GaAs ingot manufacturing method and GaAs ingot

The method addresses the challenge of balancing carrier concentration and crystallinity in GaAs ingot production by controlling Si doping and stirring during crystal growth, resulting in GaAs ingots suitable for VCSELs with improved quality and productivity.

JP7576672B2Active Publication Date: 2024-10-31DOWA ELECTRONICS MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023147887
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-21
Filing Date
2023-09-12
Publication Date
2024-10-31
Estimated Expiration
2043-09-12

AI Technical Summary

Technical Problem

Existing methods for producing GaAs ingots struggle to achieve a balance between carrier concentration and crystallinity, particularly for applications requiring high carrier concentration and low dislocation density, such as VCSELs, due to Si segregation leading to polycrystallization and impurity concentration during crystal growth.

Method used

A method involving the use of a vertical boat process with controlled Si doping and boron oxide stirring to manage Si concentration, ensuring the GaAs ingot maintains a carrier concentration of 1.5×10^18 to 2.9×10^18 cm^-3 and an etch pit density of 1200 cm^-2 or less, using Si-doped GaAs raw material and boron oxide as a sealant, with controlled stirring to prevent polycrystallization.

Benefits of technology

The method enables the production of GaAs ingots with controlled carrier concentration and low dislocation density, suitable for VCSELs, by managing Si concentration and preventing polycrystallization, thereby enhancing productivity and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576672000004
    Figure 0007576672000004
  • Figure 0007576672000005
    Figure 0007576672000005
  • Figure 0007576672000006
    Figure 0007576672000006
Patent Text Reader

Abstract

To provide a manufacturing method of a GaAs ingot for efficiently obtaining a GaAs wafer with a strictly controlled carrier concentration and a low dislocation density, and a GaAs ingot.SOLUTION: In a manufacturing method of a GaAs ingot where a Si raw material as a seed crystal and a dopant, a GaAs raw material, and boron oxide as an encapsulation agent are accommodated in a crucible and crystal growth is performed in a vertical type boat method, the GaAs raw material is a Si-doped GaAs in which a Si concentration is 20 - 200 wtppm to GaAs, a charge amount of the Si raw material is 200 - 300 wtppm to GaAs, and the boron oxide contains more than 5 mol% of SiO2 in terms of Si. After the Si raw material, the GaAs raw material and the boron oxide are molten by heating, and crystal growth is performed while a liquid boron oxide is stirred.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a GaAs ingot and to a GaAs ingot. [Background technology]

[0002] Known methods for manufacturing GaAs single crystals (hereinafter also referred to as GaAs ingots) to obtain GaAs single crystal wafers (hereinafter also referred to as GaAs wafers) include the LEC method, the horizontal boat (HB) method, the vertical temperature gradient (VGF) method, and the vertical Bridgman (VB) method. Starting from a single crystal seed crystal, a mass having a straight body of single crystal grown by these manufacturing methods is called an ingot, and wafers are cut from the straight body of the ingot. Multiple GaAs wafers can be obtained from the same GaAs ingot, and these multiple wafers are also called a wafer group.

[0003] Here, the vertical boat method, such as the vertical temperature gradient (VGF) method and the vertical Bridgman (VB) method, is a method in which a seed crystal is placed at the bottom of a crucible, a single crystal raw material melt and a sealant liquid are placed on top of the seed crystal, and the crucible is cooled from a predetermined temperature distribution to grow a crystal from the bottom of the raw material melt upward. In the vertical temperature gradient (VGF) method, the temperature itself is lowered, and in the vertical Bridgman (VB) method, the crucible is moved relatively within a predetermined temperature distribution. When manufacturing a Si-doped GaAs single crystal ingot, Si is added to the GaAs melt. Boron oxide (B2O3) is usually used as a sealant to prevent As, a volatile component, from dissociating from the ingot. During crystal growth, it is known that an oxidation-reduction reaction occurs at the interface between the GaAs melt and the liquid B2O3 according to the following reaction formula (1). 3Si(during Melt)+2B2O3=3SiO2(during B2O3)+4B(during Melt)...(1)

[0004] In the vertical boat method, the crystal is grown from the bottom to the top of the raw material melt, so impurities that are not incorporated into the crystal are concentrated in the melt. If a large amount of Si dopant (i.e., Si crystals added together with the GaAs raw material) is added to the GaAs melt to increase the carrier concentration, the equilibrium of the above reaction formula (1) advances to the right side, and a large amount of boron (B) moves into the GaAs melt. As the crystal growth progresses and the impurities become more concentrated, the generation of boron arsenide also progresses, making it impossible to obtain high crystallinity. In other words, in the GaAs single crystal obtained by this manufacturing method, there is a trade-off between carrier concentration and crystallinity.

[0005] In Patent Document 1, in the vertical boat method, plate-like gallium arsenide (GaAs) is deposited on the interface between the GaAs melt and the liquid B2O3. By arranging solid silicon dioxide, GaAs single crystals with high carrier concentration and high crystallinity were grown. A method for producing the same has been proposed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-246156 A Summary of the Invention [Problem to be solved by the invention]

[0007] In recent years, among semiconductor lasers, surface-emitting lasers such as VCSELs (vertical-cavity surface-emitting lasers) have been actively used and are being applied to optical communications, optical sensing, and other fields. For these applications, silicon (Si)-doped n-type GaAs wafers are used as device substrates, and the GaAs wafers are required to have a strictly controlled carrier concentration and a low dislocation density. Specifically, the carrier concentration should be 1.5×10 18 cm -3 More than 2.9 x 10 18 cm -3The following range is desirable, and regarding the low dislocation density, the maximum etch pit density is 1200 cm for wafers smaller than 6 inches (e.g., 4 inches or less). -2 Below, for wafers 6 inches or larger, the maximum etch pit density is 1500 cm -2 It is desirable to do the following:

