Method for producing superabsorbents
The method addresses conveyor belt cleaning challenges in superabsorbent production by using a stripping device and controlled water spraying, enhancing belt cleanliness and reducing mechanical stress for continuous production.
Patent Information
- Application Number
- JP2021517231
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-28
- Filing Date
- 2019-09-17
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2039-09-17
AI Technical Summary
Existing methods for producing superabsorbents face challenges in efficiently cleaning vibratory conveyor belts and reducing mechanical stress on them during the production process.
A method involving the use of a vibrating conveyor belt with a stripping device and controlled water spraying to remove adhering polymer gel, combined with optimized positioning and configuration of the stripping device and nozzles to prevent gel adhesion and facilitate easy cleaning.
The method effectively prevents conveyor belt caking and extends the maintenance intervals, ensuring continuous and efficient production of superabsorbents with improved belt cleanliness and reduced mechanical stress.
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for preparing superabsorbent particles by polymerizing a monomer solution or suspension. The method for producing the aqueous polymer gel is carried out by drying the aqueous polymer gel in an air circulating belt dryer. drying in a rockner; grinding; Grading and optionally The aqueous polymer gel is then thermally crosslinked on a vibrating conveyor belt (oszil Lierenden Foerderbandes) into the air circulation belt dryer, and the rotary conveyor The underside of the belt is connected to at least one stripping device (ab The underside of the rotating conveyor belt is protected from adhesion of polymer gels by the streifvorrichtung method. In one embodiment, water is sprayed onto the [Background technology]
[0002] Superabsorbents are used to manufacture diapers, tampons, sanitary napkins and other hygiene articles, but are also used as water retention agents in the gardening market. Superabsorbents are also called water-absorbing polymers.
[0003] The production of superabsorbents is described in the article "Modern Superabsorbent Polymer Technology", FL Buchholz and AT Graham, Wiley-VCH, 1998, pp. 71-103.
[0004] The properties of the superabsorbent can be adjusted, for example, via the amount of crosslinker used. Increasing the amount of crosslinker decreases the centrifuge retention capacity (CRC), which is 21.0 g / cm 2 The absorption rate at a pressure of (AUL 0.3 psi) passes through a maximum value.
[0005] Performance characteristics, e.g. 49.2g / cm 2 To improve the gel bed permeability (GBP) and absorbency under a pressure of 0.7 psi (AUL), superabsorbent particles are generally surface postcrosslinked. This increases the level of crosslinking at the particle surface, which is 49.2 g / cm 2 Absorption rate under pressure (AUL 0.7 psi) and centrifugal retention capacity (CRC) can be at least partially separated. This surface postcrosslinking can be carried out in the gel aqueous phase. However, preferably, the dried, ground and sieved polymer particles (base polymer) are surface-coated with a surface postcrosslinking agent and thermally surface postcrosslinked. Crosslinking agents suitable for this purpose are compounds capable of forming covalent bonds with at least two carboxylic acid groups of the polymer particles.
[0006] WO2008 / 087114 A1, WO2010 / 139680 A2 and EP2 700 667 A1 describe the loading of an aqueous polymer gel onto the conveying belt of an air circulating belt dryer by means of a vibrating conveyor belt. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] WO2008 / 087114 A1 [Patent Document 2] WO2010 / 139680 A2 [Patent Document 3] EP2 700 667 A1 [Non-patent literature]
[0008] [Non-Patent Document 1] Paper "Modern Superabsorbent Polymer Technology", FL Buchholz and AT Graham, Wiley-VCH, 1998, pp. 71-103. Summary of the Invention [Problem to be solved by the invention]
[0009] The object of the present invention was to provide an improved method for producing superabsorbents, in particular a simplified cleaning of the vibrating conveyor belts used and lower mechanical stress on the conveyor belt itself. [Means for solving the problem]
[0010] The purpose of this is to a) at least one ethylenically unsaturated amine having an acid group and which is at least partially neutralized; monomer, b) at least one crosslinker; c) at least one initiator; d) optionally, one or more ethylenically unsaturated monomers copolymerizable with the monomers described in a); Marr, and e) optionally, one or more water-soluble polymers; A method for producing a superabsorbent by polymerizing a monomer solution or monomer suspension comprising: It is a law, The resulting aqueous polymer gel is dried in an air circulating belt dryer, and then crushed. Tep, Grading and optionally a thermal surface postcrosslinking step, The aqueous polymer gel is introduced into an air circulating belt dryer by a vibrating conveyor belt; The underside of the rotating conveyor belt is stripped of polymer gel by at least one stripping device. Water is sprayed on the underside of the rotating conveyor belt to prevent it from sticking to the ground. This was achieved by the method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The lower side of the turning conveyor belt is the outer side of the conveyor belt, which is where the polymer gel is dispensed again after turning. The upper side of the turning conveyor belt is the inner side of the conveyor belt, which is not meant to come into contact with the polymer gel.
