Apparatus for the continuous deposition of silicon onto a substrate

By controlling the molar ratios of silicon-based intermediates and precursors, the method and apparatus prevent parasitic precipitation, enhance deposition rates, and reduce costs by optimizing silicon deposition on substrates, addressing the inefficiencies of existing chemical vapor deposition methods.

JP7578280B2Active Publication Date: 2024-11-06NEXWAFE GMBH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020523815
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-10-27
Filing Date
2018-10-25
Publication Date
2024-11-06
Estimated Expiration
2038-10-25

AI Technical Summary

Technical Problem

Existing chemical vapor deposition methods for silicon on substrates suffer from parasitic precipitation in gas lines, leading to reduced silicon layer thickness and increased manufacturing costs due to the use of etching gases like hydrogen chloride, which affect the supply rate and efficiency.

Method used

A method and apparatus that control the molar ratio of silicon-based intermediates and precursors, such as silicon tetrachloride and trichlorosilane, within the reaction chamber to prevent parasitic precipitation, optimize deposition rates, and recover excess gases, using a measuring device and control system to maintain optimal conditions.

Benefits of technology

This approach significantly reduces parasitic precipitation, enhances silicon deposition rates, lowers process costs, and increases the supply of silicon-coated substrates by optimizing the molar ratios and recycling excess gases, thereby improving process efficiency and reducing waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578280000003
    Figure 0007578280000003
  • Figure 0007578280000004
    Figure 0007578280000004
  • Figure 0007578280000005
    Figure 0007578280000005
Patent Text Reader

Abstract

A method for continuously depositing silicon on a substrate, comprising the steps of: (a) loading at least one substrate into a reaction chamber (2); (b) introducing a process gas and at least one gaseous silicon precursor into the reaction chamber (2); (c) forming a gaseous mixture in the reaction chamber (2) from at least one silicon-based intermediate product in coexistence with the gaseous silicon precursor and the process gas; (d) depositing silicon from the gaseous silicon precursor and / or the silicon-based intermediate product onto a substrate to form a silicon layer; and (e) discharging an excess of the gaseous mixture from the reaction chamber (2). The method further comprises a step (f) in which an excess of at least one component of the gaseous mixture is selected from the silicon precursor, the silicon-based intermediate product and / or the process gas and is returned to the reaction chamber (2), characterized in that the silicon precursor is introduced into the reaction chamber (2) in such a manner that the molar ratio of the silicon-based intermediate product to the silicon precursor in the process gas is 0.2:0.8 to 0.5:0.5, preferably 0.3:0.7 to 0.5:0.5, particularly preferably 0.5:0.5.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] By chemical vapor deposition of silicon onto a substrate, silicon layers with layer thicknesses of 1-200 μm can be produced for use in solar cells and microelectronics. Compared to conventional production methods by slicing silicon ingots by the Czochralski or zone melt processes, chemical vapor deposition prevents kerf loss. Furthermore, compared to conventionally produced silicon wafers with layer thicknesses in the range of 200-300 μm, a large amount of silicon is saved, resulting in significant cost savings.

[0002] In chemical vapor deposition, a substrate is placed in a reaction chamber and heated to 700°C to 1400°C. A silicon precursor is then passed through the reaction chamber, where it thermally decomposes, thereby depositing solid silicon on the substrate. Possible by-products of this chemical reaction and excess silicon precursor are diverted from the reaction chamber. With chemical vapor deposition, polycrystalline as well as monocrystalline silicon layers can be produced on crystalline substrates by chemical vapor deposition.

[0003] Silanes and chlorosilanes are particularly suitable as silicon precursors, although the use of silanes is disadvantageous due to their pyrophoricity in contact with oxygen in the air and their tendency to gas-phase nucleation. In the case of chlorosilanes, the silicon deposition reaction on the substrate is carried out in the presence of hydrogen as process gas and proceeds according to the simplified chemical equation:

number

[0004] In this case, it is clear that silicon tetrachloride (n=4) is thermally stable up to 1600 °C. Silicon is deposited on the substrate only by adding hydrogen. But even low molecular weight chlorosilanes in the gaseous state can be formed during cooling in the reaction chamber or after passing through the reaction chamber, such as trichlorosilane (n=3) and dichlorosilane (n=2), depending on the H2 concentration, temperature and pressure, according to the following:

number

[0005] This intermediate product is also thermally decomposed and guided to a much lower temperature of over 700° C. for the deposition of silicon, which deposits not only on the substrate surface but also in the gas supply and exhaust lines of the reaction chamber. This so-called parasitic deposition reduces the cross-sectional area of ​​these fluid lines, which must be periodically removed to maintain their full cross-sectional area.