[0008] From the GaAs ingot disclosed in Patent Document 1, only a limited number of wafers satisfying these conditions of maximum carrier concentration and etch pit density can be obtained, leaving a problem in terms of productivity. [Means for solving the problem]

[0009] During crystal growth, the Si concentration in the GaAs melt increases as crystallization progresses due to the segregation of Si, and the carrier concentration increases along with the Si concentration from the seed side to the tail side of the ingot. The lower limit of the carrier concentration on the seed side of the straight body of the ingot is set to 1.5×10 18 cm -3If the amount of Si raw material added as a dopant to the GaAs melt is increased in an attempt to exceed this limit, polycrystallization may occur in the early stages of crystal growth, making it impossible to obtain a single crystal ingot. For example, in the manufacture of a 4-inch GaAs ingot, if GaAs raw material that does not contain Si is used and more than 300 wtppm of Si raw material is added as a dopant, polycrystallization is likely to occur. Therefore, the inventors have conducted intensive research to achieve the above-mentioned object, and have found that in a method for producing a GaAs ingot in which a seed crystal, a Si raw material as a dopant, a GaAs raw material, and boron oxide as a sealant are placed in a crucible and crystal growth is performed by a vertical boat method, the Si raw material is used as a dopant, and a predetermined amount of Si is doped into the GaAs raw material as a raw material, and a predetermined amount of SiO2 is contained in the sealant, thereby controlling the Si concentration of the GaAs melt during crystal growth, and the carrier concentration and etch pit density can be within a desired range in most of the straight body of the ingot without polycrystallizing the ingot even if the total amount of Si in the melt exceeds an amount that may cause polycrystals if the GaAs raw material is not doped with a predetermined amount of Si (for example, 300 wtppm for 4 inches), and thus the present invention has been completed. Hereinafter, the amount obtained by adding the amount of Si in the Si raw material as a dopant to the amount of Si in the GaAs raw material is referred to as the total amount of silicon charge.

[0010] The gist and configuration of the present invention are as follows. [1] A method for producing a GaAs ingot, in which a seed crystal, a silicon raw material dopant, a GaAs raw material, and boron oxide as a sealant are placed in a crucible and crystal growth is performed by the vertical boat method, The GaAs raw material is Si-doped GaAs having a Si concentration of 20 to 200 wtppm relative to GaAs, The charge amount of the Si raw material is 200 to 300 wtppm relative to GaAs, The boron oxide contains more than 5 mol% of SiO2 calculated as Si, the Si raw material, the GaAs raw material, and the boron oxide are melted by heating, and then crystal growth is performed while stirring the liquid boron oxide. [2] A method for producing a GaAs ingot having a diameter of 140 mm or less, wherein the total silicon charge, which is the sum of the Si in the GaAs raw material and the Si raw material, exceeds 300 wtppm relative to GaAs, or A method for producing a GaAs ingot having a diameter of a straight body portion exceeding 140 mm, wherein the charge amount of the Si raw material is 200 to 250 wtppm relative to GaAs, and a total silicon charge amount, which is the sum of the Si in the GaAs raw material and the Si raw material, exceeds 250 wtppm relative to GaAs. [3] A GaAs ingot having a diameter of 140 mm or less at the body portion, in which wafers obtained from 70% or more of the body portion have a carrier concentration of 1.5×10 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1200 cm -2 is less than or equal to, or A GaAs ingot having a diameter of more than 140 mm at its straight body, in which 70% or more of the straight body is used to obtain wafers having a carrier concentration of 1.5×10 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1500 cm -2 Below is a GaAs ingot. Effect of the Invention

[0011] According to the present invention, there are provided a GaAs ingot and a method for producing the same, which enable GaAs wafers with a strictly controlled carrier concentration and a low dislocation density to be efficiently obtained. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic diagram of a GaAs ingot according to the present invention. [Diagram 2]This is a schematic diagram showing 69 areas set on a 6-inch wafer for measuring etch pit density (EPD). [Diagram 3] 1 is a schematic cross-sectional view of a manufacturing apparatus used for manufacturing a GaAs ingot according to the present invention. [Figure 4] 1 is a schematic cross-sectional view of a crucible 3 used in the manufacture of a GaAs ingot according to the present invention, showing a state in which the crucible is filled with raw materials and the like before the start of crystal growth.

[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0014] <GaAsインゴット> (Seed side, center and tail side of GaAs ingot) FIG. 1 is a schematic diagram of a GaAs ingot according to the present invention, showing the position 15 where the cone part changes to the straight body part, the position (middle) 16 which is half the length from the position 15 to the position 17, and the position 17 where the straight body part ends. The GaAs ingot has a straight body part 18 with a substantially uniform diameter through a region 19 (also called the cone part) where the diameter increases from the seed crystal 6 (also called the seed). The part from the position 17 where the straight body part ends to the completion of growth is called the tail. If the length from the position 15 where the cone part changes to the straight body part to the position 17 where the straight body part used for wafer processing ends is taken as 100%, the former position 15 is taken as 0%, and the latter position 17 is taken as 100%, then the range of 0 to 5% is taken as the seed side of the straight body part (hereinafter also referred to as the seed side), the range of 40 to 60% is taken as the center part of the straight body part (hereinafter also referred to as the center part), and the range of 88 to 100% is taken as the tail side of the straight body part (hereinafter also referred to as the tail side). The position 17 (100% position) where the straight body portion ends is the position of 90% of the volume (position of 90% crystallization rate) when the volume of the entire ingot is 100%. Figure 1 shows position 16, which is halfway (50%) between positions 15 and 17. Hereinafter, position 16 will also be referred to simply as the middle. The position of each wafer in the straight body portion as a percentage from the end of the straight body portion on the seed side is also referred to as the "position from the straight body seed." In the GaAs ingot, the solid-liquid interface moves from the seed side 15 to the tail side 17, and crystal growth occurs.

