Water-based antifouling paint composition

A water-based antifouling paint composition with a synthetic resin and high molecular weight rosin compound addresses storage stability and long-term antifouling issues, providing effective and environmentally friendly antifouling solutions.

JP7576722B1Active Publication Date: 2024-10-31CHUGOKU MARINE PAINTS
View PDF 28 Cites 0 Cited by

Patent Information

Application Number
JP2024050082
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-10-31
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

Water-based antifouling paint compositions face challenges with high water affinity leading to poor long-term antifouling properties and insufficient storage stability, particularly when containing rosin compounds.

Method used

A water-based antifouling paint composition comprising a synthetic resin, a rosin compound with a weight average molecular weight of 800 or more, and water, with specific ratios and properties to enhance storage stability and long-term antifouling performance.

Benefits of technology

The composition achieves excellent storage stability and long-term antifouling properties, reducing volatile organic compounds and minimizing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576722000001
    Figure 0007576722000001
  • Figure 0007576722000002
    Figure 0007576722000002
  • Figure 0007576722000003
    Figure 0007576722000003
Patent Text Reader

Abstract

Provided is a water-based antifouling coating composition having excellent storage stability. The present invention relates to a water-based antifouling coating composition comprising a synthetic resin (A), a rosin-based compound (B) having a weight-average molecular weight of 800 or more, and water (C).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a water-based antifouling paint composition and a method for producing the same, an antifouling coating film, a substrate with an antifouling coating film, and a method for producing a substrate with an antifouling coating film. [Background technology]

[0002] Conventionally, organic solvent diluted compositions have been used as antifouling coating compositions. In recent years, from the viewpoint of environmental conservation or improvement of the coating work environment, there has been a demand for water-based antifouling coating compositions, i.e., water-based antifouling coating compositions (see, for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 51-014936 [Patent Document 2] JP 2009-173914 A [Patent Document 3] JP 2003-277680 A [Patent Document 4] International Publication No. 2023 / 232825 Summary of the Invention [Problem to be solved by the invention]

[0004] The conversion of antifouling coating compositions to water-based compositions is effective in reducing the amount of volatile organic compounds (VOCs). However, antifouling coating films formed from water-based antifouling coating compositions have high affinity with water. Therefore, it has been difficult for such antifouling coating films to exhibit long-term antifouling properties.

[0005] In response to such problems, the present inventors have found that an antifouling coating film containing a rosin-based compound tends to have excellent antifouling properties over a long period of time. However, as a result of further investigation, the present inventors have found that the storage stability of a water-based antifouling coating composition containing a rosin-based compound may be insufficient. One object of the present disclosure is to provide a water-based antifouling coating composition having excellent storage stability. [Means for solving the problem]

[0006] One embodiment of the aqueous antifouling coating composition of the present disclosure contains a synthetic resin (A), a rosin-based compound (B) having a weight-average molecular weight of 800 or more, and water (C). Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a water-based antifouling coating composition having excellent storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present disclosure will be described in detail. Each of the components described in this specification may be used alone or in combination of two or more. In this specification, the term "polymer" may be used without any particular distinction between homopolymers and copolymers. That is, the term "polymer" is used to mean both homopolymers and copolymers.

[0009] The term "(meth)acrylate" may mean either acrylate or methacrylate. The term "(meth)acrylic" may mean either acrylic or methacrylic. The term "(meth)acrylic acid" may mean either acrylic acid or methacrylic acid.

[0010] In this specification, when the numerical range is n1~n2, if n1 < n2, it means the numerical range from n1 to n2, and if n1 > n2, it means the numerical range from n2 to n1. In this specification, when a plurality of lower limit values and upper limit values are respectively described for a certain element, the numerical range formed by combining a value arbitrarily selected from the described lower limit values and a value arbitrarily selected from the described upper limit values is also regarded as being described.

[0011] The "structural unit derived from monomer X" means that when monomer X is represented as A 1 A 2 C=CA 3 A 4 (C=C is a polymerizable carbon-carbon double bond, and A 1 ~A 4 are each an atom or group bonded to a carbon atom. ), for example, it is a structural unit represented by the following formula.

[0012] [Water-based antifouling paint composition (Composition (I))

[0013] [Water-based antifouling paint composition (Composition (I)) The water-based antifouling paint composition of the present disclosure (hereinafter also referred to as "Composition (I)") contains a synthetic resin (A), a rosin-based compound (B), and water (C), which will be described below respectively.

[0014] [Synthetic resin (A)] Examples of the synthetic resin (A) include (meth)acrylic resins, styrene resins, and urethane resins. Among these, from the viewpoints of being able to easily form an antifouling coating film excellent in crack resistance in outdoor exposure tests, crack resistance in water immersion, and long-term antifouling properties, (meth)acrylic resins and styrene resins are preferred. From the viewpoints of being able to more easily form an antifouling coating film with better crack resistance and being easily available as the synthetic resin (A), (meth)acrylic resins are more preferred.

[0015] The (meth)acrylic resin has a structural unit derived from a (meth)acrylic monomer, and may further have a structural unit derived from an ethylenically unsaturated monomer copolymerizable with the (meth)acrylic monomer (hereinafter also referred to as "other ethylenically unsaturated monomer"). The (meth)acrylic resin may be a homopolymer of a (meth)acrylic monomer, a copolymer of two or more (meth)acrylic monomers, or a copolymer of a (meth)acrylic monomer and another ethylenically unsaturated monomer. The copolymer may be, for example, a random copolymer or a block copolymer. The (meth)acrylic resin may have two or more structural units derived from a (meth)acrylic monomer. The (meth)acrylic resin may have one or more structural units derived from another ethylenically unsaturated monomer.

[0016] Examples of the (meth)acrylic monomer include (meth)acrylic acid esters, (meth)acrylic acid amides, (meth)acrylonitrile, and (meth)acrylic acid.

[0017] Examples of (meth)acrylic acid esters include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate; aryl (meth)acrylates such as phenyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; 2-hydroxypropyl (meth)acrylate; and aryl (meth)acrylates such as phenyl (meth)acrylate. hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; alkoxyalkyl (meth)acrylates such as methoxybutyl (meth)acrylate, methoxyethyl (meth)acrylate, and ethoxybutyl (meth)acrylate; epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate; and aminoalkyl (meth)acrylates such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and butylaminoethyl (meth)acrylate.

[0018] Examples of (meth)acrylic acid amides include (meth)acrylic acid aminoalkylamides such as aminoethyl(meth)acrylamide, dimethylaminomethyl(meth)acrylamide, and methylaminopropyl(meth)acrylamide; and other amide group-containing (meth)acrylic monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-methylol(meth)acrylamide, methoxybutyl(meth)acrylamide, and diacetone(meth)acrylamide.

[0019] Other ethylenically unsaturated monomers include, for example, α-olefins such as ethylene, propylene, and 1-butene; conjugated dienes such as 1,3-butadiene, isoprene, and chloroprene; styrenic monomers such as styrene, α-methylstyrene, vinyl toluene, and halogenated styrenes; vinyl esters such as vinyl acetate and vinyl propionate; unsaturated monocarboxylic acids such as crotonic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; monoesters of unsaturated dicarboxylic acids such as ethyl maleate and butyl maleate; and diesters of unsaturated dicarboxylic acids such as diethyl maleate and dibutyl maleate.

[0020] In the (meth)acrylic resin, the content of structural units derived from (meth)acrylic monomers in the total amount (100% by mass) of structural units derived from polymerizable monomers is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, still more preferably 50% by mass or more, and particularly preferably 60% by mass or more. In this specification, the content of each structural unit is measured by nuclear magnetic resonance spectroscopy (NMR).

