Epitaxial structure of semiconductor device, manufacturing method thereof, and semiconductor device
The inverse proportional thickness relationship between nucleation and buffer layers, along with a stacked buffer layer design with specific doping concentrations, addresses the thermal and lattice mismatch issues in GaN-based devices, ensuring high crystal quality and resistance, thus improving the reliability and performance of semiconductor devices.
Patent Information
- Application Number
- JP2023518044
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2021-06-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-06-09
Smart Images

Figure 0007577842000001 
Figure 0007577842000002 
Figure 0007577842000003
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE Embodiments of the present invention are in the field of semiconductor technology, and more particularly, in the field of epitaxial structures for semiconductor devices, methods for fabricating the same, and semiconductor devices. [Background technology]
[0002] The semiconductor material gallium nitride (GaN) has advantages such as a wide band gap, high electron mobility, high breakdown electric field strength, and excellent thermal conductivity. It also has strong spontaneous polarization and piezoelectric polarization effects, making it more applicable to the manufacture of high-frequency, high-voltage, and high-temperature resistant high-power electronic devices than first- and second-generation semiconductor materials, and has particularly notable advantages in the fields of radio frequency and power supplies.
[0003] Currently, when manufacturing GaN-based optoelectronic devices and power devices, there exists thermal mismatch and lattice mismatch between the GaN epitaxial layer and the substrate, and the thermal mismatch stress and lattice mismatch strain generated during the epitaxial growth process cause deformation of the epitaxial wafer, which reduces the uniformity of the epitaxial layer, reduces the yield of epitaxial products, and increases the cost. Therefore, a nucleation layer is introduced between the GaN epitaxial layer and the substrate.
[0004] However, the presence of the nucleation layer may increase the thermal resistance of the entire epitaxial layer. To solve this problem, thin nucleation layers are often used in the field. However, thin nucleation layers have the problem of poor crystal quality, which may affect the crystal quality of the GaN grown next, and ultimately the reliability of the final device. Currently, in order to manufacture third-generation semiconductor devices with excellent electrical properties and stable reliability, it is necessary to match the performance of semiconductor devices with a semiconductor epitaxial structure that has high crystal quality, good uniformity, and low industrial cost.
[0005] Therefore, how to obtain an epitaxial structure with good crystal quality and low cost without increasing thermal resistance has become an issue that must be solved immediately.
[0006] In addition, due to the existence of a relatively strong two-dimensional electron gas in the AlGaN / GaN heterostructure, the high electron mobility transistor (HEMT) formed with the AlGaN / GaN heterostructure is usually used as a depletion mode device. In order to give this device a higher breakdown voltage, better switching characteristics and more reliable performance, a highly resistive GaN buffer layer must first be obtained.
[0007] There are various methods for obtaining a high-resistance GaN buffer layer. The commonly used method is to perform C doping or Fe doping. However, the C content required to obtain a GaN buffer layer with a sufficiently high resistance may deteriorate the crystal quality, which may affect the reliability of the final device, and the deep energy level traps formed by the C impurities may tend to deteriorate the performance of the final device, such as the output power. On the other hand, the Fe content required to obtain a GaN buffer layer with a sufficiently high resistance may cause deterioration of the epitaxial layer surface and crystal quality, which may affect the performance of the final device. Therefore, how to ensure the crystal quality of the epitaxial layer while ensuring the performance of the final device is an issue that must be solved as soon as possible. Summary of the Invention
[0008] In view of the above circumstances, embodiments of the present invention provide an epitaxial structure for a semiconductor device, a manufacturing method thereof, and a semiconductor device, thereby providing an epitaxial structure having good thermal resistance and crystal quality of a nucleation layer, and thus providing an epitaxial structure having good high resistance characteristics and crystal quality of a buffer layer.
[0009] In a first aspect, an embodiment of the present invention provides an epitaxial structure for a semiconductor device, comprising: A substrate; an epitaxial layer on one side of the substrate, the epitaxial layer including a nucleation layer on one side of the substrate and a buffer layer on a side of the nucleation layer remote from the substrate; Including, The thickness of the buffer layer provides an epitaxial structure that is inversely proportional to the thickness of the nucleation layer. Optionally, the nucleation layer has a thickness h1 and the buffer layer has a thickness h2; Here, 0.1 / h2≦h1≦0.25 / h2.
[0010] Alternatively, h1=0.17 / h2.
[0011] Optionally, the nucleation layer has a thickness h1 and the substrate has a thickness h3; Here, 2*10 -5 ≦h1 / h3≦5*10 -4 It is.
[0012] Optionally, the nucleation layer has a thickness h1 and the epitaxial layer has a thickness h4; Here, 0.05≦h1 / h4≦0.3.
[0013] Optionally, 0.07≦h1 / h4≦0.1.
[0014] Optionally, the nucleation layer has a thickness h1, where 100 nm≦h1≦150 nm.
[0015] Optionally, the epitaxial layer comprises: a spacer layer located on a side of the buffer layer remote from the substrate; a potential barrier layer located on a side of the spacer layer farther from the substrate and forming a heterojunction structure together with the buffer layer; a cap layer located on a side of the potential barrier layer away from the substrate; Further includes:
[0016] Optionally, the buffer layer includes a first type buffer layer and a second type buffer layer stacked together, the first type buffer layer being located closer to the substrate, and the doping concentration of the first type buffer layer being higher than the doping concentration of the second type buffer layer.
[0017] Optionally, the first type of buffer layer includes at least one first buffer layer, and the second type of buffer layer includes at least one second buffer layer; The doping concentration of the first buffer layer is higher than the doping concentration of the second buffer layer.
[0018] Optionally, the first type buffer layer includes a first buffer layer A and a first buffer layer B that are stacked together, the first buffer layer A is located closer to the substrate, and the doping concentration of the first buffer layer A is equal to or greater than the doping concentration of the first buffer layer B; The second type buffer layer includes a second A buffer layer and a second B buffer layer which are stacked together, the second A buffer layer is located closer to the substrate, and the doping concentration of the second A buffer layer is higher than the doping concentration of the second B buffer layer.
[0019] Optionally, the first buffer layer A, the first buffer layer B, the second buffer layer A and the second buffer layer B are all doped with carbon ions; The doping concentration of carbon ions in the first A buffer layer is a first doping concentration C1, the doping concentration of carbon ions in the first B buffer layer is a second doping concentration C2, the doping concentration of carbon ions in the second A buffer layer is a third doping concentration C3, and the doping concentration of carbon ions in the second B buffer layer is a fourth doping concentration C4, where C1>C2≧C3>C4.
[0020] Optionally, the first buffer layer A and the first buffer layer B are further doped with iron ions, and the second buffer layer A and the second buffer layer B are not doped with iron ions; The doping concentration of iron ions in the first A buffer layer is a fifth doping concentration, and the doping concentration of iron ions in the first B buffer layer is a sixth doping concentration, where the fifth doping concentration is the same as the sixth doping concentration.
[0021] Optionally, the doping concentration of carbon ions in the first buffer layer A is a first doping concentration C1, and the doping concentration of iron ions in the first buffer layer A is a fifth doping concentration C5, where C1 / C5=(0.5-1.2) / 10; The doping concentration of the carbon ions in the first B buffer layer is a second doping concentration C2, and the doping concentration of the iron ions in the first B buffer layer is a sixth doping concentration C6, where C2 / C6=(0.1-0.3) / 10; The doping concentration of carbon ions in the second buffer layer is a third doping concentration C3, where C3=C2; The doping concentration of carbon ions in the second buffer layer is a fourth doping concentration C4, where C4 / C3=(1 to 2) / 10.
[0022] Optionally, the thickness of the first buffer layer is greater than the thickness of the second buffer layer.
[0023] Optionally, the first type of buffer layer includes a first buffer layer A and a first buffer layer B that are laminated together, the first buffer layer A is located closer to the substrate, and the thickness of the first buffer layer A is equal to or greater than the thickness of the first buffer layer B; The second type of buffer layer includes a second A buffer layer and a second B buffer layer which are laminated together, the second A buffer layer is located closer to the substrate, and the thickness of the second A buffer layer is greater than the thickness of the second B buffer layer.
