Method for producing aqueous alumina dispersion
A method for producing alumina dispersion using aliphatic amino acids at controlled temperatures and concentrations addresses productivity and impurity issues, resulting in a stable dispersion for ceramics and refractories.
Patent Information
- Application Number
- JP2024072363
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-26
AI Technical Summary
Existing methods for producing alumina dispersions require high temperature and pressure, leading to poor productivity and result in the presence of alkali metals and halogen elements that can cause defects in ceramics and refractories.
A method involving the heating and concentration of an aqueous solution of amorphous aluminum hydroxide and water-soluble aliphatic amino acids at 90 to 120°C for 5 to 36 hours, controlling the D/C value to 0.1-0.8, to produce a stable alumina dispersion with controlled particle size, pH, and amino acid content, minimizing alkali and halogen impurities.
The method produces a highly stable alumina dispersion with controlled viscosity and particle size, suitable for refractories and ceramics, reducing defects and improving productivity by avoiding high-pressure conditions.
Smart Images

Figure 0007577394000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an aqueous alumina dispersion. [Background technology]
[0002] Dispersions of solid fine particles such as alumina in liquids such as water are used in many applications. Alumina aqueous dispersions in which fine particles of alumina are dispersed in water have a wide range of uses, but have many problems to be solved, such as thickening of the aqueous dispersion, aggregation and precipitation of alumina, and problems caused by gelation after dispersion. In addition, their manufacturing methods often involve treating various aluminum salts with acids or alkalis, but it is necessary to reduce the presence of residual components.
[0003] Japanese Patent Laid-Open Publication No. 53-112299 (Patent Document 1) describes a method of obtaining an alumina sol by hydrothermal synthesis in the presence of a monovalent organic acid of an alumina gel obtained by neutralizing a water-soluble basic aluminum salt with an alkali. In addition, Japanese Patent Laid-Open Publication No. 57-111237 (Patent Document 2) proposes a method of producing an alumina sol by hydrothermally treating an alumina hydrate obtained by reacting a water-soluble aluminum salt with carbonic acid or a carbonate salt, mixing the treated product with a monovalent organic acid and drying, or drying the treated product and mixing it with a monovalent organic acid. In both of the above-mentioned production methods, hydrothermal treatment is required, and the hydrothermal treatment requires high pressure at a temperature exceeding 120°C, so a dedicated pressure-resistant reaction vessel is required, and productivity is poor.
[0004] Japanese Patent No. 4502133 (Patent Document 3) discloses a method for producing an acidic alumina sol, comprising: (A) a step of adding liquid or gaseous carbon dioxide to an aqueous alkali aluminate solution at a liquid temperature of 5 to 35°C to produce a reaction mixture having a pH of 10.5 to 11.2; (B) a step of hydrothermally treating the reaction mixture obtained in step (A) at a temperature of 110 to 250°C to produce an aqueous suspension containing an alumina hydrate having a boehmite structure; and (C) a step of desalting the aqueous suspension obtained in step (B) by adding water and an acid using an ultrafiltration method to form an acidic aqueous alumina sol having a pH of 3 to 7. In addition, Japanese Patent Laid-Open Publication No. 59-223223 (Patent Document 4) proposes a method for producing an alumina sol, which is characterized by neutralizing an aqueous solution of an alkali metal aluminate with an aqueous solution of an organic hydroxyl acid represented by the general formula R(OH)m(COOH)n...(I), R(OH)m(PO2H2)n...(II) (wherein m and n are 1 or more, R is a saturated or unsaturated aliphatic group having 1 to 10 carbon atoms, and the molecular weight per acid group is 200 or less). In both of the production methods of Patent Documents 3 and 4, an alkali metal aluminate (e.g., sodium aluminate, potassium aluminate) is used, so that a large amount of alkali metal remains in the alumina sol after synthesis, which causes a decrease in sintering temperature and abnormal crystal growth in the sintered body when used for ceramics or refractories, and may cause defects in the sintered body. In addition, in Patent Document 3, the hydrothermal treatment temperature exceeds 140° C. and is high pressure in the examples, so that a dedicated pressure-resistant reaction vessel is required, as in Patent Documents 1 and 2, and productivity is poor.
[0005] As a method for producing an aqueous alumina dispersion that does not use high temperature and high pressure, JP 2000-109315 A (Patent Document 5) describes a method for producing an aqueous alumina dispersion by mixing δ-alumina with a nitrogen-containing monocarboxylic acid and ultrasonically dispersing the mixture. The nitrogen-containing monocarboxylic acid used in Patent Document 5 contains an amino acid, and there is also a description of an aqueous dispersion containing an amino acid and an alumina. However, the technology of Patent Document 5 does not use an amino acid alone, but contains other acid components (specifically, nicotinic acid, lactic acid, and acetic acid) and alcohol components in addition to the amino acid, which provide storage stability for the alumina particles (Patent Document 5 Examples, etc.). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 53-112299 [Patent Document 2] Japanese Patent Publication No. 57-111237 [Patent Document 3] Patent No. 4502133 [Patent Document 4] Japanese Patent Application Publication No. 59-223223 [Patent Document 5] JP 2000-109315 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides a method for producing a highly stable aqueous alumina dispersion by utilizing only the protective stability of a water-soluble aliphatic amino acid, and for use in refractories and ceramics, with minimal alkali metal and halogen element content. [Means for solving the problem]
