Metallic paint composition and coated body
A metallic coating composition using resin-coated aluminum flakes and a specific binder resin achieves both excellent metallic appearance and chemical resistance, addressing the dual challenges of appearance and durability in automotive interior parts.
Patent Information
- Application Number
- JP2020168276
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-05
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2040-10-05
AI Technical Summary
Existing one-coat metallic paint compositions fail to simultaneously achieve an excellent metallic appearance and chemical resistance, particularly in automotive interior parts that require high chemical resistance and a one-coat solution without mixing a curing agent.
A metallic coating composition comprising resin-coated aluminum flakes with specific particle sizes, combined with a binder resin containing acrylic resin and cellulose derivatives, and an organic solvent, with a balanced ratio of these components, forms a coating film that provides both metallic appearance and chemical resistance.
The composition achieves a one-coat paint that maintains excellent metallic appearance and demonstrates high chemical resistance, including resistance to sweat, lactic acid, and sunscreen creams, while maintaining pencil hardness after chemical treatment.
Smart Images

Figure 0007575907000001 
Figure 0007575907000002 
Figure 0007575907000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a metallic coating composition for producing a metallic-toned coating film formed on the surface of a plastic substrate, and to a coated body having such a coating film. [Background technology]
[0002] In recent years, the automotive industry has been moving away from metal parts to plastic parts in order to improve fuel efficiency, and to differentiate cars from their competitors and achieve a sense of luxury, interior parts require highly aesthetic, high-brightness metallic paint.
[0003] Automotive interior parts are required to have excellent resistance to sweat, lactic acid, hand cream, sunscreen, etc., because they are in contact with human skin and hands for long periods of time. They also need to have abrasion resistance and other properties, and generally a top coat is applied after the metallic paint is applied, but to improve productivity, one-coat specifications using paint that can be used as both a primer and top coat are being considered.
[0004] Furthermore, from the perspective of process saving, there is a demand for the development of one-component paints that can be used as both undercoats and topcoats, which do not require the time of mixing a hardener and do not require consideration of the pot life after mixing.
[0005] In response to such demands, a metallic paint composition with a one-coat specification has been proposed as a paint that can provide a metallic appearance with excellent design (Patent Document 1). Also, a paint composition containing a cellulose ester derivative has been proposed as a paint that can provide excellent chemical resistance (Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-080776 A [Patent Document 2] JP 2014-208827 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in order to obtain an excellent metallic tone, it is necessary to properly orient the luster pigment, and therefore a one-coat paint composition that simultaneously provides an excellent metallic tone and chemical resistance has not yet been obtained.
[0008] An object of the present invention is to provide a metallic paint composition having excellent chemical resistance in a one-coat specification and a coated body thereof. [Means for solving the problem]
[0009] The object of the present invention has been achieved by the following. 1. A metallic paint composition comprising (A) aluminum flakes, (B) a binder resin, and (C) an organic solvent, The (A) is a resin-coated aluminum flake, and the resin-coated aluminum flake has an average particle size of 5 to 30 μm; The (B) contains an acrylic resin and a cellulose derivative, 90% by mass or more of the acrylic resin has a hydroxyl value of less than 5 mg / KOHg, The metallic coating composition has a content ratio of the acrylic resin to the cellulose derivative of 80 / 20 to 20 / 80 (parts by mass / parts by mass). 2. The metallic paint composition according to 1 above, wherein the (B) binder resin contains at least two types of cellulose derivatives, at least one of which is a cellulose derivative (B-1) having a weight average molecular weight Mw of 20,000 to 80,000, and at least one of which is a cellulose derivative (B-2) having a weight average molecular weight Mw of 80,000 to 150,000. 3. The metallic coating composition according to 1 or 2 above, wherein the content ratio of the cellulose derivative (B-1) to the cellulose derivative (B-2) is 95 / 5 to 5 / 95 (parts by mass / parts by mass). 4. A coated body comprising a plastic substrate and a coating film formed from the metallic coating composition described in any one of 1 to 3 above. 5. The coated body according to 4 above, wherein the FI value of the coating film is 20 or more. 6. The coated body according to 4 or 5 above, wherein the coating film satisfies the relationship of the following formula (I). XY=ΔH≦2nd magnitude...(I) [Wherein, X is the pencil hardness before the chemical treatment, Y is the pencil hardness after the chemical treatment, and ΔH is the grade difference in pencil hardness before and after the chemical treatment. Here, the chemical treatment refers to a method of applying 0.5 g / 100 cm of a sunscreen [containing avobenzene (3 mass%), homosalate (10 mass%), octisalate (5 mass%), and octocrylene (10 mass%) as ultraviolet absorbing agents, and also containing water (67 mass%), benzyl alcohol (1 mass%), glycerin (1 mass%), jojoba ester (1 mass%), shea butter (1 mass%), and olive emulsified wax (1 mass%) as ultraviolet absorbing agents] to the surface of the coating film of the coated body. 2 and then leave it in a dryer without forced convection at a temperature of 50±2°C for 3 hours. The pencil hardness is the pencil hardness measured in accordance with JIS K 5600-5-4:1999 (ISO / DIS 15184:1996). Effect of the Invention
[0010] According to the present invention, it is possible to provide a one-coat paint composition that simultaneously provides excellent metallic tone and chemical resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The metallic paint composition and coated body of the present invention will be described in detail below, but the present invention is not limited thereto.
