Reflective mask blanks and reflective masks

A multilayer reflective film with controlled low and high refractive index layers in reflective mask blanks addresses the challenge of high background noise in defect inspection, ensuring high reflectance and effective defect detection in EUV lithography.

JP7578093B2Active Publication Date: 2024-11-06SHIN ETSU CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021187205
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-11-17
Publication Date
2024-11-06
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

Existing reflective mask blanks for EUV lithography face challenges in detecting phase defects due to high background noise during defect inspection, which is exacerbated by the use of additive elements like nitrogen, carbon, and boron in the multilayer reflective film, leading to increased interface roughness and reduced reflectance.

Method used

A multilayer reflective film structure with alternating low and high refractive index layers, where the low refractive index layers consist of a two-layer structure of molybdenum and additional elements such as nitrogen, carbon, boron, silicon, or hydrogen, with controlled thickness and crystallinity, to maintain high reflectance and reduce background noise during defect inspection.

Benefits of technology

The proposed structure achieves high reflectance for EUV light while significantly lowering background noise during defect inspection, enabling effective detection of phase defects in reflective masks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578093000001
    Figure 0007578093000001
  • Figure 0007578093000002
    Figure 0007578093000002
Patent Text Reader

Abstract

SOLUTION: Provided is a reflective mask blank, including a substrate and a multilayer reflection film that is formed on one main surface of the substrate and reflects exposure light. The multilayer reflection film has a periodically laminated structure portion with low refractive index layers and high refractive index layers alternately laminated, and at least one of the low refractive index layer has a two-layered structure consisting of a first sublayer and a second sublayer, wherein the first sublayer contains molybdenum, and at least one additive element selected from the group consisting of nitrogen, carbon, boron, silicon and hydrogen and has a thickness of more than 0.3 nm and 0.6 nm or less, and the second sublayer contains molybdenum and is substantively free of the other elements.EFFECT: According to the invention, a reflective mask blank that includes a multilayer reflection film having a sufficiently lowered background level in defect inspection with a high reflectance with respect to exposure light can be provided.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective mask used in the manufacture of semiconductor devices such as LSIs, and a reflective mask blank which is the material thereof. [Background technology]

[0002] In the manufacturing process of semiconductor devices (semiconductor device), photolithography technology is repeatedly used, in which exposure light is irradiated onto a transfer mask, and the circuit pattern formed on the mask is transferred onto a semiconductor substrate (semiconductor wafer) via a reduced projection optical system. Conventionally, the wavelength of the exposure light has been mainly 193 nm using argon fluoride (ArF) excimer laser light, and a process called multi-patterning, which combines exposure processes and processing processes multiple times, has been used to ultimately form patterns with dimensions smaller than the exposure wavelength.

[0003] However, as the device patterns continue to become finer, the formation of even finer patterns is required, and thus EUV lithography technology using EUV (Extreme Ultra Violet) light, which has a shorter wavelength than ArF excimer laser light, as exposure light has been developed. EUV light is light with a wavelength of, for example, about 10 to 20 nm, more specifically, light with a wavelength of about 13.5 nm. This EUV light has extremely low permeability to materials, and conventional transmission type projection optical systems and masks cannot be used, so reflective optical elements are used. For this reason, reflective masks have been proposed as masks for pattern transfer. In a reflective mask, a multilayer reflective film that reflects EUV light is formed on a substrate, and an absorber film that absorbs EUV light is formed in a pattern on the multilayer reflective film. On the other hand, a mask in a state before patterning the absorber film (including a state in which a resist layer is formed) is called a reflective mask blank, and this is used as a material for a reflective mask. In general, a reflective mask and a reflective mask blank that reflect EUV light are called an EUV mask and an EUV mask blank, respectively.

[0004] The EUV mask blank has a basic structure including a low thermal expansion substrate and a multilayer reflective film formed thereon to reflect EUV light, and generally further includes an absorber film formed on the multilayer reflective film to absorb EUV light. As the multilayer reflective film, a multilayer reflective film is usually used that has a necessary reflectance for EUV light by alternately stacking molybdenum (Mo) films and silicon (Si) films. Furthermore, a ruthenium (Ru) film is formed on the outermost layer of the multilayer reflective film as a protective layer for protecting the multilayer reflective film. On the other hand, as the absorber film, tantalum (Ta) or the like that has a relatively large extinction coefficient for EUV light is used (JP Patent Publication 2002-246299 (Patent Document 1)). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-246299 A [Patent Document 2] JP 2003-114200 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the manufacturing process of a reflective mask, after a pattern is formed by etching the absorber film of a reflective mask blank, the pattern is usually inspected, and if a defect is found, the defect is corrected. However, in the case of a reflective mask, there may be a defect called a phase defect, which is a defect that reduces the reflectance due to a disturbance in the structure of the multilayer reflective film. It is extremely difficult to directly correct this phase defect after forming the pattern of the absorber film. In this situation, it is important to detect the phase defect of the reflective mask blank. For example, Japanese Patent Application Laid-Open No. 2003-114200 (Patent Document 2) discloses a technology that uses a dark-field inspection image as a method for detecting defects inside a multilayer reflective film using EUV light.