[0006] DE 10 2005 045 582 A1 describes, for example, a method for the continuous deposition of silicon on a substrate, in which parasitic deposits in the device are removed and / or prevented from forming by periodically changing the composition of the gases fed in, while silicon is simultaneously deposited on the substrate. In this case, an etching gas, i.e. hydrogen chloride, is fed into the reaction chamber at regular intervals in order to remove the parasitic deposits. This type of method has the disadvantage that the supply of silicon-coated substrates is significantly reduced due to the presence of the etching gas, because not only the parasitic deposits but all solid silicon is converted into gaseous trichlorosilane in the presence of hydrogen chloride. This not only reduces the layer thickness of the silicon layer, but also increases the production costs due to the increased number of gases used. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] DE 102005045582 Summary of the Invention [Problem to be solved by the invention]

[0008] It is therefore an object of the present invention to disclose a method and an apparatus for the continuous deposition of silicon onto a substrate, in which parasitic deposition is prevented or at least reduced and in which the delivery rate can be increased compared to the methods known from the prior art. [Means for solving the problem]

[0009] This problem is solved according to the invention by a method with the features of claim 1 and by a device with the features of claim 12.

[0010] Advantageous embodiments of the idea according to the invention are the subject of the dependent claims. The invention relates to a method for the continuous deposition of silicon on a substrate according to the preamble of claim 1. Furthermore, the invention relates to an apparatus for the continuous deposition of silicon on a substrate according to the preamble of claim 12.

[0011] The method for the continuous deposition of silicon on a substrate according to the present invention comprises the following steps: in step (a), at least one substrate is introduced into a reaction chamber; in step (b), a process gas and at least one gaseous silicon precursor are introduced into the reaction chamber; then in step (c), a gaseous mixture is formed in the reaction chamber from at least one silicon-based intermediate product in coexistence with the gaseous silicon precursor and the process gas; in step (d), a silicon layer is formed on the substrate by deposition of silicon from the silicon precursor and / or by the silicon-based intermediate product; in step (e), a surplus of the gaseous mixture is exhausted from the reaction chamber.

[0012] In the method according to the invention, essentially, in step (f) at least one component of the gaseous mixture in excess is selected from the silicon precursor, the silicon-based intermediate product and / or the process gas and returned to the reaction chamber, the silicon precursor being introduced into the reaction chamber in such a way that the molar ratio of the silicon-based intermediate product to the silicon precursor is 0.2:0.8-0.5:0.5, preferably 0.3:0.7-0.5:0.5, particularly preferably 0.5:0.5, whereby the silicon precursor is present in the inlet gas of the reaction chamber in an amount equal to or in excess of the silicon-based intermediate product.

[0013] Within the scope of the present invention, the substrate may consist of polycrystalline or monocrystalline silicon, ceramic, glass and / or combinations or layer systems thereof, but the invention is not limited thereto, since for example polymer-containing substrates or other semiconducting materials, such as carborundum or other compound semiconductors, are conceivable.

[0014] When producing silicon layers on substrates by chemical vapor deposition of chlorosilanes, less than 100%, typically 15% to 30%, of the silicon precursor used is always transformed into solid silicon, making it possible to recover at least one component of the excess of the gaseous mixture, thus reducing process costs due to the lower consumption of the silicon precursor as well as a significant reduction in waste residues that pollute the environment.

[0015] Moreover, the present invention is based on the recognition that silicon deposition is not only dependent on temperature, but also on the molar composition of the gaseous mixture, which is composed of at least one of silicon-based intermediate product, the silicon precursor, and process gas. The applicant's test results show that silicon deposition can be prevented or completely prevented by selecting an appropriate molar ratio between the silicon-based intermediate product and the silicon precursor. The basis for this recognition is that the chemical vapor deposition of silicon and / or silicon-based intermediate product from the silicon precursor tends to proceed as an equilibrium reaction, which proceeds depending on temperature and concentration. In particular, parasitic deposition can be largely prevented when the molar ratio between the silicon-based intermediate product and the silicon precursor is 0.2:0.8-0.5:0.5. Parasitic deposition can be completely prevented when the molar ratio between the silicon-based intermediate product and the silicon precursor is 0.3:0.7-0.5:0.5. Such molar ratio may be controlled by controlled introduction of the silicon precursor and by returning selected from the silicon precursor, the silicon-based intermediate product and / or the process gas to the gas supply to the reaction chamber as at least one component in excess of the gaseous mixture.