[0021] In the (meth)acrylic resin, the content of structural units derived from other ethylenically unsaturated monomers in the total amount (100 mass%) of structural units derived from polymerizable monomers is preferably 80 mass% or less, more preferably 70 mass% or less, even more preferably 60 mass% or less, still more preferably 50 mass% or less, and particularly preferably 40 mass% or less.

[0022] Examples of the (meth)acrylic resin include a (meth)acrylic monomer polymer, which is a homopolymer or copolymer of a (meth)acrylic monomer, a (meth)acrylic monomer-styrene monomer copolymer, and a (meth)acrylic monomer-vinyl ester copolymer. The (meth)acrylic resin may be, for example, a urethane modified resin or a silicone modified resin.

[0023] The (meth)acrylic resin may be of a self-crosslinking type or a non-self-crosslinking type.

[0024] From the viewpoint of easily forming an antifouling coating film having a good balance between crack resistance and antifouling properties, the glass transition temperature (Tg) of the (meth)acrylic resin is preferably -50°C or higher, more preferably -30°C or higher, even more preferably -10°C or higher, particularly preferably 0°C or higher, and is preferably 90°C or lower, more preferably 70°C or lower, even more preferably 60°C or lower, particularly preferably 50°C or lower, for example, -50 to 90°C. The Tg of the (meth)acrylic resin is the temperature (°C) at the onset value of DSC during heating, obtained by measuring the change in heat quantity in the range of -50°C to 150°C at a heating rate of 20°C / min under a nitrogen atmosphere using a differential scanning calorimeter (DSC) device.

[0025] The (meth)acrylic resin may have an acid value of more than 0 mgKOH / g. The acid value of the (meth)acrylic resin is preferably 1 mgKOH / g or more, more preferably 5 mgKOH / g or more, even more preferably 10 mgKOH / g or more, and is preferably 35 mgKOH / g or less, more preferably 30 mgKOH / g or less, even more preferably 25 mgKOH / g or less, for example, 1 to 35 mgKOH / g. A (meth)acrylic resin having an acid value of the lower limit or more tends to have excellent stability in a water-based antifouling coating composition. A composition containing a (meth)acrylic resin having an acid value of the upper limit or less tends to be able to form a coating film having excellent water resistance. The acid value of the (meth)acrylic resin is the amount (mg) of potassium hydroxide required to neutralize acid groups such as carboxy groups per 1 g of solid content of a sample, and is measured in accordance with JIS K0070:1992 (neutralization titration method).

[0026] Examples of a method for synthesizing the (meth)acrylic resin include known methods, such as a method of polymerizing a polymerizable monomer in the presence of a radical polymerization initiator by a solution polymerization method, a suspension polymerization method, a bulk polymerization method, or an emulsion polymerization method.

[0027] The (meth)acrylic resin is produced by appropriately selecting a (meth)acrylic monomer and, if necessary, other ethylenically unsaturated monomers in consideration of the structural unit, weight average molecular weight, etc., and by a known method, such as a solution radical polymerization method.

[0028] Examples of the styrene-based resin include homopolymers or copolymers of styrene-based monomers, and copolymers of styrene-based monomers and monomers copolymerizable therewith. Examples of the styrene-based monomer include styrene, α-methylstyrene, vinyltoluene, and halogenated styrenes, and among these, styrene is preferred. Examples of the monomers copolymerizable with the styrene-based monomer include the other ethylenically unsaturated monomers described above (excluding styrene-based monomers). The styrene-based resin may be, for example, a urethane-modified product or a silicone-modified product.

[0029] In this specification, styrene-based resins exclude (meth)acrylic resins. In other words, resins having structural units derived from (meth)acrylic monomers and structural units derived from styrene-based monomers are classified as (meth)acrylic resins.

[0030] The urethane resin may be a reaction product of a polyol compound and a polyisocyanate compound. Examples of the polyol compound include polyhydric alcohol, polyether polyol, polyester polyol, polyether ester polyol, (meth)acrylic polyol, polycarbonate polyol, and polyolefin polyol. Examples of the polyisocyanate compound include aliphatic polyisocyanate, alicyclic polyisocyanate, and aromatic polyisocyanate.

[0031] The weight average molecular weight (Mw) of the synthetic resin (A) is preferably 1,000 or more, more preferably 2,000 or more, and preferably 1,000,000 or less, more preferably 700,000 or less, from the viewpoint of obtaining an antifouling coating composition having excellent film-forming properties. Mw is measured by gel permeation chromatography (GPC). When the synthetic resin (A) is a so-called self-crosslinking resin that becomes highly molecular weight upon evaporation of water, Mw is not limited to the upper limit value mentioned above.

[0032] The synthetic resin (A) is preferably a water-dispersible particle that can be dispersed in water. When the synthetic resin (A) is a (meth)acrylic resin particle, the (meth)acrylic resin constituting the particle may have a hydrophilic group such as a carboxy group or a hydroxy group.

[0033] The synthetic resin (A) may be present in the composition (I) in the form of particles. For example, when the composition (I) is applied and dried, water evaporates and the particles bond together to form a film. The Z-average particle size of the synthetic resin (A) is preferably 10 nm or more, more preferably 20 nm or more, even more preferably 30 nm or more, particularly preferably 50 nm or more, and is preferably 2 μm or less, more preferably 1 μm or less, even more preferably 500 nm or less, particularly preferably 300 nm or less, for example, 10 nm to 2 μm. The synthetic resin (A) having a Z-average particle size within the above range tends to be stable in the water-based antifouling paint composition, and such a composition tends to be able to form a coating film with uniform coating film properties. In this specification, the Z-average particle size is measured at 23 ° C. by dynamic light scattering (DLS) using a particle size measuring device (e.g., Zetasizer Nano-ZS manufactured by Malvern).

[0034] The composition (I) may contain two or more types of synthetic resins (A).

[0035] The content of the synthetic resin (A) is, based on 100% by mass of the solid content of the composition (I), preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 7% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less, particularly preferably 16% by mass or less, for example, 3 to 30% by mass.

[0036] From the viewpoint of obtaining a composition having excellent coating workability, the solid content in composition (I) is preferably 40 mass % or more, more preferably 45 mass % or more, even more preferably 50 mass % or more, and is preferably 80 mass % or less, more preferably 75 mass % or less, even more preferably 70 mass % or less, for example, 40 to 80 mass %.

[0037] The solid content of composition (I) and each component (e.g., aqueous dispersion) means the heating residue when composition (I) and each component are dried in an incubator at 108° C. for 3 hours. The solid content is measured by the method described in the Examples section.

[0038] In the production of composition (I), from the viewpoint of the coating film properties, it is preferable to use an aqueous dispersion of synthetic resin (A), and more preferably an aqueous emulsion of synthetic resin (A), which tends to make the synthetic resin (A) more stable and uniformly present in composition (I), and to form a coating film with uniform coating film properties.

[0039] The aqueous emulsion of synthetic resin (A) may be prepared, for example, by emulsifying synthetic resin (A) using a surfactant, or may be prepared directly by emulsion polymerization of polymerizable monomers that form synthetic resin (A). The surfactant is not particularly limited and can be appropriately selected from cationic surfactants, anionic surfactants, and nonionic surfactants.

[0040] From the viewpoints of the stability of the dispersion and the workability in coating production, the content of the synthetic resin (A) in the aqueous dispersion is preferably 20 mass% or more, more preferably 30 mass% or more, even more preferably 40 mass% or more, and is preferably 80 mass% or less, more preferably 75 mass% or less, even more preferably 70 mass% or less, for example, 20 to 80 mass%.

