Hybrid acoustic interlayers consisting of bonded core layers made from polymer matrix nanocomposites

The use of interpenetrating polymer networks in a three-layer interlayer system addresses the damping and sound insulation challenges of laminated glazing units by enhancing vibration damping and sound insulation, achieving a significant improvement in performance and transparency.

JP7576551B2Active Publication Date: 2024-10-31SAINT-GOBAIN SEKURIT FRANCE THOUROTTE FR
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021541132
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-17
Filing Date
2020-01-14
Publication Date
2024-10-31
Estimated Expiration
2040-01-14

AI Technical Summary

Technical Problem

Existing laminated glazing units face challenges in achieving effective vibration damping and sound insulation in the frequency range of 1Hz to 10kHz due to adjustments in hydroxyl group content of the PVB inner layer affecting the glass transition temperature, leading to reduced performance at ambient temperatures.

Method used

A three-layer interlayer system using interpenetrating polymer networks (IPNs) with specific polymer phases, including polymer nanodomains and a continuous matrix, replaces the conventional PVB inner layer to enhance vibration damping and sound insulation.

Benefits of technology

The IPN-based interlayer achieves a loss factor of 4-6 times higher than conventional PVB, providing superior sound insulation and vibration damping in the frequency range of 1kHz to 10kHz and temperature range of 0°C to 40°C, with improved transparency and mechanical strength.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

In a three-layer intermediate layer, the PVB inner layer is replaced with a layer formed from a specific polymer structure different from PVB, which has a very high damping coefficient (tan δ) at temperatures close to ambient temperature in a frequency decade of 1 kHz to 10 kHz, preferably in the frequency range of 1 Hz to 10 kHz. The present invention relates to an interlayer for laminated glass comprising two outer layers of a material selected from poly(vinyl butyral) (PVB) and poly(ethylene-vinyl acetate) (EVA), assembled by an adhesive nanocomposite layer having: a first discontinuous phase consisting of polymer nanodomains having a glass transition temperature (Tg) of -50°C to -30°C, preferably -45°C to -35°C, and a second continuous polymer phase, referred to as the matrix, having a lower glass transition temperature (Tg) than the first phase, preferably below -50°C, more preferably below -60°C, wherein the first phase is dispersed within the second phase. The present invention also relates to a method for producing the interlayer, and to laminated glazing units comprising an interlayer of this type.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an interlayer having vibration damping properties for laminated glass and to a method for its manufacture. The invention also relates to a laminated glazing unit comprising an interlayer of this type for damping vibration and structure-borne noise from 1 Hz to 1000 Hz and / or for increasing the transmission loss to air-borne noise, especially over the audio frequency decade from 1 kHz to 10 kHz, and to the use of said glazing unit as a vehicle windshield and / or as architectural glazing. [Background technology]

[0002] Laminated glazing units are commonly used in the field of transportation, more specifically in automobile and aircraft windows, as well as in architecture. The function of laminated glazing units is to reduce the risk of debris protrusion in the event of sudden destruction and to delay unauthorized entry. A further advantage of laminated glazing units is to reduce the transmission of UV and / or infrared radiation, as well as to reduce the transmission of noise from the outside to the interior of the vehicle or building, thereby improving the vibration and sound comfort of passengers or occupants.

[0003] Laminated glazing units generally consist of a first glass sheet and a second glass sheet with an interlayer therebetween, and are manufactured by known methods, such as by assembly under heat and pressure.

[0004] For laminated glazing units with vibration damping properties, a three-ply interlayer has been reported that comprises two layers of poly(vinyl butyral) (PVB), also called "outer layer" or "skin", assembled by a layer of PVB, also called "inner layer" or "core". The physical chemistry of the PVB of the inner layer is different from that of the PVB of the two outer layers (see, for example, US Pat. Nos. 5,340,654 and 5,190,826, US Patent Application Publication Nos. 2006 / 021782 and 2016 / 0171961). Specifically, the PVB of the core has a lower residual hydroxyl (-OH group) content than the PVB of the skin. Residual hydroxyl content refers to the amount of hydroxyl groups remaining as side chains on the vinyl chains of the PVB after acetylation of poly(vinyl alcohol) with butyraldehyde. The high hydroxyl content of the PVB outer layer translates into a reduced compatibility with the plasticizer, which then migrates into the PVB inner layer during the autoclave process. The plasticizer increases the viscosity component, improving the vibration damping properties of the viscoelastic inner layer, while the stiff outer layer ensures the handling and mechanical strength of the intermediate layer. The contribution of the stiff outer layer to the vibration damping properties is generally very small.

