Block copolymer, resin composition, and method for producing block copolymer
A block copolymer with a specific sulfur concentration and molecular weight ratio, used in a resin composition with a polyoxyalkylene polymer, addresses odor issues at high temperatures and enhances toughness and weather resistance, suitable for applications like sealants and elastomers.
Patent Information
- Application Number
- JP2021526958
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-03
- Filing Date
- 2020-06-22
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-06-22
AI Technical Summary
Block copolymers described in existing literature suffer from severe odor when exposed to high temperatures, limiting their use in applications requiring heat resistance, and there is a need for resin compositions that can produce molded articles with high toughness and weather resistance.
A block copolymer with a specific terminal structure containing a sulfur atom, where the product of sulfur concentration and number average molecular weight is set to 60 or less, is used in a resin composition that includes a polyoxyalkylene polymer with crosslinkable functional groups, reducing odor and enhancing toughness and weather resistance.
The block copolymer significantly reduces odor at high temperatures and improves the toughness and weather resistance of molded products, making it suitable for applications such as sealants, adhesives, and elastomers.
Smart Images

Figure 0007578105000001 
Figure 0007578105000002 
Figure 0007578105000003
Abstract
Description
[Technical field]
[0001] The present specification relates to a block copolymer, a resin composition, and a method for producing the block copolymer. [Background technology]
[0002] Known living radical polymerization methods include reversible addition-fragmentation chain transfer polymerization (RAFT), nitroxy radical (NMP), atom transfer radical polymerization (ATRP), polymerization using organotellurium compounds (TERP), polymerization using organoantimony compounds (SBRP), polymerization using organobismuth compounds (BIRP), and iodine transfer polymerization. Among these, the RAFT method, the NMP method, and the ATRP method are industrially used from the viewpoints of polymerization controllability and ease of implementation, and the RAFT method has attracted particular attention because it can be applied to the widest range of vinyl monomers and is metal-free.
[0003] In the field of industrial applications such as paints, adhesives, sealing materials, elastomers, etc., resin compositions containing vinyl block copolymers obtained by living radical polymerization using the RAFT method have also been developed.
[0004] As a vinyl block copolymer obtained by the RAFT method and used in such a resin composition, Patent Document 1 discloses a block copolymer having a polymer block (A) which is a polymer having a glass transition temperature (Tg) of 150° C. or higher and contains structural units derived from styrenes and a maleimide compound, and an acrylic polymer block (B) which is a polymer having a solubility parameter of 9.9 or higher and a Tg of 20° C. or higher.
[0005] Patent Document 2 discloses, as a vinyl block copolymer obtained by the RAFT method, a block copolymer having an acrylic polymer block (A) containing a specific structural unit, which is a polymer having a Tg of 0° C. or less and containing an average of 1.0 or more crosslinkable functional groups per block, and an acrylic polymer block (B) containing a specific structural unit, which is a polymer having a Tg of 20° C. or less. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2017 / 073287 [Patent Document 2] International Publication No. 2018 / 181251 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the block copolymers described in Patent Documents 1 and 2 each have a problem in that they give off a strong odor when exposed to high temperatures, and therefore are limited in their use in applications requiring heat resistance, etc. The patent documents do not suggest or disclose anything about the odor that occurs when the block copolymer obtained by the RAFT method is exposed to high temperatures, and no means for solving the odor problem have been shown yet. Furthermore, in applications such as sealants, elastomers, and adhesives for exterior tiles, resin compositions that produce molded products with high toughness are required, and particularly in applications such as sealants and adhesives for exterior tiles, weather resistance is also required.
[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a block copolymer which has a significantly reduced odor when exposed to high temperatures, and a resin composition which can give molded articles having high toughness, and which also gives molded articles having excellent weather resistance. [Means for solving the problem]
[0009] As a result of intensive research to solve the above problems, the present inventors have found that, when a block copolymer has a specific terminal structure having a sulfur atom and the product of the sulfur concentration and the number average molecular weight in the block copolymer is set to a specific value or less, odor is significantly reduced and furthermore, the toughness of a molded article of a resin composition containing the block copolymer is high, and have completed the present invention. In particular, they have found that a molded article of a resin composition containing the block copolymer and a polyoxyalkylene polymer having a crosslinkable functional group has excellent weather resistance.
[0010] The present invention is as follows. [1] A block copolymer comprising at least two polymer blocks, at least one terminal structure of the block copolymer is a structure represented by the following general formula (1) or a thiol group, and the product of (x / 100) and y, where x is a sulfur concentration (mass%) in the block copolymer and y is a number average molecular weight of the block copolymer, is 60 or less. [ka] (R represents an alkyl group having 1 to 30 carbon atoms, an aryl group, or an aralkyl group.) [2] The block copolymer according to [1], wherein the block copolymer has a structural unit consisting of polymer block (A) / polymer block (B) / polymer block (A). [3] The block copolymer according to [1], wherein the block copolymer has a structural unit consisting of polymer block (A) / polymer block (B) / polymer block (C). [4] The block copolymer according to any one of [1] to [3], wherein at least one polymer block of the block copolymer contains a (meth)acrylic acid ester compound as a main constituent monomer. [5] The block copolymer according to any one of [2] to [4], wherein the polymer block (A) has a crosslinkable functional group. [6] The block copolymer according to [5], wherein the polymer block (A) contains an average of 0.7 or more crosslinkable functional groups per molecule. [7] A resin composition comprising the block copolymer according to any one of [1] to [6]. [8] The resin composition according to [7], further comprising a polyoxyalkylene polymer having a crosslinkable functional group. [9] The resin composition according to [7] or [8], which is used for any one of a sealing material, an adhesive, a pressure-sensitive adhesive, a coating material, and an elastomer.
[10] A method for producing a block copolymer consisting of at least two polymer blocks, comprising the steps of: producing a block copolymer (P1) consisting of at least three polymer blocks, the block copolymer having a trithiocarbonate group represented by the following general formula (2) in a central polymer block of the block copolymer, by a reversible addition-fragmentation chain transfer living radical polymerization method; and producing a block copolymer (P2) consisting of at least two polymer blocks by reacting the trithiocarbonate group of the block copolymer (P1) with a nucleophile. [ka]
[11] At least one polymer block of the block copolymer (P2) contains a (meth)acrylic acid ester compound as a main constituent monomer, At least one terminal structure of the block copolymer (P2) is a structure represented by the following general formula (1) or a thiol group, The method for producing a block copolymer according to
[10] , wherein the product of (x / 100) and y is 60 or less, where x is a sulfur concentration (mass%) in the block copolymer (P2) and y is a number average molecular weight of the block copolymer (P2). [ka] (R represents an alkyl group, an aryl group, or an aralkyl group having 1 to 30 carbon atoms.) Effect of the Invention
[0011] According to the block copolymer of the present invention, odor when exposed to high temperatures is significantly reduced, and the toughness of a molded article of a resin composition containing the block copolymer can be increased. Furthermore, the weather resistance of the molded article can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention relates to a block copolymer comprising at least two polymer blocks and having a specific terminal structure.
[0013] According to the block copolymer of the present invention, the odor generated when exposed to high temperatures is significantly reduced, and a resin composition containing the block copolymer and capable of producing a molded product having high toughness can be provided.
[0014] Various embodiments of the technology disclosed in this specification will be described in detail below. In this specification, "(meth)acrylic" means acrylic and methacrylic, "(meth)acrylate" means acrylate and methacrylate, and "(meth)acryloyl group" means acryloyl group and methacryloyl group. The block copolymer, the resin composition containing the block copolymer, and the method for producing the block copolymer will be described below.
[0015] 1. Block copolymers The block copolymer of the present invention (hereinafter referred to as "the present block copolymer") is a block copolymer consisting of at least two polymer blocks, at least one terminal structure of the present block copolymer is a structure represented by the above general formula (1) or a thiol group, and when the sulfur concentration (mass%) in the present block copolymer is x and the number average molecular weight of the block copolymer is y, the product of (x / 100) and y is 60 or less, thereby achieving the effect of significantly reducing odor when exposed to high temperatures. The product of (x / 100) and y is preferably 57.5 or less, more preferably 55.0 or less, even more preferably 52.5 or less, and even more preferably 50.0 or less. Incidentally, x and y can be measured by the method described in the Examples.
[0016] The polymer block includes the following polymer block (A) and polymer block (B).
[0017] 1-1. Polymer block (A) Examples of monomers constituting the polymer block (A) include (meth)acrylic acid alkyl ester compounds, compounds represented by the following general formula (3), styrenes, maleimide compounds, and amide group-containing vinyl compounds, and one or more of these can be used. CH2=CR 1 -C(=O)O(R 2 O) n -R 3 (3) (In the formula, R 1 represents hydrogen or a methyl group, R 2 represents a linear or branched alkylene group having 2 to 6 carbon atoms; R 3 represents hydrogen, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms. n represents an integer of 1 to 100.
[0018] Among the above monomers, (meth)acrylic acid alkyl ester compounds and compounds represented by the above general formula (3) are preferred in that they are capable of producing block copolymers having a low Tg and excellent fluidity. <(Meth)acrylic acid alkyl ester compound> Specific examples of the (meth)acrylic acid alkyl ester compound include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, and linear or branched (meth)acrylic acid alkyl ester compounds, such as (meth)acrylic acid, such as decyl (meth)acrylate and dodecyl (meth)acrylate; and aliphatic cyclic ester compounds of acrylic acid, such as cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate.
[0019] Among these, (meth)acrylic acid alkyl ester compounds having an alkyl group with 1 to 20 carbon atoms are preferred, (meth)acrylic acid alkyl ester compounds having an alkyl group with 2 to 12 carbon atoms are more preferred, and (meth)acrylic acid alkyl ester compounds having an alkyl group with 4 to 8 carbon atoms are even more preferred, since it is particularly easy to obtain a block copolymer having a low Tg and excellent fluidity.
[0020] The proportion of the structural units derived from the (meth)acrylic acid alkyl ester compound in the total structural units of the polymer block (A) can be 50% by mass or more and 100% by mass or less. If it is 50% by mass or more, it is advantageous in terms of weather resistance. Such structural units are, for example, 60% by mass or more, for example, 70% by mass or more, or for example, 80% by mass or more. Also, for example, 98% by mass or less, for example, 95% by mass or less, for example, 90% by mass or less, or for example, 85% by mass or less.
[0021] <Compound represented by general formula (3)> The compound represented by the above general formula (3) has an oxyalkylene structure such as an oxyethylene chain, an oxypropylene chain, or an oxybutylene chain when n is 1. Specific examples include methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, n-propoxyethyl (meth)acrylate, n-butoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, ethoxypropyl (meth)acrylate, n-propoxypropyl (meth)acrylate, n-butoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxybutyl (meth)acrylate, n-propoxybutyl (meth)acrylate, and n-butoxybutyl (meth)acrylate. As the (meth)acrylic acid alkoxyalkyl ester compound, since it is easy to obtain a block copolymer having a low Tg and excellent fluidity, a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group having 2 to 8 carbon atoms is preferred, and a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group having 2 to 6 carbon atoms is more preferred.
[0022] When n in the formula is 2 or more, it has a polyoxyalkylene structure such as a polyoxyethylene chain, a polyoxypropylene chain, or a polyoxybutylene chain. When n is 2 or more, R 2may be the same or different. Therefore, different types of polyoxyalkylene structures may be present in one molecule, such as a polyoxyethylene / polyoxypropylene block structure. Specific examples of the compound include polyoxyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, polyoxybutylene (meth)acrylate, and polyoxyethylene-polyoxypropylene (meth)acrylate. Examples of the compound having an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms at the terminal include methoxypolyethylene glycol (meth)acrylate, lauroxypolyethylene glycol (meth)acrylate, stearoxypolyethylene glycol (meth)acrylate, octoxypolyethylene glycol polypropylene glycol (meth)acrylate, nonylphenoxypolypropylene glycol (meth)acrylate, and phenoxypolyethylene glycol polypropylene glycol (meth)acrylate.
