Adhesive for repeatedly flexed devices, adhesive sheet, repeatedly flexed laminate member, and repeatedly flexed device

A specialized adhesive with tailored mechanical properties addresses the issue of lifting and peeling in repeatedly bent displays by minimizing stress and strain, ensuring durability and recovery in varying temperatures.

JP7576478B2Active Publication Date: 2024-10-31LINTEC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021013921
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-29
Publication Date
2024-10-31
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

Conventional adhesives used in repeatedly bent displays experience lifting or peeling at the interface between the adhesive layer and the adherend, which is not adequately addressed by existing solutions.

Method used

An adhesive with specific storage modulus and creep compliance values, along with a creep recovery rate, is developed to minimize stress and strain during repeated bending, ensuring the adhesive layer remains intact under varying temperatures.

Benefits of technology

The adhesive effectively prevents lifting and peeling at the interface, providing excellent bending resistance and recovery properties in repeated bending devices, even under extreme temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576478000003
    Figure 0007576478000003
  • Figure 0007576478000004
    Figure 0007576478000004
  • Figure 0007576478000005
    Figure 0007576478000005
Patent Text Reader

Abstract

To provide an adhesive or an adhesive sheet for a repeated-bendable device, wherein the adhesive or the adhesive sheet is applied to a repeated-bendable device to suppress its floating and peeling; and a repeated-bendable laminate and a repeated-bendable device that are less prone to floating and peeling.SOLUTION: The present invention discloses an adhesive for a repeated-bendable device. The adhesive has a storage elastic modulus G' of 0.20 MPa or less at -30°C. A creep compliance value at application of the stress of 4500 Pa is set as the minimum creep compliance J(t)min (MPa-1). The stress of 4500 Pa is continuously applied up to 1200 seconds after the measurement of J(t)min, and a maximum creep compliance value measured during its period is set as the maximum creep compliance J(t)max (MPa-1), wherein the creep compliance variation ΔlogJ(t) is 2.60 or less, calculated by the following formula (I): ΔlogJ(t)=logJ(t)max-logJ(t)min.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive and an adhesive sheet for a device that is repeatedly bent, as well as a repeatedly bent laminate member and a repeatedly bent device. [Background technology]

[0002] In recent years, bendable displays have been proposed as displays for electronic devices, which are a type of device. In addition to displays that are curved only once, repeatedly bent displays that are repeatedly bent (folded) have also been proposed.

[0003] In the above-mentioned repeatedly bent display, it is considered that one bendable member (flexible member) constituting the said bent display and another bendable member are bonded with an adhesive layer. However, when a conventional adhesive is used in a repeatedly bent display, there arises a problem that lifting or peeling occurs at the interface between the adhesive layer and the adherend.

[0004] Patent Document 1 discloses a pressure-sensitive adhesive that aims to prevent the pressure-sensitive adhesive layer from lifting or peeling even when the sheet is repeatedly bent. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-108555 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, even when such adhesives as described above are used, it is not possible to sufficiently prevent lifting or peeling caused by repeated bending.

[0007] The present invention has been made in consideration of the above-described circumstances, and aims to provide an adhesive and adhesive sheet for repeatedly flexed devices that suppress the occurrence of lifting and peeling when applied to a repeatedly flexed device, as well as a repeatedly flexed laminate member and a repeatedly flexed device that suppress the occurrence of lifting and peeling. [Means for solving the problem]

[0008] In order to achieve the above object, first, the present invention provides a pressure-sensitive adhesive for repeatedly bending devices, for bonding one flexible member and another flexible member that constitute a device that is repeatedly bent, the pressure-sensitive adhesive having a storage modulus G'(-30) of 0.20 MPa or less at -30°C, and a creep compliance value measured when a stress of 4500 Pa is applied to the pressure-sensitive adhesive being a minimum creep compliance J(t) min (MPa -1 ) and the minimum creep compliance J(t) min The stress of 4500 Pa was applied until 1200 seconds after the measurement, and the maximum creep compliance measured during that time was called the maximum creep compliance J(t). max (MPa -1 ) and the creep compliance fluctuation value ΔlogJ(t) calculated from the following formula (I) is 2.60 or less (Invention 1). ΔlogJ(t)=logJ(t) max -logJ(t) min …(I)

[0009] In the above invention (Invention 1), since the storage modulus G'(-30) at -30°C is small as described above, it is possible to reduce the stress generated by repeated bending in a low temperature environment (e.g., -30°C). Meanwhile, since the creep compliance fluctuation value is small as described above, it is possible to suppress excessive strain of the adhesive when repeatedly bent or when bent for a long period of time, regardless of the temperature environment. As a result, when applied to a repeatedly bent device, lifting or peeling is unlikely to occur at the interface between the adhesive layer and the adherend in low to high temperature environments, and excellent bending resistance is obtained.

[0010] In the above invention (Invention 1), the creep compliance value measured after 1200 seconds of continuously applying a stress of 4500 Pa to the pressure-sensitive adhesive is defined as creep compliance J(t) (s=1200) (MPa -1 ), and then the stress applied to the adhesive is set to 0 Pa, and the creep compliance value measured 100 seconds later is defined as creep compliance J(t) (s=1300) (MPa -1 ) and the creep recovery rate calculated from the following formula (II) is preferably 90% or more (Invention 2). Creep recovery rate (%) = (1-J(t)(s=1300) / J(t)(s=1200)) x 100 ... (II)

[0011] In the above inventions (Inventions 1 and 2), the storage modulus G'(85) at 85° C. is preferably 0.005 MPa or more (Invention 3).

[0012] In the above inventions (Inventions 1 to 3), it is preferable that the storage modulus change rate (-30 / 25), which is the value obtained by dividing the storage modulus G'(-30) at -30°C by the storage modulus G'(25) at 25°C, is 5.0 or less (Invention 4).

[0013] In the above inventions (Inventions 1 to 4), it is preferable that the storage modulus change rate (-30 / 85), which is the value obtained by dividing the storage modulus G'(-30) at -30°C by the storage modulus G'(85) at 85°C, is 10.0 or less (Invention 5).

[0014] In the above inventions (Inventions 1 to 5), the gel fraction is preferably 40% or more and 95% or less (Invention 6).

[0015] In the above inventions (Inventions 1 to 6), it is preferable that the pressure-sensitive adhesive contains a main adhesive agent and a low molecular weight component, the weight average molecular weight of the low molecular weight component is 400 or more and 100,000 or less, and the glass transition temperature (Tg) of the low molecular weight component is -40°C or less (Invention 7).

[0016] In the above inventions (Inventions 1 to 7), the pressure-sensitive adhesive is preferably an acrylic pressure-sensitive adhesive (Invention 8).

[0017] Secondly, the present invention provides an adhesive sheet having an adhesive layer for bonding one flexible member and another flexible member that constitute a device that is repeatedly bent, characterized in that the adhesive layer comprises the adhesive for repeatedly bent devices (Inventions 1 to 8) (Invention 9).

[0018] In the above invention (Invention 9), it is preferable that the adhesive sheet has two release sheets, and the adhesive layer is sandwiched between the release sheets so as to be in contact with the release surfaces of the two release sheets (Invention 10).

[0019] Thirdly, the present invention provides a repeatedly flexed laminated member comprising one flexible member and another flexible member constituting a device that is repeatedly flexed, and an adhesive layer that bonds the one flexible member and the other flexible member to each other, wherein the adhesive layer is made of the adhesive for repeatedly flexed devices (Inventions 1 to 8) (Invention 11).

[0020] Fourthly, the present invention provides a repeatedly flexed device (Invention 12), characterized by comprising the repeatedly flexed laminated member (Invention 11). Effect of the Invention

[0021] When the pressure-sensitive adhesive and pressure-sensitive adhesive sheet for a repeatedly flexed device according to the present invention are applied to a repeatedly flexed device, lifting or peeling is unlikely to occur at the interface between the pressure-sensitive adhesive layer and the adherend. Also, the repeatedly flexed laminate member and repeatedly flexed device according to the present invention are unlikely to cause lifting or peeling at the interface between the pressure-sensitive adhesive layer and the adherend. [Brief description of the drawings]

[0022] [Figure 1] 1 is a cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of a repeatedly bent laminated member according to one embodiment of the present invention. [Diagram 3] 1 is a cross-sectional view of a repeated bending device according to an embodiment of the present invention. [Figure 4] FIG. 2 is an explanatory diagram (side view) illustrating a dynamic bending test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, an embodiment of the present invention will be described. [Adhesive for repeatedly bending devices] The pressure-sensitive adhesive for a repeated bending device according to this embodiment (hereinafter, sometimes simply referred to as "pressure-sensitive adhesive") is an adhesive for bonding one flexible member and another flexible member constituting a repeated bending device. The repeated bending device and the flexible member will be described later.

