Boron nitride modified lithium-rich manganese-based positive electrode material and preparation method thereof
By introducing hexagonal boron nitride into the lithium-rich manganese-based positive electrode material and performing thermal post-treatment, a stable interface protective layer is formed, which solves the structural instability and oxygen release of the material, improves the overall performance of the battery, and is suitable for high-quality Application of energy density lithium-ion batteries.
Patent Information
- Application Number
- CN202411418984.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The lithium-rich manganese-based positive electrode material has problems such as large irreversible capacity loss in the first week, poor cycle stability, poor rate performance and voltage attenuation, which limits its application in lithium-ion batteries.
By introducing a specific ratio of hexagonal boron nitride (h-BN) and undergoing thermal post-treatment, in-situ modification and pre-activated of the material surface, forming a stable interface protective layer, and improving the electrochemical performance of the material.
It significantly improves the first week of Coulomb efficiency, cycle stability and rate performance, extends the battery life, adapts to the needs of high-power applications, and simplifies the preparation process and reduces costs.
Smart Images

Figure CN118943347A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of positive electrode materials, and in particular relates to a boron nitride-modified lithium-rich manganese-based positive electrode material and a preparation method thereof. Background Art
[0002] With the rapid development of electric vehicles and portable electronic devices, the demand for high energy density lithium-ion batteries is growing. Lithium-rich manganese-based cathode materials (xLi2MnO3·(1-x)LiMO2, M=Ni, Co, Mn) have attracted much attention due to their high specific capacity (>250mAh / g) and are considered to be important candidates for the next generation of lithium-ion battery cathode materials. However, there are still some key issues that restrict the practical application of this type of material: 1) Large irreversible capacity loss in the first week: usually up to 20-30%, mainly due to the oxygen evolution during the activation process of the Li2MnO3 component; 2) Poor cycle stability: During long-term cycling, the material structure is unstable and the capacity decays seriously; 3) Poor rate performance: Due to the low intrinsic electronic conductivity of the material, the capacity retention rate is low during high rate charge and discharge; 4) Voltage decay: As the number of cycles increases, the discharge platform voltage gradually decreases, affecting the energy density.
[0003] To solve these problems, researchers have proposed a variety of modification strategies, such as surface coating, element doping, morphology control, pre-activation treatment, etc. Among them, surface coating is an effective modification method that can stabilize the surface structure of the material, inhibit side reactions, and improve interface properties. Common coating materials include metal oxides (such as Al2O3, ZrO2), phosphates (such as LiPO4), etc.
[0004] According to the crystal structure type, BN mainly includes: hexagonal boron nitride (h-BN), cubic boron nitride (c-BN), orthorhombic boron nitride (r-BN), wurtzite boron nitride (w-BN). As a new type of two-dimensional material, hexagonal boron nitride (h-BN) shows unique advantages in the field of lithium-ion batteries. h-BN has excellent thermal stability, chemical inertness, structural stability and electrical insulation, which make it an ideal surface modification material.
[0005] However, there is a lack of systematic research on h-BN modified lithium-rich manganese-based materials, especially in terms of preparation method optimization and performance improvement mechanism. Existing research mainly focuses on the application of h-BN as a thermal conductive additive or diaphragm modification material, while there are few reports on its direct use for surface modification of lithium-rich positive electrode materials. Therefore, developing a simple and effective h-BN modification method and in-depth research on its influence mechanism on the electrochemical properties of lithium-rich manganese-based materials not only has important scientific significance, but also is expected to provide a new technical path for the development of high-performance lithium-ion battery positive electrode materials and promote the further development of lithium-ion battery technology. Summary of the invention
[0006] In view of the above problems, the present invention provides a boron nitride-modified lithium-rich manganese-based layered oxide positive electrode material and a preparation method thereof, 1+x Mn 1-y-z Ni y Co z O2 (0.1≤x≤0.3, 0.1≤y≤0.3, 0.05≤z≤0.2) type lithium-rich materials, by introducing a specific proportion of hexagonal boron nitride and performing thermal post-treatment, achieve in-situ modification and pre-activation of the material surface. This modification strategy aims to significantly improve the first-week coulomb efficiency, cycle life and rate performance of lithium-rich materials, especially to solve the problems of structural instability and oxygen release during high-voltage charging and discharging. The goal of the present invention is to develop a new type of positive electrode material with excellent performance, simple process and controllable cost to meet the application needs of the next generation of high-energy-density lithium-ion batteries.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is: On the one hand, the present invention provides a boron nitride-modified lithium-rich manganese-based positive electrode material, the chemical formula of which is: Li 1+ x Mn 1-y-z Ni y Co z O2·αBN, wherein 0.1≤x≤0.3, 0.1≤y≤0.3, 0.05≤z≤0.2, 0.005≤α≤0.05; the boron nitride is hexagonal boron nitride (h-BN).
