Resin sheet and method for producing same

By mixing and pressurizing lumpy boron nitride particles with specific properties, the resin sheet addresses the need for higher thermal conductivity in electronic components, enhancing heat dissipation through optimized particle arrangement and gap filling.

JP7577687B2Active Publication Date: 2024-11-05DENKA CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021565552
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-17
Filing Date
2020-12-11
Publication Date
2024-11-05
Estimated Expiration
2040-12-11

AI Technical Summary

Technical Problem

The increasing density and speed of circuits in electronic components demand resin sheets with higher thermal conductivity to efficiently dissipate heat.

Method used

A resin sheet is produced by mixing lumpy boron nitride particles formed by agglomerating scale-like primary particles, with specific size and strength ratios, and pressurizing the mixture to create a sheet that enhances thermal conductivity.

Benefits of technology

The resin sheet achieves improved thermal conductivity by forming effective heat conduction paths and filling gaps with deagglomerated boron nitride particles, outperforming conventional sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577687000003
    Figure 0007577687000003
  • Figure 0007577687000004
    Figure 0007577687000004
  • Figure 0007577687000001
    Figure 0007577687000001
Patent Text Reader

Abstract

One aspect of the present invention resides in a resin sheet manufacturing method comprising: a step of mixing lumpy boron nitride particles A formed by aggregation of scaly boron nitride primary particles a, lumpy boron nitride particles B formed by aggregation of scaly boron nitride primary particles b, and a resin to obtain a resin composition; and a step of molding the resin composition into a sheet and pressurizing the resin composition molded into a sheet, wherein the length of the boron nitride primary particles a in the lateral direction is 0.7 μm or less, the length of the boron nitride primary particles b in the lateral direction is 1 μm or more, the average particle diameter of the lumpy boron nitride particles A is 30 μm or more, the average particle size of the lumpy boron nitride particles B is smaller than the average particle size of the lumpy boron nitride particles A, and the ratio of the crushing strength of the lumpy boron nitride particles A to the crushing strength of the lumpy boron nitride particles B is 1.2 or more. According to the present invention, the thermal conductivity of the resin sheet can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin sheet and a method for producing the same. [Background technology]

[0002] In electronic components such as power devices, transistors, thyristors, and CPUs, the efficient dissipation of heat generated during use is an issue. To address this issue, conventional approaches have been to increase the thermal conductivity of the insulating layer of the printed wiring board on which the electronic components are mounted, or to attach the electronic components or printed wiring board to a heat sink via an electrically insulating thermal interface material. As such an insulating layer and thermal interface material, for example, a resin sheet (thermal conductive sheet) containing a resin and a thermally conductive filler is used.

[0003] As a thermally conductive filler, boron nitride particles have attracted attention because of their properties of high thermal conductivity, high insulation, low dielectric constant, etc. For example, Patent Document 1 discloses a thermally conductive sheet that contains a fluororesin and a thermally conductive filler containing boron nitride particles, and has a thermal resistance value of 0.90° C. / W or less under a pressure of 0.05 MPa. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-203857 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, the importance of heat dissipation has increased with the increasing speed and integration of circuits in electronic components and the increasing mounting density of electronic components on printed wiring boards, and therefore there is a demand for resin sheets with higher thermal conductivity than ever before.

[0006] Therefore, an object of the present invention is to improve the thermal conductivity of a resin sheet. [Means for solving the problem]

[0007] One aspect of the present invention is a method for producing a resin sheet, comprising the steps of: mixing aggregate boron nitride particles A formed by agglomeration of scaly boron nitride primary particles a, aggregate boron nitride particles B formed by agglomeration of scaly boron nitride primary particles b, and a resin to obtain a resin composition; forming the resin composition into a sheet; and pressurizing the resin composition formed into a sheet, wherein the length in the lateral direction of the boron nitride primary particles a is 0.7 μm or less, the length in the lateral direction of the boron nitride primary particles b is 1 μm or more, the average particle size of the aggregate boron nitride particles A is 30 μm or more, the average particle size of the aggregate boron nitride particles B is smaller than the average particle size of the aggregate boron nitride particles A, and the ratio of the crushing strength of the aggregate boron nitride particles A to the crushing strength of the aggregate boron nitride particles B is 1.2 or more.

