Coil parts
The coil component's laminated electrode structure with varying resin content in terminal electrodes addresses the issues of acid and impact resistance, ensuring reliable connection and adhesion, even under stress, by using a low-resistance first layer and a protective high-resin second layer.
Patent Information
- Application Number
- JP2020185212
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-05
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-11-05
AI Technical Summary
Conventional coil components with terminal electrodes formed using low-temperature conductive paste suffer from poor resistance to acid and impact, leading to insufficient connection reliability.
A coil component design featuring a core portion with magnetic particles and resin, where terminal electrodes consist of a first electrode layer with low resin content and low resistance, and a second electrode layer with higher resin content, laminated to improve adhesion and protect the first layer, enhancing acid and impact resistance.
The laminated electrode structure ensures improved connection reliability by reducing contact resistance, preventing resin deterioration, and maintaining adhesion strength even under external stress or impact, allowing for thicker terminal electrodes without peeling.
Smart Images

Figure 0007578464000001 
Figure 0007578464000002 
Figure 0007578464000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coil component having terminal electrodes. [Background technology]
[0002] A coil component, which has terminal electrodes (sometimes called external electrodes) formed on the outer surface of the element body (core), is known as a type of electronic component. In the manufacturing process of this coil component, it is required to form the terminal electrodes at low temperatures in order to reduce the thermal impact on the element body.
[0003] In response to such demands, Patent Document 1 discloses a technique for forming terminal electrodes using a conductive paste containing metal particles. The conductive paste of Patent Document 1 can be sintered at a low temperature of 250°C or less, and terminal electrodes can be formed without degrading the organic components contained in the element body. However, the terminal electrodes formed by the above technique have poor resistance to acids and impacts, and connection reliability is not necessarily sufficient. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-211333 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a coil component having terminal electrodes with high connection reliability. [Means for solving the problem]
[0006] In order to achieve the above object, a coil component according to the present invention comprises: a core portion including magnetic particles and a resin component; A coil portion formed by winding a conductor; a terminal electrode formed on a part of an outer surface of the core portion and electrically connected to an end of the conductor drawn out from the coil portion, The terminal electrode is a first electrode layer in contact with an end of the conductor; A second electrode layer disposed on the outside of the first electrode layer, The first electrode layer and the second electrode layer each contain a conductive powder and a resin, The second electrode layer has a higher resin content than the first electrode layer.
[0007] In the coil component of the present invention, a plurality of resin electrodes having different amounts of resin are laminated on a part of the outer surface of the core portion, which is the main body of the element. More specifically, a first electrode layer having a small amount of resin and a low resistance value is present on the side in contact with the end of the conductor drawn out from the coil portion, and a second electrode layer having a large amount of resin is laminated on the outside of the first electrode layer. By having the terminal electrode have the above structure, the adhesive strength of the terminal electrode to the core portion is improved, and the connection reliability of the terminal electrode is improved. In particular, since the second electrode layer having a large amount of resin is laminated so as to protect the first electrode layer having a low resistance value, the acid resistance and impact resistance of the terminal electrode are improved, which contributes to improving the connection reliability.
[0008] Preferably, the conductive powder of the first electrode layer includes metal nanoparticles having a particle size of at least 100 nm or less and metal microparticles having a particle size larger than that of the metal nanoparticles. By having the above characteristics, the resistance value of the first electrode layer is lowered and the electrical characteristics of the terminal electrode are further improved.
[0009] Preferably, the second electrode layer has an average thickness greater than the average thickness of the first electrode layer.With the above-mentioned characteristics, the impact resistance of the terminal electrode is further improved, and the connection reliability is further improved.
[0010] Preferably, the second electrode layer is formed by laminating a plurality of resin electrode layers. With the above-mentioned characteristics, the impact resistance of the terminal electrode is further improved.
[0011] In the present invention, the first electrode layer may be completely covered by the second electrode layer. In this case, the acid resistance and impact resistance of the terminal electrode are improved. However, the laminated structure of the first electrode layer and the second electrode layer is not limited to the above-mentioned form, and may have the following characteristics.
[0012] That is, an end of the terminal electrode may have a non-overlapping portion in which a part of the first electrode layer is not covered by the second electrode layer. By having a non-overlapping portion only in a part of the terminal electrode, it is possible to lower the resistance value of the terminal electrode while ensuring acid resistance and impact resistance.
[0013] In addition, a part of the first electrode layer may be extended toward the outer surface side of the second electrode layer, which can reduce the resistance of the terminal electrode while ensuring acid resistance and impact resistance.
[0014] The present invention is applicable to coil components such as inductors, transformers, choke coils, and common mode filters, and is particularly suitable for coil components that include an insulating coating on the inside of an element body or that contain resin. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a perspective view of a coil component according to an embodiment of the present invention, as viewed from the bottom side. [Diagram 2] FIG. 2 is a cross-sectional view taken along the line II-II shown in FIG. [Figure 3A] FIG. 3A is an enlarged cross-sectional view of a main part of a region III shown in FIG. [Figure 3B] FIG. 3B is a cross-sectional view of a main portion showing a modification of the terminal electrode shown in FIG. 3A. [Figure 4] FIG. 4 is a cross-sectional view showing a mounted state of the coil component shown in FIG. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing a modification of the coil device shown in FIG. [Figure 6]FIG. 6 is a schematic cross-sectional view showing a modification of the coil device shown in FIG. [Figure 7] FIG. 7 is a schematic cross-sectional view showing a modification of the coil device shown in FIG. [Figure 8] FIG. 8 is a perspective view of a preform used in the manufacturing process of the coil component. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, the present invention will be described in detail based on the embodiments shown in the drawings.
[0017] First embodiment As shown in FIG. 1, an inductor 2 serving as a coil component according to a first embodiment of the present invention has an element body 4 having a substantially rectangular parallelepiped shape (substantially hexahedral).
[0018] The element body 4 has a pair of end faces 4a substantially perpendicular to the X-axis, a bottom face 4b substantially perpendicular to the Z-axis, a top face 4c located on the opposite side of the bottom face 4b in the Z-axis direction, and a pair of side faces 4d substantially perpendicular to the Y-axis. The dimensions of the element body 4 are not particularly limited. For example, the dimension of the element body 4 in the X-axis direction can be 1.2 to 6.5 mm, the dimension in the Y-axis direction can be 0.6 to 6.5 mm, and the dimension in the height (Z-axis) direction can be 0.5 to 5.0 mm. In this embodiment, the X-axis, Y-axis, and Z-axis are mutually perpendicular.