[0007] In order to detect even minute phase defects with high sensitivity in defect detection, it is necessary to reduce the intensity of scattered light in defect-free parts of the multilayer reflective film during defect inspection after the multilayer reflective film is formed, that is, the background level (BGL). Therefore, while it is more advantageous for a reflective mask blank (EUV mask blank) to have a higher reflectance in the exposure light (EUV light of about 13.5 nm), it is also necessary to reduce the background level during defect inspection using the exposure light (EUV light).

[0008] When a multilayer reflective film has a periodic laminate structure of molybdenum (Mo) layers and silicon (Si) layers, the reflectivity tends to be higher when the molybdenum (Mo) does not contain added elements such as nitrogen (N), carbon (C), or boron (B). However, if the crystal grains become coarse during the formation of the molybdenum (Mo) layer, the interface roughness between the layers, the surface roughness of the multilayer reflective film, or both, will increase, resulting in a higher background level during defect inspection.

[0009] On the other hand, in order to reduce the background level, it is effective to add additive elements such as nitrogen (N), carbon (C), and boron (B) to molybdenum (Mo) to create an amorphous structure; however, this causes a large decrease in reflectance due to changes in the optical properties (n, k) caused by the additive elements and promotion of intermixing of the components of the molybdenum (Mo) and silicon (Si) layers at the interface between the two layers.

[0010] The present invention has been made to solve the above-mentioned problems, and has an object to provide a reflective mask blank and a reflective mask having a multilayer reflective film that has high reflectance and reduces the background level during defect inspection. [Means for solving the problem]

[0011] As a result of intensive research into solving the above-mentioned problems, the inventors have found that in a multilayer reflective film having a periodic stacked structure in which low refractive index layers and high refractive index layers are alternately stacked, and preferably further having a protective layer formed in contact with the side of the periodic stacked structure away from the substrate, the low refractive index layer has a two-layer structure consisting of a layer containing molybdenum (Mo) and at least one additive element selected from nitrogen (N), carbon (C), boron (B), silicon (Si) and hydrogen (H), and a layer containing molybdenum (Mo) and substantially no elements other than molybdenum (Mo), thereby resulting in a multilayer reflective film having sufficiently high reflectance to exposure light and a sufficiently reduced background level (BGL) during defect inspection, which has led to the present invention.

[0012] Accordingly, the present invention provides the following reflective mask blank and reflective mask. 1. A reflective mask blank having a substrate and a multilayer reflective film that reflects exposure light and is formed on one main surface of the substrate, the multilayer reflective film has a periodic laminate structure in which low refractive index layers and high refractive index layers are alternately laminated, At least one of the low refractive index layers constituting the multilayer reflective film has a two-layer structure consisting of a first sublayer and a second sublayer, The first sublayer comprises molybdenum (Mo) and at least one additional element selected from nitrogen (N), carbon (C), boron (B), silicon (Si) and hydrogen (H), and has a thickness of more than 0.3 nm and less than or equal to 0.6 nm; The second sublayer includes molybdenum (Mo) and is substantially free of elements other than molybdenum (Mo). figure, The crystallite size calculated from the Mo(110) diffraction peak detected by X-ray diffraction of the multilayer reflective film is 2.6 nm or more. A reflective mask blank comprising: 2. The reflective mask blank according to 1, characterized in that in the low refractive index layer, the first sublayer is formed on the substrate side, and the second sublayer is formed on the side away from the substrate. 3. The reflective mask blank according to 1 or 2, wherein the high refractive index layer contains silicon (Si). 4 The size of the first main surface of the substrate is 152 mm square, the thickness of the substrate is 6.35 mm, and the change (ΔTIR) in flatness (TIR) ​​before and after forming the multilayer reflective film within a central 142 mm square of the first main surface is 0.7 μm or less in absolute value. 3 13. The reflective mask blank according to any one of claims 1 to 12. 5 The multilayer reflective film has a protective layer formed in contact with the side of the periodic laminate structure that is away from the substrate. 4 13. The reflective mask blank according to any one of claims 1 to 12. 6 1 to 3, characterized in that an absorber film for absorbing exposure light is further provided on the multilayer reflective film. 5 13. The reflective mask blank according to any one of claims 1 to 12. 7 . 6 2. A reflective mask obtained by patterning the absorber film of the reflective mask blank according to claim 1. The present invention also relates to the following reflective mask blank and reflective mask. [1] A reflective mask blank having a substrate and a multilayer reflective film formed on one main surface of the substrate, the multilayer reflective film reflecting exposure light, the multilayer reflective film has a periodic laminate structure in which low refractive index layers and high refractive index layers are alternately laminated, At least one of the low refractive index layers constituting the multilayer reflective film has a two-layer structure consisting of a first sublayer and a second sublayer, The first sublayer comprises molybdenum (Mo) and at least one additional element selected from nitrogen (N), carbon (C), boron (B), silicon (Si) and hydrogen (H), and has a thickness of more than 0.3 nm and less than or equal to 0.6 nm; A reflective mask blank, wherein the second sublayer contains molybdenum (Mo) and is substantially free of elements other than molybdenum (Mo). [2] The reflective mask blank according to [1], wherein in the low refractive index layer, the first sublayer is formed on the substrate side, and the second sublayer is formed on the side away from the substrate. [3] The reflective mask blank according to [1] or [2], wherein the high refractive index layer contains silicon (Si). [4]. A reflective mask blank according to any one of [1] to [3], characterized in that the size of the one main surface of the substrate is 152 mm square, the thickness of the substrate is 6.35 mm, and within a central 142 mm square portion of the one main surface, the change in flatness (TIR) ​​before and after forming the multilayer reflective film (ΔTIR) is 0.7 μm or less in absolute value. [5] A reflective mask blank according to any one of [1] to [4], characterized in that the multilayer reflective film has a protective layer formed in contact with the side of the periodic stacked structure away from the substrate. [6] A reflective mask blank according to any one of [1] to [5], further comprising an absorber film on the multilayer reflective film for absorbing exposure light. [7] A reflective mask obtained by patterning the absorber film of the reflective mask blank according to [6]. Effect of the Invention

