Ceramic composition and wire-wound coil component
A ceramic composition with controlled Fe, Cu, Zn, Ni, Mn, Nb, and V content addresses chipping, cracking, and plating elongation issues in wire-wound coil components, ensuring high resistivity and reliability.
Patent Information
- Application Number
- JP2022118829
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-26
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2042-07-26
AI Technical Summary
Existing wire-wound coil components made of ferrite materials face issues such as chipping during barrel polishing, cracking during thermocompression bonding, and plating elongation, which affect their reliability and performance.
A ceramic composition containing specific proportions of Fe, Cu, Zn, Ni, Mn, Nb, and V is used to form a ceramic core, which suppresses chipping and cracking during processing and plating elongation, while maintaining high resistivity.
The ceramic composition effectively reduces chipping and cracking during manufacturing processes and enhances plating stability, achieving a specific resistance of 1.0×10^8 Ωm or more, thereby improving the reliability of wire-wound coil components.
Smart Images

Figure 0007578121000004 
Figure 0007578121000005 
Figure 0007578121000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a ceramic composition and a wire-wound coil component. [Background technology]
[0002] Patent Document 1 discloses a winding-type coil device using a drum core having a winding core and a flange. According to the coil device described in Patent Document 1, a first mounting protrusion formed on the flange at one end of the winding core and a second mounting protrusion formed on the flange at the other end of the winding core are misaligned, and therefore the coil device is said to have excellent thermal shock resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-125397 A Summary of the Invention [Problem to be solved by the invention]
[0004] Patent Document 1 describes that the drum core is produced by molding and sintering a ferrite material, such as Ni-Zn ferrite or Mn-Zn ferrite.
[0005] However, in a core made of a ferrite material, chipping may occur during barrel polishing, and cracks may occur during thermocompression bonding of the wire and the terminal electrode. In addition, when the terminal electrode provided on the bottom surface of the core is formed by plating, a defect called "plating elongation" may occur, in which the plating layer protrudes from the target position.
[0006] The present invention has been made to solve the above problems, and aims to provide a ceramic composition that is suppressed in chipping during barrel polishing, cracking during thermocompression bonding, and plating elongation, and has high resistivity. Another aim of the present invention is to provide a wire-wound coil component that includes the ceramic composition as a ceramic core. [Means for solving the problem]
[0007] The ceramic composition of the present invention is a ceramic composition containing Fe, Cu, Zn, Ni, Mn, Nb and V, and when Fe, Cu, Zn and Ni are converted to Fe2O3, CuO, ZnO and NiO, respectively, and the total amount of Fe2O3, CuO, ZnO and NiO is taken as 100 mol%, Fe, calculated as Fe2O3, is 46.70 mol% or more and 49.70 mol% or less, and Cu, calculated as CuO, is 4.00 mol% or less. and 7.50 mol% or less, Zn calculated as ZnO is 7.00 mol% or more and 33.50 mol% or less, and Ni is the balance. Per 100 parts by weight of the total amount of Fe2O3, CuO, ZnO, and NiO, Mn calculated as Mn2O3 is 300 ppm or more and 10,000 ppm or less, Nb calculated as Nb2O5 is 2 ppm or more and 30 ppm or less, and V calculated as V2O5 is 10 ppm or more and 60 ppm or less.
[0008] The wound coil component of the present invention includes a winding core portion extending in the longitudinal direction, and a pair of flange portions provided at both ends of the winding core portion facing each other in the longitudinal direction, each of the flange portions having an inner end face facing the winding core portion in the longitudinal direction, an outer end face opposite the inner end face in the longitudinal direction, a pair of side faces facing each other in the width direction, and a top face and a bottom face facing each other in the height direction; a terminal electrode provided on at least the bottom face of the flange portion of the ceramic core; and a wire wound around the winding core portion of the ceramic core and having an end electrically connected to the terminal electrode, wherein the ceramic core is made of the ceramic composition of the present invention. Effect of the Invention
[0009] According to the present invention, it is possible to provide a ceramic composition which is suppressed in chipping during barrel polishing, cracking during thermocompression bonding, and plating elongation, and has high resistivity. Furthermore, according to the present invention, it is possible to provide a wire-wound coil component including the ceramic core of the ceramic composition. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing an example of the surface of a ceramic composition of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the polished surface of the ceramic composition of the present invention. [Diagram 3] FIG. 3 is a front view showing a schematic diagram of an example of a wire-wound coil component according to the present invention. [Figure 4] FIG. 4 is a perspective view that illustrates an example of a ceramic core that constitutes the wound coil component shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The ceramic composition and the wire-wound coil component of the present invention will be described below. However, the present invention is not limited to the following configurations, and can be appropriately modified and applied within the scope of the present invention. Note that the present invention also includes a combination of two or more of the individual preferable configurations of the present invention described below.
