Methods for optimizing the property profile of solid substrate precursors

The method optimizes the production of TiO2-SiO2 mixed glass substrate precursors by dividing and homogenizing glass bodies to minimize macroscopic titanium profiles and layered structures, ensuring high numerical aperture and homogeneity for EUV lithography.

JP7577798B2Active Publication Date: 2024-11-05HERAEUS QUARZGLAS GMBH & CO KG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023114095
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-07-22
Filing Date
2023-07-11
Publication Date
2024-11-05
Estimated Expiration
2043-07-11

AI Technical Summary

Technical Problem

Existing methods for producing TiO2-SiO2 mixed glass substrates for EUV lithography face challenges in achieving high numerical aperture and reducing macroscopic titanium profiles and layered structures, especially in large-scale production, which affect the quality and homogeneity of the substrate precursors.

Method used

A method involving the production of a TiO2-SiO2 mixed glass substrate precursor by introducing silicon dioxide and titanium dioxide raw materials into a flame, forming a glass body, dividing it into rod-shaped parts, measuring and optimizing the titanium distribution, and undergoing homogenization processes to minimize macroscopic titanium profiles and layered structures, ensuring a high numerical aperture and homogeneity.

Benefits of technology

The method produces substrate precursors with a mass of over 50 kg that are substantially free of layered structures, achieving a high numerical aperture and improved homogeneity, suitable for EUV lithography applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577798000001
    Figure 0007577798000001
  • Figure 0007577798000002
    Figure 0007577798000002
  • Figure 0007577798000003
    Figure 0007577798000003
Patent Text Reader

Abstract

To provide a method for manufacturing a substrate precursor capable of reducing the influence of a property profile relevant to macroscopic manufacturing.SOLUTION: A method for manufacturing a substrate precursor having a mass of more than 100 Kg and including TiO2-SiO2 mixed glass comprises the steps of: introducing a silica dioxide raw material and a titanium dioxide raw material into a flame 225; manufacturing a layer structure relevant to microscopic manufacturing; dividing a glass body; measuring a titanium profile; forming a glass component; homogenizing the glass component; manufacturing a spherical glass system; rotating the spherical glass system; extending the spherical glass system to form a glass component; homogenizing the glass component to manufacture a substrate precursor without substantially including the layer structure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a TiO 2 -SiO 2 A method for producing a substrate precursor comprising a mixed glass. [Background technology]

[0002] EP 2 960 219 A1 describes that in EUV lithography, highly integrated structures with line widths of less than 50 nm are produced by microlithographic projection devices. Typically, operating radiation from the spectral range of 10 nm to 121 nm, referred to as the EUV range (extreme ultraviolet light, also known as "soft x-ray radiation"), is used.

[0003] The projection device is made of synthetic high-silica quartz glass doped with titanium dioxide (hereafter referred to as TiO 2 -SiO 2 Mixed Glass" or "TiO 2 -SiO 2 The mirror element is made essentially of TiO (also called "glass") and is provided with a reflective layer system. 2 -SiO 2 The mixed glasses are characterized by an extremely low coefficient of thermal expansion (CTE), a glass property that depends primarily on the titanium dioxide concentration, although it also depends on the thermal history of the glass and on several other parameters.

[0004] TiO 2 -SiO 2 The mixed glass substrate precursor is mechanically processed to form the mirror substrate and mirrored to form the mirror element.

[0005] As a result of the ever-increasing demands on the line widths to be achieved, TiO 2 -SiO 2The demands on mixed glasses are also increasing. To achieve smaller line widths, the EUV source power is frequently increased. This increase in EUV power first leads to a higher throughput of the stepper, but also to a greater heating of the mirrors. As a result, more homogeneous and better defined mirrors are required, since imaging errors increase with source power.

[0006] Furthermore, smaller structure widths require better imaging properties themselves. In this case the numerical aperture is particularly important. The optical aperture angle of the objective mirror is directly related to the optical resolution. A higher numerical aperture (i.e. a higher beam angle) allows for better resolution. However, this requires a larger mirror substrate. Summary of the Invention [Problem to be solved by the invention]

[0007] For manufacturing reasons, TiO 2 -SiO 2 Mixed glass contains a microscopic layer structure. JP 2006-240979(A) describes a method for reducing this layer structure. It has been found that in the production of substrate precursors with a desired mass of more than 100 kg, in addition to the layer structure associated with the microscopic production, a titanium profile associated with the macroscopic production also occurs, which is disadvantageous. This titanium profile associated with the production affects the quality of the final substrate precursor and is not eliminated by known methods.

[0008] technical challenges In general, the object of the present invention is to at least partially overcome the drawbacks arising from the prior art. Another object of the present invention is to provide a substrate precursor with reduced impact of titanium profile associated with macroscopic manufacturing. Also, the object of the present invention is to provide a substrate precursor with reduced impact of property profile associated with macroscopic manufacturing. Also, the object of the present invention is to provide a substrate precursor with a mass of more than 50 kg, in particular more than 100 kg, thereby achieving a high numerical aperture.

[0009] Preferred embodiments of the invention The features of the independent claims contribute to at least partially achieving at least one of the aforementioned objects. The dependent claims provide preferred embodiments which contribute to at least partially achieving at least one of the objects. |1.| Having a mass of more than 50 kg and TiO 2 -SiO 2 A method of manufacturing a substrate precursor (900) comprising a mixed glass, the method comprising: introducing (1000) a silicon dioxide source and a titanium dioxide source into a flame (225); A step (1100) of producing a glass body (300) having a titanium dioxide content of 3% by weight to a maximum of 10% by weight, the glass body (300) comprising: Titanium profiles related to macroscopic manufacturing (410, 410', 410'', 410'''), and -Layer structures related to microscopic manufacturing, A manufacturing step (1100) including: Dividing (1200) the glass body into a plurality of rod-shaped glass body portions (400, 400', 400'', 400'''); a step (1300) of spatially measuring the titanium profile (410, 410', 410'', 410''') in each of the glass body portions (400, 400', 400'', 400'''); connecting (1500) the glass body portions (400, 400', 400'', 400''') to form an elongated first glass component (600); a step (1600) of a first homogenization treatment of the first glass component (600); Pressing (1700) first glass components (600) together to create a spherical glass system (700); rotating the glass system (700) by more than 70 degrees (1800); - drawing (1900) the glass system (700) to form an elongated second glass component (800); subjecting the second glass component (800) to a second homogenization treatment (2000) to produce a substrate precursor substantially free of layer structures; Including, The measuring step comprises: predetermining (1400) a desired spatial titanium distribution (420) in a substrate precursor; Providing (1420) a model of titanium distribution (430) in a substrate precursor, the model comprising: - positioning the glass body portions (400, 400', 400'', 400''') relative to one another in the first glass component (600); - spatial titanium profiles (410, 410', 410'', 410''') in each of the glass body portions (400, 400', 400'', 400'''); and The effect of the pressing step (1700) and the rotating step (1800) on the spatial titanium profile (410, 410', 410'', 410''') in the glass body portion; providing (1420), which is dependent on calculating (1450) the optimal arrangement of the glass body portions (400, 400', 400'', 400'') relative to one another using the model such that the difference between the titanium allocation (430) and the titanium distribution (420) is minimized; a step of positioning (1470) the glass body portions (400, 400', 400'', 400''') such that in a connecting step (1500), the glass body portions (400, 400', 400'', 400''') are connected according to a calculated optimal arrangement; A method comprising: |2.| The method according to embodiment 1, characterized in that the substrate precursor has a mass of more than 100 kg, in particular more than 200 kg, in particular more than 300 kg. |3.| A step of producing a second glass body having a titanium dioxide content of 3% by weight to a maximum of 10% by weight, the second glass body being A titanium profile associated with the second macroscopic production, and - A layer structure related to the second microscopic manufacturing, and Dividing the second glass body into a plurality of rod-shaped glass body portions; 3. The method according to at least one of embodiments 1 or 2, comprising: |4.|The method according to at least one of embodiments 1 to 3, characterized in that at least three, in particular at least five, in particular at least eight glass body parts are connected to form a first glass component. |5.|The method according to at least one of the preceding embodiments, characterized in that the difference between the titanium allocation (430) and the titanium distribution (420) is less than 1.5%, in particular less than 1.0%, in particular less than 0.5%, based on the maximum value of the titanium distribution (420). |6.| The glass body has the following property profile: • OH profiles related to macroscopic production, • Macroscopic manufacturing-related CTE profiles, • Fluorine profiles related to macroscopic production; - bubble profiles related to macroscopic manufacturing, ●ODC profile related to macroscopic manufacturing, ●Ti3+ profile related to macroscopic manufacturing, • Macroscopic production-related metal impurity profiles; The method according to at least one of the preceding embodiments, comprising at least one of the following: |7.|The method of embodiment 6, characterized in that in the measuring step, at least one of the characteristic profiles is measured in each of the glass body portions. |8.|The measuring step is predetermining a desired spatial property distribution in a substrate precursor; providing a model of property distribution in a substrate precursor, the model comprising: - Arrangement of the glass body portions relative to one another in the first glass component; - spatial property profiles in each of the glass body portions; and The effect of the pressing and rotating steps on the spatial property profile in the glass body portion; Depends on,step,and, calculating the best possible arrangement of the glass body portions relative to one another by means of the model so that the sum of the differences is minimized, the sum of the differences being: The difference between titanium allocation and titanium distribution, and The second difference between property allocation and property distribution, and positioning the glass body parts so that in the connecting step, the glass body parts are connected according to a calculated best possible arrangement; 8. The method of embodiment 7, comprising: The method according to embodiment 8, characterized in that the sum of the differences is less than 1.5%, in particular less than 1.0%, in particular less than 0.5%, based on the sum of the maximum of the titanium distribution (420) and the maximum of the property distribution. |10.| The steps of producing a glass body include at least: Producing a porous soot body, a macroscopic manufacturing-related titanium profile extending substantially along a longitudinal axis, and a microscopic process-related layer structure extending substantially along a growth axis; - vitrifying the soot body to produce a cylindrical glass body; 10. The method according to at least one of embodiments 1 to 9, comprising: 11. The method according to at least one of the preceding claims, wherein the first glass component is heated prior to the pressing step. |12.|The method according to at least one of the preceding embodiments 1 to 11, characterized in that the connection is made at the relevant contact surfaces of the glass body parts.

