Recycling process for used lithium-ion batteries
The described process efficiently recovers high-purity nickel, cobalt, and lithium from spent lithium-ion batteries by heating with hydrogen, followed by aqueous treatment and solid-solid separation, addressing impurity removal and cost-efficiency challenges.
Patent Information
- Application Number
- JP2021500529
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-07-10
- Filing Date
- 2019-07-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-07-09
AI Technical Summary
Existing methods for recovering valuable metals from spent lithium-ion batteries face challenges in efficiently removing impurities such as fluorine and phosphorus compounds, achieving high purity, and reducing energy consumption and costs.
A process involving heating lithium-containing transition metal oxide materials from spent batteries in the presence of hydrogen, followed by aqueous treatment, solid-solid separation, and recovery of lithium and nickel/cobalt as hydroxides or salts, with optional steps for further extraction and purification.
The process achieves high-purity recovery of nickel, cobalt, and lithium with reduced energy consumption and cost, effectively removing impurities like fluorine and phosphorus, suitable for recycling in new battery production.
Smart Images

Figure 0007577642000001 
Figure 0007577642000002 
Figure 0007577642000003
Abstract
Description
Summary of the Invention
[0001] The present invention is directed to a process for the recovery of transition metals from nickel-containing spent lithium ion batteries, the process comprising: (a) heating a lithium-containing transition metal oxide material, containing typical impurities such as fluorine compounds (e.g., inorganic fluorides) and / or compounds of phosphorus, in the presence of H2 to a temperature in the range of 200-900°C; (b) treating the product obtained in step (a) with an aqueous medium; (c) solid-solid separation to remove Ni from the solid residue of step (b); (d) recovery of Li as hydroxide or salt from the solution obtained in step (b) and, optionally, further (e) extraction of Ni and, where applicable, Co from the solid Ni concentrate obtained in step (c).
[0002] The storage of electrical energy is a subject of increasing interest. Efficient storage of electrical energy allows electrical energy to be produced when advantageous and used when and where it is needed. Secondary electrochemical cells are well suited for this purpose because they are rechargeable. Secondary lithium batteries are of particular interest for energy storage because of their high energy density due to the small atomic weight and large ionization energy of lithium, and their widespread use in many portable electronic devices such as mobile phones, laptop computers, and mini cameras, as well as in electric vehicles. The growing demand for raw materials, especially cobalt and nickel, will pose challenges in the future.
[0003] The life span of lithium-ion batteries is not unlimited. Therefore, it is expected that the number of used lithium-ion batteries will increase. Since they contain important transition metals, such as but not limited to cobalt and nickel, as well as lithium, used lithium-ion batteries can be a valuable source of raw materials for new generation lithium-ion batteries. Therefore, an increasing amount of research is being conducted with the aim of recycling transition metals - and, optionally, lithium - from used lithium-ion batteries.
[0004] Lithium-ion batteries or lithium-ion battery components that do not meet specifications and requirements, so-called off-spec materials and manufacturing waste, can also be a source of raw materials.
[0005] Two main processes are subject to the recovery of raw materials. One main process is based on the smelting of the corresponding battery scrap and the subsequent hydrometallurgical processing of the metal alloy (matte) obtained from the smelting process. The other main process is the direct hydrometallurgical processing of the battery scrap material. The principle is disclosed in WO2017 / 091562 and in J.power Sources, 2014, 262, 255 et seq. Such hydrometallurgical processes provide the transition metals as aqueous solutions or in precipitated form, for example as hydroxides, either separately or already in the desired stoichiometry for making new cathode active materials. In the latter case, the composition of the metal salt solution can be adjusted to the desired stoichiometry by adding single metal components.
[0006] WO2017 / 091562 discloses the co-precipitation of transition metals. WO2014 / 180743 discloses a co-precipitation process in which ammonia or an amine is used.
[0007] Starting with conversion experiments using model materials such as LiCoO2, JP2012-229481 discloses a process for recovering metals from spent lithium-ion batteries, including a pre-soaking step followed by high-temperature oxidation, reductive roasting, water treatment by filtration, and recovery of lithium carbonate from the filtrate and transition metals from the residue.
[0008] Known methods for recovering such valuable materials typically face the problem that used batteries, i.e. cells containing most of these materials therein, either need to be disassembled to mechanically separate the constituents such as electrodes and electrolytes, or contain high levels of impurities such as fluorine and / or phosphorus compounds, which need to be removed to recover the desired materials in a purity that can be used for the production of new cells (battery grade materials). It was therefore an object of the present invention to provide a process that allows for the easy recovery of nickel and, if present, cobalt and manganese. Another object of the present invention was to provide a method for recovering the further valuable elements contained in the battery scrap, namely lithium, and carbon as graphite. A further object of the present invention was to provide an economical process that reduces the number of costly and / or energy consuming steps. A particular object of the present invention was to provide a process that allows for the efficient recovery of nickel, optionally cobalt and manganese, and lithium. A further object of the present invention was to provide a process for recovering said transition metals and lithium in high purity, in particular with a low content of copper and precious metals such as Ag, Au and platinum group metals.
[0009] Thus, the present process as defined for the first time is found, hereinafter also referred to as the inventive process or the inventive recycling process. The inventive process comprises the steps defined in more detail below, hereinafter also referred to as step (a), step (b), step (c) etc.:
[0010] (a) heating a lithium-containing transition metal oxide material originating from a lithium ion battery and containing fluorine compounds and / or phosphorus compounds as impurities in the presence of H2 to a temperature in the range of 200 to 900°C; (b) treating the product obtained in step (a) with an aqueous medium; (c) solid-solid separation to remove Ni and, where applicable, Co from the solid residue of step (b); (d) recovery of Li as hydroxide or salt from the solution obtained in step (b); (e) Extraction of Ni and, if applicable, Co from the solid Ni concentrate obtained in step (c).
[0011] Thus, an exemplary process of the present invention comprises the steps (a) heating the lithium-containing transition metal oxide material to a temperature in the range of 200 to 900° C. in the presence of H2; (b) treating the product obtained in step (a) with an aqueous medium; (c) solid-solid separation to remove Ni from the solid residue of step (b); (d) recovery of Li as hydroxide or salt from the solution obtained in step (b); (e) extraction of Ni and, where applicable, Co from the solid Ni concentrate obtained in step (c); The lithium-containing transition metal oxide material heated in step (a) originates from a lithium ion battery and contains fluorine in the range of 0.5 to 8, typically 1 to 8, particularly 2 to 8 wt %, and / or phosphorus in the range of 0.2 wt % to 2 wt %, based on the weight of the lithium-containing transition metal oxide material.
[0012] However, it is also possible to carry out steps (a)-(c) in the following order: step (a), step (c), step (b). In a preferred embodiment of the invention, steps (a)-(c) are carried out in the alphabetical order given above, followed by steps (d) and (e).
[0013] Step (a) involves heating the lithium-containing transition metal oxide material to a temperature in the range of 200 to 900 ° C, preferably 300 to 600 ° C, more preferably 350 to 500 ° C. In particular under oxidizing conditions, but also to a lesser extent under reducing atmospheres, it is generally preferred not to expose the lithium-containing transition metal oxide material to temperatures above 500 ° C (for example, temperatures above 450 ° C), since strong heating tends to increase the formation of insoluble species (such as LiMnO 2 ). It is therefore preferred to keep the temperature below 500 ° C or even below 450 ° C during the preparation of the lithium-containing transition metal oxide material and also in step (a), preferably to keep the material in this step at a temperature in the range of 350 to 450 ° C, in particular 380 to 440 ° C.
[0014] The atmosphere used to carry out the reduction contains 0.1-100% by volume of hydrogen. In one embodiment, it contains 3% to 50% by volume of hydrogen, the remainder being a non-oxidizing gas, preferably nitrogen, argon, steam, carbon monoxide, carbon dioxide or a mixture of at least two of these gases. Preferred non-oxidizing gases are nitrogen and steam and mixtures of nitrogen and steam. In a preferred embodiment, step (a) of the process is carried out under an atmosphere containing mainly hydrogen, for example 35-100% by volume, preferably 50-100% by volume (at standard pressure) of hydrogen, the remainder, if present, being a non-oxidizing gas.