[0008] On the other hand, the present invention provides a method for preparing the above-mentioned boron nitride modified lithium-rich manganese-based positive electrode material, comprising the following steps: S1: Preparation of lithium-rich manganese-based positive electrode materials; S2: Evenly mix the boron nitride and the lithium-rich manganese-based positive electrode material according to a mass ratio, wherein the mass ratio of the boron nitride is 0.5%-5%; S3: placing the mixed materials in a muffle furnace or a tube furnace and sintering at a certain temperature to obtain the positive electrode material.
[0009] Further, step S1 includes the following steps: S11: preparing a transition metal hydroxide or carbonate precursor by a coprecipitation method; S12: mixing the precursor with a lithium source, pre-calcining in air at 400-600° C. for 4-7 hours, and then calcining at 800-900° C. for 10-15 hours to obtain a lithium-rich manganese-based positive electrode material; The specific steps of step S11 are as follows: (1) Preparation of Mn2+ 、Ni 2+ 、Co 2+ Mixed solution of ions, with a total metal ion concentration of 1-3 mol / L; (2) Perform one of the following operations: Method 1: Prepare a NaOH solution with a concentration of 1-3 mol / L, and simultaneously add the metal ion solution and the NaOH solution to the reactor at 60°C, control the pH value at 10.5-11.5, and produce a hydroxide co-precipitation. After reacting for 10-15 hours, filter, wash, and dry to obtain a transition metal hydroxide precursor; Method 2: Prepare a Na2CO3 solution with a concentration of 1-3 mol / L, and add the metal ion solution and Na2CO3 solution to the reactor at 60°C at the same time, control the pH value at 7-8, and allow carbonate co-precipitation to occur. After reacting for 10-15 hours, filter, wash, and dry to obtain a transition metal hydroxide precursor.
[0010] Furthermore, the lithium source is a mixture of one or more of lithium carbonate, lithium oxalate, lithium oxide and lithium hydroxide.
[0011] Furthermore, the sintering temperature in step S3 is 400-700°C.
[0012] Furthermore, the heating rate in step S3 is 3-5°C / min.
[0013] Furthermore, the sintering time in step S3 is 3-7 hours.
[0014] Furthermore, the sintering atmosphere in step S3 is an air atmosphere.
[0015] The technical scheme of the boron nitride-modified lithium-rich manganese-based layered oxide positive electrode material and the preparation method thereof of the present invention realizes in-situ modification and pre-activation of the material surface by introducing a specific proportion of hexagonal boron nitride and performing thermal post-treatment. The layered structure of h-BN is similar to graphite, but has stronger polarity, which can provide a channel for the rapid transmission of lithium ions and improve the rate performance of the material. At a specific temperature, boron nitride reacts with lithium carbonate or excess lithium ions on the surface of the lithium-rich material, inducing a pre-activation reaction on the surface of the lithium-rich material, consuming part of the lithium and oxygen, and forming a stable interface protective layer. This unique interface structure improves the charge transfer kinetics and optimizes the electrode / electrolyte interface properties, thereby significantly improving the first-week coulomb efficiency, cycle stability and rate performance of the lithium-rich material, especially solving the problems of structural instability and oxygen release during high-voltage charging and discharging, thereby improving the overall performance of the battery.
[0016] The relevant reaction formula is as follows: BN + Li2MnO3+ 0.5O2+ Li2CO3→ Li3BO3+ 0.5N2+ LiMnO2+ CO2 The goal of the present invention is to develop a new cathode material with excellent performance, simple process and controllable cost to meet the application requirements of the next generation of high energy density lithium ion batteries. The modification method is simple and easy to implement, low cost and easy to mass produce and apply. The present invention provides a new idea for the development of high-performance lithium-rich cathode materials, and is expected to promote the widespread application of high energy density lithium ion batteries in the fields of electric vehicles, portable electronic devices, etc., which has important scientific significance and application value.