[0010] In this specification, range specifications also include the values ​​specified as limits. A specification of the type "in the range from X to Y" for a variable A consequently means that A can take on values ​​X, Y, and between X and Y. Thus, a one-sided range of the type "up to Y" for a variable A implies values ​​Y and less than Y.

[0011] Some of the described features relate to the term "substantially". The term "substantially" should be understood in the sense that under practical conditions and manufacturing techniques, a mathematically precise interpretation of terms such as "overlap", "perpendicular", "diameter" or "parallelism" can never be given exactly, but only within the error tolerance associated with a particular manufacturing. In particular, the term "substantially" may mean a variation of + / - 5% of the relevant value. In particular, "substantially parallel axes" includes angles between -5 degrees and 5 degrees relative to each other, and "substantially equal volumes" includes deviations of up to 5% by volume. "Devices substantially made of quartz glass" includes, for example, a quartz glass content of 95% by weight or more and 100% by weight or less. Furthermore, "substantially perpendicular" includes angles between 85 degrees and 95 degrees. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention relates to a method for producing a TiO 2 -SiO 2 1. A method of making a substrate precursor comprising a mixed glass, comprising: Introducing a silicon dioxide raw material and a titanium dioxide raw material into a flame; A step of producing a glass body having a titanium dioxide content of 3% by weight to a maximum of 10% by weight, the glass body being ○ Titanium profiles related to macroscopic manufacturing, and ○Layer structures related to microscopic manufacturing, and Dividing the glass body into a plurality of rod-shaped glass body portions; spatially measuring the titanium profile in each of the glass body portions; connecting the glass body portions to form an elongated first glass component; a step of a first homogenization treatment of the first glass component; - pressing the first glass components together to create a spherical glass system; Rotating the glass system by more than 70 degrees; - drawing the glass system to form an elongated second glass component; subjecting the second glass component to a second homogenization process to produce a substrate precursor that is substantially free of layer structures; The present invention relates to a method comprising the steps of:

[0013] In order to overcome the above-mentioned shortcomings in the prior art, according to the present invention, the measuring step includes: predetermining a desired spatial titanium distribution in a substrate precursor; Providing a model of titanium distribution in a substrate precursor, the model comprising: the arrangement of the glass body portions relative to one another in the first glass component; the spatial titanium profile in each of the glass body portions, and The effect of the pressing and rolling steps on the spatial titanium profile in the glass body portion; providing a step of: Using the model to calculate the optimal arrangement of the glass body portions relative to each other such that the difference between the titanium allocation and the titanium distribution is minimized; positioning the glass body portions such that the glass body portions are connected according to a calculated optimal arrangement in the connecting step; It is provided that the present invention includes:

[0014] The scope of the described method relates to the optimization of the spatial distribution of titanium dioxide, in particular titanium dioxide and at least one other property, in a substrate precursor. For linguistic reasons, the terms "titanium" and "titanium dioxide" are used synonymously in the following. In fact, the present invention and the specified does not relate to elemental titanium, but to titanium dioxide in its oxidized form. Furthermore, the following words and endings are used to describe the spatial distribution of titanium dioxide and / or at least one other physical or chemical property at different stages of the method: - In the glass body and glass body part, the word "profile" In substrate precursors, the word "frequency" In the model, the word "allocation" and - In the desired substrate precursor, the term "distribution."

[0015] In this respect, by way of example, the titanium profile differs from the titanium frequency in the following ways: First, it shows the titanium dioxide content at different spatial points in the glass body, and • Second, it shows the titanium dioxide content at spatially different points within the substrate precursor.

[0016] The method allows the manufacture of substrate precursors with a mass of more than 50 kg, in particular more than 100 kg, which meets the steadily increasing demand for EUV mirror elements. In this case, the method comprises the following steps: introduction In the introducing step, a silicon dioxide source (e.g., SiCl4 or OMCTS vapor) and a titanium dioxide source (e.g., TiCl4 or Ti alkoxide vapor) are subjected to flame hydrolysis. In this process, SiO 2 and TiO 2 Particles are formed.

[0017] manufacturing SiO formed within the flame hydrolysis 2 and TiO 2The particles can be deposited in two ways. In direct deposition (DQ process), the deposition is carried out on a stamp placed under a flame. In general, the temperature conditions are such that this deposition is carried out and a dense TiO 2 -SiO 2 The mixed glass is formed by vapor-phase deposition (VAD) of SiO on a carrier bar. 2 and TiO 2 The deposition takes place in the form of a film of particles. In a second step, the particles are then vitrified to form TiO 2 -SiO 2 A mixed glass is formed.

[0018] This step results in 3 weight percent (wt%) up to 10 weight percent (wt%) of TiO 2 This results in a glass body having a titanium dioxide content of SiO 2 and TiO 2 This includes microscopic manufacturing-related layer structures, also called short-wave layer structures, which result from layer-by-layer deposition of particles.

[0019] The masses given here and hereafter are always TiO 2 This relates to the amount of (titanium dioxide) and not to the element titanium.

[0020] Due to fluctuations in mass flow controllers (MFC), mechanical inaccuracies of the burner or the holder of the burner and deposition system, or stochastically and / or deterministically changing thermal boundary conditions during construction, the glass body has a weight of more than 50 kg, in particular more than 100 kg, in particular more than 200 kg, and in addition to the layer structure related to the described microscopic production, also contains a titanium profile related to the macroscopic production. The short-wave layer structure has a size of less than 1 mm, in particular less than 0.5 mm.

[0021] This macroscopic titanium profile, also called long-wave variation or long-wave titanium profile, has a specific variation length of 0.15 m to 0.75 m, in particular 0.17 m to 0.5 m, in which the titanium dioxide content varies by up to 0.5% by weight, in particular up to 0.3% by weight, in particular 0.02% by weight to 0.25% by weight, in particular 0.05% by weight to 0.2% by weight. In an exemplary glass body having a length of 1 meter, a titanium dioxide content of 10% by weight, and a macroscopic manufacturing-related variation of + / - 0.5% by weight, the titanium dioxide content may therefore vary spatially several times, in particular between 10.5% by weight and 9.5% by weight.

[0022] Split The glass body produced in the manufacturing step can have a cylindrical, rod-like or tubular shape. Along a given longitudinal axis, the glass body is divided into a plurality of rod-like glass body portions.

[0023] measurement In the measuring step, the titanium dioxide content is determined at a number of spatially different points. For example, an individual titanium profile is determined for each of the glass body parts produced in the dividing step. For this purpose, the titanium dioxide content and / or properties are measured along the longitudinal axis of the glass body part. In this case, the measuring points are at a distance of less than 5 cm, in particular less than 2 cm, from each other. The measurement accuracy in determining the titanium dioxide content is 0.005% by weight.

[0024] connection A number of glass body parts are connected to one another in a connecting step to form an elongated first glass component. In this case, the connection can be made in particular in a manner that is integrally joined within the scope of a hot process. The term "hot process" is understood to mean a method step in which the temperature of the element is increased by heat input. Examples of hot processes: - Flame-based hot processes are based on the oxidation of exothermic reactant gases. One example is the use of hydrogen (also called "H2") as fuel gas (flame hydrolysis), which reacts with oxygen (also called "O2") from the air. - Flameless hot processes use other heating systems that do not require an open flame. One example is the use of resistors to convert electrical energy into thermal energy (heat).

