solutions such as an aqueous sodium hydroxide solution and an aqueous potassium hydroxide solution. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using the swelling liquid can be carried out, for example, by immersing the cured body in the swelling liquid at 30 to 90°C for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in the swelling liquid at 40 to 80°C for 5 to 15 minutes.
[0163] The oxidizing agent is not particularly limited, but examples thereof include an alkaline permanganate solution in which a permanganate is dissolved in an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution. The concentration of the permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact P", "Concentrate Compact CP", and "Dosing Solution Securigans P" manufactured by Atotech Japan. The roughening treatment using an oxidizing agent can be performed by immersing the cured body in an oxidizing agent solution heated to 60°C to 80°C for 10 minutes to 30 minutes.
[0164] An acidic aqueous solution is used as the neutralizing liquid. An example of a commercially available product is "Reduction Solution Securigant P" manufactured by Atotech Japan. The treatment with the neutralizing liquid can be carried out by immersing the hardened body in the neutralizing liquid at 30°C to 80°C for 5 to 30 minutes. From the viewpoint of workability, etc., it is preferable to immerse the hardened body in the neutralizing liquid at 40°C to 70°C for 5 to 20 minutes.
[0165] The arithmetic mean roughness (Ra) of the surface of the first insulating layer after the roughening treatment is preferably 400 nm or less, more preferably 300 nm or less, and even more preferably 200 nm or less. The lower limit is not particularly limited, but may be 30 nm or more, 40 nm or more, or 50 nm or more.
[0166] Step (V) is a step of forming a conductor layer on the first insulating layer as necessary. The conductor layer can be formed by, for example, plating, sputtering, vapor deposition, etc., among which plating is preferred. A suitable example is a method of plating the surface of the first insulating layer by an appropriate method such as a semi-additive method or a full-additive method to form a conductor layer having a desired wiring pattern. Among these, the semi-additive method is preferred from the viewpoint of ease of production.
[0167] An example of forming a conductor layer by a semi-additive method is shown below. First, a plating seed layer is formed on the surface of a first insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by a process such as etching to form a conductor layer having a desired wiring pattern.
[0168] A first insulating layer is obtained in step (II), and step (III), step (IV), and step (V) are performed as necessary, followed by step (VI). Step (VI) is a step of laminating a second resin composition layer on the first insulating layer. The lamination of the first insulating layer and the second resin composition layer can be performed in the same manner as the lamination of the sheet support substrate and the first resin composition layer in step (I).
[0169] However, when the first resin composition layer is formed using a resin sheet, the support of the resin sheet is removed prior to step (VI). The removal of the support may be performed between step (I) and step (II), between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V).
[0170] After step (VI), step (VII) is performed. Step (VII) is a step of curing the second resin composition layer to form a second insulating layer. The second resin composition layer can be cured by the same method as the curing of the first resin composition layer in step (II). This makes it possible to obtain a laminate sheet including a plurality of insulating layers, namely, a first insulating layer and a second insulating layer.
[0171] In addition, in the method according to the embodiment, the steps of (VIII) drilling holes in the second insulating layer, (IX) roughening the second insulating layer, and (X) forming a conductor layer on the second insulating layer may be performed as necessary. The drilling of the second insulating layer in step (VIII) can be performed in the same manner as the drilling of the first insulating layer in step (III). The roughening of the second insulating layer in step (IX) can be performed in the same manner as the roughening of the first insulating layer in step (IV). Furthermore, the formation of the conductor layer on the second insulating layer in step (X) can be performed in the same manner as the formation of the conductor layer on the first insulating layer in step (V).
[0172] In the above embodiment, the laminate sheet is produced by laminating and curing two resin composition layers, namely, the first resin composition layer and the second resin composition layer, but the laminate sheet may be produced by laminating and curing three or more resin composition layers. For example, in the method according to the above embodiment, the lamination and curing of the resin composition layers in steps (VI) to (VII), and, if necessary, the drilling of the insulating layer, the roughening treatment of the insulating layer, and the formation of a conductor layer on the insulating layer in steps (VIII) to (X) may be repeatedly carried out to produce a laminate sheet. This provides a laminate sheet including three or more insulating layers.