[0012] [Porcelain composition] The ceramic composition of the present invention contains Fe, Cu, Zn, Ni, Mn, Nb and V. The ceramic composition of the present invention contains, for example, ferrite, preferably spinel-type ferrite, as a main component.
[0013] In this specification, the ceramic composition means a sintered body, preferably a core-shaped sintered body. Therefore, the ceramic composition of the present invention is a mixture of the above atoms at the atomic level. In other words, the ceramic composition of the present invention is synonymous with the ferrite sintered body.
[0014] The ceramic composition of the present invention contains Fe, calculated as Fe2O3, at 46.70 mol% or more and at 49.70 mol% or less, Cu, calculated as CuO, at 4.00 mol% or more and at 7.50 mol% or less, Zn, calculated as ZnO, at 7.00 mol% or more and at 33.50 mol% or less, and Ni as the balance, when the total amount of Fe2O3, CuO, ZnO and NiO is taken as 100 mol%.
[0015] The ceramic composition of the present invention further contains, relative to 100 parts by weight of the total amount of Fe2O3, CuO, ZnO and NiO, Mn in an amount of 300 ppm or more and 10,000 ppm or less when calculated as Mn2O3, Nb in an amount of 2 ppm or more and 30 ppm or less when calculated as Nb2O5, and V in an amount of 10 ppm or more and 60 ppm or less when calculated as V2O5.
[0016] In the ceramic composition of the present invention, by setting the contents of Fe, Cu, Zn, Ni, Mn, Nb and V within the above ranges, chipping during barrel polishing, cracking during thermocompression bonding and plating elongation can be suppressed, and the resistivity can be increased. For example, as described in the examples below, the core chipping rate during barrel polishing is 0.15% or less, the crack occurrence rate during thermocompression bonding is 0.20% or less, the plating elongation is 70 μm or less, and the resistivity (logρ) is 1.0×10 8 It is possible to obtain a ceramic composition having a hardness of Ωm or more.
[0017] The ceramic composition of the present invention may further contain Co. In that case, the ceramic composition of the present invention preferably contains 500 ppm or more and 6000 ppm or less of CoO relative to 100 parts by weight of the total amount of Fe2O3, CuO, ZnO and NiO. When the ceramic composition of the present invention contains Co in the above range, plating elongation can be further suppressed.
[0018] The content of each element can be determined by analyzing the composition of the ceramic composition using inductively coupled plasma atomic emission / mass spectrometry (ICP-AES / MS).
[0019] The ceramic composition of the present invention may further contain other elements. Also, the ceramic composition of the present invention may further contain inevitable impurities.
[0020] In the ceramic composition of the present invention, the average grain size in the sintered state is preferably 2.2 μm or more and 9.0 μm or less. When the average grain size is within the above range, chipping during barrel polishing can be further suppressed.
[0021] FIG. 1 is a schematic diagram showing an example of the surface of a ceramic composition of the present invention.
[0022] The ceramic composition 1 shown in Fig. 1 includes a plurality of grains 2 and grain boundary layers 3 between the grains 2. A large amount of Cu component is precipitated in the grain boundary layers 3, and it is believed that the plating spreads along the grain boundary layers 3.
[0023] FIG. 2 is a schematic diagram showing an example of the polished surface of the ceramic composition of the present invention.
[0024] As will be described in the Examples below, the average grain diameter of the ceramic composition is determined as the average value of grain diameters calculated from a polished surface of the ceramic composition 1 as shown in FIG.
[0025] The grain diameter of the ceramic composition can be adjusted by the firing temperature, composition, etc. For example, the grain diameter can be increased by increasing the firing temperature. Also, the grain diameter can be increased by increasing the Cu content in the ceramic composition.
[0026] The ceramic composition of the present invention is preferably produced as follows.
[0027] First, Fe2O3, CuO, ZnO, NiO, Mn2O3, Nb2O5, V2O5, and CoO as necessary are weighed out so that the composition after firing will be the specified composition, and this blended raw material is placed in a ball mill together with pure water and PSZ (partially stabilized zirconia) balls and mixed and ground in a wet manner for a specified time (e.g., 4 hours or more and 8 hours or less). After evaporating and drying, this is calcined at a specified temperature (e.g., 700°C or more and 800°C or less) for a specified time (e.g., 2 hours or more and 5 hours or less) to produce a calcined product (calcined powder).