[0008] In the above aspect, the ratio of the average particle size of the aggregate boron nitride particles B to the average particle size of the aggregate boron nitride particles A may be 0.7 or less. The content of the aggregate boron nitride particles A in the resin composition may be 50 parts by volume or more per 100 parts by volume of the total amount of the aggregate boron nitride particles A and the aggregate boron nitride particles B. The content of the aggregate boron nitride particles B in the resin composition may be 5 parts by volume or more per 100 parts by volume of the total amount of the aggregate boron nitride particles A and the aggregate boron nitride particles B.

[0009] Another aspect of the present invention is a resin sheet containing a resin, aggregate boron nitride particles A formed by aggregation of flaky boron nitride primary particles a, and flaky boron nitride primary particles b which do not form aggregate boron nitride particles and are arranged in the gaps between the aggregate boron nitride particles A, wherein the length of the lateral direction of the boron nitride primary particles a is 0.7 μm or less, the length of the lateral direction of the boron nitride primary particles b is 1 μm or more, and the average particle size of the aggregate boron nitride particles A is 30 μm or more.

[0010] In another aspect of the above, the content of the aggregate boron nitride particles A may be 50 parts by volume or more per 100 parts by volume of the total amount of the aggregate boron nitride particles A and the boron nitride primary particles b. The content of the boron nitride primary particles b may be 5 parts by volume or more per 100 parts by volume of the total amount of the aggregate boron nitride particles A and the boron nitride primary particles b.

[0011] In each of the above aspects, the resin sheet may be used as a heat dissipation sheet. Effect of the Invention

[0012] According to the present invention, the thermal conductivity of the resin sheet can be improved. [Brief description of the drawings]

[0013] [Figure 1] 1 is an SEM image of a cross section of the resin sheet obtained in Example 1. [Diagram 2] 2 is an SEM image of a cross section of the resin sheet obtained in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail.

[0015] One embodiment of the present invention is a method for producing a resin sheet, comprising a step (mixing step) of mixing aggregate boron nitride particles A, aggregate boron nitride particles B, and a resin to obtain a resin composition, and a step (molding step) of forming the resin composition into a sheet and pressurizing the resin composition formed into a sheet.

[0016] First, the mixing step will be described. The aggregate boron nitride particles A are particles formed by agglomeration of scaly boron nitride primary particles a. The length in the short side direction of the boron nitride primary particles a is 0.7 μm or less. If the length in the short side direction of the boron nitride primary particles a is greater than 0.7 μm, the number of voids in the aggregate boron nitride particles A increases, and the thermal conductivity of the resin sheet may decrease. In addition, the crushing strength of the aggregate boron nitride particles A may decrease. The aggregate boron nitride particles B are particles formed by agglomeration of scaly boron nitride primary particles b. The length in the short side direction of the boron nitride primary particles b is 1 μm or more. If the length in the short side direction of the boron nitride primary particles b is less than 1 μm, the crushing strength of the aggregate boron nitride particles B becomes high, and it may be difficult to set the ratio of the crushing strength of the aggregate boron nitride particles A to the crushing strength of the aggregate boron nitride particles B to 1.2 or more. In this manner, the aggregate boron nitride particles A and the aggregate boron nitride particles B are different particles from each other.

[0017] The short-side length of the scaly boron nitride primary particles a and b can also be referred to as the thickness of the scaly primary particles. The short-side length of the boron nitride primary particles a and b is measured as the average short-side length of 50 primary particles in an SEM image of the primary particles. The longitudinal length of the boron nitride primary particles a and b described later is also measured in the same manner.

[0018] From the viewpoint of the voids in the aggregate boron nitride particles A and the crushing strength of the aggregate boron nitride particles A, the length in the short side direction of the boron nitride primary particles a is preferably 0.65 μm or less, more preferably 0.60 μm or less. The lower limit of the range of the length in the short side direction of the boron nitride primary particles a is not particularly limited, but is, for example, 0.3 μm or more, preferably 0.4 μm or more, and more preferably 0.5 μm or more. The length in the longitudinal direction of the boron nitride primary particles a is not particularly limited, but may be, for example, 1 μm or more and 10 μm or less.

[0019] From the viewpoint of the crushing strength of the aggregate boron nitride particles B, the length of the boron nitride primary particles b in the short side direction is preferably 1.1 μm or more, more preferably 1.2 μm or more, and even more preferably 1.3 μm or more. The upper limit of the range of the length of the boron nitride primary particles b in the short side direction is not particularly limited, but is, for example, 2 μm or less, preferably 1.8 μm or less, and even more preferably 1.6 μm or less. The length of the boron nitride primary particles b in the longitudinal direction is not particularly limited, but may be, for example, 2.5 μm or more and 15 μm or less.