[0041] The aqueous dispersion of synthetic resin (A) is a dispersion in which synthetic resin (A) is dispersed in a dispersion medium containing water (hereinafter also referred to as "aqueous medium"). The aqueous medium is not particularly limited as long as it contains water. From the viewpoint of reducing the environmental load, the content of water in the aqueous medium is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0042] The aqueous medium may contain a medium other than water. Examples of such a medium include acetone, methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, diacetone alcohol, dioxane, ethylene glycol, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monohexyl ether. The above-mentioned medium may be one type or two or more types.

[0043] The pH of the aqueous dispersion of the synthetic resin (A) at 23°C is preferably 7.0 to 12.0, more preferably 7.0 to 10.0, and even more preferably 7.0 to 9.0, from the viewpoint of the stability of the aqueous dispersion. By using such an aqueous dispersion, for example, the synthetic resin (A) tends to be present stably and uniformly in the composition (I). Therefore, a coating film having uniform coating film properties can be formed by using the composition (I).

[0044] <Rosin-based compounds (B)> The rosin-based compound (B) is at least one selected from unmodified rosin and rosin derivatives. The composition (I) containing the rosin-based compound (B) in addition to the synthetic resin (A) can form an antifouling coating film with excellent antifouling properties.

[0045] Examples of rosin include natural rosin, specifically gum rosin, tall oil rosin, and wood rosin. Examples of components constituting rosin include abietic acid, neoabietic acid, dehydroabietic acid, secodehydroabietic acid, dihydroabietic acid, tetrahydroabietic acid, pimaric acid, isopimaric acid, levopimaric acid, paramatric acid, and sandaracopimaric acid. The above components constituting rosin may be one type or two or more types.

[0046] Examples of the rosin derivatives include rosin-based esters, hydrogenated rosin, disproportionated rosin, polymerized rosin (also called dimerized rosin), acid-modified rosin, and rosin-modified phenolic resin. Among these, from the viewpoint of being able to prepare a water-based antifouling coating composition having excellent storage stability and being able to form an antifouling coating film having excellent antifouling properties, rosin-based esters, hydrogenated rosin, disproportionated rosin, polymerized rosin, and acid-modified rosin are preferred, and rosin-based esters are more preferred. Examples of the acid-modified rosin include maleic acid-modified rosin, maleic anhydride-modified rosin, fumaric acid-modified rosin, and (meth)acrylic acid-modified rosin. The rosin derivative may be one type or two or more types.

[0047] Rosin and rosin derivatives may be in the form of a salt. Examples of these salts include ammonium salts and metal salts (saponified rosin and saponified rosin derivatives). Examples of the metal salts include alkali metal salts such as sodium salts and potassium salts, as well as zinc salts, copper salts, aluminum salts, magnesium salts, calcium salts, and barium salts.

[0048] The weight average molecular weight (Mw) of the rosin compound (B) is not less than 800. Although the reason is unclear, by using a rosin compound having such an Mw, it is possible to prepare a water-based antifouling coating composition having superior storage stability compared to, for example, a case where a rosin compound having a small Mw is used.

[0049] The weight average molecular weight (Mw) of the rosin compound (B) is preferably 850 or more, more preferably 900 or more, even more preferably 950 or more, and particularly preferably 1,000 or more. The weight average molecular weight (Mw) of the rosin compound (B) is preferably 3,000 or less, more preferably 2,750 or less, even more preferably 2,500 or less, still more preferably 2,250 or less, and particularly preferably 2,000 or less. The Mw is, for example, preferably 800 to 3,000, more preferably 850 to 2,750, even more preferably 900 to 2,500, still more preferably 950 to 2,250, and particularly preferably 1,000 to 2,000.

[0050] The weight average molecular weight (Mw) of the rosin compound (B) is a value calculated as a standard polystyrene by gel permeation chromatography (GPC). Details of the measurement conditions are described in the Examples section.

[0051] The rosin compound (B) preferably contains a rosin ester, and more preferably contains a rosin ester as a main component. Examples of the rosin ester include esters of rosin and alcohol, and esters of rosin derivatives (excluding esters) and alcohol. Although the reason is unclear, by using a rosin ester, a water-based antifouling coating composition having superior storage stability can be prepared compared to the case of using, for example, rosin (free rosin acid), which is a free acid, acid-modified rosin, or a salt of rosin.

[0052] The alcohol is preferably a polyhydric alcohol. The polyhydric alcohol is a compound having 2 or more alcoholic hydroxyl groups, preferably 2 to 10, more preferably 2 to 8, still more preferably 3 to 6, and particularly preferably 3 to 4. In one embodiment, the polyhydric alcohol is a trihydric or higher polyhydric alcohol having 3 or more alcoholic hydroxyl groups.

[0053] Examples of polyhydric alcohols include Aliphatic diols preferably having 20 or less carbon atoms, more preferably having 10 or less carbon atoms, and even more preferably having 6 or less carbon atoms, such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,4-cyclohexanedimethanol; and aliphatic alcohols of trihydric or higher hydric nature, preferably having 20 or less carbon atoms, more preferably having 10 or less carbon atoms, and even more preferably having 6 or less carbon atoms, such as glycerin, diglycerin, trimethylolethane, trimethylolpropane, butanetriol, pentanetriol, hexanetriol, pentaerythritol, dipentaerythritol, glucose, sucrose, and sorbitol; Examples include:

[0054] Among alcohols, polyhydric alcohols are preferred, trihydric or higher polyhydric alcohols are more preferred, trihydric or higher aliphatic alcohols are even more preferred, and glycerin or pentaerythritol is particularly preferred. That is, as the rosin-based ester, esters of rosin or its derivatives and polyhydric alcohols are preferred, esters of rosin or its derivatives and trihydric or higher polyhydric alcohols are more preferred, esters of rosin or its derivatives and trihydric or higher aliphatic alcohols are even more preferred, and esters of rosin or its derivatives and glycerin, or esters of rosin or its derivatives and pentaerythritol are particularly preferred.

[0055] Specific examples of the rosin ester include rosin ester, hydrogenated rosin ester, disproportionated rosin ester, polymerized rosin ester, acid-modified rosin ester, and rosin ester-modified phenolic resin. Among these, rosin ester, hydrogenated rosin ester, disproportionated rosin ester, polymerized rosin ester, and acid-modified rosin ester are preferred.

[0056] In one embodiment, the rosin compound (B) may further contain at least one component selected from rosin, ammonium salts of rosin, and metal salts of rosin (saponified rosin) together with the rosin ester. Examples of the metal salts of rosin include alkali metal salts such as sodium salts and potassium salts, as well as zinc salts, copper salts, aluminum salts, magnesium salts, calcium salts, and barium salts.

[0057] The rosin compound (B) preferably contains a rosin ester as a main component, i.e., in a range of more than 50 mass%. The content of the rosin ester in the rosin compound (B) is preferably more than 50 mass%, and may be, for example, 60 mass% or more, 70 mass% or more, 80 mass% or more, or 90 mass% or more. The composition (I) containing the rosin compound (B) of such an embodiment has excellent storage stability.

[0058] From the viewpoint of coating workability, storage stability, etc., the glass transition temperature (Tg) of the rosin-based compound (B) is preferably 0°C or higher, more preferably 10°C or higher, even more preferably 15°C or higher, particularly preferably 20°C or higher, and is preferably 80°C or lower, more preferably 60°C or lower, even more preferably 55°C or lower, even more preferably 50°C or lower, particularly preferably 45°C or lower, particularly preferably 40°C or lower, for example, 0 to 80°C. The Tg of the rosin-based compound (B) is measured using a differential scanning calorimeter (DSC). Details of the measurement conditions are described in the Examples section.