[0028] The calcined product (calcined powder) obtained is placed in a ball mill together with pure water, polyvinyl alcohol as a binder, a dispersant, a plasticizer, and PSZ balls, and mixed and ground in a wet manner. This mixed and ground slurry is dried and granulated in a spray dryer to produce granular powder.
[0029] A mold is prepared, and the produced granular powder is press-molded to form a green body.
[0030] Next, the molded body is fired in a firing furnace at a predetermined temperature (for example, 1000° C. or higher and 1200° C. or lower) for a predetermined time (for example, 2 hours or higher and 5 hours or lower). Through the above steps, a ceramic composition is obtained.
[0031] The ceramic composition of the present invention is used, for example, in a ceramic core of a wire-wound coil component. The use of the ceramic composition of the present invention is not particularly limited, and the ceramic composition may be used, for example, in an element such as a laminated inductor.
[0032] [Wire-wound coil components] The wound coil component of the present invention includes the ceramic composition of the present invention as a ceramic core.
[0033] Fig. 3 is a front view showing an example of a wire-wound coil component of the present invention, Fig. 4 is a perspective view showing an example of a ceramic core constituting the wire-wound coil component shown in Fig. 3.
[0034] 3 and 4 are schematic diagrams, and the dimensions and aspect ratios may differ from those of the actual product.
[0035] In the following description, terms indicating the relationship between elements (e.g., "vertical," "parallel," "orthogonal," etc.) and terms indicating the shapes of elements are not intended to be used in a strict sense, but are intended to include a range of substantial equivalence, for example, a difference of a few percent.
[0036] The wire-wound coil component 10 shown in Fig. 3 includes a ceramic core 20, a terminal electrode 50, and a wire (coil) 55. The ceramic core 20 is made of the ceramic composition of the present invention.
[0037] 3 and 4, the ceramic core 20 includes a winding core portion 30 extending in the longitudinal direction L, and a pair of flange portions 40 provided at both ends of the winding core portion 30 facing each other in the longitudinal direction L. The winding core portion 30 and the flange portions 40 are integrally formed.
[0038] In this specification, as shown in Figures 3 and 4, the direction in which a pair of flange portions 40 are aligned is defined as the longitudinal direction L, the up-down direction in Figures 3 and 4 among the directions perpendicular to the longitudinal direction L is defined as the height direction (thickness direction) T, and the direction perpendicular to both the longitudinal direction L and the height direction T is defined as the width direction W.
[0039] The winding core 30 is formed, for example, in a rectangular parallelepiped shape extending in the length direction L. The central axis of the winding core 30 extends parallel to the length direction L. The winding core 30 has a pair of main surfaces 31 and 32 facing each other in the height direction T, and a pair of side surfaces 33 and 34 facing each other in the width direction W.
[0040] In this specification, the rectangular parallelepiped shape includes a rectangular parallelepiped with chamfered corners and ridges, a rectangular parallelepiped with rounded corners and ridges, etc. In addition, the main surface and the side surfaces may be partially or entirely uneven.
[0041] A pair of flanges 40 are provided at both ends of the winding core 30 in the length direction L. Each flange 40 is formed in a thin rectangular parallelepiped shape in the length direction L. Each flange 40 is formed so as to protrude around the winding core 30 in the height direction T and width direction W. Specifically, the planar shape of each flange 40 when viewed from the length direction L is formed so as to protrude in the height direction T and width direction W relative to the winding core 30.
[0042] Each flange portion 40 has an inner end face 41 facing the winding core portion 30 in the longitudinal direction L, an outer end face 42 opposite the inner end face 41 in the longitudinal direction L, a pair of side faces 43 and 44 facing each other in the width direction W, and a top face 45 and a bottom face 46 facing each other in the height direction T. The inner end face 41 of one flange portion 40 is disposed opposite the inner end face 41 of the other flange portion 40.
[0043] The inner end surface 41 of each flange portion 40 is formed, for example, so that its entire surface extends perpendicular to the direction in which the central axis of the winding core portion 30 extends (here, the length direction L). That is, the inner end surface 41 of each flange portion 40 is formed so that its entire surface extends parallel to the height direction T. However, the inner end surface 41 of each flange portion 40 may be formed with an inclined surface.