[0020] The average particle size of the aggregate boron nitride particles A is 30 μm or more from the viewpoint of reducing the number of interfaces between the aggregate boron nitride particles in the resin sheet and improving the thermal conductivity of the resin sheet, and from the viewpoint of making the effect more easily obtainable, it is preferably 40 μm or more, more preferably 50 μm or more, even more preferably 60 μm or more, and particularly preferably 70 μm or more. The average particle size of the aggregate boron nitride particles A may be, for example, 150 μm or less, 120 μm or less, or 100 μm or less.

[0021] The average particle size of the aggregate boron nitride particles B is smaller than the average particle size of the aggregate boron nitride particles A. This allows the aggregate boron nitride particles B to enter the gaps between the aggregate boron nitride particles A, further increasing the filling rate of boron nitride in the resin sheet, and further improving the thermal conductivity of the resin sheet. Specifically, the ratio of the average particle size of the aggregate boron nitride particles B to the average particle size of the aggregate boron nitride particles A (average particle size of aggregate boron nitride particles B / average particle size of aggregate boron nitride particles A) is preferably 0.7 or less, more preferably 0.65 or less, even more preferably 0.6 or less, and particularly preferably 0.5 or less, from the viewpoint of further improving the thermal conductivity of the resin sheet. The lower limit of the ratio of the average particle size is not particularly limited, and may be, for example, 0.1 or more, 0.2 or more, or 0.25 or more. The average particle size of the aggregate boron nitride particles A and B means the volume average particle size measured by a laser diffraction scattering method.

[0022] The average particle size of the chunk boron nitride particles B is preferably selected so as to satisfy the above average particle size ratio. The average particle size of the chunk boron nitride particles B is, for example, 50 μm or less, and from the viewpoint of further improving the thermal conductivity of the resin sheet, is preferably 40 μm or less, more preferably 30 μm or less. The lower limit of the range of the average particle size of the chunk boron nitride particles B is not particularly limited, but may be, for example, 10 μm or more, 15 μm or more, or 20 μm or more.

[0023] The crushing strength of the aggregate boron nitride particles A is greater than the crushing strength of the aggregate boron nitride particles B. This makes it possible to apply pressure to the resin composition in a molding step described below so as to maintain the agglomeration of the boron nitride primary particles a in the aggregate boron nitride particles A while detaching only the agglomeration of the boron nitride primary particles b in the aggregate boron nitride particles B. Then, the voids between the aggregate boron nitride particles A can be filled with the boron nitride primary particles b generated by the detachment of the agglomeration of the aggregate boron nitride particles B. Specifically, the ratio of the crushing strength of aggregate boron nitride particles A to the crushing strength of aggregate boron nitride particles B (crushing strength of aggregate boron nitride particles A / crushing strength of aggregate boron nitride particles B) is not particularly limited as long as it can suitably break down only the agglomeration of boron nitride primary particles b in aggregate boron nitride particles B while maintaining the agglomeration of boron nitride primary particles a in aggregate boron nitride particles A in the molding step described below, but for example, from the viewpoint of further improving the thermal conductivity of the resin sheet, it is 1.2 or more, and from the viewpoint of further easily obtaining this effect, it is preferably 1.3 or more, more preferably 1.4 or more, even more preferably 1.5 or more, and particularly preferably 1.6 or more. The upper limit of the range of the crushing strength ratio is not particularly limited, but it may be, for example, 4 or less, 3 or less, or 2 or less.

[0024] The crushing strength of the aggregate boron nitride particles A and B is a value measured in accordance with JIS R1639-5:2007. A microcompression tester (for example, product name "MCT-W500" manufactured by Shimadzu Corporation) can be used as a measuring device. The crushing strength (σ, unit: MPa) is calculated from a dimensionless number (α=2.48, unitless) that changes depending on the position within the particle, the crushing test force (P, unit: N), and the particle size (d, unit: μm) as follows: σ=α×P / (π×d 2 ) is calculated using the formula:

[0025] The crushing strength of the aggregate boron nitride particles A is preferably selected so as to satisfy the above crushing strength ratio. The crushing strength of the aggregate boron nitride particles A is, for example, 4 MPa or more, and from the viewpoint of more suitably maintaining the aggregation of the boron nitride primary particles a in the aggregate boron nitride particles A in the molding step described below, is preferably 5 MPa or more, more preferably 6 MPa or more. The upper limit of the range of the crushing strength of the aggregate boron nitride particles A is not particularly limited, and may be, for example, 15 MPa or less, 12 MPa or less, or 10 MPa or less.

