Silica aerogels with enhanced alkaline stability
By treating silica aerogels with a gas mixture of water and a base or acid to reduce residual alkoxy groups, the method addresses the instability issue in alkaline environments, ensuring improved mechanical integrity and thermal insulation.
Patent Information
- Application Number
- JP2022564653
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-30
- Filing Date
- 2021-04-20
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-04-20
AI Technical Summary
Silica aerogels containing unreacted ethoxy groups are prone to hydrolyze quickly in the presence of alkaline components, leading to reduced mechanical integrity and thermal insulation properties in inorganic binder-based formulations.
A method involving the production of hydrophobized silica aerogels by treating the gel with a gas mixture of water and a base or acid to reduce residual alkoxy groups, followed by subcritical drying to maintain stability in alkaline environments.
The method results in silica aerogels with reduced ethoxy content, enhancing their stability and maintaining thermal insulation properties even in the presence of alkaline components.
Smart Images

Figure 0007577757000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a particular method for producing silica aerogel, silica aerogel with reduced ethoxy content, and the use of such aerogel for thermal insulation. [Background technology]
[0002] Silica-based aerogels and xerogels are increasingly used as very efficient insulating materials, for example in building insulation, due to their very low thermal conductivity and material density. Cost-efficient production of aerogels and xerogels is becoming increasingly important. Numerous methods are known for their production. Typically, the starting point is water glass (sodium silicate) or tetraalkoxysilanes (organic silicate esters), such as tetraethyl orthosilicate (TEOS) and tetramethyl orthosilicate (TMOS), and less widespread hydrophobic T-type alkoxysilanes, such as methyltrimethoxysilane (MTMS) or methyltriethoxysilane (MTES), are used as silicon source to form first a silica sol and then a silica gel.
[0003] Up until now, aerogels have traditionally been produced exclusively by supercritical drying, i.e. drying from supercritical fluids, typically lower alcohols (High Temperature Supercritical Drying or HTSCD), and more recently preferably CO2 (Low Temperature Supercritical Drying or LTSCD). In the drying methods mentioned above, it was necessary not to exceed the critical parameters specific to the solvent used, such as temperature and pressure. The critical temperature and pressure of CO2 are about 31°C and about 74 bar. Carrying out reactions at such high processing pressures requires relatively cost-intensive process control and capital investment for the production of aerogels.
[0004] An important breakthrough in the production of aerogels or xerogels of similar structure was realized by subcritical drying at standard pressure from hydrophobized gels containing solvents. This method is described, for example, in US5565142A1. Drying under such subcritical conditions made it possible to produce materials with almost identical properties to supercritically dried aerogels. Initially, they were named xerogels according to the classical definition, which is the term still used for aerogels subcritically dried from solvents. Rather than the classical definition of aerogels being used based on the nature of their production, in the remainder of this specification we instead refer to typical material properties (density up to 0.30 g / cm3). 3 We use a definition based on the following: less than 100% water vapor, greater than 85% porosity, and pore size 20-80 nm. Therefore, subcritically dried materials are still referred to as aerogels rather than xerogels.
[0005] WO2012 / 044052A2 relates to the preparation of optically transparent and opaque silica aerogels in granular form. This is done by injecting a water glass sol into an alcohol phase, resulting in the formation of a gel. This gel is further exchanged with alcohol and hydrophobized using a silylation reagent. The gel is then dried under normal or reduced pressure. An essential step of this method is the washing with ethanol, which is necessary to remove the water from the hydrogel phase. By using alcohol, the resulting aerogel necessarily contains a small amount of alkoxy groups.
[0006] WO2013 / 053951A1 describes a method for producing a xerogel, comprising the following series of method steps: (a) producing an alcohol-containing sol by hydrolysis of tetraethoxysilane (TEOS), (b)-(c) gelling and aging the sol, (d) hydrophobizing the sol produced and aged in steps (b) and (c), and (e) pre-drying the hydrophobized sol at a temperature below 80° C. Process and (f) optionally, thorough drying at a temperature above 100° C. Such hydrolyzed organosilicate-derived aerogels also contain a significant amount of unhydrolyzed ethoxy groups.
[0007] W.J.Malfait et al., in Chem. Mater. 2015, Vol. 27, pp. 6737-6745, describe the characterization of the surface chemistry of different types of hydrophobized aerogels and related silica foams using NMR techniques. Thus, samples prepared from tetraethoxysilane (TEOS), polyethoxydisiloxane (PEDS), or waterglass precursors were hydrophobized with trimethylsilyl (TMS) groups using hexamethyldisilazane (HMDS), trimethylchlorosilane (TMSCl), or hexamethyldisiloxane (HMDSO). Table 2 of this publication shows the content of trimethylsilyl (Si-O-TMS), ethoxy (Si-O-Et), and silanol (Si-OH) groups measured by NMR techniques. All prepared aerogel samples modified with TMS groups contained a relatively high trimethylsilyl group content (2.9-3.8 mmol / g). The ethoxy and silanol content of samples 1, 2 and 4 were 0.3, 0.6, 0.9, and 1.0, 1.0 and 1.8 mmol / g, respectively.