[0173] Furthermore, the method according to the embodiment may include any step other than the steps described above. For example, when step (I) is performed, a step of removing the sheet support substrate may be performed.
[0174] <Multi-layer flexible circuit board> The multilayer flexible substrate includes a laminate sheet. The multilayer flexible substrate may include only the laminate sheet, or may include an optional member in combination with the laminate sheet. Examples of the optional member include electronic components and coverlay films.
[0175] The multilayer flexible substrate can be manufactured by a manufacturing method including the above-mentioned method for manufacturing a laminate sheet. Thus, the multilayer flexible substrate can be manufactured by a manufacturing method including the steps of (a) preparing a resin sheet, and (b) laminating and curing a plurality of resin composition layers using the resin sheet.
[0176] The method for manufacturing a multilayer flexible substrate may further include any step in combination with the above steps. For example, the method for manufacturing a multilayer flexible substrate including an electronic component may include a step of bonding the electronic component to a laminate sheet. The bonding conditions between the laminate sheet and the electronic component may be any condition that allows a conductive connection between the terminal electrodes of the electronic component and the conductor layer as wiring provided on the laminate sheet. Also, for example, the method for manufacturing a multilayer flexible substrate including a coverlay film may include a step of laminating the laminate sheet and the coverlay film.
[0177] The multilayer flexible substrate can be used by usually folding the laminated sheets contained in the multilayer flexible substrate so that one side of the laminated sheets faces each other. For example, the multilayer flexible substrate is stored in a housing of a semiconductor device in a folded and reduced size state. Also, for example, the multilayer flexible substrate is provided on a movable part of a semiconductor device having a foldable movable part.
[0178] <Semiconductor device> The semiconductor device includes the multilayer flexible substrate. The semiconductor device includes, for example, a multilayer flexible substrate and a semiconductor chip mounted on the multilayer flexible substrate. In many semiconductor devices, the multilayer flexible substrate can be stored in the housing of the semiconductor device by folding the multilayer flexible substrate so that one side of the laminated sheets included in the multilayer flexible substrate faces each other.
[0179] Examples of the semiconductor device include various semiconductor devices used in electrical appliances (such as computers, mobile phones, digital cameras, and televisions) and vehicles (such as motorcycles, automobiles, trains, ships, and aircraft).
[0180] The semiconductor device can be manufactured by a manufacturing method including, for example, a step of preparing a multilayer flexible substrate, a step of folding the multilayer flexible substrate so that one side of the laminated sheet faces each other, and a step of storing the folded multilayer flexible substrate in a housing. EXAMPLES
[0181] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0182] <Synthesis Example 1: Synthesis of Polyimide Resin 1> In a 500 ml separable flask equipped with a nitrogen inlet tube and a stirrer, 9.13 g (30 mmol) of 5-amino-1,1'-biphenyl-2-yl 4-aminobenzoate, 15.61 g (30 mmol) of 4,4'-(4,4'-isopropylidenediphenoxy)bisphthalic dianhydride, 94.64 g of N-methyl-2-pyrrolidone, 0.47 g (6 mmol) of pyridine, and 10 g of toluene were added, and the mixture was subjected to an imidization reaction under a nitrogen atmosphere at 180°C for 4 hours while removing the toluene from the system during the reaction, to obtain a polyimide solution (non-volatile content 20% by mass) containing polyimide resin 1. No precipitation of the synthesized polyimide resin 1 was observed in the polyimide solution.
[0183] <Synthesis Example 2: Synthesis of Polyimide Resin 2> A reaction vessel equipped with a stirrer, a water divider, a thermometer, and a nitrogen gas inlet tube was charged with 65.0 g of aromatic tetracarboxylic dianhydride (SABIC Japan "BisDA-1000", 4,4'-(4,4'-isopropylidenediphenoxy)bisphthalic dianhydride), 266.5 g of cyclohexanone, and 44.4 g of methylcyclohexane, and the solution was heated to 60 ° C. Next, 43.7 g of dimer diamine (Croda Japan "PRIAMINE 1075") and 5.4 g of 1,3-bis(aminomethyl)cyclohexane were dropped, and then the imidization reaction was carried out at 140 ° C. for 1 hour. As a result, a polyimide solution (non-volatile content 30% by mass) containing polyimide resin 2 was obtained. The weight average molecular weight of polyimide resin 2 was 25,000.