[0019] In this embodiment, the element body 4 is made of a dust core (core portion) containing magnetic particles and a resin component.
[0020] The magnetic particles may be made of ferrite such as Mn-Zn ferrite or Ni-Zn ferrite, but are preferably metal magnetic particles, and more preferably soft magnetic metal magnetic particles. Examples of soft magnetic metal magnetic particles include Fe-Ni alloys, Fe-Si alloys, Fe-Co alloys, Fe-Si-Cr alloys, Fe-Si-Al alloys, Fe-containing amorphous alloys, and Fe-containing nanocrystalline alloys. In addition, the magnetic particles may contain additional components as appropriate.
[0021] In addition, when the magnetic particles are metal magnetic particles as described above, it is preferable that the particles are insulated from each other. For example, an insulating method can be a method of forming an insulating coating on the particle surface. Examples of the insulating coating include a coating formed of a resin or an inorganic material, and an oxide coating formed by oxidizing the particle surface by heat treatment. When the insulating coating is formed of a resin or an inorganic material, examples of the resin include silicone resin and epoxy resin, and examples of the inorganic material include phosphates such as magnesium phosphate, calcium phosphate, zinc phosphate, and manganese phosphate, silicates (water glass) such as sodium silicate, soda-lime glass, borosilicate glass, lead glass, aluminosilicate glass, borate glass, and sulfate glass. The thickness of the insulating coating is not particularly limited, but is preferably, for example, 5 nm to 20 nm. By forming the insulating coating, the insulation between the particles can be improved, and the withstand voltage of the inductor 2 can be improved.
[0022] The particle size of the magnetic particles contained in the element body 4 is not particularly limited, but for example, the median diameter (D50) can be within the range of 1 μm to 50 μm. The magnetic particles may be composed of a mixture of a plurality of particle groups with different particle sizes. For example, the magnetic particles contained in the element body 4 may be composed of a mixture of large particles with a D50 of 20 μm to 30 μm, medium particles with a D50 of 1 μm to 5 μm, and small particles with a D50 of 0.3 μm to 0.9 μm. Alternatively, in addition to the combination of the above three types of particle groups, combinations of large particles and medium particles, combinations of large particles and small particles, and combinations of medium particles and small particles may also be used.
[0023] In this way, by forming the magnetic particles into a plurality of particle groups, the packing rate of the magnetic particles contained in the element body 4 can be increased. As a result, various characteristics of the inductor 2, such as magnetic permeability, eddy current loss, and DC superposition characteristics, can be improved. In the above case, the large particles, medium particles, and small particles can all be formed of the same type of material, or they can be formed of different materials. The particle size of the magnetic particles can be measured by observing the cross section of the element body 4 with a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM), and performing image analysis of the obtained cross-sectional photograph using software. In this case, it is preferable to measure the particle size of the magnetic particles in terms of the circle equivalent diameter.
[0024] The magnetic particles having the above characteristics are dispersed in a resin component inside the element body 4. The resin component contained in the element body 4 is not particularly limited, and may be, for example, a thermosetting resin such as epoxy resin, phenol resin, melamine resin, urea resin, furan resin, alkyd resin, polyester resin, or diallyl phthalate resin, or a thermoplastic resin such as acrylic resin, polyphenylene sulfide (PPS), polypropylene (PP), or liquid crystal polymer (LCP). The above resin component may contain additives such as subcomponents as appropriate.
[0025] As shown in Fig. 2, a coil portion 6α is embedded inside the element body 4. This coil portion 6α is formed by winding a conductor wire 6 into a coil shape. In this embodiment, the coil portion 6α is an air-core coil wound in a typical normal-wise manner, but the winding method of the wire 6 is not limited to this. For example, the coil portion 6α may be an air-core coil wound by α-winding the wire 6, or an air-core coil wound edgewise.
[0026] The wire 6 constituting the coil portion 6α is composed of a core portion 6a mainly containing copper and an insulating layer 6b covering the outer periphery of the core portion. More specifically, the core portion 6a is composed of pure copper such as oxygen-free copper or tough pitch copper, an alloy containing copper such as phosphor bronze, brass, red brass, beryllium copper, or a silver-copper alloy, or a copper-coated steel wire. On the other hand, the insulating layer 6b is not particularly limited as long as it has electrical insulation properties. Examples of the insulating layer 6b include epoxy resin, acrylic resin, polyurethane, polyimide, polyamide-imide, polyester, nylon, polyester, and the like, or a synthetic resin in which at least two of the above resins are mixed. In this embodiment, the wire 6 is a round wire as shown in FIG. 2, and the cross-sectional shape of the conductor portion is circular.
[0027] A pair of lead-out electrode portions 61 are present on the bottom surface 4b of the element body 4. The lead-out electrode portions 61 extend along the Y-axis, and are formed by exposing the end of the wire 6 led out from the coil portion 6α to the outside of the bottom surface 4b. More specifically, in the lead-out electrode portion 61, the insulating layer 6b of the wire 6 led out to the bottom surface 4b is peeled off, and the core portion 6a of the wire 6 is exposed to the outside of the bottom surface 4b. In the inductor 2 of this embodiment, a pair of terminal electrodes 8 are formed on the outer surface of the element body 4 so as to cover the lead-out electrode portions 61, and the lead-out electrode portions 61 and the terminal electrodes 8 are electrically connected to each other.
[0028] 1 and 2, each of the pair of terminal electrodes 8 has an end surface electrode portion 8a, a bottom surface electrode portion 8b, and a wraparound portion 8c, and these portions are integrally connected to each other. The pair of terminal electrodes 8 are separated from each other in the X-axis direction and are insulated from each other.
[0029] The end electrode portion 8a covers one of the end faces 4c, and is connected to the bottom electrode portion 8b at the lower end in the Z-axis direction. The bottom electrode portion 8b is formed on a part of the bottom face 4b so as to completely cover one of the lead-out electrode portions 61, and is electrically connected to one of the lead-out electrode portions 61. The wraparound portion 8c exists on a part of the top face 4c and a part of the side face 4d, and is formed by the conductive paste used to form the end electrode portion 8a wrapping around a part of the top face 4c and a part of the side face 4d from the end face 4a side. The wraparound portion 8c is not essential, and depending on the method of forming the terminal electrode 8, the wraparound portion 8c may not be formed.