[0005] With the aim of increasing the sound insulation performance of the laminated glazing units with the above-mentioned three-ply interlayer, it has been considered to increase the plasticizer content of the PVB of the inner layer by still further decreasing the residual hydroxyl group content thereof. However, this resulted in shifting the value of the glass transition temperature (Tg) of the PVB of the core to excessively low temperatures, so that effective vibration damping in the desired frequency range of 1 Hz to 10 kHz was obtained at temperatures lower than the ambient temperature. Thus, at the service temperature of the glazing unit, the vibration damping in the desired frequency range was reduced.

[0006] Consideration has also been given to increasing the residual hydroxyl content of the inner layer PVB and further decreasing its plasticizer content, but this resulted in decreasing the viscous component of the core PVB and shifting the glass transition temperature (Tg) value of said PVB to an excessively high temperature, which in turn reduced the vibration damping ability in the desired frequency range at ambient temperature.

[0007] Thus, these two approaches, which involve adjusting the hydroxyl group content of the PVB inner layer in the interlayer, eventually reached a dead end due to the undesirable but unavoidable increase / decrease in the glass transition temperature (Tg). Summary of the Invention [Problem to be solved by the invention]

[0008] The idea behind the present invention is to replace, in the three-layer interlayer defined above, the PVB inner layer with a layer made of a specific polymer structure different from PVB, which has a very high damping coefficient (tan δ) at temperatures close to ambient temperature in a frequency decade from 1 kHz to 10 kHz, preferably in the frequency range from 1 Hz to 10 kHz. [Means for solving the problem]

[0009] The polymer system chosen by the applicant is a system with two polymer phases: a first discontinuous phase consisting of polymer nanodomains with a specific Tg between −50° C. and −30° C., preferably −45° C. and −35° C., and a second continuous polymer phase with a lower Tg than said first phase. The first phase is dispersed in the second phase, which forms a kind of matrix surrounding the nanodomains.

[0010] The Tg of the first phase is selected such that the vibrational damping reaches its maximum value in a frequency decade from 1 kHz to 10 kHz, preferably in the frequency range from 1 Hz to 10 kHz, at a temperature between 0°C and 40°C, preferably between 10°C and 30°C, more preferably between 15°C and 25°C, and even more preferably at a temperature close to 20°C.

[0011] Furthermore, the applicant has found that the use of a polymer system based on an interpenetrating polymer network (IPN) results in a higher value of loss factor (tan delta) as determined by dynamic mechanical analysis over a much wider vibration frequency range than each of the polymers forming said IPN.

[0012] Therefore, the applicant proposes the use of an interpenetrating polymer network (IPN) type polymer system to form the core of a three-ply interlayer for laminated glass. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The applicant particularly proposes the use of a latex, which is an aqueous emulsion of polymer particles, containing an IPN phase, to form the inner layer of a three-ply interlayer intended for the manufacture of laminated glazing units. The two outer layers of the interlayer may be made of poly(vinyl butyral) (PVB) or else of poly(ethylene-vinyl acetate) (EVA), which may be a substitute for PVB in certain applications.

[0014] The IPN latex is used in the present invention to bond the two outer layers of the intermediate layer together. After the coalescence of the polymer particles, the IPN latex thus forms an adhesive layer in which the IPN phase remains visible by electron microscopy. They are surrounded by a continuous polymer phase, hereafter also called matrix, which fulfills the adhesive function of the inner layer. The term "nanocomposite" used below to describe the present invention refers to this polymer structure consisting of a polymer matrix with high adhesive properties, in which are dispersed polymer nanoparticles or nanodomains that are visible in the intermediate layer even after the coalescence of the latex.