[0184] <Synthesis Example 3: Synthesis of polyimide resin 3> A 500 mL separable flask equipped with a water content receiver connected to a reflux condenser, a nitrogen inlet tube, and a stirrer was prepared. 20.3 g of 4,4'-oxydiphthalic anhydride (ODPA), 200 g of γ-butyrolactone, 20 g of toluene, and 29.6 g of 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane were added to this flask, and the mixture was stirred at 45°C for 2 hours under a nitrogen stream to carry out a reaction. Next, the reaction solution was heated and, while maintaining the temperature at about 160°C, condensed water was azeotropically removed together with toluene under a nitrogen stream. It was confirmed that a predetermined amount of water had accumulated in the water content receiver and that no water was flowing out. After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. The mixture was then cooled to obtain a polyimide solution (non-volatile content 20% by mass) containing polyimide resin 3 having a 1,1,3-trimethylindane skeleton. The obtained polyimide resin 3 had a repeating unit represented by the following formula (X1) and a repeating unit represented by the following formula (X2). The weight average molecular weight of the polyimide resin 3 was 12,000.
[0185] [ka]
[0186] [ka]
[0187] <Synthesis Example 4: Synthesis of polycarbonate-polydimethylsiloxane copolymer resin> A reactor equipped with a thermometer, a stirrer, and a reflux condenser was charged with 21,591 parts of ion-exchanged water and 3,674 parts of 48.5% aqueous sodium hydroxide solution, and 3,880 parts of 2,2-bis(4-hydroxyphenyl)propane (bisphenol A) and 7.6 parts of hydrosulfite were dissolved therein. Then, 14,565 parts of methylene chloride was added, and 1,900 parts of phosgene was blown in over 60 minutes at 22 to 30° C. with stirring. Next, add 1131 parts of 48.5% sodium hydroxide aqueous solution and 105 parts of p-tert-butylphenol dissolved in 800 parts of methylene chloride, and while stirring, add 430 parts of di-o-hydroxyphenyl-terminated polydimethylsiloxane compound (average repeat number p in the formula = about 37) represented by the following formula (4) dissolved in 1600 parts of methylene chloride at a rate of 0.0008 moles / minute per mole of 2,2-bis(4-hydroxyphenyl)propane to emulsify, then stir vigorously again. Under such stirring, add 4.3 parts of triethylamine when the reaction liquid is at 26°C, and continue stirring at a temperature of 26 to 31°C for 45 minutes to complete the reaction. After the reaction was completed, the organic phase was separated, diluted with methylene chloride, washed with water, and then acidified with hydrochloric acid and washed with water. When the conductivity of the aqueous phase was almost the same as that of ion-exchanged water, it was put into a kneader filled with warm water and the methylene chloride was evaporated while stirring to obtain a polycarbonate-polydimethylsiloxane copolymer resin powder. After dehydration, it was dried for 12 hours at 120°C in a hot air circulation dryer to obtain a polycarbonate-polydimethylsiloxane copolymer resin powder (polydimethylsiloxane structure content 8.2%, average size of polydimethylsiloxane domain 9nm, viscosity average molecular weight 19,400).