[0023] On the other hand, among the above-mentioned monomers, styrenes are preferred in that they can easily give block copolymers having a high Tg and excellent heat resistance, and maleimide compounds and amide group-containing vinyl compounds are preferred in that they can easily give block copolymers having a high Tg and excellent oil resistance. <Styrene> The styrenes include styrene and its derivatives. Specific examples of the compounds include styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, vinylxylene, vinylnaphthalene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, pn-butylstyrene, p-isobutylstyrene, pt-butylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-chloromethylstyrene, p-chloromethylstyrene, o-chlorostyrene, p-chlorostyrene, o-hydroxystyrene, m-hydroxystyrene, p-hydroxystyrene, and divinylbenzene, and one or more of these can be used. By polymerizing a monomer containing a styrene, a structural unit derived from a styrene can be introduced into the polymer block (A). Among these, from the viewpoint of polymerizability, styrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-hydroxystyrene, m-hydroxystyrene, and p-hydroxystyrene are preferred. In addition, α-methylstyrene, β-methylstyrene and vinylnaphthalene are preferred in that they can increase the Tg of the polymer block (A) and give block polymers having excellent heat resistance.
[0024] In the polymer block (A), the proportion of the structural units derived from the styrenes is preferably 1% by mass or more and 70% by mass or less based on the total structural units of the polymer (P1). More preferably, it is 5% by mass or more and 70% by mass or less, even more preferably, it is 10% by mass or more and 70% by mass or less, and even more preferably, it is 20% by mass or more and 60% by mass or less. Alternatively, it may be, for example, 20% by mass or more and 40% by mass or less. If the structural unit derived from a styrene compound is 1% by mass or more, a block copolymer having excellent moldability can be obtained. On the other hand, if the structural unit derived from a styrene compound is 70% by mass or less, a necessary amount of the structural unit derived from a maleimide compound described later can be secured, so that a block copolymer having excellent heat resistance and oil resistance can be obtained.
[0025] <Maleimide compounds> The maleimide compounds include maleimide and N-substituted maleimide compounds. Examples of the N-substituted maleimide compounds include N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-ethylmaleimide, Nn-propylmaleimide, N-isopropylmaleimide, Nn-butylmaleimide, N-isobutylmaleimide, N-tert-butylmaleimide, N-pentylmaleimide, N-hexylmaleimide, N-heptylmaleimide, N-octylmaleimide, N-laurylmaleimide, and N-stearylmaleimide; N-cyclopentylmaleimide, N-cyclohexylmaleimide, and the like; N-cycloalkyl-substituted maleimide compounds such as xylmaleimide; N-phenylmaleimide, N-(4-hydroxyphenyl)maleimide, N-(4-acetylphenyl)maleimide, N-(4-methoxyphenyl)maleimide, N-(4-ethoxyphenyl)maleimide, N-(4-chlorophenyl)maleimide, N-(4-bromophenyl)maleimide, N-benzylmaleimide, and other N-aryl-substituted maleimide compounds, among which one or more can be used. By polymerizing a monomer containing a maleimide compound, a structural unit derived from the maleimide compound can be introduced into the polymer (P1). Among the above, the compound represented by the following general formula (4) is preferred in that the oil resistance of the resulting block copolymer is more excellent. [ka] [In the formula, R 1 is hydrogen, an alkyl group having 1 to 3 carbon atoms, or PhR 2 where Ph represents a phenyl group, and R 2 represents hydrogen, a hydroxyl group, an alkoxy group having 1 to 2 carbon atoms, an acetyl group, or a halogen.
[0026] In the polymer block (A), the proportion of the structural units derived from the maleimide compound is 30% by mass or more and 99% by mass or less with respect to the total structural units of the polymer block (A). It is preferably 30% by mass or more and 95% by mass or less, more preferably 30% by mass or more and 90% by mass or less, and even more preferably 40% by mass or more and 80% by mass or less. It may be, for example, 50% by mass or more, or further, for example, 60% by mass or more. It may be, for example, 75% by mass or less, or further, for example, 70% by mass or less. It may be, for example, 50% by mass or more and 75% by mass or less, or further, for example, 60% by mass or more and 70% by mass or less. When the structural unit derived from the maleimide compound is 30% by mass or more, the resulting block copolymer has excellent heat resistance and oil resistance, whereas when it is 99% by mass or less, the block copolymer has structural units other than the structural units derived from the maleimide compound, resulting in excellent fluidity and moldability.
[0027] In order to provide better oil resistance, the present block copolymer may further contain a structural unit derived from an amide group-containing vinyl compound.
[0028] <Amido group-containing vinyl compound> Specific examples of the amide group-containing vinyl compound include (meth)acrylamide, (meth)acrylamide derivatives such as tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and (meth)acryloylmorpholine; and N-vinyl amide monomers such as N-vinyl acetamide, N-vinyl formamide, and N-vinyl isobutylamide. These compounds may be used alone or in combination of two or more.
[0029] By polymerizing a monomer containing an amide group-containing vinyl compound, a structural unit derived from the amide group-containing vinyl compound can be introduced into the polymer block (A).
[0030] Examples of other monomers besides the above include amino group-containing monomers such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate; Aliphatic cyclic ester compounds of (meth)acrylic acid, such as isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; Aromatic vinyl compounds of (meth)acrylic acid such as styrene, α-methylstyrene, benzyl (meth)acrylate, phenyl (meth)acrylate, and naphthyl (meth)acrylate; Examples of the vinyl acetate include vinyl acetate, (meth)acrylonitrile, and maleic acid monoester compounds.
[0031] <Crosslinkable functional group> The polymer block (A) preferably contains an average of 0.7 or more crosslinkable functional groups in each block, more preferably 1.0 or more, even more preferably 1.5 or more, and even more preferably 2.0 or more, from the viewpoint of improving the breaking strength of the molded product, and preferably contains 10 or less, more preferably 7 or less, and even more preferably 5 or less, from the viewpoint of excellent breaking elongation.
[0032] There is no particular limitation on the method of introducing the crosslinkable functional group, but for example, the crosslinkable functional group can be introduced by copolymerizing a vinyl monomer having a crosslinkable functional group. In this case, the polymer block (A) has a structural unit derived from a vinyl monomer having a crosslinkable functional group (hereinafter, simply referred to as a "crosslinkable structural unit"). Examples of the crosslinkable functional group include a hydrolyzable silyl group, a carboxyl group, a hydroxyl group, an epoxy group, a primary or secondary amino group, and the like, and examples of the vinyl monomer having the crosslinkable functional group include a hydrolyzable silyl group-containing vinyl compound, an unsaturated carboxylic acid, an unsaturated acid anhydride, a hydroxyl group-containing vinyl compound, an epoxy group-containing vinyl compound, a primary or secondary amino group-containing vinyl compound, an oxazoline group-containing vinyl compound, and an isocyanate group-containing vinyl compound. The above-mentioned vinyl monomer having a crosslinkable functional group can be used alone or in combination of two or more kinds.
[0033] Examples of the vinyl compound containing a hydrolyzable silyl group include vinyl silanes such as vinyl trimethoxysilane, vinyl triethoxysilane, vinyl methyl dimethoxysilane, and vinyl dimethyl methoxysilane; alkoxysilyl group-containing (meth)acrylic acid esters such as trimethoxysilylpropyl (meth)acrylate, triethoxysilylpropyl (meth)acrylate, methyl dimethoxysilylpropyl (meth)acrylate, and dimethyl methoxysilylpropyl (meth)acrylate; alkoxysilyl group-containing vinyl ethers such as trimethoxysilylpropyl vinyl ether; and alkoxysilyl group-containing vinyl esters such as vinyl trimethoxysilyl undecanoate. These compounds may be used alone or in combination of two or more. Such vinyl compounds can undergo dehydration condensation between hydrolyzable silyl groups. For this reason, they are suitable in that they can efficiently carry out the polymerization reaction for producing a block copolymer and the subsequent crosslinking reaction. In addition, since the hydrolyzable silyl group as a whole is regarded as one reaction point, in the present invention, the entire hydrolyzable silyl group is regarded as one crosslinkable functional group. In other words, one crosslinkable functional group is introduced by copolymerization of both vinyltrimethoxysilane, which has three methoxysilyl groups in the molecule, and vinylmethyldimethoxysilane, which has two methoxysilyl groups.
[0034] Examples of unsaturated carboxylic acids include (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, citraconic acid, cinnamic acid, and monoalkyl esters of unsaturated dicarboxylic acids (monoalkyl esters of maleic acid, fumaric acid, itaconic acid, citraconic acid, maleic anhydride, itaconic anhydride, citraconic anhydride, etc.), etc. These compounds may be used alone or in combination of two or more.
[0035] Examples of the unsaturated acid anhydride include maleic anhydride, itaconic anhydride, citraconic anhydride, etc. These compounds may be used alone or in combination of two or more kinds.
[0036] Examples of the hydroxy group-containing vinyl compound include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and mono(meth)acrylic acid esters of polyalkylene glycols such as polyethylene glycol and polypropylene glycol. These compounds may be used alone or in combination of two or more.
[0037] Examples of the epoxy group-containing vinyl compound include glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, etc. These compounds may be used alone or in combination of two or more.
[0038] Examples of the primary or secondary amino group-containing vinyl compound include amino group-containing (meth)acrylic acid esters such as aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, N-methylaminoethyl (meth)acrylate, and N-ethylaminoethyl (meth)acrylate; and amino group-containing (meth)acrylamides such as aminoethyl (meth)acrylamide, aminopropyl (meth)acrylamide, N-methylaminoethyl (meth)acrylamide, and N-ethylaminoethyl (meth)acrylamide.
[0039] Among the above-mentioned vinyl monomers having a crosslinkable functional group, the hydrolyzable silyl group-containing compound is preferred in that it provides molded products with excellent breaking elongation and breaking strength.
[0040] Another method for introducing a hydrolyzable silyl group as a crosslinkable functional group is as follows: 1) An addition reaction between a carboxyl group of an unsaturated carboxylic acid, which is a constituent monomer of the polymer block (A), and a hydrolyzable silyl group-containing epoxy compound. The unsaturated carboxylic acid is preferably at least one selected from the group consisting of (meth)acrylic acid, maleic anhydride, and itaconic acid. Also included is 2) an addition reaction between an epoxy group of an epoxy group-containing vinyl compound, which is a constituent monomer of the polymer block (A), and a hydrolyzable silyl group-containing amine compound. The epoxy group-containing monomer preferably contains a glycidyl group-containing (meth)acrylic acid ester.
[0041] Furthermore, by copolymerizing a polyfunctional polymerizable monomer having two or more polymerizable unsaturated groups in the molecule, a polymerizable unsaturated group can be introduced as a crosslinkable functional group into the polymer block (A). The polyfunctional polymerizable monomer is a compound having two or more polymerizable functional groups such as (meth)acryloyl groups and alkenyl groups in the molecule, and examples of the polyfunctional polymerizable monomer include polyfunctional (meth)acrylate compounds, polyfunctional alkenyl compounds, and compounds having both (meth)acryloyl groups and alkenyl groups. For example, in addition to alkylene diol diacrylate such as hexanediol diacrylate, compounds having both (meth)acryloyl groups and alkenyl groups in the molecule such as allyl (meth)acrylate, isopropenyl (meth)acrylate, butenyl (meth)acrylate, pentenyl (meth)acrylate, and 2-(2-vinyloxyethoxy)ethyl (meth)acrylate can be mentioned. These compounds may be used alone or in combination of two or more.