[0024] The pressure-sensitive adhesive according to the present embodiment preferably has a storage modulus G'(-30) of 0.20 MPa or less at -30°C, and the creep compliance value measured when a stress of 4500 Pa is applied to the pressure-sensitive adhesive is the minimum creep compliance J(t) min (MPa -1 ) and the minimum creep compliance J(t) min The stress of 4500 Pa was applied until 1200 seconds after the measurement, and the maximum creep compliance measured during that time was called the maximum creep compliance J(t). max(MPa -1 ) and the creep compliance fluctuation value ΔlogJ(t) calculated from the following formula (I) is preferably 2.60 or less. ΔlogJ(t)=logJ(t) max -logJ(t) min …(I) The details of the method for measuring the storage modulus G' and the method for measuring the creep compliance J(t) are as shown in the test examples described later. Also, "when a stress of 4500 Pa is applied to the adhesive" refers to the time when the stress is applied to the adhesive and reaches 4500 Pa.

[0025] The adhesive according to the present embodiment has a small storage modulus G'(-30) at -30°C as described above, so that the stress generated by repeated bending in a low-temperature environment (for example, -30°C) can be reduced. On the other hand, the creep compliance fluctuation value is small as described above, so that the adhesive can be prevented from being excessively distorted regardless of the temperature environment when repeatedly bent or when bent for a long time. In an adhesive that is excessively distorted, the internal structure of the adhesive also changes with deformation due to bending, and the adhesive does not return to its original state even when the bending is released, but the adhesive according to the present embodiment can suppress such excessive distortion. Although the above two physical values ​​are generally contradictory, the adhesive according to the present embodiment has both the above two physical values, and the stress against deformation is small even at a very low temperature of -30°C, and the distortion due to deformation is small. As a result, when applied to a repeatedly bent device, lifting or peeling is unlikely to occur at the interface between the adhesive layer and the adherend in low to high temperature environments, and excellent flex resistance is obtained.

[0026] From the viewpoint of the bending resistance, the storage modulus G'(-30) at -30°C of the pressure-sensitive adhesive according to the present embodiment is preferably 0.20 MPa or less, more preferably 0.15 MPa or less, particularly preferably 0.11 MPa or less, and even more preferably 0.10 MPa or less. From the viewpoint of cohesive strength, the storage modulus G'(-30) at -30°C of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is preferably 0.01 MPa or more, more preferably 0.02 MPa or more, particularly preferably 0.04 MPa or more, and even more preferably 0.08 MPa or more.

[0027] From the viewpoint of the flexural resistance, the creep compliance fluctuation value ΔlogJ(t) is preferably 2.60 or less, more preferably 2.58 or less, particularly preferably 2.56 or less, and even more preferably 2.54 or less. The lower limit of the creep compliance fluctuation value is not particularly limited, but is usually preferably 1.50 or more, particularly preferably 2.00 or more, and even more preferably 2.20 or more.

[0028] Minimum creep compliance J(t) of the adhesive according to this embodiment min The lower limit is 1MPa. -1 It is preferable that the pressure is 5MPa or more. -1 More preferably, it is 10 MPa or more. -1 It is preferable that the pressure is 15 MPa or more. -1 It is preferable that the minimum creep compliance J(t) is equal to or greater than the minimum creep compliance J(t) min By setting the lower limit value of the minimum creep compliance J(t) as above, the creep compliance fluctuation value ΔlogJ(t) is likely to satisfy the above value. min The upper limit is not particularly limited, but is usually 1000 MPa. -1 It is preferable that the pressure is equal to or lower than 100 MPa. -1 It is preferable that the pressure is 20MPa or less, and more preferable that the pressure is 20MPa or less. -1 It is preferable that:

[0029] In addition, the maximum creep compliance J(t) of the adhesive according to this embodiment max The upper limit is 10000MPa. -1 It is preferable that the temperature is 8000MPa or less. -1 More preferably, it is equal to or less than 6000 MPa. -1 It is preferable that the resistance is 5500 MPa or less, and more preferably 5500 MPa or less. -1 It is preferable that the maximum creep compliance J(t) is less than or equal to max By setting the upper limit value of the above, the creep compliance fluctuation value ΔlogJ(t) is likely to satisfy the above value. Maximum creep compliance J(t) max The lower limit is not particularly limited, but is usually 1100 MPa. -1 More preferably, it is 2000 MPa or more. -1 More preferably, it is 4000 MPa or more. -1 More preferably, it is equal to or greater than this.

[0030] The pressure-sensitive adhesive according to the present embodiment has a creep compliance value measured after 1200 seconds of continuously applying a stress of 4500 Pa to the pressure-sensitive adhesive, which is defined as creep compliance J(t) (s=1200) (MPa -1 ), and the creep compliance value measured 100 seconds after the stress applied to the pressure-sensitive adhesive was set to 0 Pa was defined as creep compliance J(t) (s=1300) (MPa -1 ) and the creep recovery rate calculated from the following formula (II) is preferably 90% or more, more preferably 92% or more, particularly preferably 94% or more, and further preferably 96% or more. Creep recovery rate (%) = (1-J(t)(s=1300) / J(t)(s=1200)) x 100 ... (II)

[0031] Because the adhesive of this embodiment exhibits the above-mentioned creep recovery rate, even when a repeatedly bent device to which the adhesive is applied is left in a bent state for a long period of time, it has excellent recovery from the bent state, and the adhesive layer is less likely to develop flex marks.

[0032] The upper limit of the creep recovery rate is not particularly limited, but is usually preferably 100% or less, more preferably 99% or less, and even more preferably 98% or less.

[0033] The creep compliance J(t) (s=1200) of the adhesive according to this embodiment has a lower limit of 1100 MPa -1 It is preferable that the pressure is 2000MPa or more. -1 More preferably, it is 4000 MPa or more. -1 More preferably, it is 4600 MPa or more. -1 It is preferable that the creep compliance J(t) (s=1200) is equal to or higher than 10000 MPa. This provides a pressure-sensitive adhesive with more appropriate stress relaxation properties. From the viewpoint of the cohesive strength of the pressure-sensitive adhesive, the upper limit of the creep compliance J(t) (s=1200) is usually 10000 MPa. -1 It is preferable that the pressure is equal to or less than 8000MPa. -1 It is preferable that the strength is 6000 MPa or less, and more preferably 6000 MPa or less. -1 It is preferable that:

[0034] In addition, the creep compliance J(t) (s=1300) of the adhesive according to this embodiment has an upper limit of 800 MPa. -1 It is preferable that the pressure is less than 400MPa. -1 More preferably, it is equal to or less than 200 MPa. -1 It is preferable that the pressure is 180MPa or less. -1 It is preferable that the creep compliance J(t) (s=1300) is not more than 1 MPa. This results in a pressure-sensitive adhesive with superior recovery. The lower limit of the creep compliance J(t) (s=1300) is not particularly limited, but is usually 1 MPa. -1 More preferably, it is 10 MPa or more. -1 More preferably, it is 100 MPa or more. -1 More preferably, it is equal to or greater than this.

[0035] The storage modulus G'(85) at 85°C of the adhesive according to this embodiment is preferably 0.005 MPa or more, more preferably 0.010 MPa or more, particularly preferably 0.020 MPa or more, and even more preferably 0.022 MPa or more. This allows the adhesive layer to maintain its cohesive force even at high temperatures without becoming too soft. The storage modulus G'(85) at 85°C of the adhesive according to this embodiment is preferably 0.10 MPa or less, more preferably 0.08 MPa or less, particularly preferably 0.06 MPa or less, and even more preferably 0.04 MPa or less. This makes it easier to obtain a product with a low storage modulus G' at low temperatures.

[0036] The storage modulus G'(25) at 25°C of the pressure-sensitive adhesive according to this embodiment is preferably 0.15 MPa or less, more preferably 0.10 MPa or less, particularly preferably 0.07 MPa or less, and even more preferably 0.04 MPa or less. This makes it easier to exhibit suitable adhesiveness. On the other hand, the storage modulus G'(25) at 25°C is preferably 0.010 MPa or more, more preferably 0.015 MPa or more, particularly preferably 0.020 MPa or more, and even more preferably 0.026 MPa or more. This not only provides excellent repeated bending properties in the standard environmental temperature range, but also provides good processability such as punching.

[0037] The pressure-sensitive adhesive according to the present embodiment has a storage modulus change rate (-30 / 25), which is the value obtained by dividing the storage modulus G'(-30) at -30°C by the storage modulus G'(25) at 25°C, of ​​preferably 5.0 or less, more preferably 4.0 or less, particularly preferably 3.5 or less, and further preferably 3.3 or less. This makes it easy to prevent the elastic modulus from becoming high at low temperatures while maintaining appropriate adhesive strength at room temperature.

[0038] The storage modulus change rate (-30 / 25) is preferably 1.50 or more, more preferably 2.00 or more, particularly preferably 2.50 or more, and further preferably 3.00 or more, which makes it easier to obtain a pressure-sensitive adhesive having excellent cohesive strength.