[0013] According to the present invention, it is possible to provide a reflective mask blank having a multilayer reflective film which has a high reflectance to exposure light and a sufficiently low background level during defect inspection. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a first embodiment of the reflective mask blank of the present invention, where (A) is a reflective mask blank in which the multilayer reflective film consists of a periodic stacking structure portion, and (B) is a reflective mask blank in which the multilayer reflective film consists of a periodic stacking structure portion and a protective layer. [Diagram 2] FIG. 1 is a cross-sectional view showing an example of a second embodiment of the reflective mask blank of the present invention, where (A) is a reflective mask blank in which the multilayer reflective film consists of a periodic stacking structure portion, and (B) is a reflective mask blank in which the multilayer reflective film consists of a periodic stacking structure portion and a protective layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will now be described in further detail. The reflective mask blank of the present invention has a substrate and a multilayer reflective film formed on the substrate (on one main surface (front surface) of the substrate) that reflects exposure light, specifically a multilayer reflective film that reflects EUV light. The reflective mask blank of the present invention is suitable as a material used for manufacturing a reflective mask. The multilayer reflective film of the present invention has a periodic stacked structure in which low refractive index layers and high refractive index layers are alternately stacked. The multilayer reflective film of the present invention may further have a protective layer formed in contact with the side of the periodic stacked structure that is separated from the substrate. In the reflective mask blank of the present invention, the multilayer reflective film is preferably composed of a periodic stacked structure, or composed of a periodic stacked structure and a protective layer. The multilayer reflective film is a film that reflects EUV light, which is exposure light, in a reflective mask. The multilayer reflective film may be provided in contact with one main surface of the substrate, or an undercoat film may be provided between the substrate and the multilayer reflective film.

[0016] The reflective mask blank of the present invention is suitable as a material (EUV mask blank) for a reflective mask (EUV mask) used in EUV lithography using EUV light as exposure light. The wavelength of EUV light used in EUV lithography using EUV light as exposure light is 13 to 14 nm, and is usually light having a wavelength of about 13.5 nm. The EUV mask blank and the EUV mask are a reflective mask blank and a reflective mask, respectively.

[0017] Fig. 1 is a cross-sectional view showing an example of a first embodiment of the reflective mask blank of the present invention, and these reflective mask blanks 100A and 100B include a substrate 11 and multilayer reflective films 12A and 12B formed on and in contact with one main surface of the substrate 11. The multilayer reflective film 12A in Fig. 1(A) is composed of a periodic laminate structure 121 in which a low refractive index layer consisting of two layers, a first sublayer and a second sublayer, and a high refractive index layer are alternately laminated from the substrate side. On the other hand, the multilayer reflective film 12B in Fig. 1(B) is composed of a periodic laminate structure 121 in which a low refractive index layer consisting of two layers, a first sublayer and a second sublayer, and a high refractive index layer are alternately laminated from the substrate side, and a protective layer 122.

[0018] A reflective mask (EUV mask) having a multilayer reflective film pattern can be manufactured by patterning the multilayer reflective film using a reflective mask blank (EUV mask blank) on which a multilayer reflective film has been formed. However, it is more common to manufacture a reflective mask (EUV mask) by further forming an absorber film as a pattern formation film on the multilayer reflective film to obtain a reflective mask blank (EUV mask blank) having a substrate, a multilayer reflective film, and an absorber film, and then patterning the absorber film.