[0008] Thus, silica aerogels and similar materials prepared from precursors containing alkoxy groups, especially ethoxy groups, in the precursor system, or derived from sol-gel and / or solvent exchange processes in solvent systems containing significant amounts of alcohols such as ethanol, will always contain significant amounts of unhydrolyzed ethoxy groups. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] U.S. Patent Publication No. 5565142A1 [Patent Document 2] International Publication No. 2012 / 044052A2 [Patent Document 3] International Publication No. 2013 / 053951A1 [Patent Document 4] U.S. Patent Number 3562177 [Patent Document 5] International Publication No. 2015 / 014813A1 [Non-patent literature]
[0010] Chem. Mater. 2015, Vol. 27, pp. 6737-6745 W. J. Malfait et al. Summary of the Invention [Problem to be solved by the invention]
[0011] It has been found that this normally remaining ethoxy content leads to some significant disadvantages during the practical use of such silica aerogels, especially when they are integrated into inorganic binder-based formulations. In such cases, the unreacted ethoxy groups tend to quickly hydrolyze in the presence of alkaline components of lime- or cement-based binders in some insulating compositions, such as aerogel-containing base coats, cement or other mortar compositions. The resulting insulating inorganic compositions then show a significant decrease in mechanical integrity, durability, and ultimately also in insulating properties.
[0012] The technical problem addressed by the present invention is to provide a silica aerogel having increased stability against such alkaline components. Another object of the present invention is to provide a method for producing such a silica aerogel. [Means for solving the problem]
[0013] The object of the present invention is to provide a method for producing a hydrophobized silica aerogel, comprising the steps of: a) preparing a hydrophobized silica gel containing an alkoxy group; b) drying the hydrophobized silica gel obtained in step a); c) treating the product obtained in step b) with a gas mixture containing water and a base or an acid. The method includes:
[0014] US 3,562,177 discloses a thickener containing hydrophilic silica aerogel particles containing 0.10% to 2.5% by weight of ammonia, which is prepared by reacting silica aerogel obtained from an aqueous solution of water glass with ammonia. However, US 3,562,177 does not disclose treating the hydrophobized silica aerogel with water and ammonia.
[0015] Surprisingly, it has been found that the method of the present invention provides hydrophobized silica aerogels with reduced content of residual alkoxy groups that are particularly suitable for the preparation of thermal insulating compositions containing an alkaline component. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] In step a) of the method of the present invention, a hydrophobized silica gel is obtained. Step a) preferably further comprises the steps of: a1) providing a mixture comprising a silica sol; a2) gelling the mixture obtained in step a1); optionally, a3) aging the gel obtained in step a2); a4) hydrophobizing the gel obtained in step a2); and optionally, a5) performing a solvent exchange on the gel already obtained in step a2) and optionally aged in step a3).
[0017] The alkoxy group is preferably a low molecular weight C1-C4 aliphatic alkoxy group and may be selected from the group consisting of methoxy (OCH3), ethoxy (OC2H5), propoxy (OC3H7), butoxy (OC4H9), and mixtures thereof. Most preferably, the alkoxy group is an ethoxy group.
[0018] The silica sol can be prepared in step a1) of the process starting from sodium silicate (water glass) solution, ion-exchanged water glass, silicic acid or colloidal silica, and mixtures thereof. Alcohol can be present during the preparation of the sol or during gelation, and can be added during the subsequent solvent exchange and / or hydrophobization before drying of the resulting silica aerogel. In this case, the resulting silica aerogel usually contains residual unhydrolyzed alkoxy groups.
[0019] Said silica gel may be obtained, in its pure form or as an alcoholic solution, from the corresponding silica sol produced in step a1) by hydrolysis of an organosilicate Si(OR)4, which may be selected from the group consisting of tetraethyl orthosilicate (TEOS, R=C2H5), tetramethyl orthosilicate (TMOS, R=CH3), tetraisopropyl orthosilicate (TPOS, R=i-Pr), and mixtures or oligomers thereof.
[0020] The reaction of organosilicate esters with water results in their hydrolysis, in which the alkoxy groups (OR) bonded to silicon are partially or completely replaced by silanol groups Si-OH, which can then react with each other to form siloxane bonds (Si-O-Si) via so-called polycondensation reactions. Hydrolysis and condensation are dynamic reactions involving many interconnected chemical equilibria that are strongly influenced by catalysts, e.g. acids and bases. Such hydrolysates of organosilicate esters, consisting of nanoscale colloidal particles composed of amorphous silica with a significant residual proportion of unhydrolyzed alkoxy groups Si-OR, usually have low viscosity and are called silicon dioxide sols or silica sols.
[0021] The silica sol may then be diluted with an organic solvent mixture consisting of an alcohol, a hydrophobizing agent, preferably activatable by an acid catalyst, and water.
[0022] It goes without saying that in addition to the alcohol, the silica sol and the hydrophobizing agent, the silica sol mixture used in step a) may contain small proportions of water, unavoidable impurities and certain additives which are customary in the manufacture of silica sols. This mixture may further contain at least one polymerizable functional silane and, optionally, also the prepared AeroThe gel material may contain one or more monomers capable of forming polymeric structures. The polymerizable functional silane advantageously contains a radically polymerizable group, as in the case of conventional vinyltrialkoxysilanes, such as vinyltriethoxysilane and vinyltrimethoxysilane, or 3-trialkoxysilylpropyl methacrylates, such as trimethoxysilylpropyl methacrylate or triethoxysilylpropyl methacrylate. Preferred monomers are likewise selected from the group of free radically polymerizable substances, such as acrylates, vinyl chloride, styrene or divinylbenzene. Additionally or alternatively, additives providing mechanical reinforcement, such as short fibers, for example glass or mineral fibers, may be added to the mixture containing the silica sol. Furthermore, the sol may also contain at least one organofunctional silane, for example with a hydrophobic group. Such organofunctional silanes can be, for example, methyltrimethoxysilane, methyltriethoxysilane, n-propyltriethoxysilane, n-propyltrimethoxysilane, n-octyltriethoxysilane, n-octyltrimethoxysilane, isopropyltriethoxysilane, isopropyltrimethoxysilane, isobutyltriethoxysilane, isobutyltrimethoxysilane, n-butyltriethoxysilane, n-butyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane.