[0016] It is generally known that the deposition rate of solid silicon on a substrate during chemical vapor deposition also depends on the composition of the gas flow introduced into the reaction chamber. Therefore, in order to optimize the deposition rate of silicon, preferably not only one but several silicon precursors can be introduced into the deposition chamber in procedure step (b). When several silicon precursors are introduced into the gas supply to the reaction chamber, the molar ratios mentioned refer to the silicon precursors. In the scope of the present invention, several chlorosilanes, in particular silicon tetrachloride and trichlorosilane, are introduced as silicon precursors in procedure step (b). In this case, the molar ratios preferably refer to the more polymeric chlorosilanes than to the silicon-based intermediate product.

[0017] Because in step (c) a gaseous mixture consisting of at least one silicon-based intermediate product, the silicon precursor and the process gas is formed in the reaction chamber, and because of silicon deposition in the following step (d), the prediction of the deduced composition of the remainder of the gaseous mixture is necessarily inaccurate. Therefore, in a first advantageous embodiment of the method, in step (f), the determination of the molar ratio of the silicon-based intermediate product to the silicon precursor is performed by a measuring device in the remainder of the gaseous mixture.

[0018] In this case, within the scope of the present invention, the measuring device is formed directly on one and / or more silicon-based intermediate products in order to determine the molar ratio or an equivalent value, in particular the concentration and / or amount and / or volumetric or mass flow rate, from which the molar ratio in the surplus of the gaseous mixture of said silicon-based intermediate products and said silicon precursor is derived. However, as an alternative, the measuring device may also be used to directly determine the molar ratio in the surplus of the gaseous mixture of said silicon-based intermediate products and said silicon precursor. Furthermore, the measuring device may be used to determine the corresponding molar ratio or concentration of one and / or more silicon-based intermediate products online. Alternatively, the measuring device may also be used only temporarily, for example at the start of the chemical vapor deposition and / or after a certain time interval, in order to determine the corresponding molar ratio or concentration of one and / or more silicon-based intermediate products. However, the present invention is not limited thereto.

[0019] In another advantageous embodiment of the invention, the molar ratio of the silicon-based intermediate product to the silicon precursor determined by the measuring device is transferred to a control device, which controls the introduction of the silicon precursor in the process gas in a molar ratio of the silicon-based intermediate product to the silicon precursor of 0.2:0.8 to 0.5:0.5, preferably 0.3:0.7 to 0.5:0.5, particularly preferably 0.5:0.5.

[0020] The transfer of the molar ratio measured by the measuring device can be performed here automatically, in particular via a data cable, or manually by a user, who reads the result of the measuring device and transmits the information to the control device. The subsequent introduction of the silicon precursor by the control device can also be performed automatically or manually by a user. In this case, within the scope of the present invention, the control device is formed as a volume flow regulator. However, the present invention is not limited thereto. Automatic adjustment is significantly advantageous in terms of process reliability and reduced operating costs.

[0021] In order to be able to carry out the chemical vapor deposition of solid silicon on a substrate as a continuous process, not only the molar ratio of the silicon-based intermediate product and the silicon precursor in the gas flow of the reaction chamber, but also the total amount of the silicon precursor and the silicon-based intermediate product plays an important role. If the total amount falls below a specific value, the deposition rate of solid silicon decreases, since silicon deposition proceeds as an equilibrium reaction. It is therefore advantageous if this total amount is kept constant during introduction into the reaction chamber, resulting in optimal conditions for solid silicon deposition. This is advantageously achieved by preferably keeping the flow into the process gas constant, while the silicon-based intermediate product and the silicon precursor are added such that first the desired molar ratio of both compounds is mutually adjusted, and then the desired total amount of both compounds is achieved. If, for example, the measuring device detects that the amount of the silicon-based intermediate product is too high, this intermediate product can also be discharged from the device, so that the maximum total amount is not exceeded in the reaction chamber.

[0022] Furthermore, in an advantageous embodiment of the method according to the invention, impurities are removed from the surplus of the gaseous mixture in step (f). To further enable recovery of one or more components of the surplus of the gaseous mixture in step (f) of the method, the method may in a preferred embodiment be provided with a recovery device in step (f), which separates at least a portion of the surplus of the gaseous mixture. Such a recovery device thereby enables not only recovery of the desired components of the surplus of the gaseous mixture, but also separation of undesired by-products of silicon deposition.