[0012] The distance of the stripping device from the discharge end of the vibrating conveyor belt is preferably less than 20% of the length of the vibrating conveyor belt, more preferably less than 10% of the length of the vibrating conveyor belt, most preferably less than 5% of the length of the vibrating conveyor belt, the length of the vibrating conveyor belt being the distance of its pivot axis from the discharge end.
[0013] The stripping device is not subject to any limitations. A suitable example is a brush arranged transversely to the running direction. It is also possible to use a scraper. The scraper is a stripping device made of a non-flexible material arranged transversely to the conveying direction. An example of a suitable non-flexible material is polytetrafluoroethylene. To avoid damage to the conveyor belt, the scraper should have minimal direct contact (if any) with the conveyor belt. The scraper should be inclined with respect to the running direction of the rotating conveyor belt. This promotes the release of the adhering polymer gel and prevents backup between the conveyor belt and the scraper. The stripped polymer gel typically falls onto the conveyor belt of the air circulation belt dryer.
[0014] The scraper is preferably inclined at an angle of 5° to 45°, more preferably at an angle of 10° to 35°, very particularly at an angle of 15° to 25°, to the horizontal counter to the running direction of the conveyor belt. The distance of the scraper from the underside of the rotating conveyor belt is preferably 0.1 to 5 mm, more preferably 0.2 to 2 mm, most preferably 0.5 to 1.5 mm.
[0015] The distance of the spray nozzle from the discharge end of the vibrating conveyor belt is preferably 1% to 50% of the length of the vibrating conveyor belt, more preferably 2% to 30% of the length of the vibrating conveyor belt, and most preferably 3% to 10% of the length of the vibrating conveyor belt, the length of the vibrating conveyor belt being the distance of the pivot axis from the discharge end.
[0016] The distance of the spray nozzle from the conveyor belt is preferably 5-50 cm, more preferably 10-30 cm, most preferably 15-25 cm.
[0017] The liquid is preferably sprayed by at least one two-phase nozzle, more preferably by at least two two-phase nozzles.
[0018] Two-phase nozzles allow atomization into fine droplets or spray mist. The atomization forms employed are solid or hollow cones of circular or elliptical shape. Two-phase nozzles may be set with external mixing or internal mixing. In the case of external mixing two-phase nozzles, the liquid and the atomizing gas leave the nozzle head through separate orifices. They are mixed in the spray jet only after leaving the spray nozzle. This allows independent control of the droplet size distribution and the throughput over a wide range. The spray cone of the spray nozzle can be adjusted by the air cap setting. In the case of internal mixing two-phase nozzles, the liquid and the atomizing gas are mixed in the spray nozzle and the biphasic mixture leaves the nozzle head through the same hole (or through several parallel holes). In the case of internal mixing two-phase nozzles, the quantitative ratio and pressure conditions are more highly coupled than in the case of external mixing spray nozzles. Small changes in throughput therefore lead to changes in the droplet size distribution. Adjustment to the desired throughput is achieved by the selected cross section of the nozzle holes.
[0019] An example of a useful atomizing gas is compressed air at 0.5 bar or more. The droplet size can be adjusted individually by the nozzle geometry, the nozzle type, the ratio of the mass flow rate of the water to the mass flow rate of the atomizing gas, and the pressure of the gas and water.
[0020] The amount of water used for spraying is preferably 2 to 20 kg / hour, more preferably 6 to 16 kg / hour, and most preferably 8 to 12 kg / hour.
[0021] The weight ratio of atomizing gas to water is preferably 2-20, more preferably 6-16, most preferably 8-12. If too little water is used, the conveyor belt will be inadequately wetted. If too much water is used, excess water will drip onto the perforated plate of the air circulation belt dryer, leading to blockages there. The use of a two-phase nozzle additionally improves water distribution, preventing larger droplets.
[0022] In a preferred embodiment of the invention, there is at least one spray nozzle beyond the stripping device in the running direction of the conveyor belt, which prevents water from dripping away from the stripping device onto the conveyor belt of the air circulation belt dryer.
[0023] In a further preferred embodiment of the present invention, there is at least one spray nozzle upstream of the conveyor belt of the air circulation belt dryer, which also prevents water from dripping onto the conveyor belt of the air circulation belt dryer.
[0024] The conveyor belt preferably has a length of 2 to 10 m, more preferably 2.5 to 8 m, and most preferably 3 to 6 m, the length of the conveyor belt being the distance of the pivot from the discharge end.
[0025] The conveyor belt preferably has a width of 0.5 to 1.5 m, more preferably 0.6 to 1.2 m, most preferably 0.7 to 0.9 m.
[0026] It is possible to use conveyor belts that are customary for this purpose. The surface of the conveyor belt, i.e. the side that will come into contact with the polymer gel, should be water-repellent and have a contact angle with water at 23° C. of preferably at least 60°, more preferably at least 80°, most preferably at least 100°. The contact angle is a measure of wettability and is measured according to DIN 53900.