[0008] That is, the present invention provides the following aspects: [1] A method for producing an aqueous alumina dispersion, comprising heating and concentrating an aqueous solution of amorphous aluminum hydroxide, a water-soluble aliphatic amino acid, and water at a temperature of 90 to 120°C for 5 to 36 hours, the volume of the aqueous solution obtained by mixing the amorphous aluminum hydroxide, the water-soluble aliphatic amino acid and water during production is defined as C, and the volume of the aqueous alumina dispersion obtained by heating and concentrating the aqueous alumina dispersion at 90 to 120°C is defined as D, the value of D / C is controlled to be 0.1 to 0.8, The resulting aqueous alumina dispersion has the following characteristics: (a) the average particle size of the dispersed particles is in the range of 5 to 500 nm; (b) when the alumina-containing aqueous dispersion is dried at 100°C, the alumina particles are composed of one or more of boehmite and pseudo-boehmite; (c) the pH of the aqueous alumina dispersion is in the range of 2.0 to 5.3; (d) the alumina aqueous dispersion contains a water-soluble aliphatic amino acid; (e) the concentration of aluminum contained in the alumina aqueous dispersion in terms of alumina (Al2O3) is in the range of 0.3 to 11.5 mass %, and (f) A method for producing an aqueous alumina dispersion, characterized in that when a base is added to the aqueous alumina dispersion to adjust the pH to 5.4 to 10, it takes 24 hours or more for the viscosity of the aqueous alumina dispersion to reach 100,000 mPa s or more. [2] The method for producing an aqueous alumina dispersion according to [1], wherein the water-soluble aliphatic amino acid is added in an amount of 1.5 to 5 moles per mole of aluminum in the amorphous aluminum hydroxide. [3] The method for producing an aqueous alumina dispersion according to [1] or [2], wherein the water-soluble aliphatic amino acid is glycine, alanine, valine, leucine, isoleucine, or a mixture thereof. [4] The method for producing an alumina aqueous dispersion according to [1] or [2], wherein the alumina aqueous dispersion has a thixotropic index (TI value) of 2 to 10, which is expressed as [viscosity at a rotation speed of 6 rpm] / [viscosity at a rotation speed of 60 rpm] measured with a Brookfield viscometer. [5] The method for producing an alumina aqueous dispersion according to [1] or [2], wherein the alumina aqueous dispersion has a chlorine, bromine or iodine content of 0 to 0.02 mass%, and a sodium or potassium content of 0 to 0.05 mass%. [6] The amorphous aluminum hydroxide can be prepared by adjusting an aqueous solution of an aluminum inorganic acid salt selected from aluminum nitrate and / or aluminum sulfate to a pH of 5 to 8 with ammonia water to generate a precipitate of amorphous aluminum hydroxide; washing the produced amorphous aluminum hydroxide with water; separating the amorphous aluminum hydroxide from water; The method for producing an aqueous alumina dispersion according to [1] or [2], further comprising a step of drying the amorphous aluminum hydroxide so that the moisture content is 60 to 80 mass %. Effect of the Invention
[0009] The alumina aqueous dispersion of the present invention contains a water-soluble aliphatic amino acid. Since the amino acid has an amino group and a carboxyl group, it becomes a zwitterion in water. Therefore, it acts as a protective group to prevent the alumina in the alumina aqueous dispersion from suddenly coagulating or gelling.
[0010] Generally, the isoelectric point of alumina (the pH at which the zeta potential becomes 0) is said to be about pH 9, and with a typical acidic alumina sol, alumina particles rapidly aggregate and the alumina aqueous dispersion rapidly thickens when the pH approaches 9. However, since the alumina aqueous dispersion of the present invention uses a water-soluble aliphatic amino acid, even if the pH is changed to 5.4 to 10 using a base such as ammonia, gelation and the like due to thickening caused by a sudden change in pH is prevented, and unlike typical protective agents, the time until the viscosity of the alumina aqueous dispersion reaches 100,000 mPa s or more can be ensured to be 24 hours or more, expanding the range of use. [Brief description of the drawings]
[0011] [Figure 1]1 is an electron microscope photograph of the dried alumina aqueous dispersion obtained in Example 1. [Diagram 2] 1 is an X-ray diffraction image of the dried alumina aqueous dispersion obtained in Example 1. [Diagram 3] 1 is an X-ray diffraction image of only glycine crystallized by drying the alumina aqueous dispersion used in Example 1. [Figure 4] 1 is an X-ray diffraction image of powder obtained by calcining the dried product of the alumina aqueous dispersion obtained in Example 1 at 700° C. for 2 hours. [Diagram 5] 1 is a graph showing the particle size distribution, based on number, of the alumina aqueous dispersion obtained in Example 1, determined by dynamic light scattering. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below based on preferred embodiments, but the present invention is not limited to the following embodiments and various modifications are possible within the scope of the claims. In the present invention, the expression "numeric value 1 to numerical value 2" in a numerical range indicates that numerical value 1 is the lower limit and numerical value 2 is the upper limit. This means a range including numerical values 1 and 2 at both ends, and is synonymous with "numerical value 1 or more and numerical value 2 or less."
[0013] The present invention provides a method for producing an alumina aqueous dispersion containing alumina as dispersed particles. The alumina aqueous dispersion of the present invention is obtained by heating and concentrating an aqueous solution obtained by mixing amorphous aluminum hydroxide, a water-soluble aliphatic amino acid, and water at a temperature of 90 to 120°C for 5 to 36 hours. In this process, the D / C value is controlled to be 0.1 to 0.8, where C is the volume of the aqueous solution obtained by mixing amorphous aluminum hydroxide, a water-soluble aliphatic amino acid, and water, and D is the volume of the alumina aqueous dispersion obtained by heating and concentrating at 90 to 120°C. Furthermore, the obtained alumina aqueous dispersion has the following characteristics: (a) the average particle size of the dispersed particles is in the range of 5 to 500 nm; (b) when the alumina-containing aqueous dispersion is dried at 100°C, the alumina particles are composed of one or more of boehmite and pseudo-boehmite; (c) the pH of the aqueous alumina dispersion is in the range of 2.0 to 5.3; (d) the alumina aqueous dispersion contains a water-soluble aliphatic amino acid; (e) the concentration of aluminum contained in the alumina aqueous dispersion in terms of alumina (Al2O3) is in the range of 0.3 to 11.5 mass %, and (f) when a base is added to the alumina aqueous dispersion to adjust the pH to 5.4 to 10, it takes 24 hours or more for the viscosity of the alumina aqueous dispersion to reach 100,000 mPa s or more; has.
[0014] The alumina water dispersion of the present invention can be synthesized by heating and concentrating an aqueous solution of amorphous aluminum hydroxide, water-soluble aliphatic amino acid, and water at a temperature of 90 to 120°C for 1 to 24 hours. In this case, the volume of the aqueous solution of amorphous aluminum hydroxide, water-soluble aliphatic amino acid, and water is C, and the volume of the aqueous solution after heating and concentrating at 90 to 120°C is D. The D / C ratio is preferably 0.1 to 0.8, more preferably 0.2 to 0.7. If the D / C value is less than 0.1, insoluble precipitates will be generated from the alumina water dispersion, making the alumina water dispersion unstable. On the other hand, if the D / C value exceeds 0.8, the heating and concentrating is insufficient and the desired alumina water dispersion cannot be obtained.