[0023] In another preferred embodiment of the method, in step (f), the silicon-based intermediate product and / or the silicon precursor and / or the process gas are returned to the reaction chamber.

[0024] In another preferred embodiment of the method, the silicon precursor is a chlorosilane, preferably silicon tetrachloride and / or trichlorosilane.

[0025] As mentioned above, the deposition rate of silicon can be optimized by preferably introducing not just one but multiple silicon precursors into the deposition chamber in procedure step (b). When multiple silicon precursors are introduced into the reaction chamber, the silicon precursors are preferably silicon tetrachloride and trichlorosilane.

[0026] Compared to other commercially available silanes, such as disilane or trisilane, chlorosilanes are significantly cheaper and less dangerous to handle, especially because they do not self-ignite in the presence of oxygen in air.Moreover, the use of chlorosilanes allows for significantly higher deposition rates and results in higher coating quality compared to the above-mentioned silanes, which significantly increases the supply of silicon-coated substrates.

[0027] It is generally known that high silicon deposition rates on substrates can be obtained in the range of 1 μm / min to 15 μm / min when trichlorosilane is used as a precursor, with silicon deposition already being obtained at temperatures above 700° C. However, the disadvantage here is that at these and higher temperatures parasitic deposition increases significantly in the gas lines of the reaction chamber. In contrast, pure silicon tetrachloride is stable up to about 1600° C. However, due to the lower ratio of silicon to chlorine, the deposition rate is significantly lower.

[0028] Applicants' testing has shown that the use of silicon tetrachloride in the presence of trichlorosilane provides optimal deposition rates while preventing parasitic deposition.

[0029] Since silicon tetrachloride is thermally stable at temperatures of 1600° C., and since silicon deposition proceeds only in the presence of oxygen at low temperatures, in another advantageous embodiment the process gas is hydrogen.

[0030] In another advantageous variant of the method according to the invention, the silicon-based intermediate product is a chlorosilane, preferably trichlorosilane.

[0031] As mentioned above, in step (b) of the procedure, a plurality of silicon precursors can be advantageously introduced into the reaction chamber, where the silicon precursors are preferably silicon tetrachloride and trichlorosilane.It is worth mentioning that in this case, trichlorosilane can be introduced into the reaction chamber as a silicon precursor on the one hand, and can also be returned to the reaction chamber as an intermediate product in step (f) of the procedure.

[0032] In order to obtain an optimal deposition of silicon on the substrate while at the same time minimizing process costs, in an advantageous embodiment of the method the total amount of silicon-based precursor and silicon-based intermediate product is present in the process gas in step (c) in a substance ratio of 1 to 10 mol %, preferably 2 to 7 mol %, particularly preferably 3 to 6 mol %.

[0033] In another advantageous embodiment of the method, the formation of a silicon layer by chemical vapor deposition of silicon on the substrate from the silicon precursor and / or the silicon-based intermediate product is carried out in the reaction chamber at a pressure between 0.8 bar and 1.2 bar.

[0034] Thus, within the scope of the present invention, the method according to the invention is carried out at approximately atmospheric pressure, which makes it possible to significantly increase the supply of silicon-coated substrates by eliminating the need to take time to evacuate the reaction chamber.

[0035] Since the rate of silicon deposition on a substrate is highly dependent on the temperature, at least the substrate is heated in the reaction chamber in another advantageous embodiment of the method according to the invention to a temperature between 700° C. and 1400° C., preferably between 1000° C. and 1300° C., particularly preferably between 1100° C. and 1200° C. This makes it possible to heat the substrate to a specific temperature, which is specifically set for the rate of silicon deposition on the substrate.

[0036] Within the scope of the present invention, not only the substrate but also the reaction chamber and / or the gas lines arranged in the reaction chamber are heated, whereby the substrate and / or the reaction chamber and / or the gas lines can be heated to different temperatures, which allows an optimal gas supply and gas return to the reaction chamber.

[0037] In another aspect of the invention, an apparatus for the continuous deposition of silicon onto a substrate, in particular for carrying out the methods according to claims 1 to 11, comprises: a reaction chamber including at least one inlet and at least one outlet for a substrate, a transport device for transporting the substrate from the inlet to the outlet through the reaction chamber, at least two gas inlets for feeding gas into the reaction chamber, at least one gas outlet for exhausting gas from the reaction chamber, at least two fluid supply pipes, preferably gas supply pipes, connected to two of the gas inlets of the reaction chamber.