[0027] The water content of the polymer gel on the conveyor belt is preferably 20-80% by weight, more preferably 30-70% by weight, and most preferably 40-60% by weight.
[0028] The temperature of the polymer gel on the conveyor belt is preferably 60 to 105°C, more preferably 70 to 100°C, and most preferably 80 to 95°C.
[0029] The invention is based on the finding that warm polymer gel adhering to a vibrating conveyor belt dries out very easily. The dried polymer gel can only be removed from the conveyor belt with great difficulty. The already dried polymer gel is often the cause of further caking. Spraying with water can keep the polymer gel moist and prevent it from drying out.
[0030] The preparation of the superabsorbent is described in detail below.
[0031] Superabsorbents are produced by polymerizing a monomer solution or suspension and are typically water-soluble.
[0032] The monomers a) are preferably water-soluble, i.e. their solubility in water at 23° C. is typically at least 1 g / 100 g water, preferably at least 5 g / 100 g water, more preferably at least 25 g / 100 g water and most preferably at least 35 g / 100 g water.
[0033] Suitable monomers a) are, for example, ethylenically unsaturated carboxylic acids, such as acrylic acid, methacrylic acid and itaconic acid. Particularly preferred monomers are acrylic acid and methacrylic acid. Very particular preference is given to acrylic acid.
[0034] Further suitable monomers a) are, for example, ethylenically unsaturated sulfonic acids, such as styrenesulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid (AMPS).
[0035] Impurities can have a significant impact on polymerization. The raw materials used should therefore have maximum purity. It is therefore often advantageous to specially purify monomer a). Suitable purification methods are described, for example, in WO02 / 055469 A1, WO03 / 078378 A1 and WO2004 / 035514 A1. A suitable monomer a) is, for example, acrylic acid purified according to WO2004 / 035514 A1, and contains 99.8460% by weight of acrylic acid, 0.0950% by weight of acetic acid, 0.0332% by weight of water, 0.0203% by weight of propionic acid, 0.0001% by weight of furfurals, 0.0001% by weight of maleic anhydride, 0.0003% by weight of diacrylic acid and 0.0050% by weight of hydroquinone monomethyl ether.
[0036] The proportion of acrylic acid and / or its salts in the total amount of monomers a) is preferably at least 50 mol %, more preferably at least 90 mol %, most preferably at least 95 mol %.
[0037] Monomer a) typically comprises a polymerization inhibitor, preferably a hydroquinone monoether, as a storage stabilizer.
[0038] The monomer solution preferably comprises at most 250 ppm by weight, preferably at most 130 ppm by weight, more preferably at most 70 ppm by weight of hydroquinone monoether, preferably at least 10 ppm by weight, more preferably at least 30 ppm by weight, in particular approximately 50 ppm by weight of hydroquinone monoether, in each case based on the non-neutralized monomer a).For example, the monomer solution can be prepared using an ethylenically unsaturated monomer having an acid group, which has an appropriate content of hydroquinone monoether.
[0039] Preferred hydroquinone monoethers are hydroquinone monomethyl ether (MEHQ) and / or alpha-tocopherol (vitamin E).
[0040] Suitable crosslinking agents b) are compounds that have at least two groups suitable for crosslinking.Such groups are, for example, ethylenically unsaturated groups that can be free-radical polymerized into polymer chains, and functional groups that can form covalent bonds with the acid groups of monomer a).In addition, polyvalent metal salts that can form coordinate bonds with at least two acid groups of monomer a) are also suitable as crosslinking agents b).
[0041] The crosslinker b) is preferably a compound having at least two polymerizable groups which can be subjected to free-radically polymerization into a polymer network. Preferred crosslinkers b) are, for example, ethylene glycol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, allyl methacrylate, trimethylolpropane triacrylate, triallylamine, tetraallylammonium chloride, tetraallyloxyethane, as described in EP 0530438 A1; di- and triacrylates, as described in EP 0547847 A1, EP 0559476 A1, EP 0632068 A1, WO 93 / 21237 A1, WO 03 / 104299 A1, WO 03 / 104300 A1, WO 03 / 104301 A1 and DE 103 31 450 A1; mixed acrylates which contain further ethylenically unsaturated groups in addition to the acrylate groups, as described in DE 103 31 456 A1 and DE 103 55 401 A1. A1; or crosslinker mixtures, as described, for example, in DE 195 43 368 A1, DE 196 46 484 A1, WO 90 / 15830 A1 and WO 02 / 032962 A2.
[0042] Preferred crosslinkers b) are pentaerythrityl triallyl ether, tetraallyloxyethane, methylene bismethacrylamide, 15-tuply ethoxylated trimethylolpropane triacrylate, polyethylene glycol diacrylate, trimethylolpropane triacrylate and triallylamine.