[0059] The acid value of the rosin compound (B) is preferably 100 mgKOH / g or less, more preferably 80 mgKOH / g or less, even more preferably 70 mgKOH / g or less, still more preferably 60 mgKOH / g or less, particularly preferably 50 mgKOH / g or less, and may be, for example, 40 mgKOH / g or less, 35 mgKOH / g or less, 30 mgKOH / g or less, 25 mgKOH / g or less, 20 mgKOH / g or less, or 15 mgKOH / g or less. A composition (I) containing a rosin compound (B) having an acid value of the above upper limit or less has excellent storage stability.

[0060] There is no particular limitation on the lower limit of the acid value of the rosin compound (B). The acid value of the rosin compound (B) may be, for example, 0 mgKOH / g or more, 5 mgKOH / g or more, or 10 mgKOH / g or more.

[0061] The acid value of the rosin compound (B) is the amount (mg) of potassium hydroxide required to neutralize acid groups such as carboxyl groups per gram of solid content of the sample, and is measured in accordance with JIS K0070:1992 (neutralization titration method).

[0062] The rosin compound (B) is preferably a water-dispersible particle that can be dispersed in water. The rosin compound (B) may be present in the composition in the form of particles. The Z-average particle size of the rosin compound (B) is preferably 10 nm or more, more preferably 20 nm or more, even more preferably 30 nm or more, particularly preferably 50 nm or more, and is preferably 2 μm or less, more preferably 1 μm or less, even more preferably 500 nm or less, particularly preferably 300 nm or less, for example, 10 nm to 2 μm. The rosin compound (B) having a Z-average particle size within the above range tends to be able to exist stably in the water-based antifouling coating composition, and such a composition tends to be able to form a coating film with uniform coating film properties.

[0063] The composition (I) may contain two or more types of rosin-based compounds (B).

[0064] In the composition (I), the content ratio of the synthetic resin (A) to the rosin-based compound (B) (content of (A):content of (B)) is, for example, 1.0:0.3 to 1.0:4.0, preferably 1.0:0.7 to 1.0:3.0, more preferably 1.0:0.9 to 1.0:2.8, even more preferably 1.0:1.2 to 1.0:2.5, still more preferably 1.0:1.4 to 1.0:2.4, and particularly preferably 1.0:1.5 to 1.0:2.3, based on mass. The composition (I) containing the synthetic resin (A) and the rosin-based compound (B) in the above content ratio can form an antifouling coating film that is well-balanced and excellent in crack resistance in outdoor exposure tests and long-term antifouling properties. When the content ratio of the rosin-based compound (B) to the synthetic resin (A) is large, the stain resistance tends to be better, and when the content ratio of the rosin-based compound (B) to the synthetic resin (A) is small, the crack resistance tends to be better.

[0065] The content of the rosin compound (B) is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and is preferably 40% by mass or less, more preferably 35% by mass or less, even more preferably 30% by mass or less, particularly preferably 25% by mass or less, for example, 3 to 40% by mass, based on 100% by mass of the solid content of the composition (I). The composition (I) of such an embodiment can form an antifouling coating film that is excellent in terms of crack resistance in outdoor exposure tests and long-term antifouling properties in a well-balanced manner.

[0066] In the production of composition (I), from the viewpoint of the coating film properties, it is preferable to use an aqueous dispersion of the rosin-based compound (B), and it is more preferable to use an aqueous emulsion of the rosin-based compound (B), which tends to make the rosin-based compound (B) more likely to be present stably and uniformly in composition (I), and to form a coating film with uniform coating film properties.

[0067] From the viewpoints of the stability of the dispersion and the workability in coating production, the content of the rosin-based compound (B) in the aqueous dispersion is preferably 20 mass% or more, more preferably 30 mass% or more, and even more preferably 40 mass% or more, and is preferably 80 mass% or less, more preferably 75 mass% or less, and even more preferably 70 mass% or less, for example, 20 to 80 mass%.

[0068] The aqueous dispersion of the rosin compound (B) is a dispersion in which the rosin compound (B) is dispersed in an aqueous medium. The aqueous medium is not particularly limited as long as it contains water. From the viewpoint of reducing the environmental load, the content of water in the aqueous medium is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. Specific examples of the medium other than water in the aqueous medium are as described above.

[0069] The pH of the aqueous dispersion of the rosin-based compound (B) at 23°C is preferably 6.0 to 12.0, more preferably 6.0 to 10.0, even more preferably 6.0 to 9.0, and particularly preferably 6.0 to 8.5, from the viewpoints of the stability of the aqueous dispersion of the rosin-based compound (B) and the stability of the synthetic resin (A) in the composition (I).

[0070] <Water(C)> The composition (I) is a water-based antifouling coating composition. The term "water-based" composition refers to a composition containing water. Examples of the water (C) include tap water, ion-exchanged water, and deionized water, and ion-exchanged water or deionized water is preferred. Examples of the water (C) include water contained in an aqueous dispersion of a synthetic resin (A) and water contained in an aqueous dispersion of a rosin-based compound (B).

[0071] The content of water (C) in the composition (I) is preferably 20% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, and is preferably 60% by mass or less, more preferably 55% by mass or less, even more preferably 50% by mass or less, for example, 20 to 60% by mass. The content of water (C) is measured by the Karl Fischer method using a moisture measuring device (for example, CA-310, manufactured by Nitto Seiko Analytech).

[0072] <Anti-fouling agent (D)> The composition (I) may further contain an antifouling agent (D). Examples of the antifouling agent (D) include inorganic antifouling agents and organic antifouling agents.

[0073] Examples of inorganic antifouling agents include copper or copper compounds (excluding pyrithione compounds) such as cuprous oxide, metallic copper powder, and cuprous thiocyanate (copper rhodanide). Among these, cuprous oxide or cuprous thiocyanate (copper rhodanide) is preferred.

[0074] Examples of organic antifouling agents include: Metal pyrithiones (pyrithione compounds) such as copper pyrithione and zinc pyrithione; Tetraalkylthiuram disulfides such as tetramethylthiuram disulfide; Carbamate compounds such as zinc dimethyldithiocarbamate, zinc ethylene bisdithiocarbamate, and bisdimethyldithiocarbamoyl zinc ethylene bisdithiocarbamate; Maleimide compounds such as 2,4,6-triphenylmaleimide, 2,3-dichloro-N-(2',6'-diethylphenyl)maleimide, and 2,3-dichloro-N-(2'-ethyl-6'-methylphenyl)maleimide; 2,4,5,6-Tetrachloroisophthalonitrile, N,N-Dimethyldichlorophenylurea, 4,5-Dichloro-2-n-octyl-4-isothiazolin-3-one, 2-Methylthio-4-tert-butylamino-6-cyclopropyl-S-triazine, chloromethyl-n-octyl disulfide, N',N'-Dimethyl-N-phenyl-(N-fluorodichloromethylthio)sulfamide, and N',N'-Dimethyl-N-tolyl-(N-fluorodichloromethylthio)sulfamide; Amine-organoborane complexes such as pyridinetriphenylborane and 4-isopropylpyridinediphenylmethylborane; and (+ / -)-4-[1-(2,3-dimethylphenyl)ethyl]-1H-imidazole (hereinafter also referred to as "medetomidine"); Examples include:

[0075] Among the organic antifouling agents, copper pyrithione, zinc pyrithione, zinc ethylene bisdithiocarbamate, 2-methylthio-4-tert-butylamino-6-cyclopropyl-S-triazine or medetomidine is preferred, and copper pyrithione, zinc ethylene bisdithiocarbamate or medetomidine is more preferred.