[0015] (Amorphous Aluminum Hydroxide) The amorphous aluminum hydroxide used to produce the alumina aqueous dispersion of the present invention can be obtained by a precipitation step of adjusting an aqueous solution of an aluminum inorganic acid salt selected from aluminum nitrate and aluminum sulfate to pH 5 to 8 with ammonia water to generate a precipitate of amorphous aluminum hydroxide, a water washing step of washing the obtained amorphous aluminum hydroxide with water, a water separation step of separating the amorphous aluminum hydroxide from the water, and a drying step of drying the amorphous aluminum hydroxide to a moisture content of 60 to 80%.
[0016] In the first precipitation step, an amorphous aluminum hydroxide precipitation step for producing amorphous aluminum hydroxide, an aqueous solution of an aluminum inorganic acid salt selected from aluminum nitrate and aluminum sulfate is controlled to pH 5 to 8 with ammonia water. The pH in this step is preferably controlled to pH 6 to 7. If the pH is less than 5, it takes a very long time for the amorphous aluminum hydroxide precipitate to settle, resulting in poor productivity. On the other hand, if the pH exceeds 8, poor dissolution occurs when water is added to the amorphous aluminum hydroxide, a water-soluble aliphatic amino acid is added, and the mixture is heated and concentrated.
[0017] The precipitation step of the amorphous aluminum hydroxide precipitate is obtained by stirring at a temperature in the range of 15 to 45°C for 0.5 to 3 hours. Preferably, the temperature is 20 to 35°C for 1 to 2 hours. If the temperature in the precipitation step is less than 15°C, the reactivity of aluminum nitrate or aluminum sulfate with ammonia will be poor, and the reaction will take time, while if it exceeds 45°C, the ammonia will volatilize violently, and the pH will not be stable. If the stirring time is less than 0.5 hours, the reaction time will be insufficient and amorphous aluminum hydroxide will not precipitate sufficiently, and if it exceeds 3 hours, amorphous aluminum hydroxide can be synthesized, but the reaction time will be too long, resulting in poor productivity.
[0018] After obtaining the amorphous aluminum hydroxide precipitate from the precipitation step, the amorphous aluminum hydroxide precipitate is washed with water (water washing step), and then the water is separated (water separation step), followed by a drying step in which the amorphous aluminum hydroxide is dried to a moisture content of 60 to 80% by mass. The moisture content in the drying step is preferably 65 to 75% by mass. If the moisture content is less than 60% by mass, the dispersibility of the amorphous aluminum hydroxide when it is reacted with a water-soluble aliphatic amino acid and water is deteriorated, and if the moisture content exceeds 80% by mass, the moisture content of the amorphous aluminum hydroxide is too high, making it difficult to handle and reducing productivity. The moisture content is measured using MX50 manufactured by A&D Co., Ltd. at 105°C for 40 minutes.
[0019] The drying method for controlling the moisture content of amorphous aluminum hydroxide to 60 to 80 mass % is not particularly limited, and the heating temperature and heating time are also not particularly limited as long as they do not cause deterioration of amorphous aluminum hydroxide. Specifically, the heating temperature used in the drying step is 70 to 110°C, preferably 80 to 100°C, and the heating time is 1 to 12 hours, preferably 2 to 8 hours.
[0020] (Water-soluble aliphatic amino acids) The water-soluble aliphatic amino acid used in the production of the alumina aqueous dispersion of the present invention can be specifically represented by R-CH(NH2)COOH (chemical formula 1). In chemical formula 1, R is C n H 2n+1 where n is an integer selected from 0 to 3, or 1 to 3. Specifically, the water-soluble aliphatic amino acid is one or more selected from glycine, alanine, valine, leucine, and isoleucine. In the chemical formula 1 of the water-soluble aliphatic amino acid, those with n of 4 or more have poor thermal decomposition properties at 600°C, and cannot exhibit the effects of the invention.
[0021] (Method of producing alumina aqueous dispersion) In the present invention, the alumina water dispersion is obtained by mixing the amorphous aluminum hydroxide, the water-soluble aliphatic amino acid and water to form an aqueous solution, and then heating and concentrating the solution at a temperature of 90°C to 120°C for 5 to 36 hours. The heating method for the heating and concentration is not particularly limited, and a normal heating method or an autoclave can be used. Heating is performed with stirring. The stirring method can be a normal stirring method. The reaction temperature and reaction time are preferably 95 to 110°C. The reaction time is preferably 5 to 24 hours. If the temperature is less than 90°C, the reaction does not proceed sufficiently to form an alumina water dispersion. On the other hand, if the temperature exceeds 120°C, a special reaction environment such as applying pressure to increase the temperature is required, which deteriorates productivity. If the heating time is less than 1 hour, the concentration is insufficient and an alumina water dispersion may not be formed, and if it exceeds 36 hours, the heating and concentration time is too long, which deteriorates productivity.
[0022] The water-soluble aliphatic amino acid is added in an amount of 1.5 to 5 moles, more preferably 1.9 to 3 moles, per mole of aluminum in the amorphous aluminum hydroxide. If the amount of the water-soluble aliphatic amino acid added is less than 1.5 moles per mole of aluminum, the amount of the water-soluble aliphatic amino acid added will be insufficient, causing alumina aggregation, whereas if it exceeds 5 moles, the amount of the water-soluble aliphatic amino acid added will be excessive, causing the excess water-soluble aliphatic amino acid to precipitate during heating and concentration.
[0023] (Characteristics of alumina water dispersion) The alumina particles contained in the alumina aqueous dispersion of the present invention have the following six characteristics: (a) The average particle size of the dispersed particles is in the range of 5 to 500 nm. (b) when the alumina-containing aqueous dispersion is dried at 100°C, the alumina particles are composed of one or more of boehmite and pseudo-boehmite; (c) The pH of the aqueous alumina dispersion is in the range of 2.0 to 5.3. (d) The alumina aqueous dispersion contains a water-soluble aliphatic amino acid. (e) The alumina (Al2O3) equivalent concentration contained in the alumina aqueous dispersion is in the range of 0.3 to 11.5 mass %. (f) When a base is added to the aqueous alumina dispersion to adjust the pH to 5.4 to 10, it takes 24 hours or more for the viscosity of the aqueous alumina dispersion to reach 100,000 mPa s or more.