[0025] First homogenization process In the first homogenization treatment, the shortwave microscopic layer structure of the first glass component is removed in one plane in a crucible-free melting process. For this purpose, the first glass component can be fixed in the chuck of a glass lathe and softened zone by zone while the chuck rotates at different speeds or in a counter-rotating manner around the axis of rotation. Due to the different rotations of the first glass component on either side of the softening zone, torsion (twisting) and therefore mechanical intermixing occurs there in the glass volume. The zone of thermo-mechanical intermixing is also called the "shear zone". The shear zone has a length of 2 cm to 8 cm, which is more than an order of magnitude longer than the length of the shortwave layer structure, which has a length of less than 1 mm. The shear zone is moved along the longitudinal axis of the first glass component and is intermixed over its length during the process. Thus, the layer structure associated with the microscopic manufacture is reduced or eliminated in one plane, in particular in the plane of the shear zone.

[0026] TiO that has passed homogenization treatment 2 -SiO 2 When the mixed glass is examined by voltage detectors and interferometers, it is found that the optical layer structure degrees of freedom parallel to the plane of the shear bands used during homogenization are less than the layer structure degrees of freedom observed perpendicular to the plane of the shear bands, indicating that the mixing effect used within the shear bands and serving to achieve the layer structure degrees of freedom is less perpendicular to the rotation axis used during the homogenization process than is observed along the rotation axis.

[0027] Push together After the first homogenization process, the first glass component is heated and mechanically pressed together, creating a spherical glass system by pressing the two ends together along the longitudinal axis of the first glass component.

[0028] rotate Relative to the longitudinal axis of the first glass component, the spherical glass system is rotated by more than 70°. The angle of rotation may in particular be between 70° and 110°, in particular between 80° and 100°.

[0029] stretching After rotation, the glass system is heated to allow longitudinal elongation, which allows the spherical glass system to be reshaped into an elongated, in particular rod-shaped, second glass component.

[0030] Second homogenization process A second homogenization of the second glass component is performed to remove the remaining microscopic manufacturing-related layer structure. The second homogenization is performed similarly to the first homogenization. For this purpose, the second glass component can be fixed in the chuck of a glass lathe and softened zone by zone while the chuck rotates at different speeds or in a counter-rotating manner around the axis of rotation. Due to the different rotations of the second glass component on either side of the softening zone, twisting (twisting) and therefore mechanical intermixing occurs again in the glass volume. The shear bands are moved along a second length of the second glass component, and in this process the second glass component is reshaped and intermixed over its length. Thus, the microscopic manufacturing-related layer structure is reduced or eliminated in one plane, in particular in the plane of the shear bands.

[0031] TiO that passed both homogenization processes 2 -SiO 2 Inspection of the mixed glass with a voltage detector and an interferometer shows that the microscopic manufacturing related layer structures are substantially eliminated, particularly in comparison to the glass body, by at least 99%.

[0032] As a result of the second homogenization treatment of the second glass component, a substrate precursor is produced that is substantially free of microscopic manufacturing related layer structures.

[0033] In one embodiment, the first glass component and / or the second glass component are fixed in a rotation device with their longitudinal axes oriented horizontally, and retention elements to minimize loss of good material can be welded to the ends of the first glass component and / or the second glass component.

[0034] Measurement according to the present invention: In order to overcome the above-mentioned shortcomings in the prior art, the measuring steps include: predetermining a desired spatial titanium distribution in a substrate precursor; Providing a model of titanium distribution in a substrate precursor, the model comprising: the arrangement of the glass body portions relative to one another in the first glass component; the spatial titanium profile in each of the glass body portions, and The effect of the pressing and rolling steps on the spatial titanium profile in the glass body portion; providing a step of: Using the model to calculate the optimal arrangement of the glass body portions relative to each other such that the difference between the titanium allocation and the titanium distribution is minimized; positioning the glass body portions such that the glass body portions are connected according to a calculated optimal arrangement in the connecting step; It is provided that the present invention includes:

[0035] Within the scope of calculating the optimal arrangement, the positions of the glass body parts relative to each other are permuted. From each permutation, the model calculates a titanium distribution, which is then compared to the titanium distribution by difference formation. From this set of differences, it is then possible to determine the optimal arrangement of the glass body parts relative to each other in which the difference between the titanium distribution and the titanium distribution, particularly the spatial difference, is minimal.

[0036] To decide in advance Within the predetermined step, SiO 2An optimal spatial distribution of titanium dioxide in the matrix is ​​determined, which is the target value for the spatial distribution of titanium in the substrate precursor and should be optimally achieved during manufacture.

[0037] Titanium distribution includes both the absolute amount of titanium dioxide in the substrate precursor and its spatial distribution. As an example, the substrate precursor may have a cubic shape. In this case, the titanium distribution may be arranged in a parabolic manner, with the maximum portion of the titanium distribution being located at the center of the surface of the substrate precursor. Furthermore, different edge regions of the substrate precursor may have the same or different titanium distributions. In a further embodiment, the titanium distribution may be arranged to be flat, i.e., uniform, across the substrate precursor.

[0038] offer The method according to the present invention involves the use of a model of titanium distribution in a substrate precursor. 2 Calculate the spatial distribution of titanium dioxide in a matrix. In this case, the following are used as input parameters of the model: A / Arrangement of the glass body portions relative to each other in the first glass component B / Individual spatial titanium profiles in multiple vitreous body sections, and C / Effect of pressing and rolling steps on the spatial titanium profile in the glass body part.

[0039] SiO based on the above input parameters 2 In calculating the spatial distribution of titanium dioxide in the matrix, the model can take further aspects into account.

[0040] In the manufacture of glass bodies, SiO 2Long-wave and short-wave variations in the amount of titanium in the matrix and / or other properties occur. The two types are affected differently in the method steps of the method disclosed herein. Using the model, the titanium distribution for multiple arrangements of glass body parts can be calculated and compared with a target value in the connecting step. Thus, the required quality of large substrate precursor can be achieved and waste can be reduced.

[0041] The starting point is that both the first and the second homogenization treatments act only on the shortwave (microscopic) layer structure and / or the shortwave (microscopic) changes in the titanium dioxide content. In contrast, the longwave changes in the titanium dioxide content remain unaffected by the two homogenization treatments. This fact is due to the different length scales of the shear bands and the titanium profile related to the macroscopic production. The shear bands have an elongated extent of only a few centimeters. Within this shear band, only the shortwave structures located in the plane of the shear band are corrected.

[0042] The long wave variations in titanium dioxide content are unaffected by the two homogenization treatments because the length of the variations in long wave variations in titanium dioxide content and / or properties is at least twice the width of the shear band.

[0043] The rotating step does not affect the shortwave (microscopic) layer structure of the titanium dioxide and / or the shortwave (microscopic) variations in the titanium dioxide content. However, the rotating step ensures that the shear bands of the first and second homogenization treatments are arranged substantially perpendicular to each other with respect to the longitudinal axis of the first glass component. As a result, the shortwave variations are smoothed out as completely as possible.

[0044] The rotating step affects the long-wave fluctuations. By pressing the first glass components together in the pressing step, the different long-wave fluctuations from the different glass body parts are mixed together. The removed volume elements of the first glass components are brought into direct proximity by the process and can be combined in the next step. As a result, depending in particular on the titanium profile and / or the property profile, it is possible to reach an amplification or attenuation of the fluctuation level of the long-wave fluctuations. Thus, the amplification or attenuation of the fluctuation level depends on the titanium profile and / or the property profile, as well as on the arrangement of the individual glass body parts relative to each other.

[0045] Finally, the glass body portions are again arranged on different planes of the substrate precursor, the number of planes depending on the mass of the substrate precursor and the number and mass of the glass body portions. For substrate precursors with a mass greater than 50 kg, the number of planes may be 2-5. For substrate precursors with a mass of more than 100 kg, the number of planes can be 3-10. For substrate precursors with a mass of more than 200 kg, the number of planes can be 5-20. For substrate precursors with a mass of more than 300 kg, the number of planes can be 10-30.

[0046] An exception to the statement that the rotating step affects the long-wavelength variations applies to the macroscopic quartz glass volume elements that are located in the center of the elongated first glass component and that are in particular between 20 cm3 and 100 cm3 in size. SiO 2 The long-wave variations of the properties, such as the amount of titanium in the matrix, are also found again in this macroscopic volume element. The rotating step only changes the position of this volume element so that it is again located at the center of the spherical glass system. During the subsequent elongation, this volume element is again located at the center of the elongated second glass component. As a result, the volume element with its long-wave variations, which are not affected by the homogenization, is again located at the center of the second glass component.

[0047] In a further embodiment, the second homogenization step is followed by a step of flowing into a graphite mold. After the step of flowing, the described quartz glass element is located in the center of the substrate precursor and therefore substantially determines its behavior. This is all the more true since a convex recess that receives the actual mirror is often ground into the substrate precursor, and therefore the volume element located directly below the recess significantly influences the behavior of the mirror during use.

[0048] As a result, the model can take into account at least one of the following aspects in order to search for optimum conditions in which the following aspects are minimal and / or optimal: D / the titanium dioxide content in the functional area, in particular in the central volume element of the substrate precursor, and E / Titanium dioxide content in different planes of the substrate precursor.