[0042] The polymerizable unsaturated group can also be introduced by producing a polymer having a functional group in the molecule, and then reacting it with a compound having a functional group and a polymerizable unsaturated group that can react with the functional group. For example, a polymer having a hydroxyl group can be produced, and then reacted with a compound having both an isocyanate group and a polymerizable unsaturated group to introduce a polymerizable unsaturated group into the polymer. Also, for example, a polymer having a carboxyl group can be reacted with a compound having both an epoxy group and a polymerizable unsaturated group.
[0043] In addition to the above, the crosslinkable functional group can also be introduced by producing the polymer block (A) in the presence of a polymerization inhibitor such as a RAFT agent having a crosslinkable functional group.
[0044] The crosslinkable constituent unit in the polymer block (A) is not particularly limited, but may be, for example, 0.01 mol% or more, for example, 0.1 mol% or more, or for example, 0.5 mol% or more, based on the total constituent units of the polymer block (A). If the amount of the crosslinkable constituent unit introduced is 0.01 mol% or more, it is easy to obtain a block copolymer with high mechanical strength. On the other hand, from the viewpoint of flexibility, the upper limit of the crosslinkable constituent unit is, for example, 95 mol% or less, for example, 90 mol% or less, for example, 80 mol% or less, or for example, 60 mol% or less. The upper limit is, for example, 50 mol% or less, for example, 40 mol% or less, for example, 30 mol% or less, for example, 20 mol% or less, or for example, 10 mol% or less.
[0045] In the polymer block (A), the proportion of the structural units derived from the other monomers is preferably in the range of 0% by mass or more and 50% by mass or less with respect to all structural units of the polymer block (A), and is, for example, 40% by mass or less, for example, 30% by mass or less, for example, 20% by mass or less, and for example, 10% by mass or less.
[0046] (number average molecular weight) The number average molecular weight of the polymer block (A) is not particularly limited, but is preferably 1,000 to 80,000. When the present block copolymer has a plurality of polymer blocks (A), the number average molecular weight of the polymer block (A) means the sum of the number average molecular weights of all the polymer blocks (A). In the present block copolymer, if the number average molecular weight of the polymer block (A) is 1,000 or more, the molded product can exhibit sufficient strength and durability. If it is 80,000 or less, good fluidity and coatability can be ensured. From the viewpoint of the strength and fluidity of the molded product, the number average molecular weight of the polymer block (A) is more preferably in the range of 2,000 to 60,000, even more preferably in the range of 3,000 to 40,000, even more preferably in the range of 4,000 to 20,000, and even more preferably in the range of 5,000 to 10,000.
[0047] 1-2. Polymer block (B) Examples of the monomer constituting the polymer block (B) include the above-mentioned (meth)acrylic acid alkyl ester compounds, the compounds represented by the above-mentioned general formula (3), styrenes, maleimide compounds, and amide group-containing vinyl compounds in the same manner as the polymer block (A) (however, different from the polymer block (A)). One or more of these can be used.
[0048] In the polymer block (B), among the above monomers, it is preferable to use an acrylic acid alkyl ester as the main constituent unit, since it is possible to obtain a block copolymer having excellent flexibility. Furthermore, among these, an acrylic acid alkyl ester compound having an alkyl group with 4 to 12 carbon atoms is preferable. Furthermore, in terms of the fluidity of the block copolymer, it is more preferable that the acrylic compound contains an acrylic acid alkyl ester compound having an alkyl group with 4 to 8 carbon atoms.
[0049] In the polymer block (B), the constituent units derived from the (meth)acrylic acid alkyl ester compound can be 50% by mass or more and 100% by mass or less. More preferably, it is 60% by mass or more and 100% by mass or less, even more preferably, it is 70% by mass or more and 100% by mass or less, and even more preferably, it is 80% by mass or more and 100% by mass or less. When the above-mentioned constituent units are in the above-mentioned range, a block copolymer having good mechanical properties tends to be obtained.
[0050] The polymer block (B) may further contain a crosslinkable constituent unit derived from the above-mentioned vinyl monomer having a crosslinkable functional group.
[0051] The crosslinkable constituent unit in the polymer block (B) is preferably provided as necessary in addition to the crosslinkable constituent unit in the polymer block (A). Although not particularly limited, the crosslinkable constituent unit can be, for example, 0.01 mol% or more, for example, 0.1 mol% or more, or for example, 0.5 mol% or more, based on the total constituent units of the polymer block (B). If the amount of the crosslinkable constituent unit introduced is 0.01 mol% or more, it is easy to obtain a block copolymer with high mechanical strength. On the other hand, from the viewpoint of flexibility, the upper limit of the crosslinkable constituent unit is, for example, 20 mol% or less, for example, 10 mol% or less, or for example, 5 mol% or less. Note that, from the viewpoint of forming a uniform crosslinked structure, it is preferable to concentrate crosslinking points in the polymer block (A), and it is preferable that the ratio of the crosslinkable constituent unit to the total constituent units of the polymer block (B) does not exceed the ratio of the crosslinkable constituent unit to the total constituent units of the polymer block (A).
[0052] (number average molecular weight) The number average molecular weight (Mn) of the polymer block (B) is not particularly limited, but is preferably from 9,000 to 250,000. In addition, when the present block copolymer has a plurality of polymer blocks (B), the number average molecular weight of the polymer block (B) means the sum of the number average molecular weights of all the polymer blocks (B). In the present block copolymer, if the number average molecular weight of the polymer block (B) is 9,000 or more, the molded product can exhibit sufficient strength and durability. If it is 250,000 or less, good fluidity and coatability can be ensured. Since the present block copolymer can form a uniform crosslinked structure, the molecular weight of the present block copolymer corresponding to the distance between crosslinking points can be ensured. From the viewpoint of the strength and fluidity of the molded product, the polymer block (B) is more preferably in the range of 14,000 to 150,000, even more preferably in the range of 19,000 to 100,000, even more preferably in the range of 23,000 to 80,000, and even more preferably in the range of 25,000 to 55,000.
[0053] 1-3.Block copolymers The present block copolymer is a block copolymer consisting of at least two polymer blocks, and preferably has one or more of each of polymer block (A) and polymer block (B). The present block copolymer may have a structural unit (ABA) consisting of polymer block (A) / polymer block (B) / polymer block (A), or may have a structural unit (ABC) consisting of polymer block (A) / polymer block (B) / polymer block (C). Examples of the monomer constituting the polymer block (C) include the above-mentioned (meth)acrylic acid alkyl ester compounds, compounds represented by the above-mentioned general formula (3), styrenes, maleimide compounds, and amide group-containing vinyl compounds in the same manner as the polymer blocks (A) and (B) (however, different from the polymer blocks (A) and (B)). One or more of these can be used.
[0054] Here, the block copolymer is A-(BA) n (where n is an integer of 1 or more), from the viewpoint of strength of the molded article, it is preferable that the polymer block (A) contains a crosslinkable structural unit. With such a structure, the polymer block (A) containing the crosslinkable structural unit acts as a crosslinked segment, so that a uniform crosslinked structure can be obtained while ensuring the molecular weight between crosslinking points, and therefore the molded article can exhibit excellent performance in terms of mechanical properties such as breaking elongation and breaking strength.
[0055] The content of the polymer block (A) in the present block copolymer relative to 100 parts by mass of the total amount of the polymer blocks (A) and (B) is not particularly limited, but is preferably 60 parts by mass or less, more preferably 2 parts by mass or more and 60 parts by mass or less, even more preferably 4 parts by mass or more and 50 parts by mass or less, still more preferably 6 parts by mass or more and 40 parts by mass or less, still more preferably 8 parts by mass or more and 30 parts by mass or less, and even more preferably 10 parts by mass or more and 20 parts by mass or less. When the present block copolymer contains a crosslinkable constitutional unit, such a range makes it easier to obtain a molded product with good mechanical properties from the polymer block (A) that serves as a crosslinking point and constitutes a crosslinked segment, and the polymer block (B) that can become a non-crosslinked segment.
[0056] The number average molecular weight (Mn) of the present block copolymer is not particularly limited, but is preferably 10,000 to 300,000. In the present block copolymer, if the number average molecular weight is 10,000 or more, the molded product can exhibit sufficient strength and durability. Also, if the number average molecular weight is 300,000 or less, good fluidity and coatability can be ensured. From the viewpoint of the strength and fluidity of the molded product, the number average molecular weight of the present block copolymer is more preferably in the range of 15,000 to 200,000, even more preferably in the range of 20,000 to 150,000, still more preferably in the range of 25,000 to 90,000, and even more preferably in the range of 30,000 to 60,000.
[0057] In addition, the molecular weight distribution (Mw / Mn) obtained by dividing the weight average molecular weight (Mw) of the block copolymer by the number average molecular weight (Mn) is preferably 4.00 or less from the viewpoint of mechanical properties (elongation at break, strength at break, etc.). When the block copolymer contains a crosslinkable structural unit, it is more preferably 3.00 or less, even more preferably 2.00 or less, still more preferably 1.80 or less, even more preferably 1.50 or less, and even more preferably 1.40 or less from the viewpoint of forming a uniform crosslinked structure and ensuring the mechanical properties (elongation at break, strength at break, etc.). In addition, the molecular weight distribution (Mw / Mn) is preferably 1.05 or more, may be 1.10 or more, or may be 1.30 or more.
[0058] 2.Resin composition The present block copolymer can be used alone as a sealing material, an adhesive, a pressure-sensitive adhesive, a coating material, an elastomer, or the like, but may also be in the form of a resin composition containing known additives, etc., as necessary.
[0059] In addition, when the present block copolymer has a crosslinkable functional group, a necessary crosslinking agent, other polymers having a crosslinkable functional group, a crosslinking accelerator, and the like can be blended depending on the type of the crosslinkable functional group to form a curable resin composition, and if necessary, a molded product depending on the application can be obtained by subjecting the composition to a heat treatment or the like.
[0060] Examples of the crosslinking agent (curing agent) include a glycidyl compound having two or more glycidyl groups, an isocyanate compound having two or more isocyanate groups, an aziridine compound having two or more aziridinyl groups, an oxazoline compound having an oxazoline group, a metal chelate compound, a butylated melamine compound, etc. Among these, the aziridine compound, the glycidyl compound, and the isocyanate compound are preferred, and among these, the isocyanate compound is preferred in terms of excellent molded product physical properties under high temperature conditions.
[0061] Examples of the aziridine compound include 1,6-bis(1-aziridinylcarbonylamino)hexane, 1,1'-(methylene-di-p-phenylene)bis-3,3-aziridyl urea, 1,1'-(hexamethylene)bis-3,3-aziridyl urea, ethylene bis-(2-aziridinyl propionate), tris(1-aziridinyl)phosphine oxide, 2,4,6-triaziridinyl-1,3,5-triazine, and trimethylolpropane-tris-(2-aziridinyl propionate).
[0062] Examples of the glycidyl compound include polyfunctional glycidyl compounds such as ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, tetraglycidylxylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, trimethylolpropane polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, and sorbitol polyglycidyl ether.
[0063] As the isocyanate compound, for example, a compound having two or more isocyanate groups is used. As the isocyanate compound, various aromatic, aliphatic and alicyclic isocyanate compounds, as well as modified products of these isocyanate compounds (modified isocyanates) can be used.