[0044] 3, the terminal electrode 50 is provided on at least the bottom surface 46 of each flange portion 40. For example, when the wire-wound coil component 10 is mounted on a circuit board, the terminal electrode 50 is electrically connected to an electrode of the circuit board. The terminal electrode 50 is made of, for example, a Ni-based alloy such as nickel (Ni)-chromium (Cr) or Ni-copper (Cu), silver (Ag), Cu, tin (Sn), or the like.
[0045] The wire 55 is wound around the winding core 30. The wire 55 has a structure in which a core wire mainly composed of a conductive material such as Cu is covered with an insulating material such as polyurethane or polyester. Both ends of the wire 55 are electrically connected to the terminal electrodes 50, respectively.
[0046] 3, a plurality of terminal electrodes 50 may be provided on the bottom surface 46 of each flange portion 40. Also, a plurality of wires 55 may be wound around the winding core portion 30.
[0047] The wire-wound coil component of the present invention is manufactured, for example, as follows.
[0048] As explained in the above [Porcelain composition], the granular powder is pressure-molded to form a green body. Next, the green body is sintered in a sintering furnace at a predetermined temperature (e.g., 1000°C or higher and 1200°C or lower) for a predetermined time (e.g., 2 hours or higher and 5 hours or lower). The resulting sintered body is placed in a barrel and polished with an abrasive. This barrel polishing removes burrs from the sintered body and gives the outer surface of the sintered body (especially the corners and ridges) a curved roundness. Through the above steps, a ceramic core as shown in FIG. 4 is obtained.
[0049] Next, a terminal electrode is formed at least on the bottom surface of the flange of the ceramic core. For example, a conductive paste containing Ag and glass frit is applied to the bottom surface of the flange, and a baking process is performed at a predetermined temperature (e.g., 800°C or higher and 820°C or lower) to form a base metal layer, and then a Ni plating film and a Sn plating film are sequentially formed on the base metal layer by electrolytic plating to form a plating layer. Alternatively, a metal terminal may be attached to the bottom surface of the flange to use it as a terminal electrode.
[0050] Next, after winding the wire around the winding core of the ceramic core, the end of the wire is joined to a terminal electrode by a known method such as thermocompression bonding. Through the above steps, a wound coil component as shown in FIG. 3 can be manufactured.
[0051] The wound coil component of the present invention is not limited to the above-mentioned embodiment, and various applications and modifications can be made within the scope of the present invention. As another shape, for example, a top plate extending in the length direction L and connecting between the flange portions may be provided. The wire may be coated with resin. The shape of the core is not limited to a drum core, and may be an annular core.
[0052] In the wire-wound coil component of the present invention, the shape and size of the winding core of the ceramic core, the shape and size of the flange of the ceramic core, the wire thickness (wire diameter), the number of turns, the cross-sectional shape of the wire, and the number of wires are not particularly limited and can be appropriately changed according to the desired characteristics and mounting location. The positions and number of terminal electrodes can also be appropriately set according to the number of wires and the application.
[0053] The present specification discloses the following:
[0054] <1> A ceramic composition containing Fe, Cu, Zn, Ni, Mn, Nb and V, When Fe, Cu, Zn and Ni are converted to Fe2O3, CuO, ZnO and NiO, respectively, and the total amount of Fe2O3, CuO, ZnO and NiO is taken as 100 mol%, Fe, converted to Fe2O3, is 46.70 mol% or more and 49.70 mol% or less, Cu, converted to CuO, is 4.00 mol% or more and 7.50 mol% or less, Zn, converted to ZnO, is 7.00 mol% or more and 33.50 mol% or less, and Ni is the balance, A ceramic composition containing, per 100 parts by weight of the total amount of Fe2O3, CuO, ZnO and NiO, 300 ppm or more and 10,000 ppm or less of Mn, calculated as Mn2O3, 2 ppm or more and 30 ppm or less of Nb, calculated as Nb2O5, and 10 ppm or more and 60 ppm or less of V, calculated as V2O5.
[0055] <2> The average grain size in the sintered state is 2.2 μm or more and 9.0 μm or less. <1> The ceramic composition according to claim 1.
[0056] <3> Furthermore, the material contains Co in an amount of 500 ppm or more and 6000 ppm or less, calculated as CoO, per 100 parts by weight of the total amount of Fe2O3, CuO, ZnO, and NiO. <1> or <2> The ceramic composition according to claim 1.