[0012] <Metallic paint composition> The metallic paint composition of the present invention is a metallic paint composition containing (A) aluminum flakes, (B) a binder resin, and (C) an organic solvent, characterized in that (A) is a resin-coated aluminum flake, the resin-coated aluminum flakes have an average particle size of 5 to 30 μm, and 7 to 20 g of resin is coated per 100 g of the aluminum flakes before coating, (B) contains an acrylic resin and a cellulose derivative, 90 mass% or more of the acrylic resin has a hydroxyl value of less than 5 mg / KOHg, and the content ratio of the acrylic resin to the cellulose derivative is 80 / 20 to 20 / 80 (parts by mass / parts by mass).
[0013] <(A) Aluminum flakes> The (A) aluminum flakes are resin-coated aluminum flakes whose surfaces are coated with resin, and have an average particle size of 5 to 30 μm, more preferably 7 to 25 μm.
[0014] The average thickness is not particularly limited, but is preferably 0.005 μm or more, and more preferably 0.02 μm or more and 3 μm or less. The average aspect ratio is 5-150, preferably 20-100.
[0015] The average particle size is determined by calculating the volume average from the particle size distribution measured by a particle size distribution measurement method using a laser diffraction method. The average thickness can be calculated from the hiding power and density of the flakes. The average aspect ratio is expressed as the average thickness / average particle size.
[0016] Examples of the resin to be coated include known resins such as acrylic resins polymerized with acrylic ester or methacrylic ester as the main component, polyester resins, and polyurethane resins, with acrylic resins being preferred.
[0017] The amount of resin coated is preferably 0.1 to 25 g, and particularly preferably 5 to 20 g, per 100 g of aluminum flakes.
[0018] The aluminum flakes of the present invention may have an inorganic compound layer or a metal layer exhibiting an interference effect. In addition, a plurality of aluminum flakes having different average particle sizes may be used, and aluminum flakes not coated with resin may be included within a range that does not impair the effects of the present invention.
[0019] The (A) resin-coated aluminum flakes of the present invention are preferably contained in an amount of 1 to 20 mass % of the solid content of the metallic coating composition, and more preferably 10 to 16 mass %.
[0020] For the aluminum frame of the present invention, commercially available resin-coated Alpaste FZ series (manufactured by Toyo Aluminum Co., Ltd.), resin-coated Alpaste BP series (manufactured by Toyo Aluminum Co., Ltd.), Asahi Kasei Aluminum Paste CP-R series (Asahi Kasei Chemicals Co., Ltd.), etc. can be used.
[0021] <(B) Binder resin> The binder resin (B) of the present invention contains an acrylic resin and a cellulose derivative, in which 90 mass % or more of the acrylic resin has a hydroxyl value of less than 5 mg / KOHg, and the content ratio of the acrylic resin to the cellulose derivative is 80 / 20 to 20 / 80 (parts by mass / parts by mass).
[0022] When multiple acrylic resins are contained, the acrylic resins having a hydroxyl value of 5 mg / KOHg or more may be contained in an amount of less than 10% by mass of the total acrylic resins, preferably less than 5% by mass, and more preferably less than 1% by mass.