[0064] Examples of aromatic isocyanates include diphenylmethane diisocyanate (MDI), crude diphenylmethane diisocyanate, tolylene diisocyanate, naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), xylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), and tolidine diisocyanate (TODI). Examples of the aliphatic isocyanate include hexamethylene diisocyanate (HDI), lysine diisocyanate (LDI), and lysine triisocyanate (LTI). Examples of the alicyclic isocyanate include isophorone diisocyanate (IPDI), cyclohexyl diisocyanate (CHDI), hydrogenated XDI (H6XDI), and hydrogenated MDI (H12MDI). In addition, examples of modified isocyanates include urethane-modified, dimers, trimers, carbodiimide-modified, allophanate-modified, biuret-modified, urea-modified, isocyanurate-modified, oxazolidone-modified, and isocyanate-terminated prepolymers of the above-mentioned isocyanate compounds.
[0065] When the resin composition disclosed in this specification contains a crosslinking agent (curing agent), the content thereof may be from 0.01 to 10 parts by mass relative to 100 parts by mass of the present block copolymer, or from 0.03 to 5 parts by mass, or from 0.05 to 2 parts by mass.
[0066] Other polymers having a crosslinkable functional group include polyoxyalkylene polymers having a crosslinkable functional group, (meth)acrylic polymers having a crosslinkable functional group (however, different from the present block copolymer), polyester polymers having a crosslinkable functional group, polyurethane polymers having a crosslinkable functional group, polybutadiene polymers having a crosslinkable functional group, hydrogenated polybutadiene polymers having a crosslinkable functional group, and hydrocarbon polymers such as polyisobutylene polymers having a crosslinkable functional group, polyamide polymers, and bisphenol polymers. Among these, when the present block copolymer has a (meth)acrylic acid ester compound as a main constituent monomer, polyoxyalkylene polymers having a crosslinkable functional group are preferred from the viewpoints of excellent compatibility, excellent mechanical properties of the molded product, and excellent weather resistance. Here, examples of the crosslinkable functional group include those mentioned above.
[0067] The polyoxyalkylene polymer having a crosslinkable functional group is not particularly limited as long as it contains a repeating unit represented by the following general formula (5). -OR 1 - (5) (In the formula, R 1 is a divalent hydrocarbon group. R in the above general formula (5) 1 Examples of such methods include the following: (CH2) n (n is an integer between 1 and 10) CH(CH3)CH2 CH(C2H5)CH2 C(CH3)2CH2 The polyoxyalkylene polymer may contain one or a combination of two or more of the repeating units. Among these, CH(CH3)CH2 is preferred from the viewpoint of excellent workability.
[0068] As the crosslinkable functional group contained in the polyoxyalkylene polymer, a crosslinkable silyl group is particularly preferred from the viewpoint of excellent compatibility, excellent mechanical properties of the molded product, and excellent weather resistance.The crosslinkable silyl group is not particularly limited, and includes alkoxysilyl group, halogenosilyl group, silanol group, etc., but alkoxysilyl group is preferred from the viewpoint of easy control of reactivity.Specific examples of the alkoxysilyl group include trimethoxysilyl group, methyldimethoxysilyl group, dimethylmethoxysilyl group, triethoxysilyl group, methyldiethoxysilyl group, dimethylethoxysilyl group, etc.
[0069] The method for producing the polyoxyalkylene polymer is not particularly limited, and examples thereof include a polymerization method using an alkali catalyst such as KOH, a polymerization method using a transition metal compound-porphyrin complex catalyst, a polymerization method using a composite metal cyanide complex catalyst, and a polymerization method using phosphazene, using a corresponding epoxy compound or diol as a raw material. The polyoxyalkylene polymer may be either a linear polymer or a branched polymer, or a combination of these may be used.
[0070] The average number of crosslinkable silyl groups contained in one molecule of the polyoxyalkylene polymer is preferably in the range of 1 to 4, and more preferably in the range of 1.5 to 3, from the viewpoints of the mechanical properties and adhesiveness of the cured product. The position of the crosslinkable silyl group contained in the polyoxyalkylene polymer is not particularly limited, and it may be located in a side chain and / or at the end of the polymer. The polyoxyalkylene polymer may be either a linear polymer or a branched polymer, or a combination of these may be used.
[0071] The number average molecular weight (Mn) of the polyoxyalkylene polymer is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 15,000 or more, from the viewpoint of mechanical properties. Mn may be 18,000 or more, 22,000 or more, or 25,000 or more. The upper limit of Mn is preferably 60,000 or less, more preferably 50,000 or less, and even more preferably 40,000 or less, from the viewpoint of workability (viscosity) during application of the curable resin composition. The range of Mn can be set by combining the above upper and lower limits, and may be, for example, 5,000 or more and 60,000 or less, 15,000 or more and 60,000 or less, 18,000 or more and 50,000 or less, or 22,000 or more and 50,000 or less.
[0072] Commercially available products may be used as the polyoxyalkylene polymer. Specific examples include "MS Polymer S203", "MS Polymer S303", "MS Polymer S810", "Silyl SAT200", "Silyl SAT350", "Silyl EST280" and "Silyl SAT30" manufactured by Kaneka Corporation, and "Exestar ES-S2410", "Exestar ES-S2420" and "Exestar ES-S3430" (all trade names) manufactured by AGC Inc.
[0073] Other examples of the additives include plasticizers, fillers, adhesion promoters, dehydrating agents, hardening accelerators, antioxidants, ultraviolet absorbing agents, and oils.
[0074] Examples of the plasticizer include polyester-based plasticizers obtained from liquid polyurethane resin, dicarboxylic acid and diol; etherified or esterified polyalkylene glycols such as polyethylene glycol and polypropylene glycol; polyether-based plasticizers such as saccharide-based polyethers obtained by addition polymerization of alkylene oxides such as ethylene oxide and propylene oxide to saccharide polyhydric alcohols such as sucrose, followed by etherification or esterification; polystyrene-based plasticizers such as poly-α-methylstyrene; and poly(meth)acrylates having no crosslinkable functional groups. Among these, poly(meth)acrylates having no crosslinkable functional groups are preferred in terms of durability such as weather resistance of the cured product. Among these, those having Mw in the range of 1,000 to 7,000 and glass transition temperature of -30°C or less are more preferred. The amount of the plasticizer used is preferably in the range of 0 to 100 parts by mass, may be in the range of 0 to 80 parts by mass, or may be in the range of 0 to 50 parts by mass, relative to 100 parts by mass of the total amount of the polyoxyalkylene polymer and the present block copolymer. Examples of fillers include light calcium carbonate with an average particle size of about 0.02 to 2.0 μm, heavy calcium carbonate with an average particle size of about 1.0 to 5.0 μm, titanium oxide, carbon black, synthetic silicic acid, talc, zeolite, mica, silica, calcined clay, kaolin, bentonite, aluminum hydroxide, barium sulfate, glass balloons, silica balloons, and polymethyl methacrylate balloons. These fillers improve the mechanical properties of the cured product, and can increase the tensile strength and tensile elongation. Among these, light calcium carbonate, heavy calcium carbonate and titanium oxide are preferred, which are highly effective in improving physical properties, and a mixture of light calcium carbonate and heavy calcium carbonate is more preferred. The amount of the filler added is preferably 20 to 300 parts by mass, more preferably 50 to 200 parts by mass, per 100 parts by mass of the total amount of the polyoxyalkylene polymer and the present block copolymer. When a mixture of light calcium carbonate and heavy calcium carbonate is used as described above, the mass ratio of light calcium carbonate / heavy calcium carbonate is preferably in the range of 90 / 10 to 50 / 50.
[0075] Examples of adhesion promoters include aminosilanes such as those available from Shin-Etsu Silicones under the trade names "KBM602", "KBM603", "KBE602", "KBE603", "KBM902" and "KBM903".
[0076] Examples of dehydrating agents include methyl orthoformate, methyl orthoacetate, and vinylsilane.
[0077] As the curing accelerator, known compounds such as tin-based catalysts, titanium-based catalysts and tertiary amines can be used. Examples of tin-based catalysts include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin diacetonate, dioctyltin dilaurate, etc. Specific examples include products sold by Nitto Kasei Corporation under the trade names "Neostan U-28", "Neostan U-100", "Neostan U-200", "Neostan U-220H", "Neostan U-303", and "SCAT-24". Examples of titanium catalysts include tetraisopropyl titanate, tetra-n-butyl titanate, titanium acetylacetonate, titanium tetraacetylacetonate, titanium ethyl acetylacetonate, dibutoxytitanium diacetylacetonate, diisopropoxytitanium diacetylacetonate, titanium octylene glycolate, and titanium lactate. Examples of tertiary amines include triethylamine, tributylamine, triethylenediamine, hexamethylenetetramine, 1,8-diazabicyclo[5,4,0]undecene-7 (DBU), diazabicyclononene (DBN), N-methylmorpholine, and N-ethylmorpholine. The amount of the curing accelerator used is preferably 0.1 to 5 parts by mass, and more preferably 0.5 to 2 parts by mass, based on 100 parts by mass of the total amount of the polyoxyalkylene polymer and the present block copolymer.
[0078] As the age resistor, usable are ultraviolet absorbers such as benzophenone-based compounds, benzotriazole-based compounds, and anilide oxalate compounds, light stabilizers such as hindered amine-based compounds, antioxidants such as hindered phenol-based compounds, heat stabilizers, and age resistors which are mixtures thereof.
[0079] Examples of ultraviolet absorbers include BASF's Tinuvin 571, Tinuvin 1130, and Tinuvin 327. Examples of light stabilizers include BASF's Tinuvin 292, Tinuvin 144, and Tinuvin 123, and Sankyo's Sanol 770. Examples of heat stabilizers include BASF's Irganox 1135, Irganox 1520, and Irganox 1330. BASF's Tinuvin B75, a mixture of ultraviolet absorber, light stabilizer, and heat stabilizer, may also be used.
[0080] Other thermoplastic resins may be added for the purpose of adjusting the performance, coatability, processability, etc. of the resin composition containing the block copolymer. Specific examples of thermoplastic resins include polyolefin resins such as polyethylene and polypropylene, styrene resins such as polystyrene, vinyl resins such as polyvinyl chloride, polyester resins, polyamide resins, etc. Also, known elastomers may be added and mixed.
[0081] The curable resin composition of the present invention can be prepared as a one-component type in which all ingredients are mixed in advance and stored in a sealed state, and then cured by absorbing moisture in the air after application. It can also be prepared as a two-component type in which ingredients such as a curing catalyst, a filler, a plasticizer, and water are mixed separately as a curing agent, and the ingredients are mixed with the polymer composition before use. The one-component type is more preferable because it is easy to handle and there is less chance of mixing errors when applying.
[0082] The resin composition containing the present block copolymer exhibits good fluidity when heated to room temperature (25° C.) to about 150° C. Therefore, it can be applied to various coating processes as well as molding processes using various methods such as extrusion molding, injection molding, and casting.
[0083] 3. Method for producing block copolymer The method for producing a block copolymer consisting of at least two polymer blocks of the present invention includes the steps of producing a block copolymer (P1) consisting of at least three polymer blocks and having a trithiocarbonate group represented by the above general formula (2) in a central polymer block of the block copolymer by a reversible addition-fragmentation chain transfer living radical polymerization method (RAFT method), and producing a block copolymer (P2) consisting of at least two polymer blocks by reacting the trithiocarbonate group of the block copolymer (P1) with a nucleophile.
