Method for preparing high purity low uranium submicron spherical silica powder

A method for producing low-uranium submicron spherical silica fine powder through high-temperature processing and acid refining addresses the limitations of existing technologies, achieving stable and cost-effective production with low uranium content.

JP7576637B2Active Publication Date: 2024-10-31JIANGSU NOVORAY NEW MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022573715
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-02
Filing Date
2022-08-29
Publication Date
2024-10-31
Estimated Expiration
2042-08-29

AI Technical Summary

Technical Problem

Existing methods for producing low-uranium spherical silica fine powder face challenges such as high energy consumption, environmental pollution, high costs, and instability in uranium content, particularly for submicron-sized products, and are limited by the need for high-purity raw materials and complex processing steps.

Method used

A method involving high-temperature firing, water quenching, wet refining with acid mixtures, and high-temperature spheroidization to produce submicron spherical silica fine powder with low uranium content, using elemental silicon or silicon-containing compounds as raw materials, and employing hydrofluoric and hydrochloric acids with hydrogen peroxide to recover uranium, followed by filtration and drying.

Benefits of technology

The method achieves stable submicron spherical silica fine powder with uranium content below 1.0 ppb, suitable for various silicon sources, reducing material requirements and environmental impact while maintaining high purity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a method for preparing high purity low uranium submicron spherical silica fine powder. [Solution] The lump raw material is first calcined, crushed, settled and dried to obtain sand raw material of 1 mm or less, the sand raw material is made into powder slurry by a wet ball mill, a mixed acid solution consisting of a hydrofluoric acid solution and a hydrochloric acid solution is then added to the powder slurry, hydrogen peroxide is added to recover the uranium element, the powder slurry is then pressure filtered, washed and dried to obtain a powder with a uranium content of 1.0 ppb or less, and finally a submicron spherical silica fine powder is obtained by a flame spheroidization method. The method of the present invention has low requirements for raw materials, is suitable for various industrial grade silicon sources, and the U content in the prepared submicron spherical silica fine powder is low and stable.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application filed with the China Patent Office on December 2, 2021, bearing application number CN202111460463.2 and entitled "Method for preparing high-purity low-uranium submicron spherical silica micropowder", the entire contents of which are incorporated herein by reference.

[0002] The present invention belongs to the technical field of preparing thermally conductive fillers, and relates to a method for preparing high-purity, low-uranium, submicron spherical silica fine powder. [Background technology]

[0003] As electronic devices become smaller and thinner, the particle size of fillers for semiconductor packaging becomes smaller and smaller. At the same time, in order to improve the filling amount and fluidity of fillers in semiconductor packaging, it is necessary to add submicron (generally 0.1μm to 1μm) fillers with high sphericity. However, with the continuous improvement of the integration degree of ultra-large scale integrated circuits, the wiring spacing becomes narrower and narrower, and strong alpha rays in the packaging material cause soft errors in signal transmission. Therefore, the requirements for alpha rays are becoming stricter for packaging materials of ultra-large scale integrated circuits and memory chips. Uranium (U) in natural ores is the most important factor that affects alpha rays. Therefore, it is necessary to control the content of uranium element and the intensity of alpha rays.

[0004] Patent Document 1: In Chinese patent application CN101570332A, silica sol is prepared using an organic silicon source, and spherical silica fine powder with U<1ppm is obtained through processes such as granulation. Patent Document 2: In Chinese patent application CN104556076A, spherical silicon fine powder without alpha rays is obtained by adopting purification, emulsification and other procedures of organic silane. However, the above method is mainly based on chemical synthesis, and uses high-purity organic silicon source and solvent to prepare high-purity low-uranium spherical silicon fine powder, which has the problems of large energy consumption, large pollution, and high cost that cannot be reduced.

[0005] Patent Document 3: In Chinese patent application CN112591756A, natural quartz with a low uranium content of about 1 ppb is used to obtain a product with a uranium content of less than 1 ppb through flame combustion. However, this method is only suitable for producing micron-sized spherical silicon fine powder, and submicron-sized products need to be processed through complex processes such as continuous grading, which cannot be obtained in one step.

[0006] Patent Document 4: In Chinese patent application CN101274365A, the uranium content of the prepared product is 0.4-5.0 ppb by controlling the content of P element and uranium in the raw material Si, but this method is strict on the raw material Si and it is difficult to obtain the raw material.