[0023] The (B) binder resin is preferably contained in an amount of 60 to 99 mass % of the solid content of the metallic coating composition, more preferably 80 to 90 mass %. The content ratio of the acrylic resin to the cellulose derivative is 80 / 20 to 20 / 80 (parts by mass / parts by mass), preferably 70 / 30 to 50 / 50.
[0024] [Acrylic resin] The acrylic resin used in the binder resin (B) of the present invention may be one used in ordinary acrylic lacquers. It is preferable that the acrylic resin is a polymer or copolymer mainly composed of an acrylic acid ester or a methacrylic acid ester. Here, the term "main component" means that the component is contained in an amount of 50 mol% or more.
[0025] At least 90% by mass of the acrylic resin of the present invention has a hydroxyl value of less than 5 mg / KOHg. The fewer the hydroxyl groups, the more preferable. And it is preferable that the Tg is 50° C. or higher.
[0026] [Cellulose derivatives] Examples of the cellulose derivatives of the present invention include cellulose ethers, cellulose esters, nitrocellulose (NC), acrylic-modified cellulose derivatives, polyester-modified cellulose derivatives, and polyurethane-modified cellulose derivatives, with nitrocellulose being particularly preferred. The nitrocellulose preferably has a nitrogen content of 10% or more.
[0027] It is preferable that the binder resin (B) of the present invention contains at least two types of cellulose derivatives, at least one of which is a cellulose derivative (CE-1) having a weight average molecular weight Mw of 20,000 to 80,000, and at least one of which is a cellulose derivative (CE-2) having a weight average molecular weight Mw of 80,000 to 150,000.
[0028] The content ratio of the cellulose derivative (CE-1) to the cellulose derivative (CE-2) is preferably 95 / 5 to 5 / 95 (parts by mass / parts by mass), and more preferably 90 / 10 to 50 / 50.
[0029] These cellulose derivatives may be used alone or in combination of two or more kinds, in which case at least one kind is preferably nitrocellulose.
[0030] <(C) Organic solvent> The organic solvents that can be used in the present invention may be those used in ordinary paints, for example, hydrocarbon solvents such as toluene and xylene, ketones such as methyl ethyl ketone and diisobutyl ketone, esters such as ethyl acetate, butyl acetate and cellosolve acetate, and alcohols such as 2-ethylhexanol.
[0031] <Antibacterial and antiviral agents> The coating composition of the present invention may contain an antibacterial agent or an antiviral agent, or may contain both an antibacterial agent and an antiviral agent. Some antibacterial agents can be imparted with antiviral functions, and some antiviral agents can be imparted with antibacterial functions. In this way, an agent that can impart both antibacterial and antiviral functions can also be called an antibacterial / antiviral agent.
[0032] Examples of antibacterial and antiviral agents include fine particles of metal ions supported on inorganic substances (porous materials such as zeolite, photocatalytic particles such as titanium oxide, phosphate minerals such as apatite, metal phosphates, etc.), metal / inorganic oxide composite particles, organic acids or inorganic acids, metal iodides, metal salts (e.g., salts of silver, copper, zinc, tungsten, or molybdenum), silver particles, copper particles, cuprous oxide particles, quaternary ammonium salts, pyrithione compounds, sulfonic acid group-containing polymers, amino group-containing polyvinyl alcohols, organic nitrogen bromine compounds, and H-type carboxyl group-containing polymers. In particular, materials containing copper element and H-type carboxyl group-containing polymers are preferred.
[0033] The content of the antibacterial agent or antiviral agent in the coating composition of the present invention is preferably 0.1 to 5 mass %, and the content of the antibacterial agent or antiviral agent in the non-volatile matter in the coating composition of the present invention is preferably 0.2 to 8 mass %.
[0034] The antibacterial or antiviral agent can be added to the coating composition in an amount of 0.1 to 5 mass % or 0.2 to 8 mass % of the non-volatile content to impart an antibacterial or antiviral function. The antibacterial or antiviral agent may be used alone or in combination of two or more.