[0015] A first subject of the present patent application is therefore an interlayer for laminated glass, comprising two outer layers of a material chosen from poly(vinyl butyral) (PVB) and poly(ethylene-vinyl acetate) (EVA), assembled by an adhesive nanocomposite layer comprising: a first discontinuous phase consisting of polymer nano-domains having a glass transition temperature (Tg) of -50°C to -30°C, preferably -45°C to -35°C; and A second continuous polymer phase, referred to as a matrix, having a lower glass transition temperature (Tg) than said first phase, preferably less than -50°C, more preferably less than -60°C, wherein the first phase is dispersed in the second phase.

[0016] The two outer layers of the intermediate layer are preferably layers of poly(vinyl butyral) (PVB).

[0017] The first phase of the polymer system chosen by the applicant consists of polymer nanodomains, preferably formed by an interpenetrating polymer network (IPN), which, as initially explained, acts as a vibration absorber at ambient temperature for a frequency decade between 1 kHz and 10 kHz, preferably in the frequency range between 1 Hz and 10 kHz, while the second polymer phase surrounding said nanodomains forms a continuous matrix around the first phase, whose function is essentially to bond the nanoparticles of the first phase to one another and to bond the two outer layers of the laminate interlayer to one another.

[0018] Thus, the polymer system selected by the applicant to obtain the inner layer of the three-layer intermediate layer according to the present invention is preferably formed from a latex. In this specification, the term "latex" means a dispersion of polymer particles in water or an aqueous solvent. According to the present invention, a latex comprises polymer particles having a core-shell structure: the core is formed from an interpenetrating polymer network (IPN) having a glass transition temperature (Tg) of -50°C to -30°C, preferably -45°C to -35°C; The shell is formed from a polymer that has a Tg low enough to cause the particles to coalesce after drying, which Tg is lower than that of the core, preferably less than -50°C, more preferably less than -60°C.

[0019] The core formed from the interpenetrating polymer network (IPN) according to the invention is obtained by two sequential polymerizations: the IPN thus comprises a first polymer (P1), which is crosslinked, and a second polymer (P2), which may or may not be crosslinked.

[0020] In one preferred embodiment of the invention, the second polymer (P2) is not crosslinked. In this case, the IPN is a "semi-interpenetrating polymer network" or semi-IPN. The second polymer may be linear or branched.

[0021] The synthesis of IPNs in the form of latexes has been known for many years and is familiar to those skilled in the art: it is described, for example, in US Pat. No. 3,833,404.

[0022] According to the invention, an IPN can be prepared as follows: forming an aqueous dispersion of a first crosslinked polymer (P1) by polymerization in emulsion, the first crosslinked polymer preferably having a Tg of greater than -30°C, more particularly greater than -20°C; incorporating monomers, with or without a crosslinking agent, into a first crosslinked polymer, which first polymer is swollen by the monomers incorporated therein and subsequently polymerized to form a second polymer of an interpenetrating polymer network having a Tg of less than -40°C, preferably less than -50°C; It can be synthesized by

[0023] If the second polymerization step is carried out in the presence of a crosslinking comonomer, it leads to the formation of a second crosslinked polymer (P2) and an IPN.

[0024] If the second polymerization step is carried out in the absence of a crosslinking comonomer, the second polymer (P2) will not be crosslinked and a semi-IPN will be formed.

[0025] Local entanglement of chains of a first polymer (P1) with chains of a second polymer (P2), which has a lower Tg than the first polymer, can give the (semi-)IPN thus formed a Tg intermediate between those of the first and second polymers.

[0026] The difference between the Tg of the first polymer (P1) and the Tg of the second polymer (P2) is preferably 10°C to 60°C, more preferably 20°C to 50°C.

[0027] According to the present invention, the glass transition temperature (Tg) is measured by differential scanning calorimetry (DSC). The glass transition temperature is determined using the midpoint method described in the standard ASTM-D-3418 for differential scanning calorimetry. The measuring instrument used by the applicant is a Discovery DSC model manufactured by TA Instruments.

[0028] The first and second polymers forming the interpenetrating polymer network may in principle be synthesized using any mixture of comonomers that are copolymerizable by radical polymerization. The Fox equation (TG Fox, Bull. Am. Phys. Soc. 1, 123 (1956)) allows the skilled person to select the comonomers and their proportions in the reaction mixture to arrive at a copolymer with the desired glass transition temperature.