[0015] The average and maximum values of the carrier concentration and the etch pit density (EPD) for the GaAs ingot according to the present invention can be obtained by measuring the wafer obtained from the straight body portion 18 of the GaAs ingot.

[0016] The diameter of the GaAs ingot 18 is not particularly limited and may be less than 140 mm or 140 mm or more. The diameter of the GaAs ingot 18 can be, for example, 50 mm or more and less than 140 mm, or 140 mm or more and 162 mm or less. The size of the wafer can be appropriately selected according to the diameter of the straight body portion 18 of the GaAs ingot, and can be, for example, 2 to 8 inches. When the diameter of the GaAs ingot 18 is less than 140 mm, usually, the size of the wafer is less than 6 inches, and when the diameter of the GaAs ingot 18 is 140 mm or more, usually, the size of the wafer is 6 inches or more.

[0017] <Manufacturing method of GaAs ingot> The manufacturing method of the GaAs ingot according to the present invention is a method of performing crystal growth by the vertical boat method with a seed crystal, a Si raw material as a dopant, a GaAs raw material, and boron oxide as a sealing agent accommodated in a crucible. As the vertical boat method, either a vertical gradient freeze (VGF) method or a vertical Bridgman (VB) method can be used.

[0018] Hereinafter, this manufacturing method will be described in more detail with reference to FIGS. 3 and 4.

[0019] (Manufacturing apparatus and temperature control) FIG. 3 schematically shows a cross-sectional view of an example of a manufacturing apparatus for use in the manufacturing method of the GaAs ingot according to the present invention. The manufacturing apparatus shown in FIG. 3 comprises an airtight container 7 which can be evacuated to a vacuum and filled with an atmospheric gas from the outside, a crucible 3 arranged in the center of the airtight container 7, a crucible storage container (susceptor) 2 which houses and holds the crucible 3, a mechanism 14 (only the lifting / rotating rod is shown) which raises and lowers and / or rotates the crucible storage container (susceptor) 2, and a heater 1 which is installed to surround the crucible storage container (susceptor) 2 within the airtight container 7. An upper rod 21 equipped with a stirring blade 20 that can rotate and move up and down is disposed on the upper part of the crucible 3. The stirring blade 20 and the upper rod 21 form a stirring means, but the stirring blade 20 is removable from the upper rod 21, and a sealant container or other members can be attached to the upper rod 21. The crucible 3 may be made of pyrolytic boron nitride (PBN). In Fig. 3, the crucible 3 is filled with a seed crystal 6, a compound semiconductor raw material 5 (also called a raw material melt), and boron oxide (B2O3) 4 as a sealant, and the airtight container 7 is filled with an inert gas 8, for example.

[0020] Fig. 4 is a schematic cross-sectional view of an example of a crucible for use in a GaAs ingot manufacturing method according to the present invention, showing a state where the crucible is filled with raw materials before the start of crystal growth. A seed crystal 6, a GaAs raw material 9, a Si raw material 10 as a dopant, and boron oxide 4 as a sealant are filled in the crucible 3 shown in Fig. 4. In Fig. 4, the GaAs raw material 9 is prepared by preparing crushed GaAs polycrystals (9A), cylindrical GaAs polycrystals (9B), and disk-shaped GaAs polycrystals (9C), and the Si raw material is placed in a container made of the cylindrical GaAs polycrystals (9B) and disk-shaped GaAs polycrystals (9C). However, the present invention is not limited to this embodiment, and for example, only crushed GaAs polycrystals may be filled.

[0021] After these fillings are completed, in a growth furnace filled with an inert gas, the GaAs raw material 9 is heated to 1238°C or higher, the melting point of GaAs, while applying a temperature gradient using a PID-controlled heater to lower the temperature on the seed crystal 6 side so as not to melt the seed crystal 6, thereby melting the GaAs raw material 9 and boron oxide 4, and dissolving the Si raw material 10 into the GaAs raw material 9. Next, the temperature near the seed crystal 6 is raised until the upper part of the seed crystal 6 melts, and the entire temperature is gradually lowered while applying a temperature gradient to obtain a GaAs ingot. At this time, the temperature drop rate is preferably 10°C / h or less.

[0022] (stir) In the GaAs manufacturing method according to the present invention, liquid boron oxide 4 is stirred during crystal growth. Stirring is preferably started between the start of crystal growth on the seed side of the straight body and the middle (1 to 50% from the seed of the straight body). Stirring is preferably continued until crystal growth on the tail side of the straight body is completed, and may be continued until crystal growth is completed.

[0023] The stirring is preferably performed by rotating a stirring means disposed in the sealant (boron oxide 4). In the present invention, it is desirable to maintain the Si concentration in the raw material melt at a relatively high level by preventing the sealant from absorbing Si as much as possible from the start of crystal growth until the start of stirring, and stirring is used to a minimum in order to suppress an extreme increase in the Si concentration due to segregation. For this reason, the rotation speed may be changed stepwise or continuously from the seed side of the straight body to the tail side, but the maximum rotation speed reached is preferably 3 rpm or less. The stirring means can have a shape in which stirring blades 20 are attached around a rotating shaft. The shape of the stirring blade 20 is not particularly limited, and may be made of a plate-like member of a predetermined shape, for example, 2 to 8 substantially rectangular plate-like members, and examples of the material include carbon, BN, etc. The plate-like members are preferably attached at an inclination angle of 45° to 135° with respect to the interface formed between the raw material melt and boron oxide 4 in a stationary state. The stirring blade 20 is preferably sized so that the area formed by the rotational trajectory when the stirring means is rotated is 30% or more of the area of ​​the interface formed between the raw material melt and boron oxide 4 in a stationary state, and more preferably 70% or more. The distance between the lower end of the stirring blade 20 and the interface formed between the raw material melt and the boron oxide 4 in a stationary state is preferably less than 2 mm, and more preferably 1 mm or less. However, it is preferable that the lower end of the stirring blade 20 does not come into contact with the interface.