[0076] The composition (I) may contain one or more antifouling agents (D).

[0077] When composition (I) contains an antifouling agent (D), the content of the antifouling agent (D) is, relative to 100 mass% of the solid content of composition (I), preferably 0.01 mass% or more, more preferably 0.1 mass% or more, even more preferably 1 mass% or more, still more preferably 5 mass% or more, particularly preferably 10 mass% or more, and is preferably 80 mass% or less, more preferably 70 mass% or less, for example, 0.01 to 80 mass%.

[0078] <Other ingredients> The composition (I) may further contain components other than the above-mentioned components (hereinafter also referred to as "other components") such as pigments and additives. Examples of the additives include dispersants, antifoaming agents, viscosity adjusters, film-forming assistants, fungicides, preservatives, pH adjusters, ultraviolet absorbers, and antioxidants. The composition (I) may contain one or more other components.

[0079] Examples of the pigment include extender pigments and color pigments. Examples of the pigment include organic pigments and inorganic pigments. The composition (I) may contain one or more pigments.

[0080] Examples of the extender pigment include talc, silica, mica, clay, potassium feldspar, calcium carbonate, kaolin, alumina white, white carbon, aluminum hydroxide, magnesium carbonate, barium carbonate, barium sulfate, zinc oxide, and zinc sulfide. When composition (I) contains a body pigment, the content of the body pigment is, relative to 100% by mass of the solid content of composition (I), preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 5% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, for example, 0.1 to 80% by mass.

[0081] Examples of color pigments include organic pigments and inorganic pigments. Examples of organic pigments include naphthol red and phthalocyanine blue. Examples of inorganic pigments include carbon black, red iron oxide, titanium white (titanium oxide), yellow iron oxide, and red iron oxide. When composition (I) contains a coloring pigment, the content of the coloring pigment is, relative to 100% by mass of the solid content of composition (I), preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, for example, 0.01 to 40% by mass.

[0082] The dispersant is preferably a material capable of improving the dispersibility of water-insoluble components (e.g., pigments) in the coating composition. By using the dispersant, for example, a coating film having a good appearance and excellent crack resistance can be easily formed. Examples of the dispersant include polymers having a pigment-adsorbing group (pigment-affinity group) and a compatible chain such as fatty acid, polyamino, polyether, polyester, polyurethane, and poly(meth)acrylate. Examples of the pigment-adsorbing group include a carboxy group, an acid anhydride group, a phosphoric acid group, an amino group, a salt group thereof, and an ammonium base. When composition (I) contains a dispersant, the content of the dispersant in 100% by mass of the solid content of composition (I) is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and is preferably 5% by mass or less, more preferably 3% by mass or less, for example, 0.1 to 5% by mass.

[0083] The defoaming agent is preferably a material capable of suppressing the generation of bubbles during the production or application of the coating composition, or a material capable of breaking bubbles generated in the coating composition.The use of the defoaming agent can, for example, suppress the generation of bubble marks or pinholes in the coating film, thus improving the film-forming property and crack resistance of the coating film.The defoaming agent can, for example, be a silicone-based defoaming agent, a polymer-based (non-silicone-based) defoaming agent, and a mineral oil-based defoaming agent. When composition (I) contains an antifoaming agent, the content of the antifoaming agent is, relative to 100 mass% of the solid content of composition (I), preferably 0.05 mass% or more, more preferably 0.1 mass% or more, and preferably 5 mass% or less, more preferably 3 mass% or less, for example, 0.05 to 5 mass%.

[0084] The viscosity modifier is preferably a material capable of suppressing the precipitation of water-insoluble matter (e.g., pigment) in the coating composition and improving the storage stability of the coating composition. Examples of the viscosity modifier include organic thixotropic agents such as hydrogenated castor oil-based thixotropic agents, amide wax-based thixotropic agents, polyethylene oxide-based thixotropic agents, and urethane-based thixotropic agents; and inorganic thixotropic agents such as clay minerals (e.g., bentonite, smectite, and hectorite) and synthetic fine silica powder. When composition (I) contains a viscosity modifier, the content of the viscosity modifier is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, and preferably 5 mass% or less, more preferably 3 mass% or less, for example, 0.01 to 5 mass%, based on 100 mass% of the solid content of composition (I).

[0085] Examples of the film-forming aid include alcohols, glycol ethers, and esters. Examples of the alcohols include isopropyl alcohol and 2,2,4-trimethylpentanediol. Examples of the glycol ethers include ethylene glycol monobutyl ether, ethylene glycol diethyl ether, diethylene glycol monobutyl ether, diethylene glycol diethyl ether, propylene glycol diethyl ether, dipropylene glycol diethyl ether, dipropylene glycol methyl ether, and dipropylene glycol n-butyl ether. Examples of the esters include 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate. When composition (I) contains a film-forming auxiliary, the content of the film-forming auxiliary is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and preferably 15 mass% or less, more preferably 5 mass% or less, for example, 0.1 to 15 mass%, based on 100 mass% of the total amount of composition (I).

[0086] <Method of manufacturing water-based antifouling paint composition> The composition (I) can be produced, for example, by mixing a synthetic resin (A), a rosin-based compound (B), and water (C). In this case, the ratio of the amounts of the synthetic resin (A) and the rosin-based compound (B) used (A):(B) is, for example, 1.0:0.3 to 1.0:4.0, preferably 1.0:0.7 to 1.0:3.0, more preferably 1.0:0.9 to 1.0:2.8, even more preferably 1.0:1.2 to 1.0:2.5, still more preferably 1.0:1.4 to 1.0:2.4, and particularly preferably 1.0:1.5 to 1.0:2.3, based on mass.

[0087] Composition (I) can be produced, for example, by charging the synthetic resin (A), the rosin-based compound (B), water (C), and, if necessary, the antifouling agent (D), and, if necessary, the other components described above, all at once or in any order into a stirring vessel, mixing the respective components using a known stirring / mixing means, and dispersing or dissolving them in the water (C).

[0088] In the production of the composition (I), from the viewpoint of workability in the production of the coating material, it is preferable to use an aqueous dispersion of the synthetic resin (A) and an aqueous dispersion of the rosin-based compound (B), and it is more preferable to use an aqueous emulsion of the synthetic resin (A) and an aqueous emulsion of the rosin-based compound (B). The details of each aqueous dispersion are as described above.

[0089] Examples of the stirring and mixing means include a paint shaker, a high-speed disperser, a sand grind mill, a basket mill, a ball mill, a three-roll mill, a Ross mixer, or a planetary mixer. Mixing (kneading) may be performed with heating or cooling depending on the season and environment.

[0090] Composition (I) is a water-based coating composition, and therefore has very little adverse effect on the environment or human body. Composition (I) has excellent storage stability. In one embodiment, composition (I) can form an antifouling coating film that has excellent crack resistance in outdoor exposure tests. Since antifouling coating films are also provided on the outer sides of ships, for example, excellent crack resistance in outdoor exposure tests is an advantageous effect. In one embodiment, composition (I) can form an antifouling coating film that has excellent antifouling properties and can inhibit the attachment of aquatic organisms for a long period of time.

[0091] The content of volatile organic compounds (VOCs) such as organic solvents in the composition (I) is preferably 150 g / L or less, more preferably 100 g / L or less, from the viewpoint of consideration of the natural environment and the painting work environment. The lower the content of VOCs in the composition (I), the more preferable it is, but the content may be, for example, 1 g / L or more, 5 g / L or more, 10 g / L or more, 20 g / L or more, or 30 g / L or more. The content of VOCs in the composition (I) may be, for example, 1 to 150 g / L.