[0029] Examples of monomers that are copolymerizable in the emulsion include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, pentyl acrylate, pentyl methacrylate, isoamyl acrylate, isoamyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, octyl acrylate, octyl methacrylate, isooctyl ... and monomers selected from the group consisting of vinyl formate, vinyl acrylate, vinyl acrylate, vinyl propionate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, styrene, and acrylonitrile.

[0030] Crosslinking comonomers are, for example, diallyl phthalate, triallyl cyanurate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol diacrylate, diethylene glycol dimethacrylate, allyl acrylate, and allyl methacrylate.

[0031] The water-insoluble monomers are advantageously mixed with small amounts, generally less than 5% by weight, of water-soluble comonomers that either copolymerize with the water-insoluble monomers or polymerize separately to form polymers that adsorb to the surface of the latex particles.

[0032] These water-soluble monomers are preferably acids, generally carboxylic acids, more preferably selected from the group consisting of methacrylic acid, acrylic acid, itaconic acid, and fumaric acid. The presence of a negative charge on the surface enhances the colloidal stability of the latex.

[0033] The emulsion polymerization is conventionally carried out in the presence of an emulsifier, preferably a non-ionic surfactant such as a polyoxyethylene glycol ester.

[0034] Traditionally, initiators that can be used for radical polymerization in emulsion must be soluble in the aqueous phase of the reaction mixture. Examples of water-soluble peroxides that may be mentioned include hydrogen peroxide or inorganic peroxides such as ammonium or potassium persulfate. The initiator may be mixed with a reducing agent such as ferrous sulfate (FeSO3) that promotes the formation of radicals.

[0035] More specifically, the inner layer of the three-layer interlayer according to the invention is obtained by applying a latex containing polymer particles with a core-shell structure as described above to one of the faces of a first sheet of PVB or EVA, followed by drying said latex. During the drying of said latex, the water or aqueous phase disappears: the core of the latex polymer particles forms a first discontinuous phase and results in polymer nanodomains having a Tg between -50°C and -30°C, and therefore these nanodomains have the same properties as the core of the latex particles described above; and Due to the low Tg shell, the polymer particles of the latex coalesce and subsequently form a second continuous polymer phase, called the matrix, that surrounds the nano-domains of the first phase.

[0036] The inventors have surprisingly found that the coalescence of polymer latex particles having the properties defined above and resulting in the formation of the two polymer phases confers good vibration damping properties to the adhesive nanocomposite layer in the core thus formed, which contributes to improved sound insulation for the part of the laminated glazing unit having this interlayer, in particular compared to a laminated glazing unit having a three-layer interlayer in which the inner layer is a PVB layer having a low residual level of hydroxyl groups.

[0037] This improvement in sound insulation is due to the loss factor tan δ (determined by dynamic mechanical analysis) of the inner layer of a three-layer intermediate layer according to the present invention being 1.6 or more, preferably 2 or more, more particularly 3 or more, or even 4 or more, over a frequency decade from 1 kHz to 10 kHz, preferably in the frequency range from 1 Hz to 10 kHz, in a temperature range from 0°C to 40°C, preferably 10°C to 30°C, more preferably 15°C to 25°C, and even more preferably at a temperature close to 20°C.

[0038] Thus, it has been surprisingly found by the inventors that the core-shell structure of the polymer particles of the above described latex, when the particles coalesce after drying the latex in a three layer interlayer according to the invention, results in a loss factor for the inner layer of the interlayer of 4-5, which is 4-6 times higher than for a conventional PVB inner layer.

[0039] The loss factor tan δ of a material corresponds to the ratio between the energy dissipated in the form of heat and the energy of elastic deformation. It therefore corresponds to a technical characteristic inherent in the nature of the material and reflects its ability to dissipate energy, more specifically sound waves. The higher the loss factor, the greater the dissipation of energy and the greater the extent to which the material acts in vibration damping. This loss factor tan δ varies as a function of temperature and the frequency of the incident wave. For a certain frequency, the loss factor reaches its maximum value at a certain temperature, which is called the glass transition temperature and is identified by dynamic mechanical analysis. This loss factor tan δ can be estimated using a rheometer or any other suitable known device. A rheometer is a measuring instrument that subjects a material sample to a deformation stress under precise temperature and frequency conditions, whereby all of the rheological parameters that characterize the material are obtained and processed. The loss factor is more specifically measured using a rotational rheometer in oscillatory mode, where the sample is subjected to a sinusoidal stress at an angular velocity ω of 1 to 1000 rad / s, at a temperature range of −100° C. to 100° C. with plateaus every 5° C. The rheometer used by the applicant is an Anton Paar MCR302 model. It should be noted that the loss factor tan δ of the inner layer determines the loss factor tan δ of the intermediate layer, which has substantially the same value as long as the volume fraction of the inner layer is not too small.