[0039] The pressure-sensitive adhesive according to the present embodiment has a storage modulus change rate (-30 / 85), which is the value obtained by dividing the storage modulus G'(-30) at -30°C by the storage modulus G'(85) at 85°C, of ​​preferably 10.0 or less, more preferably 7.0 or less, particularly preferably 5.0 or less, and further preferably 4.5 or less. This makes it easy to achieve both a low elastic modulus at low temperatures and a high elastic modulus at high temperatures.

[0040] The storage modulus change rate (-30 / 85) is preferably 1.20 or more, more preferably 2.00 or more, particularly preferably 2.50 or more, and further preferably 3.00 or more, which makes it easier to obtain a pressure-sensitive adhesive having excellent cohesive strength.

[0041] The gel fraction of the adhesive according to the present embodiment is preferably 40% or more, more preferably 50% or more, particularly preferably 60% or more, and even more preferably 70% or more. This allows the adhesive to exhibit a suitable cohesive force capable of withstanding repeated bending. As a result, the above-mentioned bending resistance is more excellent. On the other hand, the gel fraction of the adhesive according to the present embodiment is preferably 95% or less, more preferably 90% or less, particularly preferably 85% or less, and even more preferably 80% or less. This is presumed to suppress the destruction of the crosslinked structure in the adhesive due to repeated bending, and suppress the adhesive layer itself from becoming cloudy. The method for measuring the gel fraction in this specification is as shown in the test example described later.

[0042] The adhesive according to the present embodiment is not particularly limited as long as it satisfies the above physical properties, but it is preferable that it contains a low molecular weight component together with the adhesive base. The low molecular weight component preferably has a weight average molecular weight of 400 or more and 100,000 or less, and a glass transition temperature (Tg) of -40°C or less. An adhesive containing a low molecular weight component having such physical properties together with the adhesive base is likely to satisfy the above-mentioned physical properties, particularly the storage modulus G'(-30) at -30°C. The weight average molecular weight in this specification is a value measured in terms of standard polystyrene by gel permeation chromatography (GPC). The glass transition temperature (Tg) in this specification is a value measured by a differential scanning calorimeter at a heating and cooling rate of 20°C / min.

[0043] From the viewpoint of increasing the storage modulus G'(85) of the resulting pressure-sensitive adhesive or decreasing the creep compliance fluctuation value, the weight average molecular weight (Mw) of the low molecular weight component is preferably 400 or more, more preferably 1000 or more, particularly preferably 2500 or more, and even more preferably 3500 or more. Furthermore, from the viewpoint of decreasing the haze value of the resulting pressure-sensitive adhesive, the weight average molecular weight of the low molecular weight component is preferably 100000 or less, more preferably 50000 or less, particularly more preferably 20000 or less, and even more preferably 14000 or less.

[0044] The glass transition temperature (Tg) of the low molecular weight component is preferably −40° C. or lower, more preferably −45° C. or lower, particularly preferably −50° C. or lower, and even more preferably −52° C. or lower. The glass transition temperature (Tg) of the low molecular weight component is preferably −80° C. or higher, more preferably −70° C. or higher, particularly preferably −65° C. or higher, and even more preferably −60° C. or higher. Specific examples of the low molecular weight component will be described later.

[0045] The type of the adhesive according to the present embodiment is not particularly limited as long as the above-mentioned physical properties are satisfied, and may be, for example, any of an acrylic adhesive, a polyester adhesive, a polyurethane adhesive, a rubber adhesive, a silicone adhesive, etc. The adhesive may be any of an emulsion type, a solvent type, or a solventless type, and may be any of a crosslinked type or a non-crosslinked type. Among them, an acrylic adhesive that easily satisfies the above-mentioned physical properties and has excellent adhesive properties and optical properties is preferred, and a solvent-type acrylic adhesive is particularly preferred.

[0046] Specifically, the adhesive according to the present embodiment is preferably an adhesive obtained from an adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing a (meth)acrylic acid ester polymer (A) as an adhesive base, a low molecular weight component (B), and, if desired, a crosslinking agent (C). Such an adhesive is likely to satisfy the above-mentioned physical properties and is likely to provide good adhesive strength. In this specification, (meth)acrylic acid means both acrylic acid and methacrylic acid. The same applies to other similar terms. In addition, the term "polymer" is also intended to include the concept of "copolymer".

[0047] (1) Components of adhesive composition P (1-1) (Meth)acrylic acid ester polymer (A) The (meth)acrylic acid ester polymer (A) preferably contains, as monomer units constituting the polymer, an alkyl (meth)acrylic acid ester and a monomer having a reactive functional group in the molecule (reactive functional group-containing monomer).

[0048] The (meth)acrylic acid ester polymer (A) can exhibit preferable adhesiveness by containing a (meth)acrylic acid alkyl ester as a monomer unit constituting the polymer. As the (meth)acrylic acid alkyl ester, a (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 1 to 20 is preferable. The alkyl group may be linear or branched, or may have a cyclic structure.

[0049] Examples of (meth)acrylic acid alkyl esters having an alkyl group with 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, stearyl (meth)acrylate, etc. Among these, from the viewpoint of lowering the glass transition temperature (Tg) of the (meth)acrylic acid ester polymer (A) and lowering the elasticity of the resulting pressure-sensitive adhesive, (meth)acrylic acid esters having an alkyl group with 4 to 12 carbon atoms are preferred, and (meth)acrylic acid esters having an alkyl group with 5 to 10 carbon atoms are particularly preferred. Specifically, n-butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are preferred, and 2-ethylhexyl acrylate is particularly preferred. These may be used alone or in combination of two or more.

[0050] The (meth)acrylic acid ester polymer (A) preferably contains 60% by mass or more, more preferably 80% by mass or more, particularly preferably 90% by mass or more, even more preferably 95% by mass or more, and most preferably 98% by mass or more of (meth)acrylic acid alkyl esters having an alkyl group with a carbon number of 1 to 20 as monomer units constituting the polymer. This allows the (meth)acrylic acid ester polymer (A) to be given suitable adhesiveness, and also makes it easy to achieve a low elastic modulus of the resulting adhesive. In addition, the (meth)acrylic acid ester polymer (A) preferably contains 99.9% by mass or less, particularly preferably 99.5% by mass or less, and even more preferably 99.0% by mass or less of (meth)acrylic acid alkyl esters having an alkyl group with a carbon number of 1 to 20. This allows a desired amount of other monomer components to be introduced into the (meth)acrylic acid ester polymer (A).

[0051] The (meth)acrylic acid ester polymer (A) contains a reactive functional group-containing monomer as a monomer unit constituting the polymer, and reacts with the crosslinking agent (C) described below, or the crosslinking agent (C) and the low molecular weight component (B) via the reactive functional group derived from the reactive functional group-containing monomer, thereby forming a crosslinked structure (three-dimensional network structure), and a pressure-sensitive adhesive having the desired cohesive strength is obtained. The pressure-sensitive adhesive is easy to satisfy the creep compliance fluctuation value and creep recovery rate described above.

[0052] The reactive functional group-containing monomer contained in the (meth)acrylic acid ester polymer (A) as a monomer unit constituting the polymer is preferably a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer), etc. These reactive functional group-containing monomers may be used alone or in combination of two or more kinds.

[0053] Among the reactive functional group-containing monomers, hydroxyl group-containing monomers and / or carboxyl group-containing monomers are preferred, and it is particularly preferred to use a combination of hydroxyl group-containing monomers and carboxyl group-containing monomers. The hydroxyl group-containing monomers are easy to adjust the crosslink density and easy to satisfy the creep compliance fluctuation value and creep recovery rate mentioned above. In addition, the carboxyl group-containing monomers can improve the adhesive strength of the resulting pressure-sensitive adhesive and increase the adhesion to the adherend.

[0054] Examples of the hydroxyl group-containing monomer include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among the above, from the viewpoint of ease of satisfying the above-mentioned physical properties, (meth)acrylic acid hydroxyalkyl esters having a hydroxyalkyl group with 1 to 4 carbon atoms are preferred. Specifically, for example, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and the like are preferred, and in particular, 2-hydroxyethyl acrylate or 4-hydroxybutyl acrylate are preferred. These may be used alone or in combination of two or more.

[0055] Examples of the carboxyl group-containing monomer include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among them, acrylic acid is preferred from the viewpoint of the adhesive strength of the (meth)acrylic acid ester polymer (A) obtained. These may be used alone or in combination of two or more kinds.