[0057] <4> a ceramic core including a winding core portion extending in a longitudinal direction and a pair of flange portions provided at both ends of the winding core portion facing each other in the longitudinal direction, each of the flange portions having an inner end face facing the winding core portion in the longitudinal direction, an outer end face opposite the inner end face in the longitudinal direction, a pair of side faces facing each other in the width direction, and a top face and a bottom face facing each other in the height direction; a terminal electrode provided on at least the bottom surface of the flange portion of the ceramic core; a wire wound around the winding core of the ceramic core, the wire having an end electrically connected to the terminal electrode, The ceramic core is <1> ~ <3> A wire-wound coil component comprising the ceramic composition according to any one of claims 1 to 5. EXAMPLES
[0058] The ceramic composition of the present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0059] [Example 1] Fe2O3, CuO, ZnO, NiO, Mn2O3, Nb2O5 and V2O5 were weighed out so that the composition after firing would be as shown in Table 1, and this blended raw material was placed in a ball mill together with pure water and PSZ balls and wet mixed and ground for 4 hours. After evaporating and drying, the mixture was calcined at 800℃ for 2 hours to produce a calcined product.
[0060] The calcined product was mixed and ground in a ball mill together with pure water, polyvinyl alcohol as a binder, a dispersant, a plasticizer, and PSZ balls. The mixed and ground slurry was dried and granulated in a spray dryer to produce granular powder.
[0061] The granular powder thus produced is press-molded, and the dimensions after molding are as follows: - An H-shaped core sample with a length L of 3.9 mm, a width W of 2.8 mm, and a height T of 2.2 mm, or A ring-shaped sample with an outer diameter of 20 mm, an inner diameter of 12 mm, and a thickness of 1.5 mm A molded body was produced so as to satisfy the following criteria.
[0062] The produced green body was sintered for 2 hours at 1100° C. In this manner, samples 1 to 25 were produced.
[0063] The composition of the sintered body of each sample was analyzed using ICP-AES / MS to measure the content of each element. The results are shown in Table 1. Table 1 shows the content of each element converted to its oxide.
[0064] The surface resistance of the ring-shaped samples 1 to 25 was measured using a high resistance meter (Agilent Technologies, 4339A). The specific resistance (logρ) was calculated from the surface resistance and sample dimensions. The average value was calculated for each sample (n=5). The results are shown in Table 1. 8 Ωm or more is ○ (good), 1.0×10 8 The case where it was less than Ωm was judged as × (bad).
[0065] For samples 1 to 25, 20,000 core samples each were barrel polished at 80 rpm for 60 min. 8,000 samples were selected, and the core chipping rate was calculated by checking whether chipping occurred in the core samples after barrel polishing using a substrate appearance inspection device (Tokyo Wells Co., Ltd., TWA-4101). A core chipping rate of 0.15% or less during barrel polishing was judged as ○ (good), and a rate of more than 0.15% was judged as × (bad). The results are shown in Table 1.
[0066] A terminal electrode was formed on the bottom surface of each of the core samples 1 to 25. Specifically, a base metal layer was formed by applying Ag paste to the bottom surface of the core sample and performing a baking process, and then a plating layer including a Cu layer, a Ni layer, and a Sn layer was formed by plating. The plating conditions were set so that the thicknesses of the Cu layer, Ni layer, and Sn layer were 5 μm, 4 μm, and 15 μm, respectively. The dimension of the plating layer protruding from the target position was measured as the plating elongation. For each sample, n=10 pieces, and the average value was calculated. A plating elongation of 70 μm or less was judged as ○ (good), and a plating elongation of more than 70 μm was judged as × (bad). The results are shown in Table 1.
[0067] For the core samples of samples 1 to 25, the wire and the terminal electrode were bonded by thermocompression. Specifically, a heater chip heated to 450°C was used to apply a pressure of 0.8 N. The crack occurrence rate was calculated by checking whether or not cracks occurred in the core samples after thermocompression bonding using a substrate appearance inspection device (Tokyo Wells Co., Ltd., TWA-4101). The average value was calculated for each sample, with n=8000 pieces. A crack occurrence rate of 0.20% or less during thermocompression bonding was judged as ○ (good), and a rate of more than 0.20% was judged as × (bad). The results are shown in Table 1.
[0068] [Table 1]
[0069] In Table 1, samples marked with an * are comparative examples outside the scope of the present invention.
[0070] From Table 1, samples 2 to 4, 7, 8, 11, 12, 15, 16, 19, 20, 23, and 24, which contain Fe, Cu, Zn, Ni, Mn, Nb, and V within the specified ranges, have a core chipping rate of 0.15% or less during barrel polishing, a crack occurrence rate of 0.20% or less during thermocompression bonding, a plating elongation of 70 μm or less, and a resistivity (logρ) of 1.0 × 10 8 Porcelain compositions of more than Ωm have been obtained.
