Adhesive method, strain measurement method and adhesive
A bonding method with a specialized adhesive composition and thermal properties addresses crack issues in glass-based strain sensors, ensuring reliable adhesion and strain measurement in high-temperature environments.
Patent Information
- Application Number
- JP2021142661
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-01
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2041-09-01
AI Technical Summary
Cracks occur in glass-based strain sensors bonded to base materials due to significant differences in thermal expansion coefficients when subjected to repeated cooling and heating cycles, especially in high-temperature environments like exhaust gas purification devices.
A bonding method using an adhesive composed of glass powder, solvent, and binder, with specific viscosity and thermal expansion coefficient properties, applied and baked at 850°C to 1000°C, to minimize thermal stress and prevent cracking.
The method effectively suppresses crack formation in glass-based strain sensors during repeated thermal cycles, ensuring reliable adhesion and strain measurement in high-temperature conditions.
Smart Images

Figure 0007576526000002 
Figure 0007576526000003 
Figure 0007576526000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a bonding method, a strain measuring method, and an adhesive. [Background technology]
[0002] In recent years, in order to reduce adverse environmental impacts, exhaust gas purification equipment that purifies harmful substances in exhaust gases using a catalyst supported on a base material has been used. In exhaust gas purification equipment, high-temperature exhaust gas flows through the base material, so the base material is repeatedly subjected to a heat-cooling cycle in which the temperature rises to around 800°C and then falls to room temperature.
[0003] On the other hand, optical fiber sensors are known as strain sensors capable of measuring the strain of a base material at temperatures around 800° C. Optical fiber sensors are usually used by bonding them with an adhesive.
[0004] Patent Document 1 describes a glass composition for sealing that is substantially free of boron oxide and barium oxide and contains 43-53 mol% of SiO2, 12-33 mol% of CaO, 12-33 mol% of MgO, 1-7 mol% of La2O3, and 0-4.5 mol% of ZnO. The glass composition for sealing is fired in the form of powder at a temperature of 900-1150°C, thereby obtaining a thermal expansion coefficient of 80-110×10 at 50-850°C. -7 This results in a crystallized glass exhibiting a temperature of 100 / °C. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2018 / 066635 Summary of the Invention [Problem to be solved by the invention]
[0006] However, when there is a large difference in thermal expansion coefficient between the base material and the crystallized glass, repeated thermal cycling of the base material to which the strain sensor is attached can cause cracks in the crystallized glass.
[0007] An object of the present invention is to provide a bonding method capable of suppressing the occurrence of cracks in the glass even when the base material to which a strain sensor is bonded is subjected to repeated thermal cycles. [Means for solving the problem]
[0008] One aspect of the present invention is a method for bonding a strain sensor to a base material, the method comprising: applying an adhesive to the strain sensor in a state in which the strain sensor is placed on the base material; and then firing the adhesive at a temperature of 850° C. to 1000° C.; the adhesive contains a glass powder, a solvent, and a binder; a glass powder content is 60 mass % to 86 mass %; the glass powder has a viscosity of less than 7.6 dPa s at 800° C.; glass obtained by firing the glass powder at 850° C. has a viscosity of 7.6 dPa s or more at 800° C.; and a difference in thermal expansion coefficient between the base material and the glass obtained by firing the glass powder at 850° C. at a temperature of 20° C. to 800° C. is 2.5×10 -6 / K or less.
[0009] The glass powder may contain B2O3 as a main component, any one of BaO, CaO and MgO, SiO2 and Al2O3.
[0010] The glass powder may have a viscosity at 850° C. of 4.0 dPa·s or more.
[0011] The strain sensor may be a fiber optic sensor.
[0012] The base material has a thermal expansion coefficient of 1.23×10 at a temperature of 100° C. or higher and 800° C. or lower. -5 / K or more 1.33×10 -5 / K or less.
[0013] The solvent may contain terpineol.
[0014] The binder may contain ethyl cellulose.
[0015] Another aspect of the present invention is a strain measurement method including the steps of bonding the strain sensor to a base material by the above-described bonding method, and measuring the strain of the base material to which the strain sensor is bonded.
[0016] In another aspect of the present invention, an adhesive contains a glass powder, a solvent, and a binder, the glass powder content being 60% by mass or more and 86% by mass or less, the glass powder has a viscosity of less than 7.6 dPa·s at 800°C, and glass obtained by firing the glass powder at 850°C has a viscosity of 7.6 dPa·s or more at 800°C.