[0023] Step a1) of the process of the present invention, when said precursor is an alkoxysilane or an organosilicate, may be carried out in the presence of an alcohol selected from the group consisting of methanol, ethanol, n-propanol, isopropanol, butanol and mixtures thereof.
[0024] Step a1) of the process of the present invention, when said precursor is water glass or sodium silicate, ion-exchanged sodium silicate or an oligomeric silicic acid solution, may be carried out in the presence of a majority of water and any minor fraction of an alcohol selected from the group consisting of methanol, ethanol, n-propanol, isopropanol, butanol and mixtures thereof.
[0025] In the method of the present invention, said silica gel may be obtained by gelling of an inorganic precursor selected from the group consisting of sodium silicate, water glass, ion-exchanged water glass, silicic acid or colloidal silica, and mixtures thereof.
[0026] In this case, the solvent system used during any of the processing operations between steps a) and b) can be an alcoholic solvent system.
[0027] In the preparation of the silica sol, a catalytic amount of acid and a substoichiometric amount of water are preferably added to the alcohol solution of the organic silicic acid ester, where the molar ratio of the organic silicic acid ester / water / acid is maintained at 1:1-3.5:0.0001-0.01, more preferably 1:1-2.5:0.0005-0.005. Examples of acids that can be used are sulfuric acid, hydrochloric acid or nitric acid.
[0028] Hydrophobizing agents are understood to mean components that provide hydrophobicity and water repellency to the oxide surface. This is achieved by the reaction of the hydrophobizing agent with the silica surface. Examples of typical hydrophobizing agents for silica are organosilanes, organosiloxanes, and organosilazanes. From WO2015 / 014813A1, it is known that some of these hydrophobizing agents can be activated by acid catalysis, which means that in the presence of a catalytic amount of a certain acid, they can react with the silica surface at lower temperatures and / or more quickly than in the absence of a catalyst. Examples of such hydrophobizing agents that can be activated by acid catalysis, which are preferably used in the method of the present invention, include organosiloxanes and other alkylalkoxysilanes. Particularly suitable as hydrophobizing agents that can be activated by acid catalysis are hexamethyldisiloxane and trialkylalkoxysilanes, in particular trimethylalkoxysilanes, such as trimethylethoxysilane and trimethylmethoxysilane. The acid-catalyst-activatable hydrophobizing agents according to the invention are very particularly preferably selected from the group consisting of hexamethyldisiloxane, trimethylethoxysilane, trimethylmethoxysilane, and mixtures thereof.
[0029] Step a) of the process of the present invention is preferably carried out using a hydrophobizing agent activatable by an acid catalyst selected from the group consisting of hydrogen chloride, nitric acid, sulfuric acid, trimethylchlorosilane, and mixtures thereof.
[0030] The gelling process in step a2) of the method of the present invention may be initiated by addition of a base to the mixture comprising the silica sol formed in step a1), preferably followed by mixing, and shortly thereafter the final gelling and optional maturation of the gel formed in step a2) may take place in step a3).
[0031] The aforementioned Si-OH silanol groups, formed for example by hydrolysis of organosilicate groups on the surface of the already formed colloidal particles, condense in step a2) and, now catalyzed by the addition of base and optionally further heating, form a three-dimensional particle network called silicon dioxide gel or silica gel. Thus, the gel forms in an alcohol / hydrophobizing agent medium, which can also be called an "alcogel" or "organogel", and is typically subjected to a further maturation step if a second co-solvent different from the alcohol or the hydrophobizing agent is present in the solvent mixture, in which the particle network structure is mechanically reinforced by the formation of new chemical siloxane bonds between the neck regions between the particles. In practice, the sol system and the amount of base added are usually selected so that the gelation time is between 5 and 15 minutes.
[0032] The step of gelling the silica sol, i.e. process step a2), and optionally the step of aging the silica gel obtained, i.e. process step a3), are preferably carried out in the presence of a base catalyst selected from the group consisting of ammonia, lower aliphatic alkylamines, aminosilanes, ammonium fluoride, alkali metal hydroxides (in particular sodium hydroxide or potassium hydroxide), alkaline earth metal hydroxides, and mixtures thereof. Lower aliphatic amines are understood to mean primary, secondary, or tertiary alkylamines with a molar mass of less than 500 g / mol. Examples of particularly suitable aminosilanes are aminopropyltrimethoxysilane or aminopropyltriethoxysilane. The base catalyst is particularly preferably selected from the group consisting of ammonia, ammonium fluoride, or aminosilane. It is preferable to add a dilute solution of the base catalyst in a solvent, for example a dilute alcoholic ammonia solution.
[0033] Step a2) is preferably carried out within 1 hour, preferably within 30 minutes, more preferably within 10 minutes before step a3).
[0034] In a particular embodiment of the invention, steps a2) and a3) are carried out in one step, the addition of the base catalyst and the subsequent maturation of the silica sol being carried out in the same reactor.