[0019] The reflective mask blank of the present invention may further include an absorber film that absorbs exposure light formed on the multilayer reflective film. Specific examples of such reflective mask blanks include those having a substrate, a multilayer reflective film that reflects exposure light formed on one main surface of the substrate, and an absorber film that absorbs exposure light formed on the multilayer reflective film. The absorber film is a film that absorbs exposure light, specifically EUV light, and reduces reflectance. The absorber film is preferably provided in contact with the multilayer reflective film (the periodic stacked structure part or protective layer of the multilayer reflective film).

[0020] Fig. 2 is a cross-sectional view showing an example of the second embodiment of the reflective mask blank of the present invention, and these reflective mask blanks 101A and 101B include a substrate 11, multilayer reflective films 12A and 12B formed on one main surface of the substrate 11 in contact with the one main surface, and an absorber film 13 formed in contact with the multilayer reflective films 12A and 12B. The multilayer reflective film 12A in Fig. 2(A) is composed of a periodic laminate structure 121 in which a low refractive index layer consisting of two layers, a first sublayer and a second sublayer, and a high refractive index layer are alternately laminated from the substrate side. On the other hand, the multilayer reflective film 12B in Fig. 2(B) is composed of a periodic laminate structure 121 in which a low refractive index layer consisting of two layers, a first sublayer and a second sublayer, and a high refractive index layer are alternately laminated from the substrate side, and a protective layer 122.

[0021] From a reflective mask blank (EUV mask blank) having an absorber film, a reflective mask (EUV mask) having an absorber pattern (absorber film pattern) formed by patterning an absorber film can be manufactured.

[0022] The substrate preferably has low thermal expansion characteristics for EUV light exposure, and has a thermal expansion coefficient of, for example, ±2×10 -8 / ℃, preferably within ±5×10 -9 / °C. The substrate is preferably one having a sufficiently flat surface, and the surface roughness of the main surface of the substrate is preferably 0.5 nm or less, particularly 0.2 nm or less, in terms of RMS value. Such a surface roughness can be obtained by polishing the substrate. Examples of such materials include titania-doped quartz glass (SiO2-TiO2-based glass). The size of the substrate is preferably such that one main surface of the substrate is 152 mm square and the thickness of the substrate is 6.35 mm. A substrate of this size is a so-called 6025 substrate (one main surface is 6 inches square and 0.25 inches thick).

[0023] In the present invention, at least one of the low refractive index layers constituting the multilayer reflective film, and preferably all of the low refractive index layers, has a two-layer structure consisting of a first sublayer and a second sublayer. The low refractive index layer is made of a material containing molybdenum (Mo).

[0024] The first sublayer is a layer containing molybdenum (Mo) and at least one additive element selected from nitrogen (N), carbon (C), boron (B), silicon (Si) and hydrogen (H). The first sublayer is preferably an amorphous layer. The first sublayer is preferably mainly composed of molybdenum (Mo), and the content of the additive element is preferably 60 atomic % or more, particularly 80 atomic % or more. On the other hand, the amount of the additive element is preferably an amount that makes the first sublayer have an amorphous structure, and the content of the additive element is preferably 1 atomic % or more, particularly 10 atomic % or more, and is preferably 40 atomic % or less, particularly 20 atomic % or less.

[0025] The second sublayer is a layer that contains molybdenum (Mo) and is substantially free of elements other than molybdenum (Mo) (a layer consisting only of molybdenum (Mo) except for unavoidable impurities). The second sublayer is preferably a dense layer having high crystallinity.

[0026] The thickness of the low refractive index layer is preferably 2.1 nm or more, particularly 2.6 nm or more, and 3.5 nm or less, particularly 3 nm or less. Of these, the thickness of the first sublayer is preferably more than 0.3 nm, particularly 0.4 nm or more, and preferably 0.6 nm or less. By making the thickness of the first sublayer 0.6 nm or less, the reflectance of the exposure light (EUV light) can be kept high. In addition, by making the thickness of the first sublayer more than 0.3 nm, particularly 0.4 nm or more, a multilayer reflective film with a sufficiently small background level (BGL) during defect inspection can be obtained.

[0027] In the low refractive index layer, the first sublayer is preferably formed on the substrate side, and the second sublayer is preferably formed on the side away from the substrate. By arranging the first sublayer and the second sublayer in this way, the first sublayer having an amorphous structure can be formed on the high refractive index layer, and after forming the second sublayer, the high refractive index layer can be formed on the dense second sublayer having high crystallinity. In this way, it is possible to reduce the interface roughness between the low refractive index layer and the high refractive index layer caused by the coarsening of crystal grains, the surface roughness of the multilayer reflective film, or both.