[0024] The stirring is preferably performed at a rotation speed of 0.5 rpm or more when the crystal growth reaches the intermediate stage, and more preferably at a rotation speed of 2.5 rpm or more. After the intermediate stage, the segregation of Si in the melt increases and the carrier concentration reaches 2.5×10 18 cm -3 Since there is a tendency for the concentration of silicon in the molten liquid to exceed this value, strong stirring at this time is performed to promote the absorption of silicon in the encapsulant and suppress a sudden rise in the silicon concentration due to segregation, thereby suppressing the occurrence of dislocations and a sudden rise in the carrier concentration.

[0025] (seed crystal) There is no particular limitation on the seed crystal 6, and a known seed crystal can be used. There is no particular limitation on the size of the seed crystal 6, and it is sufficient that the seed crystal 6 has a cross-sectional area of, for example, 1 to 20% of the cross-sectional area having the inner diameter of the crucible 3 as a diameter, and preferably has a cross-sectional area of ​​3 to 17%. When the diameter of the crystal to be grown exceeds 100 mm, the cross-sectional area of ​​the seed crystal 6 can be 2 to 10% of the cross-sectional area having the inner diameter of the crucible as a diameter.

[0026] (Crucible inner diameter and wafer size) The inner diameter of the crucible 3 is preferably slightly larger than the desired wafer size. The desired wafer size can be, for example, 2 inches or more, and is preferably 3 inches or more. There is no particular upper limit to the wafer size, and it can be, for example, 8 inches or less. From an ingot having a straight body diameter of 140 mm or less, wafers having a diameter of, for example, 2 inches to 4 inches are produced, and from an ingot having a straight body diameter of more than 140 mm, wafers having a diameter of, for example, 6 inches to 8 inches are produced.

[0027] (GaAs raw material) As the GaAs raw material, Si-doped GaAs with a Si concentration of 20 to 200 wtppm relative to GaAs is used. The GaAs raw material used may be polycrystalline or single crystalline. The Si concentration in the GaAs raw material refers to the Si concentration calculated from the carrier concentration measured by Hall measurement. If the Si concentration calculated from the carrier concentration is within this range, single crystallization is not hindered during crystal growth even if the total amount of silicon charge to GaAs combined with the Si raw material 10 described later is large, and the carrier concentration in the resulting GaAs ingot can be easily controlled to a desired range. Since the GaAs raw material is melted for use, it is sufficient that the average Si concentration of the entire GaAs raw material used is within the above range, and GaAs raw materials with different Si concentrations may be used in combination.

[0028] Here, the Si concentration of Si-doped GaAs polycrystal calculated from the carrier concentration can be measured and calculated as follows. Note that the calculation can be done in the same way in the case of single crystal. Note that the following method of converting carrier concentration to Si concentration is based on the assumption that the dopant of GaAs is Si, and that no other p-type or n-type dopants are intentionally included. <Carrier concentration by Hall measurement> · Wafer-like objects with a thickness of approximately 1 mm are cut from the seed side and tail side of the Si-doped GaAs polycrystal. A 10 mm square scratch is made with a marking needle from the largest possible grain boundary of a polycrystalline wafer, and a 10 mm square sample is cut out from the centre of the wafer. After attaching indium electrodes to the four corners of the sample and heating it to 330-360℃, the carrier concentration is measured by the Van der Pauw method.

[0029] <Conversion of activation rate to Si concentration> The activation rate is set to 48%, and the carrier concentration is divided by 0.48 to obtain the Si atom concentration (cm -3 ) is calculated. GaAs bulk density (5.3161g / cm 3 ), Avogadro's number, and the atomic weight of Si (28.1) are used to calculate the unit of the Si atomic concentration (cm -3 ) to units (wtppm).

number

[0030] The method for synthesizing Si-doped GaAs as the GaAs raw material is not limited, and may be, for example, a method in which synthesis is performed in a crucible using the vertical boat method or a method in which synthesis is performed in a boat placed in an ampoule using the horizontal boat method. During synthesis, an amount of Si raw material corresponding to the desired Si concentration for GaAs is charged.

[0031] When the vertical boat method is used, for example, a crucible is filled with high-purity Ga, high-purity As, and a Si raw material (e.g., high-purity Si shots or crushed high-purity Si substrates), and crystals are grown to obtain Si-doped GaAs polycrystals. The crucible can be filled in the following order: half of the high-purity As, the entire amount of the Si raw material, the remaining half of the high-purity As, and high-purity Ga, but the filling order is not limited thereto. In the synthesis of GaAs polycrystals, it is preferable not to use boron oxide as a sealant in order to promote Si doping and to suppress the amount of boron in the GaAs melt when used as a GaAs raw material.

[0032] For the Si-doped GaAs used as the GaAs raw material, recycled products that have been processed or crushed, or parts other than the body part of other Si-doped GaAs single crystal ingots that are not processed into wafers (the cone part or the area after the tail side of the body part), or unnecessary parts generated during wafer processing, can also be used.

[0033] (Dopant) A silicon source material 10 is used as a dopant. The silicon source material 10 can be high-purity silicon shot or crushed high-purity silicon substrates, and is added to the GaAs source material 9. The charge amount of the Si raw material 10 is 200 to 300 wtppm relative to the GaAs in the GaAs raw material 9. It is more preferable that it is 220 to 300 wtppm or more, and further more preferable that it is 240 to 290 wtppm.