[0035] Step a3) may preferably be carried out at a temperature between 60° C. and 130° C., more preferably between 80° C. and 120° C. The usual duration of this step is between 5 and 240 minutes, preferably between 10 and 180 minutes. More preferably, step a3) of the process of the invention is carried out within 20 to 75 minutes at a temperature between 90 and 115° C. The use of a pressure vessel is preferred for carrying out steps b2) and c), since the operations are usually carried out at temperatures above the boiling point of the mixture (approximately 80° C. when ethanol is used as the solvent).
[0036] In step a4) of the process of the invention, the hydrophobization of the silica gel produced in step a2) may be initiated by the addition of a hydrophobization catalyst, which may be added to the gel or may be released directly in the silica gel.
[0037] Hydrophobizing agents that can be activated by acid catalysts are preferably used in the process of the present invention. Such hydrophobizing agents are traditionally + or H3O + It is activated in the presence of ion-generating Bronsted acids. Thus, the gelation process, which proceeds under slightly basic conditions, and the hydrophobization process, which proceeds under acidic conditions, may be carried out in the same organogel as separate operations clearly separated in time.
[0038] In a particularly preferred embodiment of the present invention, the hydrophobization catalyst is selected from the group consisting of hydrogen chloride (in gaseous or solution form), nitric acid, sulfuric acid, trimethylchlorosilane, and mixtures thereof. It is particularly preferred to use an alcoholic solution of hydrogen chloride, nitric acid, sulfuric acid, or trimethylchlorosilane as the hydrophobization catalyst.
[0039] In a further embodiment of the invention, the hydrophobization catalyst is formed in situ in the gel by a free radical decomposition process. The hydrophobization catalyst is advantageously formed by free radical decomposition of already added organochlorine compounds, such as less stable or unstable PVC, trichloromethane, chloroacetone or tetrachloroethylene. The hydrophobization catalyst is advantageously HCl and can therefore be released at the desired time, the release being brought about either by electromagnetic radiation (UV, X-ray) or by conventional radical initiators. The high optical transparency is Ku For thinner gels, the photochemical free radical decomposition process is preferred.
[0040] In a further embodiment of the invention, the hydrophobization catalyst is released in the gel by a sustained release agent, the release being optionally initiated or accelerated by thermal activation. In this case, it is preferred to use as hydrophobization catalyst hydrogen chloride, nitric acid or sulfuric acid, or their precursors, released from "sustained release" or "controlled release" additives present in the sol, such as microcapsules, nanocapsules or particles. These additives are ideally activated by externally controllable process parameters, such as pressure, temperature or electromagnetic radiation (light, radio waves, microwaves).
[0041] Steps a3) and / or a4) of the process of the invention are preferably carried out in a pressure vessel at a pressure between 1 and 20 bar, more preferably between 1.1 and 10 bar (absolute), most preferably between 1.2 and 5 bar (absolute). At standard atmospheric pressure, the boiling points of the solvent mixtures used are usually between 80 and 100° C. By analogy with the example of the pressure cooker, operation in a pressure vessel allows step a4) of the invention to be carried out at significantly higher temperatures in the range of 80-130° C., which increases the reaction rate. This allows a significant reduction in both the maturation time and the hydrophobization time (for example a reduction in maturation time from 24 hours at 65° C. to just 3 hours at 90° C.), resulting in a significant increase in the efficiency of the process.
[0042] In a particularly preferred embodiment of the present invention, the hydrophobization of the silica in step a4) is carried out at a temperature of 80-130° C. and a pressure of 1.2-4 bar within 20-180 minutes.
[0043] Step b) of the method of the present invention involves drying the hydrophobized silica gel obtained in step a), which may be carried out under subcritical or supercritical conditions, preferably under subcritical conditions.
[0044] Under "subcritical conditions" it is understood that the critical parameters specific to the solvent used, such as temperature and pressure, are not exceeded. In contrast, under "supercritical conditions" these parameters must be exceeded. Thus, under supercritical conditions, the solvent mixture used (pore liquid) exists as a supercritical fluid during drying. For example, the critical temperature and pressure of CO2 are about 31° C. and about 74 bar.
[0045] In step b) of the method of the invention, the volatile components present in the hydrophobized silica gel, such as the alcohol and any remaining hydrophobizing agent, are removed, for example by evaporation to dryness, leaving the final aerogel structure. In this step, preferably more than 95%, more preferably more than 98%, of all volatile components are removed. Volatile components of the mixture are understood to mean all components that have a boiling point below 200° C. at standard atmospheric pressure.
[0046] In a preferred embodiment of the invention, step b) is carried out at least partially under reduced pressure, more preferably at a pressure between 0.1 and 1 bar absolute. Drying under reduced pressure has the advantage that it can be carried out at lower temperatures, i.e. with reduced thermal energy requirements. Working under reduced pressure therefore allows a lower content of residual solvents (residual moisture) in the aerogel material at the same temperature, in particular at the end of drying. On the other hand, from the point of view of the process procedure, the transfer of heat with the material to be dried via convective gas exchange increases with increasing pressure, which subsequently reduces the drying time and increases the process efficiency. Step b) of the process of the invention is particularly preferably carried out at temperatures between 100 and 200 ° C and pressures between 0.1 and 4 bar.