[0038] The gas inlets are used to supply process gases, silicon-based intermediates and / or the silicon precursor to the reaction chamber.

[0039] It is important here that the device according to the invention comprises at least one control device and that a circulation tube is arranged between the gas outlet and the gas inlet of the reaction chamber, which circulation tube is connected to the fluid supply tube and the gas outlet of the reaction chamber, and that the device is provided with at least one measuring device for determining the molar ratio of the silicon-based intermediate product and the silicon precursor and / or a value equivalent thereto, and that the control device and the measuring device are configured in such a way that the flow through the supply tube can be controlled and adjusted by the control device based on a signal transmitted from the measuring device to the control device.

[0040] As mentioned above, within the scope of the present invention, the measuring device is formed directly on one and / or more silicon-based intermediate products in order to determine the concentration and / or the amount and / or the volumetric or mass flow rate from which the molar ratio in the surplus of the gaseous mixture of the silicon-based intermediate product and the silicon precursor is derived. However, as an alternative, the measuring device may also be used to directly determine the molar ratio in the surplus of the gaseous mixture of the silicon-based intermediate product and the silicon precursor. Moreover, the measuring device is formed for online determination of the corresponding molar ratio or concentration of one and / or more silicon-based intermediate products. Alternatively, the measuring device may also be used only temporarily, for example at the start of the chemical vapor deposition and / or after a certain time interval, in order to determine the corresponding molar ratio or concentration of one and / or more silicon-based intermediate products. However, the present invention is not limited thereto. Automatic adjustment is significantly advantageous in terms of process reliability and reduced operating costs.

[0041] Such an apparatus allows continuous transport of substrates into the reaction chamber, the substrates being transported from the inlet to the outlet of the reaction chamber using the transport device, the gas inlets of the apparatus according to the invention being used in this case to introduce the process gas, the silicon precursor and the excess recovered components of the gaseous precursor after they have been discharged from the reaction chamber.

[0042] In a first preferred embodiment of the device according to the invention, the measuring device is arranged in the circulation line.

[0043] In the scope of the present invention, the measuring device is integrated in the circulation pipe or is arranged adjacent to the circulation pipe. If the measuring device is integrated in the circulation pipe, the determination of the molar ratio of the silicon-based intermediate product and the silicon precursor is performed online. This measurement is performed continuously or at time intervals preset by the user. If the measuring device is arranged adjacent to the circulation pipe, the measurement of the molar ratio of the silicon-based intermediate product and the silicon precursor is performed by automatic feeding of a sample or by manually feeding an excess sample of the gaseous mixture into the measuring device by the user after taking a sample. However, the present invention is not limited thereto.

[0044] In a further preferred embodiment of the device according to the invention, the measuring device is formed as a spectrometer or as a mass flowmeter, for example as a Coriolis mass flowmeter or as a volumetric flowmeter.

[0045] When a silicon precursor and / or a silicon-based intermediate product that is liquid at room temperature is used, in an advantageous embodiment of the device, at least one of the fluid supply lines is equipped with an evaporation device, which transfers the silicon precursor and / or the silicon-based intermediate product into a gaseous state.

[0046] In another preferred embodiment of the device according to the invention, the circulation line comprises a recovery device, which is used for separation of the excess of the gaseous mixture discharged from the reaction chamber and for recovering the silicon precursor and / or the silicon-based intermediate product and / or the process gas.

[0047] In another advantageous embodiment of the device according to the invention, the recovery device is formed from a fractionator and / or a dry absorber or adsorber, by means of which the hydrogen chloride formed during the chemical vapour deposition of solid silicon and / or the silicon precursor in question can be separated during recovery of the surplus of the gaseous mixture.

[0048] Advantageously, the gaseous surplus components can be recovered separately, because they can be adjusted and / or used separately for this purpose. In order to recover the silicon precursor and / or the silicon-based intermediate product and / or the process gas separately after separation, for example by a fractionation device, the circulation line preferably comprises several partial pipes between the recovery device and the fluid supply line, which are used to separately return the process gas, the silicon-based intermediate product and / or the silicon precursor, wherein each partial pipe is provided with a separate measuring device for measuring the mass flow rate and / or the volume flow rate of the process gas, the silicon-based intermediate product and / or the silicon precursor.