[0034] For an ingot with a diameter of the body of 140 mm or less, the total silicon charge amount, which is the sum of the Si in the GaAs raw material and the Si raw material 10, is preferably more than 300 wtppm relative to GaAs. In this case, the charge amount of the Si raw material 10 is more preferably 220 to 300 wtppm or less relative to GaAs. For an ingot having a diameter of the body portion exceeding 140 mm, the charge amount of the Si source material 10 is preferably 200 to 250 wtppm relative to GaAs, more preferably 220 to 250 wtppm, and the total silicon charge amount, which is the sum of the Si in the GaAs source material and the Si source material 10, is preferably more than 250 wtppm relative to GaAs. For example, in the manufacture of a 4-inch GaAs ingot, if a GaAs raw material not containing Si is used and more than 300 wtppm of Si raw material is added as a dopant, polycrystallization tends to occur, and in the manufacture of a 6-inch GaAs ingot, if a GaAs raw material not containing Si is used and more than 250 wtppm of Si raw material is added as a dopant, polycrystallization tends to occur. However, in the case of the present invention, where Si is previously contained in the GaAs raw material, even if the total silicon charge amount is set to such an amount, it is possible to include Si in the GaAs melt without polycrystallization, and the carrier concentration of the entire straight body portion can be increased. By controlling the total silicon charge amount as described above, single crystallization during crystal growth is not hindered, and the carrier concentration in the resulting GaAs ingot can be easily controlled to a desired range. Here, the charge amount of the Si source 10 does not include the amount of silicon contained in the Si-doped GaAs source and boron oxide, and the total silicon charge does not include the amount of silicon contained in the boron oxide.

[0035] The Si raw material 10 is preferably placed below (on the seed crystal side) the center of the crucible (the position corresponding to the center of the ingot). The Si raw material 10 may be placed in a GaAs container so that the dopant in the container does not come out of the container until the temperature at which the GaAs container melts. Since silicon has a lower density than GaAs, the dopant (silicon) floats up in the melt, which may reduce the silicon concentration in the GaAs melt on the seed crystal side and reduce the silicon concentration on the seed side of the GaAs ingot. The use of a GaAs container is effective in avoiding such a situation. The GaAs raw material can be processed and used as the GaAs container, and it may be a processed Si-doped GaAs single crystal or a processed Si-doped GaAs polycrystal.

[0036] As long as the effects of the present invention are not impaired, amphoteric dopants can be used other than the Si raw material 10, and examples of such dopants include In raw materials such as high-purity In and indium compounds (e.g., high-purity indium arsenide (InAs)).

[0037] Other elements that may be considered as dopants include beryllium (Be), magnesium (Mg), aluminum (Al), carbon (C), germanium (Ge), tin (Sn), nitrogen (N), sulfur (S), selenium (Se), tellurium (Te), and even zinc (Zn), cadmium (Cd), chromium (Cr), and antimony (Sb). Although unavoidable amounts of these elements are permitted, it is preferable that they are not added intentionally.

[0038] (Sealant) Boron oxide (B2O3)4 is used as a sealant. The boron oxide 4 contains SiO2 of more than 5 mol% in terms of Si. Within this range, the amount of Si absorbed by B2O3 in the raw material melt is suppressed, and the B of B2O3 is prevented from being incorporated into the single crystal, and the Si concentration of the raw material melt can be controlled within an appropriate range even when stirring is performed. The amount of SiO2 contained in the boron oxide 4 is preferably 6 mol% or more in terms of Si. Since there is a limit to the amount of Si that can be dissolved in boron oxide, the amount of SiO2 contained in the boron oxide 4 can be 10 mol% or less in terms of Si, and is preferably 7 mol% or less.

[0039] The content of boron oxide 4 as the sealant relative to the GaAs raw material 9 can be 0.02 wt% or more, and preferably 0.03 wt% or more, in order to suppress the loss of As from the raw material melt, and can be 0.10 wt% or less, and preferably 0.06 wt% or less, in order to prevent the sealant from taking in an excessive amount of Si while being stirred.

[0040] According to the method for producing a GaAs ingot according to the present invention, a GaAs ingot having a straight body diameter of 140 mm or less is obtained, and wafers obtained from 70% or more (preferably 90% or more) of the straight body have a carrier concentration of 1.5×1018 ~2.9×10 18 cm -3 and the maximum etch pit density is 1200 cm -2 or less, or a GaAs ingot having a diameter of a straight body portion exceeding 140 mm, and wafers obtained from 70% or more of said straight body portion have a carrier concentration of 1.5×10 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1500 cm -2 A GaAs ingot is obtained, which is shown below.

[0041] That is, when the diameter of the straight body of a GaAs ingot is 140 mm or less, of the total number of wafers that can be cut from the straight body, 70% or more (preferably 90% or more) of the wafers have a carrier concentration of 1.5×10 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1200 cm -2 The following conditions are met: The maximum etch pit density is 1000 cm -2 It is more preferable that the lower limit of the maximum value of the etch pit density is not particularly limited, and may be zero. More preferably, 92% or more of the wafers satisfy the above condition, but all the wafers (100% of the wafers) may satisfy the above condition.

[0042] When the diameter of the straight body of a GaAs ingot is more than 140 mm, 70% or more of the wafers that can be cut from the straight body have a carrier concentration of 1.5×10 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1500 cm -2 The following condition is satisfied: The lower limit of the maximum value of the etch pit density is not particularly limited, and may be zero. More preferably, 75% or more of the wafers satisfy the above condition, but all the wafers (100% of the wafers) may satisfy the above condition.

[0043] (Method of measuring carrier concentration) The carrier concentration is determined by dividing a 10 mm x 10 mm area from the center of a wafer extracted from a GaAs ingot, attaching indium electrodes to the four corners, heating to 330 to 360°C, and then measuring the carrier concentration by Hall measurement using the Van der Pauw method.