[0024] Feature (a) The average particle size of the alumina particles is preferably 5 to 500 nm, more preferably 10 to 200 nm. If the average particle size is less than 5 nm, the binding with inorganic particles becomes poor, and the shape retention during molding becomes poor. On the other hand, if the average particle size exceeds 500 nm, the average particle size is too large, and when inorganic powders of several hundred nm in size are bound and sintered, the primary particles become foreign matter and become the starting point of destruction. Here, the "average particle size" refers to the average particle size measured by number standard using a Zetasizer Nano ZS (manufactured by Spectris Co., Ltd.) in an aqueous solvent by dynamic light scattering method.
[0025] Feature (b) The crystal system of alumina in the alumina aqueous dispersion of the present invention is preferably such that the particles when the alumina aqueous dispersion is dried at 100°C are composed of one or more of boehmite and pseudo-boehmite, because during high-temperature sintering of ceramics, etc., they undergo phase transition to become γ-alumina or α-alumina depending on the firing conditions.
[0026] Feature (c) The pH of the alumina aqueous dispersion of the present invention is 2.0 to 5.3, and more preferably 3.0 to 5.0. When the pH of the alumina aqueous dispersion is less than 2.0, it becomes strongly acidic, and when mixed with inorganic particles, it alters the inorganic particles, or when the alumina aqueous dispersion contacts metal, it corrodes the metal. On the other hand, when the pH of the alumina aqueous dispersion is more than 5.3 and is about 10 or less, it takes more than 24 hours for the viscosity to reach 100,000 mPa·s or more, so that it is possible to mold refractories and prepare catalyst carriers, etc. However, when the pH of the alumina aqueous dispersion exceeds 10, it takes less than 24 hours for the viscosity to reach 100,000 mPa·s or more, so that the time until the alumina aqueous dispersion loses its fluidity is too short to be suitable for molding refractories or preparing catalyst carriers, etc., in terms of storage stability. The pH of the alumina aqueous dispersion is measured using a portable pH meter "HM-40P" and a pH composite electrode "GST-2739C" (Toa DKK Co., Ltd.).
[0027] Feature (d) The alumina aqueous dispersion of the present invention contains the water-soluble aliphatic amino acid used in forming the alumina aqueous dispersion, as described above. The water-soluble aliphatic amino acid is one or more selected from glycine, alanine, valine, leucine, and isoleucine, as described above. It is designed to have good thermal decomposition properties at low temperatures. Alumina aqueous dispersions containing lactic acid, malic acid, etc. have poor thermal decomposition properties and leave carbon residues, so they are not suitable for thermal decomposition applications at relatively low temperatures (e.g., 700°C). The water-soluble aliphatic amino acid crystallizes when the water in the alumina aqueous dispersion is evaporated. Therefore, when checking the crystal system of alumina in the above characteristic (b), it is dried at 100°C, and in that case, the water-soluble aliphatic amino acid may be crystallized.
[0028] Feature (e) The concentration of aluminum in the alumina in the alumina aqueous dispersion of the present invention in terms of Al2O3 is in the range of 0.3 to 11.5 mass%, preferably 2 to 10 mass%. If the concentration in terms of Al2O3 is less than 0.3 mass%, the alumina concentration in the alumina aqueous dispersion is too low, resulting in poor adhesion when used as a binder for inorganic particles. On the other hand, if the concentration in terms of Al2O3 exceeds 11.5 mass%, the storage stability of the alumina aqueous dispersion is poor, and precipitates may precipitate in the alumina aqueous dispersion over time. The calculation of the concentration in terms of Al2O3 in the alumina aqueous dispersion of the present invention is carried out as follows.
[0029] The aluminum concentration in the alumina aqueous dispersion is measured using an aluminum concentration meter (Agilent Technologies: ICP-OCS5110) and converted to alumina (Al2O3) using the following formula: The atomic weight of aluminum is 27, the atomic weight of oxygen is 16, and the molecular weight of Al2O3 is 102. The Al2O3 equivalent concentration (mass%) = Al concentration (mass%) × (102 / 27)
[0030] Feature(f) When the alumina aqueous dispersion of the present invention is adjusted to pH 5.4-10 by adding a base (e.g., ammonia), it takes 24 hours or more for the viscosity of the alumina aqueous dispersion to reach 100,000 mPa·s or more. The water-soluble aliphatic amino acid described in the above feature (d) has an amino group and a carboxyl group, and therefore becomes a zwitterion in water. Therefore, even if the pH is changed to 5.4-10 by using a base such as ammonia, gelation due to a sudden change in pH of the aqueous dispersion is prevented, and the time until the liquid viscosity reaches 100,000 mPa·s or more can be secured to be 24 hours or more, preferably 24 hours to 720 hours, and more preferably 30 to 240 hours, which is different from that of a general protective agent. This feature is due to the fact that the usable pH range of the alumina aqueous dispersion is expanded and the time during which the viscosity remains usable is extended, making it possible to mold ceramics and refractories by adding a slurry at a neutral to basic pH.
[0031] (Other features) The alumina aqueous dispersion of the present invention has a thixotropic index (TI value) of 2 to 10. The thixotropic index is measured by a B-type viscometer (using a spindle rotor of TVB10M TM-3 manufactured by Toki Sangyo Co., Ltd.), and the thixotropic index is preferably 2 to 10, more preferably 3 to 6, as expressed by TI value = [viscosity at a rotation speed of 6 rpm] / [viscosity at a rotation speed of 60 rpm]. If the TI value is less than 2, the liquid property does not have structural viscosity, so that it becomes difficult to retain the shape when a mixture of inorganic particles and the alumina aqueous dispersion is placed in a mold and molded, and the shape collapses. On the other hand, if the TI value exceeds 10, the structural viscosity is too strong, and it becomes difficult to deform unless the shear rate is increased, and it becomes difficult to perform pouring or the like when molding using a mold.
[0032] The alumina aqueous dispersion of the present invention has a low content of halogen elements and alkali metal elements. The content of halogen elements and alkali metal elements was measured by drying the alumina aqueous dispersion at 80°C for 30 minutes and measuring the powder obtained by drying with a scanning electron microscope (energy dispersive fluorescent X-ray (EDX) mounted on JCM-7000 manufactured by JEOL Ltd.). The content of halogen elements (specifically, chlorine, bromine or iodine) is preferably 0 to 500 ppm, more preferably 0 to 200 ppm. If the content of halogen elements exceeds 500 ppm, when used in refractories, ceramics, etc., gases derived from each element are generated during firing, which tends to cause corrosion inside the furnace. In addition, the content of alkali metal elements (specifically, sodium or potassium) is preferably in the range of 0 to 500 ppm, more preferably 0 to 200 ppm. If the content of alkali metals exceeds 500 ppm, when used in refractories, ceramics, etc., the sintering temperature is lowered during firing, which causes defects in the sintered body.