[0015] In one embodiment of the present invention, step (a) has a duration ranging from 10 minutes to 30 hours, preferably from 20 minutes to 8 hours, more preferably from 30 minutes to 4 hours. Of particular technical interest is a duration of step (a) lasting from 20 to 90 minutes, in particular from 30 to 60 minutes.
[0016] The hydrogen concentration in the reducing atmosphere and the reaction time are interdependent: usually, a lower concentration of hydrogen requires a longer reduction time and vice versa.
[0017] Thus, in a preferred process of the invention, step (a) is carried out by heating the lithium-containing transition metal oxide material to a temperature in the range of 350-450 ° C. for a period of 20-90 minutes in the presence of more than 35%, particularly 50-100% by volume of H2. Within the scope of the invention, a particularly preferred process is to carry out step (a) using a temperature of 400-420 ° C. for up to 2.5 hours (particularly about 30-60 minutes) and 35 vol.% or more of hydrogen to recover Li in a particularly efficient manner, since applying too high a temperature can reduce the yield, and longer durations do not have negative effects, but tend to reduce the space-time yield, while H2 concentrations ≥ 35 vol.% are preferred due to short reaction times ≤ 2.5 hours, and using pure hydrogen, optimal space-time yields can be achieved.
[0018] In one embodiment of the present invention, the reduction conditions related to the hydrogen concentration and the duration of step (a) are selected such that at least a portion of the lithium-containing transition metal oxide material contains a paramagnetic, ferromagnetic or ferrimagnetic component that can be separated by application of a magnetic field. Preferred is the formation of a ferromagnetic or ferrimagnetic component resulting from at least partial reduction of the lithium-containing transition metal material. The extent of reduction can vary in the range of 1-100% with respect to the nickel contained in the lithium-containing transition metal material, preferably in the range of 80-100%.
[0019] The lithium-containing transition metal oxide material is a material derived from a lithium-ion battery or a part of a lithium-ion battery. Typically, the lithium-containing transition metal oxide material is obtained after mechanical removal of the casing, wiring, or circuitry, and therefore typically consists mainly of cell materials. For safety reasons, such lithium-ion batteries are fully discharged, for example by immersion in a dry conductive bath, such as metal shreds, or in a controlled manner that allows them to supply current to the power grid, for example through an inverter. Otherwise, a shortcut may occur that causes a fire and explosion hazard. Such lithium-ion batteries can be disassembled, punched, crushed, for example in a hammer mill, or shredded, for example in an industrial shredder.
[0020] Before starting step (a), it is advantageous to at least partially remove the electrolyte, in particular the electrolyte comprising an organic solvent or a mixture of organic solvents, for example by drying at subatmospheric pressure, for example at a temperature in the range of 50 to 250° C. As mentioned above, it is preferred that the lithium-containing transition metal oxide material is not exposed to higher temperatures (in particular 400° C. or higher) under oxidizing conditions before being subjected to this step (a).
[0021] In one embodiment of the present invention, the lithium-containing transition metal oxide material is from battery scrap. In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material is from mechanically treated battery scrap, for example, battery scrap processed by hammer mill or industrial shredder. Such lithium-containing transition metal oxide material can have an average particle diameter (D50) in the range of 1 μm to 1 cm.
[0022] In one embodiment of the present invention, step (a) is preceded by step (a1), which step (a1) comprises, for example, the removal of carbon or organic polymers by solid-solid separation methods. Examples of such solid-solid separation methods are electrical sorting, sieving, magnetic separation, or other sorting methods. Solid-solid separation can be carried out dry or in the presence of a suitable dispersion medium, preferably water.
[0023] In one embodiment of the present invention, the mechanically treated battery scrap is ground prior to step (a). Such grinding is preferably carried out in a ball mill or an agitated ball mill. Grinding can be carried out under wet or dry conditions, preferably under dry conditions.
[0024] In one embodiment of the present invention, the mechanically processed battery scrap is subjected to a solvent treatment to dissolve and separate the polymer binder used to bind the lithium transition metal oxide to the current collector film. Suitable solvents are N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N-ethylpyrrolidone, dimethylsulfoxide, hexamethylphosphoramide, tetramethylurea, trimethyl phosphate, and triethyl phosphate, either in pure form or in mixtures.
[0025] The above solvent treatments can be carried out in successive steps using one or more solvents, or in one step using a solvent capable of dissolving the electrolyte components and the binder polymer. The solvent is applied at a temperature range of 10°C to 200°C. Higher temperatures in the range of 50-200°C, preferably 100 and 150°C, may be required, especially for dissolving the polymer. The upper temperature limit is usually limited by the boiling point of the solvent, unless pressures above 1 bar are applied.
[0026] In one embodiment, the washing of the mechanically treated battery scrap is carried out in the absence of moisture, for example under a dry gas such as dry air, dry nitrogen, etc., using an aprotic solvent.
[0027] In one embodiment of the present invention, the lithium-containing transition metal oxide material does not contain a majority of impurities, such as, but not limited to, materials from other components or components of a lithium-ion battery. Such lithium-containing transition metal oxide materials may include off-spec materials.
[0028] However, when applicable, the lithium-containing transition metal oxide material preferably contains, in the range of 0.1 to 80% by weight, a compound other than a nickel compound such as a nickel / cobalt component or a nickel / cobalt / manganese or nickel / cobalt / aluminum compound, and in extreme cases, the precious material is a minor component. Examples of such components are carbon in a conductive form, hereinafter also referred to as conductive carbon, such as graphite, soot, and graphene. Further examples of impurities are copper and its compounds, aluminum and aluminum compounds, such as alumina, iron and iron compounds, zinc and zinc compounds, silicon and silicon compounds, such as silica and silicon oxide SiO with 0 < y ≦ 2 y , tin, silicon-tin alloys, and organic polymers such as polyethylene, polypropylene, and fluorinated polymers, such as polyvinylidene fluoride, tetrafluoroethylene polymers, etc. Further impurities include, for example, fluorine compounds that can arise from the liquid electrolyte, such as inorganic fluorides, and phosphorus compounds, in products resulting from the hydrolysis of widely used LiPF6 and LiPF6. The battery scrap serving as the starting material for the process of the present invention may be derived from multiple sources, and thus, the lithium-containing transition metal oxide material in most embodiments contains a compound other than a nickel / cobalt compound or a nickel / cobalt / manganese or nickel / cobalt / aluminum component, and when applicable, one of such components is carbon in a conductive form in the range of 2 to 65% by weight, referring to the entire lithium-containing transition metal oxide material.
[0029] In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material contains copper in the range of 20 ppm to 3% by weight, as a metal or in one or more forms of its compounds.
[0030] In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material contains aluminum in the range of 100 ppm to 15% by weight, as a metal or in one or more forms of its compounds.
[0031] In a preferred embodiment of the invention, the lithium-containing transition metal oxide material contains iron in the range of 100 ppm to 5 wt. % as a metal or an alloy or one or more of its compounds.
[0032] In a preferred embodiment of the invention, the lithium-containing transition metal oxide material contains zinc in the range of 20 ppm to 2 wt. % as a metal or an alloy or one or more forms of compounds thereof.
[0033] In a preferred embodiment of the invention, the lithium-containing transition metal oxide material contains zirconium in the range of 20 ppm to 2 wt % as a metal or an alloy or one or more of its compounds.
[0034] In a preferred embodiment of the invention, the lithium-containing transition metal oxide material contains in the range of 0.5 to 8, typically 1 to 8, in particular 2% to 8% by weight of fluorine, calculated as the sum of the organic fluoride and the inorganic fluoride in the one or more inorganic fluorides bound to the polymer.
[0035] In a preferred embodiment of the invention, the lithium-containing transition metal oxide material contains phosphorus in the range of 0.2% to 2% by weight. The phosphorus can occur in one or more inorganic compounds.
[0036] Each of the above percentages is by weight of the dry material (ie, the lithium-containing transition metal oxide material).
[0037] The lithium-containing transition metal oxide material contains nickel and cobalt. Examples of lithium-containing transition metal oxide materials can be based on lithiated nickel cobalt manganese oxide ("NCM") or lithiated nickel cobalt aluminum oxide ("NCA") or mixtures thereof.