[0188] [ka]
[0189] <Example 1: Preparation of resin composition 1> A mixture of 5 parts of a bixylenol type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: about 185), 5 parts of a naphthalene type epoxy resin ("ESN475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., epoxy equivalent: about 332), 10 parts of a bisphenol AF type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: about 238), 2 parts of a cyclohexane type epoxy resin ("ZX1658GS" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: about 135), 100 parts of the polyimide solution (non-volatile component: 20% by mass) obtained in Synthesis Example 1, and 10 parts of cyclohexanone was heated and dissolved with stirring. After cooling to room temperature, 50 parts of the polycarbonate-polydimethylsiloxane copolymer resin obtained in Synthesis Example 4 (20% by mass of non-volatile components, toluene solution), 4 parts of a triazine skeleton-containing cresol novolak-based curing agent ("LA3018-50P" manufactured by DIC Corporation, hydroxyl group equivalent of about 151, 2-methoxypropanol solution with solid content of 50%), 6 parts of an active ester-based curing agent ("EXB-8000L-65M" manufactured by DIC Corporation, active group equivalent of about 220, 1:1 solution of toluene:MEK with non-volatile components of 65% by mass), and spherical silica ("SC2500SQ" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm, specific surface area 11.2 m) were added thereto. 2 Resin composition 1 was prepared by mixing 50 parts of N-phenyl-3-aminopropyltrimethoxysilane (surface-treated with 1 part of KBM573, manufactured by Shin-Etsu Chemical Co., Ltd.) and 0.2 parts of an amine-based curing accelerator (4-dimethylaminopyridine (DMAP)) per 100 parts of silica (100 parts per 100 g / g). The mixture was uniformly dispersed using a high-speed rotary mixer and then filtered using a cartridge filter (SHP020, manufactured by ROKITECHNO).
[0190] <Example 2: Preparation of resin composition 2> Resin composition 2 was prepared by carrying out the same operations as in Example 1, except that 66.7 parts of the polyimide solution (30% by mass of non-volatile component) obtained in Synthesis Example 2 was used instead of 100 parts of the polyimide solution (20% by mass of non-volatile component) obtained in Synthesis Example 1.
[0191] <Example 3: Preparation of resin composition 3> Resin composition 3 was prepared by carrying out the same operations as in Example 1, except that 100 parts of the polyimide solution (20% by mass of non-volatile component) obtained in Synthesis Example 3 was used instead of 100 parts of the polyimide solution (20% by mass of non-volatile component) obtained in Synthesis Example 1.
[0192] <Comparative Example 1: Preparation of Resin Composition 4> Resin composition 4 was prepared by carrying out the same operations as in Example 1, except that 50 parts of a polycarbonate resin ("FPC2136" manufactured by Mitsubishi Gas Chemical Company, Inc., non-volatile content 20% by mass) was used instead of 50 parts of the polycarbonate-polydimethylsiloxane copolymer resin (non-volatile content 20% by mass, toluene solution) obtained in Synthesis Example 4.
[0193] <Comparative Example 2: Preparation of Resin Composition 5> Resin composition 5 was prepared by carrying out the same operations as in Example 1, except that 50 parts of the polycarbonate-polydimethylsiloxane copolymer resin (20% by mass of non-volatile components, toluene solution) obtained in Synthesis Example 4 was not used, and 10 parts of epoxy-modified silicone oil ("KF-105" manufactured by Shin-Etsu Chemical Co., Ltd.) was used.
[0194] <Comparative Example 3: Preparation of Resin Composition 6> Resin composition 6 was prepared by carrying out the same operations as in Example 1, except that 50 parts of a polycarbonate resin ("FPC2136" manufactured by Mitsubishi Gas Chemical Company, Inc., non-volatile content 20% by mass) was used instead of 50 parts of the polycarbonate-polydimethylsiloxane copolymer resin (non-volatile content 20% by mass, toluene solution) obtained in Synthesis Example 4, and 10 parts of an epoxy-modified silicone oil ("KF-105" manufactured by Shin-Etsu Chemical Co., Ltd.) was used.
[0195] <Comparative Example 4: Preparation of Resin Composition 7> Resin composition 7 was prepared by carrying out the same operations as in Example 1, except that 66.67 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, non-volatile component 30% by mass, 1:1 solution of MEK and cyclohexanone) was used instead of 100 parts of the polyimide solution (non-volatile component 20% by mass) obtained in Synthesis Example 1.
[0196] <Measurement of the average particle size of inorganic fillers> 100 mg of inorganic filler and 10 g of methyl ethyl ketone were weighed into a vial and dispersed by ultrasonic waves for 10 minutes. Using a laser diffraction particle size distribution measuring device (HORIBA, Ltd.'s "LA-960"), the particle size distribution of the inorganic filler was measured on a volume basis using a flow cell method with blue and red light source wavelengths. From the particle size distribution obtained, the average particle size of the inorganic filler was calculated as the median diameter.