[0026] The crushing strength of the aggregate boron nitride particles B is also preferably selected so as to satisfy the above crushing strength ratio. The crushing strength of the aggregate boron nitride particles B is, for example, 8 MPa or less, and from the viewpoint of more suitably deflocculating the agglomeration of the boron nitride primary particles b in the aggregate boron nitride particles B in the molding step described below, is preferably 7 MPa or less, more preferably 6 MPa or less. The crushing strength of the aggregate boron nitride particles B is not particularly limited as long as the agglomeration of the aggregate boron nitride particles B is not deflocculated in the mixing step described below, but may be, for example, 2 MPa or more, 3 MPa or more, or 4 MPa or more.

[0027] The content of the aggregate boron nitride particles A in the resin composition is, for example, 25% by volume or more, preferably 30% by volume or more, more preferably 35% by volume or more, based on the total volume of the resin composition, from the viewpoint of improving the thermal conductivity of the resin sheet. Also, the content of the aggregate boron nitride particles A in the resin composition is, for example, 60% by volume or less, preferably 57.5% by volume or less, more preferably 55% by volume or less, from the viewpoint of preventing the generation of voids in the resin sheet.

[0028] The content of aggregate boron nitride particles A in the resin composition, relative to 100 parts by volume of the total amount of aggregate boron nitride particles A and aggregate boron nitride particles B, is, for example, from the viewpoint of further increasing the filling rate of boron nitride in the resin sheet and further improving the thermal conductivity of the resin sheet, preferably 50 parts by volume or more, more preferably 55 parts by volume or more, even more preferably 60 parts by volume or more, and is preferably 95 parts by volume or less, more preferably 90 parts by volume or less, even more preferably 85 parts by volume or less, and particularly preferably 70 parts by volume or less.

[0029] From the viewpoint of further increasing the filling rate of boron nitride in the resin sheet and further improving the thermal conductivity of the resin sheet, the content of the aggregate boron nitride particles B in the resin composition is, for example, 5 vol% or more, preferably 10 vol% or more, and more preferably 15 vol% or more, based on the total volume of the resin composition, and for example, 25 vol% or less, preferably 22.5 vol% or less, and more preferably 20 vol% or less.

[0030] The content of aggregate boron nitride particles B in the resin composition, relative to 100 parts by volume of the total amount of aggregate boron nitride particles A and aggregate boron nitride particles B, is, for example, from the viewpoint of further increasing the filling rate of boron nitride in the resin sheet and further improving the thermal conductivity of the resin sheet, preferably 5 parts by volume or more, more preferably 10 parts by volume or more, even more preferably 15 parts by volume or more, particularly preferably 30 parts by volume or more, and is preferably 50 parts by volume or less, more preferably 45 parts by volume or less, and even more preferably 40 parts by volume or less.

[0031] Examples of resins include epoxy resins, silicone resins, silicone rubber, acrylic resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyimides, polyamideimides, polyetherimides, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS (acrylonitrile-butadiene-styrene) resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins.

[0032] The resin content in the resin composition is, based on the total volume of the resin composition, for example, 40 volume % or more, preferably 42.5 volume % or more, and more preferably 45 volume % or more, from the viewpoint of improving the thermal conductivity of the resin sheet, and for example, 60 volume % or less, preferably 57.5 volume % or less, and more preferably 55 volume % or less, from the viewpoint of preventing the occurrence of voids in the resin sheet.

[0033] In the mixing step, in addition to the aggregate boron nitride particles A, aggregate boron nitride particles B, and resin, other components may be further mixed. The other components may be, for example, a curing agent. The curing agent is appropriately selected depending on the type of resin. For example, when the resin is an epoxy resin, the curing agent may be a phenol novolac compound, an acid anhydride, an amino compound, or an imidazole compound. The content of the curing agent may be, for example, 0.5 parts by mass or more, 1 part by mass or more, 5 parts by mass or more, or 8 parts by mass or more, and 15 parts by mass or less, 12 parts by mass or less, or 10 parts by mass or less, relative to 100 parts by mass of the resin.

[0034] The molding step following the mixing step includes, for example, a step of coating the resin composition obtained in the mixing step (coating step) and a step of pressurizing the coated resin composition (pressurizing step), thereby obtaining a resin composition molded into a sheet shape (resin sheet).