[0043] Very particularly preferred crosslinkers b) are polyethoxylated and / or propoxylated glycerols which are esterified with acrylic or methacrylic acid to give di- or triacrylates, as described, for example, in WO 03 / 104301 A1. Di- and / or triacrylates of 3- to 10-tuply ethoxylated glycerol are especially preferred. Very particularly preferred are di- or triacrylates of 1- to 5-tuply ethoxylated and / or propoxylated glycerol. Most preferred are triacrylates of 3- to 5-tuply ethoxylated and / or propoxylated glycerol, in particular triacrylates of 3-tuply ethoxylated glycerol.
[0044] The amount of crosslinker b) is in each case calculated on the total amount of monomers a) used, preferably 0.05% to 1.5% by weight, more preferably 0.1% to 0.8% by weight, most preferably 0.15% to 0.5% by weight. With increasing crosslinker content, the centrifuge retention capacity (CRC) decreases, reaching 21.0 g / cm 2 At this pressure the absorption rate passes through a maximum value.
[0045] The initiators c) used may be all compounds which generate free radicals under the polymerization conditions, for example thermal, redox or photoinitiators. Suitable redox initiators are peroxodisulfate / ascorbic acid, hydrogen peroxide / ascorbic acid, sodium peroxodisulfate / sodium bisulfite and hydrogen peroxide / sodium bisulfite. Preference is given to using mixtures of thermal and redox initiators, for example sodium peroxodisulfate / hydrogen peroxide / ascorbic acid. The reducing component used is preferably the disodium salt of 2-hydroxy-2-sulfinatoacetic acid; or a mixture of the sodium salt of 2-hydroxy-2-sulfinatoacetic acid, the disodium salt of 2-hydroxy-2-sulfinatoacetic acid and sodium bisulfite. Such mixtures are available as Bruggolite® FF6 and Bruggolite® FF7 (Bruggemann Chemicals, Heilbronn, Germany).
[0046] Ethylenically unsaturated monomers d) copolymerizable with the ethylenically unsaturated monomers a) having an acid group are, for example, acrylamide, methacrylamide, hydroxyethyl acrylate, hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, dimethylaminoethyl acrylate, dimethylaminopropyl acrylate, diethylaminopropyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate.
[0047] The water-soluble polymers e) used may be polyvinyl alcohol, polyvinylpyrrolidone, starch, starch derivatives, modified celluloses, such as methylcellulose or hydroxyethylcellulose, gelatin, polyglycols or polyacrylic acids, preferably starch, starch derivatives and modified celluloses.
[0048] Typically, an aqueous monomer solution is used. The water content of the monomer solution is preferably 40% to 75% by weight, more preferably 45% to 70% by weight, most preferably 50% to 65% by weight. It is also possible to use a monomer suspension, i.e. a monomer solution having monomer a) beyond its solubility, for example sodium acrylate. If the water content increases, the energy expenditure in the subsequent drying increases, and if the water content decreases, the heat of polymerization can only be removed insufficiently.
[0049] For optimal action, preferred polymerization inhibitors require dissolved oxygen.Therefore, dissolved oxygen can be liberated from monomer solution before polymerization by inerting, i.e., flushing into inert gas, preferably nitrogen or carbon dioxide.The oxygen content of monomer solution is preferably reduced to less than 1 ppm by weight, more preferably less than 0.5 ppm by weight, and most preferably less than 0.1 ppm by weight before polymerization.
[0050] Suitable reactors for polymerization are, for example, kneading reactors or belt reactors.In kneaders, the polymer gel formed in the polymerization of aqueous monomer solution or suspension is continuously comminuted, for example by contrarotatory stirrer shafts, as described in WO2001 / 038402 A1.Polymerization on belts is described, for example, in DE 3825366 A1 and US 6,241,928.Polymerization in belt reactors forms polymer gel that needs to be comminuted, for example in extruders or kneaders.
[0051] To improve the drying properties, the comminuted polymer gel obtained by the kneader can be further extruded.
[0052] The acid groups of the resulting polymer gel are typically partially neutralized. Neutralization is preferably carried out at the monomer stage. This is typically achieved by mixing in a neutralizing agent as an aqueous solution or else preferably as a solid. The degree of neutralization is preferably 25-85 mol%, more preferably 30-80 mol%, most preferably 40-75 mol%, for which customary neutralizing agents can be used, preferably alkali metal hydroxides, alkali metal oxides, alkali metal carbonates or alkali metal hydrogen carbonates, as well as mixtures thereof. Instead of the alkali metal salts, it is also possible to use ammonia salts. Particularly preferred alkali metals are sodium and potassium, while very particular preference is given to sodium hydroxide, sodium carbonate or sodium hydrogen carbonate, as well as mixtures thereof. Here, solid carbonates and hydrogen carbonates can also be introduced in encapsulated form, preferably directly into the monomer solution before polymerization, during polymerization or after polymerization and before its drying into the polymer gel. Encapsulation is achieved by coating the surface with an insoluble or only slowly soluble material (e.g., by a film-forming polymer, an inert inorganic material, or a fusible organic material), which retards dissolution and reaction of the solid carbonate or bicarbonate to such an extent that carbon dioxide is not released until during drying and the formed superabsorbent has high internal porosity.