[0047] In a further preferred embodiment of the invention, during the implementation of step b), the carrier gas enters the reactor continuously and, after mixing with the gaseous components of the reactor, then leaves the reactor. This considerably shortens the drying step and / or allows the production of an aerogel material with low residual moisture. The carrier gas used can be, for example, nitrogen. The carrier gas used is particularly preferably preheated to a temperature of 50 to 200° C. The preheated carrier gas can advantageously be introduced into the reactor by pressure regulation to 1 to 4 bar. This promotes the transfer of heat between the introduced gas and the solid / liquid reaction mixture in the reactor. The gas inflow into the reactor per unit time and the reactor volume are preferably between 150 and 1500 h -1 It has been found to be particularly advantageous when the gas hourly space velocity (GHSV) corresponds to GHSV[h -1 ] = Gas inflow to reactor per unit time L / reactor volume L
[0048] In step c) of the process of the invention, the product obtained in step b) is treated with a gas mixture containing water and a base or acid, preferably a sufficiently volatile gas mixture. The aim of this step c) of the process is to optimize the association of water as reactant with the acid or base catalyst in order to maximize the degree of hydrolysis of the residual alkoxy, e.g. ethoxy, groups present in the hydrophobized silica gel obtained in step b) of the process.
[0049] The base or acid used in step c) of the process is preferably suitable for catalyzing the hydrolysis of alkoxysilane groups Si-OR, where R can be, for example, a methyl, ethyl, propyl, butyl, or other alkyl group. Such base or acid catalysts are preferably suitable for catalyzing the hydrolysis of sterically bulky siloxyl groups, such as Si-O-SiR 1 does not cause hydrolysis of 3, where R 1 is preferably methyl.
[0050] The base used in step c) of the process is preferably selected from the group consisting of ammonia, lower aliphatic alkylamines such as trimethylamine, dimethylamine, diethylamine, and mixtures thereof.
[0051] Suitable acids for use in step c) of the process may be selected from the group consisting of volatile mineral acids such as hydrochloric acid (HCl), hydrofluoric acid (HF), hydrobromic acid (HBr), hydroiodic acid (HI), nitric acid (HNO3), carboxylic acids such as formic acid and acetic acid, halosilanes such as trimethylchlorosilane, and mixtures thereof.
[0052] The water and the base or acid are present in the form of gas (vapor) in step c) of the method, which can facilitate the hydrolysis of the alkoxy groups in step c) and make subsequent drying of the treated aerogel unnecessary.
[0053] In step c) of the process, the molar ratio of water to base or acid is preferably at least 4, more preferably at least 5, more preferably at least 10.
[0054] The gas mixture used in step c) of the method of the invention may further comprise a carrier gas, such as nitrogen, air, argon.
[0055] An aqueous solution of a base, such as ammonia, or an acid, such as hydrochloric acid, can be vaporized by introducing a carrier gas, such as nitrogen or air, into the solution, thereby obtaining a gas mixture of carrier gas, water and base or acid, which can be used directly in step c) of the process of the invention.
[0056] The temperature maintained during step c) of the method of the present invention is preferably between 50°C and 250°C, more preferably between 75°C and 200°C, more preferably between 100°C and 180°C, more preferably between 120°C and 170°C.
[0057] The duration of step c) of the method of the present invention is preferably from 1 minute to 1000 minutes, more preferably from 2 minutes to 500 minutes, more preferably from 3 minutes to 200 minutes, more preferably from 4 minutes to 100 minutes, more preferably from 5 minutes to 30 minutes.
[0058] The present invention further relates to a silica aerogel containing trimethylsiloxyl (≡SiOSiMe3) groups, alkoxysilyl (≡SiOR) groups, and silanol (≡SiOH) groups, Maximum 0.17g / cm 3 The envelope density of The ratio N of the amount of trimethylsiloxyl groups (≡SiOSiMe3) to the sum of the amount of trimethylsiloxyl groups, alkoxysilyl groups, and silanol groups is greater than 0.5, preferably greater than 0.6, and more preferably greater than 0.7. SiOSiMe3 / (N SiOSiMe3 +N SiOR +N SiOH ), as well as A ratio N of the amount of alkoxysilane groups to the sum of the amount of alkoxysilane groups and silanol groups of 0.05 to 0.35, preferably 0.10 to 0.32, and more preferably 0.15 to 0.30. SiOR / (N SiOR +N SiOH ) It is characterized by: R is an alkyl group, preferably an alkylalkoxy group, such as methyl, ethyl, propyl, butyl, more preferably methyl or ethyl; Preferably, the amount of trimethylsiloxyl (≡SiOSiMe3) groups and alkoxysilyl (≡SiOR) groups is adjusted according to the protocol described by WJMalfait et al., Chem. Mater. 2015, Vol. 27, pp. 6737-6745. 1 The amount of silanol (≡SiOH) groups was measured by H-NMR. 29 Provided is a silica aerogel as measured by Si-NMR.
[0059] The envelope density of the silica aerogel of the present invention is up to 0.17 g / cm 3 and preferably 0.05 g / cm3 ~0.160g / cm 3 , more preferably 0.07 g / cm 3 ~0.150g / cm 3 , more preferably 0.08 g / cm 3 ~0.140g / cm 3 It is.
[0060] Envelope density can be measured for large granular (typically larger than 1-2 mm) porous materials where the large internal pore volume within the material precludes direct measurement, e.g. using simple buoyancy techniques. In this case, the granular material sample to be measured is surrounded by a medium, e.g. a free-flowing dry powder medium, which does not enter the pores but forms an "envelope" that conforms closely to the contours of the irregular surface.
[0061] The envelope density can be measured, for example, by powder pycnometry using a GeoPyc 1360 instrument (Micromeritics).