[0056] The (meth)acrylic acid ester polymer (A) preferably contains reactive functional group-containing monomers as monomer units constituting the polymer in a total amount of 0.1% by mass or more, particularly preferably 0.5% by mass or more, and more preferably 1.0% by mass or more. The (meth)acrylic acid ester polymer (A) preferably contains reactive functional group-containing monomers as monomer units constituting the polymer in a total amount of 10% by mass or less, more preferably 7% by mass or less, particularly preferably 5% by mass or less, and more preferably 2% by mass or less. Components derived from reactive functional group-containing monomers tend to increase the elastic modulus by inducing water solidification at low temperatures, but when the upper limit of the content of reactive functional group-containing monomers is as above, this tendency can be suppressed and the storage modulus G' at low temperatures can be reduced. When the (meth)acrylic acid ester polymer (A) contains reactive functional group-containing monomers as monomer units in the above amount, the storage modulus G' described above can be in a suitable range. Furthermore, when the (meth)acrylic acid ester polymer (A) contains the reactive functional group-containing monomer as a monomer unit in the above amount, the degree of crosslinking can be made relatively strong, the creep compliance fluctuation value can be reduced, and the creep recovery rate can be increased.

[0057] The (meth)acrylic acid ester polymer (A) preferably contains hydroxyl group-containing monomer as a monomer unit constituting the polymer in an amount of 0.01% by mass or more as a lower limit, more preferably 0.1% by mass or more, particularly preferably 0.4% by mass or more, and even more preferably 0.8% by mass or more. The (meth)acrylic acid ester polymer (A) preferably contains hydroxyl group-containing monomer as a monomer unit constituting the polymer in an amount of 10% by mass or less as an upper limit, more preferably 7% by mass or less, particularly preferably 4.8% by mass or less, and even more preferably 1.8% by mass or less. When the (meth)acrylic acid ester polymer (A) contains hydroxyl group-containing monomer as a monomer unit in the above amount, it becomes easier to satisfy the above-mentioned storage modulus G', creep compliance fluctuation value, and creep recovery rate.

[0058] The (meth)acrylic acid ester polymer (A) may not contain a carboxyl group-containing monomer as a monomer unit constituting the polymer, but when it contains a carboxyl group-containing monomer, it is preferable that it contains 0.005% by mass or more, more preferably 0.01% by mass or more, particularly preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more. When the (meth)acrylic acid ester polymer (A) contains a carboxyl group-containing monomer as a monomer unit constituting the polymer, it is preferable that it contains 7% by mass or less as an upper limit, more preferably 4% by mass or less, particularly preferably 1.5% by mass or less, and even more preferably 0.8% by mass or less. When the (meth)acrylic acid ester polymer (A) contains the carboxyl group-containing monomer as a monomer unit in the above amount, the resulting pressure-sensitive adhesive has better flex resistance when applied to a device that is repeatedly flexed.

[0059] The (meth)acrylic acid ester polymer (A) may contain other monomers as monomer units constituting the polymer, if desired. As the other monomers, monomers not containing reactive functional groups are preferred so as not to inhibit the above-mentioned action of the reactive functional group-containing monomer. Examples of such monomers include non-reactive nitrogen atom-containing monomers such as N-acryloylmorpholine and N-vinyl-2-pyrrolidone, (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.

[0060] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.

[0061] The weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 400,000 or more, more preferably 700,000 or more, particularly preferably 900,000 or more, and even more preferably 1,100,000 or more. This can prevent the storage modulus G' from decreasing at high temperatures and contribute to a decrease in the creep compliance fluctuation value. On the other hand, the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 3,000,000 or less, more preferably 2,000,000 or less, particularly preferably 1,700,000 or less, and even more preferably 1,400,000 or less. This can prevent the storage modulus G' from becoming too high at low temperatures. The weight average molecular weight in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0062] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more kinds.

[0063] (1-2) Low molecular weight component (B) The low molecular weight component (B) may be any component having the above-mentioned weight average molecular weight and glass transition temperature (Tg), and for example, it is preferable to use an acrylic oligomer, a silicone oligomer, an olefin oligomer, etc. When the adhesive according to the present embodiment is an acrylic adhesive and a (meth)acrylic acid ester polymer (A) is used as the adhesive main agent, it is preferable to use an acrylic oligomer from the viewpoint of compatibility with the (meth)acrylic acid ester polymer (A). By using an acrylic oligomer, the above-mentioned physical properties are more easily satisfied.

[0064] In addition, the low molecular weight component (B) preferably has a reactive functional group. The low molecular weight component (B) has a reactive functional group, which reacts with the functional group of the (meth)acrylic acid ester polymer (A) or the crosslinking agent (C) described later to form a part of the crosslinked structure, thereby obtaining a predetermined cohesive force. As a result, the creep compliance fluctuation value and creep recovery rate described above are more likely to be satisfied. In addition, the low molecular weight component (B) forms a part of the crosslinked structure and is incorporated into the adhesive, thereby suppressing bleeding out from the adhesive and preventing a decrease in adhesive strength.

[0065] Examples of the reactive functional group contained in the low molecular weight component (B) include a hydroxyl group, a carboxyl group, an epoxy group, a thiol group, etc. Among these, a hydroxyl group, which has excellent reactivity with the crosslinking agent (C) described below, particularly with an isocyanate-based crosslinking agent, or an epoxy group, which has excellent reactivity with the carboxyl group contained in the (meth)acrylic acid ester polymer (A), is preferred.

[0066] When the reactive functional group is a hydroxyl group, the amount of the hydroxyl group in the low molecular weight component (B) is preferably 1 to 1000 mgKOH / g, more preferably 5 to 100 mgKOH / g, particularly preferably 10 to 70 mgKOH / g, and even more preferably 15 to 30 mgKOH / g. When the reactive functional group is an epoxy group, the amount of the epoxy group in the low molecular weight component (B) is preferably 0.01 to 100 meq / g, more preferably 0.1 to 10 meq / g, particularly preferably 0.7 to 7 meq / g, and even more preferably 1.2 to 3 meq / g.

[0067] The acrylic oligomer is a polymer of one or more acrylic monomers and, if desired, other monomers. The acrylic oligomer preferably contains, as monomer units constituting the oligomer, an alkyl (meth)acrylate ester and a monomer containing a reactive functional group.

[0068] The content of the low molecular weight component (B) in the adhesive composition P is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, particularly preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This can contribute to lowering the storage modulus G' of the resulting adhesive, particularly the storage modulus G'(-30) at -30°C. In addition, the content is preferably 80 parts by mass or less, more preferably 50 parts by mass or less, particularly preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less. This can suppress an increase in creep compliance fluctuation value and a decrease in adhesive strength due to bleed-out, etc.

[0069] (1-3) Crosslinking agent (C) The crosslinking agent (C) crosslinks the (meth)acrylic acid ester polymer (A), or the (meth)acrylic acid ester polymer (A) and the low molecular weight component (B), to form a three-dimensional network structure, triggered by heating the adhesive composition P containing the crosslinking agent (C). This improves the cohesive strength of the resulting adhesive, making it easier to satisfy the creep compliance fluctuation value and creep recovery rate described above.

[0070] The crosslinking agent (C) may be any that reacts with the reactive functional group possessed by the (meth)acrylic acid ester polymer (A), or the (meth)acrylic acid ester polymer (A) and the low molecular weight component (B), and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, ammonium salt-based crosslinking agents, etc. The crosslinking agent (C) may be used alone or in combination of two or more.

[0071] Among the above, isocyanate-based crosslinking agents are particularly excellent in reactivity with hydroxyl groups, and epoxy-based crosslinking agents are particularly excellent in reactivity with carboxyl groups. Therefore, when the (meth)acrylic acid ester polymer (A) and / or the low molecular weight component (B) have hydroxyl groups, it is preferable to use an isocyanate-based crosslinking agent, and when the (meth)acrylic acid ester polymer (A) and / or the low molecular weight component (B) have carboxyl groups, it is preferable to use an epoxy-based crosslinking agent. In addition, when the (meth)acrylic acid ester polymer (A) has hydroxyl groups and carboxyl groups, it is preferable to use an isocyanate-based crosslinking agent and an epoxy-based crosslinking agent in combination.

[0072] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate, and their biuret and isocyanurate forms, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate or trimethylolpropane-modified xylylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.

[0073] Examples of epoxy crosslinking agents include 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, etc. Among these, N,N,N',N'-tetraglycidyl-m-xylylenediamine is preferred from the viewpoint of reactivity with carboxy groups.

[0074] The content of the crosslinking agent (C) in the adhesive composition P is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, particularly preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 30 parts by mass or less, more preferably 10 parts by mass or less, particularly preferably 5 parts by mass or less, and even more preferably 1 part by mass or less. When the content of the crosslinking agent (C) is within the above range, the creep compliance fluctuation value and creep recovery rate described above are easily satisfied.

[0075] When an isocyanate-based crosslinking agent and an epoxy-based crosslinking agent are used in combination, the content of the isocyanate-based crosslinking agent in the adhesive composition P is preferably 0.0009 parts by mass or more, more preferably 0.009 parts by mass or more, particularly preferably 0.09 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 20 parts by mass or less, more preferably 9 parts by mass or less, particularly preferably 4 parts by mass or less, and even more preferably 0.8 parts by mass or less.