[0038] Examples of layered nickel-cobalt-manganese oxides are those of the general formula Li 1+x (Ni a Co b Mn c M1 d ) 1-x O 2の Compound M 1 is selected from Mg, Ca, Ba, Al, Ti, Zr, Zn, Mo, V, and Fe, and the other variables are defined as follows: 0≦x≦0.2 0.1≦a≦0.8, 0≦b≦0.99; typically 0≦b≦0.5, preferably 0.05 <b≦0.5、 0≦c≦0.6, 0≦d≦0.1, and a+b+c+d=1.
[0039] In a preferred embodiment, in the compound according to general formula (I) Li (1+x) [Ni a Co b Mn c M 1 d ] (1-x) O2(I)
[0040] M 1 is selected from Ca, Mg, Zr, Al, and Ba; The other variables are defined as above.
[0041] An example of a lithium nickel cobalt aluminum oxide is represented by the general formula Li[Ni h Co i Al j ]O 2+r Typical values of r, h, i, and j are: h is in the range of 0.8 to 0.90; i is in the range of 0.15 to 0.19; j is in the range of 0.01 to 0.05, and r is in the range of 0 to 0.4.
[0042] Particularly preferred is Li (1+x) [Ni 0.33 Co 0.33 Mn 0.33 ] (1-x) O2, Li (1+x)[Ni 0.5 Co 0.2 Mn 0.3 ] (1-x) O2, Li (1+x) [Ni 0.6 Co 0.2 Mn 0.2 ] (1-x) O2, Li (1+x) [Ni 0.7 Co 0.2 Mn 0.1 ] (1-x) O2, Li (1+x) [Ni 0.8 Co 0.1 Mn 0.1 ] (1-x) O2, each with x defined above, Li[Ni 0.85 Co 0.13 Al 0.02 ]O2.
[0043] The lithium-containing transition metal oxide material can have a regular shape, but usually it has an irregular shape. However, it is preferable to remove as much as possible light fractions, such as organic plastics and housing parts from aluminum or copper foil, for example, in a forced gas flow.
[0044] In one embodiment, the composition of the atmosphere is changed during step (a), which can be done, for example, if volatile organic compounds are present in the feed and are removed with an inert atmosphere before switching the atmosphere to a hydrogen-containing atmosphere.
[0045] In one embodiment, an oxidizing atmosphere in the temperature range of 20-350° C. is used in step (a) prior to reduction with a hydrogen-containing atmosphere. With this embodiment, some impurity components, i.e. organic components, may be burned off or the material dries out (particularly with temperatures up to 250° C., as further described above). The preferred oxidizing gas is oxygen or an oxygen-containing gas, e.g. air. The material originating from a spent lithium-ion battery cell, containing lithium, transition metal oxides, and also fluorine and / or phosphorus compounds, is preferably not subjected to oxidation above 350° C. when carrying out the steps of the present process.
[0046] In one embodiment, a non-oxidizing and non-reducing atmosphere in the temperature range of 20-900° C., particularly 20-450° C., is used in step (a) prior to reduction with a hydrogen-containing atmosphere, whereby volatile compounds can be removed. Preferred gases are nitrogen and inert gases such as argon or carbon dioxide.
[0047] In one embodiment of the invention, step (a) is carried out in the presence of steam at a temperature range of 100-900° C., such as the temperature range specified above for step (a). Steam may also be added to remove volatile organic compounds prior to reduction under a hydrogen-containing atmosphere.
[0048] In one embodiment of the present invention, step (a) is preferably carried out in the presence of lime, quartz, or silicate(s) or silica, or a mixture of lime and silica. The lime may be selected from hydrated lime and quick lime or burnt lime. In a preferred embodiment of the present invention, step (a) is carried out in the presence of 2 to 40% by weight of lime or quartz or silicate or silica, with reference to the lithium-containing transition metal oxide material. When using such compounds, a heat treatment may be advantageous before the reduction in a hydrogen-containing atmosphere as described above. Such a heat treatment may be carried out under any atmosphere as described above, preferably an inert gas, which may also contain steam.
[0049] Step (a) can be carried out in any type of oven that allows the introduction of hydrogen or different gases. These ovens can be operated batchwise or continuously. Preferred ovens are rotary kilns and fluidized bed reactors. These reactors can be operated continuously. Different gas compositions can be applied to successive ovens or kilns, or to successive sections of a kiln. In the latter case, the gases are introduced in such a way that no mixing of the reactive gases can occur.
[0050] After carrying out step (a), the heat-treated lithium-containing transition metal oxide material is cooled, for example, to room temperature or to a temperature somewhat higher than room temperature, for example, 25 to 90°C.
[0051] In one embodiment of the present invention, step (b) is preceded by step (b1), which includes, for example, removal of carbon or organic polymers by dry solid-solid separation. Examples of such dry solid-solid separation are electric sorting, sieving, magnetic separation, or other classification methods. Here, step (b1) is introduced as an additional step. As mentioned above, dry solid-solid separation may be sufficient to separate Ni-containing solid material from the solid residue obtained in step (a). In this case, the order of steps (b) and (c) is reversed, and the Ni-containing solid residue obtained after water treatment is directly leached to extract Ni and, if applicable, other transition metals.
[0052] Step (b) of the process of the invention comprises treating the heat-treated lithium-containing transition metal oxide material - the material obtained in step (a) or the corresponding fraction of step (b1) - with an aqueous medium capable of selectively dissolving the Li-component formed in step (a) without dissolving the transition metal contained in the heat-treated material. This treatment can be carried out at ambient temperature or above, for example in the range of 20 to 150° C. When using temperatures above the boiling point of water, the treatment is carried out at elevated pressure.
[0053] In one embodiment of the invention, the aqueous medium used contains a weak acid, such as carbonic acid, formic acid or acetic acid or sulfurous acid, obtained by dissolving carbon dioxide in water at atmospheric pressure or higher. These acids are used in a concentration of 0.1 to 10% by weight in water, preferably 1 to 10% by weight. When carbonic acid is used, it is preferably used under a carbon dioxide pressure of 10 to 150 bar. In an embodiment of particular technical interest, the aqueous medium of step (b) contains neither a weak acid, nor carbon dioxide or carbonic acid.
[0054] In one embodiment of the invention, the aqueous medium used in step (b) is water, e.g., deionized water. In one embodiment of the invention, the aqueous medium used in step (b) is aqueous formic acid.
[0055] In one embodiment of the present invention, the solid residue from step (a) or the lithium-containing transition metal material fraction obtained in step (b1) is first treated with water and then after solid-liquid separation, e.g. filtration after the water treatment, treated with dilute weak acid as described above. Both extracts may be kept separately in order to separate the different dissolved Li species.
[0056] In one embodiment of the present invention, step (b) has a duration ranging from 20 minutes to 10 hours, preferably from 1 to 3 hours.
[0057] In one embodiment, step (b) is carried out at least twice to reach an optimal recovery of lithium hydroxide or lithium salt. Between each treatment, a solid-liquid separation is carried out. The resulting lithium salt solution can be solidified or treated separately to recover the solid lithium salt. The latter may be advantageous in the case of different lithium salts of different solubilities. In this case, the first extract contains mainly the more soluble lithium salt, while the subsequent extract contains a lower concentration of the less soluble salt.
[0058] In one embodiment of the present invention, the ratio of aqueous medium to the material obtained in step (a) or (b1) ranges from 1:1 to 99:1 by weight, preferably from 2:1 to 9:1.
[0059] In one embodiment of the present invention, the material obtained from step (a) or (b1) is ground before step (b) in order to deagglomerate the different solid particles from each other, if they are somehow agglomerated, for example by residual binder polymer. Such grinding is preferably carried out in a ball mill or a stirred ball mill. Grinding can be carried out under dry or wet conditions. Preferably, grinding is carried out in an aqueous medium, which is also used in the continuous step (b).
[0060] At the end of step (b), the pressure can be released, if desired. An aqueous solution containing LiOH, LiHCO3 and / or Li2CO3, or a Li salt of the acid used in step (b), is obtained.
[0061] The solid residue is contained in the aqueous solution forming a suspension. If the extraction of the Li compound(s) is carried out in two or more steps as described above, the solid residue will be contained in the slurry of the second or last step, respectively.
[0062] In a preferred embodiment of the present invention, the solid residue obtained from step (b) dispersed in the Li salt solution is recovered by a solid-liquid separation step. This can be filtration or centrifugation, or a type of settling and decantation. A flocculant, for example a polyacrylate, can be added to recover fine particles of such solid material, for example with an average diameter of 50 μm or less. The solid residue obtained in the solid-liquid separation is dispersed in water.