[0053] Optionally, a surfactant can be added to the monomer solution before or during polymerization, and the monomer solution can then be foamed with an inert gas or steam or by vigorous agitation before or during polymerization. The surfactant can be anionic, cationic, zwitterionic, or nonionic. It is preferred to use a surfactant that is gentle to the skin.
[0054] The polymer gel is then typically dried in an air circulating belt dryer until the residual moisture content, as measured by EDANA Recommended Test Method No. WSP 230.2-05 "Mass Loss Upon Heating", is preferably 0.5-10 wt.%, more preferably 1-6 wt.%, and most preferably 1.5-4 wt.%. If the residual moisture content is too high, the dried polymer gel will have too low a glass transition temperature T g and further processing is exclusively accompanied by difficulties. If the residual moisture content is too low, the dried polymer gel is too brittle and in the subsequent grinding step, an undesirable large amount of polymer particles with an excessively small particle size ("fines") is obtained. The solid content of the polymer gel before drying is preferably 25% to 90% by weight, more preferably 35% to 70% by weight, most preferably 40% to 60% by weight. The dried polymer gel is then crushed and optionally coarsely ground.
[0055] Thereafter, the dried polymer gel is typically ground and Grading and used for crushing The apparatus is typically a single or multi-stage roll mill, preferably a two or three stage roll mill. The mill may be a mill, a pin mill, a hammer mill or a vibratory mill.
[0056] The average particle size of the polymer particles removed as the product fraction is preferably 150-850 μm, more preferably 250-600 μm, and very particularly 300-500 μm. The average particle size of the product fraction can be measured by EDANA Recommended Test Method No. WSP 220.2 (05) "Particle Size Distribution", where the mass proportions of the sieved fractions are cumulatively plotted and the average particle size is determined on the graph. The average particle size, as used herein, is the mesh size value that results in a cumulative 50% by weight.
[0057] The proportion of polymer particles having a particle size above 150 μm is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
[0058] Polymer particles with too small a particle size will reduce the gel bed permeability (GBP), therefore the proportion of excessively small polymer particles ("fines") should be small.
[0059] Thus, excessively small polymer particles are preferably removed and recycled to the process before, during or immediately after polymerization, i.e., before drying of the polymer gel. The excessively small polymer particles may be wetted with water and / or an aqueous surfactant before or during recycling.
[0060] It is also possible to remove the excessively small polymer particles in a later process step, for example after surface postcrosslinking or in a separate coating step. In this case, the recycled excessively small polymer particles are surface postcrosslinked or coated in another way, for example with fumed silica.
[0061] The proportion of polymer particles having a particle size of maximum 850 μm is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
[0062] The proportion of polymer particles having a particle size of maximum 600 μm is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
[0063] Polymer particles with excessively large particle size reduce the free swelling rate, so the proportion of excessively large polymer particles should be low as well, and therefore excessively large polymer particles are typically removed and recycled to the grinding.
[0064] To further improve the properties, the polymer particles can be thermally surface crosslinked.Suitable surface crosslinking agents are compounds that contain a group that can form a covalent bond with at least two carboxylic acid groups of the polymer particles.Suitable compounds are, for example, polyfunctional amines, polyfunctional amidoamines, polyfunctional epoxides, as described in EP 0083022 A2, EP 0543303 A1 and EP 0937736 A2; difunctional or polyfunctional alcohols, as described in DE 3314019 A1, DE 3523617 A1 and EP 0450922 A2; or β-hydroxyarylamides, as described in DE 10204938 A1 and US 6,239,230.
[0065] In addition, cyclic carbonates in DE 4020780 C1, 2-oxazolidinones and derivatives thereof, such as 2-hydroxyethyl-2-oxazolidinone in DE 19807502 A1, bis- and poly-2-oxazolidinones in DE 19807992 C1, 2-oxotetrahydro-1,3-oxazines and derivatives thereof in DE 19854573 A1, N-acyl-2-oxazolidinones in DE 19854574 A1, cyclic ureas in DE 10204937 A1, bicyclic amide acetals in DE 10334584 A1, oxetanes and cyclic ureas in EP1199327 A2, and morpholine-2,3-diones and derivatives thereof in WO03 / 031482 A1 are described as suitable surface postcrosslinkers.
[0066] Preferred surface postcrosslinkers are ethylene carbonate, ethylene glycol diglycidyl ether, reaction products of polyamides with epichlorohydrin, and mixtures of propylene glycol and butane-1,4-diol.
[0067] Very particularly preferred surface postcrosslinkers are 2-hydroxyethyl-2-oxazolidinone, 2-oxazolidinone and propane-1,3-diol.
[0068] In addition, it is also possible to use surface postcrosslinkers which contain further polymerizable ethylenically unsaturated groups, as described in DE 3713601 A1.