[0092] The VOC content in the composition (I) is calculated based on the following formula (1) using the values ​​of the composition specific gravity, solids concentration, and water concentration, each of which will be described below. VOC content (g / L) = Composition specific gravity x 1000 x (100 - solid content concentration - water concentration) / 100 (1)

[0093] The specific gravity of the composition (g / mL) is a value calculated by filling a specific gravity cup having an internal volume of 100 mL with the composition at a temperature condition of 23° C. and measuring the mass of the composition. The solid content concentration (mass%) is a value calculated by the method described in the Examples section. The solid content of the composition means the heating residue when the composition is dried in an incubator at 108°C for 3 hours, as described in the Examples section.

[0094] The water concentration (mass %) is the amount of water (mass %) contained in 100 mass % of the composition, and is measured using a water meter (for example, CA-310, manufactured by Nitto Seiko Analytech) according to the Karl Fischer method.

[0095] In one embodiment, the composition (I) is preferably a one-liquid composition containing a synthetic resin (A), a rosin-based compound (B), and water (C). In such a one-liquid composition, the composition (I) has excellent storage stability.

[0096] [Uses of water-based antifouling paint compositions] The antifouling coating film of the present disclosure (hereinafter also referred to as "antifouling coating film (J)") is formed from composition (I). The substrate with the antifouling coating film of the present disclosure (hereinafter also referred to as "antifouling substrate (K)") has a substrate and an antifouling coating film (J) provided on the surface of the substrate.

[0097] The method for producing the antifouling substrate (K) comprises a step (1) of applying or impregnating the substrate (object to be coated) with the composition (I) to obtain a coated or impregnated body, and a step (2) of drying the coated or impregnated body.

[0098] Examples of the method for applying the composition (I) include known methods such as air spray coating, airless spray coating, brush coating, and roller coating. The applied or impregnated composition (I) may be dried by natural drying or by heat drying. Specifically, the applied or impregnated composition (I) is dried, for example, by leaving it under conditions of -5 to 40°C, preferably for about 1 to 10 days, more preferably for about 1 to 8 days, to obtain an antifouling coating film (J).

[0099] Alternatively, the antifouling substrate (K) can be produced by forming an antifouling coating film (J) from the composition (I) on the surface of a temporary substrate, peeling the antifouling coating film (J) from the temporary substrate, and attaching it to the substrate to be antifouled. In this case, the antifouling coating film (J) may be attached to the substrate via an adhesive layer.

[0100] The surface of the substrate may be treated with a primer, or may have a layer formed from various resin-based paints such as epoxy resin-based paints, vinyl resin-based paints, (meth)acrylic resin-based paints, urethane resin-based paints, etc. In this case, the surface of the substrate on which the antifouling coating film (J) is provided means the surface after primer treatment or the surface of the layer formed from the above-mentioned resin-based paints.

[0101] The substrate is not particularly limited. The composition (I) is preferably used in a wide range of industrial fields such as ships to make the substrate antifouling for a long period of time. For this reason, examples of the substrate include ship hull shell plates (steel plates, etc.), underwater structures, seawater or freshwater water supply and drainage pipes in various facilities, fishing materials, and other marine materials. Examples of ships include large steel ships such as container ships and tankers, fishing boats, FRP ships, wooden ships, yachts, motorboats, and personal watercraft. Examples of the hull shell plates include bottom shell plates and outer hull parts. Examples of underwater structures include oil pipelines, water conveyance piping, circulating water pipes, water supply and drainage outlets in various facilities, undersea cables, seawater utilization equipment (seawater pumps, etc.), as well as megafloats, coastal roads, undersea tunnels, port facilities, offshore wind power generation facilities, and various underwater civil engineering structures in canals and waterways. Examples of the above facilities include factories, thermal power plants, and nuclear power plants. Examples of fishing equipment include ropes, fishing gear, fishing nets, floats, and buoys. Examples of other marine equipment include swimsuits, diver suits, underwater goggles, oxygen cylinders, and torpedoes. Among these, ship hull shells, underwater structures, fishing equipment, and water supply and drainage pipes are preferred, ship hull shells and underwater structures are more preferred, and ship hull shells are particularly preferred.

[0102] In producing the antifouling substrate (K), when the substrate is a fishing net or a steel plate, the composition (I) may be directly applied to the surface of the substrate, when the substrate is a fishing net, the composition (I) may be impregnated onto the surface of the substrate, and when the substrate is a steel plate, a base material such as a rust inhibitor or a primer may be applied to the surface of the substrate in advance to form a base layer, and then the composition (I) may be applied to the surface of the base layer. In addition, for the purpose of repair, an antifouling coating film (J) may be further formed on the surface of an antifouling substrate on which an antifouling coating film (J) or a conventional antifouling coating film is formed, such as an antifouling substrate having a deteriorated antifouling coating film on a substrate.

[0103] The thickness of the antifouling coating film (J) is not particularly limited, but is, for example, about 30 to 1000 μm. When forming the antifouling coating film (J), a method of applying the composition (I) once or multiple times so that the thickness of the antifouling coating film formed by one application is preferably 10 to 300 μm, more preferably 30 to 200 μm, can be mentioned.

[0104] A ship having an antifouling coating (J) can suppress a decrease in ship speed and an increase in fuel consumption because the adhesion of aquatic organisms can be suppressed. An underwater structure having an antifouling coating (J) can maintain the function of the underwater structure for a long period of time because the adhesion of aquatic organisms can be suppressed for a long period of time. A fishing net having an antifouling coating (J) is less likely to pollute the environment and can suppress clogging of the mesh because the adhesion of aquatic organisms can be suppressed. A water supply and drainage pipe having an antifouling coating (J) on its inner surface can suppress clogging of the water supply and drainage pipe and a decrease in flow speed because the adhesion and proliferation of aquatic organisms can be suppressed.

[0105] [Example of the situation] The present disclosure relates to, for example, the following [1] to

[17] . [1] A water-based antifouling coating composition comprising a synthetic resin (A), a rosin-based compound (B) having a weight-average molecular weight of 800 or more, and water (C). [2] The aqueous antifouling coating composition according to

[11] above, wherein the content ratio (A):(B) of the synthetic resin (A) to the rosin-based compound (B) in the composition is, on a mass basis, 1.0:0.3 to 1.0:4.0. [3] The aqueous antifouling coating composition according to the above [1] or [2], wherein the content ratio (A):(B) of the synthetic resin (A) to the rosin-based compound (B) in the composition is, on a mass basis, 1.0:0.7 to 1.0:3.0. [4] The aqueous antifouling coating composition according to any one of the above [1] to [3], wherein the rosin compound (B) has an acid value of 100 mgKOH / g or less. [5] The aqueous antifouling coating composition according to any one of the above [1] to [4], wherein the rosin compound (B) contains a rosin ester. [6] The aqueous antifouling coating composition according to [5] above, wherein the rosin-based ester is an ester of rosin or a derivative thereof with a trihydric or higher polyhydric alcohol. [7] The aqueous antifouling coating composition according to any one of the above [1] to [6], wherein the synthetic resin (A) is at least one selected from the group consisting of (meth)acrylic resins, styrene resins and urethane resins. [8] The aqueous antifouling coating composition according to any one of [1] to [7] above, wherein the content of the water (C) in the composition is 20 to 60 mass %. [9] An antifouling coating film formed from the aqueous antifouling coating composition according to any one of [1] to [8] above.

[10] A substrate with an antifouling coating film, comprising: a substrate; and the antifouling coating film according to [9] provided on a surface of the substrate.