[0017] In summary, the boron nitride modified lithium-rich manganese-based positive electrode material of the present invention has the following advantages: (1) Improve the first-cycle coulombic efficiency and reduce irreversible capacity loss; (2) Improve the cycling stability of materials and extend battery life; (3) Improve the rate performance of materials to meet the needs of high-power applications; (4) The preparation method is simple and easy to produce on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a comparison diagram of the first-week charge-discharge curves of the boron nitride-modified lithium-rich manganese-based positive electrode material and the unmodified material of the present invention; Figure 2 This is a comparison chart of the cycling performance of the boron nitride modified lithium-rich manganese-based positive electrode material of the present invention and the unmodified material at a 0.1C rate; Figure 3 This is a comparison chart of the cycling performance of the boron nitride modified lithium-rich manganese-based positive electrode material of the present invention and the unmodified material at a 1C rate; Figure 4 This is a comparison chart of the rate performance of the boron nitride modified lithium-rich manganese-based positive electrode material and the unmodified material of the present invention; Figure 5 The XRD patterns of the boron nitride-modified lithium-rich manganese-based positive electrode material (Example 3) of the present invention are compared with those of the unmodified material. DETAILED DESCRIPTION
[0019] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0020] Embodiment 1:
[0021] Preparation of Li1.2 Mn 0.54 Ni 0.13 Co 0.13 O2·0.005BN material (the mass ratio of boron nitride to lithium-rich material is 0.5:99.5).
[0022] The specific steps are as follows: 1. Preparation of Mn by co-precipitation method 0.54 Ni 0.13 Co 0.13 (CO3) 0.8 Precursor: a) According to Mn 2+ :Ni 2+ :Co 2+ =4:1:1 molar ratio to prepare a 2.0 mol / L mixed salt solution; b) Prepare 2.0 mol / L Na2CO3 solution; c) Add the metal ion solution and carbonate into the reactor at the same time at 60°C, and control the pH value at 7; d) After reacting for 12 hours, the product was filtered, washed, and dried at 60°C for 12 hours to obtain a precursor.
[0023] 2. Mn 0.54 Ni 0.13 Co 0.13 (CO3) 0.8 The precursor was mixed with Li2CO3 at a molar ratio of 1:1.2, pre-calcined at 500℃ in air for 5h, and then calcined at 850℃ for 12h to obtain Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 lithium-rich materials; 3. 0.995 g of the prepared lithium-rich material was thoroughly mixed with 0.005 g of h-BN.
[0024] 4. In an air atmosphere, the temperature was raised to 600°C at a heating rate of 4°C / min, sintered for 5 hours, and naturally cooled to room temperature to obtain the final product.
[0025] Embodiment 2:
[0026] Preparation of Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2·0.01BN material (the mass ratio of boron nitride to lithium-rich material is 1:99).
[0027] The preparation method is the same as that of Example 1, except that the mixing ratio in step 3 is changed: 0.99 g of the prepared lithium-rich material is mixed with 0.1 gh-BN.
[0028] Embodiment 3:
[0029] Preparation of Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2·0.02BN material (the mass ratio of boron nitride to lithium-rich material is 2:98).
[0030] The preparation method is the same as that of Example 1, except that the mixing ratio in step 3 is changed: 0.98 g of the prepared lithium-rich material is mixed with 0.02 g of h-BN nanosheets.
[0031] Embodiment 4:
[0032] Preparation of Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2·0.03BN material (the mass ratio of boron nitride to lithium-rich material is 3:97).
[0033] The preparation method was the same as in Example 1, except that the mixing ratio in step 3 was changed: 0.97 g of the prepared lithium-rich material was mixed with 0.03 g of h-BN nanosheets.
[0034] Comparison samples:
[0035] Preparation of Li without BN addition 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 material was used as a comparison, and the preparation method was the same as steps 1-2 of Example 1.
[0036] Performance Test:
[0037] The prepared material was mixed with a conductive agent (super P) and a binder (PVDF) in a mass ratio of 8:1:1, coated on aluminum foil to make an electrode, and assembled into a 2032-type button cell for testing using a metallic lithium sheet as the negative electrode and 1M LiPF6EC / DMC (1:1, v / v) as the electrolyte.