[0040] Therefore, the use of an interlayer having an inner layer with a relatively high loss factor tan δ can further improve the sound insulation performance of a glazing unit equipped therewith.

[0041] In one preferred embodiment of the invention, the IPN nanodomains of the first phase in the core of the three-layer interlayer have a number-average equivalent diameter of 10-1000 nm, preferably 20-400 nm, ideally 30-250 nm. Said diameter is measured using a Dynamic Light Scattering (DLS) measuring instrument, which is a non-destructive spectroscopic technique that provides access to the size of particles in suspension or polymer chains in solution of approximately 1-5000 nm diameter. The measuring instrument used by the applicant is a Zetasizer Nano Series model manufactured by Malvern Instruments. The small size of the nanodomains limits the light scattering by the nanodomains, enhancing the transparency of the inner layer of the three-layer interlayer according to the invention.

[0042] The difference between the refractive index of the first phase (n1) and the refractive index of the second phase (n2) is preferably less than 0.2, preferably less than 0.1, ideally less than 0.05. The refractive indices n1 and n2 are advantageously between 1.40 and 1.60, preferably between 1.45 and 1.55. Depending on the respective values ​​of these refractive indices, the reflection of light at the interface between the core and the shell can be reduced, thereby reducing the diffusion of light by the core layer, and ultimately increasing the transparency of the laminated glass.

[0043] In one particular embodiment of the present invention, the ratio of the volume of the first phase to the volume of the second phase in the inner layer of the three-layer intermediate layer is 20 / 80 to 80 / 20, preferably 30 / 70 to 70 / 30.

[0044] The polymer forming the matrix surrounding the nano-domains is preferably the same as the second polymer (P2) forming the interpenetrating polymer network of the first phase, which may be an acrylic copolymer comprising at least one acrylic monomer.

[0045] In one embodiment, the adhesive nanocomposite layer of the three-layer interlayer according to the present invention further comprises a tackifier and / or plasticizer. The addition of the tackifier and / or plasticizer improves vibration damping, increases the loss factor value to greater than 4, aids in the coalescence of the particle shells during drying of the latex, and finally improves the adhesion of the core layer to the PVB layer in the frequency decade of 1 kHz to 10 kHz, preferably in the frequency range of 1 Hz to 10 kHz, in the temperature range of 0°C to 40°C. The tackifier may be selected from natural tackifying resins, especially rosins and terpenes, and synthetic tackifying resins such as petroleum-derived aliphatic resins, aromatic resins, and hydrogenated resins.

[0046] The tackifier used is preferably a terpene modified to be colorless and transparent and having a Gardner Index strictly less than 1 on the Gardner color scale, such as the Crystazene 110 product from DRT. The amount of tackifier may be from 1% to 8% by weight, preferably from 2% to 5% by weight, based on the total weight of the latex.

[0047] In one preferred embodiment, the adhesive nanocomposite layer is in direct contact with the two outer PVB layers of an intermediate layer according to the invention.

[0048] In one particular embodiment of the invention, the thickness of the adhesive nanocomposite inner layer of the invention is preferably 5 to 50 micrometers, more preferably 10 to 30 micrometers. The use of a core with a thickness on the micrometer scale makes it possible to reduce the risk of the latex forming the core flowing out during its application. This thickness also makes it possible to adjust the stiffness of the three-ply interlayer so as to obtain a stiffness on the scale of the laminated glazing with respect to the stresses during formation and curvature of the final laminated glazing unit, and to ensure the safety of passengers or occupants in the event of a fracture of the laminated glass.