[0017] The glass powder may have a viscosity at 850° C. of 4.0 dPa·s or more. Effect of the Invention
[0018] According to the present invention, it is possible to provide a bonding method capable of suppressing the occurrence of cracks in the glass even when the base material to which the strain sensor is bonded is subjected to repeated thermal cycles. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 illustrates an example of a device having a base material with a strain sensor adhered thereto. [Diagram 2] FIG. 13 is a diagram showing an example of the measurement results of distortion of a base material of an exhaust gas purification device when the base material is subjected to repeated cooling and heating cycles. [Diagram 3] 4 is a graph showing the relationship between viscosity η and temperature for boron-based glass powder in Examples and for boron-based glass obtained by firing the boron-based glass powder at 850° C. [Figure 4]1 is a graph showing the difference Δα in thermal expansion coefficient α at temperatures of 100° C. or higher and 800° C. or lower between ferritic stainless cast steel in an example and glass obtained by firing boron-based glass powder at 850° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0021] [Adhesion method] The bonding method of this embodiment is a method for bonding a strain sensor to a base material.
[0022] In the bonding method of this embodiment, the strain sensor is placed on a base material, and then an adhesive is applied to the strain sensor, followed by firing at a temperature of 850°C or higher and 1000°C or lower.
[0023] The adhesive contains glass powder, a solvent, and a binder.
[0024] The content of glass powder in the adhesive is preferably 60% by mass or more and 86% by mass or less. If the content of glass powder in the adhesive is less than 60% by mass, the adhesive will have poor applicability, and if it exceeds 86% by mass, the adhesive will become non-uniform.
[0025] The viscosity of the glass powder at 800°C is less than 7.6 dPa·s. If the viscosity of the glass powder at 800°C is 7.6 dPa·s or more, the glass powder will not flow easily when fired at a temperature of 850°C to 1000°C, and the strain sensor will not be able to be properly bonded to the base material.
[0026] The viscosity of the glass powder at 850° C. is preferably 4.0 dPa·s or more. When the viscosity of the glass powder at 850° C. is 4.0 dPa·s or more, the glass powder flows appropriately when fired at a temperature of 850° C. or more and 1000° C. or less.
[0027] The viscosity of glass made by firing glass powder at 850°C at 800°C is 7.6 dPa·s or more. If the viscosity of glass made by firing glass powder at 850°C at 800°C is less than 7.6 dPa·s, the glass will soften when measuring the strain of the base material at temperatures around 800°C, and the strain sensor will not be able to adhere properly to the base material.
[0028] The difference in thermal expansion coefficient (linear expansion coefficient) between the base material and glass made by firing glass powder at 850°C at temperatures between 20°C and 800°C is 2.5×10 -6 / K or less, 2.0×10 -6 The difference in thermal expansion coefficient between the base material and the glass obtained by firing glass powder at 850°C at temperatures of 20°C to 800°C is preferably 2.5×10 -6 If the temperature exceeds 100 °C, repeated thermal cycles will cause the glass to crack when the base material to which the strain sensor is attached is subjected to repeated thermal cycles.
[0029] The glass powder preferably contains B2O3 as a main component, any one of BaO, CaO and MgO, SiO2 and Al2O3.
[0030] In this specification and claims, the term "main component" refers to the component that is contained in the largest amount by mass.
[0031] The content of B2O3 in the glass powder is not particularly limited, but is, for example, from 5% by mass to 40% by mass.
[0032] The content of any one of BaO, CaO and MgO in the glass powder is not particularly limited, but is, for example, 0.01% by mass or more and 70% by mass or less.
[0033] The content of SiO2 in the glass powder is not particularly limited, but is, for example, from 0.5% by mass to 40% by mass.
[0034] The content of Al2O3 in the glass powder is not particularly limited, but is, for example, from 0.1 mass % to 30 mass %.
[0035] The solvent is not particularly limited, but examples thereof include terpineol and the like.
[0036] The binder is not particularly limited, but examples thereof include ethyl cellulose.
[0037] The adhesive may further contain a dispersant.
[0038] The dispersant is not particularly limited, but examples thereof include non-ionic surfactants such as glycerin fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and polyoxysulfitol fatty acid esters.
[0039] The strain sensor is not particularly limited as long as it is capable of measuring the strain of the base material at a temperature of about 800° C., and examples thereof include an optical fiber sensor.
[0040] The thermal expansion coefficient of the base material at temperatures between 100°C and 800°C is 1.07×10 -5 / K or more 1.28×10 -5 It is preferable that the value is equal to or less than 1 / K.
[0041] The material constituting the base material is not particularly limited, but examples thereof include ferritic stainless steel.
[0042] The base material may be a component constituting an apparatus such as an exhaust gas purification apparatus.
[0043] [Distortion measurement method] The strain measurement method of this embodiment includes a step of bonding a strain sensor to a base material by the bonding method of this embodiment, and a step of measuring the strain of the base material to which the strain sensor is bonded.
[0044] FIG. 1 shows an exhaust gas purification device as an example of a device having a base material to which a strain sensor is bonded.
[0045] The exhaust gas purification device 10 includes a base material 11 carrying a catalyst that purifies harmful substances in exhaust gas, and an optical fiber sensor 12 bonded to the base material 11 .
[0046] The strain of the base material 11 to which the optical fiber sensor 12 is bonded can be measured, for example, by using a known strain measuring device.