[0030] As described above, in the inductor 2 of this embodiment, organic components such as the insulating layer 6b of the wire 6 and the resin components constituting the powder magnetic core are contained inside the element body 4. In such an inductor 2, when a heat treatment at high temperature (500° C. or higher) is performed to form the terminal electrode 8, the organic components contained in the element body 4 are deteriorated (decomposed and burned away). For this reason, it is difficult to adopt a sintered electrode containing an inorganic binder such as glass frit as the terminal electrode 8. Therefore, in this embodiment, the terminal electrode 8 is composed of a plurality of resin electrodes (first electrode layer 81, second electrode layer 82) and an outermost layer 83.
[0031] More specifically, in the bottom electrode portion 8b of the terminal electrode 8, a first electrode layer 81 is formed as a base electrode in contact with the bottom surface 4b, and this first electrode layer 81 completely covers the lead-out electrode portion 61 and is directly connected to the lead-out electrode portion 61. In the bottom electrode portion 8b, a second electrode layer 82 is laminated on the first electrode layer 81 so as to be in contact with the outer surface of the first electrode layer 81. This second electrode layer 82 is a resin electrode having a higher resin content than the first electrode layer 81, and may be configured as a single layer as shown in FIG. 3A, or may be configured as multiple layers as shown in FIG. 3B.
[0032] On the other hand, the first electrode layer 81 does not exist in the end surface electrode portion 8a and the wraparound portion 8c of the terminal electrode 8, and the second electrode layer 82 is formed so as to be in direct contact with the outer surface of the element body 4. The second electrode layer 82 of the end surface electrode portion 8a and the wraparound portion 8c may also be a single layer or multiple layers. The outermost layer 83 is located on the outermost surface side of the terminal electrode 8, and covers the second electrode layer 82 at each portion (the end surface electrode portion 8a, the bottom surface electrode portion 8b, and the wraparound portion 8c). In this embodiment, the second electrode layer 82 completely covers the first electrode layer 81, and the first electrode layer 81 is not exposed on the outer surface of the second electrode layer 82.
[0033] Next, the features of each electrode layer constituting terminal electrode 8 will be described with reference to FIG. 3A.
[0034] First, the first electrode layer 81 is a resin electrode containing a conductive powder 11 and a resin 13, and the first electrode layer 81 may contain voids, inorganic materials, etc. in addition to the above. The resin 13 of the first electrode layer 81 is made of a thermosetting resin such as an epoxy resin or a phenolic resin. On the other hand, the conductive powder 11 of the first electrode layer 81 may be made of a metal powder such as Ag, Au, Pd, Pt, Ni, Cu, Sn, etc., or a metal powder of an alloy containing at least one of the above elements, and it is particularly preferable that the conductive powder contains Ag as the main component.
[0035] Furthermore, in this embodiment, the conductor powder 11 of the first electrode layer 81 is preferably composed of two types of particle groups (first particles 11a, second particles 11b) having different particle size distributions.
[0036] The first particles 11a are a group of particles having a particle size on the order of micrometers. Here, "particles on the order of micrometers" refers to particles having a particle size of more than 0.1 μm and not more than several tens of μm. In the cross section shown in FIG. 3, the first particles 11a of this embodiment preferably have an average particle size of 1 μm to 10 μm, and more preferably 3 μm to 5 μm.
[0037] The shape of the first particles 11a may be a nearly spherical shape, an elongated spheroid, an irregular block shape, a needle shape, or a flat shape, and is particularly preferably a needle shape or a flat shape. More specifically, in a cross section as shown in FIG. 3, the aspect ratio of the first particles 11a (ratio of the length in the longitudinal direction to the width in the lateral direction) is preferably within a range of 2 to 30. The particle size distribution and aspect ratio of the first particles 11a can be measured by observing the cross section of the first electrode layer 81 with a SEM or STEM and performing image analysis on the obtained cross section photograph. In this measurement, the average particle size of the first particles 11a is calculated in terms of the maximum length.
[0038] On the other hand, the second particles 11b are a group of particles on the order of nanometers with an average particle size smaller than that of the first particles 11a. The second particles 11b are present in an aggregated state near the outer periphery of the first particles 11a or in the gaps between the first particles 11a. When the aggregated portion of the second particles 11b is observed under magnification by STEM, the second particles 11b can be recognized as an aggregate of fine particles with a particle size of at least 100 nm or less.
[0039] As described above, it is preferable that the first particles 11a and the second particles 11b are both Ag particles in the first electrode layer 81. However, this is not limited to the above, and the metal elements constituting the main components of the first particles 11a and the second particles 11b may be different.
[0040] In the first electrode layer 81 having the above-mentioned structure, the nanometer-order second particles 11b fill the gaps between the first particles 11a and also fill the bonding interface between the lead electrode portion 61 and the first electrode layer 81. As a result, electrical connection is improved in the gaps between the particles and at the bonding interface, and the contact resistance of the terminal electrode 8 with respect to the lead electrode portion 61 can be reduced.
[0041] On the other hand, the second electrode layer 82 is a resin electrode containing conductor powder 21 and resin 23, and the second electrode layer 82 may contain voids, inorganic materials, etc., in addition to the above. The resin 23 of the second electrode layer 82 may be made of a thermosetting resin such as an epoxy resin or a phenolic resin, similar to the first electrode layer 81. The conductor powder 21 of the second electrode layer 82 may be made of a metal powder such as Ag, Au, Pd, Pt, Ni, Cu, Sn, etc., or a metal powder of an alloy containing at least one of the above elements, similar to the first electrode layer 81, and it is particularly preferable that the conductor powder contains Ag as the main component.
[0042] However, the conductor powder 21 of the second electrode layer 82 is preferably composed of only metal particles of the micrometer order, without including fine particles of the nanometer order. Specifically, the conductor powder 21 of the second electrode layer 82 preferably has an average particle size of 1 μm to 10 μm, more preferably 3 μm to 5 μm, in a cross section as shown in FIG. 3. The particle shape of the conductor powder 21 may be a shape close to a sphere, an elongated sphere, an irregular block shape, a needle shape, or a flat shape, and is particularly preferably a needle shape or a flat shape. Furthermore, the aspect ratio of each particle constituting the conductor powder 21 is preferably within a range of 2 to 30. The material, particle size, and particle shape of the conductor powder 21 in the second electrode layer 82 may be the same as or different from the first particles 11a of the first electrode layer 81.