[0024] Optionally, the first buffer layer A has a thickness of h1, the first buffer layer B has a thickness of h2, the second buffer layer A has a thickness of h3, and the second buffer layer B has a thickness of h4; Here, h2=h1, 2 / 10≦h3 / h2≦9 / 10, and 4 / 10≦h4 / h3≦9 / 10.
[0025] In a second aspect, embodiments of the present invention further provide a semiconductor device comprising an epitaxial structure according to the first aspect, the epitaxial structure comprising a substrate and, sequentially on one side of the substrate, a nucleation layer, a buffer layer, a spacer layer, a potential barrier layer and a cap layer. The semiconductor device is a source electrode and a drain electrode located on a side of the potential barrier layer away from the substrate; a gate electrode located on a side of the cap layer away from the substrate and between the source electrode and the drain electrode; Includes.
[0026] In a third aspect, embodiments of the present invention further provide a method for manufacturing an epitaxial structure for a semiconductor device, the method comprising: Providing a substrate; Producing a nucleation layer on one side of the substrate; fabricating a buffer layer on a side of the nucleation layer remote from the substrate; fabricating a spacer layer on a side of the buffer layer remote from the substrate; producing a potential barrier layer on the side of the spacer layer remote from the substrate, which forms a heterojunction structure with the buffer layer; fabricating a cap layer on a side of the potential barrier layer remote from the substrate; Including, Here, the thickness of the buffer layer is inversely proportional to the thickness of the nucleation layer.
[0027] In the epitaxial structure of the semiconductor device and the semiconductor device provided in the embodiments of the present invention, the thickness of the nucleation layer and the thickness of the buffer layer are inversely proportional to each other, which ensures that the crystal quality of the nucleation layer in the epitaxial structure is improved without increasing the thermal resistance of the nucleation layer, thereby improving the quality of the epitaxial structure and the reliability of the semiconductor device.
[0028] In addition, in the epitaxial structure of a semiconductor device and the manufacturing method thereof, and the semiconductor device provided in the embodiments of the present invention, the buffer layer includes a first type buffer layer and a second type buffer layer which are stacked, and the doping concentration of the first type buffer layer is designed to be higher than that of the second type buffer layer, thereby ensuring the high resistance characteristics of the buffer layer in the epitaxial structure and ensuring good crystal quality of the buffer layer, thereby improving the quality of the epitaxial structure and the semiconductor device. [Brief description of the drawings]
[0029] [Figure 1] 1 is a structural schematic diagram of an epitaxial structure of a semiconductor device provided in an embodiment of the present invention; [Diagram 2] 1 is a structural schematic diagram of a semiconductor device provided in an embodiment of the present invention; [Diagram 3] 1 is a flowchart of a method for manufacturing an epitaxial structure of a semiconductor device provided in an embodiment of the present invention. [Figure 4] 1 is a flowchart of a method for manufacturing a semiconductor device provided in an embodiment of the present invention. [Diagram 5] 1 is a structural schematic diagram of an epitaxial structure of a semiconductor device provided in an embodiment of the present invention; [Figure 6] 1 is a structural schematic diagram of a semiconductor device provided in an embodiment of the present invention; [Figure 7] 1 is a flowchart of a method for manufacturing an epitaxial structure of a semiconductor device provided in an embodiment of the present invention. [Figure 8] 1 is a flowchart of a method for manufacturing a semiconductor device provided in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The present invention will be described in more detail below with reference to the drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, for the sake of convenience, the drawings show only some structures related to the present invention, rather than all structures.
[0031] 1 is a structural schematic diagram of an epitaxial structure of a semiconductor device provided in an embodiment of the present invention. As shown in FIG. 1, the epitaxial structure of a semiconductor device provided in an embodiment of the present invention includes a substrate 11 and an epitaxial layer 12 located on one side of the substrate 11. The epitaxial layer 12 includes a nucleation layer 121 located on one side of the substrate 11 and a buffer layer 122 located on the side of the nucleation layer 12 farther from the substrate 11. Here, the thickness of the buffer layer 122 is inversely proportional to the thickness of the nucleation layer 121.
[0032] By way of example, substrate 11 may be one or more combinations of gallium nitride, aluminum gallium nitride, indium gallium nitride, aluminum indium gallium nitride, indium phosphide, gallium arsenide, silicon carbide, diamond, sapphire, germanium, and silicon, or any material on which Group III nitrides can be grown, and embodiments of the present invention do not limit the specific type of substrate 11.
[0033] An epitaxial layer 12 is located on one side of the substrate 11. The epitaxial layer 12 may specifically comprise a III-V compound semiconductor material.
[0034] Specifically, the epitaxial layer 12 includes a nucleation layer 121 near one side of the substrate 11 and a buffer layer 122 located on the side of the nucleation layer 121 farther from the substrate 11. Here, the nucleation layer 121 affects parameters such as crystal quality, surface topography and electrical properties of other film layers located above the nucleation layer 121 in the epitaxial layer 12. The nucleation layer 121 mainly serves to match the material of the substrate 11 with the semiconductor material layer in the heterojunction structure of the epitaxial layer 12. The buffer layer 122 serves to adhere the semiconductor material layer that needs to be grown next.
[0035] Furthermore, the material of the nucleation layer 121 may be aluminum nitride, and the material of the buffer layer 122 may be gallium nitride.
[0036] The presence of the AlN nucleation layer increases the thermal resistance of the entire epitaxial layer 12. To alleviate this problem, in the art, a thin AlN is often used as the AlN nucleation layer. However, it is very difficult to obtain high crystal quality with a thin AlN nucleation layer. Increasing the thickness of the AlN nucleation layer is one way to improve the crystal quality. However, simply increasing the AlN thickness increases the thermal resistance, which may affect the performance of the device. In the embodiment of the present invention, the thickness of the nucleation layer 121 and the thickness of the buffer layer 122 in the epitaxial layer 12 are creatively designed to be inversely proportional. That is, after increasing the thickness of the nucleation layer 121, the thickness of the buffer layer 122 needs to be decreased, and after decreasing the thickness of the nucleation layer 121, the thickness of the buffer layer 122 needs to be increased. Extensive verification has shown that when the thickness of the nucleation layer 121 in the epitaxial layer 12 is inversely proportional to the thickness of the buffer layer 122, the crystal quality of the nucleation layer 121 is improved without increasing the thermal resistance, and the crystal quality, surface topography and electrical properties of other epitaxial layers located above the nucleation layer 121 are good, so that the quality of the epitaxial structure and the entire semiconductor device are good and reliable.
[0037] From the above, in the epitaxial structure of the semiconductor device provided in the embodiment of the present invention, by making the thickness of the nucleation layer inversely proportional to the thickness of the buffer layer, the thermal resistance of the nucleation layer in the epitaxial structure is not increased, and the crystal quality of the nucleation layer is improved, thereby improving the quality of the epitaxial structure and the semiconductor device.
[0038] Based on the above example, the nucleation layer 121 has a thickness h1, and the buffer layer 122 has a thickness h2, where 0.1 / h2≦h1≦0.25 / h2.
[0039] For example, the thickness of the nucleation layer 121 in the epitaxial layer 12 is inversely proportional to the thickness of the buffer layer 122, and the thickness h1 of the nucleation layer 121 and the thickness h2 of the buffer layer 122 can be designed to satisfy 0.1 / h2≦h1≦0.25 / h2. When the thickness h1 of the nucleation layer 121 and the thickness h2 of the buffer layer 122 satisfy the above proportional relationship, it is guaranteed that the crystal quality of the nucleation layer 121 is improved without increasing the thermal resistance of the nucleation layer 121, and high reliability of the epitaxial structure and the semiconductor device is guaranteed.