[0071] [Example 2] Samples 26 to 29 were prepared by changing the grain diameter by varying the firing temperature in the composition of Sample 3 in Table 1, and were evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0072] The average grain diameter in the sintered state was calculated from the grain diameter calculated by the method described below.
[0073] The H-shaped core samples 3 and 26 to 29 were polished and surface-finished using an automatic polishing machine (Struers Corporation, Tegramin-25), and the polished surface was then observed using a scanning electron microscope (SEM). From the SEM observation images of the polished surface, the grain diameter was calculated using the image analysis software WinROOF. For each sample, the average grain diameter was determined as the average value of the grain diameters of n=50 or more. The results are shown in Table 2.
[0074] [Table 2]
[0075] As can be seen from Table 2, in samples 3, 27 and 28, in which the average grain diameter in the sintered state is 2.2 μm or more and 9.0 μm or less, the core chipping rate during barrel polishing is suppressed to 0.10% or less.
[0076] [Example 3] Samples 30 to 33 were prepared by changing the Co content in the composition of Sample 3 in Table 1, and were evaluated in the same manner as in Example 1. The Co content was measured in the same manner as in Example 1. The results are shown in Table 3.
[0077] [Table 3]
[0078] From Table 3, in samples 3, 31, and 32, which contain 500 ppm or more and 6000 ppm or less of Co, calculated as CoO, the plating elongation is suppressed to 60 μm or less. This is thought to be because the Cu pushed out to the grain boundaries is reduced by Co, increasing the resistivity, suppressing the plating elongation.
[0079] Although not shown in Table 1 of Example 1 and Table 2 of Example 2, Samples 1, 2 and 4 to 29 contain Co to the same extent as Sample 3. [Explanation of symbols]
[0080] 1. Porcelain composition 2 grains 3 Grain boundary layer 10. Wire-wound coil components 20 Ceramic Core 30 Winding core 31, 32 Main surface of the core 33, 34 Side of core 40 Flange 41 Inner end surface of flange 42 Outer end surface of flange 43, 44 Side of flange 45 Top surface of flange 46 Bottom surface of flange 50 terminal electrode 55 Wire L Length direction T Height direction W Width direction
Claims
1. A ceramic composition containing Fe, Cu, Zn, Ni, Mn, Nb and V, Fe, Cu, Zn and Ni are respectively 2 O 3 , CuO, ZnO and NiO, Fe 2 O 3 When the total amount of CuO, ZnO and NiO is 100 mol%, Fe is 2 O 3 % or more and 49.70 mol % or less when calculated as Cu; 4.00 mol % or more and 7.50 mol % or less when calculated as CuO; 7.00 mol % or more and 33.50 mol % or less when calculated as ZnO; and Ni as the balance; Fe 2 O 3 Mn is added to 100 parts by weight of the total amount of CuO, ZnO and NiO. 2 O 3 300 ppm or more and 10,000 ppm or less, Nb is converted to Nb 2 O 5 Converted to 2 ppm or more and 30 ppm or less, V to V 2 O 5 A ceramic composition containing 10 ppm or more and 60 ppm or less of fluorine, calculated as
2. 2. The ceramic composition according to claim 1, wherein the average grain size in the sintered state is 2.2 μm or more and 9.0 μm or less.
3. Furthermore, Fe 2 O 3 2. The ceramic composition according to claim 1, containing 500 ppm or more and 6000 ppm or less of Co, calculated as CoO, per 100 parts by weight of the total amount of CuO, ZnO and NiO.
4. a ceramic core including a winding core portion extending in a longitudinal direction and a pair of flange portions provided at both ends of the winding core portion opposed to each other in the longitudinal direction, each of the flange portions having an inner end surface facing the winding core portion in the longitudinal direction, an outer end surface opposite the inner end surface in the longitudinal direction, a pair of side surfaces opposed to each other in a width direction, and a top surface and a bottom surface opposed to each other in a height direction; a terminal electrode provided on at least the bottom surface of the flange portion of the ceramic core; a wire wound around the winding core of the ceramic core and having an end electrically connected to the terminal electrode, A wire-wound coil component, wherein the ceramic core is made of the ceramic composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Ferrite sintered compact and manufacturing method for ferrite sintered compact
JP2004323283A
Coil device
JP2018125397A