[0049] The model, which depends on at least the three listed input parameters A / ~C / , is a SiO2 model of the substrate precursor that may be obtained during the process steps. 2 The spatial distribution of titanium dioxide in the matrix is ​​calculated, resulting in the following: Different arrangements of the glass body portions relative to one another in the first glass component; and / or Selection of multiple glass body portions from a larger number of glass body portions combined with different arrangements of the multiple glass body portions relative to one another in the first glass component.

[0050] calculation Using the model, the possible titanium distribution in the substrate precursor calculated by permuting the arrangement of the glass body portions relative to one another is compared to the desired titanium distribution in the substrate precursor. Since the titanium distribution represents a desired target value, the arrangement of the glass body portions that has the smallest difference between the titanium distribution and the titanium distribution is selected.

[0051] As explained, the titanium profile is determined at the points in the spatial measurement step. In one variant, the model determines only a series of points, but does not determine the complete curve of the titanium distribution. According to the invention, in each case, the difference is calculated for each possible permutation of the arrangement of the glass body parts.

[0052] In one embodiment, the difference between the series of numbers is determined by root mean square (RMS).The model then checks which of all possible permutations of the arrangement of the glass body parts results in the smallest difference, i.e., the difference with the smallest magnitude.Then, the arrangement of the glass body parts with the smallest calculated difference between the titanium distribution and the titanium distribution is used in the connecting step.

[0053] In one embodiment, the difference between the series of numbers is determined by the sum of the magnitudes of the differences.

[0054] In one embodiment, the difference between the series of numbers is determined by an arithmetic mean.

[0055] In one embodiment, a minimum difference is understood to mean that the difference between the magnitude of the titanium allocation and the magnitude of the titanium distribution is less than 1.5%, in particular less than 1.0%, in particular less than 0.5% of the maximum value of the titanium distribution. The specified magnitude of the difference is therefore a relative value based on the maximum value of the titanium distribution.

[0056] In one embodiment, at least 75%, in particular at least 85%, in particular at least 90% of the surface of the substrate precursor is taken into account to determine the difference.

[0057] In one embodiment, for determining the difference, at least 75%, in particular at least 85%, in particular at least 90% of the surface of the substrate precursor, which will be mirrored in a further step to form the mirror elements, is taken into account.

[0058] Positioning The desired substrate precursor is then achieved by connecting the glass body parts in a connecting step according to the calculated optimal arrangement.

[0059] An embodiment is characterized in that the substrate precursor has a mass of more than 200 kg, in particular more than 300 kg. Within the scope of the OVD or DQ method, the titanium profile relevant for macroscopic production is 200 kg of TiO 2 -SiO 2 Based on the desired titanium dioxide content in the mixed glass, the spatial variation of titanium dioxide content can be up to 0.5%. The spatial variation of titanium dioxide content generally has a continuous profile, with a variation length of 10 cm to 50 cm. In contrast, TiO 2 -SiO 2 The shear zone in which the mixed glass is mixed within the two homogenization processes and the second shear zone have a length of 2 cm to 8 cm.

[0060] For substrate precursors with a mass of more than 100 kg, in particular more than 200 kg, in particular more than 300 kg, the first glass component has a length of more than 2 m, in particular more than 2.8 m. As a result, multiple macroscopic manufacturing-related variations in the titanium profile may occur, which do not have an impact in the case of smaller substrate precursors with a mass of less than 30 kg. One embodiment is characterized in that the method comprises the following steps after the second homogenization treatment: • softening the second glass component and reshaping the second glass component by flowing under the action of a force and pouring it into a heated mold to form a substrate precursor.

[0061] In one embodiment, the flowing step specifically comprises flowing out rod-like TiO in the second glass component. 2 -SiO 2 It can serve to convert the mixed glass into a block-shaped substrate precursor. For this purpose, the mold can have a block-shaped interior, in which the TiO of the second glass component is deposited. 2 -SiO 2The mixed glass is allowed to flow. In particular, the mold can have an interior that corresponds to the desired contour and geometry of the desired mirror, and the substrate precursor does not require any significant rework (called "near net shape").

[0062] Within the step of allowing to flow, the second glass component may be placed in a heated mold, where it may flow under its own weight or under an additional force acting in the axial direction. Instead of a slow flow in the heated mold, the second glass component may also be continuously fed into a heated zone, where the same deformation is achieved, in that the mold placed in the heated area is softened over its length.

[0063] In one embodiment, a method comprises: A step of producing a second glass body having a titanium dioxide content of 3% by weight to a maximum of 10% by weight, the second glass body being A titanium profile associated with the second macroscopic production, and ● Including a layer structure related to the second microscopic fabrication, Steps and Dividing the glass body into a plurality of rod-shaped glass body portions; The present invention is characterized by comprising:

[0064] For producing a substrate precursor having a mass of more than 100 kg, in particular more than 200 kg, in particular more than 300 kg, it may be necessary to produce not only a first glass body but also a second glass body.

[0065] In this case, the first and second glass bodies have different macroscopic manufacturing-related titanium profiles. After the manufacturing step, the glass body is divided into a plurality of rod-shaped glass body portions, and the second glass body is divided into a plurality of rod-shaped glass body portions.

[0066] In one embodiment, all of the rod-shaped glass body portions obtained from the first glass body and all of the rod-shaped glass body portions obtained from the second glass body are bonded together to form the first glass component.

[0067] In one embodiment, A plurality of rod-shaped glass body portions obtained from a first glass body; A plurality of rod-shaped glass body portions obtained from a second glass body; The number of glass body portions obtained from the sum of is greater than the number of rod-shaped glass body portions required to make the first glass component. In this case, a selection from the number of available glass body portions for the required number is made within the calculating step so that the difference between the titanium distribution and the titanium distribution is minimized.

[0068] In one embodiment ● Many glass body parts are 1.1 to 2 times larger than the rest, especially The number of glass body portions is at least 20, and the number of glass body portions joined together to form the first glass component is at most 15, and in particular The multiple glass body portions are at least 15 and at most 10 glass body portions that are joined together to form the first glass component.

[0069] The disclosed method may be selected to overcome the aforementioned deficiencies in the prior art.

[0070] One embodiment is characterized in that at least three, in particular at least five, in particular at least eight glass body parts are connected to form the first glass component.

[0071] For substrate precursors with a mass of more than 100 kg, multiple glass body parts connected to each other are required. Due to the variation length of the spatial variation of the titanium dioxide content of 10 cm to 50 cm, the method according to the invention is particularly suitable for combining more than three, especially more than five, especially more than eight glass body parts to produce a substrate precursor that meets the strict requirements of EUV microlithography.

[0072] One embodiment is characterized in that the difference between the titanium allocation and the titanium distribution is less than 1.5%, in particular less than 1.0%, in particular less than 0.5%, based on the maximum value of the titanium distribution.

[0073] Within the measuring step, the minimum difference between the titanium allocation and the titanium distribution is determined by a comparison between the model and the desired titanium distribution. Due to the ever-increasing demands on the material properties of the substrate precursor, the absolute value of the difference may be subject to the aforementioned limitations.

[0074] In one embodiment, the glass body has the following property profile: • OH profiles related to macroscopic production, • Macroscopic manufacturing-related CTE profiles, • Fluorine profiles related to macroscopic production; - bubble profiles related to macroscopic manufacturing, ●ODC profile related to macroscopic manufacturing, ●Ti3+ profile related to macroscopic manufacturing, - a macroscopic production related metal impurity profile.

[0075] In the case of OVD or DQ processes, macroscopic production-related variations of the properties listed above can occur, with lengths comparable to those of titanium dioxide, specifically 12.5 cm to 50 cm for OH, CTE, Ti3+, and 15 cm to 85 cm for fluorine, bubbles, ODC, and metal impurities.

[0076] One embodiment is characterized in that in the measuring step, at least one of the characteristic profiles is measured in each of the glass body portions.

[0077] In one embodiment, the measuring step comprises: predetermining a desired spatial property distribution in a substrate precursor; providing a model of property distribution in a substrate precursor, the model comprising: - Arrangement of the glass body portions relative to one another in the first glass component; - spatial property profiles in each of the glass body portions; and The effect of the pressing and rotating steps on the spatial property profile in the glass body portion; Depends on,step,and, calculating the best possible arrangement of the glass body portions relative to one another by means of the model so that the sum of the differences is minimized, the sum of the differences being The difference between titanium allocation and titanium distribution, and The difference between property allocation and property distribution, and positioning the glass body parts so that in the connecting step, the glass body parts are connected according to a calculated best possible arrangement; The present invention is characterized by comprising:

[0078] In parallel with the step of predetermining the titanium distribution, in this variant at least one desired spatial property distribution in the substrate precursor is predetermined, so that in addition to the titanium distribution, the at least one property distribution represents a second target value that is optimally met and / or sought in the substrate precursor.