[0040] Specifically, the thickness h1 of the nucleation layer 121 and the thickness h2 of the buffer layer 122 satisfy 0.1 / h2≦h1≦0.25 / h2, and may be h1=0.1 / h2, h1=0.15 / h2, h1=0.17 / h2, h1=0.2 / h2 or h1=0.25 / h2. In the embodiment of the present invention, the specific proportional relationship between the thickness h1 of the nucleation layer 121 and the thickness h2 of the buffer layer 122 is not limited, and it is sufficient that the thickness h1 of the nucleation layer 121 and the thickness h2 of the buffer layer 122 satisfy 0.1 / h2≦h1≦0.25 / h2. In this way, it is guaranteed that the crystal quality of the nucleation layer 121 is improved without increasing the thermal resistance of the nucleation layer 121, and the high reliability of the epitaxial structure and the semiconductor device is guaranteed.
[0041] Based on the above embodiment, preferably, the thickness h1 of the nucleation layer 121 and the thickness h2 of the buffer layer 122 may satisfy h1=0.17 / h2, which ensures that the thermal resistance and crystal quality of the nucleation layer 121 are in an optimal balance state, and the crystal quality of the nucleation layer 121 is optimal without increasing the thermal resistance of the nucleation layer 121, or the crystal quality of the nucleation layer 121 is good while the thermal resistance is minimal, which ensures that the quality of the nucleation layer 121 is optimal, and thus the reliability of the epitaxial structure and the entire semiconductor device is optimal.
[0042] Alternatively, the thickness of the nucleation layer 121 is h1 and the thickness of the substrate is h3, where 2*10 -5 ≦h1 / h3≦5*10 -4 It is.
[0043] For example, the thickness h1 of the nucleation layer 121 and the thickness h3 of the substrate 11 are 2*10 -5 ≦h1 / h3≦5*10 -4 By rationally designing the nucleation layer 121 to satisfy the above, the nucleation layer 121 can be well matched with the substrate 11 while ensuring that the nucleation layer 121 has good thermal resistance and crystal quality, and further improve the reliability of the epitaxial structure and the semiconductor device.
[0044] Specifically, the thickness h1 of the nucleation layer 121 and the thickness h3 of the substrate 11 are 2*10 -5 ≦h1 / h3≦5*10 -4 and h1 / h3=2*10 -5 , h1 / h3=5*10 -5 , h1 / h3=1*10 -4 , h1 / h3=3*10 -4 Or h1 / h3=5*10 -4 In the embodiment of the present invention, the specific proportional relationship between the thickness h1 of the nucleation layer 121 and the thickness h3 of the substrate 11 is not limited, and the ratio of the thickness h1 of the nucleation layer 121 to the thickness h3 of the substrate 11 may be 2*10 -5 ≦h1 / h3≦5*10 -4 It is sufficient to satisfy the above.
[0045] Optionally, the nucleation layer 121 has a thickness h1 and the epitaxial layer 12 has a thickness h4, where 0.05≦h1 / h4≦0.3.
[0046] For example, by rationally designing the thickness h1 of the nucleation layer 121 and the thickness h4 of the epitaxial layer 12 to satisfy 0.05≦h1 / h4≦0.3, it is possible to ensure that the thermal resistance and crystal quality of the nucleation layer 121 are good, while the thickness of the nucleation layer 121 can be sufficiently matched with the thickness of the entire epitaxial layer 12, and it is ensured that other film layers in the epitaxial layer 12 other than the nucleation layer 121 have an appropriate thickness range, thereby ensuring the high quality of the entire epitaxial layer 12 and the high reliability of the epitaxial structure and the semiconductor device.
[0047] Specifically, the thickness h1 of the nucleation layer 121 and the thickness h4 of the epitaxial layer 12 satisfy 0.05≦h1 / h4≦0.3, and may be h1 / h4=0.05, or h1 / h4=0.1, h1 / h4=0.2, or h1 / h4=0.3. In the embodiment of the present invention, the specific proportional relationship between the thickness h1 of the nucleation layer 121 and the thickness h4 of the epitaxial layer 12 is not limited, and it is sufficient that the thickness h1 of the nucleation layer 121 and the thickness h4 of the epitaxial layer 12 satisfy 0.05≦h1 / h4≦0.3.
[0048] Based on the above embodiment, preferably, the thickness h1 of the nucleation layer 121 and the thickness h4 of the epitaxial layer 12 satisfy 0.07≦h1 / h4≦0.1, which ensures that the thermal resistance and crystal quality of the nucleation layer 121 are good, while the thickness of the nucleation layer 121 can be perfectly matched with the thickness of the entire epitaxial layer 12, and further ensures that other film layers in the epitaxial layer 12 other than the nucleation layer 121 have a suitable thickness range, which further improves the quality of the entire epitaxial layer 12, and improves the reliability of the epitaxial structure and the semiconductor device.
[0049] Alternatively, when the thickness h3 of the substrate is between 400 um and 600 um, the thickness of the nucleation layer 121 is h1, where 100 nm≦h1≦150 nm.
[0050] For example, by rationally designing the thickness h1 of the nucleation layer 121 to satisfy 100 nm≦h1≦150 nm, it is ensured that the nucleation layer 121 has a relatively low thermal resistance and high crystal quality.
[0051] Specifically, the thickness h1 of the nucleation layer 121 satisfies 100 nm≦h1≦150 nm, and may be h1=100 nm, or h1=110 nm, or h1=130 nm, or h1=150 nm. In the embodiment of the present invention, the specific thickness of the nucleation layer 121 is not limited, and it is sufficient that the thickness h1 of the nucleation layer 121 satisfies 100 nm≦h1≦150 nm.
[0052] Based on the above embodiment, as shown in FIG. 1, the epitaxial layer 12 provided in the embodiment of the present invention further includes a spacer layer 123 located on the side of the buffer layer 122 farther from the substrate 11, a potential barrier layer 124 located on the side of the spacer layer 123 farther from the substrate 11 and forming a heterojunction structure together with the buffer layer 122, and a cap layer 125 located on the side of the potential barrier layer 124 farther from the substrate 11.
[0053] Exemplarily, the spacer layer 123 may be an AlN spacer layer, which can increase the potential barrier, increase the confinement of the two-dimensional electron gas, reduce alloy scattering, and improve the mobility.
[0054] The potential barrier layer 124 may be an AlGaN potential barrier layer. The potential barrier layer 124 forms a heterojunction structure together with the buffer layer 122, and forms a transport channel for the two-dimensional electron gas. The main function of the cap layer 125 is to reduce the surface state, reduce the surface leakage current of the next semiconductor device, and suppress the current collapse, thereby improving the performance and reliability of the epitaxial structure and the semiconductor device. Optionally, the material of the cap layer 125 is a group III nitride, preferably P-type doped gallium nitride (P-GaN). The P-GaN structure can effectively lower the potential barrier of the AlGaN layer.
[0055] Based on the same inventive idea as above, an embodiment of the present invention provides a semiconductor device. The semiconductor device provided in the embodiment of the present invention includes the epitaxial structure of the semiconductor device described in the above embodiment. FIG. 2 is a structural schematic diagram of the semiconductor device provided in the embodiment of the present invention. As shown in FIG. 2, the semiconductor device provided in the embodiment of the present invention includes: A substrate 11; an epitaxial layer 12 on one side of the substrate 11, the epitaxial layer 12 including, in sequence on the one side of the substrate 11, a nucleation layer 121, a buffer layer 122, a spacer layer 123, a potential barrier layer 124, and a cap layer 125; a source electrode 131 and a drain electrode 132 located on the side of the potential barrier layer 124 farther from the substrate 11; a gate electrode 133 located on the side of the cap layer 125 farther from the substrate 11 and between the source electrode 131 and the drain electrode 132; Includes.
[0056] Exemplarily, the source electrode 131 and the drain electrode 132 are located on the side of the potential barrier layer 124 remote from the substrate 11. The source electrode 131 and the drain electrode 132 each form an ohmic contact with the potential barrier layer 124. The gate electrode 133 is located between the source electrode 131 and the drain electrode 132, and is located on the side of the cap layer 125 remote from the substrate 11. The gate electrode 133 forms a Schottky contact with the cap layer 125.