[0197] <Measurement of the specific surface area of inorganic fillers> The specific surface area of the inorganic filler was measured using a fully automatic BET specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) by adsorbing nitrogen gas onto the sample surface and calculating the specific surface area using the BET multipoint method.
[0198] <Test Example 1: Confirmation of compatibility in resin composition> The prepared resin compositions 1 to 6 were stored in a refrigerator at 5°C for 3 days, and then the resin compositions were applied onto a glass plate, and the presence or absence of separation in the resin compositions was observed with an optical microscope (Hirox Co., Ltd.'s "KH8700"). When no separation was observed with the optical microscope, it was evaluated as "○", and when separation was observed, it was evaluated as "×".
[0199] <Test Example 2: Measurement and Evaluation of Linear Thermal Expansion Coefficient> The resin composition of each Example and Comparative Example was uniformly applied using a die coater onto the release-treated surface of a PET film (thickness 38 μm) that had been treated with an alkyd-based release agent, so that the resin composition layer would have a thickness of 40 μm after drying, and then dried at 80 to 120°C (average 100°C) for 6 minutes to obtain resin sheet 1.
[0200] The obtained resin sheet 1 was laminated onto a polyimide film (Upilex S, manufactured by Ube Industries, Ltd.) using a batch-type vacuum pressure laminator (MVLP-500, manufactured by Meiki Seisakusho Co., Ltd.). For lamination, the pressure was reduced for 30 seconds to 13 hPa or less, and then the laminate was pressed at 120°C for 30 seconds under a pressure of 0.74 MPa. Thereafter, the PET film was peeled off, and the resin composition was cured under curing conditions of 190°C and 90 minutes, and the polyimide film was peeled off to obtain a cured sample.
[0201] The obtained cured sample was cut into a test piece of 5 mm width and 15 mm length, and a thermomechanical analysis was performed by the tensile load method using a thermomechanical analyzer (Rigaku Corporation, "Thermo Plus TMA8310"). After mounting the sample on the device, measurements were performed twice consecutively under the measurement conditions of a load of 1 g and a heating rate of 5°C / min. The average linear thermal expansion coefficient (ppm) from 25°C to 150°C in the two measurements was calculated. A linear thermal expansion coefficient value of less than 60 ppm was evaluated as "○", and a value of 60 ppm or more was evaluated as "×".
[0202] <Test Example 3: Measurement and Evaluation of Warpage> The resin composition of each Example and Comparative Example was uniformly applied using a die coater onto the release-treated surface of a PET film (thickness 38 μm) that had been treated with an alkyd-based release agent, so that the thickness of the resin composition layer after drying would be 30 μm, and then dried at 80 to 120°C (average 100°C) for 6 minutes to obtain a resin sheet 2.
[0203] The obtained resin sheet 2 was laminated onto a laminate (Hitachi Chemical Co., Ltd., copper foil etched-out product of MCL-E-700G) using a batch-type vacuum pressure laminator (Meiki Seisakusho Co., Ltd., "MVLP-500"). The laminate was depressurized for 30 seconds to make the air pressure 13 hPa or less, and then pressed at 120 ° C for 30 seconds at a pressure of 0.74 MPa. Thereafter, the PET film was peeled off, the resin composition was cured under curing conditions of 190 ° C and 90 minutes, and the polyimide film was peeled off to obtain a cured product sample. The obtained cured product was cut into a test piece with a width of 160 mm and a length of 120 mm, and the amount of warping at the remaining one point was measured while three points were fixed. The amount of warping was evaluated as "good" when the amount of warping was less than 20 mm, and "x" when it was 20 mm or more.
[0204] The amounts of non-volatile components used in the resin compositions of the Examples and Comparative Examples, the measurement results of the Test Examples, the evaluation results, etc. are shown in Table 1 below.
[0205] [Table 1]
[0206] It was found that by using a resin composition containing (A) a polyimide resin and (B) a siloxane-containing polycarbonate resin, a cured product having a low coefficient of thermal expansion and suppressed warping can be obtained.