[0063] The solid residue dispersed in an aqueous medium, for example a Li salt solution or water as described above, is then treated according to step (c), which recovers nickel and, if applicable, Co as a nickel (and, if applicable, Co)-containing solid.
[0064] Step (c) of the present invention comprises a solid-solid separation step. In a preferred embodiment, it is a wet solid-solid separation step. This solid-solid separation step serves to separate insoluble components such as carbon and polymers, or insoluble inorganic components, e.g. metal particles or metal oxide particles, from the metal or metal oxide components of the lithium-containing transition metal oxide material. After the solid-solid separation of step (c), a solid enriched fraction is obtained, which contains the majority of Ni, and, if applicable, Co, in concentrated form. Such a solid-solid separation step can be carried out by mechanical, column or pneumatic, or hybrid flotation. In many embodiments, a collector compound is added to the slurry that renders the target components hydrophobic. Typical collector compounds for carbon and polymer particles are hydrocarbons or fatty alcohols, which are introduced in amounts of 1 g to 50 kg / t of the heat-treated lithium-containing transition metal oxide material from step (a). It is also possible to carry out the flotation process in the reverse sense, i.e. by converting originally hydrophilic components into strongly hydrophobic components by means of special collector substances, e.g. fatty alcohol sulfates or ester quats. Preferred is the direct flotation method using a hydrocarbon collector, e.g., mineral oil, kerosene, or diesel. To improve the selectivity of the flotation method for carbon and polymer particles, inhibitors can be added that reduce the amount of entrained metal and metal oxide components in the foam phase. Agents that can be used can be acids or bases to control the pH value in the range of 3 to 9. It can also be ionic components, e.g., sodium silicate, that adsorb to metal or metal oxide surfaces, or bipolar components, e.g., amino acids. To increase the efficiency of flotation, it can be advantageous to add carrier particles that form aggregates with hydrophobic target particles, e.g., polymer particles, carbonaceous particles, e.g., graphite or coal. By using magnetic carrier particles, magnetic aggregates can be formed that can be magnetically separated. If the target components are paramagnetic, ferrimagnetic, or ferromagnetic, it is also possible to separate these components by magnetic separation using high-intensity magnetic separators ("WHIMS"), medium-intensity magnetic separators ("MIMS"), or low-intensity magnetic separators ("LIMS"). Other solid-solid separation techniques exploit the density differences of the solid constituents, for example the density differences between graphite and metals or metal oxides.These techniques include the float-sink method, which uses a fluid of intermediate density relative to the density of the solid components to be separated. Another technique of this type is heavy liquid separation. Further separation techniques based on density differences are spiral and hydrocyclone.
[0065] Also, a combination of at least two of the aforementioned solid-solid separation techniques may be used.
[0066] In one preferred embodiment, the solid-solid separation in step (c) is magnetic separation.
[0067] In one embodiment of the present invention, the material obtained from step (b) is ground prior to step (c) to free different solid particles from one another, for example if they have been somehow agglomerated by residual binder polymers. Such grinding is preferably carried out in a ball mill or stirred ball mill.
[0068] In one embodiment of the present invention, step (c) is a wet solid-solid separation using an aqueous medium, preferably water, as the fluid. The ratio of the fluid medium to the solid material obtained in step (b) ranges from 1:1 to 99:1, preferably from 2:1 to 9:1 by weight.
[0069] From the wet solid-solid separation in step (c), two slurries are obtained, one containing the target transition metal containing solid material, the other containing other components such as carbonaceous materials and polymers, and also some inorganic compounds if applicable. By appropriate selection and, if necessary, combination of solid-solid separation steps, at least 60% of Ni is obtained and concentrated in one fraction. Preferably, at least 80-99% of the Ni is separated.
[0070] In one embodiment of the present invention, the liquid phase of the slurry fed to step (c) contains dissolved lithium. In this case, one or the other or both slurries resulting from the solid-solid separation of step (c) are subjected to solid-liquid separation to recover the lithium solution. The lithium solution is then further processed in step (d).
[0071] In step (d), the solution resulting from any of the preceding steps containing lithium is treated to recover the lithium as a solid material in the form of hydroxide or salt.
[0072] In one embodiment of the present invention, the Li salt or LiOH is recovered by evaporation of the water contained in the solution. It is advantageous to neutralize the residual acid by adding a stoichiometric amount of LiOH or Li2CO3 or by adding ammonia.
[0073] In one embodiment of the present invention, Li is recovered from the Li salt solution by precipitation as Li carbonate by addition of sodium or ammonium carbonate, or by dissolution of carbon dioxide, preferably by carbonic acid formed under pressure.
[0074] In a preferred embodiment of the present invention, Li is recovered as LiOH.
[0075] The resulting solid Li salt and / or LiOH can be further purified by dissolution and recrystallization as known in the art.
[0076] The solid Ni concentrate obtained from step (c) is subjected to a step (e) allowing the extraction of Ni and, if applicable, Co and - if applicable - other valuable metals such as Lithium contained in the Ni concentrate, for which extraction a smelter or an acid or ammonium carbonate can be applied.
[0077] In one embodiment of the present invention, such step (e) can be pyrometallurgical, either by smelting the solid Ni concentrate obtained in step (c) as such or as a co-feed in a smelter dedicated to Ni concentrate from mining production.
[0078] During step (e), the transition metal material is treated with a leaching agent, preferably an acid selected from sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid and citric acid, or a combination of at least two of the foregoing, for example a combination of nitric acid and hydrochloric acid. -Inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, organic acids such as methanesulfonic acid, oxalic acid, citric acid, aspartic acid, malic acid, ascorbic acid or glycine, a base such as ammonia, an aqueous solution of an amine, ammonia, ammonium carbonate or a mixture of ammonia and carbon dioxide, or - chelating agents such as EDTA or dimethylglyoxime.
[0079] In one form, the leaching agent comprises an aqueous acid, such as an inorganic or organic aqueous acid. In another form, the leaching agent comprises a base, preferably ammonia or an amine. In another form, the leaching agent comprises a complexing agent, preferably a chelating agent. In another form, the leaching agent comprises an inorganic acid, an organic acid, a base or a chelating agent.
[0080] The concentration of the leaching agent can be varied in a wide range, for example between 0.1 and 98% by weight, preferably between 10 and 80%. A preferred example of an aqueous acid is aqueous sulfuric acid, for example with a concentration in the range of 10 to 98% by weight. Preferably, the aqueous acid has a pH value in the range of -1 to 2. The amount of acid is adjusted to maintain an excess of acid with reference to the transition metal. Preferably, the pH value of the solution obtained at the end of step (e) is in the range of -0.5 to 2.5. A preferred example of a base as leaching agent is aqueous ammonia, preferably also in the presence of carbonate or sulfate ions, with a molar NH3 to metal (Ni, Co) ratio of 1:1 to 6:1, preferably 2:1 to 4:1. Suitable chelating agents, such as EDTA or dimethylglyoxime, are often applied in a molar ratio of 1:1 to 3:1.
[0081] The leaching can be carried out in the presence of an oxidizing agent. A preferred oxidizing agent is oxygen, either as a pure gas or in a mixture with an inert gas, such as nitrogen, or as air. Other oxidizing agents are oxidizing acids, such as nitric acid.
[0082] In one embodiment of the present invention, such step (e) may be carried out by dissolving the solid Ni concentrate obtained in step (c) in an acid selected from sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid and citric acid.
[0083] In one embodiment of the present invention, such step (e) may be carried out by treating the solid Ni concentrate obtained in step (c) with an aqueous solution of ammonium carbonate or ammonium bicarbonate, such aqueous solution may contain additional ammonia.
[0084] In one embodiment of the present invention, the Ni concentrate obtained from step (c) is treated in step (e) with sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid and citric acid, or a combination of at least two of the foregoing, for example a combination of nitric acid and hydrochloric acid. In the case of aqueous acids, the concentration of the acid can vary within a wide range, for example from 0.1 to 99% by weight, preferably from 10 to 96%. The amount of acid is adjusted to maintain an excess of acid. Preferably, at the end of step (e), the pH value of the resulting solution is in the range of -0.5 to 2.