[0057] Based on the same inventive idea as above, an embodiment of the present invention further provides a method for manufacturing an epitaxial structure of a semiconductor device. Figure 3 is a flow chart of the method for manufacturing an epitaxial structure of a semiconductor device provided in an embodiment of the present invention. As shown in Figure 3, the method for manufacturing an epitaxial structure of a semiconductor device provided in an embodiment of the present invention may include the following steps S110 and S120. S110: Provide a substrate. Exemplarily, the substrate material may be one or more combinations of gallium nitride, aluminum gallium nitride, indium gallium nitride, aluminum indium gallium nitride, indium phosphide, gallium arsenide, silicon carbide, diamond, sapphire, germanium, silicon, or any material on which III-nitrides can be grown. The substrate fabrication method may be atmospheric pressure chemical vapor deposition, sub-atmospheric pressure chemical vapor deposition, metal organic chemical vapor deposition, low pressure chemical vapor deposition, high density plasma chemical vapor deposition, ultra-high vacuum chemical vapor deposition, plasma enhanced chemical vapor deposition, catalytic chemical vapor deposition, hybrid physical chemical vapor deposition, rapid thermal chemical vapor deposition, vapor phase epitaxy, pulsed laser deposition, atomic layer epitaxy, molecular beam epitaxy, sputtering, or evaporation.
[0058] S120: Producing an epitaxial layer on one side of the substrate, the epitaxial layer including a nucleation layer located on one side of the substrate and a buffer layer located on a side of the nucleation layer away from the substrate, the thickness of the buffer layer being inversely proportional to the thickness of the nucleation layer.
[0059] The presence of the nucleation layer increases the thermal resistance of the entire epitaxial layer, and it is very difficult to obtain high crystal quality with a thin AlN nucleation layer, and simply increasing the AlN thickness increases the thermal resistance, which may affect the performance of the device. In the embodiment of the present invention, by creatively designing the thickness of the nucleation layer in the epitaxial layer to be inversely proportional to the thickness of the buffer layer, the crystal quality of the nucleation layer can be improved without increasing the thermal resistance, and the crystal quality, surface topography and electrical properties of other epitaxial layers located above the nucleation layer can be ensured to be good, and the quality and reliability of the entire epitaxial structure and semiconductor device can be ensured to be good.
[0060] From the above, in the manufacturing method of an epitaxial structure for a semiconductor device provided in an embodiment of the present invention, by making the thickness of the nucleation layer inversely proportional to the thickness of the buffer layer, the thermal resistance of the nucleation layer in the epitaxial structure is not increased, and the crystal quality of the nucleation layer is improved, thereby improving the quality of the epitaxial structure and the semiconductor device.
[0061] Based on the above examples, the production of an epitaxial layer on one side of the substrate can be Producing a nucleation layer on one side of the substrate; - fabricating a buffer layer on a side of the nucleation layer remote from the substrate; fabricating a spacer layer on a side of the buffer layer remote from the substrate; - producing, on the side of the spacer layer remote from the substrate, a potential barrier layer which forms a heterojunction structure together with the buffer layer; fabricating a cap layer on a side of the potential barrier layer remote from the substrate; may include:
[0062] The spacer layer increases the potential barrier, improves the limiting power of the two-dimensional electron gas, reduces alloy scattering, and improves mobility. The potential barrier layer forms a heterojunction structure together with the buffer layer, forming a channel for the two-dimensional electron gas to move. The cap layer reduces the surface state, reduces the surface leakage of the next semiconductor device, and suppresses current collapse, improving the performance and reliability of the epitaxial structure and the semiconductor device.
[0063] Based on the same inventive idea as above, an embodiment of the present invention further provides a method for manufacturing a semiconductor device. Figure 4 is a flow chart of the method for manufacturing a semiconductor device provided in an embodiment of the present invention. As shown in Figure 4, the method for manufacturing a semiconductor device provided in an embodiment of the present invention may include the following steps S210 to S230. S210: Provide a substrate. S220: Producing an epitaxial layer on one side of the substrate, the epitaxial layer including a nucleation layer, a buffer layer, a spacer layer, a potential barrier layer and a cap layer, sequentially located on one side of the substrate. S230: Fabricating a source electrode and a drain electrode on the potential barrier layer on a side remote from the substrate, and fabricating a gate electrode on the cap layer on a side remote from the substrate, the gate electrode being located between the source electrode and the drain electrode.
[0064] The source electrode and the drain electrode each form an ohmic contact with the potential barrier layer, and the gate electrode forms a Schottky contact with the cap layer.
[0065] In order to further improve the quality of the epitaxial structure and the use reliability of the epitaxial structure, the semiconductor epitaxial structure is further optimized. FIG. 5 is a structural schematic diagram of the epitaxial structure of a semiconductor device provided in an embodiment of the present invention. As shown in FIG. 5, the epitaxial structure provided in an embodiment of the present invention includes a substrate 11 and an epitaxial layer 12 located on one side of the substrate 11. The epitaxial layer 12 includes a buffer layer 122. The buffer layer 122 includes a first type buffer layer 1221 and a second type buffer layer 1222 that are stacked. The first type buffer layer 1221 is located on the side close to the substrate 11, and the doping concentration of the first type buffer layer 1221 is higher than the doping concentration of the second type buffer layer 1222.
[0066] The epitaxial layer 12 is located on one side of the substrate 11. The epitaxial layer 12 may specifically comprise a III-V compound semiconductor material.
[0067] In particular, epitaxial layer 12 includes a buffer layer 122. Buffer layer 122 serves to provide adhesion for the next layer of semiconductor material that must be grown.
[0068] The buffer layer 122 includes a first type buffer layer 1221 and a second type buffer layer 1222 that are stacked. The first type buffer layer 1221 is located closer to the substrate 11, and the second type buffer layer 1222 is located farther from the substrate 11. The material of the first type buffer layer 1221 and the second type buffer layer 1222 may be the same, preferably gallium nitride. Furthermore, the thickness and doping of the first type buffer layer 1221 and the second type buffer layer 1222 may be different.
[0069] First, the doping conditions of the first type buffer layer 1221 and the second type buffer layer 1222 will be described.
[0070] The C doping concentration required to obtain a high-resistance GaN buffer layer is >1*10 19 / cm 3However, doing so may result in a deterioration in the crystal quality of the GaN buffer layer. The Fe doping concentration required to obtain a high-resistance GaN buffer layer is >1*10 19 / cm 3 must be satisfied, but doing so may affect the performance of the final device. In the embodiment of the present invention, the buffer layer 122 includes multiple buffer layers, for example, a first type buffer layer 1221 and a second type buffer layer 1222 that are stacked together, and the first type buffer layer 1221 is located on the side closer to the substrate 11, and the doping concentration of the first type buffer layer 1221 is designed to be higher than the doping concentration of the second type buffer layer 1222, thereby achieving a high resistance buffer layer due to the specific doping concentration relationship between the first type buffer layer 1221 and the second type buffer layer 1222. For example, by making the buffer layer lightly doped, it is guaranteed that the reliability of the epitaxial structure and the semiconductor device is improved without deteriorating the performance such as leakage current and breakdown of the semiconductor device.
[0071] From the above, in the epitaxial structure provided in the embodiment of the present invention, the buffer layer includes a first type buffer layer and a second type buffer layer which are stacked, and the doping concentration of the first type buffer layer is higher than that of the second type buffer layer, thereby ensuring the high resistance characteristics of the buffer layer in the epitaxial structure and ensuring good crystal quality of the buffer layer. In addition, a high resistance buffer layer is achieved by a specific doping concentration relationship between the first type buffer layer and the second type buffer layer. For example, the buffer layer can be doped at a low concentration. In this way, it is guaranteed that the reliability of the epitaxial structure and the semiconductor device is improved without deteriorating the performance such as leakage current and breakdown of the semiconductor device.