[0069] The amount of surface postcrosslinker is preferably 0.001% to 3% by weight, more preferably 0.02% to 1% by weight, most preferably 0.05% to 0.2% by weight, in each case based on the polymer particles.
[0070] Surface postcrosslinking is typically carried out in such a way that the solution of surface postcrosslinking agent is sprayed onto dry polymer particles. After spray application, the polymer particles coated with surface postcrosslinking agent are surface postcrosslinked and dried, and surface postcrosslinking reaction can occur both before and during drying.
[0071] The spray application of the solution of the surface postcrosslinker is preferably carried out in mixers with moving mixing devices, such as screw mixers, disk mixers and paddle mixers. Particularly preferred are horizontal mixers, such as paddle mixers, and very particularly preferred are vertical mixers. The difference between horizontal mixers and vertical mixers is made by the position of the mixer shaft, i.e. horizontal mixers have a horizontally pivoted mixer shaft, and vertical mixers have a vertically pivoted mixer shaft. Suitable mixers are, for example, horizontal Pflugschar® plowshare mixers (Gebr. Lodige Maschinenbau GmbH, Paderborn, Germany), Vrieco-Nauta continuous mixers (Hosokawa Micron BV, Doetinchem, Netherlands), Processall Mixmill mixers (Processall Incorporated, Cincinnati, USA) and Schugi Flexomix® (Hosokawa Micron BV, Doetinchem, Netherlands). However, it is also possible to spray the surface postcrosslinker solution in a fluidized bed.
[0072] Surface post-crosslinking agent is typically used in the form of an aqueous solution.The penetration depth of surface post-crosslinking agent into polymer particles can be adjusted via the content of non-aqueous solvent and the total amount of solvent.
[0073] When water is used in excess as a solvent, a surfactant is advantageously added, which improves wetting and reduces the tendency to form lumps. However, preference is given to using solvent mixtures such as isopropanol / water, 1,3-propanediol / water, and propylene glycol / water, where the mixture weight ratio is preferably 20:80 to 40:60.
[0074] Surface postcrosslinking is preferably carried out in contact dryer, more preferably paddle dryer, most preferably disk dryer.Suitable dryers are, for example, Hosokawa Bepex® Horizontal Paddle Dryer (Hosokawa Micron GmbH, Leingarten, Germany), Hosokawa Bepex® Disk Dryer (Hosokawa Micron GmbH, Leingarten, Germany), Holo-Flite® Dryers (Metso Minerals Industries Inc., Danville, USA) and Nara Paddle Dryer (NARA Machinery Europe, Frechen, Germany).In addition, fluidized bed dryer can also be used.
[0075] Surface postcrosslinking can be carried out in the mixer itself by heating the jacket or blowing in warm air.Equally suitable is a downstream dryer, such as a tray dryer, a rotary tube oven or a heatable screw.It is particularly advantageous to achieve mixing and thermal surface postcrosslinking in a fluidized bed dryer.
[0076] The preferred reaction temperature is in the range of 100 to 250° C., preferably 110 to 220° C., more preferably 120 to 210° C., and most preferably 130 to 200° C. The preferred residence time at this temperature is preferably at least 10 minutes, more preferably at least 20 minutes, most preferably at least 30 minutes, and typically up to 60 minutes.
[0077] In a preferred embodiment of the present invention, the polymer particles are cooled after surface post-crosslinking.Cooling is preferably carried out in a contact cooler, more preferably in a paddle cooler, and most preferably in a disk cooler.Suitable coolers are, for example, Hosokawa Bepex® Horizontal Paddle Cooler (Hosokawa Micron GmbH, Leingarten, Germany), Hosokawa Bepex® Disc Cooler (Hosokawa Micron GmbH, Leingarten, Germany), Holo-Flite® Coolers (Metso Minerals Industries Inc., Danville, USA) and Nara Paddle Cooler (NARA Machinery Europe, Frechen, Germany).In addition, fluidized bed coolers can also be used.
[0078] In the cooler, the polymer particles are cooled to preferably 40 to 90°C, more preferably 45 to 80°C, and most preferably 50 to 70°C.
[0079] The surface postcrosslinked polymer particles are then again Grading It is possible to make excessively small Polymer particles and / or excessively large polymer particles are removed and recycled to the process.
[0080] To further improve properties, the surface postcrosslinked polymer particles can be coated or rewetted.
[0081] The rewetting is preferably carried out at 40-120°C, more preferably 50-110°C, most preferably 60-100°C. At too low temperatures the polymer particles tend to form agglomerates, at higher temperatures the water has already evaporated to a significant extent. The amount of water used for rewetting is preferably 1%-10% by weight, more preferably 2%-8% by weight, most preferably 3%-5% by weight. Rewetting improves the mechanical stability of the polymer particles and weakens their tendency to take up an electrostatic charge. Rewetting is advantageously carried out in a cooler after thermal surface postcrosslinking.