[0035] In the coating step, the resin composition is coated on a substrate (e.g., a polymer film such as a PET film) using, for example, a film applicator. The thickness of the coated resin composition may be, for example, 0.05 mm or more, 0.1 mm or more, or 0.5 mm or more, and may be 2 mm or less, 1.5 mm or less, or 1.2 mm or less. In the coating step, after the resin composition is coated on the substrate, the resin composition may be degassed, for example, under reduced pressure.

[0036] In the pressurizing step, pressure is applied to the resin composition. The pressure is appropriately selected according to the crushing strength of each of the aggregate boron nitride particles A and B so as to maintain the aggregation of the boron nitride primary particles a in the aggregate boron nitride particles A while breaking down only the aggregation of the boron nitride primary particles b in the aggregate boron nitride particles B. The pressure may be, for example, 2 MPa or more, 3 MPa or more, or 4 MPa or more, and may be 15 MPa or less, 14 MPa or less, or 13 MPa or less.

[0037] In the pressurizing step, the resin composition may be heated at the same time as the pressurizing. The heating temperature may be, for example, 100° C. or higher, 120° C. or higher, or 150° C. or higher, and 250° C. or lower, 230° C. or lower, or 200° C. or lower. This allows, for example, the resin composition (resin) to be semi-cured or completely cured.

[0038] The time for applying pressure (and heating as necessary) in the pressure step may be, for example, 10 minutes or more, 30 minutes or more, or 50 minutes or more, and may be 6 hours or less, 4 hours or less, or 2 hours or less.

[0039] In the above-described method for producing a resin sheet, as described above, aggregate boron nitride particles A and aggregate boron nitride particles B which are different from each other in terms of average particle size and crushing strength are used, and aggregate boron nitride particles A have a larger average particle size and crushing strength than aggregate boron nitride particles B. Therefore, when the resin composition is molded into a sheet in the molding step and the resin composition molded into a sheet is pressed, it is possible to maintain the aggregation of the boron nitride primary particles a in the aggregate boron nitride particles A which have a large crushing strength, while untangling the aggregation of the boron nitride primary particles b in the aggregate boron nitride particles B which have a small crushing strength. At this time, since the boron nitride primary particles a have a lateral length of 0.7 μm or less, the number of bonding sites between the boron nitride primary particles a increases, making it easier to maintain the aggregation of the boron nitride primary particles a. As a result, in the resin sheet obtained, aggregated boron nitride particles A, which have a large average particle size and are easy to form paths for heat conduction (easy to contribute to improving thermal conductivity), are present, and disaggregated boron nitride primary particles b can be present in the gaps between the aggregated boron nitride particles A, which are difficult to conduct heat in conventional resin sheets. In this case, the boron nitride primary particles b have a short-side length of 1 μm or more, and therefore are easy to contribute to improving the thermal conductivity of the resin sheet. Therefore, the resin sheet obtained by this manufacturing method exhibits excellent thermal conductivity because heat can be conducted effectively throughout the resin sheet, compared to, for example, conventional resin sheets in which only aggregated boron nitride particles are present in the resin.

[0040] In addition, since the aggregated boron nitride particles B are not deaggregated before the pressurizing step, it is easy to arrange the aggregated boron nitride particles B at positions corresponding to the gaps between the aggregated boron nitride particles A. Then, the aggregated boron nitride particles B arranged at positions corresponding to the gaps between the aggregated boron nitride particles A are deaggregated by the pressurizing step, so that the gaps between the aggregated boron nitride particles A can be sufficiently filled with the boron nitride primary particles b. This can further improve the thermal conductivity of the resin sheet. On the other hand, if non-aggregated boron nitride primary particles b are used instead of the aggregated boron nitride particles B, the moldability of the resin composition may be deteriorated or it may be difficult to disperse the boron nitride primary particles b in the resin sheet. For this reason, the filling of the gaps between the aggregated boron nitride particles A with the boron nitride primary particles b may be insufficient, and the thermal conductivity of the resin sheet may not be improved.

[0041] Another embodiment of the present invention is a resin sheet containing a resin, aggregate boron nitride particles A formed by aggregation of flaky boron nitride primary particles a, and flaky boron nitride primary particles b which do not form aggregate boron nitride particles and are disposed in the gaps between the aggregate boron nitride particles A.

[0042] The details of the resin are as described above. The resin in the resin sheet may be in a semi-cured state (also called B stage). The semi-cured state of the resin can be confirmed, for example, by a differential scanning calorimeter. The resin sheet can be further subjected to a curing process to become fully cured (also called C stage).