[0072] Based on the above embodiment, the first type buffer layer 1221 may include at least one first buffer layer, and the second type buffer layer 1222 may include at least one second buffer layer, where the doping concentration of the first buffer layer is higher than the doping concentration of the second buffer layer.
[0073] Exemplarily, the first type buffer layer 1221 may include one or more first buffer layers, and the second type buffer layer 1222 may include one or more second buffer layers, with the doping concentration of each first buffer layer being higher than the doping concentration of the second buffer layer. This ensures high resistance characteristics of the buffer layer while ensuring good crystal quality of the buffer layer. The buffer layer may also be lightly doped. This ensures that the reliability of the epitaxial structure and the semiconductor device is improved without degrading performance such as leakage current and breakdown of the semiconductor device.
[0074] Specifically, the first type buffer layer 1221 may include two first buffer layers, and the second type buffer layer 1222 may include two second buffer layers. In the embodiment of the present invention, the first type buffer layer 1221 includes two first buffer layers, and the second type buffer layer 1222 includes two second buffer layers. For example, as shown in FIG. 5, the first type buffer layer 1221 includes a first buffer layer 1221a and a first buffer layer 1221b that are stacked together, and the first buffer layer 1221a is located closer to the substrate 11. The doping concentration of the first buffer layer 1221a is equal to or higher than the doping concentration of the first buffer layer 1221b. The second type buffer layer 1222 includes a second buffer layer 1222a and a second buffer layer 1222b that are stacked together, and the second buffer layer 1222a is located closer to the substrate 11. The doping concentration of the second A buffer layer 1222a is higher than the doping concentration of the second B buffer layer 1222b.
[0075] 5, the buffer layer 122 includes, from bottom to top, a first buffer layer 1221a, a first buffer layer 1221b, a second buffer layer 1222a, and a second buffer layer 1222b. The doping concentration of either the first buffer layer 1221a or the first buffer layer 1221b is higher than the doping concentration of either the second buffer layer 1222a or the second buffer layer 1222b, the doping concentration of the first buffer layer 1221a is higher than the doping concentration of the first buffer layer 1221b, and the doping concentration of the second buffer layer 1222a is higher than the doping concentration of the second buffer layer 1222b. In this way, the doping concentration of the buffer layer located at the bottom in the buffer layer 122 is not lower than the doping concentration of the buffer layer located at the top. Furthermore, the doping concentrations of the first buffer layer 1221a, the first buffer layer 1221b, the second buffer layer 1222a, and the second buffer layer 1222b decrease in the order of increasing distance from the substrate. In this way, a high resistance buffer layer is achieved by a specific doping concentration relationship in the buffer layers, but a specific doping concentration is not required for the buffer layers. This ensures that the reliability of the epitaxial structure and the semiconductor device is improved without deteriorating the performance of the semiconductor device, such as leakage current and breakdown.
[0076] Based on the above embodiment, the first A buffer layer 1221a, the first B buffer layer 1221b, the second A buffer layer 1222a and the second B buffer layer 1222b may all be doped with carbon ions. The doping concentration of the first A buffer layer 1221a is C1, the doping concentration of the first B buffer layer 1221b is C2, the doping concentration of the second A buffer layer 1222a is C3, and the doping concentration of the second B buffer layer 1222b is C4, where C1>C2≧C3>C4.
[0077] For example, by designing the doping concentration C1 of the first A buffer layer 1221a, the doping concentration C2 of the first B buffer layer 1221b, the doping concentration C3 of the second A buffer layer 1222a, and the doping concentration C4 of the second B buffer layer 1222b to satisfy C1>C2≧C3>C4, it is ensured that the doping concentration of the lower buffer layer in the buffer layer 122 is not lower than the doping concentration of the upper buffer layer. By rationally designing the doping concentration relationship of the first A buffer layer 1221a, the first B buffer layer 1221b, the second A buffer layer 1222a, and the second B buffer layer 1222b, it is ensured that the crystal quality is not deteriorated while achieving the same effect as the conventional high resistance GaN buffer layer.
[0078] Based on the above embodiment, the first buffer layer 1221a and the first buffer layer 1221b are further doped with iron ions, and the second buffer layer 1222a and the second buffer layer 1222b are not doped with iron ions. The doping concentration of the iron ions in the first buffer layer 1221a is a fifth doping concentration, and the doping concentration of the iron ions in the first buffer layer 1221b is a sixth doping concentration, where the fifth doping concentration and the sixth doping concentration are the same.
[0079] For example, the first buffer layer 1221a and the first buffer layer 1221b may be doped with iron ions at the same concentration. The second buffer layer 1222a and the second buffer layer 1222b are not doped with iron ions. By rationally designing the doping components in each buffer layer, it is ensured that the crystal quality is not deteriorated while achieving the same effect as the conventional high resistance GaN buffer layer.
[0080] Furthermore, the doping concentration of carbon ions in the first A buffer layer 1221a is a first doping concentration C1, and the doping concentration of iron ions in the first A buffer layer 1221a is a fifth doping concentration C5, where C1 / C5=(0.5-1.2) / 10. The doping concentration of carbon ions in the first B buffer layer 1221b is a second doping concentration C2, and the doping concentration of iron ions in the first B buffer layer 1221b is a sixth doping concentration C6, where C2 / C6=(0.1-0.3) / 10. The doping concentration of carbon ions in the second A buffer layer 1222a is a third doping concentration C3, where C3=C2. The doping concentration of carbon ions in the second B buffer layer 1222b is a fourth doping concentration C4, where C4 / C3=(1-2) / 10. By rationally designing the doping ratios of carbon ions and iron ions in the same buffer layer and the doping ratios of carbon ions in different buffer layers, an excellent high-resistance buffer layer is finally ensured, the crystal quality of the buffer layer is good, and the quality and reliability of the epitaxial structure and the semiconductor device are ensured.
[0081] Furthermore, the doping concentrations of carbon ions in the first B buffer layer 1221b, the second A buffer layer 1222a, and the second B buffer layer 1222b are all directly or indirectly related to the doping concentration of carbon ions in the first A buffer layer 1221a, and the doping concentration of carbon ions in the first A buffer layer 1221a is related to the doping concentration of iron ions in the first A buffer layer 1221a. Therefore, when the doping concentration of iron ions in the first A buffer layer 1221a changes, the doping concentration of carbon ions in the first A buffer layer 1221a must be correspondingly adjusted, and the doping concentrations of carbon ions in the first B buffer layer 1221b, the second A buffer layer 1222a, and the second B buffer layer 1222b must also be correspondingly adjusted. For example, if the doping concentration of iron ions in the first A buffer layer 1221a is increased to twice the doping concentration, the doping concentration of carbon ions in the first A buffer layer 1221a needs to be adjusted correspondingly, and the doping concentrations of carbon ions in the first B buffer layer 1221b, the second A buffer layer 1222a and the second B buffer layer 1222b also need to be adjusted correspondingly.
[0082] Specifically, the doping concentration C1 of carbon ions and the doping concentration C5 of iron ions in the first A doping layer 1221a satisfy C1 / C5=(0.5~1.2) / 10, and may be C1 / C5=0.5 / 10, C1 / C5=0.8 / 10, C1 / C5=1.0 / 10, or C1 / C5=1.2 / 10. In the embodiment of the present invention, the specific doping ratio between the doping concentration C1 of carbon ions and the doping concentration C5 of iron ions in the first A doping layer 1221a is not limited, and it is sufficient to satisfy C1 / C5=(0.5~1.2) / 10. Furthermore, the doping concentration C2 of the carbon ions and the doping concentration C6 of the iron ions in the first B doping layer 1221b satisfy C2 / C6=(0.1 to 0.3) / 10, and may be C2 / C6=0.1 / 10, C2 / C6=0.2 / 10, or C2 / C6=0.3 / 10. In the embodiment of the present invention, the specific doping ratio between the doping concentration C2 of the carbon ions and the doping concentration C6 of the iron ions in the first B doping layer 1221b is not limited, and it is sufficient that C2 / C6=(0.1 to 0.3) / 10 is satisfied. Furthermore, the doping concentration C4 of the carbon ions in the second B doping layer 1222b and the doping concentration C3 of the carbon ions in the second A doping layer 1222a satisfy C4 / C3=(1-2) / 10, and may be C4 / C3=1 / 10, C4 / C3=1.5 / 10, or C4 / C3=2 / 10. In the embodiment of the present invention, the specific doping ratio between the doping concentration C4 of the carbon ions in the second B doping layer 1222b and the doping concentration C3 of the carbon ions in the second A doping layer 1222a is not limited, and it is sufficient to satisfy C4 / C3=(1-2) / 10.