[0043] 3B, the second electrode layer 82 may be formed by laminating a plurality of outer resin electrode layers 20. In this case, the number of layers of the outer resin electrode layers 20 is not particularly limited, but is preferably, for example, 2 to 3 layers, and it can be confirmed that there is a boundary line 25 between each outer resin electrode layer 20 due to the overlapping application of the raw material paste. This boundary line 25 can be observed continuously or intermittently in some cases.
[0044] Furthermore, when the second electrode layer 82 is composed of a plurality of layers, each of the plurality of outer resin electrode layers 20 may have a different resin content as long as it has a higher resin content than the first electrode layer 81. Furthermore, the material of the conductor powder 21 and the material of the resin 23 may be different in each outer resin electrode layer 20. However, in consideration of manufacturing efficiency, it is preferable that each outer resin electrode layer 20 is manufactured using the same raw material paste, and that the resin content, the material and shape of the conductor powder 21, and the material of the resin 23 are the same.
[0045] As described above, in this embodiment, a plurality of resin electrodes are laminated on the bottom electrode portion 8b, and the content ratio of the resin (13, 23) is different between the first electrode layer 81 and the second electrode layer 82. Specifically, the content ratio R2 of the resin 23 in the second electrode layer 82 is higher than the content ratio R1 of the resin 13 in the first electrode layer 81, and R2 / R1 is preferably 2.0 to 10.0, and more preferably 3.0 to 5.0.
[0046] The resin content (R1, R2) in each electrode layer can be expressed as the proportion of the area occupied by non-metallic components in the cross section of each electrode layer. Specifically, when observing the cross section of each electrode layer (81, 82) using a backscattered electron image from an SEM or a HAADF image from an STEM, the conductor powder (11, 21) made up of metallic components can be recognized as bright contrast areas, while the resin (13, 23) and non-metallic components including voids can be recognized as dark contrast areas. Therefore, the area proportion A occupied by the conductor powder in the cross section can be expressed as M and the area ratio A occupied by nonmetallic components R can be calculated by binarizing cross-sectional photographs taken with an SEM or STEM and performing image analysis.
[0047] Area ratio A occupied by non-metallic components Rmay include the area of the resin (13, 23) as well as the area of the voids. It is extremely difficult to clearly distinguish between the resin and the voids in a cross-sectional photograph, and it is not easy to accurately calculate only the area occupied by the resin (13, 23). However, the resin content (R1, R2) and the area ratio A of the non-metallic components R There is a clear positive correlation between the resin content (R1, R2) and the area ratio A occupied by non-metallic components. R Therefore, the area ratio of the nonmetallic components in the cross section of the first electrode layer 81 can be expressed as A R 1, and the area ratio of the nonmetallic components in the cross section of the second electrode layer 82 is A R 2, in this embodiment, the ratio of R2 to R1 (R2 / R1) is A R A to 1 R The ratio of 2 (A R 2 / A R This will be expressed as 1).
[0048] In this embodiment, A R 2 / A R 1 (i.e., R2 / R1) is preferably 2.0 to 10.0, and more preferably 3.0 to 5.0. R 1 is preferably 5.0% to 18.0%, and more preferably 9.0% to 13.0%. Thus, the first electrode layer 81 has a lower resin content than the second electrode layer 82, and has a lower resistance value than the second electrode layer 82. On the other hand, the second electrode layer 82 has a higher resin content than the first electrode layer 81, and therefore can absorb external stress and impact. In addition, the second electrode layer 82 has a higher resin content than the first electrode layer 81, and therefore the conductor powder 21 is less likely to flow out into the solution when exposed to an etching solution or a plating solution. In other words, the second electrode layer 82 has better resistance to acid than the first electrode layer 81.
[0049] In addition, the area ratio of the first particles 11a in the cross section of the first electrode layer 81 is A M 1a, the area ratio occupied by the second particle 11b is A M If we assume 1b, then A M A for 1bM The ratio of 1a (A M 1a / A M 1b) is preferably from 1.5 to 6.0, more preferably from 2.0 to 4.0. In the first electrode layer 81, when the content ratios of the first particles 11a and the second particles 11b satisfy the above conditions, the resistance value of the first electrode layer 81 is further reduced, and the adhesion strength of the first electrode layer 81 to the element body 4 tends to improve.
[0050] Note that the above-mentioned area ratio A M , A R are all calculated based on the cross-sectional area of each electrode layer, that is, the area of the observation field of view, and A M + A R = 100% holds (in the case of the first electrode layer 81, A M 1a + A M 1b + A R 1 = 100%, and in the case of the second electrode layer 82, A M 2 + A R 2 = 100%). Also, each area ratio A M , A R is preferably calculated as the average value by performing the above-mentioned image analysis in at least 10 fields of view or more. At this time, the observation field of view per field of view is preferably from 0.04 μm 2 to 0.36 μm 2 .
[0051] Also, in the present embodiment, the first electrode layer 81 and the second electrode layer 82 are preferably formed with predetermined thicknesses. Specifically, the average thickness T1 of the first electrode layer 81 can be from 5 μm to 30 μm, preferably from 10 μm to 20 μm. And when the second electrode layer 82 is composed of a single layer as shown in FIG. 3A, the average thickness T2 of the second electrode layer 82 is preferably thicker than the average thickness T1 of the first electrode layer 81 (that is, 1.0 < T2 / T1), more preferably T2 / T1 is from 1.5 to 2.5, and even more preferably from 1.8 to 2.2. And the maximum thickness T of the bottom electrode portion 8b having the first electrode layer 81 and the second electrode layer 82 BThe thickness is preferably 25 μm to 70 μm, and more preferably 50 μm to 70 μm.
[0052] On the other hand, when the second electrode layer 82 is composed of a plurality of layers as shown in FIG. 3B, the thickness of each of the outer resin electrode layers 20 is not particularly limited. However, the average thickness T α 2 is preferably thicker than the average thickness T1 of the first electrode layer 81 (i.e., 1.0 <T α 2 / T1), T α It is more preferable that 2 / T1 is 2.0 to 9.0, and further preferably 3.0 to 5.0. When the second electrode layer 82 is composed of a plurality of layers, the maximum thickness T B The thickness is preferably 40 μm to 80 μm, and more preferably 50 μm to 70 μm.