[0028] The high refractive index layer is preferably a film containing silicon (Si). The high refractive index layer is preferably mainly composed of silicon (Si), and the content of silicon is preferably 80 atomic % or more, and more preferably 90 atomic % or more. The high refractive index layer is preferably composed of oxygen (O), nitrogen (N), carbon (C), boron (B ) and It may contain at least one additional element selected from the group consisting of arsenic (A) and hydrogen (H), and may be composed of a multilayer structure of a layer containing an additional element and a layer not containing an additional element. The thickness of the high refractive index layer is preferably 3.5 nm or more, particularly 4 nm or more, and is preferably 4.9 nm or less, particularly 4.4 nm or less.

[0029] The thickness of the periodic laminate structure in which low refractive index layers and high refractive index layers are alternately laminated is preferably 200 nm or more, particularly 270 nm or more, and is preferably 400 nm or less, particularly 290 nm or less.

[0030] Methods for forming the periodic laminated structure include a sputtering method in which power is supplied to a target, the atmospheric gas is turned into plasma (ionized) by the supplied power, and sputtering is performed, and an ion beam sputtering method in which an ion beam is irradiated onto the target. Examples of sputtering methods include a DC sputtering method in which a direct current voltage is applied to the target, and an RF sputtering method in which a high frequency voltage is applied to the target. The sputtering method is a film formation method in which a voltage is applied to the target with a sputtering gas introduced into a chamber, the gas is ionized, and the sputtering phenomenon caused by the gas ions is utilized. In particular, the magnetron sputtering method is advantageous in terms of productivity. The power applied to the target may be DC or RF, and DC also includes pulse sputtering in which a negative bias applied to the target is reversed for a short period of time to prevent the target from charging up.

[0031] The periodic laminated structure can be formed, for example, by a sputtering method using a sputtering device capable of mounting multiple targets. Specifically, the target can be appropriately selected from a molybdenum (Mo) target for forming a layer containing molybdenum (Mo), a silicon (Si) target for forming a layer containing silicon (Si), etc., and can be formed using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas as the sputtering gas. In addition, when sputtering is reactive sputtering using a reactive gas, for example, a nitrogen-containing gas such as nitrogen (N2) gas may be used together with a rare gas when forming a film containing nitrogen (N); an oxygen-containing gas such as oxygen (O2) gas may be used together with a rare gas when forming a film containing oxygen (O); a nitrous oxide gas such as nitrous oxide (NO) gas, nitric oxide (NO) gas, and nitrogen dioxide (NO2) gas may be used together with a rare gas when forming a film containing nitrogen (N) and oxygen (O); a carbon oxide gas such as carbon monoxide (CO) gas and carbon dioxide (CO2) gas may be used together with a rare gas when forming a film containing carbon (C) and oxygen (O); a hydrogen-containing gas such as hydrogen (H2) gas may be used together with a rare gas when forming a film containing hydrogen (H); and a hydrocarbon gas such as methane (CH4) gas may be used together with a rare gas when forming a film containing carbon (C) and hydrogen (H). Furthermore, when forming a layer containing boron (B), a molybdenum (Mo) target with boron (B) added (molybdenum boride (MoB) target), a silicon (Si) target with boron (B) added (silicon boride (SiB) target), or the like can be used.

[0032] The protective layer is also called a capping layer, and is provided to protect the periodic laminated structure of the multilayer reflective film when forming a pattern on the absorber film thereon or when correcting the pattern of the absorber film. The material of the protective layer is preferably a material containing ruthenium (Ru). As the material containing ruthenium (Ru), ruthenium (Ru) alone, or a compound in which niobium (Nb) or zirconium (Zr) is added to ruthenium (Ru) is preferably used. The thickness of the protective layer is usually 5 nm or less, and particularly preferably 4 nm or less. The lower limit of the thickness of the protective layer is usually 2 nm or more.

[0033] The protective layer can be formed by a sputtering method such as an ion beam sputtering method or a magnetron sputtering method, as in the case of the periodic laminated structure. The protective layer can be formed by a sputtering method using a sputtering device capable of mounting one or more targets, specifically, a ruthenium (Ru) target, or a ruthenium (Ru) target to which niobium (Nb), zirconium (Zr), or the like is added, and a target of one or more elements selected from niobium (Nb) and zirconium (Zr) as necessary, can be formed by sputtering using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas as a sputtering gas. When the protective layer is formed of a compound containing an element other than a metal, it can be formed by reactive sputtering using a reactive gas such as an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas together with a rare gas as a sputtering gas. The target may also be a compound.

[0034] The reflectance of the multilayer reflective film depends on the composition and layer structure of the multilayer reflective film, but for example, the reflectance at an incident angle of 6° to extreme ultraviolet (EUV) radiation is preferably 65% ​​or more, particularly 66% or more, and even more preferably 67% or more.

[0035] In the present invention, the crystallite size calculated from the diffraction peak of Mo(110) detected by X-ray diffraction of the multilayer reflective film is preferably 2.6 nm or more. In such a multilayer reflective film, the refractive index of the low refractive index layer to the exposure light (EUV light) is low, and the reflectance of the multilayer reflective film is higher.