[0083] Furthermore, the doping concentration C5 of iron ions in the first buffer layer 1221a is C5=1*10 18 / cm 3 ~1*10 19 / cm 3 The doping concentration C6 of the iron ions in the first buffer layer 1221b may be C6=1*10 18 / cm 3 ~1*10 19 / cm 3The doping concentration of iron ions in the first buffer layer A 1221a and the doping concentration of iron ions in the first buffer layer B 1221b are both low doping concentrations, which ensures the stability of the epitaxial structure and the performance of the semiconductor device without affecting the crystal quality of each buffer layer. In a possible embodiment, the doping concentration C1 of carbon ions in the first buffer layer A 1221a is 2*10 17 / cm 3 The doping concentration C5 of iron ions in the first buffer layer 1221a is 2*10 18 / cm 3 The doping concentration C2 of the carbon ions in the first buffer layer 1221b is 5*10 16 / cm 3 The doping concentration C6 of iron ions in the first buffer layer 1221b is 2*10 18 / cm 3 The doping concentration C3 of the carbon ions in the second buffer layer 1222a is 5*10 16 / cm 3 The doping concentration of iron ions in the second buffer layer A 1222a is 0, and the doping concentration C4 of carbon ions in the second buffer layer B 1222b is 2.5*10 16 / cm 3 In other words, the doping concentration of iron ions in the second buffer layer 1222b may be zero.
[0084] The above examples have described the doping conditions of each buffer layer, and by rationally designing the doping concentration of each buffer layer, the high resistance characteristics of the buffer layer in the epitaxial structure can be ensured, while the good crystal quality of the buffer layer can be ensured, so that the performance of the semiconductor device, such as leakage current and breakdown, can be prevented from being degraded, and the reliability of the epitaxial structure and the semiconductor device can be improved.
[0085] The thicknesses of the first type buffer layer 1221 and the second type buffer layer 1222 will be described below.
[0086] Optionally, the thickness of the first buffer layer is greater than the thickness of the second buffer layer.
[0087] Exemplarily, the first type buffer layer 1221 may include one or more first buffer layers, and the second type buffer layer 1222 may include one or more second buffer layers. The thickness of each first buffer layer is greater than the thickness of the second buffer layer. This ensures good crystal quality of the buffer layer while ensuring high resistance characteristics of the buffer layer. The buffer layer may also be lightly doped. In this way, it is guaranteed that the reliability of the epitaxial structure and the semiconductor device is improved without degrading the performance such as leakage current and breakdown of the semiconductor device.
[0088] Specifically, the first type buffer layer 1221 may include two first buffer layers, and the second type buffer layer 1222 may include two second buffer layers. In the embodiment of the present invention, a case where the first type buffer layer 1221 includes two first buffer layers and the second type buffer layer 1222 includes two second buffer layers will be described as an example. Exemplarily, as shown in FIG. 5, the first type buffer layer 1221 includes a first A buffer layer 1221a and a first B buffer layer 1221b that are stacked together. The first A buffer layer 1221a is located on the side closer to the substrate 11. The thickness of the first A buffer layer 1221a is equal to or greater than the thickness of the first B buffer layer 1221b. The second type buffer layer 1222 includes a second A buffer layer 1222a and a second B buffer layer 1222b that are stacked together. The second A buffer layer 1222a is located on the side closer to the substrate 11. The thickness of the second first buffer layer 1222a is greater than the thickness of the second second buffer layer 1222b.
[0089] For example, as shown in FIG. 5, the buffer layer 122 may include, from bottom to top, a first A buffer layer 1221a, a first B buffer layer 1221b, a second A buffer layer 1222a, and a second B buffer layer 1222b. The thickness of either the first A buffer layer 1221a or the first B buffer layer 1221b is greater than the thickness of either the second A buffer layer 1222a or the second B buffer layer 1222b, the thickness of the first A buffer layer 1221a is greater than the thickness of the first B buffer layer 1221b, and the thickness of the second A buffer layer 1222a is greater than the thickness of the second B buffer layer 1222b. In this way, the thickness of any of the buffer layers located at the bottom of the buffer layer 122 is not less than the thickness of the buffer layer located at the top. For example, the thickness h1 of the first type A buffer layer close to the substrate is used as a reference, and the thickness of each buffer layer decreases in order in the direction away from the substrate. That is, the thickness h1 of the first type A buffer layer is a predetermined thickness, and the thicknesses h of the other buffer layers are determined according to the relationship with the thickness of h1, that is, h≦h1. In this way, a high resistance buffer layer is achieved by the specific thickness relationship in the buffer layer, and the doping concentration of the buffer layer is not required, which ensures that the performance of the semiconductor device, such as leakage current and breakdown, is not degraded, and the reliability of the epitaxial structure and the semiconductor device is improved.
[0090] Based on the above example, the thickness of the first A buffer layer 1221a is h1, the thickness of the first B buffer layer 1221b is h2, the thickness of the second A buffer layer 1222a is h3, and the thickness of the second B buffer layer 1222b is h4, where h2=h1, 2 / 10≦h3 / h2≦9 / 10, and 4 / 10≦h4 / h3≦9 / 10. For example, by rationally designing the thickness ratios among the first A buffer layer 1221a, the first B buffer layer 1221b, the second A buffer layer 1222a, and the second B buffer layer 1222b so that the thickness h1 of the first A buffer layer 1221a, the thickness h2 of the first B buffer layer 1221b, the thickness h3 of the second A buffer layer 1222a, and the thickness h4 of the second B buffer layer 1222b satisfy h2=h1, 2 / 10≦h3 / h2≦9 / 10, 410≦h4 / h3≦9 / 10, it is possible to achieve the same effect as a conventional high-resistance GaN buffer layer while ensuring that the crystal quality is not degraded.
[0091] Specifically, the thickness h2 of the first buffer layer 1221b and the thickness h3 of the second buffer layer 1222a satisfy 2 / 10≦h3 / h2≦9 / 10, and may be h3 / h2=2 / 10, h3 / h2=4 / 10, h3 / h2=6 / 10, h3 / h2=8 / 10, or h3 / h2=9 / 10. In the embodiment of the present invention, the specific proportional relationship between the thickness h2 of the first buffer layer 1221b and the thickness h3 of the second buffer layer 1222a is not limited, and it is sufficient that 2 / 10≦h3 / h2≦9 / 10 is satisfied. Furthermore, the thickness h3 of the second A buffer layer 1222a and the thickness h4 of the second B buffer layer 1222b satisfy 4 / 10≦h4 / h3≦9 / 10, and may be h4 / h3=4 / 10, h4 / h3=6 / 10, h4 / h3=8 / 10, or h4 / h3=9 / 10. In the embodiment of the present invention, the specific proportional relationship between the thickness h3 of the second A buffer layer 1222a and the thickness h4 of the second B buffer layer 1222b is not limited, and it is sufficient that they satisfy 4 / 10≦h4 / h3≦9 / 10. As a possible embodiment, the thickness h1 of the first A buffer layer 1221a may be 500 nm, the thickness h2 of the first B buffer layer 1221b may be 500 nm, the thickness h3 of the second A buffer layer 1222a may be 400 nm, and the thickness h4 of the second B buffer layer 1222b may be 300 nm.