[11] A method for producing a substrate with an antifouling coating film, comprising the steps of: (1) applying to or impregnating a substrate with the aqueous antifouling coating composition described in any one of the above items [1] to [8] to obtain a coated or impregnated body; and (2) drying the coated or impregnated body.

[12] A method for producing an aqueous antifouling coating composition, comprising the step of mixing a synthetic resin (A), a rosin-based compound (B) having a weight-average molecular weight of 800 or more, and water (C).

[13] The method for producing an aqueous antifouling coating composition according to

[12] above, wherein in the step, the ratio of the amounts of the synthetic resin (A) to the rosin-based compound (B), (A):(B), is 1.0:0.3 to 1.0:4.0 by mass.

[14] The method for producing a water-based antifouling coating composition according to

[12] or

[13] above, wherein in the step, the ratio of the amounts of the synthetic resin (A) to the rosin-based compound (B), (A):(B), is 1.0:0.7 to 1.0:3.0 by mass.

[15] The method for producing a water-based antifouling coating composition according to any one of the above

[12] to

[14] , wherein the rosin compound (B) contains a rosin ester.

[16] The method for producing the aqueous antifouling coating composition according to any one of the above

[12] to

[15] , wherein in the above step, an aqueous dispersion of the synthetic resin (A) and an aqueous dispersion of the rosin compound (B) are used.

[17] The method for producing an aqueous antifouling coating composition according to any one of

[12] to

[16] above, wherein in the step, an aqueous dispersion of the synthetic resin (A) is used, and the aqueous dispersion of the synthetic resin (A) has a pH of 7.0 to 9.0 at 23° C. EXAMPLES

[0106] The aqueous antifouling coating composition of the present disclosure will be described in more detail below with reference to examples, but the aqueous antifouling coating composition of the present disclosure is not limited to the following examples. In the following examples and comparative examples, "parts" refers to "parts by mass".

[0107] [Solid content concentration] The solid content of the composition and each component means the heating residue when the composition and each component are dried in an incubator at 108°C for 3 hours. Specifically, the heating residue is the residue of the sample obtained by weighing out 1.0 g of the composition or each component sample onto a flat-bottom dish, spreading it evenly using a wire of known mass, and drying it in an incubator at 1 atmosphere and 108°C for 3 hours. The solid content concentration (mass%) of the composition and each component was calculated from the amount of the heating residue.

[0108] [Weight average molecular weight (Mw)] The weight average molecular weight (Mw) of the rosin-based compound (B) was measured by gel permeation chromatography (GPC) under the following measurement conditions. Measurement conditions Equipment: Alliance 2695 (Waters) Column: One "TSKgel SuperH4000" and two "TSKgel SuperH2000" columns connected (both manufactured by Tosoh, inner diameter 6 mm x length 15 cm) Eluent: Tetrahydrofuran 99% (containing BHT) ·Flow rate: 0.6ml / min Detector: "RI-104" (Shodex) Column thermostat temperature: 40℃ Standard material: Standard polystyrene Sample preparation: Weigh out the sample into a sample tube. Tetrahydrofuran was added to dilute the solution approximately 100-fold.

[0109] [Glass transition temperature (Tg)] The glass transition temperature (Tg) of the rosin-based compound (B) was measured using a differential scanning calorimeter (DSC) under the following measurement conditions. Measurement conditions Equipment: "DSC Q2000" (TA Instruments) Container: Aluminum Heating rate: 20℃ / min Temperature range: -50℃ to 150℃ Temperature Modulation: None Tg measurement value: The temperature at the onset value during the second heating cycle Sample preparation: Spread a thin layer of sample on a glass dish, dry at 40℃ for 1.5 hours under reduced pressure, Approximately 3 mg of powder ground in a mortar was used.

[0110] [raw materials] <Aqueous dispersion of synthetic resin (A)> ·PRIMAL TX-100 Manufactured by Dow Chemical, A water-based emulsion of (meth)acrylic resin (self-crosslinking type), Solid concentration: 46.5% by mass, pH: 7.8, Tg: 28℃

[0111] <Aqueous Dispersion of Rosin-Based Compound (B)> Harrie Star SK-218NS Manufactured by Harima Chemicals, Aqueous emulsion of rosin ester (ester of rosin or its derivative with trihydric or higher polyhydric alcohol), solids concentration: 50% by mass, pH: 8.2 Acid value (solid content): 13.6 mg KOH / g, Mw: 1200, Tg: 35°C Aquadhes 6203 Made from Pino Pine, Aqueous dispersion of rosin ester (ester of rosin or its derivative with trihydric or higher polyhydric alcohol), solids concentration: 59% by mass, pH: 6.4 Acid value (solid content): 43.7mgKOH / g, Mw: 1000, Tg: 27℃

[0112] <Aqueous dispersion or solution of a rosin-based compound (cB) other than the above compound (B)> -Harsize NES-500 Manufactured by Harima Chemicals, Water-based emulsion of rosin, solids concentration: 50% by weight, pH: 5.7 Acid value (solid content): 246 mg KOH / g, Mw: 310, Tg: 61°C ·Bremar SP3180 35% Wasser / NH3 Made by Robert Kraemer Rosin aqueous solution, solid concentration: 35% by mass, pH: 8.8, Acid value (solid content): 251.0 mg KOH / g, Mw: 460, Tg: 90°C ·Bremar SP3180 50% Wasser / NaOH Made by Robert Kraemer Rosin aqueous solution, solid concentration: 50% by mass, pH: 9.2, Acid value (solid content): 6.2 mg KOH / g, Mw: 290, Tg: 43°C

[0113] <Extender pigment> Talc FC-1 Talc, manufactured by Fukuoka Talc Industry Co., Ltd. ·Mica Powder 325mesh Fukuoka Talc Industry Co., Ltd., Mica

[0114] <Coloring pigments> Novoperm Red F5RK Clariant Japan, Naphthol Red Mitsubishi Carbon Black Mitsubishi Chemical, carbon black

[0115] <Anti-fouling agent (D)> Lo Lo Tint 97 American Chemet Corporation, Cuprous Oxide ·Selektope I-TECH, medetomidine

[0116] <Dispersant> DISPERBYK-190 Made by BYK Japan, Solution of high molecular weight block polymer with pigment affinity group, solid content: 40% by mass

[0117] <Antifoaming agent> BYK-018 Made by BYK Japan, A mixture of foam-breaking polysiloxane and hydrophobic particles, solids concentration: 97% by mass

[0118] <Viscosity adjuster> Adekanol UH-752 Made by ADEKA, Polyether polyol urethane polymer, solid content: 28% by mass ·Bentone DE Manufactured by Elementis Specialties Inc. Hectorite Clay

[0119] <Film-forming agent> Kyowanol M Made by KH Neochem, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate Dowanol DPM Glycol Ether Manufactured by Dow Chemical, Dipropylene glycol methyl ether Dowanol DPnB Glycol Ether Manufactured by Dow Chemical, Dipropylene glycol n-butyl ether

[0120] [Preparation of antifouling paint composition] [Example 1] An antifouling coating composition was prepared as follows. Into a container, 11.8 parts of ion-exchanged water, 1.5 parts of DISPERBYK-190 (dispersant), and 0.2 parts of Bentone DE (viscosity modifier) ​​were added, and mixed using a paint shaker until each component was uniformly dispersed or dissolved in water. Then, in the container, 3.0 parts of Mica Powder 325mesh (body pigment), 37.0 parts of Lo Lo Tint 97 (stain-repellent (D)), 0.6 parts of Novoperm Red F5RK (color pigment), 0.3 parts of BYK-018 (defoamer), and 100 parts of glass beads were added, and the mixture was stirred for 1 hour using a paint shaker to disperse the components and obtain a mixture.