[0038] The detailed steps of electrode preparation and battery assembly are as follows: (1) The active material, conductive agent and binder were mixed in a mass ratio of 8:1:1, an appropriate amount of N-methylpyrrolidone (NMP) solvent was added, and the mixture was stirred for 4 hours to prepare a slurry; (2) Use a scraper method to evenly coat the slurry on the aluminum foil, and control the coating thickness to 100 μm; (3) Dry in a vacuum oven at 80°C for 12 hours; (4) Cut into discs with a diameter of 14 mm and compact to a thickness of about 60 μm; (5) The battery was assembled in a glove box filled with argon, with lithium metal sheet as the negative electrode and Celgard 2400 as the separator.
[0039] The test conditions are as follows:
[0040] (1) First week charge and discharge test: 0.1C (1C=250mA / g); (2) Cycle performance test: 0.1C, 1C, voltage range 2.0-4.8V; (3) Rate performance test: 0.1C, 0.2C, 0.5C, 1C, 2C, 3C; refer to Figure 1-Figure 4 , the relevant test results are as follows: 1. Coulomb efficiency of the first week of 0.1C charge and discharge: Example 1: 77.06% Example 2: 80.52% Example 3: 83.74% Example 4: 84.94% Comparison sample: 73.88% 2. Capacity retention rate after 100 cycles at 0.1C: Example 1: 81.00% Example 2: 87.84% Example 3: 83.90% Example 4: 87.27% Comparison sample: 81.07% 3. Capacity retention rate after 300 cycles at 1C: Example 1: 72.50% Example 2: 81.63% Example 3: 84.00% Example 4: 82.62% Comparison sample: 73.51% 4. Discharge capacity retention rate at 3C rate: Example 1: 52.32% Example 2: 56.56% Example 3: 56.70% Example 4: 53.93% Comparison sample: 49.78% In order to gain a deeper understanding of the effect of boron nitride modification on the structure of lithium-rich materials, X-ray diffraction (XRD) was performed on the examples and comparative samples.
[0041] Figure 5 The XRD patterns of the boron nitride-modified lithium-rich manganese-based positive electrode material (Example 3) of the present invention are compared with those of the unmodified material.
[0042] X-ray diffraction (XRD) analysis: XRD test was carried out on Rigaku Ultima IV diffractometer, Cu Kα ray source, scanning range 10-80°, step length 0.02°, scanning speed 5° / min. The results showed that the main diffraction peak positions of the boron nitride modified sample and the unmodified sample were basically consistent, indicating that the introduction of boron nitride did not significantly change the crystal structure of the material. However, the (003) peak intensity of the modified sample was slightly enhanced, and the peak shape was sharper, and the position of the peak changed slightly, indicating that the layered structure was optimized.
[0043] In summary, the boron nitride-modified lithium-rich manganese-based positive electrode material provided by the present invention has higher first-week efficiency, better cycle stability and rate performance than the unmodified material. By mixing different proportions of boron nitride with the prepared lithium-rich material and performing post-treatment, not only the first-week efficiency of the material is improved, but also the structural degradation of the material during the cycle is effectively inhibited. The experimental results show that when 2% of boron nitride is added (Example 3), the material performance reaches the best, the first-week coulomb efficiency is increased by nearly 7 percentage points, the capacity retention rate after 300 cycles is increased by nearly 12 percentage points, and the capacity retention rate at 3C rate is increased by nearly 7 percentage points.
[0044] The characteristic of the present invention is that, at a specific temperature, boron nitride reacts with carbonates on the surface of lithium-rich materials, inducing a pre-activation reaction on the surface of the lithium-rich materials, consuming part of the lithium and oxygen, and forming a stable interface protective layer. This unique interface structure significantly improves the first-week coulomb efficiency, cycle stability and rate performance of the material. The modification method is simple and easy, low-cost, and can be applied on a large scale. The present invention provides a new idea for the development of high-performance lithium-rich positive electrode materials, and is expected to promote the widespread application of high-energy-density lithium-ion batteries in electric vehicles, portable electronic devices and other fields, and has important scientific significance and application value.