[0007] To sum up, the existing low uranium spherical silicon micropowder manufacturing method involves selecting high purity organic silicon source and solvent to obtain high purity low uranium products through chemical synthesis, but this method brings about environmental problems; if only low uranium natural quartz with about 1 ppm is selected, only micron-scale products can be obtained, and at the same time, the requirements for raw materials are relatively high, making it difficult to realize products with a uranium content of 0.5 ppb or less; if the raw material Si is strictly selected, after simple acid treatment, the U content of the obtained product is unstable. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Chinese patent application CN101570332A [Patent Document 2] Chinese patent application CN104556076A [Patent Document 3] Chinese patent application CN112591756A [Patent Document 4] Chinese patent application CN101274365A Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a method for preparing high purity, low uranium, submicron spherical silica fine powder. [Means for solving the problem]

[0010] The technical solutions to achieve the objectives of the present invention are as follows: A method for preparing high purity low uranium submicron spherical silica fine powder, comprising the steps of: Step (1) of calcining the raw material in a high-temperature furnace at 700-1400°C for 10-20 hours under the protection of inert gas, quenching with water after calcination, crushing into sand raw material of 1 mm or less, settling and drying, and then repeating the steps of calcination-crushing-settling and drying to obtain sand raw material, the raw material being a lump raw material of elemental silicon or inorganic compound containing silicon, with a purity of 99.5% or more, a uranium content of 5-20 ppb, and a particle size of 30-100 mm; (2) A mass ratio of sand to water is set to 1-3:2-5, and a HF solution is added in an amount of 0.1‰-0.5‰ relative to the mass of water, and a powder slurry having an average particle size of 5-40 μm is obtained by a wet ball mill; (3) adding equal masses of hydrofluoric acid solution and hydrochloric acid solution to the powder slurry according to a concentration ratio of hydrofluoric acid solution and hydrochloric acid solution of 1-300:1, and at the same time, adding 0.1%-0.5% hydrogen peroxide based on the total mass of hydrofluoric acid solution and hydrochloric acid solution (mass of acid mixture solution), and adding flotation agent and collector to recover uranium element, and stirring at 30-60°C to obtain powder slurry; Step (4) of subjecting the powder slurry obtained in step (3) to pressure filtration, washing, and drying to obtain a powder having a uranium content of 1.0 ppb or less; The method includes a step (5) of introducing and igniting a carrier gas, a combustible gas and a combustion improver using a flame spheroidization method, spheroidizing the powder obtained in step (4) at a high temperature of 1800 to 2400°C, and recovering a submicron spherical silica fine powder.

[0011] Preferably, in step (1), the silicon-containing inorganic compound is one or more of silicon nitride, silicon carbide, and silicon oxide.

[0012] Preferably, in step (2), the time for wet ball milling is 5 to 30 hours.

[0013] Preferably, in step (2), the hydrofluoric acid solution has a mass concentration of 1.5%.

[0014] Preferably, in step (3), the concentration ratio of the hydrofluoric acid solution to the hydrochloric acid solution is 1-3:1.

[0015] Preferably, in step (3), the mass concentration of the hydrochloric acid solution is 0.005% to 1.5%.

[0016] Preferably, in step (3), the stirring time is 12 to 72 hours.

[0017] Preferably, in step (5), the carrier gas is oxygen, air, nitrogen, or argon, the combustible gas is natural gas (LNG), liquefied petroleum gas (LPG) or H2, and the combustion improver is air or oxygen.

[0018] Preferably, in step (5), the submicron spherical silica fine powder has an average particle size D50 of 0.1 to 1.5 μm, a U content of less than 1.0 ppb, and a SiO 2 purity of 99.90% or more. Effect of the Invention

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] The present invention uses water quenching, wet refining and oxidation of U element to treat with acid mixture to obtain stable submicron spherical silica fine powder with low U content. The method of the present invention has low requirements for raw materials and is suitable for various industrial grade silicon sources. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention will now be described in more detail with reference to specific examples.

[0022] Example 1 (1) Under the protection of argon, 10 kg of elemental silicon (99.6% purity, 15 ppb uranium content) with a particle size of 80 mm was sintered in a high-temperature furnace at 1250°C for 15 hours. After sintering, it was quenched with water, crushed into sand material of 1 mm or less, and dried by settling. Next, the steps of sintering-crushing-settling drying were repeated once. The dried sand material was collected several times and prepared.

[0023] (2) 250 kg of dried sand raw material was weighed out and added to 230 kg of water, and 0.05 kg of a hydrofluoric acid solution with a mass concentration of 1.5% was added. After being pulverized in a wet ball mill, a powder slurry with an average particle size of 35 μm was obtained.

[0024] (3) The powder slurry was transferred to a reaction vessel, and 15 kg of a 1.5% HF solution and 15 kg of a 0.5% HCl solution were added. At the same time, 0.1% hydrogen peroxide was added relative to the mass of the acid mixture solution. A flotation agent and a collector were added to recover the uranium element, and the mixture was stirred at 60°C for 24 hours to obtain a powder slurry.

[0025] (4) The powder slurry was pressure filtered, washed, and dried to obtain a powder with a uranium content of 1.0 ppb or less.