[0082] Suitable coatings for improving the swelling rate and gel bed permeability (GBP) are, for example, inorganic inert substances, such as water-insoluble metal salts, organic polymers, cationic polymers and divalent or polyvalent metal cations. Suitable coatings for dust binding are, for example, polyols. Suitable coatings for combating the undesirable tendency of polymer particles to solidify are, for example, fumed silica, such as Aerosil® 200, and surfactants, such as Span® 20. Suitable coatings for dust binding to reduce the tendency to solidify and to improve the mechanical stability are polymer dispersions as described in EP 0703265 B1 and waxes as described in US 5,840,321.
[0083] The coated and / or rewetted polymer particles are then again Grading What can be done and excessively small and / or excessively large polymer particles are removed to complete the process. is recycled to
[0084] The present invention further provides a hygiene article comprising a superabsorbent produced by the process of the present invention.
[0085] method The standard test methods referred to hereinafter as "WSP" are described in "Standard Test Methods for the Nonwovens Industry", 2005 Edition, published jointly by international strategic partners EDANA (Herrmann-Debrouxlaan 46, 1160 Oudergem, Belgium, www.edana.org) and INDA (1100 Crescent Green, Suite 115, Cary, North Carolina 27518, USA, www.inda.org), which are available from both EDANA and INDA.
[0086] The measurements should be carried out at an ambient temperature of 23±2° C. and a relative air humidity of 50±10%, unless otherwise stated. The water-absorbing polymer particles are thoroughly mixed prior to this measurement.
[0087] Centrifuge Retention Volume Centrifuge Retention Capacity (CRC) is measured by EDANA Recommended Test Method No. WSP 241.2 (05) "Fluid Retention Capacity in Saline, After Centrifugation".
[0088] Extract amount The extractables content of water-absorbing polymeric particles is determined by EDANA Recommended Test Method No. WSP 270.2 (05) "Extractable". EXAMPLES
[0089] [Example 1] An acrylic acid / sodium acrylate solution was prepared by successively mixing deionized water, 50% by weight sodium hydroxide solution and acrylic acid, with a degree of neutralization corresponding to 71.3 mol %. The solids content of the monomer solution was 38.8% by weight.
[0090] The polyethylenically unsaturated crosslinker used was polyethylene glycol-400 diacrylate (a diacrylate starting from polyethylene glycol having an average molar mass of 400 g / mol). The amount used was 2 kg of crosslinker per ton of monomer solution.
[0091] To initiate the free radical polymerization, 1.03 kg of a 0.25 wt % aqueous hydrogen peroxide solution, 3.10 kg of a 15 wt % aqueous sodium peroxodisulfate solution, and 1.05 kg of a 1 wt % aqueous ascorbic acid solution were used per ton of monomer solution.
[0092] The throughput of the monomer solution was 20 t / h. The reaction solution had a feed temperature of 23.5° C.
[0093] Each component is divided into 6.3m 3 The following amounts were metered continuously into a List Contikneter continuous kneading reactor (LIST AG, Arisdorf, Switzerland) having a capacity of: 20t / hour of monomer solution 40kg / hour of Polyethylene Glycol-400 Diacrylate 82.6 kg / h of hydrogen peroxide solution / sodium peroxodisulfate solution 21kg / hour of ascorbic acid solution
[0094] Between the addition point for the crosslinker and the addition site for the initiator, the monomer solution was inerted with nitrogen.
[0095] After about 50% of the residence time there was an additional metered addition (1000 kg / h) of fines obtained from the production process by grinding and sieving into the reactor. The residence time of the reaction mixture in the reactor was 15 minutes.
[0096] The resulting aqueous polymer gel was applied to the conveyor belt of an air circulating belt dryer by means of a vibrating conveyor belt.
[0097] The air circulation belt dryer had a length of 48 m. The conveyor belt of the air circulation belt dryer had an effective width of 4.4 m.
[0098] The vibrating conveyor belt had a length of 5 m. The conveyor belt had a width of 0.8 m and an effective width of 0.5 m. The angle of repose of the aqueous polymer gel on the conveyor belt was about 15°. The cross section of the polymer gel bed on the conveyor belt was about 0.04 m. 2 The speed of the conveyor belt was 0.5 m / s.
[0099] Starting from one end position, the vibrating conveyor belt accelerated from a first pivot angle β1 of 13° to an angular velocity of 33° / s, decelerated from a second pivot angle β2 of 20° to an angular velocity of 17° / s, and decelerated from a third pivot angle β3 to the other end position. The total pivot angle was 50°. The double pass (from the first end position to the other end position and back) lasted about 7 seconds. The rotating conveyor belt had a surface of polytetrafluoroethylene (PTFE).
[0100] The temperature of the aqueous polymer gel on the vibrating conveyor belt was 90°C.