[0049] In the scope of the present invention, the silicon-based intermediate product and / or the silicon precursor are discharged from the device after separation. For this purpose, for example, the gas scrubber and / or the fractionation device are provided with a gas outlet that is connected to a gas outlet. However, the present invention is not limited thereto, since such a gas outlet with a gas outlet can be provided in the region of the measuring device near the circulation line. However, it is advantageous to recover at least the components of the silicon-based intermediate product in order to reduce process costs. For this reason, it is also advantageous to recover the process gas, in particular hydrogen.

[0050] Further advantageous features of the invention are described below by way of example with the aid of the drawings. [Brief description of the drawings]

[0051] [Figure 1] 1 is a schematic diagram of a first embodiment of an apparatus according to the invention for the continuous deposition of silicon onto a substrate; [Diagram 2] FIG. 2 is a schematic diagram of a second embodiment of an apparatus according to the invention for the continuous deposition of silicon onto a substrate; [Diagram 3] FIG. 4 is a schematic diagram of a third embodiment of an apparatus according to the invention for the continuous deposition of silicon onto a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0052] 1 shows a first embodiment of an apparatus 1 according to the invention for the continuous deposition of silicon on a substrate, the apparatus 1 comprising a reaction chamber 2, a measuring device 3, a control device 4, a circulation pipe 5, a gas scrubber 6 and a recovery device 7.

[0053] The reaction chamber 2 comprises an inlet 8, through which the substrate to be coated can be introduced into the reaction chamber 2. Furthermore, on the side of the reaction chamber 2 facing the inlet 8, there is an outlet 9, through which the silicon-coated substrate can be removed from the reaction chamber 2. The substrate is transported into the reaction chamber 2 and removed again using a transport device 10. As shown by an arrow in FIG. 1, the substrate transport direction of the transport device 10 is from the inlet 8 to the outlet 9. The transport device 10 can be formed as a conveyor belt. Alternatively, the transport device 10 can be provided with multiple castors or formed as a rail transport.

[0054] 1, two substrates are vertically arranged and can be transferred into the reaction chamber 2 using the transfer device 10. In this case, the substrates are arranged parallel to each other, so that the sides of the substrates to be coated face each other. Furthermore, in this embodiment, the temperature of the reaction chamber 2 is 1100°C.

[0055] For the introduction of the gaseous silicon precursor and the process gas, two gas inlets 11, 12 are arranged in the reaction chamber 2 in the region of the inlet 8, via which the gaseous silicon precursor and the process gas can be introduced separately from each other into the reaction chamber. In the present embodiment, high-purity hydrogen is used as process gas. By introducing the gaseous silicon precursor and the process gas separately, the formation of parasitic deposits at the gas inlets 11, 12 can be prevented.

[0056] Furthermore, the gas inlets 11, 12 are connected to a fluid supply pipe 13, 14, respectively, through which the silicon precursor and the process gas can be fed to the gas inlets 11, 12. In this embodiment, silicon tetrachloride is used as the silicon precursor. Since silicon tetrachloride has a boiling point of 57.6° C. and is therefore liquid at room temperature, an evaporator 15 is disposed in the fluid supply pipe 13. Using the evaporator 15, the liquid silicon tetrachloride is transferred to a gaseous physical state before being introduced into the reaction chamber 2.

[0057] In order to allow the excess of the gas mixture consisting of the excess silicon precursor, the silicon-based intermediate product and the process gas to be discharged from the reaction chamber 2 after the substrate has been coated with silicon, the reaction chamber 2 is provided with a gas outlet 16 at the outlet 9. The gas outlet 16 is connected to the circulation pipe 5, which is used to return the excess of at least one component of the gaseous mixture selected from the silicon precursor, the silicon-based intermediate product and / or the process gas back into the reaction chamber 2. Furthermore, the circulation pipe 5 is connected to the fluid supply pipe 13.

[0058] In this embodiment, the gas scrubber 6, the recovery device 7 and the measurement device 3 are arranged along the circulation pipe 5, and these are connected to each other by a continuous circulation pipe 5, i.e., from the gas exhaust port 16 side to the fluid supply pipe 13 side.

[0059] The scrubber 6 is used in order to concentrate the surplus of the gaseous mixture discharged from the reaction chamber in such a way that the gaseous surplus discharged into the scrubber 6 is brought into contact with a trapping liquid, so that the available components in the surplus can be absorbed in the trapping liquid. The transferred components can be solid, liquid or gaseous substances. As a trapping liquid, for example, chlorosilanes can be used.