[0026] (5) The powder is spheronized at high temperature of 2000℃ in an oxygen-rich atmosphere, and the resulting high-purity, low-uranium, submicron spherical silica fine powder has a particle size of 0.3μm, a U content of 0.2ppb, and a SiO2 purity of 99.95%.

[0027] Example 2 (1) Under the protection of argon, 10 kg of silicon nitride (99.8% purity) with a particle size of 35 mm and 10 kg of elemental silicon (99.6% purity, uranium content of 15 ppb) were sintered in a high-temperature furnace at 900°C for 5 hours. After sintering, they were quenched with water, crushed into sand material of 1 mm or less, and dried by settling. Next, the steps of sintering-crushing-settling drying were repeated once. The dried sand material was collected several times and prepared.

[0028] (2) 250 kg of dried sand raw material was weighed out, added to 230 kg of water, and 0.05 kg of a hydrofluoric acid solution with a mass concentration of 1.5% was added. After being pulverized in a wet ball mill, a powder slurry with an average particle size of 30 μm was obtained.

[0029] (3) The powder slurry was transferred to a reaction vessel, and 15 kg of a 1.5% HF solution and 15 kg of a 0.5% HCl solution were added. At the same time, hydrogen peroxide was added in an amount of 0.3% of the mass of the acid mixture solution. A flotation agent and a collector were added to recover the uranium element, and the mixture was stirred at 60°C for 24 hours to obtain a powder slurry.

[0030] (4) The powder slurry was pressure filtered, washed, and dried to obtain a powder with a uranium content of 1.0 ppb or less.

[0031] (5) The powder is spheronized at high temperature of 2000℃ in an oxygen-enriched atmosphere, and the resulting high-purity, low-uranium, submicron spherical silica fine powder has a particle size of 0.3μm, a U content of 0.3ppb, and a SiO2 purity of 99.91%.

[0032] Example 3 (1) Under the protection of argon, 10 kg of silicon nitride (with a purity of 99.6%) with a particle size of 70 mm is sintered in a high-temperature furnace at 850°C for 15 hours. After sintering, it is quenched with water, crushed into sand material of less than 1 mm, and dried by settling. Next, the steps of sintering-crushing-settling drying are repeated once. The dried sand material is collected and prepared several times.

[0033] (2) 250 kg of dried sand raw material was weighed out and added to 230 kg of water, and 0.05 kg of a hydrofluoric acid solution with a mass concentration of 1.5% was added. After being pulverized in a wet ball mill, a powder slurry with an average particle size of 35 μm was obtained.

[0034] (3) The powder slurry was transferred to a reaction vessel, and 15 kg of a 1.5% HF solution and 15 kg of a 0.5% HCl solution were added. At the same time, 0.1% hydrogen peroxide was added relative to the mass of the acid mixture solution. A flotation agent and a collector were added to recover the uranium element, and the mixture was stirred at 35°C for 12 hours to obtain a powder slurry.

[0035] (4) The powder slurry was pressure filtered, washed, and dried to obtain a powder with a uranium content of 1.0 ppb or less.

[0036] (5) The powder is spheronized at high temperature of 2000℃ in an oxygen-rich atmosphere. The resulting high-purity, low-uranium, submicron spherical silica fine powder has a particle size of 0.3μm, a U content of 0.9ppb, and a SiO2 purity of 99.93%.

[0037] Example 4 This example is basically the same as Example 1, with the only difference being that the calcination temperature is 700° C. The resulting high-purity low-uranium submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 0.9 ppb, and a SiO2 purity of 99.90%.

[0038] Example 5 This example is basically the same as Example 1, with the only difference being that the calcination temperature is 1400° C. The resulting high-purity low-uranium submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 0.2 ppb, and a SiO2 purity of 99.96%.

[0039] Example 6 This example is basically the same as Example 1, with the only difference being that the mass concentration of the HF solution is 1.5% and the mass concentration of the HCl solution is 1.5%. The particle size of the obtained high-purity low-uranium submicron spherical silica fine powder is 0.3 μm, the U content is 0.3 ppb, and the purity of SiO2 is 99.95%.

[0040] Example 7 This example is basically the same as Example 1, with the only difference being that the mass concentration of the HF solution is 1.5% and the mass concentration of the HCl solution is 0.005%. The particle size of the obtained high-purity low-uranium submicron spherical silica fine powder is 0.3 μm, the U content is 0.8 ppb, and the purity of SiO2 is 99.88%.

[0041] Comparative Example 1 This comparative example is basically the same as Example 1, with the only difference being that only HF solution with a mass concentration of 1.5% is added instead of the acid mixture during the acid treatment process. The resulting submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 2.5 ppb, and a SiO2 purity of 99.85%.