[0079] In one variation, the sum of the differences is: The sum of the magnitude of the difference between the titanium allocation and the titanium distribution, and ● The sum of the magnitude of the difference between the property allocation and the property distribution, It can be calculated from:

[0080] Just like the titanium profile, the property profile is also measured at points. The model then calculates in each case the value of the property in the substrate precursor (property distribution) from a set of values ​​for the property. From the set of values, the model can therefore calculate the difference between the property distribution and the property distribution for each possible permutation of the arrangement of the glass body parts.

[0081] Based on that, the model calculates, for each possible permutation of the arrangement of the vitreous body parts, two independent differences, i.e. The difference between titanium allocation and titanium distribution, and The difference between property allocation and property distribution, can be determined.

[0082] In one embodiment, each of the two differences is determined by the root mean square (RMS).In one embodiment, each of the two differences is determined by the arithmetic mean.

[0083] The model then forms a sum of differences for each possible permutation, where the two differences considered can add up to each other in different ways.

[0084] Therefore, the sum of the differences is The sum of the two difference magnitudes to be considered, or The arithmetic or geometric mean of the two differences to be considered, or ● A weighted average of the two differences to be considered, It can be calculated from:

[0085] In one variant, in determining the sum of the differences, the model The difference between titanium allocation and titanium distribution, and The difference between the property allocation and the property distribution, For example, since the amount of titanium dioxide substantially affects the CTE and therefore must be specifically considered for the intended use, the difference between the titanium allocation and the titanium distribution may be considered twice or three times in determining the minimum sum of the differences.

[0086] In one embodiment, the minimum sum of differences is: the difference between the titanium distribution and the titanium distribution over at least 75%, in particular over at least 85%, in particular over at least 90% of the surface of the substrate precursor is less than 1.5%, in particular less than 1.0%, in particular less than 0.5%, based on the maximum value of the titanium distribution; the difference between the property distribution and the property distribution over at least 75%, in particular over at least 85%, in particular over at least 90% of the surface of the substrate precursor is less than 1.5%, in particular less than 1.0%, in particular less than 0.5%, based on the maximum value of the property distribution; is understood to mean.

[0087] In one embodiment, the minimum sum of differences is: the difference between the titanium distribution over at least 75%, in particular over at least 85%, in particular over at least 90% of the surface of the substrate precursor that will be mirrored in a further step to form the mirror element, and the titanium distribution is less than 1.5%, in particular less than 1.0%, in particular less than 0.5% of the maximum titanium distribution; and the difference between the property distribution and the property distribution over at least 75%, in particular over at least 85%, in particular over at least 90% of the surface of the substrate precursor which will be mirrored in a further step to form the mirror element is less than 1.5%, in particular less than 1.0%, in particular less than 0.5% of the maximum value of the property distribution, is understood to mean.

[0088] The model used in this variant is - Arrangement of the glass body portions relative to one another in the first glass component; - spatial titanium profiles and spatial property profiles in each of the glass body portions; and The effect of the pressing and rolling steps on the spatial titanium profile and spatial property profile in the glass body portion; It depends functionally on

[0089] As a result, both aspects related to titanium dioxide and aspects related to at least one additional property (eg, ODC, Ti3+, etc.) are taken into account in calculating the optimal placement of the glass body portion.

[0090] Based on a solution space of possible arrangements of the glass body portions relative to one another, the best possible arrangement of the glass body portions is determined by permutation, where the objective is to minimize the sum of the differences, which is The difference between titanium allocation and titanium distribution, and a second difference between the at least one characteristic allocation and the at least one characteristic distribution; Includes.

[0091] Subsequently, in a connecting step, the glass body parts are positioned so that they are connected according to the calculated best possible arrangement.

[0092] An embodiment is characterized in that the sum of the differences is less than 1.5%, in particular less than 1.0%, in particular less than 0.5% of the sum of the maximum of the titanium distribution and the maximum of the property distribution.

[0093] In one embodiment, the difference between the titanium allocation and the titanium distribution is less than 1.5%, in particular less than 1.0%, in particular less than 0.5% of the maximum titanium distribution; and a second difference between the at least one property allocation and the at least one property distribution is less than 1.5%, in particular less than 1.0%, in particular less than 0.5% of the maximum value of the relevant property distribution; It is characterized by:

[0094] This embodiment is particularly suitable for meeting the high demands on EUV substrate precursors: substrate precursors with differences above the listed values ​​and with second differences often cannot be used to make mirror substrates with deviations from the expected line edges of less than 3 nm.

[0095] In one embodiment, The difference between the titanium allocation and the titanium distribution is 0.15% to 1% of the maximum value of the titanium distribution; and Regarding the second difference, the second difference between the Ti3+ allocation and the Ti3+ distribution is less than 5.0%, in particular less than 2.0%, of the maximum value of the Ti3+ distribution, and the second difference between the OH allocation and the OH distribution is less than 2.0%, in particular less than 1.0%, in particular less than 0.5% of the maximum value of the OH distribution, It is characterized by:

[0096] This embodiment is particularly suitable for producing a substrate precursor capable of producing mirror substrates with deviations from predicted line edges of less than 3 nm.

[0097] In one embodiment, the step of producing the glass body includes at least: Producing a porous soot body, a macroscopic manufacturing related titanium profile extending along a longitudinal axis, and a microscopic process related layer structure extending along a growth axis; - vitrifying the soot body to produce a cylindrical glass body; The present invention is characterized by comprising:

[0098] In one embodiment of the present invention, the steps of preparing a porous soot body include: ● Liquid SiO containing more than 60% by weight of polyalkylsiloxane D4 2 Providing a feedstock; ●Liquid SiO 2 The feedstock is evaporated to produce gaseous SiO 2 a feed vapor; ●Liquid TiO 2 The feedstock was evaporated to produce gaseous TiO 2 a feed vapor; ●SiO 2 Feedstock vapor and TiO 2 The feedstock vapor is SiO 2 Particles and TiO 2 converting the resulting image into particles; ●SiO 2 Particles and TiO 2 depositing particles on a deposition surface to form a porous soot body; Includes.

[0099] Octamethylcyclotetrasiloxane (also referred to herein as D4) forms the major component during the manufacture of the soot body. The manufacture of the soot body by the steps described above reduces the thickness of the titanium dioxide profile and / or the property profile associated with the macroscopic manufacture.

[0100] One embodiment is characterized in that the first glass component is heated prior to the pressing step. By heating, the first glass component becomes at least partially viscous, facilitating mechanical deformation. Heating can be within the scope of flame-based or flameless high temperature processes.

[0101] One embodiment is characterized in that the connection is made on the associated contact surfaces of the glass body parts.

[0102] The features disclosed in this specification may be essential to the various embodiments of the invention claimed, both separately and in any combination with one another.

[0103] The values ​​specified for the difference, sum of differences, and second difference are relative values ​​related to the corresponding distributions, ie, the corresponding amounts desired in the substrate precursor.

[0104] In this specification, embodiments disclosing two or more features, each having preferred ranges or alternatives, are to be understood to include all possible combinations of those features.

[0105] In this specification, range specifications also include the values ​​specified as limits. A specification of the type "in the range from X to Y" for a variable A consequently means that A can take on values ​​X, Y, and values ​​between X and Y. Thus, a unilaterally limited range of the type "up to Y" for a variable A implies values ​​Y and less than Y.

[0106] In the following, the invention will be further explained by way of example and by means of the drawings, to which the invention is not limited. [Brief description of the drawings]

[0107] [Figure 1] FIG. 1 shows the preparation of a soot body. [Diagram 2] FIG. 2 shows the vitrification of a soot body into a glass body. [Diagram 3] FIG. 3 is a glass body. [Figure 4] FIG. 4 shows a glass body portion produced from the division of the glass body. [Diagram 5] FIG. 5 is an illustration of the titanium profile associated with the two-dimensional macroscopic fabrication in the glass body section. [Figure 6] FIG. 6 is a diagram showing the arrangement of two glass body parts. [Figure 7a] FIG. 7a is the substrate precursor. [Figure 7b] FIG. 7b is an illustration of the titanium profile of multiple glass body portions compared to a desired titanium distribution. [Figure 8] FIG. 8 is a further illustration of the titanium profile of multiple glass body portions compared to a desired titanium distribution. [Figure 9] FIG. 9 shows the first homogenization process. [Figure 10] FIG. 10 shows the first glass component pressed together. [Figure 11] FIG. 11 shows the second homogenization process. [Figure 12] FIG. 12 is a diagram of a method according to the present invention.

[0108] Description of the drawings Figure 1 shows the Ti-doped SiO 2 An apparatus 100 for producing a soot body 200 is shown. A number of flame hydrolysis burners 220 arranged in a row are positioned along a carrier tube 210 made of aluminum oxide.

[0109] The silicon dioxide and titanium dioxide raw materials are fed in gaseous form to the reaction zone of the flame hydrolysis burner 220 and are decomposed in the process by oxidation and / or hydrolysis and / or pyrolysis. In the reaction zone, SiO 2 Particles and TiO 2 Both of the particles are formed and both are deposited in layers on the carrier tube 210, and SiO 2 -TiO 2 A soot body 200 is formed. SiO 2 -TiO 2 The particles themselves are SiO with a particle size in the nanometer range. 2 The soot body 200 may be in the form of agglomerates or aggregates of primary particles.Due in particular to the layered structure, the soot body 200 may include a microscopic layer structure.