[0043] In order to prevent the occurrence of voids in the resin sheet, the resin content in the resin sheet is, based on the total volume of the resin sheet, for example, 40 volume% or more, preferably 42.5 volume% or more, and more preferably 45 volume% or more, and for example, 60 volume% or less, preferably 57.5 volume% or less, and more preferably 55 volume% or less.

[0044] Details of the boron nitride primary particles a, the aggregate boron nitride particles A, and the boron nitride primary particles b are as described above.

[0045] The content of the aggregate boron nitride particles A in the resin sheet is, for example, 25% by volume or more, preferably 30% by volume or more, more preferably 35% by volume or more, based on the total volume of the resin sheet, from the viewpoint of improving the thermal conductivity of the resin sheet. Also, the content of the aggregate boron nitride particles A in the resin sheet is, for example, 60% by volume or less, preferably 57.5% by volume or less, more preferably 55% by volume or less, from the viewpoint of preventing the generation of voids in the resin sheet.

[0046] From the viewpoint of further increasing the filling rate of boron nitride in the resin sheet and further improving the thermal conductivity of the resin sheet, the content of the boron nitride primary particles b in the resin sheet is, for example, 5 volume% or more, preferably 10 volume% or more, and more preferably 15 volume% or more, based on the total volume of the resin sheet, and for example, 25 volume% or less, preferably 22.5 volume% or less, and more preferably 20 volume% or less.

[0047] The content of the aggregate boron nitride particles A in the resin sheet, relative to 100 parts by volume of the total amount of the aggregate boron nitride particles A and the boron nitride primary particles b, is, for example, from the viewpoint of further increasing the filling rate of boron nitride in the resin sheet and further improving the thermal conductivity of the resin sheet, preferably 50 parts by volume or more, more preferably 55 parts by volume or more, even more preferably 60 parts by volume or more, and is preferably 95 parts by volume or less, more preferably 90 parts by volume or less, even more preferably 85 parts by volume or less, and particularly preferably 70 parts by volume or less.

[0048] The content of the boron nitride primary particles b in the resin sheet, relative to 100 parts by volume of the total amount of the boron nitride primary particles A and the boron nitride primary particles b, is, for example, from the viewpoint of further increasing the filling rate of boron nitride in the resin sheet and further improving the thermal conductivity of the resin sheet, preferably 5 parts by volume or more, more preferably 10 parts by volume or more, even more preferably 15 parts by volume or more, particularly preferably 30 parts by volume or more, and is preferably 50 parts by volume or less, more preferably 45 parts by volume or less, and even more preferably 40 parts by volume or less.

[0049] The thickness of the resin sheet is, for example, preferably 0.05 mm or more, more preferably 0.1 mm or more, and even more preferably 0.3 mm or more from the viewpoint of the adhesion of the resin sheet, and is preferably 1.5 mm or less, more preferably 1 mm or less, and even more preferably 0.7 mm or less from the viewpoint of the thermal conductivity of the resin sheet.

[0050] As described above, the resin sheet contains aggregated boron nitride primary particles a (aggregated boron nitride particles A), but some of the boron nitride primary particles a in the resin sheet may not form aggregated boron nitride particles (may not be aggregated). The boron nitride primary particles a that do not form aggregated boron nitride particles also fill the gaps between the aggregated boron nitride particles A. From the viewpoint of further increasing the filling rate of boron nitride in the resin sheet and further improving the thermal conductivity of the resin sheet, the content of the boron nitride primary particles a that do not form aggregated boron nitride particles (not aggregated) in the resin sheet is, for example, 1 vol% or more, preferably 3 vol% or more, more preferably 5 vol% or more, based on the total volume of the resin sheet, and is, for example, 20 vol% or less, preferably 15 vol% or less, more preferably 10 vol% or less.

[0051] The resin sheet is obtained, for example, by the above-mentioned manufacturing method. In this case, the boron nitride primary particles b that do not form the aggregated boron nitride particles in the resin sheet are generated as a result of dissolution of the aggregation of the boron nitride primary particles b in the aggregated boron nitride particles B (disintegration products of the aggregated boron nitride particles B).