[0035] Other Additives The metallic coating composition of the present invention may contain additives that are commonly used in the coating industry, such as surface conditioners, wetting agents, dispersants, emulsifiers, thickeners, anti-settling agents, anti-skinning agents, anti-sagging agents, defoamers, anti-color separation agents, leveling agents, drying agents, plasticizers, insecticides, light stabilizers, ultraviolet absorbers, antistatic agents, and conductivity imparting agents, depending on the purpose. As these additives, commercially available products can be suitably used.
[0036] In the present invention, a crosslinking agent that is used in a typical metallic resin composition can be used, but it is preferable not to use it.
[0037] <Painted body> The coated body of the present invention can be prepared by applying the metallic coating composition of the present invention onto a plastic substrate.
[0038] <Plastic substrate> In the coated body of the present invention, the plastic substrate is not particularly limited, and substrates of various shapes can be selected according to the application of the coated body. Examples of the plastic substrate include PPE (polyphenylene ether) resin, polystyrene resin, olefin polymers such as polypropylene and polyethylene, polycarbonate resin, acrylic resin such as polymethyl methacrylate, and ABS resin.
[0039] Preferably, the plastic substrate is a plastic substrate used in automotive interiors.
[0040] In the present invention, the coating amount of the coating material can be varied depending on the type and application of the plastic substrate, but is usually 20 to 400 g / m 2 40 to 200 g / m 2 The thickness of the coating film formed on the surface of the plastic substrate depends on the amount of the coating material applied.
[0041] In the present invention, a coating film can be formed by drying the paint applied to the surface of a plastic substrate. For example, when the paint is a volatile drying type paint (lacquer), the coating film can be obtained by leaving the paint at a temperature of 5°C or higher and lower than 90°C after application.
[0042] Similarly, when the coating material is a thermosetting coating material, after application, the coating material is left to stand at a temperature of 5° C. or higher and lower than 90° C. to obtain a coating film.
[0043] The coating film can be prepared by using a conventional coating method such as brush coating, roller coating, trowel coating, spatula coating, flow coater coating, or spray coating (e.g., air spray coating, airless spray coating, etc.).
[0044] <FI value> The FI value is a value indicating the flip-flop property that shows the metallic characteristics, and is defined by the following formula.
[0045]
number
[0046] In the present invention, the FI value was calculated using values at 15°, 45°, and 110° measured using "BYK-macI" (product name, manufactured by BYK-gardner). A higher FI value indicates a higher flip-flop property of the coating surface.
[0047] The coating film of the coated body of the present invention has an FI value of 20 or more, and preferably 22 or more.
[0048] Furthermore, it is preferable that the coating film satisfies the relationship of the following formula (I). XY=ΔH≦2nd magnitude...(I) [Wherein, X is the pencil hardness before the chemical treatment, Y is the pencil hardness after the chemical treatment, and ΔH is the grade difference in pencil hardness before and after the chemical treatment. Here, the chemical treatment refers to a method of applying 0.5 g / 100 cm of a sunscreen [containing avobenzene (3 mass%), homosalate (10 mass%), octisalate (5 mass%), and octocrylene (10 mass%) as ultraviolet absorbing agents, and also containing water (67 mass%), benzyl alcohol (1 mass%), glycerin (1 mass%), jojoba ester (1 mass%), shea butter (1 mass%), and olive emulsified wax (1 mass%) as ultraviolet absorbing agents] to the surface of the coating film of the coated body. 2 and then leave it in a dryer without forced convection at a temperature of 50±2°C for 3 hours. The pencil hardness is the pencil hardness measured in accordance with JIS K 5600-5-4:1999 (ISO / DIS 15184:1996).
[0049] Chemicals for the chemical treatment can be prepared as follows. (i) (Material: oil) → 200 mL beaker 1g Shea butter Jojoba esters 1g Olive emulsifying wax 1g (ii) (Materials: Water) → 200 mL beaker 1g glycerin Benzyl alcohol 1g ·Water 67g (iii) (Materials / Active Ingredients) Avobenzene 3g Homosalate 10g Octisalate 5g Octocrylene 10g Heat (i) to 60℃ and dissolve. Heat (ii) to 60°C and add it little by little to (i) while whisking, and mix. Add (iii) to the mixture and mix, then stir with a disperser.