[0049] The thickness of the outer PVB layer of a three layer interlayer of the present invention may be from 200 to 500 micrometers, preferably from 300 to 400 micrometers, and ideally approximately 380 micrometers.

[0050] In one particular embodiment of the invention, the inner layer corresponds to a volume fraction of the intermediate layer of 0.2% to 8%, preferably 0.5% to 8%, preferably 2.5% to 4%. By selecting such a volume fraction of the inner layer within the intermediate layer, a good trade-off is obtained between the stiffness requirements on the one hand and the sound insulation performance on the other hand.

[0051] The present invention also relates to a method for producing a viscoelastic interlayer for laminated glass, the method comprising the steps of: providing a first sheet of material selected from poly(vinyl butyral) (PVB) and poly(ethylene vinyl acetate) (EVA); applying to one of the faces of the first sheet a latex comprising polymer particles having a core-shell structure, The core is formed from an interpenetrating polymer network (IPN) having a Tg of -50°C to -30°C, preferably -45°C to -35°C; and The shell is formed from a polymer having a lower Tg than the core, preferably less than -50°C, more preferably less than -60°C. process, drying the latex to form an adherent nanocomposite layer; Applying to the resulting adhesive nanocomposite layer a second sheet of a material selected from poly(vinyl butyral) (PVB) and poly(ethylene-vinyl acetate) (EVA).

[0052] The application of the latex to one of the faces of the first PVB sheet is preferably carried out by known roll-to-roll liquid coating methods, more particularly by using a reverse roll coater in which the latex is fed through a nip (nip-feed reverse roll).

[0053] The drying step is preferably carried out continuously, at ambient temperature and / or in an oven at a temperature between 40° C. and 120° C., preferably between 60° C. and 100° C. This drying step is advantageously carried out under reduced pressure between 0.01 atm and 1 atm, preferably between 0.1 atm and 0.5 atm, ideally at a pressure of 0.25 atm. A second PVB sheet is then applied on top of the film obtained from drying the latex.

[0054] The process parameters such as the tension of the PVB sheet in the process, as well as the stability of the rolls and the stability of the feeding of the latex through the nip, can be controlled so that the three-layer interlayer of the present invention does not exhibit any waviness defects.

[0055] The present invention also provides A first glass sheet; a second glass sheet; an interlayer as described above disposed between the first and second glass sheets; The present invention also relates to a laminated glazing unit comprising:

[0056] In one particular embodiment of the invention, the first glass sheet has a thickness of 0.5 to 3 mm, preferably 1.4 to 2.1 mm, and the second glass sheet has a thickness of 0.5 to 2.1 mm, preferably 1.1 to 1.6 mm.

[0057] The technical advantages provided by the inventive interlayer as described in the text of this specification also relate to laminated glazing units comprising an interlayer of this type. The Applicant therefore proposes a laminated glazing unit with a specific interlayer as described above, which has good vibration damping properties in a frequency decade of 1 kHz to 10 kHz, preferably in a frequency range of 1 Hz to 10 kHz, in a temperature range of 0°C to 40°C, preferably 10°C to 30°C, more preferably 15°C to 25°C, and even more preferably at temperatures close to 20°C, at which said laminated glazing unit is used.

[0058] Additionally, the intermediate layer of the present invention comprises: and / or, most of its surfaces may be tinted to allow privacy for persons inside the vehicle or to otherwise prevent the vehicle operator from being dazzled by sunlight, or simply for aesthetic effect; and / or and / or may have a cross-section that decreases in a wedge shape from a top to a bottom of the laminated glazing unit so that the laminated glazing unit can be used as a screen for a head-up display (HUD) system; and / or The material may contain particles that have a filtering function against infrared radiation to limit the temperature rise inside the vehicle due to the sun's infrared radiation and improve the comfort of the vehicle passengers or building occupants.