[0084] 3-1. Manufacturing process of block copolymer (P1) The living radical polymerization may be any process such as a batch process, a semi-batch process, a tubular continuous polymerization process, a continuous stirred tank process (CSTR), etc. The polymerization method may be applied to various modes such as bulk polymerization without using a solvent, solution polymerization in a solvent system, emulsion polymerization in an aqueous system, mini-emulsion polymerization, or suspension polymerization.
[0085] In the RAFT method, controlled polymerization proceeds through a reversible chain transfer reaction in the presence of a specific polymerization control agent (RAFT agent) and a general free radical polymerization initiator. As the RAFT agent, a compound having a trithiocarbonate group represented by the above general formula (2) can be used. Examples of compounds having a trithiocarbonate group represented by the above general formula (2) include S,S-dibenzyl trithiocarbonate, bis[4-(2,3-dihydroxypropoxycarbonyl)benzyl]trithiocarbonate, and bis[4-(2-hydroxyethoxycarbonyl)benzyl]trithiocarbonate. Here, when the compound having a trithiocarbonate group represented by the above general formula (2) does not have a structure represented by the above general formula (1) or a thiol group as a substituent, the structure of one terminal of the block copolymer (P2) is the structure represented by the above general formula (1) or a thiol group. On the other hand, when the compound having a trithiocarbonate group represented by the above general formula (2) has a structure represented by the above general formula (1) or a thiol group as a substituent, the structures of both terminals of the block copolymer (P2) are the structures represented by the above general formula (1) or a thiol group. The amount of the RAFT agent used is appropriately adjusted depending on the types of monomer and RAFT agent used.
[0086] As the polymerization initiator used in the polymerization by the RAFT method, known radical polymerization initiators such as azo compounds, organic peroxides and persulfates can be used, but azo compounds are preferred because they are safe and easy to handle and do not easily cause side reactions during radical polymerization.Specific examples of the azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), etc. The radical polymerization initiators may be used alone or in combination of two or more.
[0087] The proportion of the radical polymerization initiator used is not particularly limited, but from the viewpoint of obtaining a polymer with a narrower molecular weight distribution, the amount of the radical polymerization initiator used relative to 1 mol of the RAFT agent is preferably 0.5 mol or less, more preferably 0.3 mol or less. In addition, from the viewpoint of stably carrying out the polymerization reaction, the lower limit of the amount of the radical polymerization initiator used relative to 1 mol of the RAFT agent is 0.001 mol. Therefore, the amount of the radical polymerization initiator used relative to 1 mol of the RAFT agent is preferably in the range of 0.001 mol to 0.5 mol, more preferably in the range of 0.005 mol to 0.3 mol.
[0088] The reaction temperature during the polymerization reaction by the RAFT method is preferably 30° C. or higher and 120° C. or lower, more preferably 40° C. or higher and 110° C. or lower, and even more preferably 50° C. or higher and 100° C. or lower. If the reaction temperature is 30° C. or higher, the polymerization reaction can proceed smoothly. On the other hand, if the reaction temperature is 120° C. or lower, side reactions can be suppressed and restrictions on usable initiators and solvents can be relaxed.
[0089] By using a compound having a trithiocarbonate group represented by the above general formula (2) as a RAFT agent, an A-(BA)n type structure consisting of polymer block (A)-polymer block (B)-polymer block (A) can be obtained by living radical polymerization. In this case, first, in the first polymerization step, polymer block (A) is obtained using the constituent monomers of polymer block (A). Then, in the second polymerization step, polymer block (B) is obtained using the constituent monomers of polymer block (B), thereby obtaining a BAB triblock copolymer. Furthermore, in the third polymerization step, polymer block (A) is obtained using the constituent monomers of polymer block (A), thereby obtaining a higher order block copolymer such as an ABABA pentablock copolymer.
[0090] In the present disclosure, regardless of the polymerization method, the polymerization of the block copolymer may be carried out in the presence of a chain transfer agent as necessary.The chain transfer agent may be a known one, specifically, ethanethiol, 1-propanethiol, 2-propanethiol, 1-butanethiol, 2-butanethiol, 1-hexanethiol, 2-hexanethiol, 2-methylheptane-2-thiol, 2-butylbutane-1-thiol, 1,1-dimethyl-1-pentanethiol, 1-octanethiol, 2-octanethiol, 1-decanethiol, 3-decanethiol, 1-undecanethiol, 1-dodecanethiol, 2- Examples of the alkylthiol compounds having an alkyl group having 2 to 20 carbon atoms, such as dodecanethiol, 1-tridecanethiol, 1-tetradecanethiol, 3-methyl-3-undecanethiol, 5-ethyl-5-decanethiol, tert-tetradecanethiol, 1-hexadecanethiol, 1-heptadecanethiol, and 1-octadecanethiol, include mercaptoacetic acid, mercaptopropionic acid, and 2-mercaptoethanol, and one or more of these can be used.
[0091] In the present disclosure, known polymerization solvents can be used in living radical polymerization.Specific examples include orthoester compounds such as trimethyl orthoacetate and triethyl orthoacetate; aromatic compounds such as benzene, toluene, xylene, and anisole; ester compounds such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; ketone compounds such as acetone and methyl ethyl ketone; dimethylformamide, acetonitrile, dimethyl sulfoxide, alcohol, water, and the like.In addition, the polymerization may be performed in a form such as bulk polymerization without using a polymerization solvent.
[0092] 3-2. Manufacturing process of block copolymer (P2) The method for producing a polymer of the present invention includes a step of reacting a trithiocarbonate group in the block copolymer (P1) with a nucleophile to obtain a block copolymer (P2). For example, when the block copolymer (P1) is a triblock copolymer, the block copolymer (P2) can be obtained as a diblock copolymer, and when the block copolymer (P1) is a pentablock copolymer, the block copolymer (P2) can be obtained as a triblock copolymer.
[0093] The nucleophilic agent includes ammonia, primary and / or secondary amine compounds, alkali metal alkoxides, hydroxides, and thiols, and these can be known compounds. By reacting a nucleophilic agent with a thiocarbonylthio group, the thiocarbonylthio group is converted to a thiol group, and it is presumed that the odor of the resulting block copolymer is reduced as a result of the Michael addition reaction between the thiol group and the remaining acrylate compound. Among these, primary and / or secondary amine compounds are preferred from the viewpoint of reactivity.
[0094] The molar equivalent of the nucleophilic agent relative to the thiocarbonylthio group is 2 to 90 molar equivalents. From the viewpoint of reaction efficiency, 3 molar equivalents or more is preferable, and the lower limit may be 4 molar equivalents or more, 5 molar equivalents or more, 10 molar equivalents or more, or 15 molar equivalents or more. Also, from the viewpoint of reducing the influence of odor due to unreacted nucleophile, 75 molar equivalents or less is preferable, 60 molar equivalents or less is more preferable, and 50 molar equivalents or less is particularly preferable.
[0095] The molecular weight of the nucleophile is preferably 150 or less, more preferably 110 or less, and particularly preferably 60 or less, from the viewpoint of ease of removing unreacted nucleophile.
[0096] As the reactor, known reactors such as a batch reactor and a tubular reactor can be used. A batch reactor is preferred since there is no risk of clogging, which is a problem with tubular reactors.
[0097] From the viewpoint of reaction efficiency, the reaction temperature is preferably 10° C. or higher, more preferably 15° C. or higher, and particularly preferably 25° C. or higher. Moreover, from the viewpoint of preventing side reactions such as nucleophilic reactions on the polymer main chain, the reaction temperature is preferably 80° C. or lower, more preferably 60° C. or lower, and particularly preferably 50° C. or lower.
[0098] The reaction time is preferably 1 hour or more, more preferably 2 hours or more, and particularly preferably 3 hours or more from the viewpoint of reaction efficiency, and is preferably 48 hours or less, more preferably 36 hours or less, and particularly preferably 24 hours or less, from the viewpoint of preventing side reactions such as nucleophilic reactions on the polymer main chain.
[0099] The reaction pressure is usually normal pressure, but may be increased or decreased as necessary.
[0100] Here, at least one polymer block of the block copolymer (P2) has a (meth)acrylic acid ester compound as a main constituent monomer, at least one terminal structure of the block copolymer (P2) is a structure represented by the above general formula (1) or a thiol group, and the product of (x / 100) and y, where x is the sulfur concentration (mass%) in the block copolymer (P2) and y is the number average molecular weight of the block copolymer (P2), is 60 or less, thereby achieving an effect of significantly reducing odor when exposed to high temperatures. The product of (x / 100) and y is preferably 57.5 or less, more preferably 55.0 or less, even more preferably 52.5 or less, and even more preferably 50.0 or less. In this respect, it is preferable to obtain the block copolymer (P2) by reacting the trithiocarbonate group in the block copolymer (P1) with a nucleophile without purifying the block copolymer (P1) by reprecipitation or the like. EXAMPLES
[0101] The present disclosure will be specifically described below based on examples. Note that the present disclosure is not limited to these examples. Note that, in the following, "parts" and "%" mean parts by mass and % by mass unless otherwise specified. The analytical methods for the block copolymers obtained in the Production Examples, Comparative Production Examples, Examples and Comparative Examples are described below.
[0102] <Molecular weight measurement> The block copolymer thus obtained was subjected to gel permeation chromatography (GPC) measurement under the conditions described below to obtain the number average molecular weight (Mn) and weight average molecular weight (Mw) in terms of polystyrene. The molecular weight distribution (Mw / Mn) was calculated from the obtained values. Measurement conditions Column: Tosoh TSKgel SuperMultiporeHZ-M x 4 Solvent: Tetrahydrofuran Temperature: 40℃ Detector: RI Flow rate: 600μL / min
[0103] <Monomer reaction rate measurement> The resulting polymer was subjected to gas chromatography (GC) measurement under the conditions described below, and the monomer reaction rate (%) was calculated from the resulting monomer concentration (wt%). Measurement conditions Columns: Capillary columns Agilent CP-Wax52CB (60m x 0.32mm ID, df = 0.5μm) and Agilent DB-1 (30m x 0.32mm ID, df = 1.0μm) Solvent: Tetrahydrofuran Column temperature: 50°C (5 min), 7°C / min, 230°C (5 min)
[0104] <Viscosity measurement> The E-type viscosity was measured under the following conditions using a TVE-20H viscometer (cone / plate type, manufactured by Toki Sangyo Co., Ltd.). Measurement conditions Cone shape: angle 1°34′, radius 24mm (less than 10000mPa·s) Angle 3°, radius 7.7mm (10000mPa s or more) Temperature: 25℃±0.5℃
[0105] <Sulfur concentration (mass%): x> The x in block copolymers d1 to d31 shown in Tables 8 and 9, and in e-2, e-4, and e-6 shown in Comparative Production Examples 1 to 3, was measured according to the following method. Note that the measurements were performed with precision to four decimal places. 2g of block copolymer was collected in each of four 20ml-PFA bottles. 1g, 2g, and 3g of the 20ppm-S standard solution were collected in three of the PFA bottles. In addition, one of the PFA bottles was left without the 20ppm-S standard solution. Furthermore, each was diluted with 2-propanol (IPA) to a total of 10g to prepare a test solution. The test solution was measured with an inductively coupled plasma (ICP) emission spectrometer to observe the emission intensity of sulfur. The sulfur concentration in the test solution was calculated from the linear regression line of the standard addition concentration and emission intensity. The dilution rate of the test solution was converted to obtain x in block copolymers d1 to d31, e-2, e-4, and e-6. The results are shown in Tables 8 and 9, and Comparative Production Examples 1 to 3. Pretreatment environment: Clean room (Class 1000) and clean draft (Class 100) ICP optical emission spectrometer: Spectro ARCOS SOP (organic solvent introduction conditions) 2-Propanol (IPA): Kanto Chemical's Primepure (M) Dimethyl sulfoxide (DMSO): Fujifilm Wako Pure Chemical Industries, Ltd. (special grade reagent) 1000 ppm-S standard solution: 1.22 g of DMSO was diluted with IPA to a total volume of 50 g, and 5 g of that was then diluted with IPA to a total volume of 50 g. 20 ppm-S standard solution: 1 g of the above 1000 ppm-S standard solution was diluted with IPA to a total volume of 50 g.