[0050] The pencil hardness specified in JIS K 5600-5-4:1999 (ISO / DIS 15184:1996) is specified in the order of hardness from lowest to highest: 6B, 5B, 4B, 3B, 2B, B, HB, F, H, 2H, 3H, 4H, 5H, 6H. A coating film with a grade of 6B has the lowest pencil hardness, while a coating film with a grade of 6H has the highest pencil hardness.
[0051] In the coated body of the present invention, the coating film must satisfy the relationship of the above formula (I), and usually satisfies the following formula (II): X ≧ Y (II) [wherein X and Y are as defined in the above formula (I)] is satisfied. Here, if the difference in pencil hardness grade of the coating film before and after the chemical treatment is 2 grades or less, the hardness of the coating film can be maintained at a high level even after the chemical treatment, and therefore excellent chemical resistance can be imparted to the coated body.
[0052] In order to keep the difference in pencil hardness of the coating film before and after chemical treatment to 2 grades or less, it is preferable to use a cellulose derivative in the paint that forms the coating film.
[0053] Furthermore, by combining the use of a cellulose derivative with an acrylic resin having a specific glass transition temperature, the difference in pencil hardness of the coating film before and after chemical treatment can be more reliably kept to 2 grades or less.
[0054] In the present invention, the glass transition temperature (Tg) is calculated using the following FOX formula.
[0055] 1 / Tg=W1 / Tg1+W2 / Tg2+···+Wi / Tgi+···+Wn / Tgn In the above FOX equation, Tg is the glass transition temperature (K) of a polymer consisting of n types of monomers, Tg(1, 2, i, n) is the glass transition temperature (K) of a homopolymer of each monomer, W(1, 2, i, n) is the mass fraction of each monomer, and W1+W2+···+Wi+···+Wn=1.
[0056] The paint may contain pigments other than aluminum flakes. Examples of pigments include color pigments, extender pigments, and metallic pigments, and can be appropriately selected depending on the color and gloss of the coating film, painting workability, strength and physical properties of the coating film, etc.
[0057] The color pigment may be any known material, such as inorganic pigments, such as titanium oxide and carbon black, or organic pigments, such as phthalocyanine pigments and azo pigments. The extender pigment may also be any known material, such as talc, mica, barium sulfate, clay, calcium carbonate, etc.
[0058] Examples of metallic pigments other than aluminum flakes include glittering pigments or scaly pigments, such as nickel powder pigments, gold powder, silver powder, bronze powder, copper powder, stainless steel powder pigments, mica pigments, graphite pigments, glass flake pigments, metal-coated glass powder, metal-coated mica powder, metal-coated plastic powder, and scaly iron oxide pigments.
[0059] From the viewpoint of chemical resistance, it is preferable that the surface of the glittering pigment or scaly pigment is surface-treated with an organic component and / or an inorganic component. When no pigment is contained, the paint can be used as a clear paint. EXAMPLES
[0060] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The hydroxyl value, heating residue, and number average molecular weight were measured by the following methods. The measurements were performed in an atmosphere of 23°C and 50% RH unless otherwise specified.
[0061] <Hydroxyl value> The free hydroxyl groups in 1 g of resin solids were completely acetylated with acetic anhydride, and the amount of potassium hydroxide required to neutralize them was then determined in mg.
[0062] <Weight average molecular weight> The weight average molecular weight (Mw) was measured by size exclusion chromatography (SEC, Tosoh Corporation; HLC-8220GPC) equipped with an RI using a TSKgel column (Tosoh Corporation). The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (Tosoh Corporation) was used as the standard substance.
[0063] <Metallic resin composition> According to the formulation shown in Table 1, the raw materials were mixed and dispersed by a known method to prepare a paint. The materials used are as follows:
[0064] <(A) Aluminum frame> (A)-1: Aluminum flake A, average particle size 10 μm, aspect ratio 70, resin coating amount 14 g / 100 g Al (manufactured by Toyo Aluminum Co., Ltd.) (A)-2: Aluminum flake B, average particle size 24 μm, aspect ratio 67, resin coating amount 9 g / 100 g Al (manufactured by Toyo Aluminum Co., Ltd.) (A)-3: Aluminum flake C, average particle size 10 μm, aspect ratio 50, resin coating amount 3 g / 100 g Al (manufactured by Toyo Aluminum Co., Ltd.) (A)-4: Aluminum flake D, average particle size 12 μm, aspect ratio 48, no resin coating (manufactured by Toyo Aluminum Co., Ltd.)