[0052] In the resin sheet described above, aggregate boron nitride particles A having an average particle size that easily forms a path for heat conduction (easy to contribute to improving thermal conductivity) are present, and boron nitride primary particles b are present in the gaps between the aggregate boron nitride particles A, which are difficult to conduct heat in conventional resin sheets. Therefore, this resin sheet can effectively conduct heat throughout the entire resin sheet compared to, for example, conventional resin sheets in which only aggregate boron nitride particles are present in the resin, and therefore exhibits excellent thermal conductivity. Therefore, the resin sheet is suitably used, for example, as a heat dissipation sheet (heat dissipation member). EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0054] <Example 1> A mixture of 100 parts by mass of naphthalene-type epoxy resin (manufactured by DIC Corporation, product name "HP4032") and 10 parts by mass of an imidazole compound (manufactured by Shikoku Chemical Industry Co., Ltd., product name "2E4MZ-CN") as a curing agent was mixed with aggregated boron nitride particles A1 (average particle size: 83.3 μm, crushing strength: 9 MPa) formed by agglomeration of scaly boron nitride primary particles a1 (length in the short side direction: 0.57 μm) and aggregated boron nitride particles B1 (average particle size: 25.8 μm, crushing strength: 5 MPa) formed by agglomeration of scaly boron nitride primary particles b1 (length in the short side direction: 1.40 μm) to a total of 50 volume % to obtain a resin composition. At this time, the mixing ratio (volume ratio) of the aggregated boron nitride particles A1 and the aggregated boron nitride particles B1 was A1:B1 = 65:35.

[0055] This resin composition was applied to a PET film to a thickness of 1 mm, and then degassed for 10 minutes under reduced pressure of 500 Pa. Then, heating and pressurization were performed for 60 minutes under conditions of a temperature of 150°C and a pressure of 10 MPa to produce a resin sheet with a thickness of 0.5 mm. An SEM image of the cross section of the obtained resin sheet is shown in Figure 1.

[0056] <Comparative Example 1> A resin sheet was produced in the same manner as in Example 1, except that aggregated boron nitride particles B2 (average particle size: 22.3 μm, crushing strength: 8 MPa) formed by agglomeration of scaly boron nitride primary particles b2 (length in the short side direction: 0.55 μm) were used instead of aggregated boron nitride particles B1. An SEM image of a cross section of the obtained resin sheet is shown in FIG.

[0057] [Table 1]

[0058] 1, the resin sheet of Example 1 contains aggregated boron nitride particles A1 formed by agglomeration of boron nitride primary particles a1, and boron nitride primary particles b1 that do not form aggregated boron nitride particles and are disposed in the gaps between the aggregated boron nitride particles A1. On the other hand, the resin sheet of Comparative Example 1 contains aggregated boron nitride particles A1 formed by agglomeration of boron nitride primary particles a1, and aggregated boron nitride particles B2 formed by agglomeration of boron nitride primary particles b2 (both aggregated boron nitride particles maintain their aggregate shape).

[0059] <Examples 2 to 5> A resin sheet was produced in the same manner as in Example 1, except that the blending ratio of the chunky boron nitride particles was changed as shown in Table 2.

[0060] <Comparative Examples 2 and 3> A resin sheet was produced in the same manner as in Comparative Example 1, except that the blending ratio of the chunky boron nitride particles was changed as shown in Table 2.

[0061] <Example 6> A resin sheet was produced in the same manner as in Example 2, except that chunky boron nitride particles B3 (average particle diameter: 43.0 μm, crushing strength: 6 MPa) composed of an aggregation of scaly boron nitride primary particles b3 (length in the short side direction: 1.20 μm) were used instead of chunky boron nitride particles B1.

[0062] <Example 7> A resin sheet was produced in the same manner as in Example 2, except that chunky boron nitride particles B4 (average particle diameter: 65.3 μm, crushing strength: 3 MPa) composed of an aggregation of scaly boron nitride primary particles b4 (length in the short direction: 1.10 μm) were used instead of chunky boron nitride particles B1.

[0063] <Comparative Example 4> A resin sheet was produced in the same manner as in Example 2, except that chunky boron nitride particles B4 (average particle size: 18.5 μm, crushing strength: 9 MPa) composed of an aggregation of scaly boron nitride primary particles b5 (length in the short direction: 0.80 μm) were used instead of chunky boron nitride particles B1.

[0064] <Comparative Example 5> A resin sheet was produced in the same manner as in Comparative Example 2, except that chunky boron nitride particles A2 (average particle diameter: 88.0 μm, crushing strength: 6 MPa) composed of an aggregation of scaly boron nitride primary particles a2 (length in the short direction: 0.70 μm) were used instead of chunky boron nitride particles A1.