[0121] After dispersion, the glass beads were removed from the mixture through a filter net (opening: 80 mesh), and to the filtrate, 11.7 parts of PRIMAL TX-100 (aqueous dispersion of synthetic resin (A)), 24.8 parts of HARIESTAR SK-218NS (aqueous dispersion of rosin-based compound (B)), 6.5 parts of Talc FC-1 (body pigment), 0.2 parts of Adekanol UH-752 (viscosity modifier), and 2.4 parts of Kyowanol M (film-forming aid) were added while rotating the disperser, and dispersed for 20 minutes to obtain an antifouling coating composition.

[0122] [Examples 2 to 8 and Comparative Examples 1 to 3] Antifouling coating compositions were prepared in the same manner as in Example 1, except that the types and amounts of each component were changed as shown in Table 1 or Table 2.

[0123] [Evaluation of the physical properties of antifouling paint compositions] <Storage stability test> The state of the antifouling coating composition of the Examples or Comparative Examples one day after preparation (initial coating state) was evaluated according to the following criteria. In addition, the antifouling coating composition of the Examples or Comparative Examples was filled into a sealed container, stored at 50°C for one month, and the state of the antifouling coating composition was evaluated according to the following criteria. (Evaluation Criteria) AA: Can be mixed uniformly by hand stirring, no lumps or grains. BB: Vigorous gelation or sedimentation, or lumps or lumps are present.

[0124] <Outdoor exposure test> A test plate was prepared by applying the antifouling coating composition of the Example or Comparative Example to a test plate already coated with an anticorrosive coating using an applicator (gap 0.5 mm). The test plate was dried at 23°C for one week, and then placed on an exposure rack conforming to JIS K 5600-7-6 (weather resistance to outdoor exposure). After six months, the occurrence of cracks in the coating was evaluated according to the following criteria. The above test was carried out on five test plates for each of the Example and Comparative Example, and the number of test plates on which cracks occurred was confirmed. (Evaluation Criteria) AA: No cracks were visible even when magnified 100 times using an optical microscope (High Speed ​​Microscope VW-9000 (manufactured by KEYENCE), lens: VW-600C). BB: Cracks are visible to the naked eye or when magnified 100 times using the optical microscope described above.

[0125] <Static soiling resistance test> An epoxy-based anticorrosive paint (product name "Banno 500", manufactured by Chugoku Paint Co., Ltd.) was applied to a sandblasted steel plate (300 mm x 100 mm x 2.3 mm) using an applicator so that the dry film thickness was 150 μm, and then dried to form a cured coating film. Next, an epoxy-based binder paint (product name "Banno 500N", manufactured by Chugoku Paint Co., Ltd.) was applied to the cured coating film so that the dry film thickness was 100 μm, and then dried at 23° C. for 1 day to prepare a test plate.

[0126] Next, the antifouling coating composition of the Example or Comparative Example was applied to the above test plate (the surface of the cured coating film of the above epoxy-based binder paint) using an applicator so that the dry film thickness was 150 μm, and the plate was dried at 23° C. for 7 days to form an antifouling coating film, thereby producing a test plate with an antifouling coating film.

[0127] This test plate with the antifouling coating film was suspended and immersed in seawater off the coast of Hatsukaichi, Hiroshima Prefecture, at a position about 2 m below the surface, and left in a static state. 12 months after the start of immersion, the area of ​​marine organisms attached to the antifouling coating film was measured, assuming that the total area (test surface) of the antifouling coating film on the test plate that was constantly submerged in seawater was 100%, and the static antifouling properties were evaluated based on the following evaluation criteria.

[0128] (Evaluation Criteria) 5: The area of ​​the test surface covered by marine organisms is less than 1%. 4: The above area is 1% or more but less than 10% of the test surface 3: The above area is 10% or more but less than 30% of the test surface 2: The above area is 30% or more but less than 70% of the test surface 1: The above area is 70% or more of the test surface

[0129] [Table 1]

[0130] [Table 2]

Claims

1. A synthetic resin (A); (B) a rosin-based compound having a weight average molecular weight of 800 or more and a glass transition temperature (Tg) of 0 to 50° C.; Water (C); A water-based antifouling coating composition comprising:

2. A synthetic resin (A), (B) a rosin-based compound having a weight average molecular weight of 800 or more; Water (C); (However, the above composition containing an emulsion of polybutene is excluded.)

3. 2. The aqueous antifouling coating composition according to claim 1, wherein a content ratio (A):(B) of the synthetic resin (A) to the rosin-based compound (B) in the composition is, on a mass basis, 1.0:0.7 to 1.0:3.

0.

4. 2. The aqueous antifouling coating composition according to claim 1, wherein the rosin compound (B) has an acid value of 100 mg KOH / g or less.

5. The aqueous antifouling coating composition according to claim 1 , wherein the rosin-based compound (B) comprises a rosin-based ester.

6. 6. The aqueous antifouling coating composition according to claim 5, wherein the rosin-based ester is an ester of rosin or a derivative thereof with a trihydric or higher polyhydric alcohol.

7. 2. The aqueous antifouling coating composition according to claim 1, wherein the synthetic resin (A) is at least one selected from the group consisting of (meth)acrylic resins, styrene resins and urethane resins.

8. 2. The aqueous antifouling coating composition according to claim 1, wherein the content of the water (C) in the composition is 20 to 60 mass %.

9. An antifouling coating film formed from the aqueous antifouling coating composition according to any one of claims 1 to 8.

10. A substrate; The antifouling coating film according to claim 9 provided on a surface of the substrate; A substrate having an antifouling coating film.

11. A step (1) of coating or impregnating a substrate with the aqueous antifouling coating composition according to any one of claims 1 to 8 to obtain a coated or impregnated body; and Step (2) of drying the coated body or the impregnated body A method for producing a substrate having an antifouling coating film, comprising the steps of:

12. A method for producing a water-based antifouling coating composition, comprising the step of mixing a synthetic resin (A), a rosin-based compound (B) having a weight-average molecular weight of 800 or more and a glass transition temperature (Tg) of 0 to 50°C, and water (C).

13. A method for producing a water-based antifouling paint composition (excluding said composition containing an emulsion of polybutene), comprising the step of mixing a synthetic resin (A), a rosin-based compound (B) having a weight-average molecular weight of 800 or more, and water (C).

14. The method for producing an aqueous antifouling coating composition according to claim 12 or 13, wherein in the step, a usage ratio (A):(B) of the synthetic resin (A) to the rosin-based compound (B) is, on a mass basis, 1.0:0.7 to 1.0:3.

0.

15. The method for producing an aqueous antifouling coating composition according to claim 12 or 13, wherein the rosin-based compound (B) comprises a rosin-based ester.

16. The method for producing an aqueous antifouling coating composition according to claim 12 or 13, wherein an aqueous dispersion of the synthetic resin (A) and an aqueous dispersion of the rosin compound (B) are used in the step.

17. The method for producing an aqueous antifouling coating composition according to claim 16, wherein the aqueous dispersion of the synthetic resin (A) has a pH of 7.0 to 9.0 at 23°C.

Citation Information

Patent Citations

  • JP1972020230U

  • Senteibootoryo

    JP1976014936A

  • Antifouling coating composition, coating film thereof, fishing gear / Fishnet coated with such coating film and antifouling method for fishing gear / Fishnet

    JP2002080778A

  • Aqueous pollution-preventing resin composition

    JP2003277680A

  • Aqueous antifouling coating composition

    JP2005213336A