[0076] When an isocyanate-based crosslinking agent and an epoxy-based crosslinking agent are used in combination, the content of the epoxy-based crosslinking agent in the adhesive composition P is preferably 0.0001 parts by mass or more, more preferably 0.001 parts by mass or more, particularly preferably 0.01 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 10 parts by mass or less, more preferably 1 part by mass or less, particularly preferably 0.8 parts by mass or less, and even more preferably 0.4 parts by mass or less.

[0077] (1-4) Various additives If desired, various additives that are commonly used in acrylic adhesives, such as a silane coupling agent, an ultraviolet absorber, an antistatic agent, a tackifier, an antioxidant, a light stabilizer, a softener, a filler, a refractive index adjuster, etc., can be added to the adhesive composition P. Note that polymerization solvents and dilution solvents described below are not included in the additives that constitute the adhesive composition P.

[0078] The pressure-sensitive adhesive composition P preferably contains the above-mentioned silane coupling agent, which improves the adhesion of the resulting pressure-sensitive adhesive layer to the flexible member that is the adherend, and provides more preferable adhesive strength.

[0079] The silane coupling agent is preferably an organosilicon compound having at least one alkoxysilyl group in the molecule, which has good compatibility with the (meth)acrylic acid ester polymer (A) and has optical transparency.

[0080] Examples of such silane coupling agents include polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; epoxy structure-containing silicon compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; Examples of the silane include capryl group-containing silicon compounds, amino group-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane, or condensates of at least one of these with alkyl group-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane. These may be used alone or in combination of two or more.

[0081] The content of the silane coupling agent in the adhesive composition P is preferably 0.01 parts by mass or more, particularly preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 1 part by mass or less, particularly preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less. When the content of the silane coupling agent is within the above range, the adhesive layer obtained has improved adhesion to the flexible member, which is the adherend, and has greater adhesive strength.

[0082] (2) Preparation of adhesive composition P The adhesive composition P can be produced by producing a (meth)acrylic acid ester polymer (A), mixing the obtained (meth)acrylic acid ester polymer (A) with a low molecular weight component (B) and, if desired, a crosslinking agent (C), and further adding additives, if desired.

[0083] The (meth)acrylic acid ester polymer (A) can be produced by polymerizing a mixture of monomers constituting the polymer by a normal radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) is preferably carried out by a solution polymerization method using a polymerization initiator as desired. By polymerizing the (meth)acrylic acid ester polymer (A) by a solution polymerization method, it becomes easy to increase the molecular weight of the obtained polymer and adjust the molecular weight distribution. Therefore, the pressure-sensitive adhesive is less likely to become biased due to long-term bending, and the recovery from a bent state is more excellent.

[0084] Examples of the polymerization solvent used in the solution polymerization method include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, and methyl ethyl ketone, and two or more of these may be used in combination.

[0085] Examples of the polymerization initiator include azo compounds and organic peroxides, and two or more of them may be used in combination. Examples of the azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane 1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].

[0086] Examples of organic peroxides include benzoyl peroxide, t-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, (3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide.

[0087] In the above polymerization step, the weight average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.

[0088] After the (meth)acrylic acid ester polymer (A) is obtained, the low molecular weight component (B), and optionally the crosslinking agent (C), additives and dilution solvent are added to the solution of the (meth)acrylic acid ester polymer (A) and thoroughly mixed to obtain a pressure-sensitive adhesive composition P (coating solution) diluted with the solvent.

[0089] In addition, when any of the above components is used in a solid state, or when precipitation occurs when the component is mixed with other components in an undiluted state, the component may be dissolved or diluted in a dilution solvent before being mixed with the other components.

[0090] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0091] The concentration and viscosity of the coating solution thus prepared are not particularly limited as long as they are within the range that allows coating, and can be appropriately selected according to the situation. For example, the adhesive composition P is diluted so that the concentration becomes 10 to 60 mass %. In addition, when obtaining the coating solution, the addition of a dilution solvent or the like is not a necessary condition, and if the adhesive composition P has a viscosity that allows coating, it is not necessary to add a dilution solvent. In this case, the adhesive composition P becomes a coating solution in which the polymerization solvent of the (meth)acrylic acid ester polymer (A) itself serves as the dilution solvent.

[0092] (3) Manufacture of adhesives The adhesive according to the present embodiment is preferably obtained from the adhesive composition P, and more preferably obtained by crosslinking the adhesive composition P. The crosslinking of the adhesive composition P can usually be carried out by a heat treatment. This heat treatment can also serve as a drying treatment for volatilizing a diluting solvent and the like from a coating film of the adhesive composition P applied to a desired object.

[0093] The heating temperature in the heat treatment is preferably 50 to 150° C., and more preferably 70 to 120° C. The heating time is preferably 10 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes.

[0094] After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23°C, 50% RH) as necessary. If this curing period is required, the adhesive is formed after the curing period has elapsed, and if no curing period is required, the adhesive is formed after the heat treatment is completed.

[0095] By the above-mentioned heat treatment (and curing), the (meth)acrylic acid ester polymer (A), or the (meth)acrylic acid ester polymer (A) and the low molecular weight component (B), are sufficiently crosslinked via the crosslinking agent (C) to form a crosslinked structure, thereby obtaining a pressure-sensitive adhesive.

[0096] In the pressure-sensitive adhesive according to the present embodiment, it is preferable to lower the storage modulus G', particularly at low temperatures, by lowering the glass transition temperature (Tg) of the (meth)acrylic acid ester polymer (A) and adding a low molecular weight component (B), while lowering the creep compliance fluctuation value by thoroughly crosslinking. This makes it easier to achieve both the storage modulus G' at -30°C (-30) and the creep compliance fluctuation value.

[0097] [Adhesive sheet] The adhesive sheet of this embodiment has an adhesive layer for bonding one flexible member and another flexible member that constitute a repeatedly bending device, and the adhesive layer is made of the adhesive described above.

[0098] FIG. 1 shows a specific configuration of one example of the pressure-sensitive adhesive sheet according to this embodiment. 1, an adhesive sheet 1 according to one embodiment is composed of two release sheets 12a, 12b and an adhesive layer 11 sandwiched between the two release sheets 12a, 12b so as to be in contact with the release surfaces of the two release sheets 12a, 12b. In this specification, the release surface of a release sheet refers to a surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without being subjected to a release treatment.

[0099] (1) Components (1-1) Adhesive layer The adhesive layer 11 is made of the adhesive according to the above-mentioned embodiment, and is preferably made of an adhesive obtained by crosslinking the adhesive composition P.

[0100] The thickness of the adhesive layer 11 in the adhesive sheet 1 according to this embodiment (measured according to JIS K7130) is preferably 1 μm or more as a lower limit, more preferably 5 μm or more, particularly preferably 10 μm or more, and even more preferably 15 μm or more. When the lower limit of the thickness of the adhesive layer 11 is as above, the desired adhesive strength is easily exerted, and lifting or peeling is less likely to occur at the interface between the adhesive layer and the adherend. In addition, the thickness of the adhesive layer 11 is preferably 300 μm or less as an upper limit, more preferably 150 μm or less, particularly preferably 90 μm or less, and from the viewpoint of obtaining a thinner repeatedly bent device, it is further preferably 40 μm or less. When the upper limit of the thickness of the adhesive layer 11 is as above, the adhesive layer and the adherend are easily maintained in contact with each other, so that the bending resistance is more excellent, and the stress applied to the adhesive layer is relatively small, so that the adhesive layer is easily restored from the bent state. The pressure-sensitive adhesive layer 11 may be formed as a single layer, or may be formed by laminating a plurality of layers.

[0101] (1-2) Release sheet Release sheets 12a and 12b protect adhesive layer 11 until adhesive sheet 1 is used, and are peeled off when adhesive sheet 1 (adhesive layer 11) is to be used. In adhesive sheet 1 according to this embodiment, one or both of release sheets 12a and 12b are not necessarily required.

[0102] Examples of the release sheets 12a and 12b include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester copolymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these films are also used. Furthermore, laminated films of these films may be used.

[0103] The release surfaces of the release sheets 12a and 12b (particularly the surfaces in contact with the adhesive layer 11) are preferably subjected to a release treatment. Examples of release agents used in the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents. It is preferable that one of the release sheets 12a and 12b is a heavy release type release sheet having a large release strength, and the other is a light release type release sheet having a small release strength.

[0104] There is no particular limitation on the thickness of the release sheets 12a and 12b, but it is usually about 20 to 150 μm.

[0105] (2) Physical properties (2-1) Haze value The haze value of the pressure-sensitive adhesive layer 11 in the pressure-sensitive adhesive sheet 1 according to this embodiment is preferably 30% or less, more preferably 10% or less, particularly preferably 1% or less, and even more preferably 0.8% or less. This makes it possible to suppress changes in the appearance of the pressure-sensitive adhesive layer 11 due to bending. There is no particular restriction on the lower limit of the haze value, but it is preferably 0% or more, more preferably 0.01% or more, and particularly preferably 0.03% or more. The haze value in this specification is a value measured in accordance with JIS K7136:2000.