[0053] The thicknesses of the electrode layers in the bottom electrode portion 8b (T1, T2, T α 2, T3) can be measured by image analysis of the XZ cross section of the bottom electrode portion 8b. In this case, it is preferable to measure the thickness in a region at least 100 μm or more inward from the end of the bottom electrode portion 8b in the X-axis direction. In addition, the thickness (T1) of the first electrode layer 81 is measured in the bonding region with the bottom surface 4b of the element body 4, not in the bonding region with the extraction electrode portion 61. More specifically, the average thickness T1 of the first electrode layer 81 is calculated by measuring the perpendicular distance from the bonding interface with the bottom surface 4b of the element body 4 to the bonding interface with the second electrode layer 82 at at least three points. The average thickness T2 of the second electrode layer 82 is calculated by measuring the perpendicular distance from the bonding interface with the first electrode layer 81 to the bonding interface with the outermost layer 83 at at least three points. The average thickness T3 of the outermost layer 83 described later may be calculated in the same manner as above. In addition, the maximum thickness T B is calculated as the maximum value of the perpendicular distance measured from the bonding interface with the bottom surface 4b of the element body 4 to the outermost surface of the bottom electrode portion 8b at least three points.
[0054] The outermost layer 83 is preferably a plating layer covering the surface of the terminal electrode 8. Specifically, the outermost layer 83 may be made of a metal such as Sn, Cu, Ni, Pt, Ag, or Pd, or an alloy containing at least one of the above metal elements, and may be a single layer or multiple layers. For example, the outermost layer 83 may have a laminated structure of a Ni plating layer and a Sn plating layer, and in this case, it is preferable that the Ni plating layer contacts the second electrode layer 82 and the Sn plating layer is located on the outermost surface side.
[0055] The average thickness T3 of the outermost layer 83 is preferably 3 μm to 20 μm. Although the outermost layer 83 is not essential depending on the usage form of the inductor 2, the presence of the outermost layer 83 can improve the wettability and adhesive strength of a bonding member such as solder to the terminal electrode 8.
[0056] Up to this point, the characteristics of each electrode layer present in the bottom electrode portion 8b have been described in detail with reference to FIG. 3. However, the second electrode layer 82 and the outermost layer 83 in the end electrode portion 8a and the wraparound portion 8c can also be formed from the same material as each layer in the bottom electrode portion 8b, and have similar characteristics. For example, the average thickness of the second electrode layer 82 in the end electrode portion 8a is 1 / 2 the average thickness T2 (or T α 2), or may be different, and T2 (or T α 2) can be about 0.1 to 1.0 times the maximum thickness T A The maximum thickness T of the bottom electrode portion 8b B It may be the same as or different from T B It can be set to about 0.04 to 1.0 times.
[0057] Next, an example of a method for manufacturing the inductor 2 in this embodiment will be described.
[0058] First, the element body 4 can be produced by a known method for producing a powder magnetic core, and the method for producing the element body 4 is not particularly limited. For example, the element body 4 can be produced using a preform 41 as shown in FIG. 8. In producing the preform 41, raw material powder of magnetic particles is kneaded with a binder, a solvent, etc. to form granules, and the granules are used as a raw material for molding. When the magnetic particles are composed of a plurality of particle groups, a plurality of raw material powders with different particle size distributions may be prepared and mixed at a desired ratio. The above granules are then filled in a mold and pressed to obtain a preform 41 having a shape as shown in FIG. 8.
[0059] The preform 41 has a pair of first flanges 41ax, a pair of second flanges 41ay, a winding core 41b, and a notch 41c, and the coil 6α is mounted on the preform 41. Specifically, the winding core 41b is formed of a substantially elliptical cylinder protruding upward along the Z axis, and the winding core 41b is inserted inside the coil 6α. The first flange 41ax protrudes along the X axis direction, and the second flange 41ay protrudes along the Y axis direction, and the coil 6α is installed on each of the flanges 41ax and 41by. The notch 41c is located between the first flange 41ax and the second flange 41ay at the four corners of the XY plane, and the end of the wire 6 passes through the notch 41c and is drawn out to the bottom surface 4b side. Furthermore, the thickness of the first flange portion 41ax is thinner than the thickness of the second flange portion 41ay, and the end portion of the wire 6 drawn out from the coil portion 6α is accommodated below the first flange portion 41ax.
[0060] After the preliminary compact 41 and the coil portion 6α are combined as described above, they are placed in a metal mold. Then, a magnetic paste containing magnetic particles and a resin component is introduced into the metal mold and injection molded to obtain a molded body that will become the element body 4. Alternatively, a magnetic sheet containing magnetic particles and a resin component may be laminated on the preliminary compact 41 with the coil portion 6α mounted thereon and compressed to obtain a molded body that will become the element body 4. The magnetic sheet used here has fluidity during molding, and the components of the magnetic sheet are filled without gaps between the preliminary compact 41 and the coil portion 6α and inside the cutout portion 41c by compression. The molded body obtained above is appropriately subjected to heat treatment or the like to harden the resin component in the molded body, thereby obtaining the element body 4.
[0061] Next, a laser is irradiated to a part of the bottom surface 4b of the element body 4, i.e., the location where the bottom surface electrode portion 8b is to be formed in FIG. 2, to form a planned electrode portion. This laser irradiation removes the insulating layer 6b of the wire 6 drawn out to the bottom surface 4b, and forms the drawn-out electrode portion 61. In addition, the laser irradiation partially removes magnetic particles and resin components contained in the element body from the outermost surface of the element body in the planned electrode portion (the outermost surface of the bottom surface 4b). The planned electrode portion can also be formed by mechanical polishing, blasting, chemical etching, or the like.
[0062] Next, the bottom electrode portion 8b is formed on the above-mentioned electrode-planed portion. The bottom electrode portion 8b can be formed by applying a conductive paste as a raw material by a printing method such as screen printing, and then curing the resin in the paste. At this time, a first conductive paste containing microparticles and nanoparticles is used as a raw material for the first electrode layer 81. The nanoparticles of the first conductive paste have a particle size of at least less than 100 nm, and the nanoparticles correspond to the second particles 11b. The microparticles of the first conductive paste correspond to the first particles 11a and have the characteristics of the first particles 11a as described above. The first conductive paste is printed so as to completely cover the extraction electrode portion 61.