[0065] (Measurement of thermal conductivity) Measurement samples with a size of 10 mm x 10 mm were cut out from each of the resin sheets obtained in the examples and comparative examples, and the thermal diffusivity A (m 2 / sec) was measured. The specific gravity B (kg / m 3 ) was measured by Archimedes' method. The specific heat capacity C (J / (kg K)) of the measurement samples was also measured using a differential scanning calorimeter (DSC; manufactured by Rigaku Corporation, product name "ThermoPlusEvo DSC8230"). Using these measured values, the thermal conductivity of each resin sheet was calculated from the formula thermal conductivity H (W / (m K)) = A × B × C. The results are shown in Table 2.

[0066] [Table 2]

Claims

1. A step of mixing aggregate boron nitride particles A formed by agglomeration of scaly boron nitride primary particles a, aggregate boron nitride particles B formed by agglomeration of scaly boron nitride primary particles b, and a resin to obtain a resin composition; forming the resin composition into a sheet shape, and pressing the resin composition formed into a sheet shape; The length of the short side of the boron nitride primary particles a is 0.7 μm or less, The length of the short side of the boron nitride primary particles b is 1 μm or more, The average particle size of the aggregate boron nitride particles A is 30 μm or more, The average particle size of the aggregate boron nitride particles B is smaller than the average particle size of the aggregate boron nitride particles A, the ratio of the crushing strength of the aggregate boron nitride particles A to the crushing strength of the aggregate boron nitride particles B is 1.2 or more; the resin is at least one resin selected from the group consisting of epoxy resin, silicone resin, silicone rubber, acrylic resin, phenolic resin, melamine resin, urea resin, unsaturated polyester, fluororesin, polyimide, polyamideimide, polyetherimide, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide-modified resin, ABS (acrylonitrile-butadiene-styrene) resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, In the step of pressing the resin composition molded into the sheet shape, agglomerations of the boron nitride primary particles b in the aggregate boron nitride particles B are deflated.

2. 2. The method according to claim 1, wherein the ratio of the average particle size of the chunk boron nitride particles B to the average particle size of the chunk boron nitride particles A is 0.7 or less.

3. 3. The manufacturing method according to claim 1, wherein the content of the aggregate boron nitride particles A in the resin composition is 50 parts by volume or more per 100 parts by volume of the total amount of the aggregate boron nitride particles A and the aggregate boron nitride particles B.

4. The manufacturing method according to any one of claims 1 to 3, wherein the content of the aggregate boron nitride particles B in the resin composition is 5 parts by volume or more per 100 parts by volume of the total amount of the aggregate boron nitride particles A and the aggregate boron nitride particles B.

5. The method according to any one of claims 1 to 4, wherein the resin sheet is used as a heat dissipation sheet.

6. Resin and agglomerated boron nitride particles A formed by agglomeration of scaly boron nitride primary particles a; and scale-like primary particles of boron nitride b which are arranged in the gaps between the aggregate boron nitride particles A and do not form aggregate boron nitride particles, The length of the short side of the boron nitride primary particles a is 0.7 μm or less, The length of the short side of the boron nitride primary particles b is 1 μm or more, The average particle size of the aggregate boron nitride particles A is 30 μm or more, The resin is at least one resin selected from the group consisting of epoxy resin, silicone resin, silicone rubber, acrylic resin, phenolic resin, melamine resin, urea resin, unsaturated polyester, fluororesin, polyimide, polyamideimide, polyetherimide, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide modified resin, ABS (acrylonitrile-butadiene-styrene) resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin.

7. 7. The resin sheet according to claim 6, wherein the content of the aggregate boron nitride particles A is 50 parts by volume or more per 100 parts by volume of the total amount of the aggregate boron nitride particles A and the boron nitride primary particles b.

8. 8. The resin sheet according to claim 6, wherein the content of the boron nitride primary particles b is 5 parts by volume or more per 100 parts by volume of the total amount of the aggregate boron nitride particles A and the boron nitride primary particles b.

9. The resin sheet according to any one of claims 6 to 8, which is used as a heat dissipation sheet.

Citation Information

Patent Citations

  • Heat conductive sheet

    JP2003060134A

  • Thermal conductive particle composition, method for producing thermal conductive particle composition, thermal conductive resin composition, and thermal conductive resin cured body

    JP2016155937A

  • Epoxy resin composition, epoxy resin sheet and metal base circuit board using the same

    JP2017082091A

  • Method for producing heat-conductive sheet

    JP2018030942A