[0085] A preferred example of an aqueous acid is aqueous sulfuric acid, for example having a concentration in the range of 10 to 98% by weight.
[0086] The treatment according to step (e) may be carried out at a temperature in the range of 20 to 200° C., in particular 20 to 130° C. If a temperature above 100° C. is desired, step (e) is carried out at a pressure above 1 bar. Otherwise, normal pressure is preferred. In the context of the present invention, normal pressure means 1 atmosphere or 1013 mbar. "Standard conditions" means normal pressure and 20° C.
[0087] In one embodiment of the present invention, step (e) is carried out in a container protected against strong acids, such as molybdenum and copper-rich steel alloys, nickel-based alloys, duplex stainless steel or glass-lined or enamel- or titanium-coated steel. Further examples are polymer liners and containers made from acid-resistant polymers, such as polyethylenes, such as HDPE and UHMPE, fluorinated polyethylenes, perfluoroalkoxyalkanes ("PFA"), polytetrafluoroethylene ("PTFE"), PVdF and FEP. FEP stands for fluorinated ethylene propylene polymer, which is a copolymer of tetrafluoroethylene and hexafluoropropylene.
[0088] The slurry obtained in step (e) may be stirred, agitated or milled, for example in a ball mill or an agitated ball mill, which often leads to better access of the water or acid to the particulate transition metal material.
[0089] In one embodiment of the present invention, step (e) has a duration ranging from 10 minutes to 10 hours, preferably from 1 to 3 hours. For example, the reaction mixture of step (e) is circulated at a power of at least 0.1 W / l or by pumping to achieve good mixing and avoid settling of insoluble components. Shearing can be further improved by using baffles. All these shearing devices must apply sufficient corrosion resistance and can be produced from similar materials and coatings as described for the vessel itself.
[0090] Step (e) may be carried out under an air atmosphere or air diluted with N. However, it is preferred to carry out step (e) under an inert atmosphere, for example nitrogen or a noble gas such as Ar.
[0091] The treatment according to step (e) results in dissolution of the NCM or NCA, including impurities other than metal compounds, e.g., carbon and organic polymer, derived from the cathode active material. In most embodiments, after carrying out step (e), a slurry is obtained. Residual lithium and transition metals, such as, but not limited to, nickel, cobalt, copper and, where applicable, manganese, are often in dissolved form in the leachate, e.g., in the form of their salts.
[0092] In one embodiment of the present invention, step (e) is carried out in the presence of a reducing agent. Examples of reducing agents are organic reducing agents such as methanol, ethanol, sugars, ascorbic acid, urea, bio-based materials containing starch or cellulose, and inorganic reducing agents such as hydrazine and its salts such as sulfates, and hydrogen peroxide. Preferred reducing agents for step (e) are those that do not leave impurities based on metals other than nickel, cobalt, or manganese. Preferred examples of reducing agents in step (e) are methanol and hydrogen peroxide. With the help of a reducing agent, e.g., Co 3+ Co 2+ or Mn(+IV) or Mn 3+ Mn 2+ It is possible to reduce it to
[0093] In a preferred embodiment of the invention, an excess of reducing agent is used, where applicable, with reference to the amounts of Co and Mn. When Mn is present, such an excess is advantageous.
[0094] In a preferred embodiment of the present invention, Co 3+ With reference to the amount of reducing agent, an excess of reducing agent is used.
[0095] In one embodiment of the present invention, the ratio of extraction medium, e.g., acidic solution and reducing agent, if applicable, to the Ni concentrate obtained in step (c) ranges from 1:1 to 99:1 by weight, preferably from 2:1 to 9:1.
[0096] In embodiments where a so-called oxidizing acid is used in step (e), it is preferred to add a reducing agent to remove unused oxidizing agent. Examples of oxidizing acids are nitric acid and a combination of nitric acid and hydrochloric acid. In the context of the present invention, hydrochloric acid, sulfuric acid and methanesulfonic acid are preferred examples of non-oxidizing acids.
[0097] Depending on the concentration of the acid used, the leachate obtained in step (e) may have a transition metal concentration in the range of 1-20% by weight, preferably 3-15% by weight.
[0098] In one embodiment, step (e) is carried out under an inert gas, such as nitrogen or argon.
[0099] In one embodiment of the present invention, the Ni concentrate obtained from step (c) is ground prior to step (e) in order to liberate the different solid particles from one another if they have somehow been agglomerated, for example by residual binder polymers. Such grinding is preferably carried out in a ball mill or a stirred ball mill.
[0100] Depending on the concentration and amount of aqueous acid used in step (e), the liquid phase obtained in step (e) may have a transition metal concentration ranging from 1 to 25% by weight, preferably from 6 to 15% by weight. The transition metal concentration depends on the solubility of the corresponding salt in the acid used. Preferably, step (e) is carried out such that the transition metal concentration of the major metals, such as Ni and, optionally, Co and Mn, is slightly below the solubility limit of the least soluble salt, in order to ensure a high metal concentration in solution.
[0101] An optional step that may be carried out after step (e) is the removal of undissolved solids, such as the carbonaceous material and polymers resulting from the battery housing. This may be carried out by filtration, centrifugation or settling and decantation with or without the addition of flocculants. The solid residue obtained may be washed with water and further processed to separate the carbonaceous and polymeric components, for example by the solid-solid separation methods described above.
[0102] In one embodiment of the present invention, step (e) and the removal of undissolved solids are carried out continuously in a continuous operation mode.
[0103] In the continuous step (e1), after dissolving the Ni concentrate of step (e), the pH value of said slurry or solution can be adjusted to 2.5-8, preferably 5.5-7.5, even more preferably 6-7. The pH value can be determined by conventional means, for example by potentiometric titration, and refers to the pH value of the continuous liquid phase at 20°C. The adjustment of the pH value is carried out by dilution with water, by addition of a base, or by a combination thereof. Examples of suitable bases are ammonia and alkali metal hydroxides, for example LiOH, NaOH, or KOH, in solid form, for example as pellets or preferably as an aqueous solution. A combination of at least two of the foregoing is also feasible, for example ammonia and aqueous caustic soda.
[0104] Preferably, optional step (e2) comprises the removal of a precipitate of carbonates, oxides, phosphates, hydroxides or oxyhydroxides of Al, Cu, Fe, Zr, Zn, Zn, or a combination of at least two of the above formed in optional step (e1). The precipitate may be formed during the adjustment of the pH value. The phosphate may be a stoichiometric or basic phosphate. Without wishing to be bound by any theory, the phosphate may be generated during the formation of phosphate by hydrolysis of the hexafluorophosphate formed during step (a) or its decomposition products. It is possible to remove the precipitate by filtration or with the aid of a centrifuge or by sedimentation. Preferred filters are belt filters, filter presses, suction filters and cross-flow filters. To improve the solid-liquid separation, a filter aid and / or a flocculant may be added.
[0105] In a preferred embodiment of the invention, step (e2) comprises an optional step (e3), which comprises treating the solution obtained after step (e1) or step (e2) with metallic nickel, metallic cobalt or metallic manganese, or any combination of at least two of the foregoing.
[0106] In an optional step (e3), the solution obtained after step (e2) is contacted with metallic nickel, cobalt or manganese, or a combination of at least two of the foregoing, for example in a column. In such an embodiment, it is advantageous to provide a column packed with metallic nickel, cobalt or manganese, or a combination of at least two of the foregoing, in agglomerated or granular form, for example as a fixed bed, and to allow a flow of the solution to pass through such a column.
[0107] In one embodiment of the present invention, step (e3) is carried out at normal pressure.
[0108] In one embodiment of the invention, step (e3) has a duration ranging from 30 minutes to 5 hours, the duration corresponding to the average residence time if step (e1) is carried out in a column.
[0109] In one embodiment of the present invention, step (e3) is carried out at a pH value in the range of 1 to 6, preferably at a pH of 2 to 5. The lower the pH value of step (e1), the higher the amount of metals selected from Ni, Co and Mn that dissolves under hydrogen production.
[0110] Step (e3) is particularly useful for removing traces of copper. By carrying out step (e3), no new impurities are introduced into the solution of transition metals that would require additional purification steps. Even if the metallic nickel, cobalt or manganese contain traces of copper, they will not dissolve.