[0060] The surplus of the purified gaseous mixture can be sent to the recovery device 7 via the circulation line 5. In this embodiment, the recovery device 7 is configured as a fractionator. It is used to separate the silicon precursor and / or the silicon-based intermediate product from the process gas. In addition, the recovery device 7 allows separation of undesired chemical vapor deposition by-products from the circulation line 5.

[0061] The measuring device 3 is arranged in the circulation pipe 5 to determine the molar ratio of the silicon-based intermediate product and the silicon precursor. In this embodiment, the measuring device 3 is formed as an infrared spectrometer, which measures the concentrations of the silicon-based intermediate product and the silicon precursor in the gas flow of the circulation pipe 5, thereby determining the molar ratio of the silicon-based intermediate product and the silicon precursor. Alternatively, the measuring device 3 may be formed as a Coriolis mass flowmeter. However, the invention is not limited thereto.

[0062] To regulate the inflow of the silicon precursor into the reaction chamber 2, a control device 4 is arranged in the fluid supply line 13, which can be formed, for example, as a gas flow regulator. The control device 4 is additionally used to control the molar ratio of the silicon-based intermediate product and the silicon precursor in the reaction chamber 2 upon introduction. For this purpose, the control device 4 is connected to the measuring device 3.

[0063] The molar ratio of the silicon-based intermediate product and the silicon precursor in the excess of the gaseous mixture in the circulation pipe 5, as determined by the measuring device 3, is transmitted to the control device 4. In order to ensure that the desired molar ratio of the silicon-based intermediate product and the silicon precursor is contained in the process gas in the reaction chamber 2 at 0.2:0.8 to 0.5:0.5, preferably 0.3:0.7 to 0.5:0.5, and particularly preferably 0.5:0.5, the control device 4 controls the amount of silicon precursor fed into the reaction chamber via the fluid supply pipe 13 and the gas inlet 12 based on the molar ratio of the silicon-based intermediate product and the silicon precursor in the excess of the gaseous mixture in the circulation pipe 5, as determined by the measuring device 3. In this embodiment, the control device 4 and the measuring device 3 are electrically connected to each other, so that the measured value of the measuring device 3 is automatically transmitted to the control device 4. However, it is also within the scope of the present invention that the user of the device 1 reads the molar ratio detected by the measuring device 3 and manually transmits it to the control device 4.

[0064] Figure 2 shows a second embodiment of an apparatus 1 according to the invention for the continuous deposition of silicon on a substrate, which is broadly identical to the embodiment described in Figure 1 and will not be described in further detail.

[0065] The control device 4 is arranged in the fluid supply pipes 13, 14 to regulate the inflow of the silicon precursor and the process gas into the reaction chamber 2. The control device 4 is used on the one hand to regulate the molar ratio of the silicon-based intermediate product and the silicon precursor in the reaction chamber 2 during introduction, and on the other hand to regulate the total amount of the silicon precursor and the silicon-based intermediate product in the process gas in step (c) to a substance ratio of 1 to 10 mol %, preferably 2 to 7 mol %, particularly preferably 3 to 6 mol %. In this embodiment too, the control device 4 is connected to the measuring device 3.

[0066] Furthermore, within the scope of the present invention, the excess process gas and / or the silicon-based intermediate product and / or the silicon precursor are discharged from the device. In this embodiment, the gas scrubber is provided for this purpose with a gas outlet 17 with an outlet 18, via which the excess process gas is discharged. However, the present invention is not limited thereto. Furthermore, the fractionation device may also be provided with a gas outlet with an outlet.

[0067] Figure 3 shows a third embodiment of an apparatus 1 according to the invention for the continuous deposition of silicon on a substrate, which is also broadly identical to the embodiment described in Figure 1 and will not be described in further detail.

[0068] The circulation line 5 is divided into three separate partial lines 51, 52, 53 downstream of the recovery device 7, respectively for the process gas, the silicon-based intermediate product and the silicon precursor. In the scope of the present invention, more than three separate partial lines are connected downstream of the recovery device, in particular for separately recovering other gases, for example hydrogen chloride. The respective mass or volumetric flow rates are determined by separate measuring devices 31, 32, 33, respectively arranged in the partial lines 51, 52, 53 downstream of the recovery device 7. From this, the molar ratio of the silicon-based intermediate product and the silicon precursor is derived. As can be seen from FIG. 3, the recovered process gas is then fed into the fluid feed line 14, and the silicon-based intermediate product and the silicon precursor into the fluid feed line 13.