[0062] The amount of the trimethylsiloxyl (≡SiOSiMe3) group and the alkoxysilyl (≡SiOR) group is 1 The H-NMR analysis is used. In particular, quantitative solid-state NMR magic angle spinning (MAS) techniques are used, with reference to known substances for quantification. The peaks corresponding to the methyl signals of the trimethylsiloxyl (≡SiOSiMe3) groups are measured. For the measurement of alkoxysilyl (≡SiOR) groups, the signals are 1 Any proton of the alkoxy group that does not overlap significantly with other protons in the H spectrum can be used. For methoxy or ethoxy groups, the protons of the methyl group are used.
[0063] 1H-NMR spectra can be recorded with a wide-bore 9.4 T magnet, corresponding to a Larmor frequency of 400.2 MHz, using a spectral width of 249.9 ppm and an acquisition time of 328 ms. Linewidth can be minimized using a 24 kHz MAS speed with a 2.5 mm zirconia rotor. All spectra are usually collected with a recycle delay of at least 5 times the T1 relaxation time, as measured in saturation recovery experiments, to ensure their quantitative nature. Full relaxation spectra of adamantane and octakis(trimethylsiloxy)silsesquioxane (Q8M8) can be used for calibration of absolute NMR signal intensities.
[0064] The amount of the silanol (≡SiOH) groups is determined by the Q 3 Assuming that the species is linked to either an alkoxy group or a hydroxyl group, Q 3 Solid-state MAS- 29 Measured by Si-NMR.
[0065] 29 Si-NMR spectra can be recorded with a wide-bore 9.4 T magnet, corresponding to a Larmor frequency of 79.5 MHz, with a spectral width of 349.3 ppm and an acquisition time of 74 ms. Linewidth can be minimized using a Bruker Avance III HD instrument applying a 4 kHz MAS speed with a 7 mm zirconia rotor.
[0066] All NMR spectra ( 1 H and 29 Si), when measured in saturation recovery experiments, are typically collected with a recycle delay of at least 5 times T1 to ensure their quantitative nature. 1 H-NMR spectra were analyzed using absolute 1 It can be used for the calibration of H-NMR signal intensities and is29 The Si-NMR spectrum is 29 This is for the calibration of Si-NMR spectra.
[0067] All samples and standards are preferably measured with a fully filled rotor, and during intensity calibration, with pulses strong enough to ensure uniform excitation and to ensure that potential inhomogeneities in sensitivity due to gradients in frequency-resolved (RF) field strength are negated: 1 For H, 83kHz. 29 For Si, it is 45kHz.
[0068] Details of the quantitative measurement of surface functional groups of hydrophobized silica aerogels by NMR techniques can be found in WJMalfait et al., Chem. Mater. 2015, Vol. 27, pp. 6737-6745. The contents of this publication regarding solid-state NMR analysis are hereby incorporated by reference.
[0069] The silica aerogel of the present invention can be prepared by the method of the present invention.
[0070] The silica aerogel according to the invention preferably has a particulate form, e.g. denoting a powder or granules. In the case of a powder, this is understood to mean particles having an average number size of up to 50 μm, while granules usually consist of particles having an average number size of 50 μm to 10 mm.
[0071] The silica aerogel of the present invention is in the form of a powder or preferably has an average number particle size d of, for example, 50 μm to 10 mm, more preferably 100 μm to 5 mm. 50 The number average particle size of the powder or granules may be measured by laser diffraction particle size analysis in accordance with ISO 13320:2009. The resulting particle size distribution may be expressed as the number average particle size, the size not exceeding 50% of all particles, with an average d 50 It is used to specify:
[0072] The thermal conductivity of the silica aerogel of the present invention is preferably between 12 mW / (mK) and 25 mW / (mK) at standard pressure and 20° C. The thermal conductivity of the aerogel bulk material in powder or granule form can be measured according to EN 12667:2001 at an average measurement temperature of 20° C., in an air atmosphere, and at standard pressure.
[0073] The silica aerogel of the present invention is 300m 2 / g, preferably 400m 2 / g~1000m 2 / g, more preferably 450m 2 / g~900m 2 / g, more preferably 550m 2 / g~850m 2 The specific surface area can have a BET surface area of 100 / g. The specific surface area is also simply called the BET surface area and can be measured by nitrogen adsorption according to the Brunauer-Emmett-Teller method in accordance with DIN 9277:2014.
[0074] The present invention further provides the use of the silica aerogel of the present invention for thermal and / or acoustic insulation.
[0075] The silica aerogels of the present invention can be used as bulk materials for thermal insulation and / or acoustic insulation, e.g., in insulating containers; in pasty formulations such as plaster, mortar, and concrete formulations; in thermal and / or acoustic insulation coatings, e.g., as energy saving thermal insulation coatings in industrial applications, as components and thin films of insulating textile products for lightweight building construction applications.
[0076] Another object of the invention is a composition for thermal and / or acoustic insulation comprising the silica aerogel of the invention.
[0077] Such thermal and / or acoustic insulation compositions may be in the form of thermal and / or acoustic insulation panels formed from the silica aerogel material of the present invention.