[0110] In particular, in the manufacture 1100 of a large volume cylindrical soot body 200 for producing a substrate precursor 900 having a mass of more than 50 kg, particularly more than 100 kg, particularly more than 200 kg, the flame hydrolysis burners 220 may be mounted on a common burner block that is moved back and forth parallel to the longitudinal axis of the carrier tube 210 between two turning points fixed relative to the longitudinal axis.

[0111] This movement of the flame hydrolysis burner 220, mechanical imprecision in the feed lines of the feedstock or the burner 220, or even fluctuations in the process temperature can result in the TiO 2 This can result in a soot body 200 having macroscopic manufacturing related spatial variations in physical properties such as content.

[0112] FIG. 2 shows the vitrification of the soot body 200. The vitrification is preferably carried out in a process chamber. Preferably, the vitrification temperature is in the range of 1200° C. to 1500° C., preferably 1250° C. to 1350° C. In order to avoid the subsequent formation of bubbles in the quartz glass, it has turned out to be advantageous if the pressure in the process chamber during vitrification is lower than outside the process chamber, i.e. if the vitrification is carried out under reduced pressure. This has the further advantage that the material of the process chamber is not affected by aggressive corrosive gases and thus the wear is reduced. Therefore, an embodiment in which the vitrification is preferably carried out at a pressure of less than 1 mbar is preferred. Within the scope of the vitrification, the soot body 200 can be moved through a vitrification furnace 250 according to the movement arrow 251.

[0113] As a result of vitrification, a glass body 300 having a titanium dioxide content of 3% by weight up to 10% by weight is obtained from the soot body 200. The manufacturing-related variations in the physical properties already present in the soot body 200 are transferred to the glass body 300, so that the glass body 300 is Titanium profiles related to macroscopic manufacturing, and -Layer structures related to microscopic manufacturing, has.

[0114] The masses specified for 3% to a maximum of 10% titanium by weight are not elemental titanium but TiO 2 (Titanium dioxide) content.

[0115] 3 shows a cylindrical glass body 300. The dotted lines indicate the portions cut out from the glass body within the dividing step 1200. The rod-shaped glass body portion 400 thus produced is shown in FIG. 4. In particular, the glass body 300 can be divided into a plurality of rod-shaped glass body portions 400 having a longitudinal axis 440. In particular, the glass body portion 400 can have a sector-shaped cross section.

[0116] The first homogenization process 1600 of the first glass component and the second homogenization process 2000 of the second glass component significantly reduce the microscopic manufacturing related layer structure such that the glass body portion 400 is substantially free of layer structure. However, the two homogenization processes 1600, 2000 do not render the substrate precursor 900 free of long-wave titanium profiles that substantially affect the quality and usefulness of the substrate precursor 900 in EUV lithography.

[0117] FIG. 4 shows a glass body part 400 in which a titanium profile 410 is spatially measured. For this purpose, the titanium dioxide content is measured at a number of measurement points (P1, P2, P3, P4, P5, P6) along the longitudinal axis 420. These measurement points are at a distance of less than 5 cm, in particular less than 2 cm, from each other. This point-by-point measurement of the titanium dioxide content reflects a clear image of the ratio in the glass body part 400. All variations in the titanium profile occur on a length scale of 0.15 m to 0.75 m.

[0118] Additionally, further macroscopic manufacturing related variations in the chemical and / or physical properties of the glass body 300 may occur due to mechanical effects within the manufacturing 1100 of the soot body 200. At least one of these variations, shown as property profile 510, may be determined in measuring step 1300 as well. The following chemical and / or physical properties having macroscopic manufacturing related property profile 510 may be measured individually or in any combination: OH content, CTE, fluorine content, bubble content, ODC content, Ti3+ content, and metal impurity content.

[0119] The property profile 510 can be measured in parallel with the titanium profile 410 in a similar manner. For this purpose, the physical property is measured at a number of measurement points (P1, P2, P3, P4, P5, P6) along the longitudinal axis 420. Again, the measurement points are at a distance of less than 5 cm, in particular less than 2 cm, from each other.

[0120] 5 shows the results of a measurement 1300 of a titanium profile 410 and a property profile 510 on a glass body portion 400. The amount of titanium dioxide in weight % or the amount of property in ppm is plotted as a function of position along the longitudinal axis 440 of the glass body portion 400. For ease of illustration, only the measurement results for six measurement points (P1, P2, P3, P4, P5, P6) are shown in FIGS.

[0121] The steps and / or aspects of the spatial measurement 1300 of the titanium profile 410 described below also apply to the spatial measurement of the at least one property profile 510.

[0122] As can be seen from the graph, the titanium dioxide content is within a given interval of 3% to 10% by weight, however, for manufacturing-related reasons, this titanium dioxide content varies between 5.4% and 6.1% by weight along the longitudinal axis 420 of the glass body portion 400.

[0123] The amount of the property measured at six measurement points (P1, P2, P3, P4), here by way of example the OH content in ppm, is also shown as property profile 510. For manufacturing-related reasons, this OH content varies along the longitudinal axis 420 of the glass body portion 400 between 150 ppm and 175 ppm.

[0124] FIG. 6 illustrates the connection 1500 of multiple, in this case two, rod-shaped glass body portions 400 , 400 ′ to form an elongated first glass component 600 .

[0125] For this purpose, the flat contact surface 401 of the first glass body part 400 and the flat contact surface 401' of the second glass body part 400' can be joined to one another by drawing and welded to one another. This is a "cold joining method" in which at most the areas adjacent to the contact surfaces are subjected to significant heating.

[0126] Alternatively, the connecting 1500 may include a connecting step in which both glass body portions 400, 400' are softened in a furnace and joined together. This is a "hot joining method" in which the individual glass body portions 400, 400' are joined together by welding. As described, the titanium dioxide profile and / or property profile is measured at multiple measurement points. For the glass body portion 400, the titanium profile 410 is measured at measurement points P1, P2, P3, P4, P5, P6 as an example. For the glass body portion 400', the titanium profile 410' is measured at measurement points P7, P8, P9, P10, P11, P12 as an example.

[0127] Thus, within the scope of the method, at least three, in particular at least five, in particular at least eight glass body portions can be connected to one another to form a first glass component 600, also shown in FIG.

[0128] As shown in FIG. 5, the titanium profile 410 varies along the longitudinal axis of the glass body portion 400. In addition, however, the titanium profile also varies between different glass body portions 400, 400'. In the prior art, these macroscopic manufacturing-related variations in the individual titanium profiles between different glass body portions 400, 400' were not even considered. Rather, until now, only a small number of glass body portions 400, 400', in particular two glass body portions 400, 400', were necessary for a substrate precursor 900 having a low mass, so that the variations occurring between the long-wave titanium profiles 410 in the glass body portions 400, 400' could be neglected. This is no longer possible in the manufacture of substrate precursors having a mass of more than 50 kg, in particular more than 100 kg, especially when at least four glass body portions must be connected to each other.

[0129] 7a, 7b and 8 show steps used within the measuring step 1300, which serve to overcome the above-mentioned drawbacks.

[0130] Using the model, it is explained how, by permuting the placement of the glass body portions 400, 400', 400'', 400''' relative to one another, the titanium distribution 430 is calculated in each case and compared to the desired titanium distribution 420.

[0131] The steps and / or aspects described below for minimizing the difference between the titanium allocation and the titanium distribution also apply to minimizing a second difference between the at least one property allocation and the at least one property distribution.

[0132] The starting point is to predetermine 1400 a desired titanium distribution 420 in the substrate precursor. In one variation, the titanium distribution 420 is determined by determining the TiO 2 The model represents a two-dimensional distribution of the amount of titanium in the substrate precursor, particularly along a centerline through the substrate precursor, and particularly at the outer surface that is subsequently mirrored. In this embodiment, the model is capable of calculating the two-dimensional titanium distribution in the substrate precursor from the two-dimensionally determined titanium profiles and their arrangement relative to each other.

[0133] Figure 7a shows a substrate precursor 900. Optimally, the substrate precursor should have a titanium distribution 420 as shown in the top graph of Figure 7b. As an example, a parabolic titanium distribution 420 with a maximum at the center of the substrate precursor may have a TiO concentration of 4.75 wt% to 5.5 wt%. 2 The interval is required to be within the range of 0 to 1000.

[0134] The desired two-dimensional titanium distribution 420 can be found in the substrate precursor 900 along a centerline 920 on the outer surface 910 that will be mirrored later. The type and design of the titanium distribution 420 can depend, among other things, on the type and conditions of use of the subsequent EUV mirror. Titanium distributions with a parabolic (or Gaussian) profile with a maximum at the center of the substrate precursor are particularly preferred. In particular, the titanium distribution, and therefore the CTE, can be adapted to the distribution of the incident EUV radiation.