[0101] Below the vibrating conveyor belt there was a stripping device. The stripping device was a vertical scraper mounted transverse to the running direction of the rotating conveyor belt. The scraper was inclined at 20° to the running direction of the rotating conveyor belt. The distance of the stripping device from the discharge end was about 5 cm, which means that the stripping device was in the area of the bending rolls. The distance of the stripping device from the rotating conveyor belt was 1 mm. The stripping device strips off the aqueous polymer gel adhering to the outside of the rotating conveyor belt.
[0102] Below the vibrating conveyor belt there were additionally three two-phase nozzles. The two-phase nozzles were arranged transversely to the running direction of the conveyor belt. The distance between the two-phase nozzles was in each case about 20 cm. The distance of the two-phase nozzles from the discharge end was about 20 cm. The distance of the two-phase nozzles from the rotating conveyor belt was about 20 cm. A total of 10 kg / h of water and 100 kg / h of air were sprayed.
[0103] The stripping device allowed for efficient cleaning of the rotating conveyor belt. Over a period of six months, there was no noticeable caking on the conveyor belt.
[0104] The aqueous polymer gel was dried by continuously flowing the air / gas mixture around the aqueous polymer gel on the air circulating belt dryer, the residence time in the air circulating belt dryer was 37 minutes.
[0105] The dried polymer gel was ground and sieved to a particle size fraction of 150-850 μm.
[0106] The resulting water-absorbing polymer particles had a centrifuge retention capacity (CRC) of 34.9 g / g and an extractables content of 8.5 wt %.
[0107] [Example 2 (Comparative Example)] The procedure was the same as in Example 1, except that the spray nozzles on the vibrating conveyor belt were switched off.
[0108] It was possible to clean the rotating conveyor belt only with difficulty by means of a stripping device. There was noticeable caking on the conveyor belt, especially where the polymer gel had already dried. After several weeks of continuous production, production had to be stopped and the conveyor belt cleaned, or it had to be replaced due to damage.
Claims
1. a) at least one ethylenically unsaturated monomer having an acid group, which is at least partially neutralized; b) at least one crosslinker, and c) at least one initiator 1. A method for producing superabsorbent particles, comprising preparing an aqueous polymer gel by polymerizing a monomer solution or suspension comprising: The method includes the steps of drying the obtained aqueous polymer gel in an air circulating belt dryer, grinding, and classifying the same; The aqueous polymer gel is introduced into the air circulating belt dryer by a rotating vibrating conveyor belt, the underside of the rotating vibrating conveyor belt is freed from adhesion of the aqueous polymer gel by at least one stripping device, and 2 to 20 kg / hour of water is sprayed by at least one spray nozzle onto the underside of the rotating vibrating conveyor belt; the at least one atomizing nozzle is at least one two-phase nozzle, and the weight ratio of atomizing gas to water is between 2 and 20; The at least one spray nozzle is located beyond the stripping device in the running direction of the rotating vibrating conveyor belt, method.
2. 2. The method of claim 1, wherein the distance of the stripping device from the discharge end of the rotating vibrating conveyor belt is less than 20% of the length of the rotating vibrating conveyor belt, and the length of the rotating vibrating conveyor belt is the distance of the pivot axis from the discharge end.
3. 3. The method according to claim 1 or 2, wherein the stripping device attached to the underside of the rotating vibrating conveyor belt is a scraper.
4. 4. The method according to claim 3, wherein the scraper is inclined at an angle of 5° to 45° to the horizontal counter to the running direction of the rotating vibrating conveyor belt.
5. 5. The method according to claim 3 or 4, wherein the distance of the scraper from the underside of the rotating vibrating conveyor belt is between 0.1 and 5 mm.
6. 6. The method according to any one of claims 1 to 5, wherein the distance of the at least one spray nozzle from the discharge end of the rotating vibrating conveyor belt is between 1% and 50% of the length of the rotating vibrating conveyor belt, and the length of the rotating vibrating conveyor belt is the distance of the pivot axis from the discharge end.
7. The method according to any one of claims 1 to 6, wherein the distance of the spray nozzle from the rotating vibrating conveyor belt is between 5 and 50 cm.
8. 8. The method according to any one of claims 1 to 7, wherein water is sprayed onto the underside of the rotating vibrating conveyor belt by at least two two-phase nozzles.
9. 9. The method according to any one of claims 1 to 8, wherein the rotating vibrating conveyor belt has a length of 2 to 10 m, the length of the rotating vibrating conveyor belt being the distance of the pivot from the discharge end.
10. 10. The method according to any one of claims 1 to 9, wherein the surface of the rotating vibrating conveyor belt has a contact angle with water of at least 60° at 23°C.
11. 11. The method according to claim 1, further comprising a step of thermal surface post-crosslinking the obtained aqueous polymer gel.
Citation Information
Patent Citations
Process and apparatus for producing water-absorbable resin of polyacrylic acid (SALT) type
EP2700667A1
Mist type belt cleaner equipment
JP1998250821A
Method for manufacturing water-absorbent resins
JP2010531366A
Method for producing superabsorbent polymer particles
JP2012528909A
Method for producing superabsorbent polymer particles with improved properties
JP2015521678A