[0036] Furthermore, in the present invention, when the size of one main surface of a substrate is 152 mm square and 6.35 mm thick, within a central 142 mm square of one main surface, it is preferable that the change (ΔTIR) in flatness (TIR: Total Indicator Reading) before and after forming a multilayer reflective film, specifically, before and after forming a periodic stacking structure portion, or before and after forming both the periodic stacking structure portion and the protective layer, is 0.7 μm or less in absolute value.

[0037] The absorber film is formed on top of the multilayer reflective film and absorbs the EUV light, which is the exposure light, to reduce the reflectance of the exposure light. In a reflective mask, a transfer pattern is formed due to the difference in reflectance between the area where the absorber film is formed and the area where the absorber film is not formed.

[0038] The material of the absorber film is not limited as long as it absorbs EUV light and can be patterned. Examples of the material of the absorber film include materials containing tantalum (Ta) or chromium (Cr). In addition, materials containing Ta or Cr may contain oxygen (O), nitrogen (N), carbon (C), boron (B), etc. Examples of materials containing Ta include Ta alone and tantalum compounds such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB, and TaCONB. Examples of materials containing Cr include Cr alone and chromium compounds such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB, and CrCONB.

[0039] The absorber film can be formed by sputtering, and magnetron sputtering is preferable. Specifically, it can be formed by sputtering using a metal target such as a chromium (Cr) target or a tantalum (Ta) target, or a metal compound target such as a chromium compound target or a tantalum compound target (a target containing a metal such as Cr or Ta and oxygen (O), nitrogen (N), carbon (C), boron (B), or the like) as a sputtering gas, using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas, or by reactive sputtering using a rare gas and a reactive gas such as an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas. The thickness of the absorber film is not particularly limited, but is usually about 60 to 80 nm.

[0040] The reflective mask blank may further have a hard mask film on the absorber film, which functions as an etching mask when the absorber film is dry etched. On the other main surface (back surface) opposite to the one main surface of the substrate, a conductive film may be provided, preferably in contact with the other main surface, for electrostatically chucking the reflective mask to an exposure device.

[0041] A hard mask film (an etching mask film for the absorber film) having etching characteristics different from those of the absorber film may be provided on the side of the absorber film that is away from the substrate, preferably in contact with the absorber film. This hard mask film functions as an etching mask when the absorber film is dry etched. After the absorber pattern is formed, the hard mask film may be left as a part of the absorber film as a reflectance reduction layer for reducing the reflectance at the wavelength of light used in an inspection such as a pattern inspection, or may be removed so as not to remain on the reflective mask. Materials for the hard mask film include materials containing chromium (Cr). A hard mask film formed of a material containing Cr is particularly suitable when the absorber film is formed of a material containing Ta and not containing Cr. When a layer (reflectance reduction layer) that mainly serves the function of reducing the reflectance at the wavelength of light used in an inspection such as a pattern inspection is formed on the absorber film, the hard mask film can be formed on the reflectance reduction layer of the absorber film. The hard mask film can be formed by, for example, a magnetron sputtering method. The thickness of the hard mask film is not particularly limited, but is usually about 5 to 20 nm.

[0042] The conductive film preferably has a sheet resistance of 100Ω / □ or less, and there is no particular restriction on the material. Examples of the material of the conductive film include materials containing tantalum (Ta) or chromium (Cr). Furthermore, materials containing Ta or Cr may contain oxygen (O), nitrogen (N), carbon (C), boron (B), and the like. Examples of materials containing Ta include Ta alone and tantalum compounds such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB, and TaCONB. Examples of materials containing Cr include Cr alone and chromium compounds such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB, and CrCONB.

[0043] The thickness of the conductive film is not particularly limited as long as it functions as an electrostatic chuck, but is usually about 20 to 300 nm. The thickness of the conductive film is preferably formed so that the film stress is balanced with the multilayer reflective film and the absorber pattern after the conductive film is formed as a reflective mask, that is, after the absorber pattern is formed. The conductive film may be formed before the multilayer reflective film is formed, or after all the films on the multilayer reflective film side of the substrate are formed. Also, after forming a part of the film on the multilayer reflective film side of the substrate, the conductive film may be formed, and then the remaining film on the multilayer reflective film side of the substrate may be formed. The conductive film may be formed, for example, by magnetron sputtering.

[0044] Furthermore, the reflective mask blank may have a resist film formed on the side farthest from the substrate. The resist film is preferably an electron beam (EB) resist. EXAMPLES

[0045] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0046] [Examples 1 to 3] A reflective multilayer film was formed on a 152mm square, 6.35mm thick low thermal expansion glass substrate (SiO2-TiO2 glass substrate) by DC pulse magnetron sputtering using a molybdenum (Mo) target and a silicon (Si) target, with both targets facing the main surface of the substrate and rotating the substrate. Each target was attached to a sputtering device that can be fitted with two targets and can discharge the targets one by one or both at the same time, and the substrate was then placed.