[0106] (2-2) Adhesive strength The adhesive strength of the adhesive sheet 1 according to the present embodiment to soda lime glass is preferably 0.1 N / 25 mm or more as a lower limit, more preferably 1.0 N / 25 mm or more, particularly preferably 1.3 N / 25 mm or more, and even more preferably 1.4 N / 25 mm or more. When the lower limit of the adhesive strength of the adhesive sheet 1 is as described above, lifting or peeling due to bending at the interface between the adhesive layer and the adherend is less likely to occur. On the other hand, the upper limit of the adhesive strength is not particularly limited, but is usually preferably 60 N / 25 mm or less, more preferably 40 N / 25 mm or less, and from the viewpoint of reworkability that allows the adhesive sheet to be reattached when the adhesive sheet is misattached, it is particularly preferably 20 N / 25 mm or less, and even more preferably 10 N / 25 mm or less. In addition, the adhesive strength in this specification basically refers to the adhesive strength measured by the 180-degree peeling method in accordance with JIS Z0237:2009, and the specific test method is as shown in the test example described later.

[0107] (3) Manufacturing of adhesive sheets As an example of manufacturing the adhesive sheet 1, a case where the adhesive composition P is used will be described. A coating solution of the adhesive composition P is applied to the release surface of one of the release sheets 12a (or 12b), and a heat treatment is performed to thermally crosslink the adhesive composition P to form a coating layer, and then the release surface of the other release sheet 12b (or 12a) is superimposed on the coating layer. If a curing period is required, a curing period is left, and if no curing period is required, the coating layer becomes the adhesive layer 11 as is. In this way, the adhesive sheet 1 is obtained. The conditions for the heat treatment and curing are as described above.

[0108] In another manufacturing example of the adhesive sheet 1, a coating solution of the adhesive composition P is applied to the release surface of one release sheet 12a, and a heat treatment is performed to thermally crosslink the adhesive composition P to form a coating layer, thereby obtaining a release sheet 12a with a coating layer. Also, a coating solution of the adhesive composition P is applied to the release surface of the other release sheet 12b, and a heat treatment is performed to thermally crosslink the adhesive composition P to form a coating layer, thereby obtaining a release sheet 12b with a coating layer. Then, the release sheet 12a with a coating layer and the release sheet 12b with a coating layer are bonded together so that both coating layers come into contact with each other. If a curing period is required, a curing period is provided, and if a curing period is not required, the laminated coating layer becomes the adhesive layer 11 as it is. This results in the above-mentioned adhesive sheet 1. According to this manufacturing example, even if the adhesive layer 11 is relatively thick, it is possible to stably manufacture it.

[0109] The coating solution of the pressure-sensitive adhesive composition P can be applied by, for example, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, or the like.

[0110] [Repeatedly bent laminated member] As shown in FIG. 2, the repeatedly bent laminated member 2 of this embodiment is composed of a first bending member 21 (one bending member), a second bending member 22 (another bending member), and an adhesive layer 11 located between them and bonding the first bending member 21 and the second bending member 22 to each other.

[0111] The pressure-sensitive adhesive layer 11 in the repeatedly folded laminated member 2 is made of the pressure-sensitive adhesive described above, or is the pressure-sensitive adhesive layer 11 of the pressure-sensitive adhesive sheet 1 described above.

[0112] The repeatedly bent laminated member 2 is a repeatedly bent device itself, or is a member constituting a part of a repeatedly bent device. The repeatedly bent device is preferably a display that can be repeatedly bent (including folding), but is not limited thereto. Examples of such repeatedly bent devices include organic electroluminescence (organic EL) displays, electrophoretic displays (electronic paper), liquid crystal displays using a plastic substrate (film) as a substrate, foldable displays, and the like, and may also be touch panels.

[0113] The first flexible member 21 and the second flexible member 22 are members that can be repeatedly bent (including folded), and examples thereof include a cover film, a barrier film, a hard coat film, a polarizing film (polarizing plate), a polarizer, a retardation film (retardation plate), a viewing angle compensation film, a brightness enhancement film, a contrast enhancement film, a diffusion film, a semi-transmissive reflective film, an electrode film, a transparent conductive film, a metal mesh film, a film sensor (touch sensor film), a liquid crystal polymer film, a light-emitting polymer film, a film-like liquid crystal module, an organic EL module (organic EL film, organic EL element), an electronic paper module (film-like electronic paper), and a TFT (Thin Film Transistor) substrate.

[0114] The Young's modulus of the first bending member 21 and the second bending member 22 is preferably 0.1 to 10 GPa, particularly preferably 0.5 to 7 GPa, and further preferably 1 to 5 GPa. When the Young's modulus of the first bending member 21 and the second bending member 22 is within this range, it becomes easy to repeatedly bend each bending member.

[0115] The thickness of each of the first flexible member 21 and the second flexible member 22 is preferably 10 to 3000 μm, particularly preferably 25 to 1000 μm, and further preferably 50 to 500 μm. When the thicknesses of the first flexible member 21 and the second flexible member 22 are within this range, it becomes easy to repeatedly bend each flexible member.

[0116] To manufacture the above-mentioned repeatedly bent laminated member 2, as an example, one release sheet 12a of the adhesive sheet 1 is peeled off and the exposed adhesive layer 11 of the adhesive sheet 1 is attached to one surface of the first flexible member 21.

[0117] Thereafter, the other release sheet 12b is peeled off from the adhesive layer 11 of the adhesive sheet 1, and the exposed adhesive layer 11 of the adhesive sheet 1 is bonded to the second flexible member 22 to obtain the repeatedly bent laminated member 2. As another example, the bonding order of the first flexible member 21 and the second flexible member 22 may be reversed.

[0118] [Repeated bending device] The repeatedly bent device according to this embodiment includes the repeatedly bent laminate member 2, and may be composed of only the repeatedly bent laminate member 2, or may include one or more repeatedly bent laminate members 2 and other flexible members. When one repeatedly bent laminate member 2 and another repeatedly bent laminate member 2 are laminated, or when the repeatedly bent laminate member 2 and another flexible member are laminated, it is preferable to laminate them via the adhesive layer 11 of the adhesive sheet 1 described above.

[0119] In the repeatedly bent device according to this embodiment, the adhesive layer is made of the above-mentioned adhesive, so that when the device is repeatedly bent or when the device is left in a bent state for a long period of time, lifting or peeling is unlikely to occur at the interface between the adhesive layer 11 and the adherend (the first flexible member 21 and the second flexible member 22). In addition, when the adhesive constituting the adhesive layer 11 satisfies the above-mentioned creep recovery rate, the device is also excellent in recovery from a bent state.

[0120] A repeatedly bending device as an example of this embodiment is shown in Fig. 3. Note that the repeatedly bending device according to the present invention is not limited to this repeatedly bending device.

[0121] 3, the repeatedly bent device 3 according to this embodiment is configured by laminating, from the top, a cover film 31, a first adhesive layer 32, a polarizing film 33, a second adhesive layer 34, a touch sensor film 35, a third adhesive layer 36, an organic EL element 37, a fourth adhesive layer 38, and a TFT substrate 39. The cover film 31, the polarizing film 33, the touch sensor film 35, the organic EL element 37, and the TFT substrate 39 correspond to the flexible member.

[0122] At least one of the first adhesive layer 32, the second adhesive layer 34, the third adhesive layer 36, and the fourth adhesive layer 38 is the adhesive layer 11 of the adhesive sheet 1 described above. It is preferable that two or more of the first adhesive layer 32, the second adhesive layer 34, the third adhesive layer 36, and the fourth adhesive layer 38 are the adhesive layer 11 of the adhesive sheet 1 described above, and it is most preferable that all of the adhesive layers 32, 34, 36, and 38 are the adhesive layer 11 of the adhesive sheet 1.

[0123] The above-described embodiments are described for the purpose of facilitating understanding of the present invention, and are not described for the purpose of limiting the present invention. Therefore, each element disclosed in the above embodiment is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0124] For example, either one or both of release sheets 12a, 12b in pressure-sensitive adhesive sheet 1 may be omitted, and a desired flexible member may be laminated in place of release sheets 12a and / or 12b. EXAMPLES

[0125] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0126] Example 1 1. Preparation of (meth)acrylic acid ester polymer (A) 98.5 parts by mass of 2-ethylhexyl acrylate, 1.0 parts by mass of 4-hydroxybutyl acrylate, and 0.5 parts by mass of acrylic acid were copolymerized by a solution polymerization method to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of this (meth)acrylic acid ester polymer (A) was measured by the method described below, and the weight average molecular weight (Mw) was 1.2 million.