[0033] The alumina aqueous dispersion of the present invention must be designed to select materials that do not contain halogen gases such as chlorine and bromine that can damage furnaces when fired at high temperatures for ceramics or refractories, alkali metal elements such as sodium and potassium that can lower the sintering temperature of ceramics or refractories, or phosphorus and silica that can create different crystal phases.
[0034] The alumina aqueous dispersion of the present invention is thermally decomposed at low temperatures and leaves no organic residue. In order to confirm that the alumina aqueous dispersion of the present invention is thermally decomposed at low temperatures, a sample of the alumina aqueous dispersion dried at 100°C for 1 hour was heated in a platinum pan (TG-DTA60 manufactured by Rigaku Corporation) at a temperature rise rate of 10°C / min in a setting range of 25 to 650°C in an environment with an air flow rate of 100 ml / min, and the state of thermal decomposition was confirmed. The temperature at which the weight loss is completed is preferably in the range of 400 to 700°C, more preferably 450 to 650°C. The firing time is preferably in the range of 2 to 300 minutes, more preferably 5 to 60 minutes. If the temperature at which the weight loss is completed is less than 400°C, decomposition will start when resin or the like is blended and molding or the like is performed at a temperature of about 300°C, and there is a problem that the molded body will become unstable. On the other hand, if the temperature at which weight loss is complete exceeds 700°C, there is an issue that residual charcoal is likely to remain inside when firing thick refractories, ceramics, etc., which can cause defects and cracks. If the temperature at which weight loss is complete is less than two minutes, there is an issue that the thermal decomposition speed is too fast when firing large refractories or ceramics at a specified temperature, making it easy for firing variations to occur between the edges and the center, while if the temperature at which weight loss is complete exceeds 300 minutes, there is an issue that productivity decreases.
[0035] In the present invention, an aqueous solution obtained by adding water to amorphous aluminum hydroxide gel as a main raw material and adding a water-soluble aliphatic amino acid is heated and concentrated at 90 to 120°C for 5 to 36 hours to obtain an aqueous alumina dispersion having a pH of 2.0 to 5.3, an average particle size measured on a number basis in the range of 5 to 500 nm, an alumina (Al2O3) equivalent concentration of 0.3 to 11.5 mass% and a thixotropic index (TI value) in the range of 2 to 10. The aqueous alumina dispersion of the present invention can be calcined at a temperature of 400 to 700°C for 2 to 300 minutes to complete the thermal decomposition of organic matter, and can provide an aqueous alumina dispersion for ceramics and refractories in which the time required for the viscosity of the aqueous alumina dispersion to reach 100,000 mPa·s or more when the pH is adjusted to 5.4 to 10 by adding a base such as ammonia can be 24 hours or more.
[0036] The alumina aqueous dispersion of the present invention, through its material design, has a reduced content of halogen elements (i.e., chlorine, bromine, iodine) and a reduced content of alkali metals (i.e., sodium, potassium) that reduce the sintering temperature of ceramics and refractories, making it possible to provide an alumina aqueous dispersion that can reduce sintered defects caused by the addition of sodium or potassium to the sintering temperature without generating harmful halogen gases during firing.
[0037] The alumina aqueous dispersion of the present invention can thermally decompose organic matter at a relatively low temperature of 400 to 700°C, and contains a water-soluble aliphatic amino acid, so that it does not reach a viscosity of 100,000 mPa·s for more than 24 hours in neutral to weakly alkaline conditions, which is difficult for acidic alumina sol to achieve, and can be used as an inorganic binder over a wide pH range because it can be mixed with inorganic fillers such as ceramics and refractories and molded over a long period of time. In addition, the alumina aqueous dispersion of the present invention has an average particle size of 5 to 500 nm, so it is excellent in transparency, sinterability, etc., and can be used for alumina coating on glass, metals, etc., surface modification of catalyst carriers, fine abrasives, etc. EXAMPLES
[0038] The present invention will be described in more detail with reference to examples. The present invention should not be construed as being restricted to these examples. In the examples, "parts", "%" and the like are based on mass unless otherwise specified.
[0039] [Example 1] The alumina aqueous dispersion in the present invention was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.1 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then it was dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65.5%.
[0040] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of glycine was added, and the mixture was heated and concentrated at 200 rpm at 120°C for 8 hours to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 2.6 moles.
[0041] [Example 2] The alumina aqueous dispersion in the present invention was synthesized as follows. After 2250 g of 0.17 mol / l aluminum sulfate aqueous solution was placed in a 20 L separable flask, 1260.1 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 7.0. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, resulting in a moisture content of 65.1%.
[0042] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of glycine was added and the mixture was heated and concentrated at 120°C for 8 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 2.6 moles.
[0043] [Example 3] The alumina aqueous dispersion in the present invention was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1060.1 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.2. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then it was dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65.1%.
[0044] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1550 g of glycine was added and the mixture was heated and concentrated at 110°C for 20 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 4.1 moles.
[0045] [Example 4] The alumina aqueous dispersion in the present invention was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.2. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65.1%.
[0046] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of glycine was added and the mixture was heated and concentrated at 120°C for 20 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 2.6 moles.
[0047] [Example 5] The alumina aqueous dispersion in the present invention was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then it was dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65.5%.
[0048] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1300 g of valine was added and the mixture was heated and concentrated at 110°C for 20 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of valine added per mole of aluminum in the amorphous aluminum hydroxide was 2.2 moles.
[0049] [Example 6] The alumina aqueous dispersion in the present invention was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 71%.
[0050] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of glycine was added and the mixture was heated and concentrated at 110°C for 20 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 3.1 moles.
[0051] [Example 7] The alumina aqueous dispersion in the present invention was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Works, Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then it was dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65.5%.
[0052] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 500 g of glycine and 500 g of valine were added and the mixture was heated and concentrated at 200 rpm at 110°C for 20 hours to obtain an alumina aqueous dispersion. The total amount of glycine and valine added per mole of aluminum in the amorphous aluminum hydroxide was 2.6 moles.