[0044] (Method of measuring etch pit density (EPD)) Etch pit density (EPD) is measured by pretreating the surface of a wafer extracted from a GaAs ingot with a sulfuric acid-based mirror-finish etching solution (H2SO4:H2O2:H2O = 3:1:1 (volume ratio)), then immersing it in molten KOH at a liquid temperature of 320°C for 35 minutes to generate etch pits, and then counting the number of etch pits. Etch pits are those that have a hexagonal shape characteristic of zinc blende crystals and have a major axis (the length of the diagonal line passing through the center) of 20 μm or more.

[0045] The etch pit density (EPD) is measured by setting areas of 3 mm diameter at 69 or 37 points on the wafer, observing each area with a microscope, and counting the etch pits that have occurred. The 69-point or 37-point area is to be distributed evenly over the entire surface of the wafer. For a 6-inch wafer, an area of ​​69 points is set at positions evenly distributed at 15 mm intervals, and for a 3-inch wafer, an area of ​​37 points is set at positions evenly distributed at 10 mm intervals. When the 69 areas are set at equally distributed positions, the areas are spaced 5 mm apart for a 2-inch wafer, 10 mm apart for a 4-inch wafer, and 20 mm apart for an 8-inch wafer. FIG. 2 shows a schematic diagram of 69 areas set on a 6-inch wafer.

[0046] A 10x objective lens with a field of view diameter of 1.73 mm was used to observe each area. For each area, the field of view with the most pits was found, and the etch pits were counted. The number of etch pits counted was calculated as the number of etch pits per unit area (cm-2 ) is converted. Among the converted values of the number of etch pits in each area, the maximum value is defined as the maximum value of the etch pit density (EPD). Also, the average value of the converted values of the number of etch pits in each area is defined as the average value of the etch pit density (EPD).

[0047] The GaAs wafer according to the present invention has a strictly controlled carrier concentration and a low dislocation density, and is suitable as a substrate for surface-emitting lasers such as VCSELs (vertical-cavity surface-emitting lasers).

[0048] What has been described above shows examples of typical embodiments of the present invention, and the present invention is not limited thereto.

Example

[0049] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited by the following examples at all.

[0050] (GaAs raw material) <GaAs raw material 1> It is a GaAs polycrystal produced by synthesizing 6N (purity of 99.9999% or more) Ga and 6N As.

[0051] <GaAs raw material 2> It is a Si-doped GaAs polycrystal synthesized by the vertical boat method using 350 wtppm of high-purity Si for 6N (purity of 99.9999% or more) Ga and 6N As without using B2O3 as a sealing agent. The Si concentration converted from the measurement value of Hall measurement is 80 wtppm with respect to GaAs. Since B2O3 is not used, boron is not added to the Si-doped GaAs polycrystal.

[0052] <GaAs raw material 3> It is a recycled product obtained by crushing parts other than the straight body part in other single crystal ingots. The Si concentration converted from the measurement value of Hall measurement is 33 wtppm with respect to GaAs. Boron is contained in the raw material.

[0053] <GaAs raw material 4> This is a Si-doped GaAs polycrystal synthesized by the vertical boat method using high-purity Si at 450 wtppm for 6N (purity of 99.9999% or more) Ga and 6N As without using B2O3 as a sealing agent. The Si concentration换算 from the measurement value of Hall measurement is 175 wtppm with respect to GaAs. Since B2O3 is not used, boron is not added to the Si-doped GaAs polycrystal.

[0054] (Sealing agent) <Sealing agent 1> It is B2O3 containing 7 mol% of SiO2 in terms of Si.

[0055] <Sealing agent 2> It is B2O3 containing 5.3 mol% of SiO2 in terms of Si.

[0056] (Crystal number 1) Using a manufacturing apparatus having the configuration shown in Fig. 3, a GaAs ingot was manufactured. The stirring blades are four square plate-like members made of materials that do not affect crystal properties, such as carbon and BN, attached to a rod, and the area formed by the rotation locus when rotated is 50% or more of the area of the interface formed by the GaAs melt and B2O3 in a stationary state.

[0057] (Filling of raw materials into the crucible) A PBN crucible with an inner diameter of 112 mm and an inner diameter of the seed part of 6 to 6.5 mm was prepared as the crucible. As shown in FIG. 4, the crucible was filled with 11,900 g of GaAs raw material 1 and GaAs seed crystals cut so that the (100) plane was the crystal growth surface. The diameter of the GaAs seed crystal was adjusted by combining mechanical grinding and etching so that it was 0.5 mm smaller than the inner diameter of the seed part of each crucible. In the middle of filling the GaAs raw material 1, high-purity Si shots were filled as a dopant (Si raw material) at 300 wtppm relative to GaAs. No impurity elements were intentionally added other than Si. The granular dopant (Si raw material) 10 was filled in a GaAs container sandwiched between the top and bottom of a cylindrical GaAs polycrystal 9B and disk-shaped GaAs polycrystals 9C, and the dopant in the container was prevented from coming out of the GaAs container until the temperature at which the GaAs container melted.

[0058] <Crystal growth> After these raw materials were filled, 550 g of sealing material 1 was filled. The filled crucible was set in a crucible storage container (susceptor). The inside of the manufacturing apparatus shown in Figure 3 was repeatedly evacuated and replaced with Ar gas to create an inert gas atmosphere, and then a single crystal was grown by the VGF method. In the crystal growth process, the raw material in the crucible was first heated to above 1238°C, the melting point of GaAs, to produce a melt while applying a temperature gradient using a PID-controlled heater to lower the temperature on the seed crystal side so as not to melt the GaAs seed crystal. After that, the temperature near the seed crystal was raised so that the top of the seed crystal melted, and then the temperature in the entire furnace was lowered at a rate of 0.5°C / h or less while applying a temperature gradient, thereby growing an n-type GaAs ingot with Si as the dopant. When the ingot had grown to the point where the cone part had grown to the crystal body, the stirring blade was inserted into the sealant so that the distance between the interface between the sealant (boron oxide) and the raw material melt and the bottom end of the stirring blade was 1 mm or less, and the bottom end did not come into contact with the interface. The stirring blade rotation speed was kept at 0 rpm until the ingot had grown to the middle, and then rotated at 0.5 rpm from the middle to the tail, and stirring was continued until the tail had grown. The resulting GaAs ingot has n-type conductivity.