[0047] FIG. 2 shows an example of the measurement results of the distortion of the base material 11 when the base material 11 is subjected to repeated thermal cycles.
[0048] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the above embodiment may be modified as appropriate within the scope of the spirit of the present invention. EXAMPLES
[0049] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0050] [Examples 1 and 2, Comparative Example 1] A boron-based glass powder containing a specified amount (see Table 1) of B2O3 as the main component, BaO, CaO, or MgO, SiO2, and Al2O3, an appropriate amount of terpineol (manufactured by Nippon Fragrance Pharmaceuticals), Ethocel STD100IND (manufactured by Nisshin Kasei) as ethyl cellulose, and Rheodol TW-0106V as polyoxyethylene sorbitan monooleate were mixed together to obtain an adhesive. Here, the adhesive of Comparative Example 1 was non-uniform.
[0051] [Table 1] Figure 3 shows the relationship between viscosity η and temperature for boron-based glass powder and for boron-based glass obtained by firing the boron-based glass powder at 850°C. Here, the boron-based glass powder used in measuring the viscosity and the boron-based glass powder used in firing are compacts.
[0052] From FIG. 3, it can be seen that the viscosity of boron-based glass powder at 800°C is less than 7.6 dPa·s, and that the viscosity of boron-based glass obtained by firing boron-based glass powder at 850°C is 7.6 dPa·s or more at 800°C.
[0053] With the optical fiber sensor placed on a base material made of ferritic stainless cast steel, an adhesive was applied to the optical fiber sensor using a dispenser, and then the sensor was baked for 1 hour at 850°C to bond the optical fiber sensor to the base material. At this time, a steel plate and a steel pipe were used as the base materials to which the adhesive was applied in Example 1 and Example 2, respectively.
[0054] Figure 4 shows the difference Δα in thermal expansion coefficient α at temperatures between 100°C to 800°C between ferritic stainless cast steel and glass made by firing boron-based glass powder at 850°C. Here, the thermal expansion coefficient α of ferritic stainless cast steel at temperatures between 100°C to 800°C is 1.07×10 -5 / K or more 1.28×10 -5 / K or less.
[0055] From Figure 4, Δα is 2.5×10 -6 It can be seen that this is below / K.
[0056] [Distortion measurement] Using a strain measuring device (commercially available), the strain was measured when the base material to which the optical fiber sensor was attached was subjected to repeated thermal cycles. As a result, no cracks were observed in the glass when either the adhesive of Example 1 or Example 2 was used. [Explanation of symbols]
[0057] 10 Exhaust gas purification equipment 11 Base material 12 Optical fiber sensor
Claims
1. 1. A method for bonding a strain sensor to a base material, comprising: The strain sensor is placed on the base material, and then an adhesive is applied to the strain sensor, followed by firing at a temperature of 850° C. or more and 1000° C. or less; The adhesive contains a glass powder, a solvent, and a binder, and the content of the glass powder is 60% by mass or more and 86% by mass or less, The glass powder contains B 2 O 3 as a main component and has a viscosity of less than 7.6 dPa·s at 800° C.; The glass obtained by firing the glass powder at 850° C. has a viscosity of 7.6 dPa s or more at 800° C., The difference in thermal expansion coefficient between the base material and the glass obtained by firing the glass powder at 850° C. at a temperature of 100° C. to 800° C. is 2.5×10 -6 / K or less.
2. The glass powder contains any one of BaO, CaO and MgO and SiO 2 And, Al 2 O 3 The bonding method according to claim 1 ,
3. 3. The bonding method according to claim 1, wherein the glass powder has a viscosity of 4.0 dPa·s or more at 850°C.
4. The bonding method according to claim 1 , wherein the strain sensor is an optical fiber sensor.
5. The base material has a thermal expansion coefficient of 1.07×10 at a temperature of 100° C. or higher and 800° C. or lower. -5 / K or more 1.28×10 -5 The bonding method according to claim 1 , wherein the viscosity is 0.1 to 0.5 μm.
6. The bonding method according to claim 1 , wherein the solvent contains terpineol.
7. The bonding method according to claim 1 , wherein the binder contains ethyl cellulose.
8. A step of adhering the strain sensor to a base material by the bonding method according to any one of claims 1 to 7; and measuring the strain of the base material to which the strain sensor is adhered.
9. Contains glass powder, a solvent, and a binder; The content of the glass powder is 60% by mass or more and 86% by mass or less, The glass powder contains B 2 O 3 as a main component and has a viscosity of less than 7.6 dPa·s at 800° C.; The adhesive, wherein the glass obtained by firing the glass powder at 850°C has a viscosity of 7.6 dPa·s or more at 800°C.
10. The adhesive according to claim 9 , wherein the glass powder has a viscosity of 4.0 dPa·s or more at 850° C.
Citation Information
Patent Citations
Crystalline glass composition and adhesive material using the same
JP2013056795A
Crystalline glass composition
JP2013241323A
Pressure sensor, method for manufacturing pressure sensor, and mass flow rate control device