[0106] <product of (x / 100) and y> The number average molecular weight (Mn) of block copolymers d1 to d31 shown in Tables 8 and 9, and e-2, e-4, and e-6 shown in Comparative Production Examples 1 to 3 was defined as y, and the product of (x / 100) and y was calculated. The results are shown in Tables 8 and 9, and Comparative Production Examples 1 to 3.
[0107] <Odor Intensity> The odor intensity of block copolymers d1 to d31 shown in Tables 8 and 9, and e-2, e-4 and e-6 shown in Comparative Production Examples 1 to 3 was measured by the following method. After placing 1 g of the block copolymer in a test tube, an odor bag (manufactured by AS ONE Corporation) was attached to the test tube, and the odor intensity in the odor bag after heating at 60° C. for 30 minutes was subjected to a sensory evaluation. The sensory evaluation panel consisted of five members, each of whom prepared an odorless bag separately and compared it with the sample to evaluate it. They then scored the sample on a 6-point scale between 0 and 5 points according to the following criteria, and the average score was taken as the odor intensity of the sample. A break of at least 3 minutes was taken after each sample evaluation. The results are shown in Tables 10 and 11. 0 points: Odorless 1 point: Barely detectable odor 2 points: A weak odor that is easy to identify 3 points: Easily detectable odor 4 points: Strong odor 5 points: Strong odor
[0108] <Block copolymer composition ratio> The composition ratio of the obtained block copolymer is 1 Identification and calculation were performed using H-NMR measurement.
[0109] <Preparation and evaluation methods of resin compositions in examples and comparative examples> Each component was blended according to the blending ratio shown in Table 1 below (Blend A, Blend B, Blend C, and Blend D), and resin compositions were prepared according to a conventional method.
[0110] The abbreviations in Table 1 have the following meanings. Polyoxyalkylene polymer X: a polypropylene glycol having both ends silylated, as described in Synthesis Example 1 below Polyoxyalkylene polymer Y: Branched modified silicone Exestar ES-S3430 (AGC) UP-1110: Acrylic plasticizer, ARUFON (registered trademark) UP-1110 (manufactured by Toagosei Co., Ltd.) jER828: Epoxy resin jER828 (manufactured by Mitsubishi Chemical Corporation) jER Cure H30: Epoxy hardener jER Cure H30 (manufactured by Mitsubishi Chemical Corporation) Light calcium carbonate: Hakuenka CCR (manufactured by Shiraishi Calcium Co., Ltd.) Heavy calcium carbonate: Super SS (manufactured by Maruo Calcium Co., Ltd.) R820: Titanium oxide R-820 (manufactured by Ishihara Sangyo Kaisha) #45: Carbon black #45 (Ishihara Sangyo Kaisha) · Irganox1010: Phenolic antioxidant, Irganox1010 (manufactured by BASF) B75: Anti-aging agent, Tinuvin B75 (manufactured by Chiba Specialties) SH6020: 3-(2-aminoethylamino)propyltrimethoxysilane, SH6020 (manufactured by Dow Corning Toray Co., Ltd.) S340: N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)propanamine, Silaace S340 (JNC Corporation) SZ6300: Vinyltrimethoxysilane, SZ6300 (manufactured by Dow Corning Toray Co., Ltd.) U-220H: Tin catalyst (dibutyltin diacetylacetonate), Neostan U-220H (manufactured by Nitto Kasei Co., Ltd.)
[0111] [Table 1]
[0112] <Tensile test> Each resin composition (Formulation A, Formulation B, and Formulation D) was applied to a Teflon (registered trademark) sheet at room temperature (25°C) to a thickness of 2 mm, and cured at 23°C and 50% RH for 6 days, and then at 50°C in a saturated water vapor atmosphere for 1 day to produce a cured sheet with a thickness of 2 mm. In addition, each resin composition (formulation C) was dissolved in tetrahydrofuran (THF) to prepare a solution with a base resin concentration of 10%, which was poured into a mold and the THF was dried and distilled off to produce a cast sheet with a thickness of 2 mm. Test pieces were punched out from the sheet obtained above using a No. 3 dumbbell, and the breaking elongation [EL (%)] and breaking strength [Ts (MPa)] were measured using a tensile tester (Autograph AGS-J, manufactured by Shimadzu Corporation). The measurements were performed at a tensile speed of 200 mm / min in an environment of a temperature of 23°C and a humidity of 50%. The tensile product was calculated as follows: Tensile product = breaking elongation [EL (%)] × breaking strength [Ts (MPa)] / 2
[0113] <Weather resistance test> Each resin composition (formulation D) was applied to a Teflon (registered trademark) sheet at room temperature (25°C) to a thickness of 2 mm, and cured for one week at 23°C and 50% RH to produce a cured sheet. The resulting cured sheet was placed in a metaling weather meter (DAIPLA METAL WEATHER KU-R5NCI-A manufactured by Daipla Wintes) and subjected to an accelerated weather resistance test. The irradiation conditions were 63°C, 70% RH, and illuminance of 80 mW / cm. 2 The test was carried out for 1500 hours, with a 2-minute shower once every 2 hours. After 1500 hours, the surface condition was visually checked (whether cracks had occurred) and the color difference (△E) was obtained using a color difference meter (Spectrocolorimeter SE-2000, manufactured by Nippon Denshoku Co., Ltd.), and the weather resistance was evaluated based on the degree of fading. The color difference (△E) was calculated based on the lightness (L*) and chromaticity (a) in the red-green direction measured with the spectrocolorimeter. * ) and yellow-blue chromaticity (b * ) was calculated by substituting the value of
number
[0114] <Adhesive strength test> Tests were conducted using mortar boards and exterior mosaic tiles in accordance with JIS A5557 (2006) adhesive strength test method for organic adhesives for exterior tiling. Each adhesive composition (formulation D) was applied to a mortar board (TP Giken, 10 x 50 x 50 mm) to a thickness of approximately 5 mm, and then drawn with a comb trowel, followed by adhering a commercially available exterior mosaic tile (45 x 45 mm) conforming to the JIS A5209 regulations. After curing for 4 weeks at 23°C and 50% RH, a special jig was attached to the tile side and the mortar side, and a tensile tester (Autograph AGS-J, Shimadzu Corporation) was used to measure the adhesive strength at 23°C and a tensile speed of 3 mm / min.
[0115] <Synthesis of polyoxyalkylene polymer having crosslinkable functional group> Zinc hexacyanocobaltate glyme complex (0.05 g), polypropylene glycol (Mn: 2000, 50 g), and propylene glycol (510 g) were placed in a 1000 mL pressure-type stirred tank reactor equipped with an oil jacket, heated to 120 ° C, and reacted until the pressure change disappeared. Next, the mixture was heated under vacuum at 120 ° C for 1 hour to distill off the volatile components. Then, a 28% methanol solution of sodium methoxide (12.6 g) was added, and the pressure was reduced at 100 ° C for 1 hour to distill off the methanol. Next, allyl chloride (5.2 g) was added, and the mixture was heated at 100 ° C for 2 hours. Then, the reaction solution was washed twice with water (300 ml) to remove the salt. After dehydration by vacuum heating at 100°C for 2 hours, chloroplatinic acid hexahydrate (0.02g) and methyldimethoxysilane (8.3g) were added and reacted for 4 hours to obtain a double-ended silylated polypropylene glycol (also called "polyoxyalkylene polymer X"). The molecular weight of polyoxyalkylene polymer X was Mn 22,900 and Mw 25,200 as determined by GPC (gel permeation chromatography) (polystyrene equivalent).
[0116] <Production of polymer block (A)> (Synthesis Example 1: Production of polymer a-1) In a 500 mL flask equipped with a stirrer and a thermometer, S,S-dibenzyl trithiocarbonate (hereinafter also referred to as "DBTTC") (7.4 g), 2,2'-azobis(2-methylbutyronitrile) (hereinafter also referred to as "ABN-E") (0.49 g), n-butyl acrylate (hereinafter also referred to as "nBA") (75 g), trimethoxysilylpropyl methacrylate (25 g) and trimethyl orthoacetate (hereinafter also referred to as "MOA") (5.1 g) were charged as RAFT agents, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 60 ° C. After 7 hours, the mixture was cooled to room temperature and the reaction was stopped. The molecular weight of the obtained polymer a-1 was Mn 3,300, Mw 5,200, and Mw / Mn 1.59 by GPC (gel permeation chromatography) measurement (polystyrene equivalent). The reaction rates of nBA and trimethoxysilylpropyl methacrylate were 75% and 98%, respectively, as determined by GC (gas chromatography).
[0117] (Synthesis Examples 2 to 18: Production of Polymers a-2 to a-18) Polymers a-2 to a-18 were obtained by the same procedure as in Synthesis Example 1, except that the raw materials were used as shown in Table 2 and the reaction temperature and reaction time were appropriately adjusted. The molecular weight of each polymer and the reaction rate of the monomer were measured and shown in Tables 2 and 3.
[0118] In Tables 2 and 3, the abbreviations other than those described in Synthesis Example 1 refer to the following compounds. EA: Ethyl acrylate ·TDA: Tetradecyl acrylate PhMI: N-phenylmaleimide St: styrene
[0119] [Table 2]
[0120] [Table 3]
[0121] <Production of triblock copolymer> (Synthesis Example 19: Production of triblock copolymer b-1) Polymer a-1 (5.3 g), nBA (95 g), ABN-E (0.10 g) and MOA (42 g) obtained in Synthesis Example 1 were charged into a 500 mL flask equipped with a stirrer and a thermometer, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was started in a thermostatic bath at 60 ° C. Copolymerization of the remaining unreacted nBA and trimethoxysilylpropyl methacrylate in Synthesis Example 1 with the newly added nBA proceeded, but since the remaining unreacted trimethoxysilylpropyl methacrylate was in a trace amount, homopolymerization of nBA occurred almost entirely. After 6 hours, the mixture was cooled to room temperature to stop the reaction. The molecular weight of the obtained triblock copolymer b-1 was Mn 66,000, Mw 74,600, and Mw / Mn 1.13 by GPC (gel permeation chromatography) measurement (polystyrene equivalent). The reaction rate of the remaining unreacted nBA in Synthesis Example 1 and the newly added nBA was 84% in total, as determined by GC (gas chromatography) measurement.
[0122] (Synthesis Examples 20 to 42: Production of triblock copolymers b-2 to b-24) The raw materials were used as shown in Tables 4 and 5, and the reaction time was appropriately adjusted, but the same operation as in Synthesis Example 19 was carried out to obtain triblock copolymers b-2 to b-24. The molecular weight and monomer reaction rate of each triblock copolymer were measured and shown in Tables 4 and 5.