[0092] In the above embodiment, the thickness of each buffer layer is described. By rationally designing the thickness of each buffer layer, the high resistance property of the buffer layer in the epitaxial structure is ensured, while the good crystal quality of the buffer layer is ensured, and the performance such as leakage current and breakdown of the semiconductor device is not deteriorated, and the reliability of the epitaxial structure and the semiconductor device is improved.
[0093] In the above embodiment, a specific design method of the epitaxial layer is described based on the doping concentration and thickness of each different buffer layer. It should be understood that the doping concentration and thickness conditions of different buffer layers can be considered comprehensively when actually designing the epitaxial layer. For example, in the case of a buffer layer with a relatively large thickness, the doping concentration can be relatively high, and in the case of a buffer layer with a relatively small thickness, the doping concentration can be relatively low. By comprehensively considering the doping concentration and thickness conditions of different buffer layers, the high resistance characteristics of the buffer layer in the epitaxial structure are ensured, while the good crystal quality of the buffer layer is ensured, and the reliability of the epitaxial structure and the semiconductor device is improved without deteriorating the performance such as leakage current and breakdown of the semiconductor device.
[0094] Based on the above embodiment, as shown in FIG. 5 , the epitaxial layer 12 provided in the embodiment of the present invention may further include a nucleation layer 121 located on the side of the buffer layer 122 closer to the substrate 11, a spacer layer 123 located on the side of the buffer layer 122 farther from the substrate 11, a potential barrier layer 124 located on the side of the spacer layer 123 farther from the substrate 11 and forming a heterojunction structure together with the buffer layer 122, and a cap layer 125 located on the side of the potential barrier layer 124 farther from the substrate 11.
[0095] Illustratively, the nucleation layer 121 influences parameters such as the crystal quality, surface topography, and electrical properties of other film layers located above the nucleation layer 121 in the epitaxial layer 12. The nucleation layer 121 primarily serves to match the material of the substrate 11 with the semiconductor material layers in the heterojunction structure of the epitaxial layer 12.
[0096] The spacer layer 123 may be an AlN spacer layer, which can increase the potential barrier, increase the confinement of the two-dimensional electron gas, reduce alloy scattering, and improve mobility.
[0097] The potential barrier layer 124 may be an AlGaN potential barrier layer. The potential barrier layer 124 forms a heterojunction structure together with the buffer layer 122, and forms a transport channel for the two-dimensional electron gas.
[0098] The main function of the cap layer 125 is to reduce the surface state, reduce the surface leakage current of the next semiconductor device, and suppress the current collapse, thereby improving the performance and reliability of the epitaxial structure and the semiconductor device. Optionally, the material of the cap layer 125 is a group III nitride, preferably P-type doped gallium nitride (P-GaN). The P-GaN structure can effectively lower the potential barrier of the AlGaN layer.
[0099] Based on the same inventive idea as above, an embodiment of the present invention provides a semiconductor device. The semiconductor device provided in the embodiment of the present invention includes the epitaxial structure of the semiconductor device described in the above embodiment. FIG. 6 is a structural schematic diagram of the semiconductor device provided in the embodiment of the present invention. As shown in FIG. 6, the semiconductor device provided in the embodiment of the present invention includes: A substrate 11; an epitaxial layer 12 on one side of the substrate 11, the epitaxial layer 12 including, in sequence on the one side of the substrate 11, a nucleation layer 121, a buffer layer 122, a spacer layer 123, a potential barrier layer 124, and a cap layer 125; a source electrode 131 and a drain electrode 132 located on the side of the potential barrier layer 124 farther from the substrate 11; a gate electrode 133 located on the side of the cap layer 125 farther from the substrate 11 and between the source electrode 131 and the drain electrode 132; Includes.
[0100] Exemplarily, the source electrode 131 and the drain electrode 132 are located on the side of the potential barrier layer 124 remote from the substrate 11. The source electrode 131 and the drain electrode 132 each form an ohmic contact with the potential barrier layer 124. The gate electrode 133 is located between the source electrode 131 and the drain electrode 132, and is located on the side of the cap layer 125 remote from the substrate 11. The gate electrode 133 forms a Schottky contact with the cap layer 125.
[0101] It should be understood that the embodiment of the present invention ensures, from the viewpoint of the structural design of the semiconductor device, that the crystal quality of the nucleation layer in the semiconductor device is improved without increasing the thermal resistance of the nucleation layer. Semiconductor devices include high-power gallium nitride high electron mobility transistors (HEMTs) that operate in high-voltage and high-current environments, silicon-on-insulator (SOI) transistors, gallium arsenide (GaAs)-based transistors, metal-oxide-semiconductor field-effect transistors (MOSFETs), metal-semiconductor field-effect transistors (MISFETs), double heterojunction field-effect transistors (DHFETs), junction field-effect transistors (JFETs), metal-semiconductor field-effect transistors (MESFETs), and metal-semiconductor heterojunction field-effect transistors (MFETs). Field-Effect Transistor (abbreviated as MISHFET) or other field effect transistors, but are not limited to these.
[0102] Based on the same inventive idea as above, an embodiment of the present invention further provides a method for manufacturing an epitaxial structure of a semiconductor device. Figure 7 is a flow chart of the method for manufacturing an epitaxial structure of a semiconductor device provided in an embodiment of the present invention. As shown in Figure 7, the method for manufacturing an epitaxial structure of a semiconductor device provided in an embodiment of the present invention may include the following steps S110 and S120. S110: Provide a substrate. S120: Producing an epitaxial layer on one side of the substrate, the epitaxial layer including a buffer layer, the buffer layer including a first type buffer layer and a second type buffer layer stacked together, the first type buffer layer being located closer to the substrate, and the doping concentration of the first type buffer layer being higher than the doping concentration of the second type buffer layer.
[0103] The C doping concentration required to obtain a high-resistance GaN buffer layer is >1*10 19 / cm 3 However, doing so may result in a deterioration in the crystal quality of the GaN buffer layer. The Fe doping concentration required to obtain a high-resistance GaN buffer layer is >1*10 19 / cm 3 must be satisfied, but doing so may affect the performance of the final device. In the embodiment of the present invention, the buffer layer 122 includes multiple buffer layers, for example, a first type buffer layer 1221 and a second type buffer layer 1222 that are stacked together, and the first type buffer layer 1221 is located closer to the substrate 11, and the doping concentration of the first type buffer layer 1221 is designed to be higher than the doping concentration of the second type buffer layer 1222, thereby achieving a high resistance buffer layer due to the specific doping concentration relationship between the first type buffer layer 1221 and the second type buffer layer 1222, and not requiring a specific doping concentration of the buffer layer. For example, by making the buffer layer lightly doped, it is guaranteed that the reliability of the epitaxial structure and the semiconductor device is improved without deteriorating the performance of the semiconductor device, such as leakage current and breakdown.
[0104] From the above, in the manufacturing method of the epitaxial structure of the semiconductor device provided in the embodiment of the present invention, the buffer layer includes a first type buffer layer and a second type buffer layer which are stacked, and the doping concentration of the first type buffer layer is higher than that of the second type buffer layer, thereby ensuring the high resistance characteristics of the buffer layer in the semiconductor device and ensuring good crystal quality of the buffer layer. In addition, the specific doping concentration relationship between the first type buffer layer and the second type buffer layer achieves a high resistance buffer layer, and does not require a specific doping concentration of the buffer layer. For example, the buffer layer can be doped at a low concentration. In this way, it is guaranteed that the reliability of the epitaxial structure and the semiconductor device is improved without deteriorating the performance of the semiconductor device, such as leakage current and breakdown.