[0127] 2. Preparation of adhesive composition 100 parts by mass (solid content equivalent; the same applies below) of the (meth)acrylic acid ester polymer (A) obtained in the above step 1 and a hydroxyl group-containing acrylic oligomer (B1; product name "ARUFON (registered trademark)" manufactured by Toagosei Co., Ltd.) as a low molecular weight component (B) were mixed. 15 parts by mass of 1,2-dimethyl-2,4-diphenyl-2,4-diphenyl-1,1-diisocyanate (UH-2000, hydroxyl group content: 20 mg KOH / g, Mw: 11000, Tg: -55°C) was mixed as an isocyanate-based crosslinking agent (C1) with 0.3 parts by mass of trimethylolpropane-modified xylylene diisocyanate (XDI; manufactured by Soken Chemical Industries, Ltd., product name "TD-75"), as an epoxy-based crosslinking agent (C2) with 0.2 parts by mass of N,N,N',N'-tetraglycidyl-m-xylylene diamine, as an epoxy-based crosslinking agent (C2), and with 0.2 parts by mass of 3-glycidoxypropyltrimethoxysilane (SC1) as a silane coupling agent, and the mixture was thoroughly stirred and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.

[0128] 3. Manufacturing of adhesive sheets The obtained adhesive composition coating solution was applied by a knife coater to the release-treated surface of a heavy-release type release sheet (manufactured by Lintec Corporation, product name "SP-PET752150"), one side of which was a polyethylene terephthalate film treated with a silicone-based release agent. The coating layer was then heated at 90°C for 1 minute to form a coating layer.

[0129] Next, the coating layer on the heavy release type release sheet obtained above and a light release type release sheet (manufactured by Lintec Corporation, product name "SP-PET381130"), one side of which is a polyethylene terephthalate film treated with a silicone-based release agent, are attached so that the release-treated surface of the light release type release sheet comes into contact with the coating layer, and the sheet is cured for 7 days under conditions of 23°C and 50% RH to produce an adhesive sheet having an adhesive layer with a thickness of 25 μm, that is, an adhesive sheet having a configuration of heavy release type release sheet / adhesive layer (thickness: 25 μm) / light release type release sheet. The thickness of the adhesive layer is a value measured using a constant pressure thickness gauge (manufactured by Techroc Corporation, product name "PG-02") in accordance with JIS K7130.

[0130] Here, the formulations (solid content equivalent) of the pressure-sensitive adhesive composition when the (meth)acrylic acid ester polymer (A) is taken as 100 parts by mass (solid content equivalent) are shown in Table 1. The details of the abbreviations and the like shown in Table 1 are as follows. [(Meth)acrylic acid ester polymer (A)] 2EHA: 2-ethylhexyl acrylate 4HBA: 4-hydroxybutyl acrylate AAc: acrylic acid [Low molecular weight component (B)] B1: Hydroxyl-containing acrylic oligomer (manufactured by Toagosei Co., Ltd., product name "ARUFON (registered trademark) UH-2000", hydroxyl content: 20 mg KOH / g, Mw: 11000, Tg: -55°C) B2: Epoxy group-containing acrylic oligomer (manufactured by Toa Gosei Co., Ltd., product name "ARUFON UG-4010", epoxy group content: 1.4 meq / g, Mw: 2900, Tg: -57°C) B3: Non-functional acrylic oligomer (Toagosei Co., Ltd., product name "ARUFON UP-1000", Mw: 3000, Tg: -77℃) [Isocyanate-based crosslinking agent (C1)] XDI: Trimethylolpropane modified xylylene diisocyanate (manufactured by Soken Chemical Industries, Ltd., product name "TD-75") TDI: Trimethylolpropane modified tolylene diisocyanate (manufactured by Toyochem Co., Ltd., product name "BHS8515") [Epoxy-based crosslinking agent (C2)] N,N,N',N'-Tetraglycidyl-m-xylylenediamine [Silane coupling agents] SC1: 3-glycidoxypropyltrimethoxysilane SC2: 1,6-bis(trimethoxysilyl)hexane

[0131] [Examples 2 to 4, Comparative Examples 1 to 4] An adhesive sheet was produced in the same manner as in Example 1, except that the types and ratios of the monomers constituting the (meth)acrylic acid ester polymer (A), the weight average molecular weight (Mw) of the (meth)acrylic acid ester polymer (A), the type and amount of the low molecular weight component (B), the type of isocyanate-based crosslinking agent (C1), the amount of the epoxy-based crosslinking agent (C2), and the type of silane coupling agent were changed as shown in Table 1.

[0132] The weight average molecular weight (Mw) mentioned above is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement). <Measurement conditions> GPC measuring device: Tosoh HLC-8020 GPC columns (passed in the following order): Tosoh Corporation TSK guard column HXL-H TSK gel GMHXL (×2) TSK gel G2000HXL Measurement solvent: Tetrahydrofuran ·Measurement temperature: 40℃

[0133] [Test Example 1] (Measurement of gel fraction) The adhesive sheets prepared in the examples and comparative examples were cut to a size of 80 mm x 80 mm, the adhesive layer was wrapped in a polyester mesh (product name: Tetron mesh #200), and the mass was measured using a precision balance. The mass of the mesh alone was subtracted to calculate the mass of the adhesive alone. This mass was designated as M1.

[0134] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The adhesive was then removed and air-dried for 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%, and then dried in an oven at 80°C for 12 hours. After drying, the mass was weighed using a precision balance, and the mass of the adhesive alone was calculated by subtracting the mass of the mesh alone. The mass at this time was designated M2. The gel fraction (%) was expressed as (M2 / M1) x 100. The results are shown in Table 2.

[0135] [Test Example 2] (Measurement of storage modulus G') The pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets prepared in the Examples and Comparative Examples were laminated together to form a laminate having a thickness of 800 μm. A cylindrical body having a diameter of 8 mm (height of 800 μm) was punched out from the resulting laminate of pressure-sensitive adhesive layers to form a sample.

[0136] The storage modulus G' of the above samples was measured under the following conditions by a torsional shear method using a viscoelasticity measuring device (manufactured by Anton Paar, product name "MCR302") in accordance with JIS K7244-6, and the storage modulus G'(-30) at -30°C, the storage modulus G'(25) at 25°C, and the storage modulus G'(85) at 85°C (MPa) were obtained. The results are shown in Table 2. Measurement frequency: 1Hz Heating rate: 5℃ / min Distortion: 1% Normal force: 1.0N Measurement temperature: -30℃~140℃

[0137] Based on the obtained results, the storage modulus change rate (-30 / 25), which is the value obtained by dividing the storage modulus G'(-30) by the storage modulus G'(25), and the storage modulus change rate (-30 / 85), which is the value obtained by dividing the storage modulus G'(-30) by the storage modulus G'(85), were calculated. The results are shown in Table 2.

[0138] [Test Example 3] (Creep Compliance Measurement) The pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets prepared in the Examples and Comparative Examples were laminated together to form a laminate having a thickness of 800 μm. A cylindrical body having a diameter of 8 mm (height of 800 μm) was punched out from the resulting laminate of pressure-sensitive adhesive layers to form a sample.

[0139] A viscoelasticity measuring device (manufactured by Anton Paar, product name "MCR302") was used to continuously apply a stress of 4500 Pa under the following conditions, and the creep compliance J(t) (MPa -1 From the measurement results, the value when a stress of 4500 Pa was applied was determined as the minimum creep compliance J(t) min (MPa -1 ) and the minimum creep compliance J(t) min The maximum creep compliance J(t) measured up to 1200 seconds after max (MPa -1 ) was derived. Measurement temperature: 25℃ Measurement points: 1000 points (logarithmic plot)

[0140] The minimum creep compliance obtained, J(t) min (MPa -1 ) and maximum creep compliance J(t) max (MPa -1 ) and the creep compliance variation value ΔlogJ(t) was calculated based on the following formula (I). The results are shown in Table 2. ΔlogJ(t)=logJ(t) max -logJ(t) min …(I)

[0141] In addition, a viscoelasticity measuring device (manufactured by Anton Paar, product name "MCR302") was used to continuously apply a stress of 4500 Pa to the above sample under the following conditions, and then the applied stress was reduced to 0 Pa and this state was maintained for a while. During this time, the creep compliance J(t) (MPa -1 The creep compliance measured 1200 seconds after the start of the application of a stress of 4500 Pa was defined as creep compliance J(t) (s=1200) (MPa -1 ), and the creep compliance measured 100 seconds after the applied stress was set to 0 Pa was defined as creep compliance J(t) (s = 1300) (MPa -1 ) was decided. Measurement temperature: 25℃ Measurement points when stress is applied: 1000 points (logarithmic plot) Measurement points when stress is removed: 1000 points (logarithmic plot)

[0142] The obtained creep compliance J(t)(s=1200)(MPa -1 ) and creep compliance J(t)(s=1300)(MPa -1 The creep recovery rate (%) was calculated from the above data based on the following formula (II). The results are shown in Table 2. Creep recovery rate (%) = (1-J(t)(s=1300) / J(t)(s=1200)) x 100 ... (II)

[0143] [Test Example 4] (Haze value measurement) The adhesive layer of the adhesive sheet produced in the examples and comparative examples was attached to glass to prepare a measurement sample. After background measurement was performed on the glass, the haze value (%) of the measurement sample was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH5000") in accordance with JIS K7136:2000. The results are shown in Table 2.