[0053] [Example 8] The alumina aqueous dispersion in the present invention was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 67%.
[0054] 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel and dispersed by stirring, then 1000g of glycine was added and heated and concentrated at 100℃ for 24 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 2.7 moles.
[0055] [Comparative Example 1] The alumina aqueous dispersion in Comparative Example 1 was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1960.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 8.9. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (KBS-12 manufactured by Kansai Centrifugal Separation Works, Ltd.) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then it was dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65%.
[0056] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of glycine was added and the mixture was heated and concentrated at 110°C for 20 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 2.9 moles.
[0057] [Comparative Example 2] The alumina aqueous dispersion in Comparative Example 2 was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then it was dried for 8 hours at 100°C in a tray dryer, and the moisture content was 45%.
[0058] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of glycine was added and the mixture was heated and concentrated at 110°C for 20 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 1.9 moles.
[0059] [Comparative Example 3] The alumina aqueous dispersion in Comparative Example 3 was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65%.
[0060] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 3500 g of glycine was added and the mixture was heated and concentrated at 110°C for 20 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 9.0 moles.
[0061] [Comparative Example 4] The alumina aqueous dispersion in the comparative example was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65%.
[0062] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of glycine was added and the mixture was heated and concentrated at 200 rpm at 45°C for 20 hours to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 2.9 moles.
[0063] [Comparative Example 5] The alumina aqueous dispersion in the comparative example was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65%.
[0064] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 100 g of glycine was added and the mixture was heated and concentrated at 110°C for 20 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 0.3 moles.
[0065] [Comparative Example 6] The alumina aqueous dispersion in the comparative example was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65%.
[0066] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of glycine was added and the mixture was heated and concentrated at 110°C for 1 hour at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 2.9 moles.
[0067] [Comparative Example 7] The alumina aqueous dispersion in the comparative example was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.6 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Manufacturing Co., Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65%.
[0068] 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel and stirred to disperse it, then 2386.6g of 23.1mol / l lactic acid was added and stirred at 45℃ and 250rpm for 1 hour to synthesize an aqueous solution of basic aluminum lactate. The aqueous solution of basic aluminum lactate was heated and concentrated at 100℃ and 250rpm for 20 hours to obtain an aqueous dispersion of alumina. The amount of glycine added per 1mol of aluminum in the amorphous aluminum hydroxide was 2.5mol.
[0069] [Comparative Example 8] The alumina aqueous dispersion in the comparative example was synthesized as follows. 2250 g of 0.5 mol / l aluminum nitrate aqueous solution was added to a 20 L separable flask, and then 1160.1 g of 13.3 mol / l ammonia water was added while stirring at 250 rpm, and the mixture was stirred for 1 hour at a temperature of 30°C, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000 rpm for 1 minute in a centrifuge (Kansai Centrifugal Separation Works, Ltd., KBS-12) and 4 L of water were added three times to wash the amorphous aluminum hydroxide gel, and then it was dried for 1 hour in a tray dryer set at 100°C, and the moisture content was 65.5%.
[0070] After adding 6695 g of water to 1137.5 g of the dried amorphous aluminum hydroxide gel, 1000 g of acetic acid was added and the mixture was heated and concentrated at 120°C for 8 hours at 200 rpm to obtain an alumina aqueous dispersion. The amount of glycine added per mole of aluminum in the amorphous aluminum hydroxide was 3.3 moles.
[0071] The alumina aqueous dispersions obtained in Examples 1 to 8 and Comparative Examples 1 to 8 were subjected to the measurements described below, and the results are shown in Tables 1 to 4.
[0072] Al 2 O 3 (%) The Al concentrations in Examples 1 to 8 and Comparative Example 7 were measured using an aluminum concentration meter (ICP-OCS5110 manufactured by Agilent Technologies), and the Al concentrations were converted to Al2O3 concentrations and are shown in Tables 1 to 4.
[0073] pH The pH of the alumina aqueous dispersion was measured using a portable pH meter (manufactured by Toa DKK Co., Ltd.: HM-40P, pH composite electrode "GST-2739C"). The results are shown in Tables 1 to 4.
[0074] D / C The volume of the aqueous solution obtained by mixing amorphous aluminum hydroxide, water-soluble aliphatic amino acid, and water was taken as C, and the volume of the aqueous alumina dispersion obtained by heating and concentrating it at 90 to 120° C. was taken as D, and D / C was calculated. The results are shown in Tables 1 to 4.
[0075] Crystal system when dried at 100℃ The crystal systems of Examples 1 to 8 and Comparative Example 7 when dried at 100° C. were measured using an X-ray diffractometer (MiniFlex600, manufactured by Rigaku Corporation). The results are shown in Tables 1 to 4.
[0076] TI value (thixotropic index) The thixotropic index (TI value) was measured by measuring the viscosity using a B-type viscometer (a spindle rotor of TVB10M TM-3 manufactured by Toki Sangyo Co., Ltd.), and calculated as TI value = [viscosity at a rotation speed of 6 rpm] / [viscosity at a rotation speed of 60 rpm]. The results are shown in Tables 1 to 4.
[0077] Average particle size The average particle diameters of the alumina in Examples 1 to 8 and Comparative Example 7 were measured by dynamic light scattering in an aqueous solvent using a Zetasizer Nano ZS (manufactured by Spectris, Inc.), and the average particle diameters measured by number are shown in Tables 1 to 4.
[0078] Liquid viscosity check result after 24 hours To the alumina aqueous dispersions of Examples 1 to 8 and Comparative Example 7, 25% ammonia water was added to adjust the pH to 9, and then the dispersions were sealed to prevent evaporation and left to stand at room temperature for 24 hours. Then, a B-type viscometer (Toki Sangyo Co., Ltd.: TVB10M TM-3 spindle rotor) was used to check whether the viscosity exceeded 100,000 mPa s after 24 hours, and the results are shown in Tables 1 to 4. Evaluation criteria Good: Viscosity of liquid (aqueous dispersion) after 24 hours is less than 100,000 mPa s ×: Viscosity of liquid (aqueous dispersion) after 24 hours is 100,000 mPa s or more
[0079] Chlorine, bromine, iodine, sodium, potassium concentrations The concentrations of chlorine, bromine, iodine, sodium, and potassium in Examples 1 to 8 and Comparative Example 7 were measured using EDS (energy dispersive fluorescent X-ray) with a scanning electron microscope (JEOL Ltd. JCM-7000 equipped with energy dispersive fluorescent X-ray (EDX)) and are shown in Tables 1 to 4. nd: not detected.