Claims

1. An apparatus (1) for the continuous deposition of silicon onto a substrate, comprising: - a reaction chamber (2), said reaction chamber (2) comprising at least one inlet (8) and at least one outlet (9) for the substrate; - a transport device (10) for transporting the substrate from the inlet (8) to the outlet (9) through the reaction chamber (2); - at least two gas inlets (11, 12) for feeding gases into said reaction chamber (2); - at least one gas outlet (16) for discharging gas from said reaction chamber (2); - an apparatus comprising at least two fluid supply pipes (13, 14), preferably gas supply pipes, connected to the two gas inlets (11, 12) of the reaction chamber (2), The apparatus (1) has at least one control device (4), and at least one circulation pipe (5) is arranged between the gas exhaust port (16) of the reaction chamber (2) and the gas inlet (12), and the circulation pipe (5) is connected to the fluid supply pipe (13) and the gas exhaust port (16) of the reaction chamber (2); The device (1) comprises at least one measuring device (3) for determining the molar ratio of the silicon-based intermediate product to the silicon precursor and / or a value equivalent thereto, and wherein the control device (4) and the measuring device (3) are configured in such a way that the flow through the supply lines (13, 14) can be controlled and adjusted by the control device (4) on the basis of a signal transmitted from the measuring device (3) to the control device (4).

2. 2. Apparatus according to claim 1, characterized in that the measuring device (3) is arranged in the circulation line (5).

3. 3. The device according to claim 1 or 2, characterized in that the measuring device (3) is designed as a spectrometer, as a mass flowmeter or as a volume flowmeter.

4. At least one of the fluid supply pipes (13, 14) has an evaporation device (15); 4. Apparatus according to claim 1, characterized in that the evaporation device is used for transferring the silicon precursor and / or the silicon-based intermediate product into the gaseous state.

5. The circulation pipe (5) has a gas scrubber (6) and / or a recovery device (7), 5. An apparatus according to claim 1, wherein the recovery device (7) is preferably configured as a fractionation device and / or has a dry absorber or dry adsorber.

6. The circulation pipe (5) has a plurality of partial pipes (51, 52, 53) between the recovery device (7) and the fluid supply pipe (13, 14), The partial tubes (51, 52, 53) are used for separately refluxing process gas, the silicon-based intermediate product and / or the silicon precursor, 6. The apparatus according to claim 5, characterized in that each partial pipe (51, 52, 53) is equipped with a separate measuring device (31, 32, 33) for determining the mass flow rate and / or the volume flow rate of the process gas, the silicon-based intermediate product and / or the silicon precursor.

7. A method for the continuous deposition of silicon onto a substrate, comprising the steps of: (a) at least one substrate is loaded into a reaction chamber (2); (b) introducing a process gas and at least one gaseous silicon precursor into the reaction chamber (2); (c) forming a gaseous mixture in the reaction chamber (2) with the gaseous silicon precursor, the process gas, and at least one silicon-based intermediate product that is a reaction product of the silicon precursor; (d) depositing silicon from the gaseous silicon precursor and / or silicon-based intermediate onto the substrate to form a silicon layer; (e) the excess of the gaseous mixture is discharged from the reaction chamber (2); The method further comprises a step (f) in which at least one excess component of the gaseous mixture, selected from the silicon precursor, the silicon-based intermediate product and / or the process gas, is returned to the reaction chamber (2); In this case, in the method, The silicon precursor is introduced into the reaction chamber (2) in such a manner that the molar ratio of the silicon-based intermediate product to the silicon precursor is 0.2:0.8 to 0.5:0.5, preferably 0.3:0.7 to 0.5:0.5, particularly preferably 0.5:0.5, in the process gas; adjusting a corresponding molar ratio of the silicon-based intermediate product to the silicon precursor in the gas stream entering the reaction chamber; the silicon precursor is a chlorosilane; 7. Apparatus according to claim 1 for carrying out a method, characterized in that the silicon-based intermediate product is a chlorosilane.

Citation Information

Patent Citations

  • apparatus and method for continuous chemical vapor deposition under atmospheric pressure and their use

    DE102005045582B3

  • Formation of amorphous silicon film

    JP1984064516A

  • Method for analyzing hydrogen chloride gas in producing polycrystalline silicon

    JP1995277720A

  • Manufacturing method and manufacturing system of silicon substrate for solar cell

    JP2004071970A

  • Method for producing polycrystalline silicon

    JP2009062209A