[0065] <(B) Binder resin> (B)-1: Acrylic resin varnish A, hydroxyl value 0 g / KOH, Tg 95°C (DIC Corporation) (B)-2: Nitrocellulose A Mw60,000 (KOREA CNC LTD.) (B)-3: Nitrocellulose B Mw 100,000 (manufactured by Asahi Kasei Corporation) (B)-4: Acrylic resin varnish B, hydroxyl value 20 mg / KOH, Tg 70°C (DIC Corporation)
[0066] <(C) Organic solvent> (C)-1: Ketone solvent (methyl isobutyl ketone) (C)-2: Ester solvent (methoxybutyl acetate) <Other> Additive: Polyethylene wax dispersion (NV 10% by mass, manufactured by Gifu Ceramics Manufacturing Co., Ltd.)
[0067] [Table 1]
[0068] Next, the coating material was spray-coated on an ABS resin plate in such an amount that the dry film thickness was 10 to 20 μm, and the plate was left to stand for 10 minutes, after which it was dried at 80° C. for 30 minutes to obtain the coated bodies of the examples and comparative examples. The following tests were carried out on the sample coated bodies. The results are shown in Table 2.
[0069] <Metallic Tone Evaluation> <FI value> The calculation was performed using the values at 15°, 45°, and 110° measured using "BYK-macI" (trade name, manufactured by BYK-gardner).
[0070] <Chemical resistance test> The alkali resistance and acid resistance were evaluated by the following method.
[0071] <Alkaline discoloration resistance> Using the above test specimen, an alkali resistance test was conducted in accordance with JIS K 5600-6-1:2016 Method 2 (absorption medium method). However, the test liquid was a 0.1N sodium hydroxide aqueous solution, and the specimen was placed in a thermostatic chamber maintained at 50±2°C and left for 3 hours. After that, the specimen was washed with water and wiped, and the coating surface condition of the test area was visually evaluated according to the following criteria. ○: No change on the coating surface △: Slight discoloration was observed on the coating surface. ×: Discoloration was observed on the coating surface.
[0072] <Acid discoloration resistance> Using the above test specimens, an acid resistance test was conducted in accordance with JIS K 5600-6-1:2016 Method 2 (absorption medium method). However, the test liquid was a 0.1N sulfuric acid aqueous solution, and after leaving it for 24 hours under standard conditions (25±2°C, 50±5% RH), the test plate was washed with water and wiped, and the coating surface condition of the test area was visually evaluated according to the following criteria. ○: No change on the coating surface △: Slight discoloration was observed on the coating surface. ×: Discoloration was observed on the coating surface.
[0073] <Oil and grease stain resistance test> ≪Pencil hardness≫ First, the pencil hardness of the coating film before chemical treatment was determined using a scratch hardness test pencil (Uni MITSUBISHI, manufactured by Mitsubishi Pencil Co., Ltd.) in accordance with JIS K 5600-5-4:1999 (ISO / DIS 15184:1996). Next, a sunscreen agent [containing avobenzene (3% by mass), homosalate (10% by mass), octisalate (5% by mass), and octocrylene (10% by mass) as ultraviolet absorbers, and also containing water (67% by mass), benzyl alcohol (1% by mass), glycerin (1% by mass), jojoba ester (1% by mass), shea butter (1% by mass), and olive emulsified wax (1% by mass)] was applied to the coating film surface of the coated body at a concentration of 0.5 g / 100 cm. 2 The coating was applied at a ratio of 100:1 to 100:1, and then left in a dryer without forced convection at a temperature of 50±2°C for 3 hours for chemical treatment. The coating was then washed with water to remove the sunscreen, and finally the pencil hardness of the coating after chemical treatment was determined using the same method. The change in hardness before and after treatment is indicated by arrows in Table 2. ○: The hardness after the chemical treatment was unchanged from the hardness before the chemical treatment. △: The hardness after chemical treatment is one grade lower than the hardness before chemical treatment. ×: The hardness after the chemical treatment is reduced by 2 or more grades from the hardness before the chemical treatment.