[0063] On the other hand, a second conductive paste containing only microparticles as a conductive powder is used as a raw material for the second electrode layer 82. The microparticles of the second conductive paste correspond to the conductive powder 21 and have the characteristics of the conductive powder 21. In this embodiment, the second conductive paste is printed on the first conductive paste so as to completely cover the first conductive paste printed earlier. When the second electrode layer 82 is configured with a plurality of layers, the second electrode layer 82 shown in FIG. 3B can be formed by applying (printing) the second conductive paste multiple times. Alternatively, when forming the end surface electrode portion 8a, the raw material paste for the end surface electrode portion 8a can be made to wrap around onto the bottom surface electrode portion 8b, thereby forming the second electrode layer 82.
[0064] After printing the raw paste by the above method, the element body 4 is heat-treated under predetermined conditions to harden the resin (13, 23) in the raw paste. The conditions of the heat treatment may be appropriately determined according to the type of resin component used, but for example, it is preferable to set the treatment temperature (holding temperature) to 170°C to 230°C and the holding time to 60 min to 90 min. By performing the heat treatment under such conditions, the bottom electrode portion 8b can be formed without deteriorating the resin component contained in the element body 4 or the insulating layer 6b. In addition, during the above heat treatment, the resin hardens and the nanoparticles in the first conductive paste are bonded to each other while growing in the gaps between the microparticles and at the contact interface of the extraction electrode portion 61, becoming the second particles 11b. The hardening treatment of the raw paste may be performed each time after printing each electrode layer paste, or may be performed collectively after printing all the electrode layer pastes.
[0065] Next, a second electrode layer 82 is also formed on the end surface 4a side of the element body 4. The second electrode layer 82 on the end surface 4a side is formed by dipping the end surface 4a side of the element body 4 in the second conductive paste used above. At this time, a part of the upper surface 4c and the side surface 4d connected to the end surface 4a are also dipped in the second conductive paste, and the wraparound portion 8c is formed. After dipping in the raw material paste in this way, similar to the formation of the bottom electrode portion 8b, a heat treatment is performed to harden the resin 23 in the raw material paste, and the second electrode layer 82 is also formed on the end surface 4a side.
[0066] After the two types of resin electrodes (81, 82) are formed by the above procedure, the outermost layer 83 is formed by a method such as barrel plating. The method for forming the outermost layer 83 is preferably a plating process, but is not limited to this, and the outermost layer 83 may also be formed by a sputtering method or a vapor deposition method.
[0067] By the manufacturing method as described above, an inductor 2 having a pair of terminal electrodes 8 formed on an element body 4 is obtained. The manufacturing method of the inductor 2 is not limited to the above method and may be modified as appropriate. For example, a mother molded body having a plurality of coil portions 6α embedded therein may be produced, and then a plurality of element bodies 4 may be obtained by cutting the mother molded body. By employing such a method, production efficiency is improved.
[0068] Next, a description will be given of an example of a usage form of the inductor 2 according to this embodiment. The inductor 2 can be used by being surface-mounted on a substrate 100 such as a circuit board, as shown in FIG.
[0069] In surface mounting of the inductor 2, solder paste or conductive adhesive can be used as the bonding member 50. For example, the bonding member 50, which is solder paste, is applied to a predetermined position on the surface of the substrate 100, and the inductor 2 is pressed against the bonding member 50, thereby mounting the inductor 2 on the substrate 100. At this time, the bonding member 50 is not only interposed between the bottom electrode portion 8b and the substrate 100, but also wets and spreads on the outer surface of the end electrode portion 8a, forming a fillet by the bonding member 50 on the outside of the end electrode portion 8a. By forming a fillet on the end electrode portion 8a side in this manner, the bonding strength of the mounting portion can be sufficiently ensured.
[0070] 4, the entire inductor 2 after mounting may be covered with a sealing material 90. There are no particular limitations on the sealing material 90, and for example, epoxy resin, silicone resin, or the like can be used.
[0071] (Summary of the first embodiment) In the inductor 2 of this embodiment, the terminal electrode 8 includes a first electrode layer 81 having a low resin content and low resistance, and a second electrode layer 82 having a high resin content. These resin electrodes (81, 82) can be formed at a low temperature of 250° C. or less, and deterioration of the resin component contained in the element body 4 and the insulating layer 6b can be prevented during the formation of the terminal electrode 8.
[0072] In addition, low-temperature sintered electrodes containing metal particles are known, and the low-temperature sintered electrodes can also be formed at a low temperature of 250°C or less. However, the conventional low-temperature sintered electrodes have poor resistance to acids, and when exposed to an etching solution or a plating solution in the process of forming a plating electrode, the metal components (particularly metal particles) in the low-temperature sintered electrodes flow out into the solution. As a result, there is a risk of a decrease in production efficiency and deterioration of the characteristics of the low-temperature sintered electrodes (deterioration of adhesion strength and contact resistance, etc.). In addition, when the conventional low-temperature sintered electrodes are formed to a thickness of 50 μm or more, the adhesion strength to the element body is extremely reduced. Therefore, it is difficult to form the conventional low-temperature sintered electrodes to a thickness of 50 μm or more, and they are easily peeled off due to external stress or impact. In addition, it is not possible to ensure a sufficient mounting height in surface mounting.
[0073] In contrast, in the terminal electrode 8 of this embodiment, the second electrode layer 82 having a large amount of resin is formed on the first electrode layer 81 having a low resistance, so that even if exposed to an etching solution or a plating solution, the metal components (11, 21) are unlikely to flow out into the solution. That is, the terminal electrode 8 of this embodiment exhibits excellent acid resistance. In addition, since the first electrode layer 81 having a low resistance is present at the portion in contact with the extraction electrode portion 61, the contact resistance of the terminal electrode 8 can be reduced. Furthermore, since the second electrode layer 82 is laminated on the first electrode layer 81, the adhesive strength of the terminal electrode 8 to the element body 4 can be sufficiently ensured. That is, the terminal electrode 8 of this embodiment has a low contact resistance, is unlikely to peel off even when subjected to external stress or impact, and exhibits excellent impact resistance. Since the terminal electrode 8 has the above-mentioned characteristics, the inductor 2 of this embodiment has a better connection reliability of the terminal electrode 8 than a conventional low-temperature sintered electrode.
[0074] In particular, the first electrode layer 81 and the second electrode layer are laminated at the bottom electrode portion 8b, which is a portion connected to the extraction electrode portion 61 and which is a mounting portion when surface-mounted on the substrate 100. By forming a laminated structure of the first electrode layer 81 and the second electrode layer at this portion, the following effects can be obtained.