[0111] Optional step (f) involves precipitation of the transition metals as mixed hydroxides or mixed carbonates, preferably as mixed hydroxides.
[0112] In a preferred embodiment of the invention, step (f) is carried out by adding ammonia or an organic amine such as dimethylamine or diethylamine, preferably ammonia, and at least one inorganic base such as lithium hydroxide, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate or potassium bicarbonate, or a combination of at least two of the foregoing. Preference is given to the addition of ammonia and sodium hydroxide.
[0113] In one embodiment of the present invention, step (f) is carried out at a temperature ranging from 10 to 85° C., preferably from 20 to 50° C. In one embodiment of the present invention, the organic amine- or ammonia-concentration ranges from 0.05 to 1 mol / l, preferably from 0.1 to 0.7 mol / l. The term "ammonia concentration" in this context includes the concentrations of ammonia and ammonium. The Ni in the mother liquor 2+ and Co 2+ Particular preference is given to amounts of ammonia in which the solubility of each is less than or equal to 1000 ppm, more preferably less than or equal to 500 ppm.
[0114] In one embodiment of the present invention, mixing is carried out during step (f) of the process of the present invention, for example using a stirrer, rotor-stator mixer, or ball mill. It is preferred to introduce a stirrer power of at least 1 W / l, preferably at least 3 W / l, more preferably at least 5 W / l, into the reaction mixture. In one embodiment of the present invention, a stirrer power of up to 25 W / l may be introduced into the reaction mixture.
[0115] Optional step (f) of the process of the present invention may be carried out in the presence or absence of one or more reducing agents. Examples of suitable reducing agents are hydrazine, primary alcohols such as, but not limited to, methanol or ethanol, as well as ascorbic acid, glucose, and alkali metal sulfites. It is preferred not to use a reducing agent in step (f). When manganese is present in a majority amount in the transition metal oxide material, for example at least 3 mole % with reference to the transition metal portion of the respective cathode active material, it is preferred to use a reducing agent, or an inert atmosphere, or both in combination.
[0116] Step (f) of the process of the invention may be carried out under an atmosphere of an inert gas such as, for example, nitrogen or argon or carbon dioxide.
[0117] In one embodiment of the present invention, step (f) is carried out at a pH value in the range of 9 to 13.5, preferably 11 to 12.5 for hydroxides and 7.5 to 8.5 for carbonates. The pH values refer to the pH values of the mother liquors measured at 23° C.
[0118] Step (f) may be carried out in a batch reactor or - preferably - continuously, for example in a continuous stirred tank reactor or in a cascade of two or more, for example two or three, continuous stirred tank reactors.
[0119] Step (f) of the process of the invention can be carried out under air, under an inert gas atmosphere, for example under a noble gas or nitrogen atmosphere, or under a reducing atmosphere. An example of a reducing gas is, for example, SO2. Preference is given to working under an inert gas atmosphere, in particular under nitrogen gas.
[0120] For purposes of further purification, the solid recovered in step (f) may be dissolved in an acid, such as hydrochloric acid or, more preferably, sulfuric acid.
[0121] By carrying out the process of the present invention, it is possible to recover the transition metals nickel and cobalt and, if applicable, manganese from cathode materials containing nickel and cobalt and, if applicable, also manganese, in a form which allows them to be very easily converted into cathode active materials. In particular, the process of the present invention allows the recovery of transition metals such as nickel and cobalt and, optionally, manganese, which contain only acceptable trace amounts of impurities such as copper, iron and zinc, e.g., less than 10 ppm copper, preferably even less, e.g., 1-5 ppm.
[0122] In one embodiment of the present invention, the solid Ni concentrate obtained in step (c) is treated with ammonium bicarbonate in aqueous solution at a concentration of 0.2-30% by weight, preferably 1-20% by weight. The slurry may be heated to a temperature of 30-150° C. Above the boiling point of the mixture, the heating is carried out under pressure. Below the boiling point, it is advantageous to apply pressure in order to maintain sufficient ammonia and carbon dioxide in the system.
[0123] The treatment with ammonium (bi)carbonate may be carried out under an inert atmosphere or in the presence of oxygen, e.g., air. The leach or solution may also contain additional ammonia and / or hydrogen peroxide.
[0124] The ammonium (bi)carbonate treatment dissolves Ni and, where applicable, Co and Cu as ammonium complexes. The concentration of the metal ammonium complexes in the leachate may range from 0.2 to 30% by weight of metal, preferably from 1 to 15% by weight. The solution obtained by this treatment is subjected to solid-liquid separation to obtain a solution containing mainly Ni and, where applicable, Co and Cu ammonium complexes, and a separated solid residue containing mainly other transition metals, where applicable, i.e. Mn and Fe.
[0125] The resulting solution can be heated and the ammonia removed by purging with carbon dioxide. With this first Ni carbonate, and with a longer treatment advantageously at a more elevated temperature, Co carbonate is also obtained as a precipitate. This allows both metals to be separated. In one embodiment of the present invention, Ni carbonate and Co carbonate are not separated from each other. The precipitated mixed Ni / Co carbonate is separated from the mother liquor and dissolved with sulphuric acid or other acid to obtain a solution of the corresponding Ni and, if applicable, Co salts. This solution may also contain small amounts of Cu salts, which may be removed by treatment with metallic Ni, Co or Mn as described above. Other impurities such as Fe or Al, which may be contained in low concentrations, may also be removed by precipitation of hydroxides or carbonates at pH values of 2.5 to 8 as described above.
[0126] Ni and Co hydroxides may co-precipitate from the purified Ni and, where applicable, Co salt solutions.
[0127] In one embodiment of the present invention, the solution is further processed to extract the Ni and Co salts separately, for example, by solvent extraction. Pure metals can be recovered from the separated Ni and Co salts via electrochemical methods known in the art.
[0128] The present invention is further illustrated by examples.
[0129] Metallic impurities and phosphorus were determined by elemental analysis using ICP-OES (Inductively Coupled Plasma-Optical Emission Spectroscopy) or ICP-MS (Inductively Coupled Plasma-Mass Spectroscopy). Total carbon was measured with a thermal conductivity detector (CMD) after combustion. Fluorine was detected with an ion-sensitive electrode (ISE) after combustion for total fluorine or after H3PO4 distillation for ionic fluorides. The phase composition of the solids was determined by powder X-ray diffraction (PXRD).
[0130] Nl: normal liter, liter under standard conditions (1 atmosphere, 20°C). Unless otherwise specified, percentages refer to % by weight. The expressions % by weight and wt% may be used interchangeably. Whenever mentioned, the terms "room temperature" and "ambient temperature" mean a temperature of about 18-25°C.
[0131] Example 1: Step (a.1) Heat treatment in the presence of H 32.8 g of spent cathode active material containing similar molar amounts of nickel, cobalt, and manganese; 17.5 g of organic carbon in the form of graphite and soot and residual electrolyte; A quantity of 60 g of mechanically treated battery scrap containing 9.7 g of additional impurities including Al (0.6 g), Cu (0.5 g), F (total: 2.2 g), Fe (0.55 g), P (0.3 g), Zn (0.04 g), Zr (0.15 g), Mg (2 mg), Ca (6 mg) was placed in a graphite crucible in a tube furnace and heated to 400 °C during 45 min under argon flow (20 Nl / h). The temperature was kept constant for 7.5 h under a flow of 10 wt% hydrogen in argon (22 Nl / h) until the hydrogen flow was stopped and the furnace was cooled to ambient temperature under argon flow. 50.1 g of heat-treated material was recovered from the crucible and showed XRD signals of Ni / Co alloy, graphite, and LiOH.
[0132] Step (b.1) Water treatment of the product obtained in step (a.1)
[0133] 5.5 g of the material obtained in step (a.1) was slurried in 53 mL of deionized water, stirred at ambient temperature for 30 min, and then filtered. The clear filtrate contained 133 mg of Li + The solution was found to contain 212 mg hydroxide anions, 93 mg carbonate ions, and 13 mg fluoride ions, corresponding to a lithium leaching efficiency of 46%, with 65% of the lithium present as LiOH.