[0080] Thermal decomposition evaluation The thermal decomposition properties of Examples 1 to 8 and Comparative Example 7 were evaluated by dropping 5 g of the alumina aqueous dispersion of Examples 1 to 8 and Comparative Example 7 into a 50 ml alumina crucible (Nikkato Corporation), drying the mixture at 100°C for 5 minutes using a hot air circulation dryer, and then firing the mixture at 650°C for 15 minutes in an electric furnace (FO200, Yamato Scientific Corporation). The appearance (color) of the mixture remaining in the alumina crucible was confirmed, and the results are shown in Tables 1 to 4.
[0081] [Table 1]
[0082] [Table 2]
[0083] [Table 3]
[0084] [Table 4]
[0085] The alumina aqueous dispersion of Example 1 was dried in a glass evaporating dish at 100° C. for 10 minutes and observed at 100,000 times magnification using a field emission scanning electron microscope (JEOL Ltd., JSM-7001F). The results are shown in FIG.
[0086] The alumina aqueous dispersion of Example 1 was placed in a glass evaporating dish and dried in a hot air circulation dryer at 100° C. for 20 minutes, and the powder and glycine were measured using an X-ray diffraction device (Mini Flex600, manufactured by Rigaku Corporation). The results are shown in FIG. 2 and FIG. 3.
[0087] The alumina water dispersion of Example 1 was placed in a glass evaporating dish and dried in a hot air circulation dryer at 100°C for 20 minutes, and the powder was placed in an alumina crucible and fired in an electric furnace (Yamato Scientific Co., Ltd.: FO200) at 700°C for 2 hours. The powder was measured using an X-ray diffraction device (Rigaku Co., Ltd.: Mini Flex600) and the evaluation results are shown in Figure 4.
[0088] The alumina aqueous dispersion of Example 1 was measured in an aqueous solvent by dynamic light scattering using a Zetasizer Nano ZS (manufactured by Spectris Corporation), and the results measured on a number basis are shown in FIG.
[0089] As shown in Tables 1 and 2, in all of Examples 1 to 5, 7 and 8, an alumina aqueous dispersion of boehmite was prepared, and the Al2O3 value, pH, average particle size, and TI value were within the range of the present invention. When the mixture was baked at 600°C for 15 minutes, white matter was confirmed, no organic matter was found to remain after baking, and it was confirmed that the thermal decomposition of the organic matter was completed. It was also confirmed that when the pH was adjusted to 10 with ammonia, the viscosity did not exceed 100,000 mPa·s after 24 hours. In addition, in Example 6, an alumina aqueous dispersion of boehmite + pseudo-boehmite was prepared, and the Al2O3 value, pH, average particle size, and TI value were within the range of the present invention. When the mixture was baked at 650°C for 15 minutes, white matter was confirmed, no organic matter was found to remain after baking, and it was confirmed that the thermal decomposition of the organic matter was completed. It was also confirmed that when the pH was adjusted to 10 with ammonia, the viscosity did not exceed 100,000 mPa·s after 24 hours.
[0090] In Comparative Example 1, as shown in Table 3, the pH of the amorphous aluminum hydroxide was too high at 8.9, and thus some amorphous aluminum hydroxide remained undissolved in the next step. In Comparative Example 2, the moisture content of the amorphous aluminum hydroxide was low at 45%, and thus some amorphous aluminum hydroxide remained undissolved. In Comparative Example 3, glycine was in excess of 9.0 moles relative to aluminum, and thus glycine precipitated during heating and concentration. In Comparative Example 4, the heating temperature during the formation of the aqueous alumina dispersion was too low at 45° C., and thus heating and concentration could not be performed, and thus an aqueous alumina dispersion could not be produced. Furthermore, in Comparative Example 4, the D / C was high at 0.98, and the pH of the aqueous alumina dispersion was also high at 6.5.
[0091] In Comparative Example 5, the amount of glycine added is too small at 0.3 moles relative to aluminum, so when the alumina aqueous dispersion is heated and concentrated, the amount of protective agent is too small, and alumina particles aggregate. In Comparative Example 6, the heating time is too short at 1 hour, so there is insufficient time for heating and concentration, and an alumina aqueous dispersion cannot be produced. In Comparative Example 6, the pH of the alumina aqueous dispersion is also high at 5.6, and the D / C is also high at 0.91. In Comparative Example 7, a boehmite-based alumina aqueous dispersion can be produced, but since it contains lactic acid, thermal decomposition is insufficient at 650°C x 15 minutes heating, the film surface is black, and it does not become alumina. In addition, there is a problem with low-temperature thermal decomposition. In Comparative Example 8, acetic acid is used instead of a water-soluble aliphatic amino acid, so an alumina aqueous dispersion appears to be formed, but the protective effect of the water-soluble aliphatic amino acid does not work, and white precipitates form during storage (poor storage stability).
[0092] FIG. 1 is an electron microscope image of the alumina aqueous dispersion of Example 1 dried at 100° C. for 10 minutes. It can be seen that the majority of the particles have a primary particle size of 100 nm or less, confirming that the desired alumina aqueous dispersion was synthesized.
[0093] FIG. 2 shows the X-ray diffraction of the alumina water dispersion of Example 1 dried at 100°C for 20 minutes, and FIG. 3 shows the X-ray diffraction of glycine (crystallized glycine) alone when the alumina water dispersion was dried at 100°C for 20 minutes. In FIG. 2, the peak of boehmite is indicated by →, and the peak of glycine is indicated by the tip of the → arrow filled in black, and it is confirmed that the peak of crystallized glycine and the peak of boehmite are mixed. It was confirmed that an alumina particle dispersion was created in which boehmite particles and crystallized glycine, which is a water-soluble aliphatic amino acid, are mixed. If the crystallized glycine in FIG. 3 is removed from FIG. 2, the X-ray diffraction of boehmite is obtained.
[0094] FIG. 4 shows the X-ray diffraction pattern of the alumina aqueous dispersion of Example 1 which was dried at 100° C. for 20 minutes and then fired at 750° C. for 2 hours. It shows a gamma alumina peak pattern, and it was confirmed that by increasing the firing temperature of the alumina particle dispersion in which boehmite particles and glycine coexist, glycine is thermally decomposed and the boehmite particles undergo a phase transition to gamma alumina.