[0045] The boron nitride modification method of the present invention has the following advantages: (1) simple operation and easy large-scale production; (2) no need to use expensive or toxic precursors and environmentally friendly; (3) significant modification effect and can simultaneously improve multiple electrochemical performance indicators; (4) wide application range and can be extended to other types of lithium-ion battery cathode materials. This simple and effective modification method provides a new idea for the development of high-performance lithium-rich cathode materials and is expected to promote the practical application of high-energy-density lithium-ion batteries.
[0046] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A boron nitride-modified lithium-rich manganese-based positive electrode material, characterized in that: Its chemical formula is: Li 1+x Mn 1-y- z Ni y Co z O2·αBN, wherein 0.1≤x≤0.3, 0.1≤y≤0.3, 0.05≤z≤0.2, 0.005≤α≤0.05; the boron nitride is hexagonal boron nitride (h-BN).
2. The method for preparing a boron nitride-modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The steps include: S1: Preparation of lithium-rich manganese-based positive electrode materials; S2: Evenly mix the boron nitride and the lithium-rich manganese-based positive electrode material according to a mass ratio, wherein the mass ratio of the boron nitride is 0.5%-5%; S3: placing the mixed materials in a muffle furnace or a tube furnace and sintering at a certain temperature to obtain the positive electrode material.
3. The method for preparing a boron nitride-modified lithium-rich manganese-based positive electrode material according to claim 2, characterized in that: Step S1 includes the following steps: S11: preparing a transition metal hydroxide or carbonate precursor by a coprecipitation method; S12: mixing the precursor with a lithium source, pre-calcining in air at 400-600° C. for 4-7 hours, and then calcining at 800-900° C. for 10-15 hours to obtain a lithium-rich manganese-based positive electrode material; The specific steps of step S11 are as follows: (1) Preparation of Mn 2+ 、Ni 2+ 、Co 2+ Mixed solution of ions, with a total metal ion concentration of 1-3 mol / L; (2) Perform one of the following operations: Method 1: Prepare a NaOH solution with a concentration of 1-3 mol / L, and simultaneously add the metal ion solution and the NaOH solution to the reactor at 60°C, control the pH value at 10.5-11.5, and produce a hydroxide co-precipitation. After reacting for 10-15 hours, filter, wash, and dry to obtain a transition metal hydroxide precursor; Method 2: Prepare a Na2CO3 solution with a concentration of 1-3 mol / L, and add the metal ion solution and Na2CO3 solution to the reactor at 60°C at the same time, control the pH value at 7-8, and allow carbonate co-precipitation to occur. After reacting for 10-15 hours, filter, wash, and dry to obtain a transition metal hydroxide precursor.
4. The method for preparing a boron nitride-modified lithium-rich manganese-based positive electrode material according to claim 3, characterized in that: The lithium source is a mixture of one or more of lithium carbonate, lithium oxalate, lithium oxide and lithium hydroxide.
5. The method for preparing a boron nitride-modified lithium-rich manganese-based positive electrode material according to claim 2, characterized in that: The sintering temperature in step S3 is 400-700°C.
6. The method for preparing a boron nitride-modified lithium-rich manganese-based positive electrode material according to claim 2, characterized in that: The heating rate in step S3 is 3-5°C / min.
7. The method for preparing a boron nitride-modified lithium-rich manganese-based positive electrode material according to claim 2, characterized in that: The sintering time in step S3 is 3-7 hours.
8. The method for preparing a boron nitride-modified lithium-rich manganese-based positive electrode material according to claim 2, characterized in that: The sintering atmosphere in step S3 is an air atmosphere.
Citation Information
Patent Citations
Synthesis and surface modification method of lithium excessive laminar oxide anode material
CN102208607A
Composite cathode active material, cathode and lithium battery including the composite cathode active material, and method of preparing the composite cathode active material
CN102842715A
Method for preparing coated lithium ion battery cathode material of lithium nickel manganese oxide
CN103715409A
Laminated rare earth composite nickel-based battery positive electrode material and preparation method thereof
CN103811728A
BN-coated cobalt-free Ni-Mn solid solution Ni-based positive electrode material
CN106257718A
Cited By
Mo-assisted co-doped disordered rock salt Li1. 3Mn0. 4Nb0. 3O2 lithium-rich positive electrode material as well as preparation method and application thereof
CN121948551A
High performance static electrochemical device
WO2026218061A1