[0134] Step (c.1) Solid-solid separation to remove Ni from the solid residue of step (b.1)
[0135] A quantity of 12 g of hydrotreated material obtained from step (a.1) was slurried in 100 ml of deionized water and dispersed with the aid of a sonotrode using a blade stirrer at 800 rpm for 10 min. The slurry was introduced into a lab-scale high-intensity wet magnetic separator series L model 4 from Eriez Magnetics Europe Ltd. Steel wool was placed between the poles of the separator in the canister. The feed slurry was pumped into the matrix within 5 min while keeping the matrix magnetized at 1 Tesla. To fully recover the non-magnetic fraction, the attached solids were rinsed with deionized water until a clear and colorless solution was obtained from the outlet. After removing the electric field, the magnetic fraction was removed from the canister by rinsing again with deionized water. Both recovered slurries were filtered and dried in an oven to obtain 9.0 g of magnetic fraction and 1.25 g of non-magnetic fraction. The non-magnetic fraction contained 86% by weight of carbon, and less than 0.2% by weight of inorganic and organic fluorine. The Ni, Co, and Mn metal content of the magnetic fraction was 52 wt%.
[0136] Step (d.1): Recovery of Li salt from the solution obtained in step (b.1)
[0137] 31.5 g of the clear filtrate obtained in step (b), containing a total of 79 mg of lithium ions, was concentrated to dryness under reduced pressure. The flask was backfilled with dry nitrogen and transferred to an argon-filled glove box. 215 mg of solid material was recovered, showing X-ray diffraction signals mainly of LiOH and traces of Li2CO3.
[0138] Step (e.1): Acid extraction of Ni and Co from the solid Ni concentrate obtained in step (c.1)
[0139] In a stirred 250 mL batch reactor, 3.0 g of material obtained as the magnetic fraction from step (c.1) was suspended in 50 g of deionized water and heated to 40° C. A mixture of 33.4 g H2SO4 (96% H2SO4) in 20.0 g deionized water was slowly added, followed by a mixture of 3.62 g H2SO4 (96% H2SO4), 1.2 g of aqueous hydrogen peroxide (30% H2O2) in 3.47 g deionized water. Slow gas evolution was observed with only slight foam formation. The resulting slurry was stirred at 60° C. for 3 hours and then cooled to ambient temperature. The resulting mixture was filtered through a glass frit and the solid residue was washed with 62.2 g of deionized water. 111.4 g of red, clear filtrate was recovered containing 535 mg Ni, 535 mg Co, 423 mg Mn, corresponding to a leaching efficiency of more than 95% for Ni, Co, and Mn, respectively.
[0140] Alternative process (e.1): Ammonia extraction of Ni and Co from the solid Ni concentrate obtained in process (c.1)
[0141] In a stirred 250 mL batch reactor, 3.0 g of material obtained as the magnetic fraction in step (c.1) is suspended in a mixture of 117 g of 25% aqueous ammonia, 20 g of ammonium carbonate, and 9 g of deionized water and heated to 60 °C with stirring. 40.1 g of aqueous hydrogen peroxide (30% H2O2) is added with stirring over a period of 5 h. The reaction is exothermic with evolution of gas. The resulting slurry is stirred at 60 °C for 3 h and then cooled to ambient temperature. The resulting mixture is filtered through a glass frit and the solid residue is washed with 60.3 g of deionized water. 204.7 g of dark, clear combined filtrate is recovered, containing 534 mg Ni, 520 mg Co, 2 mg Mn, corresponding to leaching efficiencies of 95% and 94% for Ni and Co, respectively, while the leaching efficiency of Mn is only 0.5%. Such an ammonia leaching process may be advantageous where Mn may interfere with subsequent separation steps.
[0142] Example 2: Step (a.1) Heat treatment in the presence of H A quantity of 20 g of mechanically treated battery scrap containing 55 wt. % of spent cathode active material with similar molar amounts of nickel, cobalt and manganese, 29 wt. % of organic carbon in the form of graphite and soot and residual electrolyte, and 16 wt. % of further impurities containing Al (1 wt. %), Cu (0.8 wt. %), F (total: 3.7 wt. %), Fe (0.9 wt. %), P (0.5 wt. %), Zn (0.07 wt. %), Zr (0.3 wt. %), Mg (<0.01 wt. %), Ca (0.01 wt. %) is placed in a rotary oven and heated to 400, 410, 420, 430, 450, 470, 500 ° C., respectively, for 45 min under argon flow (20 Nl / h). At each temperature, the temperature is kept constant for another 45 min under hydrogen flow (100%, 20 Nl / h). The hydrogen flow is then stopped and the furnace is allowed to cool to ambient temperature under flowing argon. The heat-treated material is recovered from the oven and shows XRD signals of Ni / Co alloy, graphite, and LiOH. The amount of Li in the heated material is measured after each heating run.
[0143] Step (b.1) Water treatment of the product obtained in step (a.1) 5 g of the material from step (a.1) is slurried in 50 mL of deionized water, stirred at ambient temperature for 30 minutes, and then filtered. The clear filtrate is found to contain lithium, hydroxide, carbonate, and fluoride in the concentrations listed below (Table 1). [Table 1]
[0144] Steps (c1), (d1) and (e1) are carried out as in Example 1.
[0145] Example 3: Step (a.1) Heat treatment in the presence of H A quantity of 20 g of mechanically treated battery scrap containing 55 wt. % of spent cathode active material with similar molar amounts of nickel, cobalt, and manganese, 29 wt. % of organic carbon in the form of graphite and soot and residual electrolyte, and 16 wt. % of further impurities containing Al (1 wt. %), Cu (0.8 wt. %), F (total: 3.7 wt. %), Fe (0.9 wt. %), P (0.5 wt. %), Zn (0.07 wt. %), Zr (0.3 wt. %), Mg (<0.01 wt. %), Ca (0.01 wt. %) is placed in a rotary oven and heated to 400 ° C. for 45 min under argon flow (20 Nl / h). The temperature is kept constant for 15, 30, 45, 60, 150, or 450 min under hydrogen flow (100%, 20 Nl / h), as described in Table 2. The hydrogen flow is then stopped and the furnace is allowed to cool to ambient temperature under flowing argon. The heat-treated material is recovered from the oven and shows XRD signals of Ni / Co alloy, graphite, and LiOH. The amount of Li in the heated material is measured after each heating run.
[0146] Step (b.1) Water treatment of the product obtained in step (a.1) Five grams of the material from step (a.1) is slurried in 50 mL of deionized water, stirred at ambient temperature for 30 minutes, and then filtered. The clear filtrate is found to contain lithium, hydroxide, carbonate, and fluoride in the concentrations listed below (Table 2). [Table 2]
[0147] Steps (c1), (d1) and (e1) are carried out as in Example 1.
[0148] Example 4 Step (a.3) Solvent treatment before heat treatment A quantity of 750 g of mechanically treated battery scrap containing 55 wt. % spent cathode active material with similar molar amounts of nickel, cobalt, and manganese, 29 wt. % organic carbon in the form of graphite and soot and residual electrolyte, and 16 wt. % further impurities containing Al (1 wt. %), Cu (0.8 wt. %), F (total: 3.7 wt. %), Fe (0.9 wt. %), P (0.5 wt. %), Zn (0.07 wt. %), Zr (0.3 wt. %), Mg (<0.01 wt. %), Ca (0.01 wt. %) was mixed with 2.5 L of water, stirred for 60 min at ambient temperature, and then filtered.
[0149] Step (a.1) Heat treatment in the presence of H
[0150] 20 g of material obtained in step (a.3) are placed in a rotating oven and heated to 400 °C for 45 min under argon flow (20 Nl / h). The temperature is kept constant for several hours under a hydrogen / argon mixture flow (20 Nl / h); the hydrogen concentration is 3, 5, 7, 10, 14, 25, 35, or 100 vol.%, respectively, as described in Table 3 below. The hydrogen flow is then stopped and the furnace is allowed to cool to ambient temperature under argon flow. The heat-treated material is recovered from the oven and shows XRD signals of Ni / Co alloy, graphite, and LiOH. The amount of Li in the heated material is measured after each heating experiment.