[0059] <Evaluation> The straight body portion of the grown GaAs ingot was sliced ​​with a wire saw into wafers. The wafer size was equivalent to 4 inches. The length of the straight body portion was calculated based on the total number of wafers obtained from the straight body portion, which was 297, and the position of each wafer from the straight body seed was calculated. The carrier concentration was measured by the method described above for the wafers cut from the positions from the straight body seed shown in Table 1. In addition, the average and maximum EPD values ​​were measured by the method described above for the wafers cut from the positions from the straight body seed shown in Table 1. In addition, for the carrier concentration and EPD from the seed side to the tail side, which are the measured wafer positions (1st to 287th) listed in Table 1, the carrier concentration of the wafers in the measurement range from the seed side to the tail side was calculated as 1.5 × 10 for the total number of wafers (297) cut from the GaAs ingot. 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1200 cm -2 The following percentages (percentage of wafers that satisfy the specified conditions) were calculated and are shown in Table 1. In calculating the percentage of wafers that satisfy the specified conditions, wafers located outside the wafers on the tail side among the wafers to be measured and on the side closer to 100% from the straight body seed were deemed not to satisfy the specified conditions.

[0060] (Crystal number 2~3) GaAs ingots of crystal numbers 2 and 3 were produced and evaluated in the same manner as crystal number 1, except that the conditions were changed as shown in Table 1. The obtained GaAs ingots have an n-type conductivity.

[0061] (Crystal No. 4) A GaAs ingot of crystal number 4 was produced and evaluated in the same manner as crystal number 1, except that after filling the GaAs seed crystal, GaAs raw material 1, and high-purity Si shot, a quartz plate (disk-shaped with a diameter of 51 mm and a thickness of 5 mm) was placed thereon, and then filling with sealing agent 1. The obtained GaAs ingot had an n-type conductivity.

[0062] [Table 1]

[0063] Table 1 shows GaAs ingots with a diameter of 140 mm or less. For crystal numbers 2 and 3, 96.6% of the total number of wafers (297 wafers) in the measurement range from the seed side to the tail side in Table 1 had a carrier concentration of 1.5 × 10 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1200 cm -2 The following conditions were met: Crystal No. 1 is an example of a GaAs ingot grown using high-purity GaAs polycrystalline raw material that was not doped with Si, but the percentage of wafers that satisfied the above conditions was only 60.9%. Crystal No. 4 is an example in which a GaAs ingot was produced using a quartz plate, and corresponds to Patent Document 1. In this example, the quartz plate reduces the effect of suppressing the increase in the Si concentration due to stirring, so the increase in the carrier concentration from the center onwards could not be suppressed, and the percentage of wafers that satisfied the above conditions was only 67.6%. For crystal numbers 1 and 4, even if the wafers located closer to 100% from the seed than the wafer closest to the tail among the wafers being measured satisfy the specified conditions, the proportion of wafers that satisfy the conditions is less than 70%.

[0064] (Crystal No. 5) <Filling the crucible with raw materials> A PBN crucible with an inner diameter of 159.9 mm and an inner diameter of 6.0 to 6.5 mm was prepared as the crucible. The crucible was filled with 20,000 g of GaAs raw material 1 and GaAs seed crystals cut so that the (100) plane was the crystal growth surface. The diameter of the GaAs seed crystals was adjusted by combining mechanical grinding and etching so that it was about 0.5 mm smaller than the inner diameter of the seed part of each crucible. In the middle of filling the GaAs polycrystals, high-purity Si shots were filled as a dopant (Si raw material) at 210 wtppm relative to the GaAs. No impurity elements were intentionally added other than Si.

[0065] <Crystal growth> After these raw materials were filled, 965±10 g of sealant 2 was filled. The filled crucible was set in a crucible storage container (susceptor). The inside of the manufacturing apparatus shown in Figure 3 was repeatedly evacuated and replaced with Ar gas to create an inert gas atmosphere, and then a single crystal was grown by the VGF method. In the crystal growth process, the raw material in the crucible was first heated to above 1238°C, the melting point of GaAs, to produce a melt while applying a temperature gradient using a PID-controlled heater to lower the temperature on the seed crystal side so as not to melt the GaAs seed crystal. After that, the temperature near the seed crystal was raised so that the top of the seed crystal melted, and then the temperature in the entire furnace was lowered at a rate of 0.5°C / h or less while applying a temperature gradient, thereby growing an n-type GaAs ingot with Si as the dopant. When the ingot had grown to the point where the cone part reached the crystal body part, the stirring blade was inserted into the sealant so that the distance between the interface between the boron oxide sealant and the raw material melt and the lower end of the stirring blade was 1 mm or less, and the lower end did not come into contact with the interface. The rotation speed of the stirring blade 20 was kept at 0 rpm until the ingot grew to the middle, and then rotated at 0.5 rpm from the middle to the tail, and stirring was continued until the tail growth was completed. The resulting GaAs ingot has n-type conductivity.