[0135] To explain the procedure, in FIG. 7b, it is assumed that the substrate precursor 900 is formed from only four glass body portions 400, 400', 400'', 400'''. As in FIG. 6, they are positioned relative to each other to form a rod-shaped glass body 300. In this case, the four glass body portions 400, 400', 400'', 400''' have been joined together in the following arrangement to form the first glass component 600: ● An arrangement in which the terminal side of the glass body portion 400 is connected to the front surface of the glass body portion 400' (point E2); A configuration in which the end side of the glass body portion 400' is connected to the front surface of the glass body portion 400'' (point E3); ● An arrangement in which the terminal side of glass body portion 400'' is connected to the front surface of glass body portion 400''' (point E4).

[0136] The middle graph in FIG. 7b shows titanium profiles 410, 410', 410'', 410''' of four glass body portions 400, 400', 400'', 400''' made from at least one glass body 300. The TiO content in weight percent in each of the four glass body portions 400, 400', 400'', 400'''' is 2 A set of measurements of the amount of is plotted.

[0137] To overcome the aforementioned drawbacks, a model is used that is capable of calculating the titanium distribution 430 within the substrate precursor 900. In this case, the model uses the following as input parameters: the arrangement of the glass body portions 400, 400', 400'', 400''' relative to one another in the first glass component 600; - spatial titanium profiles 410, 410', 410'', 410''' in each of the glass body portions 400, 400', 400'', 400'''', and - Effect of pressing step 1700 and rotating step 1800 on spatial titanium profiles 410, 410', 410'', 410'' in glass body portions 400, 400', 400'', 400''''.

[0138] Based on this configuration, the model calculates the titanium distribution 430 in the substrate precursor 900. This titanium distribution 430 is shown in the bottom graph of Figure 7b.

[0139] As shown in FIG. 7b, the illustrated profile of the calculated titanium distribution 430 does not simply correspond to a linear sequence of the illustrated profiles of the titanium profiles 410, 410', 410'', 410''' in the assumed arrangement. Rather, the method steps of the methods disclosed herein result in spatial positions and orientations of the titanium profiles 410, 410', 410'', 410''' after passing through the method that no longer correspond to the spatial positions that the glass body portions 400, 400', 400'', 400''' corresponding to the titanium profiles had in the first glass body 300. Thus, the spatial orientations of the titanium profiles 410, 410', 410'', 410''' may be affected by the TiO 2 The model is changed as needed to calculate the location and amount of

[0140] The calculated titanium distribution 430 shown in FIG. 7 b has a zigzag profile and therefore deviates significantly from the desired parabolic titanium distribution 420 .

[0141] To achieve the optimal arrangement, the possible arrangements of the glass body parts are permuted. In this model, the effect of all possible arrangements of the glass body parts on the titanium distribution 430 is calculated. FIG. 8 is used to illustrate this. The starting point is an arrangement, deviating from FIG. 7, of four glass body parts 400, 400', 400'', 400''', which are joined together in the following arrangement to form the first glass component 600: A configuration in which the end side of the glass body portion 400'' is connected to the front surface of the glass body portion 400''' (point E2); A configuration in which the end side of the glass body portion 400'' is connected to the front surface of the glass body portion 400' (point E3); ● An arrangement in which the terminal side of the glass body portion 400' is connected to the front surface of the glass body portion 400 (point E4).

[0142] The model calculates a titanium distribution 430' in the substrate precursor 900 from the titanium profiles 410'', 410''', 410', 410. This titanium distribution 430' is more similar to the desired titanium distribution 420, both in amount and profile, than the titanium distribution 430 shown in Figure 7b.

[0143] The model in particular calculates from any possible arrangement of the glass body parts 400, 400', 400'', 400''' the corresponding titanium distribution 430, 430' and compares it with the desired titanium distribution 420. For this purpose, all possible arrangements of the glass body parts 400, 400', 400'', 400''' are permuted. Based on this information, the model in each case forms the difference between the titanium distribution and the titanium distribution 420. The optimal arrangement is the arrangement in which the magnitude of the difference between two spatially identical points on the substrate precursor, in particular the maximum magnitude of the difference, is minimal.

[0144] The glass body portions 400, 400', 400'', 400''' are then positioned and connected according to the optimal arrangement.

[0145] Similarly, in addition to the titanium distribution, at least one property distribution can represent a second target value that is optimally met and / or desired in the substrate precursor 900. The model used in this variation is: the arrangement of the glass body portions 400, 400', 400'', 400''' relative to one another in the first glass component 600; - spatial titanium profiles 410, 410', 410'', 410''' and spatial property profiles 510 in each of the glass body portions 400, 400', 400'', 400'''', and The effect of the pressing and rotating steps on the spatial titanium profile 410, 410', 410'', 410''' and the spatial property profile 510 in the glass body portion 400, 400', 400'', 400''', It depends functionally on

[0146] As a result, both aspects related to the element titanium dioxide and aspects related to at least one additional property (eg, ODC, Ti3+, etc.) are taken into account in calculating the optimal arrangement of the glass body portion.

[0147] Based on a solution space of possible arrangements of the glass body portions relative to one another, the best possible arrangement of the glass body portions 400, 400', 400'', 400''' is determined, where the objective is to minimize the sum of the differences, where the sum of the differences is: The difference between titanium allocation and titanium distribution, and a second difference between the at least one characteristic allocation and the at least one characteristic distribution; Includes.

[0148] 9 shows a first homogenization process 1600 of the first glass component 600 made from the glass body portion 400'', 400''', 400', 400. Both the glass body and the first glass component 600 made from the glass body portion 400'', 400''', 400', 400 contain a layer structure related to the microscopic manufacturing. To reduce this and / or to make it possible to produce a substrate precursor 900 that is substantially free of layer structures, two homogenization processes are performed in sequence.

[0149] In a first homogenization process 1600, the first glass component 600 is fixed to a glass lathe 605 equipped with one or more burners 220 and homogenized by a remolding process as described in EP 673888 A1 with the aim of completely removing the layer structure.

[0150] The glass lathe 605 has two chucks 610, 610', which can be rotated (650, 650') independently of each other. The first glass component 600 is fixed between the two chucks 610, 610'. The two holding elements 620, 620' can ensure a better fit between the chucks 610, 610' and the first glass component 600. By the burner 220, the first glass component 600 is heated in spots and softened in the process, resulting in a shear zone 630. This shear zone 630 allows external forces, such as torsional, tensile or compressive forces, to be introduced into the rod-shaped first glass component 600. Within the shear zone 630, regions with different stresses or undergoing different movements result, which are associated with shear effects or expansion and compression effects. To generate this force, the two chucks 610, 610' can rotate (650, 650') in opposite directions in each case.

[0151] The first homogenization process 1600 effectively reduces the microscopic manufacturing-related layer structure in the plane of the shear bands of the first glass component 600. However, the reduction of the microscopic manufacturing-related layer structure perpendicular to the plane of the shear bands of the first glass component 600 is significantly less.

[0152] In order to remove the residues of the layer structure in the second homogenization process 2000, the first glass component 600 must be reshaped. FIG. 10 shows the pressing (1700) of the first glass component 600 to create a spherical glass system 700. For this purpose, the first glass component 600 is heated and compressed by a burner 220. The pressing 1700 can be performed by moving the two chucks 610, 610′ towards each other, as indicated by the movement arrow 612. The glass system 700 is then rotated (1800) by more than 70 degrees. For this purpose, the glass system 700 is removed from the chucks 610, 610′ and rotated, as the movement arrow 615 is intended to illustrate. This rotation ensures that in the second homogenization process 2000, the parts of the layer structure that were only slightly or not at all corrected in the first homogenization process 1600 are effectively reduced. After rotation 1800 of the glass system 700 through more than 70 degrees, the system is again secured to the chucks 610, 610'. This is followed by elongation 1900 of the glass system 700. This mechanical reshaping of the spherical glass system 700 into an elongated second glass component 800 is performed by heating the glass system 700 using burners 220 and moving the chucks 610, 610' away from each other, as illustrated by the movement arrow 613.

[0153] FIG. 11 shows a second homogenization process 2000 of the second glass component 800. The second homogenization process 2000 is performed substantially similarly to the first homogenization process 1600. The crucial difference is that by rotating 1800, the layer structure, which was previously substantially perpendicular to the longitudinal axis of the glass lathe 605, is now arranged in the direction of the longitudinal axis of the glass lathe 605. The second glass component 800 is fixed between two chucks 610, 610' of the glass lathe 605. By means of the burner 220, the second glass component 800 is spot-heated and softened in the process, creating a second shear zone 640. This second shear zone 640 allows an external force, such as a torsional force, a tensile force or a compressive force, to be introduced into the rod-shaped second glass component 800. Within the second shear zone 640, regions with different stresses or undergoing different movements thereby arise, which are associated with shear effects or expansion and compression effects. To generate this force, the two chucks 610, 610' can rotate (650, 650') in opposite directions in each case.