[0151] Step (b.1) Water treatment of the product obtained in step (a.1) Five grams of the material from step (a.1) is slurried in 50 mL of deionized water, stirred at ambient temperature for 30 minutes, and then filtered. The clear filtrate is found to contain lithium, hydroxide, carbonate, and fluoride in the concentrations listed below (Table 3). [Table 3]
[0152] Steps (c1), (d1) and (e1) are carried out as in Example 1. Aspects of the present disclosure include the following. [1] 1. A process for the recovery of transition metals from spent lithium ion batteries containing nickel, the process comprising: (a) A lithium-containing transition metal oxide material derived from a lithium-ion battery and containing fluorine compounds and / or phosphorus compounds as impurities is treated with H 2 heating to a temperature in the range of 200 to 900°C in the presence of (b) treating the product obtained in step (a) with an aqueous medium; (c) solid-solid separation to remove Ni from the solid residue of step (b); (d) recovery of Li as hydroxide or salt from the solution obtained in step (b); (e) extraction of Ni and, where applicable, Co from the solid Ni concentrate obtained in step (c). [2] 1. A process for the recovery of transition metals from spent lithium ion batteries containing nickel, the process comprising: (a) heating a lithium-containing transition metal oxide material in the presence of H2 to a temperature in the range of 200 to 900°C; (b) treating the product obtained in step (a) with an aqueous medium; (c) solid-solid separation to remove Ni from the solid residue of step (b); (d) recovery of Li as hydroxide or salt from the solution obtained in step (b); (e) extraction of Ni and, where applicable, Co from the solid Ni concentrate obtained in step (c), The process, wherein the lithium-containing transition metal oxide material heated in step (a) originates from a lithium ion battery and contains fluorine in the range of 2 wt% to 8 wt% and / or phosphorus in the range of 0.2 wt% to 2 wt% compared to the weight of the lithium-containing transition metal oxide material. [3] 3. The process of claim 1 or 2, wherein the heating temperature in step (a) is in the range of 350-500°C, and preferably 35% by volume or more of hydrogen is present in step (a), and the heating temperature in step (a) is in the range of 350-450°C. [4] 4. The process of claim 1 or 2 or 3, wherein the lithium-containing transition metal oxide material used in step (a) is obtained from a lithium ion battery after mechanical removal of a casing, wiring, or circuitry and discharging, and the material is not exposed to a temperature of 400° C. or greater under oxidizing conditions prior to being subjected to step (a). [5] Step (e) is - smelting the solid Ni concentrate obtained in step (c); - treatment of the solid Ni concentrate obtained in step (c) with an acid selected from sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid, and citric acid, or a combination of at least two of the foregoing; - treatment of the Ni concentrate obtained in step (c) with ammonium (bi)carbonate; The process according to any one of aspects 1 to 4, comprising one or more of the steps, preferably one of the steps described above. [6] The process of any of aspects 1-4, wherein step (e) comprises treating the Ni concentrate obtained in step (c) with a base, such as ammonia, an aqueous solution of an amine, ammonia, ammonium carbonate, or a mixture of ammonia and carbon dioxide. [7] The process according to any of aspects 5 and 6, wherein the solution containing Ni and, where applicable, Co salts is treated with ammonia or an alkali metal hydroxide to obtain a solution having a pH value in the range of 2.5 to 8. [8] The process according to any of embodiments 5 and 6, wherein the solution containing Ni and, where applicable, Co salts is treated with metallic nickel, metallic cobalt, or metallic manganese, or any combination of at least two of the foregoing. [9] The process of any of the preceding embodiments, wherein prior to step (b), the carbon or organic polymer is removed by dry-solid separation.
[10] The process of any of the preceding aspects, comprising in step (d) recovering lithium as lithium hydroxide.
[11] The process of any of the preceding aspects, comprising in step (d) recovering lithium as a carbonate salt by precipitation.
[12] 12. The process according to any of the preceding aspects, comprising an additional step (f) of precipitating nickel and, where applicable, cobalt and / or manganese as (mixed) hydroxides, oxyhydroxides or carbonates, e.g. by raising the pH value to a value above 8, wherein step (f) is preferably carried out by addition of at least one agent selected from the group consisting of lithium hydroxide, sodium hydroxide, ammonia and potassium hydroxide.
[13] 13. The process according to any of the preceding aspects, wherein step (a) is carried out in the presence of steam.
[14] The process according to any of the preceding aspects, wherein step (a) is carried out in the presence of lime, quartz, silica, or a silicate.
[15] The process according to any of the preceding aspects, comprising an additional step prior to step (a), said additional step comprising contacting material from spent lithium ion batteries with water and / or an organic solvent, followed by a solid-liquid separation step.
Claims
1. 1. A process for the recovery of transition metals from spent lithium ion batteries containing nickel and optionally cobalt, said process comprising: (a) A lithium-containing transition metal oxide material derived from a lithium ion battery and containing a fluorine compound and / or a phosphorus compound as an impurity is dissolved in 0.1 to 100% by volume of H 2 heating to a temperature in the range of 200 to 900° C. in a reducing atmosphere containing (b) treating the product obtained in step (a) with an aqueous medium; (c) solid-solid separation to remove Ni from the solid residue of step (b); (d) recovery of Li as hydroxide or salt from the solution obtained in step (b); (e) extraction of Ni and, if the used lithium ion battery contains Co, Co from the solid Ni concentrate obtained in step (c), The process, wherein the lithium-containing transition metal oxide material used in step (a) is obtained from a lithium ion battery after mechanically removing the casing, wiring, or circuitry and discharging, and the lithium-containing transition metal oxide material is not exposed to a temperature of 400° C. or higher under oxidizing conditions before being subjected to step (a).
2. The process of claim 1, wherein the lithium-containing transition metal oxide material heated in step (a) contains fluorine in the range of 2 wt. % to 8 wt. % and / or phosphorus in the range of 0.2 wt. % to 2 wt. % relative to the weight of the lithium-containing transition metal oxide material.
3. 3. The process of claim 1 or 2, wherein the heating temperature in step (a) is in the range of 350 to 500°C, preferably 35% by volume or more of hydrogen is present in step (a) and the heating temperature in step (a) is in the range of 350 to 450°C.
4. Step (e) is - smelting of the solid Ni concentrate obtained in step (c); - treatment of the solid Ni concentrate obtained in step (c) with an acid selected from sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid and citric acid, or a combination of at least two of the foregoing; - treatment of the Ni concentrate obtained in step (c) with ammonium (bi)carbonate; A process according to any one of claims 1 to 3, comprising one or more of the steps, preferably one of the steps mentioned above.
5. The process according to any of claims 1 to 3, wherein step (e) comprises treating the Ni concentrate obtained in step (c) with a base (e.g., ammonia, an aqueous solution of an amine, ammonia, ammonium carbonate, or a mixture of ammonia and carbon dioxide).
6. 6. The process according to claim 4 or 5, wherein a solution containing Ni and, if the used lithium ion battery contains Co, a Co salt is treated with ammonia or an alkali metal hydroxide to obtain a solution having a pH value in the range of 2.5 to 8.
7. 6. The process of claim 4, wherein a solution containing Ni and, if the used lithium ion batteries contain Co, a Co salt is treated with metallic nickel, metallic cobalt, or metallic manganese, or any combination of at least two of the foregoing.
8. The process according to any one of claims 1 to 7, wherein prior to step (b), carbon or organic polymers are removed by dry-solid separation techniques.
9. 9. The process of any one of claims 1 to 8, comprising in step (d) recovering lithium as lithium hydroxide.
10. 10. The process of any one of claims 1 to 9, comprising in step (d) recovering lithium as the carbonate by precipitation.
11. 11. The process according to any of the preceding claims, comprising an additional step (f) of precipitating nickel and, if the used lithium ion battery contains cobalt and / or manganese, cobalt and / or manganese as (mixed) hydroxides, oxyhydroxides or carbonates, for example by raising the pH value to a value above 8, step (f) being preferably carried out by addition of at least one agent selected from the group consisting of lithium hydroxide, sodium hydroxide, ammonia and potassium hydroxide.
12. The process of any one of claims 1 to 11, wherein step (a) is carried out in the presence of steam.
13. The process according to any one of claims 1 to 12, wherein step (a) is carried out in the presence of lime, quartz, silica, or a silicate.
14. 14. The process according to any one of claims 1 to 13, comprising an additional step prior to step (a), said additional step comprising contacting the lithium-containing transition metal oxide material from a spent lithium ion battery with water and / or an organic solvent, followed by a solid-liquid separation step.
Citation Information
Patent Citations
Processing method and recycling method of lithium battery
JP2005026088A
Recycling method and processing unit of battery pack
JP2012204000A