[0105] Based on the above examples, the production of an epitaxial layer on one side of the substrate can be Producing a nucleation layer on one side of the substrate; - fabricating a buffer layer on a side of the nucleation layer remote from the substrate; fabricating a spacer layer on a side of the buffer layer remote from the substrate; - producing, on the side of the spacer layer remote from the substrate, a potential barrier layer which forms a heterojunction structure together with the buffer layer; fabricating a cap layer on a side of the potential barrier layer remote from the substrate; may include:
[0106] The nucleation layer matches the substrate material with the semiconductor material layer in the heterojunction structure of the epitaxial layer. The spacer layer increases the potential barrier, improves the confinement of the two-dimensional electron gas, reduces alloy scattering, and improves mobility. The potential barrier layer forms a heterojunction structure with the buffer layer to form a transport channel for the two-dimensional electron gas. The cap layer reduces surface states, reduces surface leakage in the subsequent semiconductor device, and suppresses current collapse, improving the performance and reliability of the epitaxial structure and the semiconductor device.
[0107] Based on the same inventive idea as above, an embodiment of the present invention further provides a method for manufacturing a semiconductor device. Figure 8 is a flow chart of the method for manufacturing a semiconductor device provided in an embodiment of the present invention. As shown in Figure 8, the method for manufacturing a semiconductor device provided in an embodiment of the present invention may include the following steps S210 to S230. S210: Provide a substrate. S220: Producing an epitaxial layer on one side of the substrate, the epitaxial layer including a nucleation layer, a buffer layer, a spacer layer, a potential barrier layer and a cap layer, sequentially located on one side of the substrate. S230: Fabricating a source electrode and a drain electrode on the potential barrier layer on a side remote from the substrate, and fabricating a gate electrode on the cap layer on a side remote from the substrate, the gate electrode being located between the source electrode and the drain electrode.
[0108] The source electrode and the drain electrode each form an ohmic contact with the potential barrier layer, and the gate electrode forms a Schottky contact with the cap layer.
[0109] It should be noted that the above description is merely a preferred embodiment of the present invention and the technical principles used. Those skilled in the art can understand that the present invention is not limited to the specific embodiments described herein, and various obvious modifications, rearrangements, mutual combinations and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in detail by the above embodiments, the present invention is not limited to the above embodiments, and may further include many other equivalent embodiments without departing from the spirit of the present invention, and the scope of the present invention is determined by the appended claims.
Claims
1. 1. An epitaxial structure for a semiconductor device, comprising: A substrate; an epitaxial layer located on one side of the substrate, the epitaxial layer including a nucleation layer located on one side of the substrate and a buffer layer located on a side of the nucleation layer remote from the substrate; Including, a thickness ratio of the buffer layer to the nucleation layer such that the product of the buffer layer thickness and the nucleation layer thickness is equal to or greater than a first predetermined value and equal to or less than a second predetermined value that is greater than the first predetermined value; the buffer layer includes a first type buffer layer and a second type buffer layer stacked one on the other, the first type buffer layer being located closer to the substrate, and the doping concentration of the first type buffer layer being higher than the doping concentration of the second type buffer layer; the first type of buffer layer includes at least one first buffer layer, and the second type of buffer layer includes at least one second buffer layer; the doping concentration of the first buffer layer is higher than the doping concentration of the second buffer layer; the first type buffer layer includes a first buffer layer A and a first buffer layer B stacked together, the first buffer layer A being located closer to the substrate, and the doping concentration of the first buffer layer A being equal to or greater than the doping concentration of the first buffer layer B; the second type buffer layer includes a second A buffer layer and a second B buffer layer that are stacked together, the second A buffer layer is located closer to the substrate, and the doping concentration of the second A buffer layer is higher than the doping concentration of the second B buffer layer; the first buffer layer A, the first buffer layer B, the second buffer layer A, and the second buffer layer B are all doped with carbon ions; The doping concentration of carbon ions in the first buffer layer A is a first doping concentration C1, the doping concentration of carbon ions in the first buffer layer B is a second doping concentration C2, the doping concentration of carbon ions in the second buffer layer A is a third doping concentration C3, and the doping concentration of carbon ions in the second buffer layer B is a fourth doping concentration C4, where C1>C2≧C3>C4. An epitaxial structure characterized by:
2. 2. The epitaxial structure according to claim 1, wherein the thickness of the nucleation layer is h1 (μm), the thickness of the buffer layer is h2 (μm), and the product of the thickness of the nucleation layer and the thickness of the buffer layer is h1 × h2, and 0.1≦h1 × h2≦0.
25.
3. 3. The epitaxial structure of claim 2, wherein h1=0.17 / h2.
4. If the thickness of the nucleation layer is h1, the thickness of the substrate is h3, and the thickness ratio obtained by dividing the thickness of the nucleation layer by the thickness of the substrate is h1 / h3, then 2×10 -5 ≦h1 / h3≦5×10 -4 2. The epitaxial structure of claim 1, wherein:
5. 2. The epitaxial structure according to claim 1, wherein the thickness of the nucleation layer is h1, the thickness of the epitaxial layer is h4, and the thickness ratio obtained by dividing the thickness of the nucleation layer by the thickness of the epitaxial layer is h1 / h4, and the ratio satisfies 0.05≦h1 / h4≦0.
3.
6. 6. The epitaxial structure of claim 5, wherein 0.07≦h1 / h4≦0.
1.
7. 2. The epitaxial structure according to claim 1, wherein the thickness of said nucleation layer is h1 (nm), and the thickness satisfies 100 (nm)≦h1≦150 (nm).
8. the first buffer layer A and the first buffer layer B are further doped with iron ions, and the second buffer layer A and the second buffer layer B are not doped with iron ions; 2. The epitaxial structure of claim 1, wherein the doping concentration of iron ions in the first buffer layer A is a fifth doping concentration, and the doping concentration of iron ions in the first buffer layer B is a sixth doping concentration, wherein the fifth doping concentration is the same as the sixth doping concentration.
9. The doping concentration of carbon ions in the first buffer layer is C1 ( / cm 3 ), and the doping concentration of iron ions in the first buffer layer A is C5 ( / cm 3 ), then C1 / C5 = (0.5 to 1.2) / 10, The doping concentration of carbon ions in the first buffer layer is C2 ( / cm 3 ), and the doping concentration of iron ions in the first buffer layer is C6 ( / cm 3 ), then C2 / C6 = (0.1 to 0.3) / 10, The doping concentration of carbon ions in the second buffer layer is C3 ( / cm 3 ), then C3 = C2, The doping concentration of carbon ions in the second buffer layer is set to C4 ( / cm 3 9. The epitaxial structure according to claim 8, wherein C4 / C3=(1 to 2) / 10.
10. 10. The epitaxial structure of claim 9, wherein the thickness of the first buffer layer is greater than the thickness of the second buffer layer.
11. the first type of buffer layer includes a first buffer layer A and a first buffer layer B that are stacked together, the first buffer layer A is located closer to the substrate, and the thickness of the first buffer layer A is equal to or greater than the thickness of the first buffer layer B; 11. The epitaxial structure of claim 10, wherein the second type buffer layer comprises a second A buffer layer and a second B buffer layer stacked together, the second A buffer layer being located closer to the substrate, and the thickness of the second A buffer layer being greater than the thickness of the second B buffer layer.
12. A method for manufacturing an epitaxial structure for a semiconductor device for manufacturing the epitaxial structure according to any one of claims 1 to 11, comprising the steps of: providing a substrate; fabricating a nucleation layer on one side of the substrate; forming a buffer layer on the side of the nucleation layer remote from the substrate; fabricating a spacer layer on a side of the buffer layer remote from the substrate; forming a potential barrier layer on the side of the spacer layer remote from the substrate, which forms a heterojunction structure together with the buffer layer; forming a cap layer on the side of the potential barrier layer remote from the substrate; Including, The manufacturing method, wherein the thickness of the buffer layer is inversely proportional to the thickness of the nucleation layer.
Citation Information
Patent Citations
High pressure resistant nitride semiconductor epitaxial structure and growing method thereof
CN104600109A
Fabrication method for transistor with composite gate dielectric GaN-based insulating gate and high electron mobility
CN106373884A
Group 13 nitride semiconductor substrate
JP2016219690A
Substrate for semiconductor device, semiconductor device, and manufacturing method of substrate for semiconductor device
JP2018046207A
Epitaxial substrate and method for manufacturing epitaxial substrate