[0123] [Table 4]
[0124] [Table 5]
[0125] <Production of Pentablock Copolymer> (Synthesis Example 43: Preparation of pentablock copolymer c-1) A 500 mL flask equipped with a stirrer and a thermometer was charged with the triblock copolymer b-1 (141 g) obtained in Synthesis Example 19, trimethoxysilylpropyl methacrylate (1.17 g), ABN-E (0.043 g) and MOA (0.44 g), and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was started in a thermostatic bath at 60 ° C. Copolymerization of the remaining unreacted nBA in Synthesis Example 19 and the newly added trimethoxysilylpropyl methacrylate proceeded, and after 7 hours, the mixture was cooled to room temperature to stop the reaction, and a solution containing pentablock copolymer c-1 was obtained. The molecular weight of the obtained pentablock copolymer c-1 was Mn 68,200, Mw 79,800, and Mw / Mn 1.17 by GPC (gel permeation chromatography) measurement (polystyrene equivalent). The pentablock copolymer c-1 is a pentablock copolymer having a polymer block (A) consisting of nBA and trimethoxysilylpropyl methacrylate and a polymer block (B) consisting of nBA, and has the structural unit (A)-(B)-(A)-(B)-(A). From the polymerization rate, the composition ratio of the polymer block (A) and the acrylic polymer block (B) was (A) / (B) / (A) / (B) / (A)=2 / 41 / 14 / 41 / 2wt%, or in summary, (A) / (B)=18 / 82wt%.
[0126] (Synthesis Examples 44 to 66: Production of Pentablock Copolymers c-2 to c-24) Pentablock copolymers c-2 to c-24 were obtained by the same procedure as in Synthesis Example 43, except that the raw materials used were as shown in Tables 6 and 7. The molecular weight of each block copolymer and the (A) / (B) ratio or (A) / (B) / (C) ratio of the polymer blocks are shown in Tables 6 and 7.
[0127] In addition, the abbreviations in Table 7 other than those mentioned above represent the following compounds. ACMO: Acryloylmorpholine
[0128] [Table 6]
[0129] [Table 7]
[0130] <Post-treatment process of pentablock copolymers C-1 to C-24 and triblock copolymer B-23> (Production Example 1: Production of triblock copolymer d-1) The solution containing the pentablock copolymer c-1 obtained in Synthesis Example 43 was thoroughly degassed by bubbling with nitrogen, and then n-propylamine (2.78 g, 40 molar equivalents relative to the thiocarbonylthio groups of the pentablock copolymer c-1) was added, and the decomposition reaction of the thiocarbonyl groups was initiated in a thermostatic bath at 40° C. After 4 hours, the reaction was stopped by cooling to room temperature, and a solution containing a triblock copolymer d-1 was obtained. The solution was depressurized to 20 kPa and kept at 120° C. in a thin-film evaporator to continuously distill off volatile components such as unreacted monomers and solvents, and the non-volatile component, triblock copolymer d-1, was recovered. The obtained triblock copolymer d-1 has a polymer block (A) consisting of nBA and trimethoxysilylpropyl methacrylate and a polymer block (B) consisting of nBA, and is a triblock copolymer having a structural unit of (A)-(B)-(A), and is a Michael adduct of a thiol formed by decomposing the thiocarbonylthio group of the block copolymer c-1 with n-propylamine and a residual acrylate compound contained in the block copolymer c-1. 1From H-NMR measurements, it was confirmed that the peak (4.8 ppm) of hydrogen bonded to the carbon adjacent to the thiocarbonylthio group observed in the pentablock copolymer c-1 disappeared in the triblock copolymer d-1, and peaks (3.3 ppm, 2.9 ppm) derived from the Michael adduct with the residual acrylate compound (terminal molecular structure represented by general formula (1)) appeared. On the other hand, the molecular weight of the triblock copolymer d-1 was Mn 41,400, Mw 51,800, and Mw / Mn 1.25. In addition, the number of crosslinkable functional groups per molecule contained in block (A) was calculated to be 3.9 on average from the amount of trimethoxysilylpropyl methacrylate introduced per RAFT agent. Furthermore, x was 0.129, the product of (x / 100) and y was 53.4, and the E-type viscosity was 500,500 mPa s.
[0131] (Production Example 2: Production of triblock copolymer d-2) The solution containing the block copolymer c-1 obtained in Synthesis Example 43 was purified by reprecipitation from a mixed solvent of methanol / water = 80 / 20 mass ratio, and vacuum dried to obtain a block copolymer c-1. Pentablock copolymer c-1 (100 g), ethyl acetate (40 g) and MOA (10 g) were charged into a 500 mL flask equipped with a stirrer and a thermometer, and after sufficient degassing by nitrogen bubbling, n-propylamine (2.78 g, 40 molar equivalents relative to the thiocarbonylthio group of the pentablock copolymer c-1) was charged, and the decomposition reaction of the thiocarbonyl group was started in a thermostatic bath at 40 ° C. After 4 hours, the reaction was stopped by cooling to room temperature to obtain a solution containing a triblock copolymer d-2. The solution was depressurized to 20 kPa and kept at 120° C. in a thin-film evaporator to continuously distill off volatile components such as unreacted monomers and solvents, and the non-volatile component, triblock copolymer d-2, was recovered. The obtained triblock copolymer d-2 has a polymer block (A) consisting of nBA and trimethoxysilylpropyl methacrylate and a polymer block (B) consisting of nBA, and is a triblock copolymer having a structural unit of (A)-(B)-(A), in which the thiocarbonylthio group of the block copolymer c-1 is decomposed by n-propylamine and the ω-terminus becomes a thiol group. 1 From H-NMR measurements, it was confirmed that the peak (4.8 ppm) of hydrogen bonded to the carbon adjacent to the thiocarbonylthio group observed in the pentablock copolymer c-1 disappeared in the triblock copolymer d-2, and all of it was decomposed to thiols. On the other hand, the molecular weight of the triblock copolymer d-2 was Mn 41,800, Mw 52,300, and Mw / Mn 1.25. In addition, the number of crosslinkable functional groups per molecule contained in block (A) was calculated to be 3.9 on average from the amount of trimethoxysilylpropyl methacrylate introduced per RAFT agent. Furthermore, x was 0.129, the product of (x / 100) and y was 53.9, and the E-type viscosity was 501,000 mPa s.
[0132] (Production Examples 3 to 31: Production of triblock copolymers d-3 to d-23 and d-25 to d-31, and diblock copolymer d-24) The raw materials were used as shown in Tables 8 and 9, and the operation was carried out in the same manner as in Production Example 1 except that the desolvation temperature was appropriately adjusted, to obtain triblock copolymers d-3 to d-23 and d-25 to d-31, and diblock copolymer d-24. The molecular weight of each block copolymer was measured and shown in Tables 8 and 9. In addition, the number of crosslinkable functional groups per molecule contained in block (A) was calculated from the amount of methyldimethoxysilylpropyl methacrylate introduced per RAFT agent, and shown in Tables 8 and 9. Furthermore, x, the product of (x / 100) and y, and E-type viscosity are shown in Tables 8 and 9.
[0133] In addition, the abbreviations of the amine compounds in Tables 8 and 9 mean the following compounds. PAm: n-propylamine BAm: n-butylamine HAm: n-Hexylamine
[0134] [Table 8]
[0135] [Table 9]
[0136] Synthesis of RAFT agents (Synthesis of 1,4-bis(n-dodecylsulfanylthiocarbonylsulfanylmethyl)benzene) 1-Dodecanethiol (42.2 g), 20% KOH aqueous solution (63.8 g), and trioctylmethylammonium chloride (1.5 g) were added to a round-bottom flask and cooled in an ice bath. Carbon disulfide (15.9 g) and tetrahydrofuran (hereinafter also referred to as "THF") (38 ml) were added and stirred for 20 minutes. A THF solution (170 ml) of α,α'-dichloro-p-xylene (16.6 g) was added dropwise over 30 minutes. After reacting at room temperature for 1 hour, the mixture was extracted from chloroform, washed with pure water, dried with anhydrous sodium sulfate, and concentrated with a rotary evaporator. The obtained crude product was purified by column chromatography and then recrystallized from ethyl acetate to obtain 1,4-bis(n-dodecylsulfanylthiocarbonylsulfanylmethyl)benzene (hereinafter also referred to as "DLBTTC") represented by the following formula (6) in a yield of 80%. 1 H-NMR measurement confirmed peaks of the target compound at 7.2 ppm, 4.6 ppm, and 3.4 ppm. [ka]
[0137] (Comparative Manufacturing Example 1) In a 1L flask equipped with a stirrer and a thermometer, DLBTTC (9.9 g), ABN-E (0.246 g), nBA (400 g) and acetonitrile (100 g) were charged as RAFT agents, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 60 ° C. After 4 hours, the mixture was cooled to room temperature to stop the reaction. The above polymerization solution was purified by reprecipitation from a mixed solvent of methanol / water = 70 / 30 mass ratio, and vacuum dried to obtain polymer e-1. The molecular weight of the obtained polymer e-1 was Mn 25,300, Mw 30,400, and Mw / Mn 1.20 by GPC measurement (polystyrene equivalent). Polymer e-1 (100.0 g), ABN-E (0.065 g), nBA (37.5 g), triethoxysilylpropyl methacrylate (2.5 g) and MOA (50 g) were charged into a 0.5 L flask equipped with a stirrer and a thermometer, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 70° C. After 4 hours, the mixture was cooled to room temperature to stop the reaction, and a solution containing triblock copolymer e-2 was obtained. The solution was decompressed to 20 kPa, and volatile components such as unreacted monomers and solvents were continuously distilled off using a thin-film evaporator maintained at 120° C., to recover the non-volatile component triblock copolymer e-2. The molecular weight of the obtained triblock copolymer e-2 was Mn 35,000, Mw 45,200, and Mw / Mn 1.29. Triblock copolymer e-2 has a polymer block (A) consisting of nBA and triethoxysilylpropyl methacrylate, and a polymer block (B) consisting of nBA, and has a structural unit of (A)-(B)-(A). From the polymerization rate, the composition ratio of the polymer block (A) and the acrylic polymer block (B) was (A) / (B)=28 / 72 wt%. In addition, the number of crosslinkable functional groups per molecule contained in block (A) was calculated to be 2.1 on average from the amount of triethoxysilylpropyl methacrylate introduced per RAFT agent. Furthermore, x was 0.557, and the product of (x / 100) and y was 195.
[0138] (Comparative Manufacturing Example 2) In a 1L flask equipped with a stirrer and a thermometer, 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid (37 g), ABN-E (2.8 g), nBA (371 g), methyldimethoxysilylpropyl methacrylate (67 g) and MOA (22 g) were charged as RAFT agents, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 60 ° C. After 7 hours, the mixture was cooled to room temperature and the reaction was stopped. The molecular weight of the obtained polymer e-3 was Mn 2,800, Mw 4,100, and Mw / Mn 1.50 by GPC (gel permeation chromatography) measurement (polystyrene equivalent). Polymer e-3 (41 g), nBA (361 g), ABN-E (0.39 g) and MOA (98 g) were charged into a 1 L flask equipped with a stirrer and a thermometer, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 60 ° C. After 5 hours, the mixture was cooled to room temperature to stop the reaction, and then methyldimethoxysilylpropyl methacrylate (5.5 g) and ABN-E (0.79 g) were charged, thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 60 ° C. After 7 hours, the mixture was cooled to room temperature to stop the reaction, and a solution containing triblock copolymer e-4 was obtained. The solution was decompressed to 20 kPa, and volatile components such as unreacted monomers and solvents were continuously distilled off using a thin-film evaporator maintained at 120° C., to recover the non-volatile component triblock copolymer e-4. The molecular weight of the obtained triblock copolymer e-4 was Mn 37,400, Mw 42,200, and Mw / Mn 1.13, as measured by GPC (gel permeation chromatography) (polystyrene equivalent). Triblock copolymer e-4 has a polymer block (A) consisting of nBA and methyldimethoxysilylpropyl methacrylate, and a polymer block (B) consisting of nBA, and has a structural unit of (A)-(B)-(A). From the polymerization rate, the composition ratio of the polymer block (A) and the acrylic polymer block (B) was (A) / (B)=14 / 86 wt%. In addition, the number of crosslinkable functional groups per molecule contained in block (A) was calculated to be 3.9 on average from the amount of methyldimethoxysilylpropyl methacrylate introduced per RAFT agent. Furthermore, x was 0.278, and the product of (x / 100) and y was 104.