[0075] When a coil component such as an inductor is directly surface-mounted on a substrate, there is a risk that the terminal electrodes (particularly the terminal electrodes on the mounting surface side) will peel off due to flexural deformation of the substrate. In the inductor 2 of this embodiment, resin electrodes (81, 82) are laminated on the bottom electrode portion 8b, and among these resin electrodes, the second electrode layer 82 in particular can absorb external stress and impact. Therefore, in the inductor 2 of this embodiment, even if an external force such as flexural deformation of the substrate 100 is applied to the mounting portion, peeling of the terminal electrodes 8 (particularly the bottom electrode portion 8b) can be more effectively prevented.
[0076] Furthermore, in the inductor 2 of this embodiment, even if the bottom electrode portion 8b is thickened, the adhesive strength of the terminal electrode 8 to the element body 4 can be sufficiently ensured. Furthermore, by thickening the second electrode layer 82, the adhesive strength can be further increased. Therefore, in the mounted state shown in FIG. 4, the mounting height H from the bottom surface 4b to the surface of the substrate 100 can be sufficiently ensured and can be easily controlled to a suitable height. Although the mounting height H is not particularly limited, the inductor 2 of this embodiment can easily achieve a mounting height H (50 μm or more) that is difficult to achieve with conventional low-temperature sintered electrodes.
[0077] The bonding member 50 used for mounting contains flux such as a solvent, and after mounting, the flux may accumulate between the bottom surface 4b and the substrate 100. In the inductor 2 of this embodiment, the mounting height H can be sufficiently ensured as described above, so that the generated flux can be easily removed. In addition, as shown in FIG. 4, the inductor 2 may be entirely covered with a sealing material 90 after mounting. Even in this case, in the inductor 2 of this embodiment, the mounting height H can be sufficiently ensured, so that the sealing material 90 can be easily filled in the gap between the bottom surface 4b and the substrate 100, and the inductor 2 can be sealed without any voids.
[0078] In addition, when the content of the resin 13 in the first electrode layer 81 is controlled to the preferred range as described above, the conductive powder 11 may be composed of only metal particles of the micrometer order. However, preferably, the conductive powder 11 in the first electrode layer 81 has the following configuration. That is, in this embodiment, the first electrode layer 81 contains the first particles 11a of the micrometer order and the second particles 11b having a particle size of 100 nm or less as the conductive powder 11. The second particles 11b are present in an aggregated state in the gaps between the first particles 11a and at the bonding interface with the lead electrode portion 61. With this configuration, the resistance value of the first electrode layer 81 can be further reduced, and the electrical characteristics of the terminal electrode 8 can be further improved. In addition, the adhesive strength of the terminal electrode 8 (particularly the bottom electrode portion 8b) to the element body 4 can be further increased, and the connection reliability of the terminal electrode 8 can be further improved.
[0079] Furthermore, in this embodiment, the average thickness T2 (or T α 2) is thicker than the average thickness T1 of the first electrode layer 81, and the first electrode layer 81 and the second electrode layer 82 are formed to the predetermined thickness as described above. By controlling the thickness of each resin electrode to a predetermined condition, the acid resistance and impact resistance of the terminal electrode 8 can be further improved, and the bonding reliability of the terminal electrode 8 can be further improved.
[0080] Furthermore, as shown in FIG. 3B, the second electrode layer 82 can be configured with multiple layers, in which case the impact resistance of the terminal electrode 8 can be further improved.
[0081] Second embodiment In the second embodiment, a modified example of the terminal electrode 8 will be described with reference to Figures 5 to 7. In the second embodiment, the description of the configuration common to the first embodiment will be omitted and the same reference numerals will be used.
[0082] 5, similarly to the first embodiment, a first electrode layer 81, a second electrode layer 82, and an outermost layer 83 are laminated in a bottom electrode portion 8b, and the second electrode layer 82 and the outermost layer 83 are laminated in an end electrode portion 8a and a wraparound portion 8c. However, in the bottom electrode portion 8b of the inductor 2a, a non-overlapping portion 8d exists at an end portion in the X-axis direction where a part (tip portion) of the first electrode layer 81 is not covered with the second electrode layer 82.
[0083] In this non-overlapping portion 8d, the outermost layer 83 is formed on the outer surface of the first electrode layer 81 without the second electrode layer 82 therebetween, and the outermost layer 83 and the first electrode layer 81 are in direct contact and electrically joined together. Therefore, in the inductor 2a, the contact resistance of the terminal electrode 8 can be further reduced.
[0084] The non-overlapping portion 8d is located at a predetermined distance L1 in the X-axis direction from the contact point between the lead-out electrode portion 61 and the bottom electrode portion 8b, and the predetermined distance L1 is preferably 0.01 mm to 0.40 mm. The length L2 of the non-overlapping portion 8d in the X-axis direction is preferably 0.05 mm to 0.2 mm. Since the non-overlapping portion 8d is located at the end of the bottom electrode portion 8b away from the lead-out electrode portion 61 and has a predetermined length, the contact resistance can be further reduced while the acid resistance and impact resistance of the terminal electrode 8 are sufficiently ensured.
[0085] 6, the first electrode layer 81 may be formed not only on the bottom electrode portion 8b but also on the end electrode portion 8a and the wraparound portion 8c. The first electrode layer 81 on the end surface 4a side may be formed from the same material as the first electrode layer 81 on the bottom surface 4b side, and the thickness may be approximately the same as that on the bottom surface 4b side.
[0086] When the first electrode layer 81 is also formed on the end face 4a side, the terminal electrode 8 may have a structure as shown in Fig. 7. In the inductor 2c shown in Fig. 7, at the connection portion between the end face electrode portion 8a and the bottom face electrode portion 8b, a part of the first electrode layer 81 on the end face 4a side is partially drawn out toward the outer surface side of the second electrode layer 82. In other words, the first electrode layer 81 on the end face 4a side is interposed between the second electrode layer 82 on the end face 4a side and the second electrode layer 82 on the bottom face 4b side.
[0087] 7, a part of the first electrode layer 81 drawn out to the outer surface side wraps around the outer surface of the second electrode layer 82 on the bottom surface 4b side, forming an overlapping portion 8e in which a part of the first electrode layer 81 is laminated on the outer surface of the second electrode layer 82. Note that in the overlapping portion 8e, the second electrode layer 82 on the end surface 4a side may further wrap around and be laminated outside the first electrode layer 81 that wraps around from the end surface 4a side.