Claims
1. (A) a polyimide resin, (B) a siloxane-containing polycarbonate resin, (C) an inorganic filler, and (D) an epoxy resin; The content of the component (A) is 1% by mass or more and 50% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass, The content of the (B) component is 1% by mass or more and 30% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass, The content of the (C) component is 10% by mass or more, based on 100% by mass of the non-volatile components in the resin composition; The content of the (D) component is 10% by mass or more, based on 100% by mass of the non-volatile components in the resin composition; A resin composition, the cured product obtained by curing the resin composition under curing conditions of 190°C for 90 minutes has a linear thermal expansion coefficient of less than 60 ppm from 25°C to 150°C at a heating rate of 5°C / min.
2. (A) a polyimide resin, (B) a siloxane-containing polycarbonate resin, (C) an inorganic filler, and (D) an epoxy resin; The content of the component (A) is 50% by mass or less, based on 100% by mass of the non-volatile components in the resin composition; the mass ratio of the component (A) to the component (B) (component (A) / component (B)) is 0.1 or more and 20 or less; The content of the (C) component is 10% by mass or more, based on 100% by mass of the non-volatile components in the resin composition; The content of the (D) component is 10% by mass or more, based on 100% by mass of the non-volatile components in the resin composition; A resin composition, the cured product obtained by curing the resin composition under curing conditions of 190°C for 90 minutes has a linear thermal expansion coefficient of less than 60 ppm from 25°C to 150°C at a heating rate of 5°C / min.
3. The resin composition according to claim 1 or 2, wherein the weight average molecular weight of the component (A) is 1,000 or more and 100,000 or less.
4. The resin composition according to any one of claims 1 to 3, wherein the component (B) is a polycarbonate-polysiloxane copolymer comprising a polycarbonate block having a polycarbonate structure and a polysiloxane block having a polysiloxane structure.
5. The resin composition according to claim 4, wherein the polysiloxane structure is a polydialkylsiloxane structure.
6. The resin composition according to claim 4 or 5, wherein the polycarbonate structure is an aromatic polycarbonate structure.
7. The resin composition according to any one of claims 4 to 6, wherein the content of the polysiloxane structure in the component (B) is 1 mass% or more and 30 mass% or less, when the component (B) is 100 mass%.
8. The resin composition according to any one of claims 1 to 7, wherein the viscosity average molecular weight of component (B) is 13,000 or more and 25,000 or less.
9. The resin composition according to any one of claims 1 to 8, wherein the component (C) is silica.
10. The resin composition according to any one of claims 1 to 9, wherein the content of the component (C) is 30% by mass or more and 60% by mass or less, when the non-volatile components in the resin composition are 100% by mass.
11. The resin composition according to any one of claims 1 to 10, further comprising (E) a curing agent.
12. The resin composition according to claim 11, wherein the component (E) comprises a curing agent selected from a phenol-based curing agent, a naphthol-based curing agent, an active ester-based curing agent, a benzoxazine-based curing agent, a cyanate ester-based curing agent, and a carbodiimide-based curing agent.
13. The resin composition according to claim 11, wherein the component (E) comprises an active ester-based curing agent.
14. The resin composition according to any one of claims 1 to 13, which is for forming an insulating layer of a multilayer flexible substrate.
15. A cured product of the resin composition according to any one of claims 1 to 13.
16. A resin sheet comprising a support and a resin composition layer formed from the resin composition according to any one of claims 1 to 13 provided on the support.
17. A multilayer flexible substrate comprising an insulating layer formed by curing the resin composition according to any one of claims 1 to 14.
18. A semiconductor device comprising the multilayer flexible substrate according to claim 17.
Citation Information
Patent Citations
Polyether polysiloxane block copolymer - - - - ether and blends of polycarbonate organosiloxane
JP1985501007A
Resistance film parallel type radio wave absorbing element
JP1987040798A
Radio wave absorbing wall
JP1987040799A
Training apparatus for correcting golf swing
JP1988043680A
Electrostatic 4-phase electric field rotating device
JP1988087181A