[0059] The present invention also relates to the use of the above mentioned laminated glazing unit as a vehicle windshield and / or as architectural glazing for attenuating vibration and structure-borne noise from 1 Hz to 1000 Hz and / or for increasing the loss of transmission to air-borne noise in the audio frequency decade from 1 kHz to 10 kHz. When the glazing unit of the present invention is used as a windshield, it naturally meets all the conditions of UN Regulation No. 43 (or simply Regulation R43) for impact resistance in order to ensure its mechanical strength. Some of the embodiments of the present disclosure are described in [Item 1] to [Item 16] below. [Item 1] 1. An interlayer for laminated glazing, comprising two outer layers of a material selected from poly(vinyl butyral) (PVB) and poly(ethylene-vinyl acetate) (EVA), assembled by an adhesive nanocomposite layer comprising: a first discontinuous phase consisting of polymer nano-domains having a glass transition temperature (Tg) of -50°C to -30°C, preferably -45°C to -35°C; and A second continuous polymer phase, referred to as a matrix, having a lower glass transition temperature (Tg) than said first phase, preferably less than -50°C, more preferably less than -60°C, wherein said first phase is dispersed in said second phase. [Item 2] 2. The interlayer for laminated glazing according to claim 1, characterized in that the two outer layers are layers of poly(vinyl butyral) (PVB). [Item 3] 3. The intermediate layer according to claim 1 or 2, wherein the nano-domains of the first phase are formed from an interpenetrating polymer network (IPN) comprising a first polymer (P1) that is crosslinked and a second polymer (P2) that may or may not be crosslinked. [Item 4] 4. The intermediate layer according to any one of items 1 to 3, wherein the nano-domains forming the first phase have a number average equivalent diameter of 10 to 1000 nm, preferably 20 to 400 nm, and ideally 30 to 250 nm. [Item 5] 5. The intermediate layer according to any one of claims 1 to 4, wherein the adhesive nanocomposite layer has a thickness of 5 to 50 micrometers, preferably 10 to 30 micrometers. [Item 6] 4. The intermediate layer according to claim 3, wherein the second polymer (P2) is not crosslinked. [Item 7] 7. The intermediate layer according to any one of items 3 to 6, wherein the first polymer (P1) has a Tg higher than -30°C, preferably higher than -20°C. [Item 8] 7. The intermediate layer according to any one of items 3 to 6, wherein the second polymer (P2) has a Tg of less than -50°C, preferably less than -60°C. [Item 9] 9. The intermediate layer according to item 7 or 8, wherein the difference between Tg of the first polymer (P1) and Tg of the second polymer (P2) is 10°C to 60°C, preferably 20°C to 50°C. [Item 10] 10. The intermediate layer according to any one of items 3 to 9, wherein the polymers P1 and P2 are acrylic copolymers comprising at least one acrylic monomer. [Item 11] 11. The intermediate layer according to any one of items 1 to 10, wherein the difference between the refractive index (n1) of the first phase and the refractive index (n2) of the second phase is less than 0.2, preferably less than 0.1, and ideally less than 0.05. [Item 12] Item 12. The intermediate layer according to any one of items 1 to 11, wherein the adhesive nanocomposite layer is in direct contact with the two outer layers. [Item 13] 13. The intermediate layer according to any one of items 1 to 12, wherein the ratio of the volume of the first phase to the volume of the second phase is from 20 / 80 to 80 / 20, preferably from 30 / 70 to 70 / 30. [Item 14] 1. A method for producing an interlayer for laminated glazing, comprising the steps of: providing a first sheet of material selected from poly(vinyl butyral) (PVB) and poly(ethylene vinyl acetate) (EVA); applying to one of the faces of the first sheet a latex comprising polymer particles having a core-shell structure, the core is formed from an interpenetrating polymer network (IPN) having a Tg of -50°C to -30°C, preferably -45°C to -35°C; and The shell is formed from a polymer having a lower Tg than the core, preferably less than -50°C, more preferably less than -60°C. process, drying the latex to form an adhesive nanocomposite layer; Applying to the resulting adhesive nanocomposite layer a second sheet of a material selected from poly(vinyl butyral) (PVB) and poly(ethylene-vinyl acetate) (EVA). [Item 15] Item 15. A method for producing an interlayer for laminated glazing according to item 14, wherein the drying step is carried out at ambient temperature and / or in an oven at a temperature between 40°C and 120°C, preferably between 60°C and 100°C. [Item 16] A first glass sheet; a second glass sheet; The intermediate layer according to any one of items 1 to 13, which is disposed between the first and second glass sheets; A laminated glazing unit comprising:

Claims

1. 1. An interlayer for laminated glazing comprising two outer layers of a material selected from poly(vinyl butyral) (PVB) and poly(ethylene-vinyl acetate) (EVA) assembled by an adhesive nanocomposite inner layer comprising: The adhesive nanocomposite inner layer comprises a polymer based on an interpenetrating polymer network (IPN), and the adhesive nanocomposite inner layer has a loss factor tan δ of 1.6 or more as determined by dynamic mechanical analysis at a temperature range of 0° C. to 40° C. and a frequency decade of 1 kHz to 10 kHz. Middle layer: a first discrete phase consisting of polymer nano-domains having a glass transition temperature (Tg) of -50°C to -30°C; and A second continuous polymer phase, referred to as a matrix, having a lower glass transition temperature (Tg) than said first discrete phase, wherein said first discrete phase is dispersed in said second continuous polymer phase.

2. 10. The interlayer for laminated glazing according to claim 1, wherein the two outer layers are layers of poly(vinyl butyral) (PVB).

3. 3. The intermediate layer of claim 1 or 2, wherein the polymer nano-domains of the first discontinuous phase are formed from an interpenetrating polymer network (IPN) comprising a first polymer (P1) that is crosslinked and a second polymer (P2) that may or may not be crosslinked.

4. The intermediate layer of any one of claims 1 to 3, wherein the polymer nano-domains forming the first discontinuous phase have a number average equivalent diameter of 10 to 1000 nm.

5. The intermediate layer of any one of claims 1 to 4, wherein the adhesive nanocomposite inner layer has a thickness of 5 to 50 micrometers.

6. 4. The intermediate layer according to claim 3, wherein the second polymer (P2) is not crosslinked.

7. The polymer nano-domains of the first discontinuous phase are formed from an interpenetrating polymer network (IPN) comprising a first polymer (P1), which is crosslinked, and a second polymer (P2), which may or may not be crosslinked; The intermediate layer according to any one of claims 3 to 6, wherein the first polymer (P1) and the second polymer (P2) are acrylic copolymers comprising at least one acrylic monomer.

8. 8. The intermediate layer according to any one of claims 1 to 7, wherein the difference between the refractive index of the first discontinuous phase (n1) and the refractive index of the second continuous polymer phase (n2) is less than 0.

2.

9. The intermediate layer of any one of claims 1 to 8, wherein the inner adhesive nanocomposite layer is in direct contact with the two outer layers.

10. 10. The intermediate layer of any one of claims 1 to 9, wherein the ratio of the volume of the first discontinuous phase to the volume of the second continuous polymeric phase is from 20 / 80 to 80 / 20.

11. 1. A method for producing an interlayer for laminated glazing, comprising the steps of: providing a first sheet of material selected from poly(vinyl butyral) (PVB) and poly(ethylene-vinyl acetate) (EVA); applying to one of the faces of the first sheet a latex comprising polymer particles having a core-shell structure, the core is formed from an interpenetrating polymer network (IPN) having a Tg of -50°C to -30°C; and The shell is formed from a polymer having a lower Tg than the core. process, drying the latex to form an inner bonded nanocomposite layer, the inner bonded nanocomposite layer having a loss factor tan δ of 1.6 or greater as determined by dynamic mechanical analysis at a temperature range of 0° C. to 40° C. and a frequency decade of 1 kHz to 10 kHz; Applying to the resulting adhesive nanocomposite inner layer a second sheet of a material selected from poly(vinyl butyral) (PVB) and poly(ethylene-vinyl acetate) (EVA).

12. The method for producing an intermediate layer for laminated glass as described in claim 11, wherein the drying step of the latex to form an adhesive nanocomposite inner layer is carried out at ambient temperature and / or in an oven at a temperature of from 40°C to 120°C.

13. A first glass sheet; a second glass sheet; The interlayer according to any one of claims 1 to 10, disposed between the first and second glass sheets. A laminated glazing unit comprising:

Citation Information

Patent Citations

  • Anti-vibration structure using thermally polymerized epoxide

    JP1996511571A

  • Damping glass and plastic laminates

    JP2001506198A

  • Emulsion for sound deadener

    JP2005105133A

  • Laminated body using gel and method of manufacturing the same

    JP2010111081A

  • Intermediate film for glass laminate and glass laminate

    JP2016108220A