[0095] FIG. 5 shows the particle size distribution of the alumina aqueous dispersion of Example 1 measured on a number basis. It was confirmed that the average particle size was 22 nm and that the alumina aqueous dispersion did not contain coarse particles exceeding 100 nm.
[0096] The present invention also encompasses the following aspects: [1] A method for producing an aqueous alumina dispersion, comprising heating and concentrating an aqueous solution of amorphous aluminum hydroxide, a water-soluble aliphatic amino acid, and water at a temperature of 90 to 120°C for 5 to 36 hours, the volume of the aqueous solution obtained by mixing the amorphous aluminum hydroxide, the water-soluble aliphatic amino acid and water during production is defined as C, and the volume of the aqueous alumina dispersion obtained by heating and concentrating the aqueous alumina dispersion at 90 to 120°C is defined as D, the value of D / C is controlled to be 0.1 to 0.8, The resulting aqueous alumina dispersion has the following characteristics: (a) the average particle size of the dispersed particles is in the range of 5 to 500 nm; (b) when the alumina-containing aqueous dispersion is dried at 100°C, the alumina particles are composed of one or more of boehmite and pseudo-boehmite; (c) the pH of the aqueous alumina dispersion is in the range of 2.0 to 5.3; (d) the alumina aqueous dispersion contains a water-soluble aliphatic amino acid; (e) the concentration of aluminum contained in the alumina aqueous dispersion in terms of alumina (Al2O3) is in the range of 0.3 to 11.5 mass %, and (f) A method for producing an aqueous alumina dispersion, characterized in that when a base is added to the aqueous alumina dispersion to adjust the pH to 5.4 to 10, it takes 24 hours or more for the viscosity of the aqueous alumina dispersion to reach 100,000 mPa s or more. [2] The method for producing an aqueous alumina dispersion according to [1], wherein the water-soluble aliphatic amino acid is added in an amount of 1.5 to 5 moles per mole of aluminum in the amorphous aluminum hydroxide. [3] The method for producing an aqueous alumina dispersion according to [1] or [2], wherein the water-soluble aliphatic amino acid is glycine, alanine, valine, leucine, isoleucine, or a mixture thereof. [4] The method for producing an alumina aqueous dispersion according to any one of [1] to [3], wherein the alumina aqueous dispersion has a thixotropic index (TI value) of 2 to 10, which is expressed as [viscosity at a rotation speed of 6 rpm] / [viscosity at a rotation speed of 60 rpm] measured with a Brookfield viscometer. [5] The method for producing an alumina aqueous dispersion according to any one of [1] to [4], wherein the alumina aqueous dispersion has a chlorine, bromine or iodine content of 0 to 0.02 mass%, and a sodium or potassium content of 0 to 0.05 mass%. [6] The amorphous aluminum hydroxide can be prepared by adjusting an aqueous solution of an aluminum inorganic acid salt selected from aluminum nitrate and / or aluminum sulfate to a pH of 5 to 8 with ammonia water to generate a precipitate of amorphous aluminum hydroxide; washing the produced amorphous aluminum hydroxide with water; separating the amorphous aluminum hydroxide from water; The method for producing an aqueous alumina dispersion according to any one of [1] to [5], further comprising a step of drying the amorphous aluminum hydroxide so that the moisture content is 60 to 80 mass %.
Claims
1. The method for producing an aqueous alumina dispersion comprises heating and concentrating an aqueous solution of amorphous aluminum hydroxide, a water-soluble aliphatic amino acid, and water at a temperature of 90 to 120° C. for 5 to 36 hours, the volume of the aqueous solution obtained by mixing the amorphous aluminum hydroxide, the water-soluble aliphatic amino acid and water during production is defined as C, and the volume of the aqueous alumina dispersion obtained by heating and concentrating the aqueous alumina dispersion at 90 to 120° C. is defined as D, the value of D / C is controlled to be 0.1 to 0.8, The amorphous aluminum hydroxide can be prepared by adjusting an aqueous solution of an aluminum inorganic acid salt selected from aluminum nitrate and / or aluminum sulfate to a pH of 5 to 8 with aqueous ammonia to form a precipitate of amorphous aluminum hydroxide; washing the produced amorphous aluminum hydroxide with water; separating the amorphous aluminum hydroxide from water; drying the amorphous aluminum hydroxide to a moisture content of 60 to 80% by mass; The water-soluble aliphatic amino acid is added in an amount of 1.5 to 5 moles per mole of aluminum in the amorphous aluminum hydroxide, The obtained aqueous alumina dispersion is The alumina aqueous dispersion has a chlorine, bromine or iodine content of 0 to 0.02 mass %, a sodium or potassium content of 0 to 0.05 mass %, and Features as below: (a) the average particle size of the dispersed particles is in the range of 5 to 500 nm; (b) when the alumina-containing aqueous dispersion is dried at 100° C., the alumina particles are composed of at least one of boehmite and pseudo-boehmite; (c) the pH of the aqueous alumina dispersion is in the range of 2.0 to 5.3; (d) the alumina aqueous dispersion contains a water-soluble aliphatic amino acid; (e) Alumina (Al) of aluminum contained in an alumina aqueous dispersion 2 O 3 ) the converted concentration is in the range of 0.3 to 11.5% by mass, and (f) when a base is added to the alumina aqueous dispersion to adjust the pH to 5.4 to 10, the time required for the viscosity of the alumina aqueous dispersion to reach 100,000 mPa·s or more is 24 hours or more.
2. 2. The method for producing an aqueous alumina dispersion according to claim 1, wherein the water-soluble aliphatic amino acid is glycine, alanine, valine, leucine, isoleucine or a mixture thereof.
3. The method for producing an alumina aqueous dispersion according to claim 1 or 2, wherein the alumina aqueous dispersion has a thixotropic index (TI value) of 2 to 10, the TI value being expressed as [viscosity at a rotation speed of 6 rpm] / [viscosity at a rotation speed of 60 rpm] measured by a B-type viscometer.
Citation Information
Patent Citations
Production of alumina sol
JP1978112299A
Production of alumina sol
JP1982111237A
Manufacture of alumina sol
JP1984223223A
Alumina sol composition
JP1986283335A
Alumina dispersant and alumina dispersion
JP2000109315A
Cited By
Alumina aqueous dispersion and method for producing same
JP7808393B1
Castable refractories and precast blocks
JP7834229B1