[0066] <Evaluation> The straight body portion of the grown GaAs ingot was sliced ​​with a wire saw into wafers. The wafer size was equivalent to 6 inches. The length of the straight body portion was calculated based on the total number of wafers obtained from the straight body portion being 161, and the position of each wafer from the straight body seed was calculated. The final cut surface was located 20 mm from the end of the ingot opposite the seed crystal side (towards the seed side). The carrier concentration was measured by the method described above for the wafers cut from the positions from the straight body seed shown in Table 2. In addition, the average and maximum EPD were measured by the method described above for the wafers cut from the positions from the straight body seed shown in Table 2. In addition, for the carrier concentration and EPD from the seed side to the tail side, which are the measured wafer positions (2nd to 148th wafers) listed in Table 2, the carrier concentration of the wafers in the measurement range from the seed side to the tail side was calculated as 1.5 × 10 for the total number of wafers (161 wafers) cut from the GaAs ingot. 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1500 cm -2 The following percentages (percentage of wafers satisfying the specified conditions) are shown in Table 2. In calculating the percentage of wafers satisfying the specified conditions, wafers positioned outside the wafers to be measured were considered not to satisfy the specified conditions.

[0067] (Crystal No. 6) A GaAs ingot of crystal number 6 was produced and evaluated in the same manner as crystal number 5, except for changing the conditions shown in Table 2. The resulting GaAs ingot has an n-type conductivity.

[0068] (Crystal No. 7) A GaAs ingot of crystal number 7 was produced and evaluated in the same manner as crystal number 6, except that GaAs source material 4 (Si concentration 175wtppm) was used as shown in Table 2, and the rotation speed of the stirring blade was kept at 0 rpm until the growth reached the middle, and then rotated at 2.5 rpm from the middle to the tail. The conductivity type of the obtained GaAs ingot was n-type.

[0069] [Table 2]

[0070] Table 2 shows GaAs ingots with a diameter of more than 140 mm in the straight body. For crystal number 6, 79.1% of the total number of wafers (161) in the measurement range from the seed side to the tail side obtained from the straight body had a carrier concentration of 1.5 × 10 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1500 cm -2 The following conditions were met: For crystal number 7, 77.1% of the total number of wafers (161) in the measurement range from the seed side to the tail side obtained from the straight body had a carrier concentration of 1.5 × 10 18 ~2.9×10 18 cm -3 and the maximum etch pit density is 1500 cm -2 The following conditions were met: On the other hand, crystal No. 5 is an example in which a GaAs ingot was grown using high-purity GaAs polycrystalline raw material that was not doped with Si, but the proportion of wafers that satisfied the above conditions was only 37.7%. In the case of crystal number 5, even if the wafers positioned outside the wafer to be measured satisfy the predetermined conditions, the ratio of wafers that satisfy the conditions is less than 70%. [Industrial Applicability]

[0071] INDUSTRIAL APPLICABILITY According to the present invention, it is possible to provide a GaAs ingot which has a strictly controlled carrier concentration and from which GaAs wafers having a low dislocation density can be efficiently obtained, and a method for producing the same, and thus the present invention is highly industrially useful. [Explanation of symbols]

[0072] 1 Heater 2 Crucible storage container (susceptor) 3 Crucible Boron oxide 5. Compound semiconductor raw materials (raw material melt) 6 seed crystals 7. Airtight container 8. Inert Gas 9 GaAs polycrystalline raw material 10 Si raw material 14 Crucible lifting and rotation mechanism 15 The position where the cone section changes to the straight body section 16 Halfway between position 15 and position 17 (middle) 17 End of the straight body 18 GaAs ingot straight body 19 Cone part of GaAs ingot 20 Stirring blade 21 Upper Rod 30 6 inch wafers 31 Area

Claims

1. A method for producing a GaAs ingot, comprising: placing a seed crystal, a silicon source material as a dopant, a GaAs source material, and boron oxide as a sealant in a crucible and growing the crystal by a vertical boat method; The GaAs raw material is Si-doped GaAs having a Si concentration of 20 to 200 wtppm relative to GaAs, The charge amount of the Si raw material is 200 to 300 wtppm relative to GaAs, The boron oxide is more than 5 mol% of SiO in terms of Si. 2 Including, the Si raw material, the GaAs raw material, and the boron oxide are melted by heating, and then crystal growth is carried out while stirring the liquid boron oxide.

2. A method for producing a GaAs ingot having a diameter of 140 mm or less, wherein the total silicon charge amount, which is the sum of the Si in the GaAs raw material and the Si raw material, exceeds 300 wtppm relative to GaAs; or 2. A method for producing a GaAs ingot having a diameter of a straight body portion exceeding 140 mm, wherein the charge amount of the Si raw material is 200 to 250 wtppm relative to GaAs, and a total silicon charge amount, which is the sum of the Si in the GaAs raw material and the Si raw material, exceeds 250 wtppm relative to GaAs.

3. A 4-inch Si-doped GaAs ingot, wherein 4-inch wafers obtained from 70% or more of the straight body have a carrier concentration of 1.5×10 18 ~2.9 x 10 18 cm -3 and the maximum etch pit density is 1200 cm -2 is less than or equal to, or A Si-doped GaAs ingot having a diameter of a straight body portion of more than 140 mm, wherein wafers obtained from 70% or more of the straight body portion have a carrier concentration of 1.5×10 18 ~2.9 x 10 18 cm -3 and the maximum etch pit density is 1500 cm -2 Below is a Si-doped GaAs ingot.

Citation Information

Patent Citations

  • Semi-insulating III-V wafers with low etch pit density (EPD)

    JP2010526755A

  • Si-DOPED GaAs SINGLE CRYSTAL INGOT AND PROCESS FOR PRODUCING THE SAME, AND Si-DOPED GaAs SINGLE CRYSTAL WAFER PRODUCED FROM THE Si-DOPED GaAs SINGLE CRYSTAL INGOT

    JP2012006829A

  • METHOD FOR PRODUCING GaAs SINGLE CRYSTAL AND GaAs SINGLE CRYSTAL WAFER

    JP2012246156A

  • Low etch pit density 6 inch semi-insulating gallium arsenide wafers

    US20200190696A1

  • Gallium arsenide crystalline body and gallium arsenide crystal substrate

    WO2019008663A1