[0042] Comparative Example 2 This comparative example is basically the same as Example 1, with the only difference being that no acid mixture treatment was performed. The resulting submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 13 ppb, and a SiO2 purity of 99.80%.

[0043] Comparative Example 3 This comparative example is basically the same as Example 1, with the only difference being that the firing temperature is 500° C. The resulting submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 3.3 ppb, and a SiO2 purity of 99.90%.

[0044] Comparative Example 4 This comparative example is basically the same as Example 1, with the only difference being that the HCl solution is replaced with CH3COOH. The resulting submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 2.6 ppb, and a SiO2 purity of 99.84%.

[0045] Comparative Example 5 This comparative example is basically the same as Example 1, with the only difference being that the HCl solution was replaced with HNO3. The resulting submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 1.9 ppb, and a SiO2 purity of 99.87%.

[0046] Comparative Example 6 This comparative example is basically the same as Example 1, with the only difference being that the 0.5% HCl solution was replaced with a 0.003% HCl solution by mass concentration. The resulting submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 2.4 ppb, and a SiO2 purity of 99.91%.

[0047] Comparative Example 7 This comparative example is basically the same as Example 1, with the only difference being that the HF solution with a mass concentration of 1.5% was replaced with a HF solution with a mass concentration of 0.05%. The resulting submicron spherical silica fine powder has a particle size of 0.3 μm, a U content of 2.7 ppb, and a SiO2 purity of 99.83%.

[0048] The above description of the examples is only used to help understand the method and core idea of ​​the present invention. Those skilled in the art can make some improvements and modifications to the present invention without departing from the principles of the present invention, and these improvements and modifications are also within the scope of protection of the claims. Various modifications to these examples are readily apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not intended to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing high purity low uranium submicron spherical silica fine powder, comprising the steps of: Step (1) of calcining the raw material in a high-temperature furnace at 700-1400°C for 10-20 hours under the protection of inert gas, quenching with water after calcination, crushing into sand raw material of 1 mm or less, settling and drying, and then repeating the steps of calcination-crushing-settlement and drying to obtain sand raw material, the raw material being a lump raw material of single silicon having a purity of 99.5% or more, a uranium content of 5-15 ppb, and a particle size of 30-100 mm; Step (2) of making the mass ratio of sand to water 1-3:2-5, and adding 0.1‰-0.5‰ of HF solution to the mass of water, and obtaining a powder slurry having an average particle size of 5-40 μm by a wet ball mill; (3) adding equal masses of hydrofluoric acid solution and hydrochloric acid solution to the powder slurry according to a concentration ratio of hydrofluoric acid solution and hydrochloric acid solution of 1-300:1, and simultaneously adding 0.1%-0.5% hydrogen peroxide based on the total mass of hydrofluoric acid solution and hydrochloric acid solution, and adding flotation agent and collector to recover uranium element, and stirring at 30-60°C to obtain powder slurry; Step (4) of subjecting the powder slurry obtained in step (3) to pressure filtration, washing and drying to obtain a powder having a uranium content of 1.0 ppb or less; and (5) introducing and igniting a carrier gas, a combustible gas and a combustion improver using a flame spheroidization method, spheroidizing the powder obtained in step (4) at a high temperature of 1800 to 2400°C, and recovering a submicron spherical silica fine powder. A preparation method comprising the steps of:

2. In step (2), the wet ball milling time is 5 to 30 hours.

2. The method of claim 1.

3. In step (2), the mass concentration of the hydrofluoric acid solution is 1.5%.

2. The method of claim 1.

4. In step (3), the concentration ratio of the hydrofluoric acid solution to the hydrochloric acid solution is 1 to 3:

1.

2. The method of claim 1.

5. In step (3), the mass concentration of the hydrochloric acid solution is 0.005% to 1.5%.

5. The preparation method according to claim 1 or 4.

6. In step (3), the stirring time is 12 to 72 hours.

2. The method of claim 1.

7. In step (5), the carrier gas is oxygen, air, nitrogen, or argon.

2. The method of claim 1.

8. In step (5), the flammable gas is natural gas, liquefied petroleum gas or H 2 is 2. The method of claim 1.

9. In step (5), the combustion improver is air or oxygen.

2. The method of claim 1.

Citation Information

Patent Citations

  • Silicon metal powder and production method thereof, composition of spherical silicon dioxide powder and resin

    CN101274365A

  • High-purity low-radioactivity spherical silicon micropowder and preparation method thereof

    CN101570332A

  • Preparation method of ultrahigh-purity amorphous spherical silica powder

    CN104556076A

  • High-purity low-radioactivity spherical silica powder and preparation method thereof

    CN112591756A

  • Spherical silica particle, resin composition and semiconductor liquid sealing material

    JP2006256913A