[0144] [Test Example 5] (Measurement of adhesive strength) The light release type release sheet was peeled off from the adhesive sheet obtained in the Examples and Comparative Examples, and the exposed adhesive layer was attached to an easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "PET A4300", thickness: 100 μm) having an easy-adhesion layer, to obtain a laminate of heavy release type release sheet / adhesive layer / PET film. The obtained laminate was cut into a width of 25 mm and a length of 110 mm.

[0145] In an environment of 23°C and 50% RH, the heavy release type release sheet was peeled off from the laminate, and the exposed adhesive layer was attached to a soda lime glass plate (manufactured by Nippon Sheet Glass Co., Ltd., product name "Soda Lime Glass", thickness: 1.1 mm), and pressurized for 20 minutes at 0.5 MPa and 50°C in an autoclave manufactured by Kurihara Seisakusho Co., Ltd. After that, it was left for 24 hours under conditions of 23°C and 50% RH, and then the adhesive strength (N / 25mm) was measured when the laminate of the PET film and the adhesive layer was peeled off from the adherend using a tensile tester (manufactured by Orientec Co., Ltd., Tensilon) under conditions of a peel speed of 300 mm / min and a peel angle of 180 degrees. The measurement was performed under conditions other than those described here in accordance with JIS Z0237:2009. The results are shown in Table 2.

[0146] [Test Example 6] (Evaluation of bending resistance) In an environment of 23°C and 50% RH, the light release type release sheet was peeled off from the adhesive sheet produced in the examples and comparative examples, and the exposed adhesive layer was attached to one side of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "PET50TA063", thickness: 100 μm). Next, the heavy release type release sheet was peeled off, and the exposed adhesive layer was attached to a polyimide film (thickness: 50 μm). Then, after pressurizing at 0.5 MPa and 50°C for 20 minutes in an autoclave manufactured by Kurihara Seisakusho Co., Ltd., the laminate was left for 24 hours under conditions of 23°C and 50% RH. The laminate consisting of the PET film / adhesive layer / polyimide film thus obtained was cut into a width of 50 mm and a length of 200 mm, which was used as a sample.

[0147] Both ends of the obtained sample were fixed to two holding plates of a bending tester with a constant temperature and humidity chamber (manufactured by Yuasa System Co., Ltd., product name "CL09-typeD01-FSC90") as shown in Figure 4. At this time, the polyimide film side of the sample was fixed to the inside of the bend. Then, the sample was bent 200,000 times in temperature environments of -30°C, 25°C, and 80°C, with a bending diameter of 3 mmφ, a stroke of 80 mm, and a bending speed of 60 rpm.

[0148] After the dynamic bending test, the sample was visually inspected for peeling at the interface between the adhesive layer and the adherend at the bent portion. The bending resistance was evaluated according to the following criteria. The results are shown in Table 2. ⊚: No traces were present in the bent portion. ○: Line marks are present at the bend, but when viewed from directly in front, the line marks are barely visible. △: Line marks were present at the bent portion, and the line marks were visible even when viewed from the front. Or, minute air bubbles were generated at the bent portion. ×: Lifting and peeling occurred at the bent portion.

[0149] [Table 1]

[0150] [Table 2]

[0151] As can be seen from Table 2, the adhesive layer of the adhesive sheet of the embodiment had excellent flex resistance, and lifting or peeling was unlikely to occur at the interface between the adhesive layer and the adherend when bent for long periods of time, regardless of whether the environment was low, normal, or high temperature. [Industrial Applicability]

[0152] The present invention is suitable for bonding one flexible member and another flexible member that constitute a repeatedly bending device. [Explanation of symbols]

[0153] 1...Adhesive sheet 11...Adhesive layer 12a, 12b...Release sheet 2…Repeatedly bent laminated member 21...First flexible member 22...Second flexible member 3. Repeated bending device 31…Cover film 32...First adhesive layer 33...Polarizing film 34...Second adhesive layer 35...Touch sensor film 36...Third adhesive layer 37...Organic EL element 38...Fourth adhesive layer 39...TFT substrate S: Test piece P…Retaining plate

Claims

1. A pressure-sensitive adhesive for repeatedly bending devices for bonding one flexible member and another flexible member that constitute a device that is repeatedly bent, comprising: The pressure-sensitive adhesive has a storage modulus G'(-30) of 0.20 MPa or less at -30 ° C.; The creep compliance value measured when a stress of 4500 Pa is applied to the adhesive is defined as the minimum creep compliance J(t). min (MPa -1 ) and the minimum creep compliance J(t) min The stress of 4500 Pa was applied until 1200 seconds after the measurement, and the maximum creep compliance value measured during that time was defined as the maximum creep compliance J(t). max (MPa -1 ) and the creep compliance fluctuation value ΔlogJ(t) calculated from the following formula (I) is 2.60 or less.

1. A pressure-sensitive adhesive for use in a repeatedly flexed device. ΔlogJ(t)=logJ(t) max −log J(t) min … (I)

2. The creep compliance value measured after 1200 seconds of continuously applying a stress of 4500 Pa to the adhesive was defined as creep compliance J(t) (s=1200) (MPa -1 ), and then the stress applied to the pressure-sensitive adhesive is set to 0 Pa, and the creep compliance value measured 100 seconds later is defined as creep compliance J(t) (s=1300) (MPa -1 2. The pressure-sensitive adhesive for repeated flexion devices according to claim 1, characterized in that the creep recovery rate calculated from the following formula (II) is 90% or more: Creep recovery rate (%) = (1 - J (t) (s = 1300) / J (t) (s = 1200)) x 100 ... (II)

3. The pressure-sensitive adhesive for repeated flexion devices according to claim 1 or 2, characterized in that the pressure-sensitive adhesive has a storage modulus G'(85) at 85°C of 0.005 MPa or more.

4. The pressure-sensitive adhesive for repeated bending devices according to any one of claims 1 to 3, characterized in that the storage modulus change rate (-30 / 25), which is the value obtained by dividing the storage modulus G'(-30) at -30 ° C. by the storage modulus G'(25) at 25 ° C., is 5.0 or less.

5. The pressure-sensitive adhesive for repeated bending devices according to any one of claims 1 to 4, characterized in that the storage modulus change rate (-30 / 85), which is the value obtained by dividing the storage modulus G'(-30) at -30 ° C. by the storage modulus G'(85) at 85 ° C., is 10.0 or less.

6. The pressure-sensitive adhesive for repeated bending devices according to any one of claims 1 to 5, characterized in that the pressure-sensitive adhesive has a gel fraction of 40% or more and 95% or less.

7. The pressure-sensitive adhesive contains a main adhesive agent and a low molecular weight component, The weight average molecular weight of the low molecular weight component is 400 or more and 100,000 or less, The glass transition temperature (Tg) of the low molecular weight component is −40° C. or lower. The pressure-sensitive adhesive for repeated bending devices according to any one of claims 1 to 6.

8. The pressure-sensitive adhesive for repeated bending devices according to any one of claims 1 to 7, characterized in that the pressure-sensitive adhesive is an acrylic pressure-sensitive adhesive.

9. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding one flexible member and another flexible member that constitute a device that is repeatedly bent, The pressure-sensitive adhesive layer is made of the pressure-sensitive adhesive for repeated bending devices according to any one of claims 1 to 8. A pressure-sensitive adhesive sheet characterized by:

10. The pressure-sensitive adhesive sheet has two release sheets, The pressure-sensitive adhesive layer is sandwiched between the two release sheets so as to be in contact with the release surfaces of the release sheets. The pressure-sensitive adhesive sheet according to claim 9 .

11. A flexible member and another flexible member that constitute a device that is repeatedly bent; a pressure-sensitive adhesive layer that bonds the first flexible member and the second flexible member to each other; A repeatedly bent laminated member comprising: The pressure-sensitive adhesive layer is made of the pressure-sensitive adhesive for repeated bending devices according to any one of claims 1 to 8. A repeatedly bent laminated member characterized in that

12. A repeatedly flexed device comprising the repeatedly flexed laminate member according to claim 11.

Citation Information

Patent Citations

  • Adhesive for optical film, adhesive layer for optical film, optical member and image display device

    JP2016108555A

  • Adhesive composition, adhesive layer, adhesive sheet and image display device

    JP2017095655A

  • Adhesive for repeatedly bending device, adhesive sheet, repeatedly bending laminate member, and repeatedly bending device

    JP2019108502A

  • Laminate, adhesive layer, and adhesive sheet

    JP2020131565A

  • Adhesive for repeated bending device, adhesive sheet, repeated bending laminate member and repeated bending device

    JP2020139036A