[0047] First, while argon (Ar) gas (flow rate: 12 SCCM) was flowed into the chamber, power was applied to the silicon (Si) target to form a 4.2 nm thick silicon (Si) layer as a high refractive index layer, and then the application of power to the silicon target was stopped.

[0048] Next, while argon gas (flow rate: 14 SCCM) and nitrogen (N2) gas (flow rate: 15 SCCM) were both flowing into the chamber, power was applied to the molybdenum target to form a molybdenum nitride layer (MoN layer) as the first sublayer of the low refractive index layer, and the application of power to the molybdenum target was stopped. The molybdenum nitride layer was formed under conditions that allowed the molybdenum nitride to have an amorphous structure. The thickness of the first sublayer was 0.4 nm in Example 1, 0.5 nm in Example 2, and 0.6 nm in Example 3.

[0049] Next, while argon gas (flow rate: 15 SCCM) was flowing into the chamber, power was applied to the molybdenum target to form a layer of molybdenum alone (Mo layer) as the second sublayer of the low refractive index layer, and the application of power to the molybdenum target was stopped. The thickness of the second sublayer was adjusted so that the entire low refractive index layer, which is the combination of the first sublayer and the second sublayer, was 2.8 nm.

[0050] The operation of forming these low refractive index layers and high refractive index layers constitutes one cycle, and this was repeated 40 times to form the low refractive index layer for the 40th cycle, after which a 4.2 nm thick silicon (Si) layer was formed on the top layer by the above method to form the periodic laminated structure of the multilayer reflective film. The thickness of each layer can be controlled by the magnitude of the power applied to the target, the length of time that power is applied to the target, or both, and the formed thickness can be confirmed by a transmission electron microscope image using cross-sectional energy dispersive X-ray spectroscopy (TEM-EDX), etc.

[0051] Next, a ruthenium (Ru) target was used on the periodic laminated structure, and the target was placed facing the main surface of the substrate. While the substrate was being rotated, a protective layer was formed on the periodic laminated structure by DC pulse magnetron sputtering. First, after the periodic laminated structure was formed, the substrate on which the periodic laminated structure was formed was placed, without being taken out into the atmosphere, from the sputtering device in which the periodic laminated structure was formed, via a transport path that maintained a vacuum state. teeth , Ruthenium (Ru) Attach the target, Periodic laminated structure A substrate on which the above-mentioned was formed was placed.

[0052] Next, while flowing argon gas (flow rate: 10 SCCM) into the chamber, power was applied to the ruthenium target to form a layer of simple ruthenium (Ru layer) with a thickness of 2.5 nm, and then the application of power to the ruthenium target was stopped to obtain a multilayer reflective film consisting of a periodic stacked structure and a protective layer.

[0053] The reflectance spectrum of the obtained multilayer reflective film with respect to EUV light (wavelength 13 to 14 nm) at an incident angle of 6° was measured using an EUV mask automatic reflectometer (euv tech., LPR-1016). The background level (BGL) during inspection was measured using an EUV mask blanks defect inspection / review device (Lasertec Corporation, ABICS E120) using EUV light as inspection light. As a result, the central wavelength (wavelength at the midpoint of the half-width of the main maximum) of the EUV reflection spectrum was 13.53±0.04 nm, and the maximum reflectance was 67.11% in Example 1, 66.74% in Example 2, and 66.29% in Example 3. The background level (BGL) was 374 in Example 1, 371 in Example 2, and 374 in Example 3.

[0054] In addition, the obtained multilayer reflective film was subjected to out-of-plane measurement using an X-ray diffractometer (Rigaku Corporation, SmartLab) equipped with a Cu target cathode to obtain an X-ray diffraction profile of the multilayer reflective film. From the observed Mo(110) diffraction peak, the following Scherrer equation was used: Crystallite size (nm) = Kλ / βcosθ (In the formula, K is the Scherrer constant (0.9), λ is the measured X-ray wavelength (0.15418 nm), β is the half-width in radians of the diffraction peak, and θ is the Bragg angle of the diffraction peak.) The Mo crystallite size was calculated using the formula: The calculated Mo crystallite size was 2.8 nm for Example 1, 2.7 nm for Example 2, and 2.6 nm for Example 3, which showed that Mo had high crystallinity.

[0055] Furthermore, for the substrate (reflective mask blank) on which the obtained multilayer reflective film was formed, the flatness (TIR) ​​was measured within a 142 mm square area in the center of the main surface using a mask flatness measuring device (UltraFlat200, manufactured by Tropel) before and after the formation of the multilayer reflective film, and the change (ΔTIR) in flatness (TIR) ​​before and after the formation of the multilayer reflective film was calculated. The absolute value of ΔTIR was 0.60 μm for Example 1, 0.57 μm for Example 2, and 0.56 μm for Example 3.