[0078] The thermal and / or acoustic insulation composition, or the corresponding panel, may resist the transmission of heat and / or sound, thereby having thermal and / or acoustic insulation properties. EXAMPLES
[0079] Comparative Example 1 A silicon dioxide sol concentrate was prepared by alcohol hydrolysis of TEOS in ethanol at room temperature using a molar ratio of TEOS / water / sulfuric acid of 1:3.0:0.001 with an equivalent silica content expressed as 20 wt.% SiO2 at 35 °C. The sol concentrate was then left overnight before use. The sol concentrate was then diluted with HMDSO and ethanol such that the HMDSO content in the sol was 30 wt.% to a final sol concentration equivalent to 5.7 wt.% SiO2. A 2% by volume dilute ethanolic ammonia solution was then added to the sol, which gelled within 8-10 min. The fresh organogel was placed in a sealed steel tube pressure vessel, covered with a small amount of ethanol, and aged at 95 °C for 2 h.
[0080] After aging, the sealed tube was cooled to room temperature and carefully opened. The aged gel was then mechanically crushed and the gel granule particles were placed again in the steel tube. Subsequently, a mixture of dilute nitric acid, ethanol and HMDSO was added, barely covering the gel particles. The steel tube was resealed and placed in a 100°C oil bath, where it was maintained for 2 hours for hydrophobization. After completion of hydrophobization and cooling to 45°C, the gel particles were removed and subsequently dried in a convection drying oven under nitrogen at 150°C.
[0081] The final aerogel material had a mass of 0.115 g / cm 3 The aerogels had an envelope density of 0.018 mm and a typical packed-bed thermal conductivity for a granular sample of 0.0184 W / (mK). Other chemical data for the aerogels are summarized in Table 1.
[0082] Example 1 Laboratory-scale production of aerogel granules The aerogel material with remaining alkoxy groups from Comparative Example 1 was then kept in the same oven and the oven temperature was increased to 165°C. Once the new temperature setting was reached, the oven was opened immediately, a thin capillary tube connected to a syringe pump was placed under the aerogel sample and the door was closed again. Hydrolysis of the ethoxy groups was now initiated by adding 6M aqueous ammonium hydroxide at a rate of 300mL / h. After 40 minutes, the addition was stopped and the remaining water / ammonia mixture in the oven was purged with a stream of nitrogen for an additional 10 minutes. The final aerogel material was then removed and characterized, measuring 0.118g / cm 3 The aerogels had an envelope density of 0.018 mm and a typical packed-bed thermal conductivity for a granular sample of 0.0184 W / (mK). Other chemical data for the aerogels are summarized in Table 1.
[0083] Example 2 The procedure was identical to that described in Example 1, except that the drying temperature was 160° C. and the ethoxy group hydrolysis step was performed immediately after the drying step by starting the addition of aqueous ammonium hydroxide solution through a capillary placed at the beginning of the drying step. The physicochemical data of the aerogels are summarized in Table 1.
[0084] Example 3 The procedure was identical to that described in Example 1, except that the ethoxy group hydrolysis step was carried out by injection of 3M aqueous trifluoroacetic acid at a rate of 200 mL / h, and the addition was maintained over a period of 25 min. The physicochemical data of the aerogels are summarized in Table 1.
[0085] Example 4 Industrial production of aerogel granule materials The pilot plant used consisted of a stirred batch reactor for the production of the sol, and a tube bundle reactor with top and bottom sealing lids, as well as a downstream further heated hydrophobization reactor, a phase separation unit, and a hybrid convection / contact drying unit. The periphery of the equipment consisted of appropriate auxiliary units (heaters, heat exchangers, condensers) and solvent tanks, as well as storage of the various reagents. The tube bundle reactors consisted of parallel tube heat exchangers, each with an internal diameter of 23 mm, and a cover that could be purged with a heat transfer fluid medium. The reactors were mounted on the floor of the factory premises at a fixed angle of 19° to the horizontal.
[0086] First, 76 L of sol, consisting of 30 kg ethanol, 30 kg sol concentrate, 4.3 kg water, and 25.8 kg HMDSO, was prepared by diluting the PEDS sol concentrate with ethanol and HMDSO in a stirred reactor preheated to 45° C. The diluted ethanol ammonia solution was then added and the thus activated sol was transferred via a transfer line, under equalization of pressure, to a tube bundle reactor preheated to 60° C. with both lids closed. After transferring the sol, the top and bottom valves to the reactor were also closed, so that the heat exchange tubes were isolated in the tightly closed reactor along with the formed gel rods.
[0087] The temperature of the reactor was then increased to 112°C by heating the heat exchange medium. The pressure rose rapidly to a value of 2.5 bar. After an aging time of 60 minutes, the top and bottom valves were carefully opened to discharge the synthesis fluid into the discharger. Now the heating of the tube bundle heat exchanger was reduced to 102°C. Now 18.5 l of a diluted sulfuric acid in ethanol solution, mixed in a stirred batch reactor and preheated to 60°C, was injected into the reactor and circulated at a constant flow of 4 l / min. The hydrophobization catalyst was then injected at the same temperature for another 75 minutes.
[0088] Once hydrophobization was complete, the reactor was immediately cooled to a temperature of 73° C. and vented to ambient pressure. The bottom lid of the reactor was opened and the resulting hydrophobized gel bar was separated from the liquid phase by a phase separation unit and transferred to a drying unit where the gel was dried to constant weight under nitrogen flow at 160° C. After the drying unit, the aerogel granules were sent through a heated tunnel containing an atmosphere of 1.1 vol.% ammonia and 350 mbar water vapor with a residence time of 17 minutes. At the end of this tunnel, the final aerogel material was removed via a load lock device.
[0089] Analysis of the material reveals a density of 0.108 g / cm 3 An envelope density of 1.0 μm and a layer thermal conductivity of 17.9 mW / (mK) were demonstrated. Other chemical data for the aerogel are summarized in Table 1.