[0154] This second homogenization process 2000 effectively reduces microscopic manufacturing related layer structures in a direction perpendicular to the longitudinal axis of the first glass component 600 and / or in the direction of the longitudinal axis of the second glass component 800. After passing through both the first homogenization process 1600 and the second homogenization process 2000, a substrate precursor 900 is obtained that is substantially free of layer structures.

[0155] Figure 12 shows TiO 2 -SiO 2 The steps in the method for producing a substrate precursor 900 containing mixed glass and having a mass of over 100 kg are shown. This includes: Step 1000 of introducing a silicon dioxide raw material and a titanium dioxide raw material into a flame; Step 1100 for producing a glass body having a titanium dioxide content of 3% to a maximum of 10% by weight, the glass body being Titanium profiles related to macroscopic manufacturing, and -Layer structures related to microscopic manufacturing, A manufacturing step 1100 comprising: Step 1200 of dividing the glass body into a plurality of rod-shaped glass body portions; A step 1300 of spatially measuring the titanium profile in each of the glass body portions; connecting (1500) glass body portions to form an elongated first glass component; A step 1600 of a first homogenization treatment of a first glass component; Pressing (1700) first glass components together to create a spherical glass system; Step 1800 rotates the glass system by over 70 degrees; stretching (1900) the glass system to form an elongated second glass component; subjecting the second glass component to a second homogenization treatment (2000) to produce a substrate precursor 900 substantially free of layer structures; Includes.

[0156] The method includes a step 1300 of measuring: Predetermining 1400 a desired spatial titanium distribution in the substrate precursor 900; providing 1420 a model of titanium distribution in the substrate precursor 900, the model comprising: - Arrangement of the glass body portions relative to one another in the first glass component; - spatial titanium profile in each of the vitreous body portions; and The effect of the pressing and rolling steps on the spatial titanium profile in the glass body portion; and a step 1420 of providing, A step 1450 of calculating, using the model, the optimal arrangement of the glass body portions relative to each other such that the difference between the titanium allocation and the titanium distribution is minimized; In the connecting step, a step 1470 of positioning the glass body parts so that the glass body parts are connected according to the calculated optimal arrangement; The present invention is characterized by comprising:

[0157] Reference sign 100 devices 200 Suits 210 Carrier tube 220 Burner or flame hydrolysis burner 225 Flame 250 Vitrification Furnace 251 Movement Arrow 300 Glass body 400, 400', 400'' glass body 401, 401' contact surface 410, 400', 400'', 400'' Titanium Profiles 420 Titanium Distribution 430 Titanium Allocation 440 Longitudinal axis 510 Property Profile 600 First Glass Component 605 Glass Lathe 610, 610' Chuck 612 Movement Arrow 613 Movement Arrow 615 Movement Arrow 620, 620' two retaining elements 630 Shear Zone 640 Second Shear Zone 650, 650' rotation 700 Spherical Glass System 800 Second Glass Component 900 Substrate Precursor 910 Exterior 920 center line 1000 Introduction 1100 Manufacture 1200 Divide 1300 Spatially Measured 1400 Predetermine Offering 1420 models 1450 Calculate the optimal layout 1470 Positioning the glass body 1500 Connect the glass body parts 1600 First homogenization process 1700 Push together 1800 Rotating Glass System 1900 Extend 2000 Second homogenization process

Claims

1. A method for producing a substrate precursor (900) having a mass of more than 50 kg and comprising a TiO2-SiO2 mixed glass, comprising: Introducing (1000) a silicon dioxide source and a titanium dioxide source into a flame (225); A step (1100) of producing a glass body (300) having a titanium dioxide content of 3% by weight up to 10% by weight, said glass body (300) comprising: Titanium profiles related to macroscopic manufacturing (410, 410', 410'', 410'''), and -Layer structures related to microscopic manufacturing, A manufacturing step (1100) comprising: Dividing (1200) the glass body into a plurality of rod-shaped glass body portions (400, 400', 400'', 400'''); a step (1300) of spatially measuring the titanium profile (410, 410', 410'', 410''') in each of the glass body portions (400, 400', 400'', 400'''); connecting (1500) said glass body portions (400, 400', 400'', 400''') to form an elongated first glass component (600); a step (1600) of a first homogenization treatment of said first glass component (600); pressing (1700) said first glass components (600) together to create a spherical glass system (700); rotating (1800) the glazing system (700) by more than 70 degrees; drawing (1900) the glass system (700) to form an elongated second glass component (800); subjecting the second glass component (800) to a second homogenization treatment (2000) to produce a substrate precursor (900) substantially free of layer structures; Including, The measuring step further comprises: predetermining (1400) a desired spatial titanium distribution (420) in said substrate precursor (900); Providing (1420) a model of titanium distribution (430) in the substrate precursor (900), the model comprising: the arrangement of the glass body portions (400, 400', 400'', 400'') relative to one another in the first glass component (600); the titanium profiles (410, 410', 410'', 410''') in each of the glass body portions (400, 400', 400'', 400'''); and The effect of the pressing step (1700) and the rotating step (1800) on the titanium profile (410, 410', 410'', 410''') in the glass body portion; providing (1420), which is dependent on calculating (1450) an optimal arrangement of the glass body portions (400, 400', 400'', 400''') relative to one another using the model such that the difference between the titanium allocation (430) and the titanium distribution (420) is minimized; positioning (1470) the glass body portions (400, 400', 400'', 400''') such that in the connecting step (1500), the glass body portions (400, 400', 400'', 400''') are connected according to the calculated optimal arrangement; A method comprising:

2. The method of claim 1, wherein the substrate precursor (900) has a mass greater than 100 kg.

3. below: Producing a second glass body having a titanium dioxide content of 3% to a maximum of 10% by weight, said second glass body comprising: A titanium profile associated with the second macroscopic production, and - a layer structure associated with the second microscopic fabrication; and Dividing the second glass body into a plurality of rod-shaped glass body portions; 3. The method according to claim 1 or 2, comprising:

4. 3. The method of claim 1 or 2, characterized in that at least three glass body parts are connected to form the first glass component.

5. 3. The method of claim 1 or 2, characterized in that the difference between the titanium allocation (430) and the titanium distribution (420) is less than 1.5% based on a maximum value of the titanium distribution (420).

6. The glass body has the following property profile (510): • OH profiles related to macroscopic production; • Macroscopic manufacturing related CTE profile; • Fluorine profiles related to macroscopic production; - bubble profiles related to macroscopic manufacturing, - ODC profile related to macroscopic manufacturing; • Macroscopic production related Ti3+ profiles; • Macroscopic production-related metal impurity profiles; 3. The method according to claim 1 or 2, characterized in that it comprises at least one of the following:

7. 7. The method of claim 6, wherein in the measuring step, at least one of the characteristic profiles (510) is measured in each of the glass body portions (400, 400', 400'', 400''').

8. The measuring step further comprises: predetermining a desired spatial property distribution in said substrate precursor (900); providing a model of property distribution in the substrate precursor (900), the model comprising: the arrangement of the glass body portions relative to one another in the first glass component; a spatial property profile (510) in each of said glass body portions; and The effect of the pressing and rotating steps on the spatial property profile in the glass body portion; Depends on,step,and, calculating the best possible arrangement of said glass body parts (400, 400', 400'', 400''') relative to one another by means of a model so that the sum of differences is minimized, said sum of differences being: the difference between said titanium allocation (430) and said titanium distribution (420), and a second difference between the property allocation and the property distribution; and positioning the glass body parts (400, 400', 400'', 400''') such that in the connecting step (1500) the glass body parts (400, 400', 400'', 400''') are connected according to a calculated best possible arrangement; The method of claim 7, comprising:

9. 9. The method of claim 8, wherein the sum of the differences is less than 1.5% based on the sum of the maximum of the titanium distribution (420) and the maximum of the property distribution.

10. The step of manufacturing the glass body (1100) comprises at least the following steps: Producing a porous soot body (200), a titanium profile associated with said macroscopic fabrication extending substantially along a longitudinal axis, and a layer structure associated with said microscopic fabrication extending substantially along a growth axis; - vitrifying the soot body to produce a cylindrical glass body; 3. The method according to claim 1 or 2, comprising:

11. 3. The method of claim 1 or claim 2, characterized in that the first glass component (600) is heated prior to the pressing step (1700).

12. 3. Method according to claim 1 or 2, characterized in that the connection (1500) is made at the associated contact surface (401) of the glass body part (400, 400', 400'', 400''').

Citation Information

Patent Citations

  • Method for manufacturing homogeneous silica-titania glass

    JP2006240979A

  • Method of finishing pre-polished glass substrate surface

    JP2007022903A

  • Method for producing silica-titania glass having no stria

    JP2007186348A

  • Glass with low OH and OD levels

    JP2010528960A

  • Blanks of titanium-doped glass with a high silica content for mirror substrates used in EUV lithography, and method for manufacturing the same.

    JP2013506614A