[0056] [Comparative Example 1] A multilayer reflective film was formed in the same manner as in Example 1, except that the thickness of the molybdenum nitride layer was 0.3 nm. The obtained multilayer reflective film was evaluated for the central wavelength of the EUV reflection spectrum, the maximum reflectance, the BGL, and the crystallite size of Mo in the same manner as in Example 1. In addition, the substrate (reflective mask blank) on which the obtained multilayer reflective film was formed was evaluated for ΔTIR in the same manner as in Example 1. As a result, the central wavelength of the EUV reflection spectrum was 13.53±0.04 nm, the maximum reflectance was a high value of 67.64%, and the BGL was high at 437. In addition, the crystallite size of Mo was 2.9 nm, and the absolute value of ΔTIR was 0.70 μm.

[0057] [Comparative Example 2] A multilayer reflective film was formed in the same manner as in Example 1, except that the thickness of the molybdenum nitride layer was 0.7 nm. The obtained multilayer reflective film was evaluated for the central wavelength of the EUV reflection spectrum, the maximum reflectance, the BGL, and the crystallite size of Mo in the same manner as in Example 1. In addition, the substrate (reflective mask blank) on which the obtained multilayer reflective film was formed was evaluated for ΔTIR in the same manner as in Example 1. As a result, the central wavelength of the EUV reflection spectrum was 13.53±0.04 nm, the maximum reflectance was low at 64.25%, and the BGL was high at 490. In addition, the crystallite size of Mo was 2.5 nm, and the absolute value of ΔTIR was 0.73 μm.

[0058] [Comparative Example 3] A multilayer reflective film was formed in the same manner as in Example 1, except that a molybdenum nitride layer was not formed, and only a layer of molybdenum alone was used as a low refractive index layer having a thickness of 2.8 nm. The obtained multilayer reflective film was evaluated for the central wavelength of the EUV reflection spectrum, the maximum reflectance, the BGL, and the crystallite size of Mo in the same manner as in Example 1. In addition, the substrate (reflective mask blank) on which the obtained multilayer reflective film was formed was evaluated for ΔTIR in the same manner as in Example 1. As a result, the central wavelength of the EUV reflection spectrum was 13.53±0.04 nm, the maximum reflectance was a high value of 67.50%, and the BGL was high at 488. In addition, the crystallite size of Mo was 3.1 nm, and the absolute value of ΔTIR was 1.10 μm. [Explanation of symbols]

[0059] 100A, 100B, 101A, 101B Reflective mask blanks 11 Substrate 12A, 12B Multilayer reflective coating 121 Periodic layered structure 122 Protective layer 13 Absorber membrane

Claims

1. A reflective mask blank having a substrate and a multilayer reflective film formed on one main surface of the substrate and reflecting exposure light, the multilayer reflective film has a periodic laminate structure in which low refractive index layers and high refractive index layers are alternately laminated, At least one of the low refractive index layers constituting the multilayer reflective film has a two-layer structure consisting of a first sublayer and a second sublayer, The first sublayer comprises molybdenum (Mo) and at least one additional element selected from nitrogen (N), carbon (C), boron (B), silicon (Si) and hydrogen (H), and has a thickness of more than 0.3 nm and less than or equal to 0.6 nm; the second sublayer comprises molybdenum (Mo) and is substantially free of elements other than molybdenum (Mo); A reflective mask blank, characterized in that the multilayer reflective film has a crystallite diameter of 2.6 nm or more calculated from a diffraction peak of Mo (110) detected by X-ray diffraction.

2. 2. The reflective mask blank according to claim 1, wherein in the low refractive index layer, the first sublayer is formed on the substrate side, and the second sublayer is formed on a side away from the substrate.

3. 3. The reflective mask blank according to claim 1, wherein the high refractive index layer contains silicon (Si).

4. The reflective mask blank according to any one of claims 1 to 3, characterized in that the size of the one main surface of the substrate is 152 mm square, the thickness of the substrate is 6.35 mm, and within a central 142 mm square portion of the one main surface, the change in flatness (TIR) ​​(ΔTIR) before and after forming the multilayer reflective film is 0.7 μm or less in absolute value.

5. 5. The reflective mask blank according to claim 1, wherein the multilayer reflective film has a protective layer formed in contact with the side of the periodic stacked structure away from the substrate.

6. 6. The reflective mask blank according to claim 1, further comprising an absorber film on the multilayer reflective film for absorbing exposure light.

7. A reflective mask obtained by patterning the absorber film of the reflective mask blank according to claim 6.

Citation Information

Patent Citations

  • Reflecting type exposure mask, its manufacturing method and semiconductor element

    JP2002246299A

  • Method and device for inspecting multilayered mask for defect

    JP2003114200A

  • Reflective mask blank, reflective mask and multilayered film reflection mirror

    JP2006093454A

  • Reflective mask blank for EUV lithography or substrate with reflective layer for EUV lithography, and manufacturing method therefor

    JP2015109366A

  • Substrate with multilayer reflective film, reflective mask blank and reflective mask, and method for manufacturing semiconductor device

    JP2020166249A