[0139] (Comparative Manufacturing Example 3) In a 1L flask equipped with a stirrer and a thermometer, DBTTC (33 g), ABN-E (2.2 g), nBA (389 g), methyldimethoxysilylpropyl methacrylate (53 g) and MOA (23 g) were charged as RAFT agents, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 70°C. After 4 hours, the mixture was cooled to room temperature and the reaction was stopped. The molecular weight of the obtained polymer e-5 was Mn 3,900, Mw 5,300, and Mw / Mn 1.35, as measured by GPC (gel permeation chromatography) (polystyrene equivalent). Polymer e-5 (49 g), n-butyl acrylate (354 g), ABN-E (0.43 g), ethyl acetate (78 g) and MOA (19 g) were charged into a 1 L flask equipped with a stirrer and a thermometer, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 60° C. After 5 hours, the mixture was cooled to room temperature to stop the reaction, and a solution containing triblock copolymer e-6 was obtained. The solution was decompressed to 20 kPa, and volatile components such as unreacted monomers and solvents were continuously distilled off using a thin-film evaporator maintained at 120° C., to recover the non-volatile component triblock copolymer e-6. The molecular weight of the obtained triblock copolymer e-6 was Mn 33,300, Mw 37,200, and Mw / Mn 1.12, as measured by GPC (gel permeation chromatography) (polystyrene equivalent). Triblock copolymer e-6 has a polymer block (A) consisting of nBA and methyldimethoxysilylpropyl methacrylate, and a polymer block (B) consisting of nBA, and has a structural unit of (A)-(B)-(A). From the polymerization rate, the composition ratio of the polymer block (A) and the acrylic polymer block (B) was (A) / (B)=11 / 89 wt%. In addition, the number of crosslinkable functional groups per molecule contained in block (A) was calculated to be 2.0 on average from the amount of methyldimethoxysilylpropyl methacrylate introduced per RAFT agent. Furthermore, x was 0.267, and the product of (x / 100) and y was 88.8.
[0140] <Preparation and evaluation of resin composition> Example 1 Using the triblock copolymer d-1 obtained in Production Example 1 as the base resin, resin compositions (mixture A and mixture B) were prepared according to the above-mentioned recipe (Table 1), and sheets (molded products) were produced by the above-mentioned method. The measurement results of the mechanical properties of the sheets are shown in Table 10.
[0141] (Examples 2 to 23, 25 to 29, Comparative Examples 1 to 3) Using the triblock copolymers d-2 to d-23 and d-25 to d-29 obtained in Production Examples 2 to 23, 25 to 29, and the triblock copolymers e-2, e-4 and e-6 obtained in Comparative Production Examples 1 to 3, resin compositions (mixtures A and B) were prepared according to the above-mentioned recipe (Table 1), and sheets (molded products) were produced by the above-mentioned method. The measurement results of the mechanical properties of the sheets are shown in Tables 10 and 11.
[0142] (Example 24) Using the diblock copolymer d-24 obtained in Production Example 24, a resin composition (mixture B) was prepared according to the above-mentioned recipe (Table 1), and a sheet (molded product) was produced by the above-mentioned method. The measurement results of the mechanical properties of the sheet are shown in Table 11.
[0143] (Examples 30 and 31) Using the triblock copolymers d-30 and d-31 obtained in Production Examples 30 and 31, resin compositions (mixture C) were prepared according to the above-mentioned recipe (Table 1), and sheets (molded products) were produced by the above-mentioned method. The measurement results of the mechanical properties of the sheets are shown in Table 11.
[0144] [Table 10]
[0145] [Table 11]
[0146] (Examples 32 and 33, Comparative Example 4) A resin composition (mixture D) was prepared according to the above-mentioned mix table (Table 1) using the triblock copolymers d-2 and d-8 obtained in Production Examples 2 and 8, and the triblock copolymer e-6 obtained in Comparative Production Example 3, and mixed using a planetary mixer at 60°C and 10 Torr for 1 hour to obtain an adhesive composition. Table 12 shows the test results of the mechanical properties, weather resistance, and adhesive strength of the sheet of each adhesive composition, which were performed by the above-mentioned methods.
[0147] [Table 12]
[0148] <Odor Intensity and Mechanical Properties> As is clear from the results of Examples 1 to 33, the block copolymer of the present invention has a significantly reduced odor when exposed to high temperatures, and the sheets obtained from the resin compositions containing the block copolymer (blended A, blended B, blended C, and blended D) exhibited good mechanical properties (elongation at break and strength at break) and were excellent in toughness. Among these, Examples 1 to 29 (blended A and blended B) are particularly suitable for use as sealing materials, and Examples 30 and 31 (blended C) are particularly suitable for use as elastomers. In contrast, the block copolymers having a product of (x / 100) and y of more than 60 (comparative examples 1 to 4) had a severe odor when exposed to high temperatures and were difficult to use in practice.
[0149] <Weather resistance and adhesive strength> As is clear from the results of Examples 32 and 33, the sheet obtained from the resin composition (blended D) containing the block copolymer of the present invention had excellent weather resistance, and when the resin composition was used as an exterior tile adhesive, it had excellent adhesive strength. From this, it can be said that the resin composition of the present invention is particularly suitable for use as a sealant and an exterior tile adhesive. In contrast, the sheet obtained from the resin composition containing the block copolymer in which the product of (x / 100) and y is more than 60 (Comparative Example 4) was poor in weather resistance and adhesive strength. [Industrial Applicability]
[0150] The block copolymer has a significantly reduced odor when exposed to high temperatures, and can increase the toughness of molded products of resin compositions containing the block copolymer. Therefore, it can be used as a sealant, adhesive, pressure sensitive adhesive, paint, elastomer, etc., and is particularly suitable for use as a sealant and exterior tile adhesive because it has excellent weather resistance. The adhesive composition containing the resin composition of the present invention also has excellent adhesion, so it can be suitably used as an exterior tile adhesive.
Claims
1. A block copolymer consisting of at least two polymer blocks, The block copolymer has one or more polymer blocks (A) and one or more polymer blocks (B), the polymer block (A) has a constituent unit derived from at least one monomer selected from the group consisting of a (meth)acrylic acid alkyl ester compound, a compound represented by the following general formula (3), a styrene compound, a maleimide compound, and an amide group-containing vinyl compound, CH 2 =CR 1 -C(=O)O(R 2 O) n -R 3 (3) (In the formula, R 1 represents hydrogen or a methyl group, R 2 represents a linear or branched alkylene group having 2 to 6 carbon atoms; R 3 represents hydrogen, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms; and n represents an integer of 1 to 100. the polymer block (B) contains 50% by mass or more and 100% by mass or less of a structural unit derived from a (meth)acrylic acid alkyl ester compound, a content ratio of the polymer block (A) in the block copolymer is 60 parts by mass or less relative to 100 parts by mass of the total amount of the polymer block (A) and the polymer block (B), The polymer block (A) contains an average of 0.7 or more crosslinkable functional groups per molecule, a ratio of the crosslinkable constituent units in the polymer block (B) is 5 mol % or less based on all constituent units of the polymer block (B) and does not exceed a ratio of the crosslinkable constituent units to all constituent units of the polymer block (A); At least one terminal structure of the block copolymer is a structure represented by the following general formula (1) or a thiol group: The block copolymer, wherein the product of (x / 100) and y is 60 or less, is where x is a sulfur concentration (mass%) in the block copolymer and y is a number average molecular weight of the block copolymer. 【Chemistry 1】 (R represents an alkyl group having 1 to 30 carbon atoms, an aryl group, or an aralkyl group.)
2. The block copolymer according to claim 1 , wherein the block copolymer has a structural unit consisting of polymer block (A) / polymer block (B) / polymer block (A).
3. the block copolymer has a structural unit consisting of polymer block (A) / polymer block (B) / polymer block (C), The polymer block (C) has a structural unit derived from at least one monomer selected from the group consisting of a (meth)acrylic acid alkyl ester compound, a compound represented by the general formula (3), a styrene, a maleimide compound, and an amide group-containing vinyl compound (however, different from the polymer blocks (A) and (B)), The block copolymer of claim 1 .
4. A resin composition comprising the block copolymer according to any one of claims 1 to 3.
5. The resin composition according to claim 4, further comprising a polyoxyalkylene polymer having a crosslinkable functional group.
6. The resin composition according to claim 4 or 5, which is used as any one of a sealing material, an adhesive, a pressure sensitive adhesive, a coating material, and an elastomer.
7. A method for producing a block copolymer comprising at least two polymer blocks, comprising the steps of: A step of producing a block copolymer (P1) comprising at least three polymer blocks and having a trithiocarbonate group represented by the following general formula (2) in a central polymer block of the block copolymer by a reversible addition-fragmentation chain transfer living radical polymerization method; and reacting a nucleophilic agent with the trithiocarbonate group of the block copolymer (P1) to produce a block copolymer (P2) having one or more polymer blocks (A) and one or more polymer blocks (B), the polymer block (A) has a structural unit derived from at least one monomer selected from the group consisting of a (meth)acrylic acid alkyl ester compound, a compound represented by the following general formula (3), a styrene, a maleimide compound, and an amide group-containing vinyl compound, and has a crosslinkable functional group; CH 2 =CR 1 -C(=O)O(R 2 O) n -R 3 (3) (In the formula, R 1 represents hydrogen or a methyl group, R 2 represents a linear or branched alkylene group having 2 to 6 carbon atoms, R 3 represents hydrogen, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and n represents an integer of 1 to 100.) the polymer block (B) has a structural unit derived from a (meth)acrylic acid alkyl ester compound, the content ratio of the crosslinkable constituent units in the polymer block (B) is 5 mol % or less with respect to all constituent units of the polymer block (B) and does not exceed the content ratio of the crosslinkable constituent units with respect to all constituent units of the polymer block (A); A method for producing a block copolymer. 【Chemistry 2】
8. At least one polymer block of the block copolymer (P2) contains 50% by mass or more and 100% by mass or less of a structural unit derived from a (meth)acrylic acid ester compound, At least one terminal structure of the block copolymer (P2) is a structure represented by the following general formula (1) or a thiol group, where x is a sulfur concentration (mass%) in the block copolymer (P2) and y is a number average molecular weight of the block copolymer (P2), the product of (x / 100) and y is 60 or less. A method for producing the block copolymer according to claim 7. 【Chemistry 3】 (R represents an alkyl group having 1 to 30 carbon atoms, an aryl group, or an aralkyl group.)
9. the polymer block (A) contains an average of 0.7 or more crosslinkable functional groups per molecule, 9. The method for producing a block copolymer according to claim 7 or 8, wherein a content ratio of the polymer block (A) in the block copolymer is 60 parts by mass or less with respect to 100 parts by mass of a total amount of the polymer block (A) and the polymer block (B).
Citation Information
Patent Citations
Water crosslinking encapsulant
JP2011525201A
Method for removing thiocarbonylthio groups from polymers produced by RAFT polymerization.
JP2015505881A
Polymer composition
JP2019167446A
Novel chain transfer agent and emulsion polymerization using same
WO2011093401A1
Block copolymer, method for producing same, and use of same
WO2017073287A1