[0074] <Appearance> The coating surface after the above chemical treatment was washed with water to remove the sunscreen agent, and the appearance of the coating after the chemical treatment was visually evaluated according to the following criteria. ○: No change on the coating surface. △: Traces or slight discoloration are observed on the coating surface. ×: Discoloration, shrinkage, blistering, or peeling is observed on the coating surface.
[0075] <<Close Contact>> The coating film after the above chemical treatment was used as a test specimen, and a straight cut was made on the surface of the coating film with a cutter knife at a cutting angle of 60°, and then another cut was made at an angle of 60° to the first cut. Cellophane tape was then firmly attached to cover the cut, and the cellophane tape was peeled off at an angle of 45° to the coating film surface. After peeling off the cellophane tape, the degree of peeling of the coating film was visually judged according to the following evaluation criteria. ○: No peeling at all. △: There is slight peeling at the cut area. ×: The coating surface at the cut portion was completely peeled off.
[0076] <Wear> The coating film after the above chemical treatment was used as a test specimen, and a friction test was performed by reciprocating a 2 kg abrasive attached to cotton canvas against the coating surface 200 times. The result was visually evaluated according to the following criteria. ○: No change on the coating surface. △: Scratches were observed on the coating surface, but the base material was not exposed. ×: The substrate is partially or entirely exposed.
[0077] [Table 2]
[0078] As can be seen from the results in Table 2, the present invention makes it possible to obtain a metallic paint composition having excellent chemical resistance in a single coat specification and a coated body thereof.
Claims
1. A metallic paint composition comprising (A) aluminum flakes, (B) a binder resin, and (C) an organic solvent, (A) is a resin-coated aluminum flake, and the resin-coated aluminum flake has an average particle size of 5 to 30 μm; The (B) contains an acrylic resin and a cellulose derivative, 90% by mass or more of the acrylic resin has a hydroxyl value of less than 5 mg / KOHg, The metallic coating composition has a content ratio of the acrylic resin to the cellulose derivative of 80 / 20 to 20 / 80 (parts by mass / parts by mass).
2. The metallic paint composition according to claim 1, wherein the binder resin (B) contains at least two types of cellulose derivatives, at least one of which is a cellulose derivative (CE-1) having a weight average molecular weight Mw of 20,000 to 80,000, and at least one of which is a cellulose derivative (CE-2) having a weight average molecular weight Mw of 80,000 to 150,000.
3. The metallic paint composition according to claim 1 or 2, wherein the content ratio of the cellulose derivative (CE-1) to the cellulose derivative (CE-2) is 95 / 5 to 5 / 95 (parts by mass / parts by mass).
4. A coated body comprising a plastic substrate and a coating film formed from the metallic coating composition according to any one of claims 1 to 3.
5. The coated body according to claim 4, wherein the paint film has an FI value of 20 or more.
6. The coated body according to claim 4 or 5, wherein the coating film satisfies the following formula (I): X-Y=ΔH≦2nd grade...(I) [Wherein, X is the pencil hardness before the chemical treatment, Y is the pencil hardness after the chemical treatment, and ΔH is the grade difference in pencil hardness before and after the chemical treatment. Here, the chemical treatment refers to a method of applying 0.5 g / 100 cm of a sunscreen agent [containing avobenzene (3 mass%), homosalate (10 mass%), octisalate (5 mass%), and octocrylene (10 mass%) as ultraviolet absorbers, and also containing water (67 mass%), benzyl alcohol (1 mass%), glycerin (1 mass%), jojoba ester (1 mass%), shea butter (1 mass%), and olive emulsified wax (1 mass%)] to the surface of the coating film of the coated body. 2 and then leaving it at a temperature of 50±2° C. for 3 hours. The pencil hardness is the pencil hardness measured in accordance with JIS K 5600-5-4:1999 (ISO / DIS 15184:1996).
Citation Information
Patent Citations
One coat metallic coating material composition
JP2002080776A
Solid drawing material and method for producing the same
JP2004210842A
Multi-component base coating material, color toning method, and repairing coating method
JP2013040293A
Coating material composition and method for forming coating film
JP2013053235A
Coated body
JP2014208827A