[0090] [Table 1]
[0091] Envelope density was measured by powder pycnometry using a GeoPyc 1360 instrument (Micromeritics).
[0092] As described in WJ Malfait et al., Chem. Mater. 2015, Vol. 27, pp. 6737-6745, the amount of trimethylsiloxyl (≡SiOSiMe3) groups and alkoxysilyl (≡SiOR) groups is 1 The amount of silanol (≡SiOH) groups was measured by H-NMR. 29 Measurements were performed by Si-NMR.
Claims
1. 1. A method for producing a hydrophobized silica aerogel, comprising the steps of: a) preparing a hydrophobized silica gel containing an alkoxy group; b) drying the hydrophobized silica gel obtained in step a); c) hydrolyzing the alkoxy groups of the product obtained in step b) with a gas mixture containing water and a base or acid; Including, A process wherein said step c) is carried out at a temperature of 50-250° C., the duration of said step c) is 1-1000 minutes, and in said step c) the molar ratio of water to base or acid is at least 4.
2. The alkoxy group is methoxy (OCH 3 ), ethoxy (OC 2 H 5 ), propoxy (OC 3 H 7 ), butoxy (OC 4 H 9 2. The method of claim 1, wherein the alkyl alkoxy group is selected from the group consisting of aryl, aryloxy ...
3. 3. The method according to claim 1 or 2, wherein the hydrophobized silica gel of step a) is obtained by hydrolysis of an organosilicate selected from the group consisting of tetraethyl orthosilicate (TEOS), tetramethyl orthosilicate (TMOS), tetraisopropyl orthosilicate (TPOS), and mixtures or oligomers thereof.
4. 3. The method according to claim 1 or 2, wherein step a) comprises gelling an inorganic precursor selected from the group consisting of sodium silicate, water glass, ion-exchanged water glass, silicic acid or colloidal silica, and mixtures thereof.
5. The method according to claim 1, wherein step a) is carried out using a hydrophobizing agent activatable by an acid catalyst selected from the group consisting of hydrogen chloride, nitric acid, sulfuric acid, trimethylchlorosilane, and mixtures thereof.
6. The method of claim 1, wherein step a) is carried out using an acid-catalyst-activatable hydrophobizing agent selected from the group consisting of hexamethyldisiloxane, trimethylethoxysilane, trimethylmethoxysilane, and mixtures thereof.
7. The method according to claim 1 or 2, wherein the step a) comprises the steps of: a1) preparing a mixture containing a silica sol; a2) gelling the mixture to obtain a silica gel; and a3) hydrophobizing the silica gel to obtain a hydrophobized silica gel.
8. The method according to claim 7, further comprising, prior to step a3), a step of aging the silica gel obtained in step a2) in the presence of a base catalyst selected from the group consisting of ammonia, ammonium fluoride, aminosilanes, and mixtures thereof.
9. 9. The method according to claim 1, wherein step b) is carried out under subcritical conditions.
10. 10. The process according to any one of claims 1 to 9, wherein the base used in process step c) is selected from the group consisting of ammonia, lower aliphatic alkylamines, and mixtures thereof.
11. The acid used in step c) of the method is hydrochloric acid (HCl), hydrofluoric acid (HF), hydrobromic acid (HBr), hydroiodic acid (HI), nitric acid (HNO 3 11. The method of any one of claims 1 to 10, wherein the organic solvent is selected from the group consisting of volatile mineral acids such as volatile organic compounds, carboxylic acids such as formic acid and acetic acid, halosilanes such as trimethylchlorosilane, and mixtures thereof.
12. Trimethylsiloxyl (≡SiOSiMe 3 ) groups, alkoxysilyl (≡SiOR) groups, and silanol (≡SiOH) groups, Maximum 0.17 g / cm 3 The envelope density of The ratio of trimethylsiloxyl groups (≡SiOSiMe) to the total amount of trimethylsiloxyl groups, alkoxysilyl groups, and silanol groups 3 ) the ratio of the amount N SiOSiMe3 / (N SiOSiMe3 +N SiOR +N SiOH ) is greater than 0.5, and Ratio N of the amount of alkoxysilane groups to the total amount of alkoxysilane groups and silanol groups SiOR / (N SiOR +N SiOH ) is between 0.05 and 0.30 It is characterized by: R is an alkyl group; Trimethylsiloxyl (≡SiOSiMe 3 The amount of alkoxysilyl (≡SiOR) groups is 1 The amount of silanol (≡SiOH) groups was measured by H-NMR. 29 Silica aerogel as measured by Si-NMR.
13. 13. Use of the silica aerogel according to claim 12 for thermal and / or acoustic insulation.
14. As a bulk material for thermal insulation and / or sound insulation materials, such as insulating containers, or pasty formulations such as plaster, mortar, and concrete formulations, or thermal insulation and / or sound insulation coatings; As energy-saving thermal insulation coatings in industrial applications or As components and films of insulating textile products for lightweight building construction applications; Use of the silica aerogel according to claim 13.
15. A heat insulating and / or sound insulating composition comprising the silica aerogel according to claim 12.
Citation Information
Patent Citations
Method for the production of an aerogel material
JP2016530199A
Ammonia containing silica-and-organo-silica-aerogel thickening agents and their preparation
US3562177A
Preparation of high porosity xerogels by chemical surface modification.
US5565142A
Method of preparing silica aerogel granules
WO2012044052A2
Process for manufacturing xerogels
WO2013053951A1