[0088] The structure having the overlapping portion 8e as shown in FIG. 7 can be realized by forming the first electrode layer 81 and the second electrode layer 82 of the bottom electrode portion 8b by printing, and then forming the first electrode layer 81 and the second electrode layer 82 of the end electrode portion 8a by dipping. That is, when the end electrode portion 8a is formed by dipping, the raw material paste flows around to the surface side of the bottom electrode portion 8b, thereby forming the overlapping portion 8e. With such an electrode formation method, the terminal electrodes can be efficiently formed in the required locations. That is, the inductor 2c having the structure shown in FIG. 7 can be efficiently produced and is suitable for mass production.
[0089] In the inductor 2c, the first electrode layer 81 with a low resistance value is drawn out to the outer surface side of the terminal electrode 8 that contacts the bonding member 50 during surface mounting, so that the resistance value of the terminal electrode 8 can be further reduced. Also, a part of the first electrode layer 81 on the end face 4a side wraps around onto the bottom electrode portion 8b to form an overlapping portion 8e, which further improves the adhesion strength of the bottom electrode portion 8b to the bottom surface 4b. In addition, the bottom electrode portion 8b becomes even less likely to peel off. As a result, the connection reliability of the terminal electrode 8 can be further improved.
[0090] In addition, as shown in FIG. 7, when the first electrode layer 81 having a low resistance value is partially extended to the outer surface side of the terminal electrode 8, the content of the resin 23 in the second electrode layer 82 can be made higher than that in the inductor 2 shown in FIG. 2. For example, in the embodiment shown in FIG. 7, the content A of the resin 23 R 2 (≈R2) can be set to 20% or more and 90% or less. Even if the content of the resin 23 is increased, the electrical characteristics of the terminal electrode 8 can be ensured to a certain extent.
[0091] As described above, the positions where the first electrode layer 81 and the second electrode layer 82 are formed are not limited to the mode shown in the first embodiment, and may be, for example, the modes shown in Figures 5 to 7. Note that in the inductors 2a to 2c shown in Figures 5 to 7, the first electrode layer 81 and the second electrode layer 82 having the same characteristics as in the first embodiment are laminated at the joint with the extraction electrode portion 61. Therefore, even in the case of these modified examples, the same effects as in the first embodiment can be obtained.
[0092] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made within the scope of the present invention.
[0093] For example, in Fig. 2 to Fig. 7, the coil portion 6α is made of a round wire 6, but the type of wire 6 is not limited to this and may be a rectangular wire having a substantially rectangular cross-sectional shape. Alternatively, the wire may be a square wire or a Litz wire made by twisting together thin wires. Furthermore, the coil portion 6α may be made by laminating conductive plate materials.
[0094] In the above embodiment, the lead electrode portion 61 is located on the bottom surface 4b, but the lead electrode portion 61 may be located on the end surface 8a or the side surface 4d, or may be located across multiple surfaces. In this case, the location of the terminal electrode 8 may be appropriately changed according to the location of the lead electrode portion 61.
[0095] The first core portion 41 constituting the element body 4 may also be a sintered body of ferrite powder or metal magnetic powder. Furthermore, the element body 4 itself may be an FT-type, ET-type, EI-type, UU-type, EE-type, EER-type, UI-type, drum-type, toroidal-type, pot-type, or cup-type compact core, and an inductor element may be formed by winding a coil around the compact core. In this case, the wire 6 constituting the lead-out electrode portion 61 does not need to be embedded inside the element body, and may be led out along the outer periphery of the core and connected to the terminal electrode 8.
[0096] Furthermore, the coil component according to the present invention is not limited to an inductor, but may be a coil component such as a transformer, a choke coil, or a common mode filter, or a composite coil component including an inductor region and a capacitor region. Among these coil components, the present invention is particularly suitable for coil components that include a coil with an insulating coating inside the element body 4 or a coil component that includes resin. [Explanation of symbols]
[0097] 2 … Inductor 4 … Element body 4a … End face 4b … Bottom surface 4c…Top surface 4d…side 41 ... Preform 41ax … 1st collar part 41ay … 2nd tsuba part 41b … Winding core part 41c … Cutout 6α … Coil section 6 … Wire 6a … Core part 6b … Insulating layer 61 … Extraction electrode part 8 … Terminal electrode 8a... End face electrode part 8b…Bottom electrode part 8c … Wraparound section 8d… Non-overlapping part 8e … Overlapping part 81 … First electrode layer 11 ... Conductive powder (first electrode layer) 11a … 1st particle 11b…Second particle 13 … Resin (first electrode layer) 82…Second electrode layer 20 … Outer resin electrode layer 21 ... Conductive powder (second electrode layer) 23 … Resin (second electrode layer) 25 … Borderline 83 … Outermost layer 50 ... Joint material 90 ... Encapsulating material 100 ... Substrate
Claims
1. a core portion including magnetic particles and a resin component; A coil portion formed by winding a conductor; a terminal electrode formed on a part of an outer surface of the core portion and electrically connected to an end of the conductor drawn out from the coil portion, The terminal electrode is a first electrode layer in contact with an end of the conductor; a second electrode layer disposed outside the first electrode layer; The first electrode layer and the second electrode layer each contain a conductive powder and a resin, a content of the resin in the second electrode layer is greater than a content of the resin in the first electrode layer, The average thickness of the second electrode layer is greater than the average thickness of the first electrode layer, A coil component in which a non-overlapping portion of the first electrode layer that is not covered by the second electrode layer exists from a location a predetermined distance (L1) in the first axial direction along the same plane from the contact point between the conductor and the first electrode layer toward the end of the terminal electrode.
2. The conductor powder of the first electrode layer includes Metal nanoparticles having a particle size of at least 100 nm or less; The coil component according to claim 1 , further comprising metal microparticles having a particle size larger than that of the metal nanoparticles.
3. 3. The coil component according to claim 1, wherein the second electrode layer is formed by laminating a plurality of resin electrode layers.
4. 4. The coil component according to claim 1, wherein a portion of the first electrode layer is partially extended toward an outer surface side of the second electrode layer.
5. A coil component as described in claim 1 or 2, wherein the thickness of the first electrode layer is not constant, and the thickness of the first electrode layer is thinner in the portion where the diameter of the conductor pulled out from the coil portion is the largest.
Citation Information
Patent Citations
Method of forming electrode of electronic parts
JP1988045813A
Chip type electronic component and manufacturing method of the same
JP2013069713A
Method of manufacturing surface mount inductor
JP2013211333A
Method for manufacturing surface mounted inductor
JP2014225590A
Electronic component
JP2019012790A